Method for manufacturing hot-dip galvanized steel sheet

The method of annealing in a non-oxidizing atmosphere with controlled hydrogen levels and oxidation treatment enhances the surface quality and delayed fracture resistance of hot-dip galvanized steel sheets, overcoming previous challenges in high-strength steel sheets by preventing selective oxidation and ensuring effective hydrogen release.

WO2024224581A1PCT designated stage expired Publication Date: 2024-10-31JFE STEEL CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/016784
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing methods for manufacturing hot-dip galvanized steel sheets struggle to achieve both excellent delayed fracture resistance and good surface quality, particularly in high-strength steel sheets, as reducing hydrogen levels can lead to selective oxidation of elements like Si and Mn, affecting plating properties and surface quality.

Method used

A method involving annealing in a non-oxidizing atmosphere with specific temperature and hydrogen concentration conditions, followed by oxidation treatment and controlled cooling, to optimize hydrogen release and surface quality, ensuring a low hydrogen concentration in the steel sheet and preventing selective oxidation of easily oxidizable elements.

Benefits of technology

This approach results in hot-dip galvanized steel sheets with a beautiful surface appearance and excellent delayed fracture resistance, effectively addressing the limitations of previous techniques by optimizing annealing conditions and hydrogen management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention makes it possible to manufacture a hot-dip galvanized steel sheet of which the surface has a pleasing appearance lacking non-plating, and which has excellent delayed fracture resistance. This method for manufacturing a hot-dip galvanized steel sheet includes annealing a steel sheet in a non-oxidizing atmosphere and then hot-dip galvanizing the steel sheet. The annealing in the non-oxidizing atmosphere includes a first step and a second step. In the first step, a steel sheet is annealed for a predetermined time in a reducing atmosphere having a high hydrogen concentration and a predetermined dew point and temperature so as to reduce the Fe oxide present in the surface layer of the steel sheet. In the subsequent second step, the steel sheet is annealed for a predetermined time in a non-oxidizing atmosphere having a low hydrogen concentration and a predetermined dew point and temperature, and the hydrogen dissolved in the steel is discharged from the steel sheet. If necessary, an oxidation treatment for generating Fe oxide on the surface layer of the steel sheet in a prescribed oxidizing atmosphere is performed before annealing.
Need to check novelty before this filing date? Find Prior Art

Description

Manufacturing method of hot-dip galvanized steel sheet

[0001] The present invention relates to a method for producing a hot-dip galvanized steel sheet.

[0002] In recent years, surface-treated steel sheets, which are steel sheets imparted with rust resistance, including galvannealed steel sheets (including galvannealed steel sheets) with excellent rust resistance, have been widely used in fields such as automobiles, home appliances, and building materials. Furthermore, from the viewpoint of improving automobile fuel efficiency and collision safety, the application of high-strength steel sheets to automobile body materials has been progressing in order to reduce the thickness of automobile bodies by increasing the strength of the body material, thereby reducing the weight and increasing the strength of the automobile body itself. Generally, galvannealed steel sheets are produced by using hot-rolled steel sheets or cold-rolled steel sheets as base materials, recrystallizing the base steel sheets in a CGL annealing furnace, and then galvanizing them. Galvannealed steel sheets are produced by further alloying treatment after hot-dip galvanizing.

[0003] Annealing requires that steel sheets be held in a reducing atmosphere containing hydrogen. During this process, hydrogen in the furnace penetrates the steel sheet. When the steel sheet is subsequently cooled and hot-dip plated, the hydrogen remains in the steel sheet as diffusible hydrogen in the steel. Because hydrogen is impermeable through plating, diffusible hydrogen in the steel is not released from the steel sheet after plating. Therefore, a problem has arisen in that a large amount of diffusible hydrogen in the steel reduces delayed fracture resistance. In particular, in high-strength steel sheets with a tensile strength of 780 MPa or more, hydrogen in the steel tends to remain after annealing, significantly reducing delayed fracture resistance. This problem is due to the fact that high-strength steel sheets with a tensile strength of 780 MPa or more require the formation of hard structures such as martensite and bainite to achieve a desired strength. To achieve this, an austenite phase must be formed during the annealing process. However, the austenite phase is more likely to absorb large amounts of hydrogen than the ferrite phase, and because the hydrogen diffusion rate is slower, once hydrogen is absorbed during the annealing process, it is difficult to release it during the cooling process.

[0004] Conventionally, as a technique for reducing the amount of hydrogen in a steel sheet, for example, the following has been proposed. 2A technique is disclosed in which dehydrogenation is performed at 450 to 550°C in an atmosphere with a hydrogen concentration of 8 to 20%, followed by hot-dip galvanization. Patent Document 2 also discloses a technique in which a hot-rolled steel sheet is subjected to reduction annealing in the range of 650 to 950°C and then hot-dip galvanization, in which the amount of hydrogen in the steel sheet is reduced by controlling the relationship between the annealing temperature and the hydrogen concentration in the annealing furnace so as to satisfy the following formula (1): 1≦H≦−0.05×RT+57.5 (1) where H is the hydrogen concentration in the furnace, and RT is the annealing temperature.

[0005] Furthermore, Patent Document 3 discloses a technique for obtaining good surface quality in a method of hot-dip galvanizing after reduction annealing a steel sheet containing Si, Mn, and Al, by controlling the hydrogen concentration in the furnace during reduction annealing to be 10% by volume or more, and the relationship between the hydrogen partial pressure and the water vapor partial pressure in the furnace atmosphere gas at 650°C or higher but lower than 750°C to satisfy the following formula (2), and similarly controlling the relationship between the hydrogen partial pressure and the water vapor partial pressure in the furnace atmosphere gas at 750°C or higher but lower than 950°C to satisfy the following formula (3): log(P H2O / P H2 )≦-1.55...(2) -0.91≦log(P H2O / P H2 ) ≦−0.635 ... (3)

[0006] Japanese Patent Application Laid-open No. 54-130443 Patent No. 3266008 Patent No. 5811841

[0007] However, while the techniques disclosed in Patent Documents 1 and 2 are both intended to suppress blistering (plating blistering) in hot-rolled steel sheets, in order to improve the delayed fracture resistance of high-strength steel sheets having an austenitic phase, it is necessary to further reduce the amount of hydrogen in the steel by further reducing the hydrogen content in the atmosphere. However, further reducing the amount of hydrogen in the atmosphere promotes selective oxidation of easily oxidizable elements such as Si and Mn contained in the high-strength steel sheet, thereby impairing galvanization and preventing good surface quality. Therefore, the methods disclosed in Patent Documents 1 and 2, which uniformly reduce hydrogen in the furnace, are difficult to achieve good surface quality and delayed fracture resistance. Furthermore, the technique disclosed in Patent Document 3 aims to improve the galvanization of steel containing Si, Mn, and Al and obtain good surface quality by varying the ratio of water vapor partial pressure to hydrogen partial pressure depending on the annealing temperature. However, it is necessary to control the hydrogen concentration in the furnace to 10% or more, and the technique does not take into consideration reducing the hydrogen concentration in the steel. As a result, it is difficult to improve the delayed fracture resistance of high-strength steel sheets.

