Polycarbonate composition, and preparation method therefor and use thereof
By controlling the sulfur content of the glass fiber and using maleic anhydride grafted polymers, the interfacial bonding force of the polycarbonate composition is improved, and the problems of low flexural modulus and poor stability of the polycarbonate composition in the moist heat aging test are solved. , achieving high rigidity and high humidity and heat aging stability, and is suitable for the preparation of high-performance products such as lens holders.
Patent Information
- Application Number
- PCT/CN2024/090168
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Existing polycarbonate compositions have low flexural modulus and poor wet and heat stability in wet and heat aging tests, and cannot meet the high mechanical strength and high wet and heat aging requirements of the lens holder.
By controlling the sulfur content of the glass fiber to less than or equal to 500ppm, combined with the maleic anhydride graft polymer, the interface bonding force between the glass fiber and the polycarbonate resin is improved, preventing the reduction of the flexural modulus, and improving the humid heat aging stability.
The flexural modulus and wet-heat aging stability of the polycarbonate composition are significantly improved, and the retention rate of the notched impact strength of the cantilever reaches 83.9%-92.5%, making it suitable for the preparation of high-performance lens holders.
Smart Images

Figure PCTCN2024090168-FTAPPB-I100001 
Figure PCTCN2024090168-FTAPPB-I100002 
Figure PCTCN2024090168-FTAPPB-I100003
Abstract
Description
A polycarbonate composition and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of polymer materials, and more particularly to a polycarbonate composition, a preparation method thereof, and an application thereof. Background Art
[0002] Polycarbonate (PC) is an excellent engineering plastic with excellent overall performance, including high mechanical strength, good impact toughness, dimensional stability, good heat resistance, and good electrical insulation. It is widely used in home appliances, digital products, IT products, and other fields. Glass fiber-reinforced polycarbonate materials have advantages such as high strength, excellent temperature resistance, good corrosion resistance, good stress cracking resistance, and good electrical properties. They are widely used in various fields, especially in the preparation of lens brackets in the imaging equipment industry.
[0003] With the development of lens holders that are more refined and have higher performance, the materials are required to have higher mechanical strength, and the lens holders need to meet relevant requirements for moisture and heat resistance tests.
[0004] While ablating glass fibers using existing conventional methods improves impact strength and stain resistance to a certain extent, it also significantly reduces the interfacial bonding between the glass fiber and the polycarbonate resin, significantly reducing the material's flexural modulus and rendering it unsuitable for use in lens mount products. Furthermore, existing conventional methods fail to specifically improve the polycarbonate composition's notched Izod impact strength retention of over 83.9% in a damp-heat aging test at 85°C, 85% humidity, and 1000 hours.
[0005] Summary of the Invention
[0006] The technical problem to be solved by the present invention is to overcome the defects and shortcomings of the existing polycarbonate composition, namely low flexural modulus and poor wet heat aging stability, and to provide a polycarbonate composition. By controlling the sulfur content of the glass fiber, the flexural modulus of the polycarbonate composition is prevented from being significantly reduced, and the retention rate of the cantilever beam notched impact strength of the polycarbonate composition in a wet heat aging test at 85°C, 85% humidity, and 1000 hours is effectively improved, so that the material has high rigidity and high wet heat aging stability.
[0007] Another object of the present invention is to provide a method for preparing the polycarbonate composition.
[0008] Another object of the present invention is to provide an application of a polycarbonate composition in the preparation of lens holders and other bracket products.
[0009] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0010] A polycarbonate composition comprising the following components in parts by weight:
[0011] 100 parts of polycarbonate; 8-40 parts of glass fiber; 0.1-1 parts of maleic anhydride grafted polymer; 0-5 parts of processing aid;
[0012] The sulfur content of the glass fiber is less than or equal to 500 ppm, preferably 88-400 ppm; more preferably 125-310 ppm, further preferably 133-220 ppm, and even more preferably 140-210 ppm.
[0013] The content of sulfur in the composition is determined by the following method:
[0014] Weigh 10g of the composition and add 100ml of dichloromethane to dissolve the polycarbonate. The glass fiber will not react in the solvent and will precipitate. The precipitate is filtered and separated, and then washed with deionized water three times. It is then dried at 100℃ for 1h to obtain independent glass fibers.
