Method for producing high-strength hot-dip galvanized steel sheet
The method optimizes the production of high-strength hot-dip galvanized steel sheets by controlled oxidation and reduction annealing, addressing weld cracking and delayed fracture issues through enhanced LME cracking resistance and reduced hydrogen embrittlement, ensuring both strength and appearance quality for automotive applications.
Patent Information
- Application Number
- PCT/JP2023/016785
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-31
AI Technical Summary
High-strength hot-dip galvanized steel sheets face challenges with resistance weld cracking resistance and delayed fracture due to residual stress and hydrogen embrittlement, particularly when high levels of C and Si are added, leading to liquid metal embrittlement and brittle fractures.
A method involving controlled oxidation and reduction annealing of steel sheets with specific temperature and atmosphere conditions to optimize Si and Mn content, reducing hydrogen concentration, and using a two-stage reduction annealing process to form low solid solution Si and C layers, enhancing LME cracking resistance and suppressing delayed fracture.
The method produces high-strength hot-dip galvanized steel sheets with excellent resistance weld cracking resistance and improved delayed fracture resistance, maintaining appearance quality and reducing hydrogen-induced embrittlement, suitable for lightweight and strong automobile bodies.
Smart Images

Figure JP2023016785_31102024_PF_FP_ABST
Abstract
Description
Manufacturing method for high-strength hot-dip galvanized steel sheet
[0001] The present invention relates to a method for producing a high-strength hot-dip galvanized steel sheet having excellent resistance weld cracking resistance and delayed fracture resistance.
[0002] In recent years, there has been a strong demand for improved automobile fuel efficiency from the perspective of protecting the global environment. Furthermore, there has also been a strong demand for improved automobile safety from the perspective of ensuring the safety of passengers in the event of a collision. To meet these demands, it is necessary to achieve both weight reduction and high strength in automobile bodies. Therefore, in the case of hot-dip galvanized steel sheets, which are used as raw materials for automobile parts, efforts are being made to reduce the thickness of steel sheets by increasing their strength. However, since many automobile parts are manufactured by forming steel sheets, these steel sheets are required to have excellent formability in addition to high strength.
[0003] There are various methods for increasing the strength of hot-dip galvanized steel sheets. Methods that can increase the strength of hot-dip galvanized steel sheets without significantly impairing their formability include utilizing martensite by adding C and solid-solution strengthening by adding Si. Meanwhile, in the manufacture of automotive parts, press-formed parts are often assembled by resistance welding (spot welding). If a steel sheet contains a large amount of C or Si, residual stress is generated near the weld during resistance welding. This causes zinc in the coating layer to melt and diffuse into the grain boundaries, potentially resulting in liquid metal embrittlement (LME), which can lead to intergranular cracking (LME cracking) in the steel sheet. In particular, when welding is performed with a welding electrode angled relative to the steel sheet, the residual stress increases, potentially leading to cracking. Since residual stress is thought to increase as the strength of the steel sheet increases, LME cracking is a concern.
[0004] Furthermore, it is known that as the strength of steel increases, delayed fracture due to hydrogen embrittlement becomes more likely to occur. This tendency is particularly pronounced in high-strength steels with a tensile strength of 1180 MPa or more. Delayed fracture is a phenomenon in which high-strength steel is subjected to a static load stress (a load stress less than the tensile strength) and, after a certain period of time, suddenly undergoes brittle fracture without any apparent plastic deformation. While this delayed fracture is often caused by hydrogen that penetrates into the steel sheet due to corrosion caused by the operating environment, hydrogen that penetrates into the steel sheet during the annealing process of a continuous hot-dip galvanizing line (CGL) can also deteriorate the mechanical properties of steel sheets, particularly those with a tensile strength of 980 MPa or more, leading to brittle fracture.
[0005] As described above, there is a demand for high-strength steel sheets that are excellent in resistance weld cracking resistance (hereinafter also simply referred to as "LME cracking resistance") and that suppress deterioration of delayed fracture resistance caused by hydrogen in the steel.
[0006] Conventionally, as a method for improving uncoated defects that occur in Si-added steel, Patent Document 1 discloses a method for improving the coating quality by using O 2 The surface of the Si-added steel is oxidized by heating it to 700°C or higher in an atmosphere containing 2 Patent Document 2 discloses a method of reducing the catalyst in an atmosphere containing O 2 The surface of the Si-added steel is oxidized by heating to 600°C or higher and 850°C or lower in an atmosphere containing 2 O and H 2 Patent Document 3 also discloses a method for reducing oxidized steel sheet in an atmosphere containing Si. The method increases the air ratio in a direct fired furnace (DFF) to oxidize the surface of Si-added steel and reduce the oxides in the surface layer of the steel sheet by log(P H2O / P H2) is -3.4 or more and -1.1 or less. However, although these methods make it possible to adjust the amount of oxidation of the steel sheet and ensure good appearance quality, they have the problem that they are unable to obtain sufficient resistance to LME cracking and delayed fracture due to the suppression of LME cracking that occurs in Si-added steel and the presence of a large amount of hydrogen that has penetrated into the steel during annealing.
[0007] Patent No. 5652219 Patent No. 6052270 Patent No. 6172297
[0008] Therefore, an object of the present invention is to provide a high-strength hot-dip galvanized steel sheet that ensures the appearance quality of the steel sheet, has excellent LME cracking resistance, and can simultaneously suppress deterioration of delayed fracture resistance due to hydrogen embrittlement.
[0009] The present inventors have investigated the O 2 By appropriately controlling the concentration and temperature, the appearance quality of the steel sheet is ensured. 2 O concentration, H 2 The inventors have found that optimizing the concentration makes it possible to achieve excellent resistance weld cracking resistance and simultaneously suppress deterioration of delayed fracture resistance due to hydrogen embrittlement, and have completed the present invention.
[0010] The present invention has been made based on the above findings. That is, the gist and configuration of the present invention are as follows.
[0011] [1] A method for producing a high-strength hot-dip galvanized steel sheet, comprising oxidizing a steel sheet containing, by mass%, Si: 0.45% to 2.0%, followed by reduction annealing and hot-dip galvanizing, wherein in the oxidation treatment, N 2 and 500 ppm by volume or more of O 2 The steel sheet is oxidized in an oxidation step in a temperature range of 500°C to 800°C in an atmosphere containing 2In the second reduction annealing step, the steel sheet after the first reduction annealing is subjected to an annealing atmosphere having a dew point of −10° C. or higher and +20° C., in which hydrogen is added in an amount of 2.0% by volume or higher and 8.0% by volume or lower, and the balance is N. 2 and the hydrogen concentration in the first reduction annealing in the previous stage is H 2 a, the hydrogen concentration in the second reduction annealing in the latter stage is H 2 When b is set, H 2 a>H 2
[0014] A method for producing a high-strength hot-dip galvanized steel sheet, comprising holding the steel sheet at a temperature of 700°C or higher and 950°C or lower for 30 seconds or lower and 300 seconds or lower in an atmosphere having a hydrogen concentration adjusted to satisfy b, followed by hot-dip galvanizing. [2] A method for producing a high-strength hot-dip galvanized steel sheet according to [1], wherein the reduction annealing is performed using an annealing furnace that is divided into two or more sections in the running direction of the steel sheet and is capable of annealing in two or more different atmospheres. [3] A method for producing a high-strength hot-dip galvanized steel sheet according to [1] or [2], wherein the steel sheet is hot-dip galvanized and then subjected to an alloying treatment for hot-dip galvanizing. [4] A method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to [3], wherein the oxidation treatment is performed in a temperature-raising step of the steel sheet that is performed as a pre-step of reduction annealing. [5] A method for producing a high-strength hot-dip galvanized steel sheet according to [4], wherein the oxidation treatment is performed in a temperature range of at least 50°C or higher, from 500°C to 800°C. [6] The method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to [5], wherein the oxidation treatment is performed using a direct-fired heating furnace (DFF), and the steel sheet surface is oxidized by setting the air ratio of at least a part of the atmosphere in the heating furnace to 1.0 or more. [7] The oxidation treatment is performed using a direct-fired heating furnace that is divided into two or more parts in the running direction of the steel sheet and is capable of oxidizing in two or more atmospheres, and in a first heating zone in the front stage of the heating furnace, when the air ratio in the temperature range where the oxidation treatment is performed is α, the oxidation treatment is performed by setting the air ratio of the temperature range where the oxidation treatment is performed to 200°C or more, and setting the average heating rate at 200°C or more to 10°C / s or more and 50°C / s or less .... 1 In the second heating zone at the rear of the heating furnace, the steel sheet that has passed through the first heating zone is heated to a temperature of 0.9 or more, and the air ratio is 0.9 or less, and the T 1 (°C) is calculated from the following formula (2) under the condition that the average heating rate is 5°C / sec or more and 30°C / sec or less. 2The method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to [6], wherein the steel sheet is heated to a temperature of at least T 1 =28.2[Si]+7.95[Mn]-86.2α+666 ---(1) T 2 =T 1 +30 --- (2) where [Si] is the Si content (mass%) contained in the steel sheet, and [Mn] is the Mn content (mass%) contained in the steel sheet. [8] The oxidation treatment is carried out by N 2 and 500 ppm by volume or more of O 2 Including CO, CO 2 , H 2 O, NO X [9] The method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to [5] and [8], wherein the oxidation treatment is carried out using a radiant tube-type heating furnace.
