Method for producing modified recycled carbon black and modified recycled carbon black

The continuous combustion process addresses the poor reinforcing properties of recycled carbon black by removing rubber residues, enabling enhanced bonding with rubber components and continuous production, thus improving the performance of recycled carbon black in rubber products.

WO2024224657A1PCT designated stage expired Publication Date: 2024-10-31TOKAI CARBON CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/032624
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2023-09-07
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Recycled carbon black produced from pyrolyzing waste tires has poor reinforcing properties for rubber products due to the presence of rubber residues on its surface, which inhibit adsorption and require batch-wise production methods.

Method used

A continuous method involving a main burner and optional auxiliary burner to oxidize and decompose rubber residues from recycled carbon black using a controlled combustion process, ensuring the carbon black is modified to enhance its surface properties and bonding with rubber components.

Benefits of technology

The method effectively removes rubber residues, enhancing the reinforcing properties of recycled carbon black and allowing for continuous production, thereby improving the performance of rubber products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023032624_31102024_PF_FP_ABST
    Figure JP2023032624_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This method for producing modified recycled carbon black is characterized by involving a main burner modification step in which main burner fuel, an oxygen-containing gas, and a recycled carbon black raw material are continuously supplied to a main burner generating flames by burning fuel, to burn the main burner fuel, and while continuously generating flames by the main burner, the recycled carbon black raw material is introduced into the flames and allowed to pass through the flames, wherein the total carbon burning rate of the main burner represented by formula (1) is less than 100.0%. Formula (1): main burner total carbon burning rate (%) = (A / (B + C)) × 100. According to the present invention, it is possible to provide a method for producing modified recycled carbon black, the method being capable of effectively removing rubber residues attached to a surface of a recycled carbon black raw material and being able to be continuously performed.
Need to check novelty before this filing date? Find Prior Art

Description

Modified recycled carbon black manufacturing method and modified recycled carbon black

[0001] The present invention relates to recycled carbon black having a modified surface state, a method for producing the same, and a rubber composition using the same.

[0002] In recent years, efforts to reduce the burden on the global environment, such as carbon neutrality and sustainability, have been actively pursued. As part of these sustainability efforts, the carbon black industry is also considering the use of recycled carbon black obtained by pyrolysis of waste tires.

[0003] As a method for producing recycled carbon black by pyrolysis of waste tires or the like, for example, Patent Document 1 discloses a method in which waste tires are pyrolyzed at approximately 500°C while circulating nitrogen gas, and Patent Document 2 discloses a method in which waste rubber is treated in a two-stage pyrolysis process and the obtained material is pulverized.

[0004] Patent No. 5813985 WO2013 / 095145A1

[0005] However, recycled carbon black, which is obtained by pyrolyzing rubber products such as waste tires, has rubber residues, mainly composed of rubber charcoal, attached to its surface. When the recycled carbon black is mixed with a rubber composition, these rubber residues inhibit the adsorption of the recycled carbon black to the rubber component.

[0006] Therefore, recycled carbon black has a problem in that it has a low reinforcing effect on rubber products due to its weak bond with the rubber component.

[0007] Therefore, there is a demand for recycled carbon black with high reinforcing properties for rubber products. Furthermore, from an industrial viewpoint, a method for producing recycled carbon black with high reinforcing properties for rubber products continuously, rather than batchwise, is needed.

[0008] Therefore, an object of the present invention is to provide a method for producing modified recycled carbon black that can effectively remove rubber residue adhering to the surface of recycled carbon black and can be carried out continuously.

[0009] As a result of extensive research, the inventors have discovered that by continuously supplying main burner fuel, oxygen-containing gas, and recycled carbon black having charcoal adhering thereto to a main burner which burns fuel to generate a flame, and burning the main burner fuel, while continuously generating a flame in the main burner, and then introducing the recycled carbon black having rubber charcoal adhering thereto and passing it through the flame, the rubber residue adhering to the surface of the recycled carbon black is rapidly oxidized and decomposed by the high-temperature flame, which led to the completion of the present invention.

[0010] That is, the present invention provides a method for producing modified recycled carbon black, characterized in that: (1) a main burner modification step is performed by continuously supplying main burner fuel, oxygen-containing gas, and recycled carbon black having rubber carbonized particles adhered thereto to a main burner that is burning fuel to generate a flame, thereby burning the main burner fuel, and continuously introducing the recycled carbon black having rubber carbonized particles adhered thereto into the flame while the main burner is continuously generating a flame, thereby passing the recycled carbon black through the flame; and the main burner total carbon combustion rate, expressed by the following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized particles adhered thereto that is supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner), is less than 100.0%. (2) The method for producing modified recycled carbon black according to (1), characterized in that the main burner reforming step is a main burner reforming step (1) that sets the main burner flame combustion rate, expressed by the following formula (2): Main burner flame combustion rate (%) = (A / C) × 100 (2) (wherein A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner), to 100.0% or more. (3) The method for producing modified recycled carbon black according to (1), characterized in that the main burner reforming step is a main burner reforming step (2) that sets the main burner flame combustion rate, expressed by the following formula (2): Main burner flame combustion rate (%) = (A / C) × 100 (2) (wherein A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner), to less than 100.0%.(4) An auxiliary burner is provided downstream of the main burner, which burns auxiliary burner fuel to generate a flame, and an auxiliary burner reforming step is provided in which, while continuously generating a flame with the auxiliary burner, recycled carbon black after the main burner reforming step (1) is introduced into the flame generated by the auxiliary burner and passed through the flame, and the auxiliary burner reforming step makes the auxiliary burner flame combustion rate, expressed by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (wherein D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner), 100.0% or more, and satisfies the following formula (4): All burner total carbon combustion rate (%) = ((A + D) / (B + C + E)) × 100 (4) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto that is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel that is supplied to the auxiliary burner). (5) An auxiliary burner is provided downstream of the main burner, which burns auxiliary burner fuel to generate a flame, and an auxiliary burner reforming step is provided in which, while continuously generating a flame with the auxiliary burner, recycled carbon black after the main burner reforming step (1) is introduced into the flame generated by the auxiliary burner and passed through the flame, and the auxiliary burner reforming step satisfies the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (wherein D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner.and an auxiliary burner modification step (2) in which an auxiliary burner flame combustion rate, represented by the following formula (4), is less than 100.0%, and an overall burner total carbon combustion rate, represented by the following formula (4): Overall burner total carbon combustion rate (%) = ((A + D) / (B + C + E)) × 100 (4) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material adhered thereto, which is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel, which is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel, which is supplied to the auxiliary burner). (6) An auxiliary burner is provided downstream of the main burner, which burns auxiliary burner fuel to generate a flame, and an auxiliary burner reforming step is provided in which, while continuously generating a flame with the auxiliary burner, recycled carbon black after the main burner reforming step (2) is introduced into the flame generated by the auxiliary burner and passed through the flame, and the auxiliary burner reforming step makes the auxiliary burner flame combustion rate, expressed by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (wherein D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner), 100.0% or more, and satisfies the following formula (4): All burner total carbon combustion rate (%) = ((A + D) / (B + C + E)) × 100 (4) (In the formula, A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black to which rubber carbonized material is attached that is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel that is supplied to the auxiliary burner.(1) an auxiliary burner modification step for modifying the total carbon combustion rate of all burners, expressed as (a) above, to less than 100.0%; (7) An auxiliary burner is provided downstream of the main burner, which burns auxiliary burner fuel to generate a flame, and an auxiliary burner reforming step is provided in which, while continuously generating a flame with the auxiliary burner, recycled carbon black after the main burner reforming step (2) is introduced into the flame generated by the auxiliary burner and passed through the flame, and the auxiliary burner reforming step makes the auxiliary burner flame combustion rate, expressed by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (wherein D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner), less than 100.0%, and satisfies the following formula (4): All burner total carbon combustion rate (%) = ((A + D) / (B + C + E)) × 100 (4) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto that is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel that is supplied to the auxiliary burner).(8) A method for producing modified recycled carbon black according to (2) or (3), comprising an auxiliary fuel pyrolysis step in which a fuel nozzle is provided downstream of the main burner, and auxiliary fuel is introduced from the fuel nozzle into or near a flame generated by the main burner, thereby pyrolyzing the auxiliary fuel, wherein the auxiliary fuel pyrolysis step achieves an overall reaction total carbon combustion rate of less than 100.0%, as expressed by the following formula (5): Total carbon combustion rate (%) = (A / (B+C+F)) × 100 (5) (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material adhering thereto, which is supplied to the main burner, C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner, and F represents the theoretical amount of oxygen required for complete combustion of the auxiliary fuel supplied from the fuel nozzle). (9) A method for producing modified recycled carbon black according to (1), characterized in that it comprises a particle size adjustment step of pulverizing and / or classifying the recycled carbon black to which the rubber carbonized material is attached before carrying out the main burner modification step. (10) Modified recycled carbon black obtained by carrying out any of the methods for producing modified recycled carbon black according to (1) to (9).