[0015] 1-3 g of the glass fiber sample is weighed, placed in a microwave digestion tank, concentrated nitric acid is added, the tank is covered, and the tank is placed in a microwave digester for digestion. After the digestion process is completed, the tank is cooled to room temperature, the solution is transferred to a 100 mL volumetric flask, the digestion tank and the lid are washed with water three times, the washing liquid is added to the volumetric flask, and the volume is adjusted to the scale with water. Under the specified instrument working conditions, the zero point is calibrated using the first point S0 (0.0) in the standard working solution, the luminescence intensity of the sulfur element in the standard working solution is measured, and an ICP inductively coupled plasma emission spectrometer is used to draw a working curve based on the sulfur content and the corresponding measured luminescence intensity value, and the sulfur content in the glass fiber sample is measured under the same conditions as the working curve.
[0016] After extensive research, the inventors of the present application have discovered that the sulfur content of glass fiber is closely related to the content of hydrophilic surfactants such as sulfonic acid in the glass fiber. By controlling the sulfur content of the glass fiber to be less than or equal to 500 ppm, the hydrophilicity of the glass fiber can be appropriately reduced without destroying the original properties of the glass fiber. While ensuring that the glass fiber has appropriate hydrophilicity, the compatibility of polycarbonate and glass fiber is improved by grafting maleic anhydride polymer, so that the glass fiber and polycarbonate resin have good interfacial bonding strength, ultimately achieving the purpose of preventing a significant decrease in the flexural modulus of the polycarbonate composition while having high wet heat aging stability.
[0017] Preferably, the hydrophilicity of the glass fiber satisfies the following condition: the bubble disappearance time is greater than or equal to 3 minutes. The hydrophilicity of the glass fiber is measured by the following method: 5 g of a glass fiber sample is weighed and placed in a mixed solution of 10 ml of alcohol and 40 ml of pure water, and shaken for 1 minute until bubbles are formed throughout the glass fiber. The timer is started and the time it takes for bubbles to disappear is recorded.
[0018] More preferably, the hydrophilicity of the glass fiber satisfies the following condition: 3 min ≤ bubble disappearance time ≤ 5 min.
[0019] Preferably, the glass fiber is treated as follows: burning the glass fiber to a loss on ignition of ≥0.8% to make the sulfur content of the glass fiber less than or equal to 500 ppm; or eluting the glass fiber to make the sulfur content of the glass fiber less than or equal to 500 ppm.
[0020] In a specific embodiment, the burning temperature and / or burning time can be controlled to control the ignition loss of the glass fiber, thereby controlling the sulfur content of the glass fiber.
[0021] Optionally, the calcination temperature may be 600-800° C., and the calcination time may be 60-120 minutes.
[0022] In a specific embodiment, the glass fiber can be eluted in an ethanol aqueous solution, and the sulfur content of the glass fiber can be controlled by controlling the weight ratio of ethanol to water in the ethanol aqueous solution and / or the elution time.
[0023] Optionally, the concentration of the ethanol aqueous solution may be 1 ml / (1-3) ml, and the elution time may be 8-12 hours.
[0024] Preferably, the polycarbonate composition comprises the following components in parts by weight: 100 parts of polycarbonate; 15-25 parts of glass fiber; 0.3-0.8 parts of maleic anhydride grafted polymer; and 0-3 parts of processing aid.
[0025] The average retained length L of the glass fibers in the polycarbonate composition is 250 to 350 mm. Research conducted by the present applicant has found that, in the present invention, when the average retained length L of the glass fibers in the polycarbonate composition is 250 to 350 mm, the polycarbonate composition simultaneously exhibits high rigidity, low anisotropy, and good wet-heat stability. The average diameter of the glass fibers can be 7 to 15 μm.
[0026] Optionally, the melt mass flow rate of the polycarbonate is 2.5 to 20 g / 10 min, the test standard is GB / T3682.1-2018, and the test conditions are 300° C. and 1.2 kg.
[0027] In order to further reduce the anisotropy of the composition and thus reduce the warpage of the composition, preferably, the melt mass flow rate of the polycarbonate is 3 to 10 g / 10 min, the test standard is GB / T3682.1-2018, and the test conditions are 300° C. and 1.2 kg.
[0028] Optionally, the maleic anhydride grafted polymer is one or more of maleic anhydride grafted PS, maleic anhydride grafted ABS or maleic anhydride grafted PE.
[0029] Preferably, the maleic anhydride grafted polymer is one or more of maleic anhydride grafted PS or maleic anhydride grafted ABS.
[0030] Optionally, in the maleic anhydride grafted polymer, the mass grafting rate of maleic anhydride is 5 to 30%, preferably 16 to 25%, and more preferably 17 to 20%.