[10] The method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to [5], [8] and [9], wherein the reduction annealing is carried out using a radiant tube-type heating / soaking furnace.
[11] The method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to [5], [8] and [9], wherein the second reduction annealing is carried out using an annealing atmosphere containing 2.0 vol% or more and less than 5.0 vol% of hydrogen, the balance being N. 2
[12] In the first reduction annealing, the annealing atmosphere contains 5.0% by volume or more and 12% by volume or less of hydrogen, the balance being N. 2 In the second reduction annealing, the hydrogen content of the annealing atmosphere is 2.0% by volume or more and less than 3.0% by volume, and the balance is N. 2 The method for producing a high-strength hot-dip galvanized steel sheet according to any one of [1] to
[11] , comprising:
[0012] According to the present invention, it is possible to provide a high-strength hot-dip galvanized steel sheet which has excellent LME cracking resistance in welds, good appearance quality, and in which the hydrogen content in the steel, which is a factor in deteriorating delayed fracture resistance, is sufficiently reduced.
[0013] Fig. 1 is a structural diagram of a test material for evaluating LME cracking resistance. The upper diagram in Fig. 2 is a plan view of a plate assembly with a welded portion, and the lower diagram is a drawing showing a cross section in the plate thickness direction after cutting the plate assembly with a welded portion at the cutting position shown in the upper diagram.
[0014] Hereinafter, an embodiment of the present invention will be described.
[0015] In the following description, the units of the content of each element in the composition of the Si-containing steel sheet and the content of each element in the composition of the coating layer are all in mass %, and are simply expressed as % unless otherwise specified. Furthermore, in this specification, a numerical range expressed using "to" means a range that includes the numerical values written before and after "to" as the lower and upper limits. Furthermore, in this specification, a high-strength steel sheet means that the tensile strength TS of the steel sheet measured in accordance with JIS Z 2241 (2011) is 590 MPa or more.
[0016] Here, the term "steel sheet" refers to a steel sheet manufactured by cold rolling or hot rolling. Generally, steel sheets are manufactured by cold rolling or hot rolling, but in the present invention, the manufacturing method of the steel sheet is not particularly limited.
[0017] First, the chemical composition of the Si-containing steel sheet will be described.
[0018] Si: 0.45% or more and 2.0% or less Si is an effective element for achieving high strength in steel sheets because it has a significant effect of increasing the strength of steel through solid solution (solid solution strengthening ability) without significantly impairing workability. On the other hand, Si also has a negative effect on the resistance weld crack resistance of welded parts. When Si is added to achieve high strength in steel sheets, a content of 0.45% or more is required. Furthermore, if the Si content is less than 0.45%, no particular problems arise with the resistance weld crack resistance of welded parts, and there is little need to apply the present invention. On the other hand, if the Si content exceeds 2.0%, the hot rolling and cold rolling properties are significantly reduced, adversely affecting productivity and reducing the ductility of the steel sheet itself. Therefore, the Si content is set to a range of 0.45% or more and 2.0% or less. The Si content is preferably 0.7% or more, more preferably 0.9% or more. Furthermore, the Si content is preferably 1.8% or less, more preferably 1.6% or less.
[0019] The Si-containing steel sheet according to this embodiment must contain Si in the above range, but other elements are permissible as long as they fall within the composition ranges of ordinary steel sheets, and are not particularly limited. However, if the Si-containing steel sheet according to this embodiment is to have a high strength of 590 MPa or more in tensile strength (TS), it is preferable that the steel sheet have the following composition.
[0020] C: 0.3% or less C improves the workability of the steel sheet by forming martensite or the like as a steel structure. When C is contained, in order to obtain good weldability, the C content is preferably 0.3% or less, and more preferably 0.25% or less. There is no particular restriction on the lower limit of C, but in order to obtain good workability, it is preferable that C be 0.03% or more, and more preferably 0.05% or more.
[0021] Mn: 1.0% or more and 4.0% or less Mn is an element that strengthens steel through solid solution strengthening, improves hardenability, and promotes the formation of retained austenite, bainite, and martensite. These effects are achieved by including 1.0% or more of Mn. On the other hand, if the Mn content is 4.0% or less, the above effects can be achieved without increasing costs. Therefore, the Mn content is preferably 1.0% or more, and more preferably 4.0% or less. The Mn content is more preferably 1.8% or more. Furthermore, the Mn content is more preferably 3.3% or less.
[0022] P: 0.1% or less (excluding 0%). By suppressing the P content, it is possible to prevent a decrease in weldability. Furthermore, it is possible to prevent P from segregating at grain boundaries, thereby preventing deterioration of ductility, bendability, and toughness. Furthermore, adding a large amount of P promotes ferrite transformation, which increases the grain size. Therefore, it is preferable that the P content be 0.1% or less. There is no particular lower limit for P, but due to production technology constraints, it is greater than 0%, and is usually 0.001% or more.
[0023] S: 0.03% or less (excluding 0%) The S content is preferably 0.03% or less, and more preferably 0.02% or less. By suppressing the S content, it is possible to prevent a decrease in weldability and a decrease in ductility during hot rolling, thereby suppressing hot cracking and significantly improving surface properties. Furthermore, by suppressing the S content, coarse sulfides are formed as an impurity element, which can prevent a decrease in the ductility, bendability, and stretch flangeability of the steel sheet. These problems become more pronounced when the S content exceeds 0.03%, so it is preferable to reduce the S content as much as possible. The lower limit of S is not particularly limited, but is greater than 0% due to constraints on production technology, and is usually 0.0001% or more.
[0024] N: 0.010% or less (excluding 0%) The N content is preferably 0.010% or less. By setting the N content to 0.010% or less, N forms coarse nitrides with Ti, Nb, and V at high temperatures, which prevents the effect of increasing the strength of the steel sheet by adding Ti, Nb, and V from being impaired. In addition, by setting the N content to 0.010% or less, a decrease in toughness can be prevented. Furthermore, by setting the N content to 0.010% or less, the occurrence of slab cracks and surface defects during hot rolling can be prevented. The N content is preferably 0.005% or less, more preferably 0.003% or less, and even more preferably 0.002% or less. The lower limit of the N content is not particularly limited, but is greater than 0% due to production technology constraints, and is usually 0.0005% or more.
[0025] Al: 0.1% or less (excluding 0%) Because Al is thermodynamically most easily oxidized, it oxidizes before Si and Mn, suppressing the oxidation of Si and Mn in the outermost layer of the steel sheet and promoting the oxidation of Si and Mn inside the steel sheet. This effect is achieved when the Al content is 0.01% or more. On the other hand, an Al content exceeding 0.1% increases costs. Therefore, if Al is added, the Al content is preferably 0.1% or less. There is no particular lower limit for Al, but it is greater than 0% and is usually 0.001% or more.