[0011] According to the present invention, it is possible to provide a method for producing modified recycled carbon black that can effectively remove rubber residue adhering to the surface of recycled carbon black and can be carried out continuously.

[0012] FIG. 1 is a modified recycled carbon black manufacturing apparatus according to an embodiment of the present invention for carrying out a modified recycled carbon black manufacturing method; FIG. 2 is a schematic diagram showing an embodiment of a main burner reforming step; FIG. 3 is a schematic diagram showing an embodiment of a main burner reforming step and an auxiliary burner reforming step; FIG. 4 is a schematic end view showing the structure of an embodiment of a main burner; FIG. 5 is a schematic end view showing the structure of another embodiment of a main burner; FIG. 6 is a Raman spectrum of an embodiment of modified recycled carbon black according to the present invention; FIG. 7 is a Raman spectrum of an embodiment of recycled carbon black before modification.

[0013] Hereinafter, an embodiment of the present invention will be described in detail with reference to the accompanying drawings. The detailed description of the present invention below is an example of an embodiment, and the present invention should not be construed as being limited to this embodiment.

[0014] FIG. 1 is a schematic diagram of an example of a modified recycled carbon black production apparatus for illustrating the modified recycled carbon black production method of the present invention. In FIG. 1, the modified recycled carbon black production apparatus 1 includes a burner reforming section 2, which is equipped with a main burner 3, an auxiliary burner 4, and a cooling water supply pipe 5, and a collection section 7, which is equipped with a bag filter. The burner reforming section 2 and the collection section 7 are connected by a connecting pipe 6. The main burner 3 is installed above the burner reforming section 2, and is connected to a supply pipe for main burner fuel 11, a supply pipe for oxygen-containing gas 12, and a supply pipe for raw recycled carbon black and carrier gas 13. Furthermore, the auxiliary burner 4 is connected to a supply pipe for auxiliary burner fuel 14 and oxygen-containing gas 15.

[0015] As shown in Figure 2, in the burner reforming section 2, fuel is burned in the main burner 3 to generate a flame 21. With the flame 21 generated in the main burner 3, main burner fuel 11, oxygen-containing gas 12, raw recycled carbon black, and carrier gas 13 are continuously supplied to the main burner 3 from the fuel supply side toward the flame 21. This allows the main burner 3 to continuously generate the flame 21 while the raw recycled carbon black is introduced from the fuel supply side into the flame 21 generated by the main burner 3 and passes through the flame 21. As the raw recycled carbon black passes through the flame 21 generated by the main burner 3, the surface of the recycled carbon black is modified. Figure 2 shows the direction of movement 22 of the raw recycled carbon black, and the recycled carbon black moves from the fuel supply side toward the tip of the flame 21 generated by the main burner 3.

[0016] As shown in Figure 3, in the burner reforming section 2, in addition to reforming using the main burner 3, reforming using the auxiliary burner 4 can also be performed. As in Figure 2, recycled carbon black is introduced into flame 21 generated by main burner 3 and passed through flame 21. After that, fuel is combusted by auxiliary burner 4 to generate flame 23. With flame 23 generated by auxiliary burner 4, the recycled carbon black that has passed through flame 21 generated by main burner 3 is introduced into flame 23 generated by auxiliary burner 4 and passed through flame 23. Then, as the recycled carbon black that has passed through flame 21 generated by main burner 3 passes flame 23 generated by auxiliary burner 4, the surface of the recycled carbon black is further modified. Figure 3 shows the movement direction 22 of the recycled carbon black. After passing flame 21 generated by main burner 3, the recycled carbon black is introduced into flame 23 generated by auxiliary burner 4 and passes through flame 23.

[0017] In the burner reforming section 2, the main burner 3 is always used to reform the recycled carbon black, and the auxiliary burner 4 is also used to reform the recycled carbon black as needed.

[0018] After the raw recycled carbon black is passed through the flame generated by the main burner 3 in the burner reforming section 2, or after it is passed through the flame generated by the main burner 3 and the flame generated by the auxiliary burner 4, cooling water is supplied into the burner reforming section 2 from a cooling water supply pipe 5 installed below the burner reforming section 2, and the recycled carbon black is brought into contact with the cooling water 16 to be cooled.

[0019] Next, the cooled recycled carbon black and gases such as combustion gas, decomposition gas, and water vapor are introduced into a collection unit 7 via a connecting pipe 6, and separated into gas 17 and modified recycled carbon black 18 by a bag filter installed in the collection unit 7, thereby obtaining modified recycled carbon black 18.

[0020] The method for producing modified recycled carbon black of the present invention includes a main burner modification step of continuously supplying main burner fuel, oxygen-containing gas, and recycled carbon black having rubber carbonized particles attached thereto to a main burner that is burning fuel to generate a flame, thereby burning the main burner fuel, and continuously introducing the recycled carbon black having rubber carbonized particles attached thereto into the flame while the main burner is continuously generating a flame, thereby allowing the recycled carbon black to pass through the flame; and the method is characterized by achieving a main burner total carbon combustion rate, expressed by the following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized particles attached thereto that is supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner).

[0021] The main burner modification step in the method for producing modified recycled carbon black of the present invention is a step of modifying the surface of the recycled carbon black to which carbides are attached by continuously supplying main burner fuel, oxygen-containing gas, and recycled carbon black to which carbides are attached to a main burner that burns fuel to generate a flame.

[0022] In the main burner reforming process, recycled carbon black (hereinafter also referred to as raw recycled carbon black) having charcoal attached thereto, which is the raw material for reforming, is carbon black obtained by pyrolyzing rubber products such as waste tires, and is carbon black having rubber residue, primarily composed of rubber charcoal, attached to its surface. Examples of raw recycled carbon black, which is the raw material for reforming, include PB365 manufactured by Enrestec, BolderBlack manufactured by Bolder Industries, DE-Black manufactured by Delta Energy, and MondoBlack manufactured by ECOLOMONDO. Such raw recycled carbon black may be produced by any production method, and is not particularly limited, but examples thereof include the method described in Patent Document 2.

[0023] The raw material recycled carbon black has a Raman spectrum of 1350±10 cm in a Raman spectrum obtained by measuring with an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak (D band) having a peak top in the range of 1580 ± 20 cm -1 The peak intensity of a peak (G band) having a peak top in this range (hereinafter also referred to as the G band intensity when the D band intensity is taken as 100) is 112 or more and 200 or less, preferably 112 or more and 190 or less. The G band intensity when the D band intensity is taken as 100 will be described later.

[0024] Raw recycled carbon black is obtained by modifying recycled carbon black obtained by pyrolysis of rubber products such as waste tires. Therefore, the ash content of raw recycled carbon black is, for example, 3.0% or more and 50.0% or less, preferably 5.0% or more and 35.0% or less.

[0025] In the present invention, the ash content means a value measured by the method specified in JIS K 6218-2.

[0026] The main burner fuel in the main burner reforming step is not particularly limited as long as it burns with the oxygen in the oxygen-containing gas when it comes into contact with the flame generated by the main burner and generates a flame. Examples of the fuel include hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene, hydrogen, ammonia, mixed gases of these, and gases generated by the thermal decomposition of rubber and plastics. Also included as liquid fuels are aromatic hydrocarbons such as naphthalene and anthracene, coal-based hydrocarbons such as creosote oil and tar oil, petroleum-based heavy oils such as FCC residual oil and ethylene heavy end oil, acetylenic unsaturated hydrocarbons, and aliphatic hydrocarbons such as hexane, vegetable oils such as rapeseed oil and soybean oil, and oils generated by the thermal decomposition of rubber and plastics. Hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene are preferred because they produce a higher flame temperature.

