SiC SUBSTRATE AND SiC COMPOSITE SUBSTRATE
By controlling the Raman shift value and nitrogen distribution in biaxially oriented SiC substrates, the warping issue in SiC substrates is mitigated, improving their stability and manufacturing efficiency.
Patent Information
- Application Number
- PCT/JP2023/040963
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2023-11-14
- Publication Date
- 2024-10-31
AI Technical Summary
SiC substrates often experience warping during epitaxial film formation and semiconductor manufacturing, leading to cracks and poor suction issues, which existing methods are insufficient to fully address.
A SiC substrate with a biaxially oriented SiC layer, where the Raman shift value difference between the Si and C planes is controlled to reduce warpage, achieved by measuring Raman shift values at specific intervals and optimizing nitrogen and rare earth element concentrations.
The controlled Raman shift value reduces in-plane nitrogen distribution and elastic strain, effectively minimizing substrate warpage, enhancing the stability and processing efficiency of SiC substrates.
Smart Images

Figure JP2023040963_31102024_PF_FP_ABST
Abstract
Description
SiC substrate and SiC composite substrate
[0001] The present invention relates to a SiC substrate and a SiC composite substrate.
[0002] SiC (silicon carbide) has attracted attention as a wide-bandgap material capable of controlling high voltages and high power with low loss. In particular, in recent years, power semiconductor devices using SiC materials (SiC power devices) are expected to be used in a variety of applications because they are more compact, consume less power, and are more efficient than those using Si semiconductors. For example, the adoption of SiC power devices can reduce the size and improve the efficiency of converters, inverters, on-board chargers, etc. for electric vehicles (EVs) and plug-in hybrid vehicles (PHEVs). Therefore, the development of SiC wafers, which form the backbone of SiC power devices, has attracted considerable attention.
[0003] To fabricate a SiC power device, it is necessary to epitaxially grow a SiC single crystal on a SiC substrate. However, warping may occur in the SiC substrate, and it is desirable to suppress this warping. As an example of reducing the warping of the substrate, Patent Document 1 (JP 2022-120059 A) describes a method for reducing the maximum half-width of the peak corresponding to the folded mode of the vertical optical branch in the Raman spectrum of the SiC substrate by Δ max The minimum value is Δ min When this is done, Δ max -Δ min Patent Document 2 (WO2021 / 111835A1) discloses a SiC substrate having a first main surface and a second main surface opposite to the first main surface, in which, when the average value of wave numbers showing a peak corresponding to the folded mode of the vertical optical branch in the Raman spectrum of SiC in a first square region in the first main surface is defined as a first wave number, and the average value of wave numbers showing a peak corresponding to the folded mode of the vertical optical branch in the Raman spectrum of SiC in a second square region in the first main surface is defined as a second wave number, the absolute value of the difference between the first wave number and the second wave number is 0.2 cm -1Patent Document 3 (JP 2017-75074 A) discloses a SiC substrate having a 4H crystal structure, which includes a carbon surface-side main surface and a silicon surface-side main surface, in which the nitrogen concentration in the carbon surface-side main surface is higher than the nitrogen concentration in the silicon surface-side main surface, and the difference in Raman peak shift between the carbon surface-side main surface and the silicon surface-side main surface is 0.2 cm -1 Patent Document 4 (WO2017 / 057742A1) discloses a SiC single crystal ingot having a SiC single crystal on a seed crystal, in which a substrate cut out from the ingot has a Raman index (A-B) of 0.20 or less, which is the difference between a Raman shift value (A) measured at the center and a Raman shift value (B) measured at the periphery. Patent Document 5 (JP 2016-164120 A) discloses a SiC single crystal ingot having a surface basal plane dislocation density of 100 / cm 2 More than 1000 pieces / cm 2 Hereinafter, the threading screw dislocation density is 160 / cm 2 More than 500 pieces / cm 2 The document also discloses a SiC single crystal wafer having a diameter of 150 mm or more and 300 mm or less and a Raman index of 0.03 or more and 0.2 or less.