[0026] The component composition may further optionally contain one or more elements selected from the group consisting of B: 0.005% or less, Ti: 0.2% or less, Cr: 1.0% or less, Mo: 1.0% or less, Cu: 1.0% or less, Ni: 1.0% or less, Nb: 0.20% or less, Sb: 0.200% or less, V: 0.5% or less, Ta: 0.1% or less, W: 0.5% or less, Zr: 0.1% or less, Sn: 0.20% or less, Ca: 0.005% or less, Mg: 0.005% or less, and REM (Rare Earth Metal): 0.005% or less.
[0027] B: 0.005% or less B is an element effective in improving the hardenability of steel. To improve hardenability, the B content is preferably 0.0003% or more, and more preferably 0.0005% or more. However, excessive addition of B reduces formability, so the B content is preferably 0.005% or less.
[0028] Ti: 0.2% or less Ti is effective for precipitation strengthening of steel. There is no particular limitation on the lower limit of Ti, but in order to obtain the effect of adjusting strength, it is preferable to set it to 0.005% or more. However, if Ti is added in excess, the hard phase becomes excessively large and formability decreases, so when Ti is added, the Ti content is preferably set to 0.2% or less, and more preferably 0.05% or less.
[0029] Cr: 1.0% or less The Cr content is preferably 0.005% or more. By setting the Cr content to 0.005% or more, hardenability is improved and the balance between strength and ductility can be improved. When Cr is added, the Cr content is preferably 1.0% or less from the viewpoint of preventing an increase in costs.
[0030] Mo: 1.0% or less The Mo content is preferably 0.005% or more. By setting the Mo content to 0.005% or more, the effect of adjusting strength can be obtained. The Mo content is more preferably 0.05% or more. Furthermore, when Mo is added, the Mo content is preferably 1.0% or less from the viewpoint of preventing an increase in costs.
[0031] Cu: 1.0% or less The Cu content is preferably 0.005% or more. By setting the Cu content to 0.005% or more, the formation of the residual γ phase can be promoted. Furthermore, when Cu is added, the Cu content is preferably 1.0% or less from the viewpoint of preventing an increase in costs.
[0032] Ni: 1.0% or less The Ni content is preferably 0.005% or more. By setting the Ni content to 0.005% or more, the formation of the residual γ phase can be promoted. Furthermore, when Ni is added, the Ni content is preferably 1.0% or less from the viewpoint of preventing an increase in costs.
[0033] Nb: 0.20% or less When Nb is contained in an amount of 0.005% or more, the effect of improving strength can be obtained. Furthermore, when Nb is contained, the Nb content is preferably 0.20% or less from the viewpoint of preventing an increase in costs.
[0034] Sb: 0.200% or less Sb can be added from the viewpoint of suppressing nitriding and oxidation of the steel sheet surface, or decarburization caused by oxidation in the region extending to a depth of several tens of microns from the steel sheet surface. By suppressing nitriding and oxidation of the steel sheet surface, Sb prevents a decrease in the amount of martensite formed on the steel sheet surface, improving the fatigue properties and surface quality of the steel sheet. To achieve this effect, the Sb content is preferably 0.001% or more. On the other hand, to obtain good toughness, the Sb content is preferably 0.200% or less.
[0035] V: 0.5% or less The effect of improving strength can be obtained by including 0.005% or more of V. Furthermore, when V is included, from the viewpoint of preventing an increase in costs, the V content is preferably 0.5% or less.
[0036] Ta: 0.1% or less When Ta is contained in an amount of 0.001% or more, the effect of improving strength can be obtained. Furthermore, when Ta is contained, from the viewpoint of preventing an increase in cost, the Ta content is preferably 0.1% or less.
[0037] W: 0.5% or less When W is contained in an amount of 0.005% or more, the effect of improving strength can be obtained. Furthermore, when W is contained, from the viewpoint of preventing an increase in costs, the W content is preferably 0.5% or less.
[0038] Zr: 0.1% or less When Zr is contained in an amount of 0.0005% or more, the effect of improving strength can be obtained. Furthermore, when Zr is contained, from the viewpoint of preventing an increase in costs, the Zr content is preferably 0.1% or less.
[0039] Sn: 0.20% or less Sn is an element that is effective in suppressing denitrification, deboronation, etc., and suppressing a decrease in the strength of steel. To obtain this effect, a Sn content of 0.002% or more is preferable. On the other hand, to obtain good impact resistance, the Sn content is preferably 0.20% or less.
[0040] Ca: 0.005% or less When Ca is contained in an amount of 0.0005% or more, the morphology of sulfides can be controlled and ductility and toughness can be improved. Furthermore, from the viewpoint of obtaining good ductility, when Ca is contained, the Ca content is preferably 0.005% or less.
[0041] Mg: 0.005% or less When Mg is contained in an amount of 0.0005% or more, the morphology of sulfides can be controlled and ductility and toughness can be improved. Furthermore, when Mg is contained, from the viewpoint of preventing an increase in costs, the Mg content is preferably 0.005% or less.
[0042] REM: 0.005% or less When REM is contained in an amount of 0.0005% or more, the morphology of sulfides can be controlled and ductility and toughness can be improved. Furthermore, when REM is contained, the REM content is preferably 0.005% or less from the viewpoint of obtaining good toughness.
[0043] The Si-containing steel sheet of this embodiment contains the above-mentioned components, with the remainder being Fe and unavoidable impurities. The Si-containing steel sheet may be either a cold-rolled steel sheet or a hot-rolled steel sheet.
[0044] Next, the oxidation treatment, reduction annealing, and hot-dip galvanizing will be described.
[0045] In the present invention, the temperatures specified in the oxidation treatment, reduction annealing, and cooling after annealing are all "steel sheet temperatures."
[0046] The manufacturing method of the present invention is a method for manufacturing a hot-dip galvanized steel sheet, in which a steel sheet containing 0.45% to 2.0% Si is subjected to an oxidation treatment, followed by reduction annealing and hot-dip galvanizing. In the oxidation heating step, the steel sheet is heated in a predetermined oxidizing atmosphere to be oxidized, thereby generating Fe oxide in the surface layer of the steel sheet. The subsequent reduction annealing step comprises a step of reducing the oxidized steel sheet in different atmospheres in the previous and subsequent steps.
[0047] In the first reduction annealing, which is the first stage of reduction annealing, the steel sheet is recrystallized in an Fe reducing atmosphere having a predetermined hydrogen concentration and dew point, thereby reducing the Fe oxide produced in the oxidizing heating step and forming a reduced iron layer on the surface of the steel sheet. In the subsequent second reduction annealing, which is the second stage of reduction annealing, the steel sheet is recrystallized in an Fe reducing atmosphere having a predetermined hydrogen concentration and dew point, thereby providing a low-solubility Si and C layer on the surface of the steel sheet to improve LME cracking resistance, and simultaneously releasing hydrogen dissolved in the steel from the steel sheet. The reduction-annealed steel sheet is cooled to a predetermined temperature and then immersed in a hot-dip galvanizing bath for hot-dip galvanizing. The manufacturing method of the present invention also includes a case in which an alloying treatment of hot-dip galvanizing is performed after hot-dip galvanizing to produce a galvannealed steel sheet.
[0048] In the present invention, the oxidation heating step and the subsequent reduction annealing step are usually carried out in a continuous annealing furnace having, in order from the inlet side, an oxidation zone (a zone for oxidation treatment), a reduction zone (a zone for first reduction annealing in reduction annealing), a soaking zone (a zone for second reduction annealing in reduction annealing), and a cooling zone.
[0049] The manufacturing method of the present invention will be described below in the order of oxidation treatment, reduction annealing (first reduction annealing, second reduction annealing, cooling after annealing), and hot-dip galvanizing.
[0050] First, the oxidation treatment will be described.
[0051] In this oxidation treatment, N 2 and 500 ppm by volume or more of O 2The steel sheet is oxidized in an oxidation step at a temperature in the range of 500° C. to 800° C. in an atmosphere containing the above-mentioned elements. In the present invention, the steel sheet is oxidized in this oxidation treatment and then reduced in the subsequent reduction annealing to form a reduced iron layer on the surface layer of the steel sheet, thereby preventing Si and Mn from diffusing into the surface layer of the steel sheet and being oxidized, and thereby ensuring galvanizability.
[0052] O in the atmosphere where oxidation is performed 2 By setting the concentration to 500 ppm by volume or more, oxidation of the steel sheet is promoted. 2 If the concentration is less than 500 ppm by volume, oxidation of the steel sheet will be insufficient, resulting in the formation of oxides of Si and Mn, which will deteriorate the platability.