[0008] Therefore, an object of the present invention is to solve the above-mentioned problems of the conventional art and to provide a manufacturing method by which a hot-dip galvanized steel sheet having an attractive surface appearance without bare spots and excellent delayed fracture resistance can be manufactured.

[0009] As a result of extensive investigations aimed at solving the above-mentioned problems, the present inventors have found that in a method for producing a hot-dip galvanized steel sheet in which a steel sheet is annealed in a non-oxidizing atmosphere and then hot-dip galvanized, a hot-dip galvanized steel sheet excellent in coating appearance and delayed fracture resistance can be produced by optimizing the annealing conditions in a non-oxidizing atmosphere. The present invention has been made based on this finding, and the gist of the present invention is as follows. [1] A method for producing a hot-dip galvanized steel sheet (including the case where an alloying treatment is performed after hot-dip galvanizing) in which a steel sheet is annealed in a non-oxidizing atmosphere in a continuous annealing furnace and then hot-dip galvanized, wherein the annealing comprises: a first step of holding the steel sheet at a temperature of 650°C to 950°C in an atmosphere with a dew point of -55°C to +20°C and a hydrogen concentration of 5 to 25% by volume for a period of 20 to 150 seconds; and a second step of holding the steel sheet that has undergone the first step at a temperature of 700°C to 950°C in an atmosphere with a dew point of -50°C to +20°C and a hydrogen concentration of 0.2 to less than 5.0% by volume for a period of 30 to 300 seconds. [2] In the production method of the above [1], a method for producing a hot-dip galvanized steel sheet is further comprising the step of: 2[3] A method for producing a hot-dip galvanized steel sheet, comprising carrying out an oxidation treatment at a temperature of 400°C or more and 900°C or less in an atmosphere containing 1000 volume ppm or more of hydrogen. [3] A method for producing a hot-dip galvanized steel sheet in the production method described above in [2], wherein the oxidation treatment is carried out in the process of raising the temperature of the steel sheet for the annealing. [4] A method for producing a hot-dip galvanized steel sheet in the production method described above in [3], wherein the oxidation treatment is carried out over a temperature rise range of 50°C or more in the process of raising the temperature of the steel sheet for the annealing. [5] A method for producing a hot-dip galvanized steel sheet in any of the production methods described above in [1] to [4], wherein the atmosphere in the first annealing step has a hydrogen concentration of 8 volume % or more. [6] A method for producing a hot-dip galvanized steel sheet in any of the production methods described above in [1] to [5], wherein the atmosphere in the second annealing step has a hydrogen concentration of 2.0 volume % or more. [7] A method for producing a hot-dip galvanized steel sheet in any of the methods [1] to [6] above, wherein the hydrogen concentration (however, the amount of diffusible hydrogen) in the substrate steel sheet of the produced hot-dip galvanized steel sheet is 0.30 mass ppm or less. [8] A method for producing a hot-dip galvanized steel sheet in any of the methods [1] to [7] above, wherein the Si content of the substrate steel sheet is 0.1 mass % or more. [9] A method for producing a hot-dip galvanized steel sheet in any of the methods [1] to [8] above, wherein the total area fraction of martensite, bainite, and retained γ in the substrate steel sheet is 30% or more, and the tensile strength is 780 MPa or more.

[10] A method for producing a hot-dip galvanized steel sheet in any of the methods [1] to [8] above, wherein the total area fraction of martensite, bainite, and retained γ in the substrate steel sheet is 50% or more, and the tensile strength is 980 MPa or more.

[11] In the manufacturing method of any one of the above [1] to

[10] , the steel sheet that has undergone the annealing is cooled in an atmosphere having a dew point of −20° C. or less and a hydrogen concentration of 5 to 25% by volume at an average cooling rate of 5° C. / s in a temperature range from a final holding temperature in the annealing to 600° C., and further cooled to a temperature of 150 to less than 600° C., and then heated as necessary, and immersed in a hot-dip galvanized coating bath to perform hot-dip galvanized coating.

[0010] According to the present invention, in a method for producing a hot-dip galvanized steel sheet, which comprises annealing a steel sheet and then hot-dip galvanizing the steel sheet, the annealing is carried out in a first step with a high hydrogen concentration and a second step with a low hydrogen concentration, each under specific conditions, thereby producing a hot-dip galvanized steel sheet having an attractive surface appearance free of bare spots and excellent delayed fracture resistance. Furthermore, in the present invention, by carrying out an oxidation treatment before the annealing and then carrying out the annealing under more specific conditions, a hot-dip galvanized steel sheet having even higher levels of coating appearance and excellent delayed fracture resistance can be produced.

[0011] In the present invention, the temperatures specified for the oxidation treatment, annealing, and cooling after annealing are all "steel sheet temperatures." In addition, in the present invention, a non-oxidizing atmosphere refers to an atmosphere in which iron does not oxidize, and is an atmosphere in which selective oxidation of easily oxidizable additive elements such as Si and Mn is acceptable. In addition, in the present invention, a reducing atmosphere refers to an atmosphere in which iron oxide can be reduced to iron. In addition, the type of hot-dip galvanized steel sheet to which the present invention is applicable is not particularly limited as long as it is a plated steel sheet having a plating layer containing zinc as a main component, and includes not only hot-dip galvanized steel sheet (GI) and galvannealed steel sheet (GA), but also hot-dip zinc-aluminum alloy-plated steel sheet, hot-dip zinc-aluminum-silicon alloy-plated steel sheet, hot-dip zinc-aluminum-magnesium alloy-plated steel sheet, and the like, and the detailed coating composition of each is also not limited. In the following description, the units of "%" used for the content of each element in the composition of a steel sheet (also referred to as a base steel sheet or a base steel sheet), the content of each element in the composition of a coating bath, and the degree of alloying of a coating layer are all "mass%," and the units of "%" used for the hydrogen concentration in the atmosphere during annealing and cooling are all "volume%." Furthermore, "high strength" steel sheet means that the tensile strength TS of the steel sheet measured in accordance with JIS Z2241 (2011) is 590 MPa or more.

[0012] The manufacturing method of the present invention is a method for manufacturing a hot-dip galvanized steel sheet, in which a steel sheet is annealed in a non-oxidizing atmosphere and then hot-dip galvanized. The annealing in the non-oxidizing atmosphere includes a first step and a second step. In the first step, the steel sheet is annealed in a reducing atmosphere with a high hydrogen concentration and a predetermined dew point, thereby reducing naturally oxidized Fe present in the surface layer of the steel sheet. In the subsequent second step, the steel sheet is annealed in a non-oxidizing atmosphere with a low hydrogen concentration and a predetermined dew point, thereby releasing hydrogen dissolved in the steel from the steel sheet. The annealed steel sheet is cooled to a predetermined temperature and then immersed in a hot-dip galvanized coating bath to be hot-dip galvanized. The manufacturing method of the present invention also includes a case in which an alloying treatment is performed after hot-dip galvanizing to produce a hot-dip galvannealed steel sheet.