[0004] JP 2022-120059 A WO2021 / 111835A1 JP 2017-75074 A WO2017 / 057742A1 JP 2016-164120 A
[0005] As described above, although methods for reducing substrate warpage have been investigated, further improvements are required. In particular, warpage of SiC substrates poses a problem when polishing SiC substrates after epitaxial film formation and when manufacturing semiconductor devices. Specifically, warpage can cause cracks when the SiC substrate is attached to a polishing table and poor adhesion when the SiC substrate is vacuum-fixed during the semiconductor manufacturing process.
[0006] The present inventors have now discovered that warpage of a SiC substrate can be reduced by controlling the Raman shift value, which indicates a peak corresponding to the shear wave acoustic branch of the Raman spectrum in the SiC substrate.
[0007] Therefore, an object of the present invention is to provide a SiC substrate with small warpage.
[0008] According to the present invention, the following aspects are provided: [Aspect 1] A SiC substrate having a biaxially textured SiC layer, wherein the maximum value k of the Raman shift value in the Si-face and the C-face of the SiC substrate is max and the minimum value k min The difference is 0.50 cm -1 The Raman shift value is a value obtained by measuring Raman shift values showing peaks corresponding to shear wave acoustic branches of a Raman spectrum at 1 mm intervals on two lines passing through the center point of the Si-face and intersecting each other at right angles in the Si-face of the SiC substrate, and measuring Raman shift values showing peaks corresponding to shear wave acoustic branches of a Raman spectrum at 1 mm intervals on two lines passing through the center point of the C-face and intersecting each other at right angles in the C-face of the SiC substrate. max and the minimum value k min The difference is 0.20 cm -1 The SiC substrate according to aspect 1, wherein the N concentration of the biaxially oriented SiC layer is 5.0×10 or less. 18 atoms / cm 3 The SiC substrate according to aspect 1 or 2, wherein the rare earth element concentration of the biaxially textured SiC layer is 1.0×10 or more. 14 ~5.0 x 10 15 atoms / cm 3 The SiC substrate according to any one of Aspects 1 to 3. [Aspect 5] A SiC composite substrate comprising a SiC single crystal substrate and the SiC substrate according to any one of Aspects 1 to 4 on the SiC single crystal substrate.
[0009] 1 is a longitudinal sectional view of a SiC composite substrate 10; FIG. 2 is a manufacturing process diagram of a SiC composite substrate 10; FIG. 3 is a conceptual diagram showing the configuration of an aerosol deposition (AD) apparatus 50; FIG. 4 is a top view of a SiC substrate 10 for explaining a method for measuring the amount of warpage of a SiC substrate 10; FIG. 5 is a schematic sectional view of a SiC substrate 10 for explaining a method for measuring the amount of warpage of a SiC substrate 10; FIG. 6 is a schematic sectional view of a SiC substrate 10 for explaining a method for measuring the amount of warpage of a SiC substrate 10;
[0010] The SiC substrate according to the present invention has a biaxially oriented SiC layer. The SiC substrate has a maximum Raman shift value k max and the minimum value k min The difference is 0.50 cm -1 The Raman shift values are obtained by measuring Raman shift values showing peaks corresponding to shear wave acoustic branches of the Raman spectrum at 1 mm intervals on two mutually orthogonal lines passing through the center point of the Si-face within the Si-face of the SiC substrate, and measuring Raman shift values showing peaks corresponding to shear wave acoustic branches of the Raman spectrum at 1 mm intervals on two mutually orthogonal lines passing through the center point of the C-face within the SiC substrate. Note that the Si-face and C-face of the SiC substrate refer to the Si-face and C-face of the biaxially oriented SiC layer when the SiC substrate is composed of a biaxially oriented SiC layer, and refer to the Si-face and C-face of the composite substrate when the SiC substrate is a composite substrate including a biaxially oriented SiC layer and a SiC single crystal substrate (in this case, the surface of the biaxially oriented SiC layer may be the Si-face and the surface of the SiC single crystal substrate may be the C-face, or the surface of the biaxially oriented SiC layer may be the C-face and the surface of the SiC single crystal substrate may be the Si-face). The Raman shift value showing a peak corresponding to the shear wave acoustic branch of the Raman spectrum is typically FTA(2 / 4)E 2 (wave number 200cm -1 In this way, by controlling the Raman shift value showing the peak corresponding to the shear wave acoustic branch of the Raman spectrum in the SiC substrate, it is possible to reduce the warpage of the SiC substrate.