[0053] In the oxidation treatment, oxidation of the steel sheet is promoted by setting the steel sheet temperature (maximum temperature reached by the steel sheet) to 500° C. or higher. If the steel sheet temperature is less than 500° C., oxidation is insufficient, and oxides of Si and Mn are formed, resulting in a decrease in platability.
[0054] On the other hand, if the steel sheet temperature (maximum temperature reached by the steel sheet) exceeds 800°C, oxidation of the steel sheet becomes excessive, and reduction is not completed in the subsequent reduction annealing (first step), causing a phenomenon known as pickup in which oxides peel off and adhere to the rolls in the subsequent reduction annealing step. When pickup occurs on the rolls, indentations occur in the steel sheet, significantly impairing the appearance of the galvanized steel sheet.
[0055] Next, reduction annealing will be described.
[0056] The reduction annealing must be carried out in different atmospheres in the first and second stages.
[0057] In the first reduction annealing in the first stage, the steel sheet that has undergone oxidation treatment is annealed at a dew point of -45°C or higher and +20°C or lower, a hydrogen concentration of 5.0% by volume or higher and 25% by volume or lower, and a balance of N. 2 The temperature is maintained at 650° C. or higher and 900° C. or lower for 20 seconds or higher and 150 seconds or lower in an atmosphere containing
[0058] The Fe oxide formed by the oxidation treatment is reduced in a reducing atmosphere in this first reduction annealing to form a reduced iron layer on the steel sheet surface, preventing Si and Mn from diffusing into the steel sheet surface and oxidizing, thereby ensuring galvanizability. Since the subsequent second reduction annealing in a low hydrogen concentration atmosphere hardly progresses in reduction, it is necessary to complete the reduction of the Fe oxide in this first reduction annealing. Furthermore, by controlling the reduction annealing temperature, dew point, and hydrogen concentration, it is possible to form a layer on the surface with low concentrations of solute Si and solute C, which adversely affect LME resistance. While the mechanism behind this is unclear, Si is known to be an easily oxidizable element and is oxidized even in an Fe reducing atmosphere. In particular, H 2 It can be considered that when the O concentration increases, oxides are generated inside the steel sheet, and the amount of dissolved Si decreases around the oxides. 2 This is oxidized by O and released into the furnace as CO gas, which reduces the C concentration in the steel sheet surface layer. These factors are thought to improve LME cracking resistance.
[0059] If the annealing temperature of the steel sheet in the first reduction annealing step is less than 650°C, reduction will be insufficient, and Fe oxide will cause roll pickup, resulting in defects in the steel sheet. In the subsequent second reduction annealing step, the Fe oxide will not be substantially reduced, resulting in bare spots. On the other hand, if the annealing temperature of the steel sheet exceeds 900°C, the furnace body will be significantly affected. For this reason, the annealing temperature of the steel sheet is set to 650°C or higher and 900°C or lower.
[0060] Regarding the dew point of the atmosphere in the first reduction annealing step, lowering the dew point below −45°C requires equipment to lower the dew point, which increases costs. On the other hand, if the dew point exceeds +20°C, there is a risk of damage to the furnace body. Therefore, the dew point is set to −45°C or higher and +20°C or lower. Regarding the hydrogen concentration, the higher the hydrogen concentration, the faster the reduction of Fe oxide is completed, but the higher the hydrogen concentration, the more likely hydrogen is to remain in the steel. If the hydrogen concentration is less than 5.0 vol%, the reduction is insufficient. On the other hand, if the hydrogen concentration exceeds 25 vol%, the reduction effect saturates and a large amount of hydrogen dissolves in the steel, making it difficult to sufficiently reduce the amount of hydrogen in the steel even in the subsequent second reduction annealing step. Therefore, the hydrogen concentration is set to 5.0 vol% or higher and 25 vol% or lower. From the above viewpoints, the hydrogen concentration is more preferably 10 vol% or higher. On the other hand, from the viewpoint of running costs, the hydrogen concentration is preferably 20 vol% or lower, and more preferably 15 vol% or lower.
[0061] Furthermore, the low solute Si and C surface layer for improving LME cracking resistance is more likely to form when the dew point is high and the hydrogen concentration is low. Therefore, the dew point is preferably -20°C or higher, and more preferably -5°C or higher. The hydrogen concentration is preferably 15% by volume or lower. The low solute Si and C layer for improving LME resistance is mainly formed in the second reduction annealing step. It is preferable that a certain amount of the low solute Si and C layer is also formed in the first reduction annealing by setting the dew point to -20°C or higher.
[0062] If the holding time at 650°C or higher and 900°C or lower in the first reduction annealing step is less than 20 seconds, reduction will not be sufficiently completed. On the other hand, since reduction is sufficiently completed with a holding time of 150 seconds or less, a holding time of more than 150 seconds actually reduces productivity. The longer the holding time, the more easily the low-solubility Si and C surface layer, which is used to improve LME cracking resistance, is formed. The amount of hydrogen in the steel saturates with a holding time of about 20 seconds, and the influence of the holding time is not significant. For these reasons, the holding time at 650°C or higher and 900°C or lower in the first reduction annealing step is set to 20 seconds or higher and 150 seconds or lower.
[0063] In the second reduction annealing in the latter stage, the steel sheet that has been subjected to the first reduction annealing step is subjected to a hydrogen concentration of 2.0% by volume or more and 8.0% by volume or less, and a residual N 2and the hydrogen concentration in the first reduction annealing in the previous stage is H 2 a, the hydrogen concentration in the second reduction annealing in the latter stage is H 2 When b is set, H 2 a>H 2 The steel sheet is then held at a temperature of 700°C or higher and 950°C or lower for 30 seconds or shorter in an atmosphere in which the hydrogen concentration is adjusted to satisfy condition b. In this second reduction annealing step, a surface layer containing low amounts of solute Si and C is sufficiently formed in the steel sheet that has been reduced in the first reduction annealing step in order to improve the LME cracking resistance, and at the same time, hydrogen is released from the steel sheet by maintaining the steel sheet in a low hydrogen atmosphere.
[0064] As described above, the surface layer containing low amounts of dissolved Si and C, which is intended to improve LME cracking resistance, is more likely to be formed when the dew point is high and the hydrogen concentration is low.
[0065] Therefore, from the viewpoint of sufficiently forming a surface layer of low-solubility Si and C, the dew point in the second reduction annealing step is preferably −10° C. or higher, and more preferably 0° C. or higher. On the other hand, if the dew point exceeds +20° C., the reduced Fe formed in the first reduction annealing step may be reoxidized, impairing platability, and dew point control is also difficult, raising concerns about the impact on the furnace body. For this reason, the dew point is set to −10° C. or higher and +20° C. or lower.
[0066] Similarly, the hydrogen concentration in the second reduction annealing step is preferably 8.0 vol% or less from the viewpoint of sufficiently forming a surface layer of low-solubility Si and C. More preferably, it is less than 5.0 vol%. Regarding the hydrogen concentration in the steel sheet, the lower the hydrogen concentration, the more hydrogen dissolved in the steel sheet is released in the first reduction annealing step. However, it is difficult to uniformly control the hydrogen concentration in the furnace to less than 2.0 vol%, and there is a concern that the steel sheet may be oxidized in areas with low hydrogen concentration. Therefore, the hydrogen concentration is set to 2.0 vol% or more. The balance of the annealing atmosphere in the second reduction annealing step is N. 2 Includes.
[0067] In the first reduction annealing, the hydrogen content of the annealing atmosphere is 5.0% by volume or more and 12% by volume or less, and the balance is N. 2 In the case where the alloy contains the above, in the second reduction annealing, the hydrogen in the annealing atmosphere is 2.0 vol% or more and less than 3.0 vol%, and the balance is N 2By optimizing the hydrogen concentrations in the annealing atmospheres for the first reduction annealing and the second reduction annealing, respectively, it is possible to further reduce hydrogen in the steel sheet.