[0013] Furthermore, by performing an oxidation treatment in a predetermined oxidizing atmosphere before annealing to generate Fe oxide in the surface layer of the steel sheet, an even more beautiful surface appearance can be obtained. The steel sheet structure and its chemical composition that serve as the base material of the hot-dip galvanized steel sheet will be described in detail later. In the present invention, the oxidation treatment and the subsequent annealing in a non-oxidizing atmosphere are usually performed in a continuous annealing furnace having, from the entry side, an oxidation zone (a zone for the oxidation treatment), a reducing zone (a zone for the first step of annealing), a soaking zone (a zone for the second step of annealing), and a cooling zone. Here, the oxidation treatment is not an essential step and can be performed appropriately as needed.

[0014] The manufacturing method of the present invention will be described below in the order of oxidation treatment, annealing (first step, second step, cooling after annealing), and hot-dip galvanizing. 2 The temperature of the steel sheet is controlled to 400°C or higher and 900°C or lower in an atmosphere containing 1000 volume ppm or more of O, thereby forming Fe oxide in the surface layer of the steel sheet. 2 Surprisingly N 2 , CO, CO 2 , H 2 It may contain one or more of O and NOx. 2 is an inert gas, CO is a gas for adjusting oxidation and reduction, CO 2 is an inert gas, H 2 O can be contained as a gas for adjusting oxidation and reduction. 2, H 2 O and NOx can be contained as fuel gas, gas derived from the components of the steel sheet being annealed, impurity gas in the atmosphere, or combustion gas of fuel.

[0015] In the present invention, the steel sheet is oxidized by this oxidation treatment and then reduced in the subsequent annealing (first step) to form a reduced iron layer on the surface of the steel sheet, thereby preventing Si and Mn from diffusing into the surface of the steel sheet and being oxidized, thereby further improving the galvanizability. 2 The oxidation treatment in an atmosphere containing 1000 volume ppm or more of O is an extremely important process for achieving both excellent surface quality and excellent delayed fracture resistance at a high level. Furthermore, the improvement effect is particularly remarkable in steels containing 0.1% or more of Si and 1.5% or more of Mn. 2 By setting the concentration to 1000 ppm by volume or more, oxidation of the steel sheet is promoted. 2 If the concentration is less than 1000 ppm by volume, the oxidation of the steel sheet will be insufficient, and oxides of Si and Mn will be formed, which may result in a decrease in platability. 2 , CO, CO 2 , H 2 The oxidation treatment may contain O, NOx, etc., and the ratios thereof are not particularly limited. Although a more beautiful surface appearance can be obtained by the oxidation treatment, this step is not an essential requirement because it is possible to obtain a hot-dip galvanized steel sheet with excellent delayed fracture resistance even without the oxidation treatment.

[0016] In the oxidation treatment, the oxidation of the steel sheet is promoted by setting the steel sheet temperature to 400°C or higher. If the steel sheet temperature is below 400°C, the amount of oxidation is insufficient, resulting in the formation of Si and Mn oxides, which may reduce the effect of improving galvanic properties. On the other hand, if the steel sheet temperature exceeds 900°C, the amount of oxidation of the steel sheet becomes excessive, and reduction may not be completed in the subsequent reduction annealing (first step), resulting in the remaining iron oxide impairing galvanic properties. Therefore, the oxidation treatment is preferably performed at 400°C or higher and 900°C or lower. Here, performing the oxidation treatment at 400°C or higher and 900°C or lower means that the oxidation treatment temperature is at least within the range of 400 to 900°C and does not exceed 900°C. Therefore, within this condition, part of the oxidation treatment may be performed at less than 400°C (for example, when the oxidation treatment is performed during the temperature increase process from 300°C to 700°C). The oxidation treatment is preferably performed for a treatment time of 1 to 30 seconds. That is, from the viewpoint of ensuring a sufficient amount of oxidation and improving plating properties, the treatment time is preferably 1 s or more, more preferably 2 s or more, and even more preferably 3 s or more, whereas from the viewpoint of preventing excessive oxidation and suppressing pick-up, the treatment time is preferably 30 s or less, more preferably 20 s or less, and even more preferably 15 s or less.

[0017] This oxidation treatment can also utilize a process of heating the steel sheet to the annealing temperature. For example, a soaking chamber capable of controlling the atmosphere can be installed during the steel sheet heating process, and the steel sheet surface can be oxidized by maintaining a constant temperature in a predetermined atmosphere. Alternatively, the steel sheet surface can be oxidized by controlling the atmosphere inside a direct-fire heating furnace equipped with a direct-fire burner while increasing the temperature. Simultaneous heating and oxidation treatment can provide industrial advantages, such as a compact furnace and improved production speed. When oxidizing the surface of a steel sheet while heating it, a sufficient amount of oxidation can be achieved by providing an oxidizing atmosphere over a temperature range (temperature range) of 50°C or more after the steel sheet temperature reaches 400°C. If the temperature range in which the steel sheet is exposed to the oxidizing atmosphere is less than 50°C, the amount of oxidation will be insufficient, resulting in the formation of Si and Mn oxides, which will reduce the effectiveness of improving galvanizability. When oxidizing the surface of a steel sheet while heating it, the heating rate within the oxidation temperature range is preferably 3 to 25°C / s to ensure an appropriate amount of oxidation.

[0018] Here, the direct-flame burner used for the oxidation treatment can be a burner that heats the steel sheet by directly applying the burner flame, which is a mixture of fuel such as coke oven gas (COG), a by-product gas from steel mills, and air, to the steel sheet surface. Heating with a direct-flame burner increases the temperature of the steel sheet faster than radiant heating methods, thereby offering the advantage of shortening the furnace length and increasing the steel sheet transport speed. Furthermore, if the direct-flame burner has an air ratio of 0.95 or higher, i.e., a high ratio of air to fuel, unburned oxygen remains in the flame, which can promote the oxidation of the steel sheet. Therefore, adjusting the air ratio makes it possible to control the oxygen concentration in the atmosphere. In addition to COG, liquefied natural gas (LNG), ammonia gas, hydrogen gas, etc. can be used as fuel for the direct-flame burner.

[0019] First Annealing Step In the first annealing step, the steel sheet is held at a temperature of 650°C to 950°C for 20 seconds to 150 seconds in an atmosphere with a dew point of -55°C to +20°C and a hydrogen concentration of 5% to 25% in which the iron oxide is reduced. The natural iron oxide present in the surface layer of the steel sheet is reduced in a reducing atmosphere in the first annealing step to ensure galvanizability. Because the reduction hardly progresses in the subsequent second step in a low-hydrogen-concentration atmosphere, the reduction of the iron oxide must be completed in this first step. This first step is essential for obtaining a good coating appearance. Furthermore, when oxidation treatment is performed, intentionally formed iron oxide is reduced in a reducing atmosphere in the first reduction annealing step to form a reduced iron layer on the surface layer of the steel sheet, preventing Si and Mn from diffusing into the surface layer and oxidizing, thereby further improving the appearance. Similarly, because the reduction hardly progresses in the subsequent second step in a low-hydrogen-concentration atmosphere, the reduction of the iron oxide must be completed in this first step.