[0011] As described above, warpage may occur in SiC substrates, and while it is desirable to suppress this warpage, conventional methods are insufficient, and further improvements in warpage are desired. In this regard, the present invention advantageously solves this problem. In particular, controlling the Raman shift value that exhibits a peak corresponding to the shear wave acoustic branch of the Raman spectrum in a SiC substrate means that the in-plane distribution of nitrogen and the elastic strain distribution in the SiC substrate can be reduced. It is believed that reducing the in-plane distribution of nitrogen and the elastic strain distribution in the SiC substrate can reduce the warpage of the SiC substrate.
[0012] The SiC substrate of the present invention has a maximum Raman shift value k of 100 nm when measuring Raman shift values that show peaks corresponding to shear wave acoustic branching in the Raman spectrum within the Si-plane and C-plane. max and the minimum value k min The difference is 0.50 cm -1 less than 0.20 cm, preferably -1 Here, as described above, within the Si-face of the SiC substrate, Raman shift values showing peaks corresponding to the shear wave acoustic branch of the Raman spectrum are measured at 1 mm intervals on two lines passing through the center point of the Si-face and intersecting at right angles, and within the C-face of the SiC substrate, Raman shift values showing peaks corresponding to the shear wave acoustic branch of the Raman spectrum are measured at 1 mm intervals on two lines passing through the center point of the C-face and intersecting at right angles. max and the minimum value k min The difference between the maximum and minimum Raman shift values can be considered as the difference between the maximum and minimum Raman shift values when measured over the entire surface (entire region) of the SiC substrate.
[0013] The SiC substrate or biaxially oriented SiC layer has an off-axis angle, which is preferably 0.1 to 12°, more preferably 1 to 5° from the
[0001] axis of the SiC substrate or biaxially oriented SiC layer.
[0014] Examples of rare earth elements contained in the biaxially oriented SiC layer include Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc, and combinations thereof. From the viewpoint of reducing warpage of the substrate, the rare earth element is preferably Y or Ce, and more preferably Y.
[0015] The rare earth element concentration of the biaxially oriented SiC layer is 1.0 × 10 14 ~5.0 x 10 15 atoms / cm 3 is preferably 5.0 × 10 14 ~5.0 x 10 15 atoms / cm 3 and more preferably 5.0 × 10 14 ~1.4 × 10 15 atoms / cm 3 is.
[0016] The N concentration of the biaxially oriented SiC layer is 1.0 × 10 18 atoms / cm 3 It is preferably 5.0 × 10 or more, and more preferably 5.0 × 10 18 atoms / cm 3 More preferably, 8.0 × 10 18 atoms / cm 3 The upper limit of the N concentration is not particularly limited, but is preferably 1.0 × 10 21 atoms / cm 3 It is preferably equal to or less than 1.0 × 10 20 atoms / cm 3 More preferably, 1.0 × 10 19 atoms / cm 3 The following is the result.