[0027] Examples of the oxygen-containing gas used in the main burner reforming step include oxygen gas, a gas containing oxygen, and air, with air being preferred from the viewpoint of economy.

[0028] In the main burner reforming process, the main burner fuel, oxygen-containing gas, and recycled carbon black having carbides attached thereto are continuously supplied from the fuel supply side to the main burner, which is burning the main burner fuel to generate a flame, thereby burning the main burner fuel, and while continuously generating a flame in the main burner, the raw recycled carbon black is introduced into the flame generated by the main burner and passed through the flame.

[0029] In the main burner reforming step, the raw recycled carbon black is supplied to the main burner using a carrier gas. The carrier gas may be an inert gas such as nitrogen gas, argon gas, or helium gas, or an oxygen-containing gas such as oxygen gas, a gas containing oxygen, or air. An oxygen-containing gas is preferred as the carrier gas because it facilitates oxidation of the raw recycled carbon black.

[0030] In the main burner reforming process, the raw recycled carbon black transported in the carrier gas, the oxidizing gas, and the main burner fuel can be supplied to the main burner via separate routes. Alternatively, in the main burner reforming process, the raw recycled carbon black and the oxidizing gas can be mixed first, and the resulting mixture and the main burner fuel can be supplied to the main burner.

[0031] In the main burner reforming step, when the raw material recycled carbon black and the oxygen-containing gas are introduced into the flame, a mixed flow of the raw material recycled carbon black and the oxygen-containing gas is introduced into the flame. This allows the oxygen-containing gas to be present in the vicinity of the raw material recycled carbon black when it is introduced into the flame. This allows priority to be given to contact between the raw material recycled carbon black and the oxygen-containing gas over contact between the raw material recycled carbon black and the fuel gas, making it easier for oxidation of the raw material recycled carbon black to occur.

[0032] In the main burner reforming step, (i) when the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel are introduced into the flame, the raw recycled carbon black is positioned at the center, the oxygen-containing gas is positioned so as to surround the raw recycled carbon black, and the main burner fuel is positioned so as to surround the oxygen-containing gas, when viewed in a plane perpendicular to the direction of movement of the raw recycled carbon black, and the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel can be introduced into the flame; and (ii) when the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel are introduced into the flame, the main burner fuel is positioned at the center, when viewed in a plane perpendicular to the direction of movement of the raw recycled carbon black, (iii) when the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel are introduced into the flame, when viewed from a plane perpendicular to the direction of movement of the raw recycled carbon black, the raw recycled carbon black can be placed at the center, the main burner fuel can be placed so as to surround the raw recycled carbon black, and the oxygen-containing gas can be placed so as to surround the main burner fuel, and the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel can be introduced into the flame. Of these, (i) and (ii) are preferred in that they allow an oxygen-containing gas to be present in the vicinity of the raw material recycled carbon black when it is introduced into the flame, thereby allowing contact between the raw material recycled carbon black and the oxygen-containing gas to take precedence over contact between the raw material recycled carbon black and the fuel gas, thereby facilitating oxidation of the raw material recycled carbon black.

[0033] In the main burner reforming process, the temperature of the flame generated by the main burner is high, so when the raw recycled carbon black passes through the flame generated by the main burner, the rubber residue, mainly composed of rubber charcoal, adhering to the surface of the raw recycled carbon black is quickly oxidatively decomposed and removed. Furthermore, in the main burner reforming process, the raw recycled carbon black is supplied to the main burner together with the main burner fuel and oxygen-containing gas, and is exposed to high temperatures only while passing through the flame generated by the main burner, so the time of exposure to high temperatures is short. Therefore, the surface of the raw recycled carbon black is selectively oxidized.

[0034] On the other hand, when raw recycled carbon black is supplied to a heating furnace together with an oxidizing gas and oxidized in the heating furnace, the temperature to which the raw recycled carbon black is exposed is not as high as that of the flame, and the time for which the raw recycled carbon black is heated is long. If the temperature to which the raw recycled carbon black is exposed is low, oxidation will proceed from the parts that are easily oxidized and decomposed, but if the time is long, oxidation will progress to the interior of the raw recycled carbon black particles, forming pores in the raw recycled carbon black.

[0035] In the main burner reforming step, the main burner total carbon combustion rate, expressed by the following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) × 100 (1) (where A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required to completely combust the recycled carbon black having rubber carbonized particles attached thereto that is supplied to the main burner, and C refers to the theoretical amount of oxygen required to completely combust the main burner fuel that is supplied to the main burner.) Note that A is the amount of oxygen supplied to the main burner per unit time, B is the amount of theoretical oxygen required per unit time to completely combust the carbon content calculated by assuming that all components excluding ash of the recycled carbon black having rubber carbonized particles attached thereto that is supplied to the main burner are carbon, and C is the amount of theoretical oxygen required per unit time to completely combust the main burner fuel that is supplied to the main burner.

[0036] In the main burner reforming process, controlling the main burner total carbon combustion rate to less than 100.0% means preventing complete combustion of the main burner fuel and raw recycled carbon black supplied to the main burner. If the main burner fuel and raw recycled carbon black supplied to the main burner were completely burned, the recycled carbon black would be oxidized and lost, and modified recycled carbon black would not be obtained. Therefore, by controlling the main burner total carbon combustion rate to less than 100.0%, modification by oxidative decomposition of the surface of the raw recycled carbon black can be achieved. From the viewpoint of the balance between the recovery amount of the resulting modified particles and the amount of rubber char that needs to be removed, the main burner total carbon combustion rate is preferably 10.0% or more and 90.0% or less, more preferably 15.0% or more and 80.0% or less.

[0037] In the method for producing modified recycled carbon black of the present invention, the main burner modification step includes a main burner modification step (1) that sets the main burner flame combustion rate, expressed by the following formula (2): Main burner flame combustion rate (%) = (A / C) × 100 (2) (where A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner), to 100.0% or more.

[0038] In the main burner reforming process (1), controlling the main burner flame combustion rate to 100.0% or more means completely combusting the main burner fuel supplied to the main burner. In the main burner reforming process (1), by setting the main burner flame combustion rate to 100.0% or more, the surface of the raw recycled carbon black is more easily oxidized, thereby improving the oxidative removal of residual rubber adhering to the raw recycled carbon black. From the viewpoint of the balance between the flame temperature and the amount of rubber char that needs to be removed, the main burner flame combustion rate is preferably 105.0% or more and 500.0% or less, and more preferably 110.0% or more and 400.0% or less. Since the main burner reforming process (1) is a form of the main burner reforming process, the main burner total carbon combustion rate is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.

[0039] In the method for producing modified recycled carbon black of the present invention, the main burner modification step may be a main burner modification step (2) that adjusts the main burner flame combustion rate, expressed by the following formula (2): Main burner flame combustion rate (%) = (A / C) × 100 (2) (where A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner), to less than 100.0%.

[0040] In the main burner reforming step (2), controlling the main burner flame combustion rate to less than 100.0% means preventing complete combustion of the main burner fuel supplied to the main burner. Heating the main burner fuel under conditions that prevent complete combustion of the main burner fuel causes the main burner fuel to pyrolyze and generate carbides. The generated carbides are then attached to the surface-modified recycled carbon black as it passes through the flame generated by the main burner, thereby adjusting the specific surface area of ​​the modified recycled carbon black. From the viewpoint of the appropriate value of specific surface area for improving the reinforcement properties of rubber, the main burner flame combustion rate is preferably 20.0% or more and 99.0% or less, more preferably 30.0% or more and 95.0% or less. Since the main burner reforming step (2) is one form of the main burner reforming step, the main burner total carbon combustion rate is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.

[0041] The method for producing modified recycled carbon black of the present invention can include an auxiliary burner modification step in which an auxiliary burner is provided downstream of the main burner to burn auxiliary burner fuel to generate a flame, and the recycled carbon black after the main burner modification step is introduced into the flame generated by the auxiliary burner while the flame is continuously generated by the auxiliary burner, and the recycled carbon black is passed through the flame. In the method for producing modified recycled carbon black of the present invention, the auxiliary burner modification step is performed as necessary.