[0020] If the annealing temperature of the steel sheet in the first step is less than 650°C, reduction will be insufficient, resulting in roll pickup of iron oxide, which will cause defects in the steel sheet. Furthermore, in the subsequent second step, the iron oxide will not be substantially reduced, resulting in bare spots. On the other hand, if the annealing temperature of the steel sheet exceeds 950°C, the furnace body life will be significantly reduced. Therefore, the annealing temperature of the steel sheet is set to 650°C or higher but not higher than 950°C. When the base material is a cold-rolled steel sheet, the annealing temperature is preferably set to 750°C or higher from the viewpoint of ensuring predetermined strength and ductility through recrystallization. Furthermore, to obtain a high-strength steel sheet with a tensile strength of 780 MPa or higher, it is necessary to ensure a predetermined total area fraction of martensite, bainite, and retained γ (retained austenite), and therefore the annealing temperature is preferably set to 780°C or higher. While a high annealing temperature in the first step promotes selective oxidation of Si and Mn and increases the amount of hydrogen in the steel, the present invention controls the atmosphere and holding time in the first and second steps, thereby achieving excellent surface quality and excellent delayed fracture resistance. When the dew point of the atmosphere in the first step is +20°C or less, it is possible to reduce Fe oxide in the steel sheet surface layer, and selective oxidation of Si and Mn can also be suppressed within a specified annealing time range. Setting the dew point below -55°C requires special equipment for lowering the dew point, which increases costs. On the other hand, if the dew point exceeds +20°C, the dew point distribution in the furnace becomes large, making dew point control difficult and raising concerns about the impact on the furnace body. Therefore, the dew point is set to -55°C or higher and +20°C or lower.

[0021] In the first step, the higher the hydrogen concentration, the faster the reduction of Fe oxide is completed and the more suppressed the selective oxidation of Si and Mn. However, the higher the hydrogen concentration, the more easily hydrogen dissolves in the steel, resulting in a decrease in delayed fracture resistance. If the hydrogen concentration is less than 5%, reduction is insufficient. On the other hand, if the hydrogen concentration exceeds 25%, the reduction effect saturates and a large amount of hydrogen dissolves in the steel, making it difficult to sufficiently reduce the amount of hydrogen in the steel in the subsequent second step. For this reason, the hydrogen concentration in the first step is set to 5% or more and 25% or less. Furthermore, if oxidation treatment is performed, the hydrogen concentration is preferably 8% or more to ensure sufficient reduction. On the other hand, from the viewpoints of running costs and reducing hydrogen in the steel, the hydrogen concentration is preferably 22% or less, and more preferably 18% or less.

[0022] If the holding time in the first step at 650°C or higher but 950°C or lower is less than 20 seconds, reduction will not be fully completed. Furthermore, the area ratio of martensite and bainite required to obtain high-strength steel with a tensile strength of 780 MPa or higher will not be sufficiently secured. On the other hand, since reduction is fully completed with a holding time of 150 seconds or less, a holding time of more than 150 seconds unnecessarily reduces productivity. Furthermore, selective oxidation of Si and Mn progresses, deteriorating surface quality and coating adhesion. The amount of hydrogen in the steel saturates after a holding time of approximately 20 seconds, and the holding time does not have a significant effect. Therefore, the holding time in the first step at 650°C or higher but 950°C or lower is set to 20 seconds or higher but 150 seconds or lower.

[0023] - Second annealing step In the second annealing step, the steel sheet that has undergone the first annealing step is held at a temperature of 700°C to 950°C for 30 seconds to 300 seconds in an atmosphere with a dew point of -50°C to +20°C and a hydrogen concentration of 0.2% to less than 5.0%. In this second step, the steel sheet that has been reduced in the first step is maintained in a low-hydrogen atmosphere, thereby releasing hydrogen from the steel sheet. If the annealing temperature of the steel sheet in the second step is less than 700°C, dehydrogenation is not promoted. On the other hand, if the annealing temperature exceeds 950°C, the furnace body is significantly affected. For this reason, the annealing temperature of the steel sheet is set to 700°C to 950°C. From the viewpoint of reducing the amount of hydrogen in the steel, the annealing temperature in the second step is preferably 860°C or less, and more preferably 830°C or less. Furthermore, in order to obtain a high-strength steel plate having a tensile strength of 780 MPa or more, it is necessary to ensure a predetermined total area ratio of martensite, bainite, and retained γ, and the annealing temperature in the second step is preferably 780°C or more.

[0024] In the second step, the lower the dew point, the less the impact on the furnace body. However, achieving a dew point below −50°C requires special equipment to control the dew point, which increases costs. On the other hand, if the dew point exceeds +20°C, the reduced Fe formed in the first step may reoxidize, impairing galvanic properties. Furthermore, dew point control is difficult, raising concerns about the impact on the furnace body. Therefore, the dew point is set to −50°C or higher and +20°C or lower. From the perspective of controllability, a dew point of +10°C or lower is preferable, and +5°C or lower is more preferable. In the second step, the lower the hydrogen concentration, the more hydrogen dissolved in the steel sheet in the first step is released. However, it is difficult to uniformly control the hydrogen concentration in the furnace to less than 0.2%, and there is a concern that the steel sheet may reoxidize in areas with low hydrogen concentration. Therefore, the hydrogen concentration is set to 0.2% or higher. On the other hand, a hydrogen concentration of 5.0% or higher does not sufficiently reduce the amount of hydrogen in the steel, so the hydrogen concentration is set to less than 5.0%. From the above perspectives, the hydrogen concentration is preferably 1.0% or higher, and more preferably 2.0% or higher. Similarly, the hydrogen concentration is more preferably 4.0% or less.

[0025] If the holding time at 700°C or higher and 950°C or lower in the second step is less than 30 seconds, hydrogen desorption is not fully completed. On the other hand, hydrogen desorption is fully completed with a holding time of 300 seconds or shorter, so a holding time of more than 300 seconds actually reduces productivity. Furthermore, selective oxidation of Si and Mn progresses, deteriorating surface quality and coating adhesion. Therefore, the holding time at 700°C or higher and 950°C or lower in the second step is set to 30 seconds or longer and 300 seconds or shorter. From the viewpoint of fully desorbing hydrogen from the steel, the holding time at 700°C or higher and 950°C or lower in the second step is preferably set to 50 seconds or longer. In the present invention, a high concentration of hydrogen is required to reduce the Fe oxide naturally present on the steel sheet surface or the Fe oxide generated by the oxidation treatment in the first step of annealing. Therefore, a large amount of hydrogen dissolves in the steel. Therefore, a balance between reduction and dehydrogenation is important. Therefore, the conditions for the first and second steps of annealing must be optimized as described above. Although there are no particular restrictions on the method for changing the hydrogen concentration in the first and second annealing steps, it is possible to easily control the atmospheres in the first and second steps individually by dividing a furnace, using furnaces connected via seal rolls, and controlling the hydrogen concentration and dew point of the gas fed into each furnace. In the present invention, it is preferable to anneal the steel sheet using a continuous annealing furnace that is capable of controlling two or more separate different atmospheres.