[0017] The biaxially oriented SiC layer is preferably oriented in the c-axis and a-axis directions. Furthermore, the SiC substrate is preferably composed of a biaxially oriented SiC layer. The biaxially oriented SiC layer may be a SiC single crystal, a SiC polycrystal, or a mosaic crystal, as long as it is oriented in the two axes of the c-axis and the a-axis. A mosaic crystal is a collection of crystals that do not have clear grain boundaries but whose crystal orientations, along either the c-axis or the a-axis, are slightly different. The method for evaluating the orientation is not particularly limited, and known analytical techniques such as EBSD (Electron Backscatter Diffraction Patterns) and X-ray pole figures can be used. For example, when using the EBSD method, inverse pole figure mapping of the surface (plate surface) of the biaxially oriented SiC layer or a cross section perpendicular to the plate surface can be measured. In the obtained inverse pole figure mapping, when the following four conditions are satisfied, the biaxially oriented SiC layer can be defined as being oriented in two directions, namely, the approximately normal direction and the approximately in-plane direction: (A) the first axis, (B) the second axis, (C) the tilt angle from the first axis is distributed within ±10°; and (D) the tilt angle from the second axis is distributed within ±10°. In other words, when the above four conditions are satisfied, the biaxially oriented SiC layer is determined to be oriented in two directions, namely, the c-axis and the a-axis. For example, when the approximately normal direction to the plate surface is oriented to the c-axis, the approximately in-plane direction may be oriented in a specific direction (e.g., the a-axis) perpendicular to the c-axis. The biaxially oriented SiC layer may be oriented in two directions, namely, the approximately normal direction and the approximately in-plane direction, but it is preferable that the approximately normal direction is oriented to the c-axis. The smaller the tilt angle distribution in the approximately normal direction and / or the approximately in-plane direction, the smaller the mosaic property of the biaxially oriented SiC layer, and the closer it is to zero, the closer it is to a single crystal. Therefore, from the viewpoint of the crystallinity of the biaxially oriented SiC layer, it is preferable that the tilt angle distribution be small in both the approximately normal direction and the approximately in-plane direction, for example, ±5° or less is more preferable, and ±3° or less is even more preferable.
[0018] The SiC substrate of the present invention is preferably in the form of a SiC composite substrate. That is, according to a preferred embodiment of the present invention, there is provided a SiC composite substrate comprising a SiC single crystal substrate and the above-described SiC substrate on the SiC single crystal substrate. In this way, by providing the SiC composite substrate with a SiC substrate having a controlled Raman shift value that exhibits a peak corresponding to the shear wave acoustic branch of the Raman spectrum, warping of the SiC composite substrate can be reduced.
[0019] The SiC single crystal substrate is typically a layer composed of a SiC single crystal and has a crystal growth surface. The polytype and off-axis angle of the SiC single crystal are not particularly limited, but the polytype is preferably 4H or 6H, and the off-axis angle is preferably 0.1 to 12° from the
[0001] axis of the single crystal SiC. The polytype is more preferably 4H, and the off-axis angle is more preferably 1 to 5° from the
[0001] axis of the single crystal SiC.
[0020] The SiC substrate of the present invention may be in the form of a freestanding substrate of a biaxially oriented SiC layer alone, or in the form of a SiC composite substrate accompanied by a SiC single crystal substrate. Therefore, if necessary, the biaxially oriented SiC layer may finally be separated from the SiC single crystal substrate. Separation of the SiC single crystal substrate may be performed by any known method, without particular limitation. Examples include a method of separating the biaxially oriented SiC layer using a wire saw, a method of separating the biaxially oriented SiC layer by electrical discharge machining, and a method of separating the biaxially oriented SiC layer using a laser. Furthermore, when a biaxially oriented SiC layer is epitaxially grown on a SiC single crystal substrate, the biaxially oriented SiC layer may be placed on a separate support substrate after separation of the SiC single crystal substrate. The material of the separate support substrate is not particularly limited, and a suitable material may be selected from the viewpoint of material properties. For example, from the viewpoint of thermal conductivity, metal substrates such as Cu, and ceramic substrates such as SiC and AlN may be used.