[0068] If the annealing temperature of the steel sheet in the second reduction annealing step is less than 700°C, the low-solubility Si and C layer at the surface is not sufficiently formed, and dehydrogenation is not promoted. On the other hand, if the annealing temperature exceeds 950°C, the furnace body is significantly affected. For this reason, the annealing temperature of the steel sheet is set to 700°C or higher and 950°C or lower.
[0069] The holding time in the second reduction annealing step is set to 30 seconds or more and 300 seconds or less. If it is less than 30 seconds, a sufficient surface layer with low solid solution Si and C is not formed. On the other hand, if it exceeds 300 seconds, productivity may decrease.
[0070] Here, the hydrogen concentration in the first reduction annealing in the previous stage is H 2 a, the hydrogen concentration in the second reduction annealing in the latter stage is H 2 When b is set, H 2 a>H 2 The reason for this is that the hydrogen that has entered the steel in the first reduction annealing step in the preceding stage is to be reduced in the second reduction annealing step in the following stage.
[0071] In the present invention, a high concentration of hydrogen is required to reduce the Fe oxide produced by the oxidation treatment in the first reduction annealing step of reduction annealing. This makes it difficult to sufficiently form a surface layer with low solute Si and C to improve LME cracking resistance, and a large amount of hydrogen dissolves in the steel. Therefore, it is important to sufficiently form the surface layer with low solute Si and C, and further, to strike a balance between oxidation-reduction and the dehydrogenation of hydrogen in the steel. For this reason, it is necessary to optimize the conditions for the first reduction annealing step and the second reduction annealing step of reduction annealing as described above. For optimization, it is preferable to use an annealing furnace that is divided into two or more sections in the running direction of the steel sheet and is capable of annealing in two or more different atmospheres.
[0072] The oxidation treatment is preferably carried out in a temperature increasing step of the steel sheet which is carried out as a pre-step of reduction annealing, because this allows efficient oxidation treatment at an optimum temperature which varies depending on the steel composition.
[0073] Furthermore, the oxidation treatment is preferably carried out within a temperature range of at least 50°C, i.e., 500°C to 800°C. Here, the "temperature range" refers to the temperature range during heating from 500°C to 800°C. For example, when oxidation treatment is carried out within a temperature range of 550 to 600°C, the temperature range is 50°C. Furthermore, when oxidation treatment is carried out within a temperature range of 450 to 600°C, the temperature range corresponding to 500°C to 800°C is 100°C. This is because oxidation treatment for obtaining the amount of reduced iron required to improve galvanizability can be carried out more uniformly. While the reason why oxidation treatment is more uniform when carried out within a temperature range of 50°C or higher is unclear, it is believed that, because the oxidation behavior of steel sheets varies depending on the temperature range, starting oxidation at a relatively low temperature, where the oxidation rate is slow, results in more uniform oxidation.
[0074] Here, the heating furnace used in the oxidation zone where the oxidation treatment is performed can be a direct-fire type equipped with a direct-fire burner (direct-fired furnace (DFF)) or a radiant tube type equipped with an atmosphere-controlled chamber.
[0075] The direct-fire method is a method of heating a steel sheet by a burner that directly applies the burner flame, which is a mixture of fuel such as coke oven gas (COG), a by-product gas from a steel mill, and air, to the steel sheet surface. Heating with a direct-fire burner has the advantage of increasing the temperature of the steel sheet faster than radiant heating methods, thereby shortening the furnace length or increasing the line speed. Furthermore, when the air ratio of at least a portion of the atmosphere in the direct-fire burner is set to 1.0 or higher and the ratio of air to fuel is increased, unburned oxygen remains in the flame, which promotes oxidation of the steel sheet and oxidizes the steel sheet surface. Therefore, adjusting the air ratio makes it possible to control the oxygen concentration in the atmosphere. COG, liquefied natural gas (LNG), hydrogen gas, ammonia gas, etc. can be used as fuel for the direct-fire burner. Therefore, in the case of the direct-fire method, CO, CO₂, and CO₂ are generated as oxidation products of the fuel gas components in the oxidation furnace depending on the type of fuel used. 2 , H 2 O, NO X etc. and the N of the combustion air components 2 Therefore, the oxidation process is2 and 500 ppm by volume or more of O 2 Including CO, CO 2 , H 2 O, NO X The treatment is carried out in an atmosphere containing one or more of the following:
[0076] The radiant tube method heats steel plates using radiant heat from a heated tube. Compared to a direct flame burner, this method has a slower temperature rise rate, which means the furnace length is longer, but it has the advantage of being easier to maintain and inspect.
[0077] In either method, it is sufficient to obtain a sufficient amount of oxidation of the steel sheet, and it is sufficient that part or all of the heating furnace is controlled to a specified atmosphere. In particular, in the radiant tube method, since the heating rate is slow, it is possible to cover part of the furnace with a chamber and control only that part to a specified atmosphere.
[0078] When a direct-fired method is used in this oxidation treatment, the oxidation treatment may be divided into two or more steps, and a direct-fired heating furnace capable of oxidation in two or more atmospheres may be used. The reason for this is that, in the subsequent reduction annealing, this is effective for forming a surface layer with low solute Si and C contents necessary for LME cracking resistance, and for promoting dehydrogenation which affects delayed fracture resistance, thereby reducing hydrogen in the furnace.
[0079] If the steel sheet is oxidized too much in this oxidation treatment, the oxide peels off during the subsequent reduction annealing, causing a phenomenon known as pickup, in which the oxide adheres to the roll. Pickup on the roll significantly impairs the appearance of the galvanized steel sheet. This pickup is likely to occur when the hydrogen concentration is 10% by volume or less in the first reduction annealing step of the subsequent reduction annealing. This occurs because the reducing power of the atmosphere is reduced, making pickup more likely to occur, particularly in the early stages of reduction annealing. If the hydrogen concentration exceeds 10% by volume in the first reduction annealing step of the subsequent reduction annealing, there is no particular need to separate the process into two or more steps. If the hydrogen concentration is 10% by volume or less in the first reduction annealing step of the subsequent reduction annealing, it is an important requirement for obtaining a beautiful surface appearance free of indentations and the like.
[0080] When a direct-fired heating furnace having two or more separated zones is used for the oxidation heating step, in the first heating zone of the first stage, the cold-rolled sheet is heated to a heating temperature T calculated from the following formula (1) under the condition that the average heating rate at 200°C or higher is 10°C / sec or more and 50°C / sec or less, where the air ratio of the direct-fired heating furnace is α. 1 (°C) or higher. 1 is preferably 750°C or less. 1 = 28.2 [Si] + 7.95 [Mn] - 86.2 α + 666 --- (1) Where, [Si] is the mass % of Si in the steel, [Mn] is the mass % of Mn in the steel, and α is the air ratio of the direct-fired heating furnace.
[0081] Here, the reason for determining the above formula (1) will be explained.
[0082] In order to suppress the oxidation of Si and Mn on the surface of the steel sheet before hot dip coating, it is important to form internal oxidation of Si and Mn. In the stage prior to the oxidation heating process, it is advisable to actively carry out oxidation treatment in order to generate iron oxide, which serves as an oxygen source for the internal oxidation of Si and Mn.
[0083] To obtain a sufficient amount of iron oxide, it is necessary to control the heating atmosphere and temperature. The atmosphere is controlled by adjusting the air ratio of the direct-fired heating furnace. Increasing the air ratio, or the ratio of air to fuel, allows unreacted oxygen to remain in the flame, which can promote the oxidation of the steel sheet.
[0084] Furthermore, the heating temperature may be changed depending on the Si and Mn contents. In order to suppress the oxidation of Si and Mn on the steel sheet surface, it is preferable to oxidize Si and Mn inside the steel sheet. As the Si and Mn contents increase, the amount of oxygen required for internal oxidation also increases. Therefore, the higher the Si and Mn contents, the better the oxidation temperature. In particular, since it is known that Si suppresses the oxidation reaction of iron when added to steel, the higher the Si content, the better the oxidation temperature.