[0026] Cooling after Annealing: After annealing (second step), the steel sheet is preferably cooled in an atmosphere with a dew point of −20°C or lower and a hydrogen concentration of 5% to 25% in a temperature range from the final holding temperature in the annealing to 600°C at an average cooling rate of 5°C / s or higher, and further cooled to a temperature of 150°C to less than 600°C. The steel sheet is then heated as needed and immersed in a hot-dip galvanized bath for hot-dip galvanizing. Cooling at an average cooling rate of 5°C / s or higher in a temperature range from the final holding temperature after annealing to 600°C can achieve the desired steel sheet strength and inhibit the penetration of hydrogen in the atmosphere into the steel sheet during cooling. An average cooling rate of less than 5°C / s tends to decrease the steel sheet strength and also tends to decrease the delayed fracture resistance due to the penetration of hydrogen in the atmosphere into the steel sheet. Here, the final holding temperature in the second step of annealing refers to the temperature at which a steel sheet annealed within ranges satisfying the annealing temperature, hydrogen concentration, dew point, and holding time requirements of the second step of annealing does not satisfy at least one of the requirements. The average cooling rate (°C / s) is obtained by dividing the difference between the cooling start temperature (the final holding temperature) (°C) and the cooling end temperature (600°C) by the cooling time (s).

[0027] Regarding the cooling zone atmosphere, hydrogen has a high cooling capacity, so the higher the hydrogen concentration in the atmosphere, the faster the cooling rate can be. However, if the hydrogen concentration is too high, hydrogen may penetrate into the steel sheet during cooling. Therefore, the hydrogen concentration is preferably 5% or more and 25% or less. A hydrogen concentration of less than 5% may not ensure a sufficient cooling rate, which may result in a decrease in steel sheet strength. Furthermore, a decrease in cooling rate may lead to increased hydrogen penetration during cooling, which may also lead to a decrease in delayed fracture resistance. On the other hand, if the hydrogen concentration exceeds 25%, the effect saturates, and even if the cooling rate is fast, hydrogen may penetrate into the steel sheet during cooling, which may lead to a decrease in delayed fracture resistance. Furthermore, by setting the dew point to −20°C or less, it is possible to prevent the steel sheet from reoxidizing at low temperatures and thereby reducing its galvanizability. That is, if the dew point exceeds −20°C, the steel sheet may reoxidize at low temperatures and thus reduce its galvanizability.

[0028] Hot-dip galvanizing conditions are not particularly limited, and typical conditions may be used. That is, preferably, the steel sheet is cooled to a temperature of 150°C or higher but lower than 600°C under the conditions described above, and then heated to the bath temperature as needed. The steel sheet is then immersed in a hot-dip galvanizing bath for coating. For GA and GI, the coating bath typically contains Zn, Al, and unavoidable impurities. While the composition is not specifically specified, the Al concentration in the bath is generally about 0.05% or higher and 0.190% or lower. An Al concentration of less than 0.05% increases the occurrence of bottom dross, which adheres to the steel sheet and easily becomes a defect. On the other hand, an Al concentration of more than 0.190% increases the occurrence of top dross, which also adheres to the steel sheet and easily becomes a defect. The addition of Al also increases costs. The hot-dip galvanizing bath temperature is typically about 440 to 500°C.

[0029] There is no particular limitation on the amount of coating per side by hot dip galvanizing, but it is generally 25 to 80 g / m 2 The coating weight per side is controlled to about 25 g / m 2 If the thickness is less than 80 g / m, not only is the corrosion resistance liable to decrease, but it is also difficult to control the coating weight. 2 If the alloying degree exceeds 7%, the coating adhesion is likely to decrease. There are no particular restrictions on the method for adjusting the coating weight, but gas wiping is generally used, and adjustment is made by adjusting the gas pressure of the gas wiping, the distance between the wiping nozzle and the steel sheet, etc. When alloying treatment is performed after hot-dip galvanizing, there are no particular restrictions on the degree of alloying of the coating layer after the alloying treatment, but generally, an alloying degree of about 7 to 15% is preferred. If the alloying degree is less than 7%, the η phase will remain and press formability will likely decrease, while if it exceeds 15%, the coating adhesion will likely decrease.

[0030] Next, the base steel sheet of the hot-dip galvanized steel sheet will be described. The base steel sheet may be either a cold-rolled steel sheet or a hot-rolled steel sheet. Furthermore, since delayed fracture resistance is a problematic characteristic of high-strength steel sheets, the steel sheet is preferably a high-strength steel sheet having a tensile strength TS of 590 MPa or more, preferably 780 MPa or more, and more preferably 980 MPa or more. The composition of the base steel sheet is not particularly limited as long as it is within the composition range of ordinary cold-rolled steel sheets or hot-rolled steel sheets, but the following composition is preferred. Furthermore, the thickness of the steel sheet is not particularly limited, but is generally about 0.5 to 3.2 mm.

[0031] A preferred composition of the base steel sheet will be described below.

[0032] C: 0.8% or less (excluding 0%) C has the effect of improving workability by forming martensite or the like as a steel structure, but in order to obtain good weldability, the C content is preferably 0.8% or less, and more preferably 0.3% or less. There is no particular lower limit for the C content, but in order to obtain good workability, the C content is preferably 0.03% or more, and more preferably 0.05% or more.

[0033] Si: 3.0% or less (excluding 0%) Si is an effective element for achieving high strength in steel sheets because it has a significant effect of increasing the strength of steel through solid solution (solid solution strengthening ability) without significantly impairing workability. On the other hand, Si is also an element that adversely affects the resistance weld cracking resistance characteristics of welds. When Si is contained to increase the strength of steel sheets, a content of 0.1% or more is preferable. On the other hand, if the Si content exceeds 3.0%, the hot rolling property and cold rolling property are significantly reduced, which may adversely affect productivity or lead to a decrease in the ductility of the steel sheets themselves. For this reason, it is preferable that Si be contained in a range of 3.0% or less. From this viewpoint, the Si content is more preferably 2.5% or less, and particularly preferably 2.0% or less.

[0034] Mn: 1.3% or more and 3.5% or less Mn is an element that strengthens steel through solid solution strengthening, improves hardenability, and promotes the formation of residual γ, bainite, and martensite. These effects are achieved by including 1.3% or more of Mn. Therefore, the Mn content is preferably 1.3% or more, and more preferably 1.8% or more. On the other hand, if the Mn content is 3.5% or less, the above effects can be achieved without increasing costs. Therefore, the Mn content is preferably 3.5% or less, and more preferably 3.3% or less.

[0035] P: 0.1% or less (excluding 0%). By suppressing the P content, it is possible to prevent a decrease in weldability, and further, it is possible to prevent P from segregating at grain boundaries, thereby preventing deterioration in ductility, bendability, and toughness. Furthermore, if a large amount of P is contained, the ferrite transformation is promoted, which increases the grain size. Therefore, it is preferable that the P content be 0.1% or less. There is no particular lower limit for the P content, but it is usually preferable to set it to 0.001% or more due to constraints on production technology.

[0036] S: 0.03% or less (excluding 0%) It is preferable to reduce the S content as much as possible. By suppressing the S content, deterioration in weldability can be prevented, and deterioration in ductility during hot rolling can be prevented, thereby suppressing hot cracking and significantly improving surface properties. Furthermore, by suppressing the S content, deterioration in delayed fracture resistance, ductility, bendability, and stretch flangeability of the steel sheet due to the formation of coarse sulfides as an impurity element can be prevented. Since the problems caused by S become significant when the S content exceeds 0.03%, the S content is preferably 0.03% or less, and more preferably 0.02% or less. From the viewpoint of improving delayed fracture resistance, the S content is preferably 0.01% or less, and more preferably 0.003% or less. Although the lower limit of the S content is not particularly limited, it is usually preferable to set it to 0.0001% or more due to constraints on production technology.