[0021] Manufacturing Method of SiC Composite Substrate The SiC composite substrate of the present invention can be preferably manufactured by (a) forming a predetermined textured precursor layer on a SiC single crystal substrate, (b) heat-treating the textured precursor layer on the SiC single crystal substrate to convert at least a portion thereof near the SiC single crystal substrate into a SiC substrate (biaxially textured SiC layer), and, if desired, (c) performing processing such as grinding or polishing to expose the surface of the biaxially textured SiC layer. However, the manufacturing method of the SiC composite substrate is not limited as long as it can produce a SiC substrate with a controlled Raman shift value that exhibits a peak corresponding to the shear wave acoustic branch of the Raman spectrum. For example, a manufacturing method that can increase the nitrogen flow rate during heat treatment is preferred. In this case, a gas-phase method such as CVD or sublimation or a liquid-phase method such as solution processing may be used. The rare earth element concentration and / or N concentration in the SiC substrate (biaxially textured SiC layer) can be preferably controlled by adding a rare earth compound to the raw material during the formation of the textured precursor layer or by changing the heat treatment conditions (gas flow rate, heat treatment temperature, holding time, etc.). According to this manufacturing method, it is possible to preferably produce a SiC substrate having a controlled Raman shift value that exhibits a peak corresponding to the shear wave acoustic branch of the Raman spectrum, and it is possible to effectively reduce warpage of the SiC substrate or a SiC composite substrate using the same.
[0022] A preferred method for manufacturing a SiC composite substrate will now be described. Fig. 1 is a longitudinal cross-sectional view of a SiC composite substrate 10 (a cross-sectional view of the SiC composite substrate 10 cut longitudinally along a plane including the central axis of the SiC composite substrate 10), and Fig. 2 is a process diagram for manufacturing the SiC composite substrate 10.
[0023] As shown in FIG. 1, a SiC composite substrate 10 of this embodiment includes a SiC single crystal substrate 20 and a SiC substrate 30 on the SiC single crystal substrate.
[0024] 2(a) Step of Forming Textured Precursor Layer As shown in Fig. 2(a), the textured precursor layer 40 will become the SiC substrate (biaxially textured SiC layer) 30 by heat treatment, which will be described later. In the step of forming the textured precursor layer 40, the textured precursor layer 40 is formed on the crystal growth surface of the SiC single crystal substrate 20.
[0025] The orientation precursor layer 40 can be formed by any known method. Examples of methods for forming the orientation precursor layer 40 include solid-phase deposition methods such as aerosol deposition (AD) and HPPD (supersonic plasma particle deposition), vapor-phase deposition methods such as sputtering, evaporation, sublimation, and various CVD (chemical vapor deposition) methods, and liquid-phase deposition methods such as solution growth. A method in which the orientation precursor layer 40 is formed directly on the SiC single crystal substrate 20 can be used. Examples of CVD methods that can be used include thermal CVD, plasma CVD, mist CVD, and metal-organic CVD. Alternatively, a polycrystalline body previously prepared by sublimation, various CVD, sintering, or the like can be used as the orientation precursor layer 40, and then placed on the SiC single crystal substrate 20. Alternatively, a molded body for the orientation precursor layer 40 can be prepared in advance and then placed on the SiC single crystal substrate 20. Such an alignment precursor layer 40 may be a tape-molded body produced by tape casting, or may be a green compact produced by pressure molding using a uniaxial press or the like.
[0026] When forming these textured precursor layers 40, it is preferable that the raw materials for the textured precursor layers 40 contain a rare earth compound. This allows the concentration of the rare earth compound in the biaxially textured SiC layer to be controlled. The rare earth compound is not particularly limited, but examples include oxides, nitrides, carbides, and fluorides of at least one rare earth element selected from the 17 rare earth elements described above. Oxides of rare earth elements are preferred as the rare earth compound.