[0031] The maleic anhydride grafting rate is tested using an acid-base titration method. The test procedure involves accurately weighing 0.4g of a dried maleic anhydride grafted sample into a 250ml stoppered Erlenmeyer flask. Add approximately 80ml of xylene. Once the sample is fully dissolved, pipette in an appropriate amount of a KOH-ethanol standard solution. Reflux the solution at a predetermined temperature for a predetermined time. After cooling, shake the Erlenmeyer flask thoroughly while pipetting in an appropriate amount of a HCl-isopropanol standard solution. Add 1-2 drops of phenolphthalein indicator and titrate with the KOH-ethanol standard solution. The titration endpoint is reached when the solution changes from colorless to light red. Record the volume V0 of the KOH-ethanol standard solution added during sample reflux, the volume V1 of the KOH-ethanol standard solution consumed in titration, and the volume V2 of the HCl-isopropanol standard solution added. C1 and C2 are the concentrations of the KOH-ethanol solution and HCl-isopropanol, respectively. Calculate the grafting rate of the sample according to the formula: A grafted = ((V0+V1)C1-V2C2) / m.
[0032] Optionally, the processing aid includes one or more of a stabilizer, a flame retardant, an anti-drip agent, a lubricant, a release agent, a plasticizer, a filler, an antistatic agent, an antibacterial agent or a colorant.
[0033] Optionally, the stabilizer is one or more of hindered phenols, phosphites or benzotriazoles.
[0034] Optionally, the flame retardant is one or more of a phosphate flame retardant, a sulfonate flame retardant or a brominated polycarbonate.
[0035] Optionally, the anti-drip agent is a polytetrafluoroethylene anti-drip agent.
[0036] Optionally, the lubricant is one or more of polytetrafluoroethylene lubricants, polyethylene lubricants or silicone lubricants.
[0037] Optionally, the release agent is one or more of a PPA release agent, a montan wax release agent or a silicone release agent.
[0038] Optionally, the plasticizer is one or more of acrylic acid or silicone rubber.
[0039] Optionally, the filler is one or more of talc, wollastonite or mica.
[0040] Optionally, the antistatic agent is one or more of glycerides or polyethers.
[0041] Optionally, the antibacterial agent is one or more of silver ions, anilides, imidazoles, thiazoles, isothiazolone derivatives, quaternary ammonium salts, bisguanidines or phenols.
[0042] Optionally, the colorant is one or more of carbon black, titanium dioxide, phthalocyanine blue or anthraquinone red.
[0043] The present invention also protects a method for preparing the polycarbonate composition described in any one of the above items, comprising the following steps:
[0044] Polycarbonate, maleic anhydride grafted polymer and processing aid are added to the extruder from the main feed port, glass fiber is added to the extruder from the side feed port, melt-extruded at 270-290° C., granulated, and dried to obtain the polycarbonate composition.
[0045] The extruder may be a twin-screw extruder.
[0046] The polycarbonate composition prepared by the present invention has excellent high rigidity, high toughness and wet heat stability, and can be widely used in the preparation of plastic products. The present invention particularly protects the use of the polycarbonate composition in the preparation of lens holders.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The present invention discloses a polycarbonate composition. By controlling the sulfur content of glass fiber, the flexural modulus of the polycarbonate composition is prevented from being significantly reduced. The polycarbonate composition also effectively improves the retention rate of the cantilever beam notched impact strength in a wet heat aging test at 85°C, 85% humidity, and 1000 hours, thereby ensuring that the material has high rigidity and high wet heat aging stability.
[0049] The polycarbonate composition of the present invention has an anisotropy coefficient of less than or equal to 1.63, a flexural modulus of 3245 to 6560 MPa, and an Izod notched impact strength of 6.2 to 14.6 KJ / m 2 The retention rate of the Izod notched impact strength in the damp heat aging test at 85°C, 85% humidity and 1000h can reach 83.9% to 92.5%. DETAILED DESCRIPTION
[0050] The present invention will be further described below in conjunction with specific embodiments, but the examples do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the examples of the present invention are conventionally purchased raw materials and reagents.
[0051] Such as: Table 1
[0052] Table 2
[0053] Examples 1 to 16
[0054] A polycarbonate composition comprises the following components, measured in parts by weight: polycarbonate, glass fiber, and a maleic anhydride grafted polymer, wherein the specific content of each component is shown in Table 1 below.