[0037] N: 0.010% or less (excluding 0%) By setting the N content to 0.010% or less, it is possible to prevent N from forming coarse nitrides with Ti, Nb, and V at high temperatures, thereby preventing the effect of increasing the strength of the steel sheet due to the addition of Ti, Nb, and V from being impaired. Furthermore, by setting the N content to 0.010% or less, it is possible to prevent a decrease in toughness. Furthermore, by setting the N content to 0.010% or less, it is possible to prevent the occurrence of slab cracks and surface defects during hot rolling. For this reason, the N content is preferably set to 0.010% or less, more preferably 0.005% or less, even more preferably 0.003% or less, and particularly preferably 0.002% or less. There is no particular restriction on the lower limit of the N content, but it is usually preferable to set it to 0.0005% or more due to constraints on production technology.

[0038] Al: 0.1% or less. Because Al is thermodynamically most easily oxidized, it oxidizes before Si and Mn, suppressing the oxidation of Si and Mn at the outermost layer of the steel sheet and promoting the oxidation of Si and Mn inside the steel sheet. This effect is achieved when the Al content is 0.01% or more. On the other hand, an Al content exceeding 0.1% increases costs. Therefore, when Al is contained, the Al content is preferably 0.1% or less. Although there is no particular lower limit for the Al content, removing impurity-level Al also increases costs, so it is preferably 0.001% or more. As mentioned above, the Al content is preferably 0.01% or more.

[0039] The steel plate may further contain, as necessary, one or more elements selected from B: 0.005% or less, Ti: 0.2% or less, Cr: 1.0% or less, Nb: 0.20% or less, Mo: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Sb: 0.20% or less, V: 0.5% or less, Ta: 0.1% or less, W: 0.5% or less, Zr: 0.1% or less, Sn: 0.20% or less, Ca: 0.005% or less, Mg: 0.005% or less, and REM: 0.005% or less.

[0040] B: 0.005% or less B is an element effective in improving the hardenability of steel. To improve hardenability, the B content is preferably 0.0003% or more, and more preferably 0.0005% or more. However, since an excessive B content reduces formability, the B content is preferably 0.005% or less.

[0041] Ti: 0.2% or less Ti is an element effective for precipitation strengthening of steel. There is no particular limitation on the lower limit of Ti, but in order to obtain the effect of adjusting strength, it is preferable to set it to 0.005% or more. However, if Ti is added in excess, the hard phase becomes excessively large and formability decreases, so when Ti is contained, the Ti content is preferably set to 0.2% or less, and more preferably 0.05% or less.

[0042] Cr: 1.0% or less When 0.005% or more of Cr is contained, hardenability is improved and the balance between strength and ductility can be improved. However, from the viewpoint of preventing an increase in costs, the Cr content is preferably 1.0% or less.

[0043] Nb: 0.20% or less Although the effect of improving strength can be obtained by including 0.005% or more of Nb, from the viewpoint of preventing an increase in costs, the Nb content is preferably 0.20% or less.

[0044] Mo: 1.0% or less When Mo is contained in an amount of 0.005% or more, the strength adjusting effect is obtained, and this effect is particularly enhanced when the Mo content is 0.05% or more. However, from the viewpoint of preventing an increase in costs, the Mo content is preferably 1.0% or less.

[0045] Cu: 1.0% or less When Cu is contained in an amount of 0.005% or more, the formation of residual gamma phase can be promoted. However, from the viewpoint of preventing an increase in costs, when Cu is contained, the Cu content is preferably 1.0% or less.

[0046] Ni: 1.0% or less When Ni is contained in an amount of 0.005% or more, the formation of residual gamma phase can be promoted. However, from the viewpoint of preventing an increase in costs, when Ni is contained, the Ni content is preferably 1.0% or less.

[0047] Sb: 0.20% or less Sb can be added from the viewpoint of suppressing nitriding and oxidation of the steel sheet surface, or decarburization of the steel sheet surface in a region of several tens of microns caused by oxidation. By suppressing nitriding and oxidation of the steel sheet surface, Sb prevents a decrease in the amount of martensite formed on the steel sheet surface, improving the fatigue properties and surface quality of the steel sheet. To achieve this effect, the Sb content is preferably 0.001% or more. On the other hand, to obtain good toughness, the Sb content is preferably 0.20% or less.

[0048] V: 0.5% or less When V is contained in an amount of 0.005% or more, the effect of improving strength can be obtained. However, from the viewpoint of preventing an increase in costs, when V is contained, the V content is preferably 0.5% or less.

[0049] Ta: 0.1% or less When Ta is contained in an amount of 0.001% or more, the effect of improving strength can be obtained. However, from the viewpoint of preventing an increase in costs, when Ta is contained, the Ta content is preferably 0.1% or less.

[0050] W: 0.5% or less When W is contained in an amount of 0.005% or more, the effect of improving strength can be obtained. However, from the viewpoint of preventing an increase in costs, when W is contained, the W content is preferably 0.5% or less.

[0051] Zr: 0.1% or less When Zr is contained in an amount of 0.0005% or more, the effect of improving strength can be obtained. However, from the viewpoint of preventing an increase in costs, when Zr is contained, the Zr content is preferably 0.1% or less.

[0052] Sn: 0.20% or less Sn is an element that is effective in suppressing denitrification, deboronation, etc., and thus suppressing a decrease in the strength of steel, and in order to obtain such an effect, it is preferable that the Sn content be 0.002% or more. On the other hand, when Sn is contained, in order to obtain good impact resistance, the Sn content is preferably 0.20% or less.

[0053] Ca: 0.005% or less When Ca is contained in an amount of 0.0005% or more, the morphology of sulfides can be controlled and ductility and toughness can be improved. However, from the viewpoint of obtaining good ductility, when Ca is contained, the Ca content is preferably 0.005% or less.

[0054] Mg: 0.005% or less When Mg is contained in an amount of 0.0005% or more, the morphology of sulfides can be controlled and ductility and toughness can be improved. However, from the viewpoint of preventing an increase in costs, when Mg is contained, the Mg content is preferably 0.005% or less.

[0055] REM: 0.005% or less When REM is contained in an amount of 0.0005% or more, the morphology of sulfides can be controlled and ductility and toughness can be improved. However, from the viewpoint of obtaining good toughness, when REM is contained, the REM content is preferably 0.005% or less.

[0056] The remainder of the steel sheet other than the above-mentioned component composition is Fe and unavoidable impurities.

[0057] The structure of the base steel sheet (substrate steel sheet) is not particularly limited, but in order to ensure a tensile strength of 780 MPa or more, it is preferable to have the following steel sheet structure. That is, it is preferable to set the total area ratio of martensite, bainite, and retained γ (retained austenite) to 30% or more, thereby obtaining a base steel sheet with a tensile strength of 780 MPa or more. Furthermore, by setting the total area ratio of martensite, bainite, and retained γ to 50% or more, it is possible to obtain a base steel sheet with a tensile strength of 980 MPa or more. The hot-dip galvanized steel sheet produced according to the present invention has a low hydrogen concentration in the substrate steel sheet and excellent delayed fracture resistance. In particular, it is preferable that the hydrogen concentration (however, the amount of diffusible hydrogen) in the substrate steel sheet is 0.30 ppm by mass or less, and it is particularly preferable that it is 0.25 ppm by mass or less. Here, the amount of diffusible hydrogen refers to the amount of hydrogen in the steel sheet measured by the method described in the Examples below.