[0027] In addition, when various CVD methods, sublimation methods, solution growth methods, etc. are used to form the textured precursor layer 40 directly on the SiC single crystal substrate 20, epitaxial growth may occur on the SiC single crystal substrate 20, resulting in the formation of the SiC substrate 30, without the heat treatment process described below. However, the textured precursor layer 40 is preferably in an unoriented state upon formation, i.e., amorphous or unoriented polycrystalline, and is preferably oriented using the SiC single crystal as a seed in a subsequent heat treatment process. This effectively reduces crystal defects that reach the surface of the SiC substrate 30. Although the reason for this is unclear, it is believed that the reorganization of the crystalline structure of the solid-phase textured precursor layer once formed using the SiC single crystal as a seed may also be effective in eliminating crystal defects. Therefore, when various CVD methods, sublimation methods, solution growth methods, etc. are used, it is preferable to select conditions that do not cause epitaxial growth in the textured precursor layer 40 formation process.
[0028] However, preferred are methods of forming the texture precursor layer 40 directly on the SiC single crystal substrate 20 using the AD method or various CVD methods, or methods of placing a polycrystalline body separately prepared by sublimation, various CVD methods, sintering, or the like on the SiC single crystal substrate 20. These methods enable the texture precursor layer 40 to be formed in a relatively short time. The AD method is particularly preferred because it does not require a high-vacuum process and has a relatively fast film formation rate. When using a pre-prepared polycrystalline body as the texture precursor layer 40, it is necessary to take measures such as sufficiently smoothing the surface of the polycrystalline body to improve adhesion between the polycrystalline body and the SiC single crystal substrate 20. Therefore, from a cost perspective, the method of directly forming the texture precursor layer 40 is preferred. The method of placing a pre-prepared compact on the SiC single crystal substrate 20 is also preferred as a simple method, but because the texture precursor layer 40 is composed of powder, a sintering process is required in the heat treatment step described below. Both methods can use known conditions, but below we will describe a method of forming an orientation precursor layer 40 directly on a SiC single crystal substrate 20 by the AD method or thermal CVD method, and a method of placing a pre-prepared molded body on a SiC single crystal substrate 20.
[0029] The AD method is a technology in which fine particles or fine particle raw material are mixed with a gas to form an aerosol, and this aerosol is then sprayed at high speed from a nozzle to collide with a substrate, forming a coating. The AD method has the advantage of being able to form a coating at room temperature. An example of a film-forming apparatus (AD apparatus) used in this AD method is shown in FIG. 3 . The AD apparatus 50 shown in FIG. 3 is configured as an apparatus used in the AD method, in which raw material powder is sprayed onto a substrate under an atmosphere at a pressure lower than atmospheric pressure. This AD apparatus 50 includes an aerosol generation unit 52 that generates an aerosol of raw material powder containing raw material components, and a film-forming unit 60 that sprays the raw material powder onto a SiC single crystal substrate 20 to form a film containing the raw material components. The aerosol generation unit 52 includes an aerosol generation chamber 53 that contains raw material powder and generates aerosol by receiving a supply of carrier gas from a gas cylinder (not shown), a raw material supply pipe 54 that supplies the generated aerosol to the film formation unit 60, and a vibrator 55 that applies vibrations at a frequency of 10 to 100 Hz to the aerosol generation chamber 53 and the aerosol therein. The film formation unit 60 includes a film formation chamber 62 that sprays the aerosol onto the SiC single crystal substrate 20, a substrate holder 64 that is disposed inside the film formation chamber 62 and fixes the SiC single crystal substrate 20, and an XY stage 63 that moves the substrate holder 64 in the X-axis and Y-axis directions. The film formation unit 60 also includes an injection nozzle 66 that has a slit 67 formed at its tip and sprays the aerosol onto the SiC single crystal substrate 20, and a vacuum pump 68 that depressurizes the film formation chamber 62. The injection nozzle 66 is attached to the tip of the raw material supply pipe 54.