[0055] Table 1 Composition of the polycarbonate composition of each embodiment (in parts by weight)
[0056] Continued Table 1:
[0057] The preparation method of the polycarbonate composition is as follows:
[0058] Polycarbonate and maleic anhydride grafted polymer are added to a twin-screw extruder from a main feed port, and glass fiber or correspondingly treated glass fiber is added to the twin-screw extruder from a side feed port. The extruder is melt-extruded and granulated at 270-290° C., and the polycarbonate composition is obtained after drying.
[0059] Comparative Examples 1 to 5
[0060] A polycarbonate composition comprising the following components in parts by weight:
[0061] Polycarbonate, glass fiber, maleic anhydride grafted polymer, wherein the specific content of each component is shown in Table 2 below.
[0062] Table 2 Composition of the polycarbonate compositions of the comparative examples (in parts by weight)
[0063] The preparation method of the polycarbonate composition is the same as that in the embodiment, and will not be repeated here.
[0064] Result detection
[0065] (1) Test method for loss on ignition of glass fiber: Take 3g of glass fiber and burn it at 650℃ for 1h. Weigh it and record it as X. Combustible content = (3-X) / 3*100.
[0066] (2) Test method for sulfur content of glass fiber:
[0067] Weigh 1-3 g of glass fiber sample, place it in a microwave digestion tank, add concentrated nitric acid, cover it, and place it in a microwave digester for digestion; after the digestion process is completed, cool it to room temperature, transfer the solution to a 100 mL volumetric flask, wash the digestion tank and cover with water three times, add the washing liquid to the volumetric flask, and dilute to the scale with water.
[0068] Under the determined instrument working conditions, the zero point was corrected with the first point S0 (0.0) in the standard working solution, and the luminescence intensity of the sulfur element in the standard working solution was measured. The ICP inductively coupled plasma emission spectrometer drew a working curve based on the sulfur content and the corresponding measured luminescence intensity value, and the sulfur content in the glass fiber sample was measured under the same conditions as the working curve.
[0069] (3) Glass fiber hydrophilicity test method: Weigh 5g of glass fiber sample and place it in a mixed solution of 10ml of alcohol and 40ml of pure water. Shake for 1 minute until bubbles appear throughout the fiber. Start timing and record the time when the bubbles disappear. If the bubble disappearance time is greater than 5 minutes, it is judged to have low hydrophilicity; if the bubble disappearance time meets 3 minutes ≤ bubble disappearance time ≤ 5 minutes, it is judged to have medium hydrophilicity; if the bubble disappearance time is less than 3 minutes, it is judged to have high hydrophilicity.
[0070] (4) Anisotropy test method: Polycarbonate composition particles are added to an injection molding machine, melted at a temperature of 270°C to 290°C, and injection molded into tensile specimens according to ISO 527-2-2019. The linear expansion coefficients in the transverse and longitudinal directions are tested according to ASTM D696-2016. The linear expansion coefficient in the flow direction is recorded as Af, and the linear expansion coefficient in the flow direction is recorded as At. The anisotropy coefficient = (At-Af) / Af. The lower the anisotropy coefficient, the better.
[0071] (5) Rigidity test: The polycarbonate composition particles were added to an injection molding machine, melted at a temperature of 270°C to 290°C, and injection molded into bending specimens according to the ISO 178-2019 standard. The bending modulus of 5 specimens was tested and the average value was taken.
[0072] (6) Toughness test: The polycarbonate composition particles were added to an injection molding machine, melted at a temperature of 270°C to 290°C, and injection molded into impact specimens according to the ISO 180-2019 standard. The cantilever beam notched impact strength of 5 specimens was tested, with the notch type being Type A, and the average value was taken.
[0073] (7) Wet heat stability test: The polycarbonate composition particles were added to an injection molding machine and melted at a temperature of 270°C to 290°C. Ten impact bars according to the ISO 180 standard were injection molded. The performance of five bars was tested and the average value was recorded as X1. The remaining five bars were placed in a wet heat aging chamber at 85°C and 85% humidity for 1000 hours. The impact performance was tested and the average value was recorded as X2. Impact retention rate = (X1-X2) / X1*100.
[0074] (8) Average glass fiber retention length L: tested using ISO 22314-2008 glass fiber retention length test standard.