[0042] The auxiliary burner reforming step in the method for producing modified recycled carbon black of the present invention is a step in which a flame is generated by burning auxiliary burner fuel downstream of the flame generated by the main burner, and the recycled carbon black after the main burner reforming step is continuously supplied so as to be introduced into the flame generated by the auxiliary burner and passed through the flame, thereby modifying the surface of the recycled carbon black.

[0043] The recycled carbon black that is reformed in the auxiliary burner reforming step is the recycled carbon black that has been subjected to the main burner reforming step, i.e., the recycled carbon black that has passed through the flame generated by the main burner or the recycled carbon black that has passed near the tip of the flame generated by the main burner.

[0044] In the auxiliary burner reforming step, auxiliary burner fuel and oxygen-containing gas are continuously supplied to the auxiliary burner to continuously generate a flame. The position of the flame generated by the auxiliary burner is the tip of the flame generated by the main burner, within the flame generated by the main burner and near the tip of the flame, or outside the flame generated by the main burner and near the tip of the flame, preferably outside the flame generated by the main burner and near the tip of the flame.

[0045] The fuel for the auxiliary burner in the auxiliary burner reforming step is not particularly limited as long as it burns with the oxygen in the oxygen-containing gas when it comes into contact with the flame generated by the auxiliary burner and generates a flame. Examples of the fuel include hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene, hydrogen, ammonia, mixed gases of these, and gases generated by the thermal decomposition of rubber and plastics. Also, liquid fuels include aromatic hydrocarbons such as naphthalene and anthracene, coal-based hydrocarbons such as creosote oil and tar oil, petroleum-based heavy oils such as FCC residual oil and ethylene heavy end oil, acetylenic unsaturated hydrocarbons, and aliphatic hydrocarbons such as hexane, vegetable oils such as rapeseed oil and soybean oil, and oils generated by the thermal decomposition of rubber and plastics. Hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene are preferred because they produce a higher flame temperature.

[0046] Examples of the oxygen-containing gas used in the auxiliary burner reforming step include oxygen gas, a gas containing oxygen, and air, with air being preferred from the viewpoint of economy.

[0047] Then, in the auxiliary burner reforming step, the auxiliary burner fuel is burned to generate a flame in the auxiliary burner, and while the flame is continuously generated in the auxiliary burner, the recycled carbon black after the main burner reforming step is introduced into the flame generated by the auxiliary burner and passed through the flame.

[0048] The auxiliary burner reforming step involves setting the auxiliary burner flame combustion rate, expressed by the following formula (3): auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (wherein D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner), to 100.0% or more, and also setting the auxiliary burner flame combustion rate, expressed by the following formula (4): all burner total carbon combustion rate (%) = ((A + D) / (B + C + E)) × 100 (4) (where A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto that is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel that is supplied to the auxiliary burner.) An example of such a process is an auxiliary burner modification step (1) that reduces the total carbon combustion rate of all burners, expressed as follows: to less than 100.0%. Note that D is the amount of oxygen supplied to the auxiliary burner per unit time, and E is the amount of theoretical amount of oxygen required per unit time for complete combustion of the auxiliary burner fuel that is supplied to the auxiliary burner.

[0049] In the auxiliary burner modification step (1), controlling the total carbon combustion rate of all burners to less than 100.0% means preventing complete combustion of the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burners. If the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burners were to be completely combusted, the recycled carbon black would be oxidized and lost, and modified recycled carbon black would not be obtained. From the viewpoint of the balance between the amount of modified particles recovered and the amount of rubber char that needs to be removed, the total carbon combustion rate of all burners is preferably 15.0% or more and 90.0% or less, more preferably 20.0% or more and 80.0% or less.

[0050] In the auxiliary burner reforming step (1), controlling the auxiliary burner flame combustion rate to 100.0% or more means completely combusting the auxiliary burner fuel supplied to the auxiliary burner. By setting the auxiliary burner flame combustion rate to 100.0% or more in the auxiliary burner reforming step (1), the surface of the recycled carbon black after the main burner reforming step is more easily oxidized, thereby improving the oxidative removal of residual rubber adhering to the recycled carbon black after the main burner reforming step. In other words, the auxiliary burner reforming step (1) can improve the oxidative removal of residual rubber that was not completely removed even after the main burner reforming step (1). From the viewpoint of the balance between the flame temperature and the amount of rubber char that needs to be removed, the auxiliary burner flame combustion rate is preferably 105.0% or more and 600.0% or less, more preferably 110.0% or more and 500.0% or less. Since the auxiliary burner reforming process (1) is one form of the auxiliary burner reforming process, the total carbon combustion rate of all burners is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.

[0051] The auxiliary burner reforming step involves making the auxiliary burner flame combustion rate, expressed by the following formula (3): auxiliary burner flame combustion rate (%) = (D / E) × 100 (3) (wherein D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner), less than 100.0%, and also making the auxiliary burner flame combustion rate, expressed by the following formula (4): all burner total carbon combustion rate (%) = ((A + D) / (B + C + E)) × 100 (4) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto which is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel which is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel which is supplied to the auxiliary burner.)

[0052] In the auxiliary burner modification step (2), controlling the total carbon combustion rate of all burners to less than 100.0% means preventing complete combustion of the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burners. If the auxiliary burner fuel and recycled carbon black supplied to the auxiliary burners were to be completely combusted, the recycled carbon black would be oxidized and lost, and modified recycled carbon black would not be obtained. From the viewpoint of the balance between the amount of modified particles recovered and the amount of rubber char that needs to be removed, the total carbon combustion rate of all burners is preferably 15.0% or more and 90.0% or less, more preferably 20.0% or more and 80.0% or less.

[0053] In the auxiliary burner modification step (2), controlling the auxiliary burner flame combustion rate to less than 100.0% means preventing complete combustion of the auxiliary burner fuel supplied to the auxiliary burner. Heating the auxiliary burner fuel under conditions that prevent complete combustion of the auxiliary burner fuel causes the auxiliary burner fuel to pyrolyze and generate char. The generated char is then attached to the surface-modified recycled carbon black as it passes through the flame generated by the auxiliary burner, thereby adjusting the specific surface area of ​​the modified recycled carbon black. From the viewpoint of the appropriate value of specific surface area for improving the reinforcement properties of rubber, the auxiliary burner flame combustion rate is preferably 2.0% or more and 90.0% or less, more preferably 5.0% or more and 80.0% or less. Since the auxiliary burner reforming step (2) is one form of the auxiliary burner reforming step, the total carbon combustion rate of all burners is less than 100.0%, preferably 15.0% or more and 90.0% or less, and more preferably 20.0% or more and 80.0% or less.

[0054] The method for producing modified recycled carbon black of the present invention can include an auxiliary fuel pyrolysis step in which a fuel nozzle is provided downstream of the main burner and auxiliary fuel is introduced into or near the flame generated by the main burner, thereby pyrolyzing the auxiliary fuel. The method for producing modified recycled carbon black of the present invention can include an auxiliary fuel pyrolysis step as needed.

[0055] Among the methods for producing modified recycled carbon black according to the present invention, an apparatus for carrying out an embodiment having an auxiliary fuel pyrolysis step is, for example, the modified recycled carbon black production apparatus 1 shown in FIG. 1 , which does not have an auxiliary burner and is provided with a fuel nozzle for introducing auxiliary fuel into or near the flame generated by the main burner.

[0056] The auxiliary fuel pyrolysis step in the method for producing modified recycled carbon black of the present invention is a step in which auxiliary fuel is introduced into or near a flame generated by a main burner, the auxiliary fuel is pyrolyzed to generate char, and the generated char is used to modify the surface of the recycled carbon black after the main burner reforming step. The auxiliary fuel is supplied from a position at the tip of the flame generated by the main burner, within the flame generated by the main burner and near the tip of the flame, or outside the flame generated by the main burner and near the tip of the flame.

[0057] What is reformed in the auxiliary fuel pyrolysis step is recycled carbon black after the main burner reforming step, i.e., recycled carbon black that has passed through the flame generated by the main burner or recycled carbon black that has passed through the flame generated by the main burner.