[0085] The above formula (1) was obtained by multiple regression analysis, and it was found that the Si content, Mn content, and direct-fired furnace air ratio are related to the furnace outlet temperature (heating ultimate temperature T 1) was determined from the results of an analysis of the impact on
[0086] From the above, in the first heating zone, the heating temperature T calculated from the above formula (1) 1 It is preferable to heat the mixture to a temperature of 0.1°C or higher. However, the upper limit of the air ratio α during heating in the first heating zone is preferably 1.5 or lower in order to suppress excessive iron oxidation reaction and prevent the occurrence of subsequent pick-up. Furthermore, if the air ratio is low, the oxidizing properties of the atmosphere become weak, and even if formula (1) is satisfied, a sufficient amount of oxidation may not be ensured. Therefore, it is preferable that the air ratio α be 0.9 or higher.
[0087] Furthermore, in the first heating zone, it is preferable to set the average heating rate at 200°C or higher to 10 to 50°C / sec. If the average heating rate exceeds 50°C / sec, the heating time in the first heating zone will be short, making it impossible to form a sufficient amount of iron oxide. On the other hand, if the average heating rate is less than 10°C / sec, a long heating time will be required, resulting in a decrease in production efficiency. Furthermore, if excessive iron oxide is formed, Fe oxide will peel off in the reducing atmosphere furnace in the subsequent reduction annealing, causing the pickup phenomenon. Therefore, the average heating rate at 200°C or higher is set to 10 to 50°C / sec. The average heating rate (°C / sec) here is determined based on the heating end temperature (maximum steel sheet temperature (T 1 It can be obtained by dividing the difference between the temperature rise start temperature (200°C or higher) (°C) and the temperature rise start temperature (200°C or higher) by the temperature rise time (s).
[0088] In the second heating zone at the rear stage, the cold-rolled sheet after the first heating zone at the front stage is heated in a direct-fired heating furnace at an air ratio of ≦0.9 and T 1 Under the condition that the average heating rate is 5°C / sec or more and 30°C / sec or less, T calculated from the following formula (2) 2 Heat to a temperature of 100°C or higher. 2 =T 1 +30 --- (2)
[0089] The second heating zone prevents the occurrence of pick-up phenomenon even if the hydrogen concentration in the furnace is reduced in the subsequent reduction annealing step, making it possible to obtain a beautiful surface appearance free of dents and the like.
[0090] In order to prevent the occurrence of the pick-up phenomenon, it is important to reduce a part of the surface (surface layer) of the steel sheet that has been oxidized. To perform such a reduction treatment, it is necessary to control the air ratio of the burner of the direct-fired heating furnace to 0.9 or less. 2 By reducing the concentration, the surface layer of the iron oxide is partially reduced, which prevents direct contact between the furnace rolls and the iron oxide during the subsequent reduction annealing process, thereby preventing the occurrence of the pick-up phenomenon. If the air ratio exceeds 0.9, the reduction reaction becomes difficult to occur, so the air ratio is set to 0.9 or less. Furthermore, to ensure stable combustion in a direct-fired heating furnace, an air ratio of 0.7 or more is preferred.
[0091] The heating temperature of the second heating zone in the latter stage is T 2 If the temperature is lower than T, the reduction reaction is unlikely to occur, and the effect of suppressing the occurrence of the pick-up phenomenon cannot be obtained. 2 In order to reduce unnecessary heating costs, the temperature is preferably 750° C. or less.
[0092] In the second heating zone, T 1 It is preferable that the average temperature rise rate (average heating rate) exceeding 5°C / sec is 5°C / sec or more and 30°C / sec or less. If the average temperature rise rate exceeds 30°C / sec, the heating time in the second heating zone will be short, and a sufficient amount of iron oxide will not be reduced. On the other hand, if the average temperature rise rate is less than 5°C / sec, heating will take a long time, and production efficiency will decrease. 1 "Average heating rate above T" 1 The average heating rate (°C / sec) refers to the average heating rate from the temperature exceeding the maximum temperature reached by heating in the second heating zone to the temperature reached in the third heating zone. Here, the average heating rate (average heating rate) (°C / sec) is obtained by dividing the difference between the temperature at the end of heating (maximum temperature reached by the steel sheet) (°C) and the temperature at the start of heating by the heating time (s).
[0093] As mentioned above, the oxidation treatment is 2 and 500 ppm by volume or more of O 2 and other CO, CO 2 , H 2 O, NO XIt is preferable to carry out the oxidation treatment in an atmosphere containing one or more of the following gases: 1) ammonia; 2) ammonia; 3) ammonia; 4) ammonia; 5) ammonia; 6) ammonia; 7) ammonia; 8) ammonia; 9) ammonia; 10) ammonia; 11) ammonia; 12) ammonia; 13) ammonia; 14) ammonia; 15) ammonia; 16) ammonia; 17) ammonia; 18) ammonia; 19) ammonia; 19) ammonia; 12) ammonia; 19 ...
[0094] It may be preferable to carry out the oxidation treatment using a radiant tube type heating furnace, which has the advantage of being easier to maintain and being able to suppress variations in width direction, compared to a direct-fired heating furnace, when a chamber capable of controlling the atmosphere for the oxidation treatment is provided inside the radiant tube type heating furnace.
[0095] Furthermore, the reduction annealing is preferably carried out using a radiant tube type heating furnace. Also, it is preferable to carry out the reduction annealing using a radiant tube type heating / soaking furnace, because it is easy to control the inside of the furnace to a reducing atmosphere and it is also advantageous in terms of equipment costs.
[0096] Hot-dip galvanizing is a process in which the annealed sheet after reduction annealing is subjected to hot-dip galvanizing treatment in a hot-dip galvanizing bath containing 0.12 to 0.22 mass % of Al.
[0097] In the present invention, the Al concentration in the zinc plating bath is preferably 0.12 to 0.22 mass%. If the Al concentration is less than 0.12 mass%, an Fe-Zn alloy phase is formed during plating, which can lead to poor plating adhesion and uneven appearance. If the Al concentration exceeds 0.22 mass%, a thick Fe-Al alloy phase is formed at the plating / base steel interface during plating, resulting in poor weldability. Furthermore, the high Al content in the bath can lead to the formation of a large amount of an Al oxide film on the surface of the plated steel sheet, which can impair not only weldability but also appearance.
[0098] In some cases, alloying treatment is carried out after hot dip galvanizing, and the present invention is also effective in this case.
[0099] The Al concentration in the plating bath when alloying is preferably 0.12 to 0.17 mass%. If the Al concentration is less than 0.12 mass%, an Fe-Zn alloy phase is formed during plating, which can deteriorate the plating adhesion and cause uneven appearance. If the Al concentration is more than 0.17 mass%, a thick Fe-Al alloy phase is formed at the plating / base steel interface during plating, which acts as a barrier to the Fe-Zn alloying reaction, increasing the alloying temperature and possibly deteriorating the mechanical properties.
[0100] Other conditions during hot-dip galvanizing are not limited, but for example, the hot-dip galvanizing bath temperature is usually in the range of 440 to 500°C, and the steel sheet is immersed in the galvanizing bath at a sheet temperature of 440 to 550°C, and the coating amount can be adjusted by gas wiping or the like.
[0101] As the alloying treatment, the steel sheet after the hot dip galvanizing treatment is heated at a temperature in the range of 450 to 550° C. for 10 to 60 seconds.
[0102] Although there are no particular limitations on the degree of alloying after alloying treatment (Fe concentration in the plating layer), a degree of alloying in which the Fe concentration is 7 to 15 mass % is preferred. If the Fe concentration is less than 7 mass %, the η phase remains, resulting in poor press formability, and if it exceeds 15 mass %, the plating adhesion is poor.
[0103] [Example 1] A 1.2 mm cold-rolled sheet having the chemical composition shown in Table 1 was subjected to annealing and hot-dip galvanizing in a CGL. Oxidation heating was performed using a direct-fire heating furnace equipped with a nozzle-mix burner under the conditions shown in Table 2. The oxidation start temperature was set to 300°C. Since the oxidation start temperature does not particularly affect the coating appearance, a temperature below 300°C may be used as the oxidizing atmosphere. Reduction annealing was performed using a radiant tube-type heating furnace separated into two zones by seal rolls under the conditions shown in Table 2, followed by cooling. Subsequently, hot-dip galvanizing was performed using a 460°C galvanizing bath containing 0.135 mass% Al, and the coating weight was reduced to approximately 50 g / m per side by gas wiping. 2 In Table 2, in the first reduction annealing, the steel sheet was held at the maximum temperature reached for the time shown in the table, and in the second reduction annealing, the steel sheet was held at the maximum temperature reached for the time shown in the table.