[0058] Steel having the chemical composition shown in Table 1 was melted and cast into a slab, which was then hot-rolled, pickled, and cold-rolled to form a cold-rolled steel sheet with a thickness of 1.2 mm. This cold-rolled steel sheet was used as the base steel sheet for the hot-dip galvanized steel sheet. In a CGL equipped with an all-radiant tube (ART) annealing furnace, the steel sheet was annealed under the conditions shown in Tables 2 and 3, and then hot-dip galvanized (coating composition: Zn-0.2 mass% Al) and gas-wiped to a coating weight per side of approximately 50 g / m. 2 Separately from the above examples, steel sheets were oxidized and annealed under the conditions shown in Tables 4 to 9 in a CGL equipped with a DFF-type annealing furnace, and then hot-dip galvanized (coating composition: Zn-0.2 mass% Al) and gas-wiped to a coating weight per side of approximately 50 g / m 2 The temperature was adjusted to 100°C, and then, for some examples, an alloying treatment was performed. Note that No. 3 (Tables 4 and 5) is an example in which oxidation treatment was performed at a constant temperature, and the holding time (treatment time) of the oxidation treatment was 8 seconds. For the other examples, the oxidation treatment was performed during temperature increase, and the temperature increase rate of this oxidation treatment was in the range of 5 to 20°C / s.

[0059] The hot-dip galvanized steel sheets thus obtained were subjected to measurement of the amount of diffusible hydrogen in the steel sheets and evaluation of the coating appearance and delayed fracture resistance using the following measurement and evaluation methods. The results, along with the manufacturing conditions, are shown in Tables 2 to 9. In the oxidation treatments of the Examples in Tables 4 to 9, the "oxidation start temperature" refers to the sheet temperature at the entry side of the oxidation zone in the heating zone of a DFF annealing furnace, the "oxidation end temperature" refers to the sheet temperature at the exit side of the oxidation zone, and the oxygen concentration refers to the oxygen concentration in the oxidation zone. Therefore, the range from the oxidation start temperature to the oxidation end temperature is the oxidation treatment temperature. Furthermore, the "oxidation temperature range" refers to the temperature range over which the steel sheet rises in the oxidation zone (the temperature range from the oxidation start temperature to the oxidation end temperature), and the "maximum steel sheet temperature" refers to the maximum steel sheet temperature in the heating zone of a DFF annealing furnace. Therefore, if the "maximum steel sheet temperature" is higher than the "oxidation end temperature," this indicates that the steel sheet was further heated in a non-oxidizing atmosphere in the zone next to the oxidation zone (a zone other than the oxidation zone).

[0060] Measurement of the amount of diffusible hydrogen in steel sheet (hydrogen analysis method) A rectangular test piece measuring 30 mm in major axis length and 5 mm in minor axis length was taken from the width center of a hot-dip galvanized steel sheet. The coating layer of the test piece was removed using a router. Immediately, hydrogen analysis was performed using a thermal desorption analyzer under conditions of an analysis start temperature of 25°C, an analysis end temperature of 300°C, and a heating rate of 200°C / hour. The amount of released hydrogen (mass ppm / min), which is the amount of hydrogen released from the surface of the test piece at each temperature, was measured. The total amount of released hydrogen from the analysis start temperature to 300°C was calculated as the amount of diffusible hydrogen in the steel. Here, a steel with a diffusible hydrogen content of 0.25 mass ppm or less was evaluated as excellent (⊚), and a steel with a diffusible hydrogen content of more than 0.25 mass ppm but not more than 0.30 mass ppm was evaluated as good (◯). From experience, when the amount of diffusible hydrogen in steel exceeds 0.30 ppm by mass, the delayed fracture resistance property is often reduced, and therefore, steels having a diffusible hydrogen content of more than 0.30 ppm by mass were rated as poor ("x").

[0061] - Evaluation of plating appearance The plating appearance of hot-dip galvanized steel sheets was visually observed, and those with no visible patterns or irregularities were rated as excellent (◎), those with patterns or irregularities but no unplated defects or indentations caused by picking up on the rolls were rated as good (○+), and those with unplated defects or indentations caused by picking up on the rolls were rated as poor (×). Furthermore, those without unplated defects or indentations caused by picking up on the rolls but with a scale pattern in the shape of a V mark in the sheet running direction as a sign of such defects were rated as passing (○), although not good (○+).

[0062] Tensile Test Test specimens were taken from the hot-dip galvanized steel sheet in a direction perpendicular to the rolling direction (so that the sheet width direction was the tensile direction), and a tensile test was performed on these test specimens in accordance with JIS Z2241 (2011) to measure the tensile strength (TS).

[0063] Observation and Measurement of Base Steel Sheet Microstructure The total area ratios of martensite, bainite, and retained γ in the base steel sheet microstructure were measured as follows. A sample was cut so that the observation surface was a thickness cross section (L cross section) parallel to the rolling direction of the steel sheet. This observation surface was polished with diamond paste and then finish-polished with alumina. The observation surface of the sample was then etched with 3 vol% nital to reveal the microstructure. The observation position on this sample observation surface was a quarter of the sheet thickness, and five fields of view were observed using an SEM at a magnification of 3000x. The total area of ​​martensite, bainite, and retained γ was calculated from the obtained microstructure images, and the area ratio was calculated by dividing this total area by the measured area for each of the five fields. The average of these values ​​was used as the total area ratio of martensite, bainite, and retained γ. The martensite, bainite, retained γ, and other microstructures were identified as follows. Martensite: There are two types of martensite: tempered martensite and fresh martensite. Tempered martensite is represented by gray or dark gray areas close to black in SEM photographs. Tempered martensite exhibits a massive morphology with boundaries at prior γ grain boundaries and interfaces with other structures such as ferrite. However, tempered martensite may contain other structures such as bainite, resulting in a concave shape. Tempered martensite contains many carbides, but depending on the plane orientation, the amount of carbides may be small. Fresh martensite is represented by gray or white areas in SEM photographs. Fresh martensite is massive, granular, plate-like, or film-like, and does not contain carbides. Bainite is represented by dark gray areas in SEM photographs. Bainite exhibits the morphology of film-like, plate-like, or massive morphology in which some or all of these adjacent regions are connected, and contains a small amount of carbides. Bainite also includes bainite that has been tempered after formation to coarsen the carbides. Residual γ is a region that has the same color and shape as the above-mentioned fresh martensite. Note that retained γ and fresh martensite cannot be distinguished using an SEM.