[0058] In the auxiliary fuel pyrolysis process, auxiliary fuel is introduced from a fuel nozzle provided downstream of the main burner. At this time, when the auxiliary fuel is supplied to the fuel nozzle and introduced from the fuel nozzle to the flame generated by the main burner or its vicinity, the auxiliary fuel supplied to the fuel nozzle is not mixed with an oxygen-containing gas. The auxiliary fuel used in the auxiliary fuel pyrolysis step is not particularly limited as long as it can be thermally decomposed by the heat of the flame of the main burner. Examples of the auxiliary fuel include hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene, mixed gases of these, and gases generated by the thermal decomposition of rubber or plastics. Also included as liquid fuels are aromatic hydrocarbons such as naphthalene and anthracene, coal-based hydrocarbons such as creosote oil and tar oil, petroleum-based heavy oils such as FCC residual oil and ethylene heavy end oil, acetylenic unsaturated hydrocarbons, and aliphatic hydrocarbons such as hexane, vegetable oils such as rapeseed oil and soybean oil, and oils generated by the thermal decomposition of rubber or plastics. Of these, hydrocarbon gases such as methane, ethane, propane, natural gas, ethylene, and acetylene are preferred in terms of uniformly modifying the recycled carbon black.

[0059] In the auxiliary fuel pyrolysis step, the total carbon combustion rate of all reactions, expressed by the following formula (5): Total Reaction Total Carbon Burnup Rate (%) = (A / (B+C+F)) × 100 (5) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black to which rubber carbonized material is attached that is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel that is supplied to the main burner, and F refers to the theoretical amount of oxygen required for complete combustion of the auxiliary fuel that is supplied from the fuel nozzle), is set to less than 100.0%. Note that F is the amount per unit time of the theoretical amount of oxygen required for complete combustion of the auxiliary fuel that is supplied from the fuel nozzle.

[0060] In the auxiliary fuel pyrolysis step, controlling the total carbon burn rate through all reactions to less than 100.0% means preventing complete combustion of the main burner fuel, recycled carbon black, and auxiliary fuel supplied to the main burner. If the main burner fuel, recycled carbon black, and auxiliary fuel supplied to the main burner were completely combusted, the recycled carbon black would be oxidized and lost, preventing the production of modified recycled carbon black. Furthermore, by heating the auxiliary fuel under conditions that do not completely combust the auxiliary fuel supplied from the auxiliary nozzle, the auxiliary fuel is pyrolyzed to produce char. The resulting char can then be attached to the surface-modified recycled carbon black, thereby adjusting the specific surface area of ​​the modified recycled carbon black. From the viewpoint of balancing the recovery amount of the resulting modified particles and the amount of rubber char that needs to be removed, the total carbon burn rate through all reactions is preferably 15.0% to 90.0%, more preferably 20.0% to 80.0%.

[0061] In the main burner reforming step, the supply amounts of raw material recycled carbon black, oxygen-containing gas, and main burner fuel are appropriately selected so as to achieve a predetermined main burner total carbon combustion rate. In the main burner reforming step (1), the supply amounts are appropriately selected so as to achieve a predetermined main burner total carbon combustion rate and main burner flame combustion rate. For example, the supply amount of air as the oxygen-containing gas is 100.0 Nm3 / hour, the supply of city gas (composition: methane 88%, ethane 6%, propane 5%, butane 1%) as fuel for the main burner is 1.8 Nm 3 / hour or more 8.7Nm 3 / hour or less, preferably 2.3 Nm 3 / hour or more 8.3Nm 3 In the main burner reforming step (2), the supply rate of the raw recycled carbon black is appropriately selected so as to achieve a predetermined main burner total carbon combustion rate and main burner flame combustion rate. For example, the supply rate of air as the oxygen-containing gas is 100.0 Nm 3 / hour, the supply of city gas as fuel for the main burner is 9.2 Nm 3 / hour or more 45.0Nm 3 / hour or less, preferably 9.6 Nm 3 / hour or more 30Nm 3 The feed rate of the raw recycled carbon black is 2 kg / hour or more and 75 kg / hour or less, preferably 3 kg / hour or more and 55 kg / hour or less.

[0062] In the auxiliary burner reforming step, the supply amounts of the oxygen-containing gas and auxiliary burner fuel are appropriately selected so as to achieve a predetermined total carbon burn rate and auxiliary burner flame combustion rate. In the auxiliary burner reforming step (1), the supply amounts of air as the oxygen-containing gas for the main burner are appropriately selected so as to achieve a predetermined total carbon burn rate and auxiliary burner flame combustion rate. For example, 3 / hour, the supply amount of air as oxygen-containing gas for the auxiliary burner is 5.0 Nm 3 / hour or more 100.0Nm 3 / hour or less, preferably 10.0 Nm 3 / hour or more 90.0Nm 3 / hour or less, and the supply of city gas as fuel for the auxiliary burner is 0.2 Nm 3 / hour or more 8.7Nm 3 / hour or less, preferably 0.5 Nm 3 / hour or more 7.5Nm 3In the auxiliary burner reforming step (2), the total carbon combustion rate of all burners and the flame combustion rate of the auxiliary burner are appropriately selected. For example, the air supply amount as the oxygen-containing gas for the main burner is set to 100.0 Nm 3 / hour, the supply amount of air as oxygen-containing gas for the auxiliary burner is 2 Nm 3 / hour or more 50.0Nm 3 / hour or less, preferably 5.0 Nm 3 / hour or more 40.0Nm 3 / hour or less, and the supply of city gas as fuel for the auxiliary burner is 0.5 Nm 3 / hour or more 50.0Nm 3 / hour or less, preferably 1.0 Nm 3 / hour or more 30.0Nm 3 In the auxiliary fuel pyrolysis step, the amount of air supplied as oxygen-containing gas for the main burner is appropriately selected so as to achieve a predetermined total reaction carbon combustion rate. For example, 3 / hour, the amount of city gas supplied as auxiliary fuel is 0.5 Nm 3 / hour or more 50.0Nm 3 / hour or less, preferably 1.0 Nm 3 / hour or more 30.0Nm 3 / hours or less.

[0063] If the auxiliary burner reforming step is not performed or the auxiliary fuel pyrolysis step is not performed, the modified recycled carbon black obtained after the main burner reforming step, i.e., by passing through the flame generated by the main burner, is cooled by contacting it with water, nitrogen gas, the metal wall of a heat exchanger, etc. If the auxiliary burner reforming step is performed, the modified recycled carbon black obtained after the main burner reforming step and the auxiliary burner reforming step, i.e., by passing through the flame generated by the main burner and the flame generated by the auxiliary burner, is cooled by contacting it with water, nitrogen gas, the metal wall of a heat exchanger, etc. If the auxiliary fuel pyrolysis step is performed, the modified recycled carbon black obtained after the main burner reforming step and the auxiliary fuel pyrolysis step, i.e., by passing through the flame generated by the main burner and by the auxiliary fuel pyrolysis step, is cooled by contacting it with water, nitrogen gas, the metal wall of a heat exchanger, etc. At this time, the modified recycled carbon black is at a high temperature after passing through the flame, and when it comes into contact with water, the water turns into steam.

[0064] After the modified recycled carbon black is cooled, the cooled modified recycled carbon black is separated from gases such as combustion gas, decomposition gas, and water vapor using a solid / gas separator such as a bag filter or a cyclone, thereby obtaining the modified recycled carbon black.

[0065] The method for producing modified recycled carbon black of the present invention can include a particle size adjustment step of pulverizing and / or classifying the raw recycled carbon black before carrying out the main burner modification step. By carrying out the particle size adjustment step before carrying out the main burner modification step, the variation in particle size of the raw recycled carbon black supplied to the main burner modification step can be reduced, thereby reducing the variation in the surface modification of the raw recycled carbon black in the main burner modification step.

[0066] The pulverizing device used in the particle size adjusting step is not particularly limited, and examples thereof include a roller mill, a jet mill, a hammer mill, a pin mill, a cutter mill, a roll crusher, a stamp mill, a ring mill, etc. The classifying device used in the particle size adjusting step is also not particularly limited, and examples thereof include a mechanical classifier equipped with a classification rotor or the like to achieve centrifugal classification, a classifier that achieves centrifugal classification by a swirling flow (free vortex or semi-free vortex) generated by supplying a high-speed airflow, and a classifier that utilizes the inertial force of particles accelerated by a bending high-speed airflow and the Coanda effect.