[0104]
[0105]
[0106] Next, the appearance of the high-strength hot-dip galvanized steel sheets obtained as described above was evaluated, and the tensile properties were investigated. Furthermore, the LME cracking resistance, dehydrogenation behavior, and damage to the furnace body were evaluated. The measurement and evaluation methods are described below.
[0107] <Appearance> The appearance of the steel sheet was visually observed, and those without any appearance defects such as bare spots, indentations due to the pick-up phenomenon, or uneven alloying were rated as "◎", those with slight appearance defects but within the acceptable range for the product were rated as "◯", and those with clear uneven alloying, bare spots, or indentations were rated as "×". If the above evaluation was "◯" or "◎", the appearance was judged to be good.
[0108] <Tensile Properties> Tensile properties were measured using a JIS No. 5 test piece with the rolling direction as the tensile direction according to a method in accordance with JIS Z2241.
[0109] <LME cracking resistance> A test piece was cut out from a hot-dip galvanized steel sheet, measuring 150 mm in the longitudinal direction and 50 mm in the transverse direction, with the direction perpendicular to the rolling (TD) as the longitudinal direction and the rolling direction as the transverse direction. The test piece was cut out to the same size, and the coating weight of the hot-dip galvanized layer on one side was 50 g / m. 2 The test specimen was stacked with a test hot-dip galvanized steel sheet (thickness: 1.2 mm, TS: 980 MPa class) to form a sheet assembly. This sheet assembly was assembled so that the hot-dip galvanized layer of the test specimen was aligned with the hot-dip galvanized layer surface of the commercially available hot-dip galvanized steel sheet. As shown in Figure 1, this sheet assembly was fixed to a fixing table via a 2.0 mm thick spacer at a 5° inclination, the maximum inclination expected for some part shapes. The spacer was a pair of steel plates measuring 50 mm in the longitudinal direction, 45 mm in the transverse direction, and 2.0 mm thick. The longitudinal end faces of each of the pair of steel plates were aligned with both transverse end faces of the sheet assembly. Therefore, the distance between the pair of steel plates constituting the spacer was 60 mm. The fixing table was a single plate with a hole in the center.
[0110] Next, using a servomotor-operated single-phase AC (50 Hz) resistance welding machine, the sheet assembly was pressed with a pair of electrodes (tip diameter: 6 mm) while being deflected. Resistance welding was performed under the following conditions: a pressure of 3.5 kN, a hold time of 0.10 or 0.16 seconds, and a welding current and welding time that resulted in a nugget diameter of 5.9 mm for the weld (i.e., the welding current and welding time were appropriately adjusted for each sheet assembly so that the nugget diameter was 5.9 mm). This produced a sheet assembly with a weld. The pair of electrodes pressed the sheet assembly from above and below in the vertical direction, and the lower electrode pressed the test piece through a hole in the fixture. During pressing, the lower electrode and the fixture were fixed so that the lower electrode of the pair of electrodes was in contact with a plane extending from the contact surface between the spacer and the fixture, and the upper electrode was movable. The upper electrode was also in contact with the center of the hot-dip galvanized steel sheet for the test.
[0111] The hold time refers to the time from when the welding current is finished flowing to when the electrodes start to be released. The nugget diameter refers to the distance of the end 10 of the nugget in the longitudinal direction of the sheet assembly, as shown in Figure 2.
[0112] Next, as shown in Figure 2, the sheet assembly with the weld was cut to include the weld (nugget), and the cross section of the weld was observed with an optical microscope (200x magnification). The resistance weld crack resistance properties of the weld were evaluated according to the following criteria. Here, the upper diagram in Figure 2 is a plan view of the sheet assembly with the weld, showing the cutting position. The lower diagram in Figure 2 is a drawing showing a cross section in the sheet thickness direction of the sheet assembly after cutting, and schematically shows cracks that occurred in the test specimen. Note that if cracks occur in the test hot-dip galvanized steel sheets, the stress in the test specimen will be dispersed, preventing appropriate evaluation. For this reason, data from when no cracks occurred in the test hot-dip galvanized steel sheets was used as an example.
[0113] If the evaluation below was "◯" or "◎", the resistance weld crack resistance characteristics of the welded part were judged to be good and excellent, respectively, and if it was "×", the resistance weld crack resistance characteristics of the welded part were judged to be poor.
[0114] ⊚: No cracks of 0.1 mm or more in length are observed with a hold time of 0.10 seconds. ◯: Cracks of 0.1 mm or more in length are observed with a hold time of 0.10 seconds, but no cracks of 0.1 mm or more in length are observed with a hold time of 0.16 seconds. ×: Cracks of 0.1 mm or more in length are observed with a hold time of 0.16 seconds.
[0115] <Dehydrogenation Behavior> A rectangular test piece measuring 30 mm in major axis length and 5 mm in minor axis length was taken from the width center of a hot-dip galvanized steel sheet. The coating layer of the test piece was removed using a router. Immediately, hydrogen analysis was performed using a thermal desorption analyzer under conditions of an analysis start temperature of 25°C, an analysis end temperature of 300°C, and a heating rate of 200°C / hour. The amount of released hydrogen (mass ppm / min), which is the amount of hydrogen released from the surface of the test piece at each temperature, was measured. The total amount of released hydrogen from the analysis start temperature to 300°C was calculated as the amount of diffusible hydrogen in the steel. Here, a diffusible hydrogen amount in the steel of 0.01 mass ppm or less was rated as the highest grade "◎++", a grade of 0.06 mass ppm or less was rated as very good "◎+", a grade of 0.10 mass ppm or less was rated as good "◎", and a grade of 0.30 mass ppm or less was rated as pass grade "◯". Furthermore, based on experience, when the amount of diffusible hydrogen in steel exceeds 0.30 ppm by mass, the delayed fracture resistance of the steel sheet often deteriorates, and therefore, a value of 0.30 ppm by mass or more was marked as ×. The dehydrogenation behavior was judged to be excellent when marked with "◎" or "◯".
[0116] <Damage to Furnace Body> Damage to the furnace body was evaluated by visual inspection to see whether discoloration was observed on the steel shell (SUS310S) inside the annealing furnace. Here, when no discoloration was observed on the steel shell, it was rated as "Good" and determined that no damage to the furnace body was caused. When clear discoloration was observed, it was rated as "Poor" and determined that damage to the furnace body was caused. The results obtained above are shown in Table 3 together with the manufacturing conditions.
[0117]
[0118] As can be seen from Table 3, the examples of the present invention, despite being high-strength hot-dip galvanized steel sheets containing Si, are excellent in LME cracking resistance, have good coating appearance, and have a small amount of diffusible hydrogen in the steel sheet, and are expected to have good delayed fracture resistance and cause little damage to the furnace body. On the other hand, the comparative examples produced outside the scope of the present invention are inferior in at least one of LME cracking resistance, coating appearance, amount of diffusible hydrogen in the steel sheet, and damage to the furnace body.
[0119] [Example 2] Similarly, a 1.2 mm cold-rolled sheet having the chemical composition shown in Table 1 was subjected to annealing and hot-dip galvanizing in a CGL. Oxidation heating was performed in a direct-fire heating furnace having a nozzle mix burner separated into two zones under the conditions shown in Table 4. Reduction annealing was performed in a radiant tube heating furnace separated into two zones by seal rolls under the conditions shown in Table 4, followed by cooling. Subsequently, hot-dip galvanizing was performed using a bath containing 0.135% Al at 460°C, and then the coating weight was reduced to approximately 50 g / m by gas wiping. 2 In Table 4, in the first reduction annealing, the steel sheet was held at the maximum temperature reached for the time shown in the table, and in the second reduction annealing, the steel sheet was held at the maximum temperature reached for the time shown in the table.
[0120] Subsequently, the appearance of the high-strength hot-dip galvanized steel sheets obtained as described above was evaluated, and the tensile properties were investigated in the same manner as in Example 1. Furthermore, the LME cracking resistance, dehydrogenation behavior, and damage to the furnace body were evaluated.
[0121]
[0122] The results obtained as described above are shown in Table 5.