[0075] The specific test results are shown in Table 3 below:
[0076] From the above data, it can be seen that the polycarbonate composition of the present invention has an anisotropy coefficient of less than or equal to 0.92, a flexural modulus of 3120 to 6560 MPa, and an Izod notched impact strength of 7 to 14.6 KJ / m 2 The notched Izod impact strength retention rate in a 1000h damp heat aging test at 85°C and 85% humidity can reach 88.5-93.9%. It has excellent low anisotropy and damp heat stability, while also having high rigidity and toughness, making it particularly suitable for surveillance lens products.
[0077] When the sulfur content of glass fiber is 500 ppm or less, it prevents the formation of interfacial voids due to reduced surface bonding between the glass fiber and the resin matrix. This prevents interfacial voids from absorbing energy during impact damage and preventing fracture, thereby improving the material's notched impact strength. Furthermore, it prevents the weakening of the bonding between the glass fiber and the resin, which could lead to a decrease in the material's modulus.
[0078] It can be seen from the examples and comparative examples 1 and 4 that the sulfur content of glass fiber 4-1 and glass fiber 3-1 is greater than 500 ppm, and the wet heat stability of comparative examples 1 and 4 is significantly reduced.
[0079] Obviously, the above embodiments of the present invention are merely examples for the purpose of clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all embodiments here. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention shall be included within the scope of protection of the claims of the present invention.
Claims
1. A polycarbonate composition, characterized in that By weight, it includes the following components: 100 parts of polycarbonate; 8-40 parts of glass fiber; 0.1-1 parts of maleic anhydride grafted polymer; 0-5 parts of processing aid; Wherein, the sulfur content of the glass fiber is less than or equal to 500 ppm.
2. The polycarbonate composition according to claim 1, characterized in that The hydrophilicity of the glass fiber meets the following conditions: the bubble disappearance time is greater than or equal to 3 minutes; wherein, the hydrophilicity of the glass fiber is measured by the following method: weigh 5 g of the glass fiber sample, place it in a mixed solution of 10 ml of alcohol and 40 ml of pure water, shake it for 1 minute until the whole bubble is shaken, start timing, and record the time when the bubbles disappear.
3. The polycarbonate composition according to claim 1, wherein The glass fiber is treated by: burning the glass fiber until the loss on ignition is ≥0.8% so that the sulfur content of the glass fiber is less than or equal to 500 ppm; or, by eluting, eluting the glass fiber until the sulfur content of the glass fiber is less than or equal to 500 ppm.
4. The polycarbonate composition according to claim 1, characterized in that The sulfur content of the glass fiber is preferably 88 to 400 ppm, more preferably 125 to 310 ppm, and further preferably 133 to 220 ppm; the hydrophilicity of the glass fiber satisfies the following condition: 3 min ≤ bubble disappearance time ≤ 5 min.
5. The polycarbonate composition according to claim 1, wherein The average retention length L of the glass fibers in the polycarbonate composition is 250 to 350 mm.
6. The polycarbonate composition according to claim 1, wherein The melt mass flow rate of the polycarbonate is 2.5 to 20 g / 10 min, the test standard is GB / T3682.1-2018, and the test conditions are 300° C. and 1.2 kg.
7. The polycarbonate composition according to claim 1, wherein The maleic anhydride grafted polymer is one or more of maleic anhydride grafted PS, maleic anhydride grafted ABS or maleic anhydride grafted PE; the mass grafting rate of maleic anhydride is 5-30%.
8. The polycarbonate composition according to claim 1, wherein The processing aids include one or more of stabilizers, flame retardants, anti-dripping agents, lubricants, mold release agents, plasticizers, fillers, antistatic agents, antibacterial agents or colorants.
9. The method for preparing the polycarbonate composition according to any one of claims 1 to 8, characterized in that: The steps include: Polycarbonate, maleic anhydride grafted polymer and processing aids are added to the extruder from the main feed port, and glass fiber is added to the extruder from the side feed port. The extruder is melt-extruded at 270-290°C, granulated, and dried. Then the polycarbonate composition is obtained.
10. Use of the polycarbonate composition according to any one of claims 1 to 8 in the preparation of a lens holder.
Citation Information
Patent Citations
Preparation method of high-gloss air conditioner outdoor unit shell
CN107793731A
Polycarbonate composition and preparation method thereof
CN111995854A
Polycarbonate composition and preparation method and application thereof
CN112210201A
Polycarbonate composition as well as preparation method and application thereof
CN116478524A
High rigidness glass fiber reinforced polycarbonate flame retardant resin composition having improved strength and hardness and molded article thereof
KR1020150067740A