[0067] The main burner is not particularly limited as long as it can burn the main burner fuel to generate a flame, and can continuously supply the main burner fuel, oxygen-containing gas, and raw recycled carbon black from the fuel supply side to combust the main burner fuel, and can continuously introduce the raw recycled carbon black into the flame while generating the flame with the main burner, allowing it to pass through the flame.

[0068] An example of the main burner is the main burner shown in Fig. 4. Fig. 4 is a schematic end view of the main burner. In Fig. 4, the main burner 30a has a supply path 33 for raw recycled carbon black and carrier gas at the center of the burner, and an outlet 37 for the raw recycled carbon black and carrier gas is formed on the flame generation side. The main burner 30a also has a supply path 32 for oxygen-containing gas surrounding the supply path 33 for raw recycled carbon black and carrier gas, and an outlet 36 for oxygen-containing gas is formed on the flame generation side. The main burner 30a also has a supply path 31 for main burner fuel surrounding the oxygen-containing gas supply path 32, and an outlet 35 for main burner fuel is formed on the flame generation side. When viewed from a plane perpendicular to the direction of movement of the raw recycled carbon black, a circular supply path for the raw recycled carbon black and carrier gas is formed in the center, a cylindrical supply path for the oxygen-containing gas is formed surrounding the supply paths for the raw recycled carbon black and carrier gas, and a cylindrical supply path for the main burner fuel is formed surrounding the supply path for the oxygen-containing gas. In the embodiment shown in Figure 4, the supply paths for the raw recycled carbon black and carrier gas, the supply path for the oxygen-containing gas, and the supply path for the main burner fuel open at the end of the main burner on the flame side.

[0069] By supplying the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel from the fuel supply side of the main burner 30a, the raw recycled carbon black is placed at the center of the flame, the oxygen-containing gas is placed surrounding the raw recycled carbon black, and the main burner fuel is placed surrounding the oxygen-containing gas, and the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel can be introduced. By using the main burner 30a, the oxygen-containing gas can be placed near the raw recycled carbon black when the raw recycled carbon black, carrier gas, oxygen-containing gas, and main burner fuel are introduced into the flame, so that contact between the raw recycled carbon black and the oxygen-containing gas takes priority over contact between the raw recycled carbon black and the fuel gas, making it easier for oxidation of the raw recycled carbon black to occur.

[0070] An example of the main burner is shown in Fig. 5. Fig. 5 is a schematic end view of the main burner. In Fig. 5, the main burner 30b has a supply path 33 for raw recycled carbon black and carrier gas at the center of the burner, and an outlet 37 for the raw recycled carbon black and carrier gas is formed on the flame generation side. The main burner 30b also has a supply path 32 for oxygen-containing gas surrounding the supply path 33 for raw recycled carbon black and carrier gas, and an outlet 36 for oxygen-containing gas is formed on the flame generation side. The main burner 30b also has a supply path 31 for main burner fuel surrounding the oxygen-containing gas supply path 32, and an outlet 35 for main burner fuel is formed on the flame generation side. The outlet 37 for the raw recycled carbon black and carrier gas, the outlet 36 for the oxygen-containing gas, and the outlet 35 for the main burner fuel open to a mixing chamber 38, and the mixed flow is ejected toward the flame from the mixing chamber 38. In the embodiment of Fig. 5, the supply paths for the raw recycled carbon black and carrier gas, the supply path for the oxygen-containing gas, and the supply path for the main burner fuel open to a mixing chamber formed before the flame-side end of the main burner, and the mixing chamber opens to the flame-side end of the main burner.

[0071] Further, examples of the main burner structure include those described in Japanese Patent No. 3001561, Japanese Patent No. 5367471, Japanese Patent No. 3312228, Japanese Patent No. 4769276, Japanese Patent Laid-Open No. 2021-50897, Japanese Patent Laid-Open No. 2010-156025, and Japanese Patent No. 6580710.

[0072] In the method for producing modified recycled carbon black of the present invention, the G band intensity and the nitrogen adsorption specific surface area N of the modified recycled carbon black are increased by performing the main burner modification step, or by performing the main burner modification step and the auxiliary burner modification step. 2 The modified recycled carbon black can be obtained with an SA in the range shown below. The G band intensity and the nitrogen adsorption specific surface area N 2Modified recycled carbon black having an SA within the range shown below has strong bonding with the rubber component and does not have excessively high cohesion, thereby enhancing the reinforcing properties of rubber products. Therefore, the method for producing modified recycled carbon black of the present invention can continuously produce modified recycled carbon black that can enhance the reinforcing properties of rubber products.

[0073] The modified recycled carbon black obtained by the method for producing modified recycled carbon black of the present invention is recycled carbon black obtained by pyrolysis of rubber products such as waste tires, with the surface modified. More specifically, the modified recycled carbon black of the present invention is recycled carbon black obtained by pyrolysis of rubber products such as waste tires, with all or part of the rubber residue, mainly composed of rubber charcoal, adhered to the surface of the recycled carbon black removed.

[0074] The recycled carbon black having rubber carbonized material attached to the surface has a Raman spectrum of 1350±10 cm in Raman spectrum obtained by measuring with an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 When the peak intensity of the peak having a peak top in the range of 1580±20 cm is set to 100, -1 The peak intensity of the peak having a peak top in the range is 112 or more.

[0075] In contrast to such recycled carbon black with rubber char adhering to the surface, modified recycled carbon black has the rubber residue, mainly composed of rubber char adhering to the surface, removed. Therefore, in the Raman spectrum obtained by measuring with laser Raman spectroscopy at an excitation wavelength of 532 nm, -1 When the peak intensity of the peak (D band) having a peak top in the range of 1580 ± 20 cm -1The peak intensity of a peak (G band) having a peak top in this range is 84 to 111. When the D band intensity of the recycled carbon black is taken as 100, if the G band intensity is within this range, there will be no or very little rubber residue adhering to the surface of the recycled carbon black, and the recycled carbon black will have a strong bond with the rubber component, resulting in enhanced reinforcing properties for rubber products. From the viewpoint of ensuring an appropriate reaction with the rubber and improving reinforcing properties, the G band intensity is preferably 85 to 110, more preferably 90 to 105, when the D band intensity of the recycled carbon black is taken as 100. On the other hand, if the G band intensity exceeds the above range, there will be a large amount of rubber residue adhering to the surface of the recycled carbon black, and the bond between the recycled carbon black and the rubber component will be weak. On the other hand, if the G band intensity is below the above range, there will be many defects in the graphite structure on the carbon black surface, resulting in excessively high surface activity, which will promote aggregation of carbon black particles in the rubber and reduce the reinforcing properties of the rubber.

[0076] In the present invention, the G band intensity and the D band intensity, when the D band intensity is set to 100, refer to values ​​calculated from the Raman spectrum obtained by measuring under the measurement conditions (1) below and then performing the data processing (2). (1) Using an HR-800 manufactured by Horiba, Ltd. as a laser Raman spectrometer, several grains of the carbon black sample to be measured are placed on a slide glass and rubbed several times with a spatula to flatten the surface, and then the measurement is performed under the following measurement conditions: YAG laser (excitation wavelength): 532 nm Number of grooves: 600 gr / mm Filter: D0.6 Objective lens magnification: 100x Exposure time: 150 seconds Number of accumulations: 2 (2) Measurement wavelength (Raman shift) of the obtained spectrum: 2100 cm -1The signal intensity at 1350±10 cm was set to 0, and the average value was calculated for each of the 39 adjacent data points constituting the spectrum. Then, smoothing was performed to obtain a spectral curve connecting the average values. -1 The peak top intensity observed in this range is taken as 100. An example of the spectrum obtained in this case is shown in FIG.