[0123]
[0124] As can be seen from Table 5, the inventive examples, despite being high-strength hot-dip galvanized steel sheets containing Si, have excellent LME cracking resistance, good coating appearance, and low amounts of diffusible hydrogen in the steel sheets, so that good delayed fracture resistance can be expected and damage to the furnace body is minimal. Furthermore, by using a direct-fired heating furnace with the oxidation heating process separated into two zones, LME cracking resistance, coating appearance, and reduction of diffusible hydrogen in the steel are all achieved at a high level.
[0125] [Example 3] Similarly, a 1.2 mm cold-rolled sheet having the chemical composition shown in Table 1 was subjected to annealing and hot-dip galvanizing in a CGL. Oxidation heating was performed under the conditions shown in Table 6 in a direct-fire heating furnace having a nozzle mix burner separated into two zones. Reduction annealing was performed under the conditions shown in Table 6 in a radiant tube heating furnace separated into two zones by seal rolls, followed by cooling. The hydrogen concentrations in both the first reduction annealing and the second reduction annealing in the annealing furnace during reduction annealing were reduced. Subsequently, hot-dip galvanizing was performed using a 460°C bath containing 0.135% Al, and then the steel sheet was gas wiped to a coating weight of approximately 50 g / m. 2 In Table 6, in the first reduction annealing, the steel sheet was held at the maximum temperature reached for the time shown in the table, and in the second reduction annealing, the steel sheet was held at the maximum temperature reached for the time shown in the table.
[0126] Subsequently, the appearance of the high-strength hot-dip galvanized steel sheets obtained as described above was evaluated, and the tensile properties were investigated in the same manner as in Example 1. Furthermore, the LME cracking resistance, dehydrogenation behavior, and damage to the furnace body were evaluated.
[0127]
[0128] The results obtained as described above are shown in Table 7.
[0129]
[0130] As can be seen from Table 7, the inventive examples, despite being high-strength hot-dip galvanized steel sheets containing Si, have excellent LME cracking resistance, good coating appearance, and a small amount of diffusible hydrogen in the steel sheet, so that good delayed fracture resistance can be expected and damage to the furnace body is minimal. Furthermore, by lowering the hydrogen concentration in the annealing furnace, it is possible to minimize diffusible hydrogen in the steel.
[0131] The high-strength hot-dip galvanized steel sheet obtained by the production method of the present invention has excellent appearance quality and resistance weld cracking resistance, and at the same time, can suppress deterioration of delayed fracture resistance due to hydrogen embrittlement, and can be used as a surface-treated steel sheet for reducing the weight and increasing the strength of automobile bodies themselves.
[0132] REFERENCE SIGNS LIST 1 Test hot-dip galvanized steel sheet 2 Test piece 3 Spacer 4 Electrode 5 Fixing base 6 Nugget 7 Nugget diameter 8 Cutting line
Claims
1. A method for producing a high-strength hot-dip galvanized steel sheet, comprising oxidizing a steel sheet containing, by mass%, 0.45% to 2.0% Si, followed by reduction annealing and hot-dip galvanizing, wherein the oxidation treatment is carried out to remove N 2 and 500 volume ppm or more O 2 The steel sheet is oxidized in an oxidation step in which the temperature is set to 500° C. or more and 800° C. or less in an atmosphere containing the above-mentioned, and the reduction annealing is performed in different atmospheres in the front and rear stages. In the first reduction annealing in the front stage, the steel sheet is oxidized in an atmosphere containing the above-mentioned, the dew point of which is −45° C. or more and +20° C. or less, and the hydrogen is 5.0 vol.% or more and 25 vol.% or less, and the balance N. 2 In the latter stage, the steel sheet after the first reduction annealing is subjected to a second reduction annealing in an atmosphere containing 2.0 vol. % or more and 8.0 vol. % or less of hydrogen and the balance N at a dew point of −10 ℃ or more and +20 ℃ or less of an annealing atmosphere. 2 and the hydrogen concentration in the first reduction annealing step is H 2 a, the hydrogen concentration in the second reduction annealing in the latter stage is H 2 When b, H 2 a>H 2 The method for producing a high-strength hot-dip galvanized steel sheet comprises holding the steel sheet at a temperature of 700°C or higher and 950°C or lower for 30 seconds or longer and 300 seconds or shorter in an atmosphere in which the hydrogen concentration is adjusted to satisfy b) and then performing hot-dip galvanization.
2. The method for producing high-strength hot-dip galvanized steel sheet according to claim 1, wherein the reduction annealing is performed in an annealing furnace that is divided into two or more parts in the running direction of the steel sheet and is capable of annealing in two or more different atmospheres.
3. A method for producing a high-strength hot-dip galvanized steel sheet according to claim 1 or 2, wherein the steel sheet is subjected to hot-dip galvanizing and then to an alloying treatment of the hot-dip galvanizing.
4. A method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 3, wherein the oxidation treatment is carried out in a temperature increasing process of the steel sheet which is carried out as a pre-process of reduction annealing.
5. The method for producing a high-strength hot-dip galvanized steel sheet according to claim 4, wherein the oxidation treatment is carried out at a temperature in the range of 500°C or higher and 800°C or lower, at least 50°C or higher.
6. A method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 5, wherein the oxidation treatment is performed using a direct-fired furnace (DFF) and the air ratio of at least a part of the atmosphere in the furnace is set to 1.0 or more to oxidize the steel sheet surface.
7. The oxidation treatment is performed using a direct-fired heating furnace that is divided into two or more parts in the steel sheet running direction and capable of oxidizing in two or more atmospheres. In the first heating zone in the front stage of the heating furnace, when the air ratio in the temperature range in which the oxidation treatment is performed is α, the average heating rate at 200°C or higher is 10°C / sec or more and 50°C / sec or less, and the T calculated from the following formula (1) is performed. 1 In the second heating zone at the rear of the heating furnace, the steel sheet that has passed through the first heating zone is heated to a temperature of 0.9 or less and an air ratio of 0.9 or less and a temperature of 0.5 or less. 1 (°C) is calculated from the following formula (2) under the condition that the average heating rate is 5°C / sec or more and 30°C / sec or less. 2 The method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 6, wherein the steel sheet is heated to a temperature of at least T 1 =28.2[Si]+7.95[Mn]-86.2α+666 ---(1) T 2 = T 1 +30 --- (2) Here, [Si] is the Si content (mass%) contained in the steel plate, and [Mn] is the Mn content (mass%) contained in the steel plate.
8. The oxidation treatment is carried out using N 2 and 500 volume ppm or more O 2 Including CO, CO 2 , H 2 O, NO X The method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 7, wherein the method is carried out in an atmosphere containing one or more of:
9. The method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 5 and 8, wherein the oxidation treatment is carried out using a radiant tube type heating furnace.
10. A method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 5, 8 and 9, wherein the reduction annealing is carried out using a radiant tube type heating / soaking furnace.
11. In the second reduction annealing, the hydrogen in the annealing atmosphere is 2.0 vol.% or more and less than 5.0 vol.%, and the balance is N 2 The method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 10, comprising:
12. In the first reduction annealing, the hydrogen in the annealing atmosphere is 5.0 vol.% or more and 12 vol.% or less, and the balance is N 2 In the second reduction annealing, the hydrogen in the annealing atmosphere is 2.0 vol.% or more and less than 3.0 vol.%, and the balance is N. 2 The method for producing a high-strength hot-dip galvanized steel sheet according to any one of claims 1 to 11, comprising:
Citation Information
Patent Citations
Method for manufacturing alloyed hot-dip galvanized steel sheets with excellent plating adhesion and sliding properties
JP5652219B2
High-strength hot-dip galvanized steel sheet and manufacturing method thereof
JP6052270B2
Manufacturing method and manufacturing equipment for high-strength hot-dip galvanized steel sheet
JP6172297B2
Method for producing hot dip galvannealed steel sheet having excellent plating adhesion and sliding property
JP2012149307A
Method for manufacturing steel sheet products with a metal protective layer formed by hot-dip plating.
JP2014525986A
Cited By
Method for analyzing the thickness of a low solid solution Si concentration layer and method for evaluating the LME resistance of steel materials
JP7841671B1
Method for analyzing thickness of low solubility solution si concentration layer and method for evaluating lme resistance of steel material
WO2026105490A1