[0064] To ensure the strength of the steel plate, the total area ratio of martensite, bainite, and retained γ must be controlled. However, the remainder may include the following structures, but is not limited to these. Ferrite: Ferrite is the black area in the SEM photograph. Ferrite has a massive morphology and contains almost no carbides. Bainitic ferrite contains almost no carbides internally and has mechanical properties similar to ferrite, so it belongs to the ferrite group. Ferrite may contain granular or massive fresh martensite, granular or massive retained γ, or both. Carbide: Carbide is the white area in the SEM photograph. Carbide has a granular or film-like morphology. Carbide mainly forms finely inside ferrite, martensite, and bainite. Therefore, the area ratio of carbide is not excluded from the area ratio of each structure, but is included in the area ratio of each structure.・Structures other than those mentioned above In addition to the above, nitrides such as TiN, carbonitrides such as (Nb,Ti)(C,N), sulfides such as MnS and CaS, Al 2 O 3 , SiO 2 The total area percentage of oxides such as tungsten and tantalum may also be a few percent. Since the area percentages of these are small, these area percentages are included in the area percentages of each structure containing them. Pearlite may also be included. The area percentage of pearlite is calculated.

[0065] Here, the size and abundance of each structure are not particularly limited, but as one embodiment of the present invention, the following sizes and abundances can be exemplified. The aspect ratio is the ratio of the length of the major axis to the length of the minor axis perpendicular to the major axis, the thickness is the length of the minor axis, and the circle equivalent diameter is the diameter when the area of ​​each structure is taken as the area of ​​a circle. Tempered martensite: Aspect ratio ≦8, circle equivalent diameter ≦30 μm Distribution density of carbides inside the structure: 0.10 to 12 pieces / μm 2Fresh martensite and residual γ Lumpy: Aspect ratio ≦8, equivalent circle diameter: 3 to 30 μm Granular: Aspect ratio ≦8, equivalent circle diameter: 0.40 μm or more, less than 3 μm Plate or film: Aspect ratio greater than 8, Thickness: 0.10 to 8 μm Bainite Film or plate: Aspect ratio greater than 8, Thickness ≦8 μm Lumpy: Aspect ratio ≦8, equivalent circle diameter ≦30 μm Distribution density of carbides within the structure: 0.10 to 6 particles / μm in all forms 2 Carbide Granular: Aspect ratio ≦ 8, Equivalent circle diameter: 0.01 μm or more, less than 0.40 μm Film-like: Aspect ratio greater than 8, Equivalent circle diameter: 0.01 μm or more, less than 0.10 μm

[0066] Evaluation of Delayed Fracture Resistance: A rectangular test specimen with a major axis length of 100 mm and a minor axis length of 20 mm was taken from the hot-dip galvanized steel sheet in the direction perpendicular to the rolling direction. A punched hole with a diameter of 15 mm and a clearance of 12.5% ​​was formed at the center of the major and minor axes of the test specimen. The test specimen was subjected to a tensile test, and the delayed fracture resistance was evaluated based on whether or not delayed fracture occurred through the punched hole. To prevent the release of diffusible hydrogen in the steel due to aging, the time from taking the rectangular test specimen from the hot-dip galvanized steel sheet to starting the delayed fracture tensile test (tensile speed: 10 mm / min) was limited to within 10 minutes. The loading time in the tensile test was a maximum of 100 hours. The maximum stress at which no cracks (here, "cracks" refers to fractures under tensile stress loading) occurred after 100 hours of loading was defined as the critical stress, and the delayed fracture resistance was evaluated by the ratio of the critical stress to the yield stress. The evaluation criteria for delayed fracture resistance were as follows: when the critical stress / yield stress was 1.10 or more, it was given an excellent "◎", when it was less than 1.10 and 1.05 or more, it was given a good "◯", when it was less than 1.05 and 1.00 or more, it was given a pass "△" although it was not good (◯), and when it was less than 1.00, it was given a poor "×". Note that the delayed fracture resistance evaluated in the delayed fracture test is generally lower (disadvantageous) for steel sheets with higher strength.

[0067] According to Tables 2 to 9, the hot dip galvanized steel sheets of the present invention have a beautiful surface appearance with no unplated areas, and also have excellent delayed fracture resistance.

[0068]

[0069]

[0070]

[0071]

[0072]

[0073]

[0074]

[0075]

[0076]

Claims

1. A method for producing a hot-dip galvanized steel sheet, in which a steel sheet is annealed in a non-oxidizing atmosphere in a continuous annealing furnace and then hot-dip galvanized (however, including the case where an alloying treatment is performed after the hot-dip galvanized plating), the annealing includes a first step of holding the steel sheet at a temperature of 650°C to 950°C in an atmosphere with a dew point of -55°C to +20°C and a hydrogen concentration of 5 to 25% by volume for a period of 20 to 150 seconds, and a second step of holding the steel sheet that has been subjected to the first step at a temperature of 700°C to 950°C in an atmosphere with a dew point of -50°C to +20°C and a hydrogen concentration of 0.2 to less than 5.0% by volume for a period of 30 to 300 seconds.

2. The steel sheet before the annealing is subjected to O 2 The method for producing a hot-dip galvanized steel sheet according to claim 1, further comprising the step of carrying out an oxidation treatment at a temperature of 400° C. or higher and 900° C. or lower in an atmosphere containing 1000 ppm by volume or more of 3. The method for producing a hot-dip galvanized steel sheet according to claim 2, wherein the oxidation treatment is carried out during the process of increasing the temperature of the steel sheet for the annealing.

4. The method for producing a hot-dip galvanized steel sheet according to claim 3, wherein the oxidation treatment is carried out over a temperature rise range of 50°C or more in the process of raising the temperature of the steel sheet for the annealing.

5. The method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 4, wherein the atmosphere in the first annealing step has a hydrogen concentration of 8 volume % or more.

6. The method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 5, wherein the atmosphere in the second annealing step has a hydrogen concentration of 2.0 volume % or more.

7. A method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 6, wherein the hydrogen concentration (however, the amount of diffusible hydrogen) in the base steel sheet of the produced hot-dip galvanized steel sheet is 0.30 mass ppm or less.

8. A method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 7, wherein the Si content of the base steel sheet is 0.1 mass% or more.

9. The method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 8, wherein the total area ratio of martensite, bainite and residual γ in the base steel sheet is 30% or more, and the tensile strength is 780 MPa or more.

10. The method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 8, wherein the total area ratio of martensite, bainite and residual γ in the base steel sheet is 50% or more, and the tensile strength is 980 MPa or more.

11. A method for producing a hot-dip galvanized steel sheet according to any one of claims 1 to 10, comprising cooling the steel sheet subjected to the annealing at an average cooling rate of 5°C / s or more in a temperature range from the final holding temperature in the annealing to 600°C in an atmosphere having a dew point of -20°C or less and a hydrogen concentration of 5 to 25% by volume, and further cooling to a temperature of 150°C or more but less than 600°C, heating the steel sheet as necessary, and immersing the steel sheet in a hot-dip galvanized plating bath to perform hot-dip galvanization.

Citation Information

Patent Citations

  • Image generation apparatus, image generation method, and image generation program

    JP2025130443A

  • Manufacturing method of hot-dip galvanized steel sheet without coating blisters

    JP3266008B2

  • Manufacturing method for Si-containing high-strength alloyed hot-dip galvanized steel sheet

    JP5811841B2

  • Manufacture of hot dip aluminized steel sheet

    JP1994158255A

  • Manufacturing method of hot dip galvanized steel sheet

    JP2018188717A