[0077] As shown in FIG. 6, the modified recycled carbon black has a Raman spectrum of 1350±10 cm in a Raman spectrum obtained by measuring at an excitation wavelength of 532 nm by laser Raman spectroscopy. -1 A peak having a peak top in the range of 1580 ± 20 cm (D band) -1 A peak (G band) having a peak top in the range of

[0078] Then, from the values ​​of the peak intensity of the D band and the peak intensity of the G band, the peak intensity of the G band is calculated, assuming that the peak intensity of the D band is 100. According to the studies of the present inventors, the greater the amount of rubber carbonized matter attached to the recycled carbon black, the greater the intensity of the G band. Therefore, it was found that the degree of removal of rubber carbonized matter from the recycled carbon black can be determined by comparing the magnitude of the peak intensity of the G band with the peak intensity of the D band.

[0079] Figure 6 shows the Raman spectrum of an example of modified recycled carbon black, in which the peak intensity of the G band is 93 when the peak intensity of the D band is set to 100, which is within the range of 84 to 111. On the other hand, Figure 7 shows the Raman spectrum of an example of recycled carbon black before modification, in which the peak intensity of the G band is 113 when the peak intensity of the D band is set to 100, which is outside the range of 84 to 111. This shows that the recycled carbon black before modification shown in Figure 7 has rubber char adhering to its surface, while the modified recycled carbon black shown in Figure 6 has had the rubber char adhering to its surface removed by modification.

[0080] Nitrogen adsorption specific surface area N of modified recycled carbon black2 SA is 15m 2 / g or more 350m 2 / g or less. The nitrogen adsorption specific surface area N 2 When the SA is within the above range, the cohesive force of the recycled carbon black is kept low, thereby enhancing the reinforcing properties of rubber products. 2 From the viewpoint of optimizing the contact area with the rubber and improving the reinforcing properties of the rubber, SA is preferably 20 m 2 / g or more 300m 2 / g or less, more preferably 30m 2 / g or more 250m 2 On the other hand, the nitrogen adsorption specific surface area N 2 If the SA is less than the above range, the surface area in contact with the rubber is small, the reinforcing effect is not sufficiently exhibited, and the reinforcing properties of the rubber are reduced. On the other hand, if the SA exceeds the above range, the cohesive force of the recycled carbon black becomes too high, and the reinforcing properties of the rubber product are reduced.

[0081] In the present invention, the nitrogen adsorption specific surface area N 2 SA means a value measured by nitrogen adsorption amount in accordance with the method specified in JIS K6217-2 2001 "Testing methods for basic performance of carbon black for rubber".

[0082] The DBP (Dibutylphthalate) absorption capacity of the modified recycled carbon black is 60 cm 3 / 100g or more 200cm 3 / 100g or less is preferable, and 70cm 3 / 100g or more 195cm 3 / 100g or less is more preferable, and 80cm 3 / 100g or more 190cm 3On the other hand, if the DBP absorption is less than the above range, the dispersibility of the carbon black deteriorates when the carbon black is compounded in a rubber composition, and the reinforcing properties of the resulting rubber tend to decrease, whereas if the DBP absorption exceeds the above range, the processability of the resulting rubber may decrease when the carbon black is compounded in a rubber composition.

[0083] In the present invention, the DBP absorption amount means a value measured by the method specified in JIS K6217-4 "Carbon black for rubber - Fundamental properties - Part 4, Determination of DBP absorption amount".

[0084] The modified recycled carbon black is obtained by modifying recycled carbon black obtained by pyrolysis of rubber products such as waste tires. Therefore, the ash content of the modified recycled carbon black is 3.0% or more and 50.0% or less, and preferably 5.0% or more and 35.0% or less.

[0085] In the present invention, the ash content means a value measured by the method specified in JIS K 6218-2.

[0086] The invention will now be illustrated by the following examples.

[0087] (Example 1) The modified recycled carbon black manufacturing apparatus 1 shown in Figure 1 was used. First, city gas (composition: methane 88%, ethane 6%, propane 5%, butane 1%) was used as fuel for the main burner at a flow rate of 16.0 Nm 3 / hour, and air as the oxygen-containing gas at 215.0 Nm 3 The gas was supplied to the main burner for 10.0 Nm / hour, and a flame was generated. Subsequently, the supply of city gas and air was continued, and the flame generation was continued. 3Using a conveying air flow of 1 / hour, raw recycled carbon black was supplied to the main burner at a rate of 15 kg / hour and passed through the flame, thereby carrying out the main burner modification process. The raw recycled carbon was previously pulverized using a cutter mixer. The modified recycled carbon black that had passed through the flame was cooled with cooling water, and the gas was separated using a bag filter to obtain modified recycled carbon black. At this time, the main burner total carbon combustion rate was 79.0%. In addition, the main burner flame combustion rate was 128.0%. Next, the nitrogen adsorption specific surface area N of the obtained modified recycled carbon black was measured. 2 The G band intensity was measured when the SA and D band intensities were set at 100. As a result, the nitrogen adsorption specific surface area N 2 SA is 202m 2 / g, and the G band intensity was 93 when the D band intensity was 100. In Example 1, the auxiliary burner reforming step was not carried out.

[0088] Raw material recycled carbon black: Recycled carbon black obtained by pyrolysis of waste tires, Enrestec PB365, ash content: 18.6%, G band strength relative to D band strength: 100: 113 N 2 SA: 76m 2 / g

[0089] (Example 2) City gas 26.0 Nm 3 / hour, and 205.0 Nm3 of air as the oxygen-containing gas. 3 The reforming treatment was carried out under the same conditions as in Example 1, except that the feed rate was changed to 33 kg / hour and the raw recycled carbon black was changed to 33 kg / hour. At this time, the main burner total carbon combustion rate was 39.0%. The main burner flame combustion rate was 72.0%. As a result, the nitrogen adsorption specific surface area N 2 SA is 62m 2 / g, and the G band intensity was 99 when the D band intensity was 100.

[0090] (Example 3) In addition to the conditions of Example 2, 3.0 Nm3 of city gas was used as auxiliary fuel from the auxiliary burner. 3 / hour, air 85.0 Nm3 as oxygen-containing gas for auxiliary burner 3 / hour to generate a flame, and additional treatment was performed using the auxiliary burner flame. At this time, the main burner total carbon combustion rate was 39.0%. The main burner flame combustion rate was 72.0%. In addition, the auxiliary burner flame combustion rate was 258.0%, and the total carbon combustion rate of all burners was 52.0%. As a result, the nitrogen adsorption specific surface area N 2 SA is 162m 2 / g, and the G band intensity was 94 when the D band intensity was 100. That is, in Example 3, the main burner reforming step and the auxiliary burner reforming step were carried out.

[0091] (Example 4) In addition to the conditions of Example 1, 12.0 Nm3 of city gas was used as auxiliary fuel from the auxiliary burner. 3 / hour, 30.0 Nm3 of air as oxygen-containing gas for auxiliary burner 3 / hour to generate a flame, and additional treatment was performed using the auxiliary burner flame. At this time, the total carbon combustion rate of the main burner was 79.0%. The main burner flame combustion rate was 128.0%. In addition, the auxiliary burner flame combustion rate was 23.0%, and the total carbon combustion rate of all burners was 61.0%. As a result, the nitrogen adsorption specific surface area N 2 SA is 113m 2 / g, and the G band intensity was 97 when the D band intensity was 100. That is, in Example 4, the main burner reforming step and the auxiliary burner reforming step were carried out.

[0092] Example 5 A modified recycled carbon black manufacturing apparatus 1 shown in FIG. 1 was used in which the auxiliary burner 4 was replaced with a fuel nozzle. First, city gas (composition: methane 88%, ethane 6%, propane 5%, butane 1%) was used as fuel for the main burner at a flow rate of 16.0 Nm 3 / hour, and air as the oxygen-containing gas at 215.0 Nm 3 The gas was supplied to the main burner for 10.0 Nm / hour, and a flame was generated. Subsequently, the supply of city gas and air was continued, and the flame generation was continued. 3 Using conveying air for 1 hour, raw recycled carbon black was supplied to the main burner at a rate of 15 kg / hour, and the flame was passed through to carry out the main burner reforming process. 12.0 Nm3 of city gas was used as fuel from the fuel nozzle.3 The auxiliary fuel pyrolysis step was carried out by supplying 10 ... 2 SA is 90m 2 / g, and the G band intensity was 96 when the D band intensity was 100. That is, in Example 5, the main burner reforming step and the auxiliary fuel pyrolysis step were carried out.

[0093] According to the present invention, recycled carbon black that bonds strongly to rubber components and has high reinforcing properties for rubber products can be continuously produced. Therefore, rubber products having performance equivalent to that of virgin carbon black can be industrially advantageously produced using recycled carbon black obtained by pyrolysis of rubber products such as waste tires.

[0094] REFERENCE SIGNS LIST 1 Modified recycled carbon black manufacturing apparatus 2 Burner reforming section 3 Main burner 4 Auxiliary burner 5 Cooling water supply pipe 6 Connecting pipe 7 Collection section 11 Fuel for main burner 12, 15 Oxygen-containing gas 13 Raw recycled carbon black and carrier gas 14 Fuel for auxiliary burner 16 Cooling water 17 Gas 18 Modified recycled carbon black 21 Flame generated by main burner 22 Direction of movement of raw recycled carbon black 23 Flame generated by auxiliary burner 30a, 30b Main burner 31 Supply path for main burner fuel 32 Supply path for oxygen-containing gas 33 Supply path for raw recycled carbon black and carrier gas 35 Outlet for main burner fuel 36 Outlet for oxygen-containing gas 37 Outlet for raw recycled carbon black and carrier gas 38 Mixing chamber

Claims

1. A method for producing modified recycled carbon black, comprising: a main burner modification process in which main burner fuel, oxygen-containing gas, and recycled carbon black having rubber carbonized particles attached thereto are continuously supplied to a main burner which burns fuel to generate a flame, and the main burner fuel is combusted; and while continuously generating a flame in the main burner, the recycled carbon black having rubber carbonized particles attached thereto is introduced into the flame and passed through the flame; and the main burner total carbon combustion rate, expressed by the following formula (1): Main burner total carbon combustion rate (%) = (A / (B+C)) x 100 (1) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized particles attached thereto which is supplied to the main burner, and C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel which is supplied to the main burner). is less than 100.0%.

2. A method for producing modified recycled carbon black according to claim 1, characterized in that the main burner reforming step is a main burner reforming step (1) for making the main burner flame combustion rate, expressed by the following formula (2): Main burner flame combustion rate (%) = (A / C) x 100 (2) (wherein A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner), 100.0% or more.

3. A method for producing modified recycled carbon black according to claim 1, wherein the main burner reforming step is a main burner reforming step (2) for making the main burner flame combustion rate, expressed by the following formula (2): Main burner flame combustion rate (%) = (A / C) x 100 (2) (wherein A represents the amount of oxygen supplied to the main burner, and C represents the theoretical amount of oxygen necessary for complete combustion of the main burner fuel supplied to the main burner), less than 100.0%.

4. An auxiliary burner is provided downstream of the main burner for burning auxiliary burner fuel to generate a flame, and an auxiliary burner reforming process is provided in which recycled carbon black after the main burner reforming process (1) is introduced into the flame generated by the auxiliary burner while continuously generating a flame with the auxiliary burner, and passes through the flame, wherein the auxiliary burner reforming process has an auxiliary burner flame combustion rate represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (wherein D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner) of 100.0% or more, and the following formula (4): Total burner total carbon combustion rate (%) = ((A+D) / (B+C+E)) x 100 (4) 3. The method for producing modified recycled carbon black according to claim 2, further comprising an auxiliary burner modification step (1) for making an all-burner total carbon combustion rate, represented by the formula: (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto which is supplied to the main burner, C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel which is supplied to the main burner, D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel which is supplied to the auxiliary burner).

5. An auxiliary burner is provided downstream of the main burner for burning auxiliary burner fuel to generate a flame, and an auxiliary burner reforming process is provided in which recycled carbon black after the main burner reforming process (1) is introduced into the flame generated by the auxiliary burner while continuously generating a flame with the auxiliary burner, and passes through the flame, wherein the auxiliary burner reforming process has an auxiliary burner flame combustion rate represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (wherein D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner) of less than 100.0%, and the following formula (4): Total burner total carbon combustion rate (%) = ((A+D) / (B+C+E)) x 100 (4) 3. The method for producing modified recycled carbon black according to claim 2, further comprising an auxiliary burner modification step (2) for modifying an all-burner total carbon combustion rate, represented by the formula: (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto which is supplied to the main burner, C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel which is supplied to the main burner, D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel which is supplied to the auxiliary burner).

6. An auxiliary burner is provided downstream of the main burner for burning auxiliary burner fuel to generate a flame, and an auxiliary burner reforming process is provided in which recycled carbon black after the main burner reforming process (2) is introduced into the flame generated by the auxiliary burner while continuously generating a flame with the auxiliary burner, and passes through the flame, wherein the auxiliary burner reforming process has an auxiliary burner flame combustion rate represented by the following formula (3): Auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (wherein D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner) of 100.0% or more, and the following formula (4): Total burner total carbon combustion rate (%) = ((A+D) / (B+C+E)) x 100 (4) 4. The method for producing modified recycled carbon black according to claim 3, further comprising an auxiliary burner modification step (1) for making an all-burner total carbon combustion rate, represented by the formula: (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto which is supplied to the main burner, C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel which is supplied to the main burner, D represents the amount of oxygen supplied to the auxiliary burner, and E represents the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel which is supplied to the auxiliary burner).

7. An auxiliary burner is provided downstream of the main burner for burning auxiliary burner fuel to generate a flame, and an auxiliary burner reforming process is provided in which recycled carbon black after the main burner reforming process (2) is introduced into the flame generated by the auxiliary burner while continuously generating a flame with the auxiliary burner, and passes through the flame, wherein the auxiliary burner reforming process has an auxiliary burner flame combustion rate represented by the following formula (3): auxiliary burner flame combustion rate (%) = (D / E) x 100 (3) (wherein D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen necessary for complete combustion of the auxiliary burner fuel supplied to the auxiliary burner) of less than 100.0%, and the following formula (4): total burner carbon combustion rate (%) = ((A+D) / (B+C+E)) x 100 (4) (wherein A refers to the amount of oxygen supplied to the main burner, B refers to the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material attached thereto which is supplied to the main burner, C refers to the theoretical amount of oxygen required for complete combustion of the main burner fuel which is supplied to the main burner, D refers to the amount of oxygen supplied to the auxiliary burner, and E refers to the theoretical amount of oxygen required for complete combustion of the auxiliary burner fuel which is supplied to the auxiliary burner).

8. A method for producing modified recycled carbon black as set forth in claim 2 or 3, characterized in that it comprises an auxiliary fuel pyrolysis step in which a fuel nozzle is provided downstream of the main burner and auxiliary fuel is introduced from the fuel nozzle into or near a flame generated by the main burner, thereby pyrolyzing the auxiliary fuel, wherein the auxiliary fuel pyrolysis step achieves an overall reaction total carbon combustion rate of less than 100.0%, as represented by the following formula (5): Total carbon combustion rate (%) = (A / (B+C+F)) x 100 (5) (wherein A represents the amount of oxygen supplied to the main burner, B represents the theoretical amount of oxygen required for complete combustion of the recycled carbon black having rubber carbonized material adhering thereto, which is supplied to the main burner, C represents the theoretical amount of oxygen required for complete combustion of the main burner fuel supplied to the main burner, and F represents the theoretical amount of oxygen required for complete combustion of the auxiliary fuel supplied from the fuel nozzle.) 9. A method for producing modified recycled carbon black as described in claim 1, characterized in that it includes a particle size adjustment process of crushing and / or classifying the recycled carbon black to which the rubber carbonized material is attached prior to carrying out the main burner modification process.

10. Modified recycled carbon black obtained by carrying out the method for producing modified recycled carbon black according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Burner lance for charging powdery and granular material into smelting reduction furnace, and method for producing molten metal by smelting reduction

    JP2010156025A

  • Burner for manufacturing of inorganic spheroidized particle, inorganic spheroidized particle manufacturing device and method for manufacturing inorganic spheroidized particle

    JP2021050897A

  • Burner for manufacturing inorganic spherical particles and its burner device

    JP3001561B1

  • Burner for producing inorganic spherical particles

    JP3312228B2

  • Burner for producing inorganic spheroidal particles

    JP4769276B2