[0030] It is known that the AD method can cause pores in the film or result in a compacted film depending on the film formation conditions. For example, it is easily affected by the collision speed of the raw material powder with the substrate, the particle size of the raw material powder, the agglomeration state of the raw material powder in the aerosol, the amount sprayed per unit time, etc. The collision speed of the raw material powder with the substrate is affected by the pressure difference between the film formation chamber 62 and the spray nozzle 66, the opening area of the spray nozzle, etc. Therefore, to obtain a dense oriented precursor layer, it is necessary to appropriately control these factors.
[0031] In the thermal CVD method, a commercially available or other known film forming apparatus can be used. The source gas is not particularly limited, but silicon tetrachloride (SiCl 4 ) gas and silane (SiH 4 ) gas, and methane (CH 4 ) gas and propane (C 3 H 8 The film formation temperature is preferably 1000 to 2200°C, more preferably 1100 to 2000°C, and even more preferably 1200 to 1900°C.
[0032] It is known that when a film is formed on a SiC single crystal substrate 20 using thermal CVD, epitaxial growth may occur on the SiC single crystal substrate 20, forming a SiC substrate 30. However, the orientation precursor layer 40 is not oriented at the time of its formation, i.e., amorphous or non-oriented polycrystalline, and it is preferable to use a SiC single crystal as a seed crystal during the heat treatment process to cause crystalline rearrangement. It is known that the formation of an amorphous or polycrystalline layer on a SiC single crystal using thermal CVD is affected by factors such as the film formation temperature, the gas flow rates of the Si source and the C source and their ratio, and the film formation pressure. The film formation temperature has a significant effect, and from the perspective of forming an amorphous or polycrystalline layer, a lower film formation temperature is preferable, preferably less than 1700°C, more preferably 1500°C or less, and even more preferably 1400°C or less. However, if the film formation temperature is too low, the film formation rate itself also decreases, so from the perspective of the film formation rate, a higher film formation temperature is preferable.
[0033] When a pre-prepared compact is used as the orientation precursor layer 40, it can be produced by molding raw material powder of the orientation precursor. For example, when press molding is used, the orientation precursor layer 40 is a press-molded body. The press-molded body can be produced by press molding raw material powder of the orientation precursor based on a known method, for example, by placing the raw material powder in a mold and pressing it at a pressure of preferably 100 to 400 kgf / cm. 2 , more preferably 150 to 300 kgf / cm 2The sheet can be fabricated by pressing the SiC single crystal substrate 20 at a pressure of 1000 psi. Furthermore, the molding method is not particularly limited, and in addition to press molding, tape casting, extrusion molding, slip casting, doctor blade molding, and any combination thereof can be used. For example, when using tape casting, additives such as binders, plasticizers, dispersants, and dispersion media are appropriately added to the raw material powder to form a slurry, and this slurry is then discharged and molded into a sheet by passing it through a narrow slit-shaped discharge port. The thickness of the sheet-shaped molded body is not limited, but from the perspective of handling, a thickness of 5 to 500 μm is preferable. Furthermore, if a thick orientation precursor layer is required, multiple sheets of this molded body can be stacked to achieve the desired thickness. These molded bodies are subsequently heat-treated on the SiC single crystal substrate 20, and the portion near the SiC single crystal substrate 20 becomes the SiC substrate 30. In this method, the molded body must be sintered in the heat treatment process described below. The SiC substrate 30 is preferably formed after the molded body is sintered and integrated with the SiC single crystal substrate 20 as a polycrystalline body. If the compact is not sintered, epitaxial growth using the SiC single crystal as a seed may not occur sufficiently. For this reason, the compact may contain additives such as sintering aids in addition to the SiC raw material.
[0034] (b) Heat Treatment Step As shown in FIG. 2(b), in the heat treatment step, a stack in which an orientation precursor layer 40 is stacked or placed on a SiC single crystal substrate 20 is heat-treated to produce a SiC substrate 30. The heat treatment method is not particularly limited as long as epitaxial growth occurs using the SiC single crystal substrate 20 as a seed. It can be performed in a known heat treatment furnace, such as a tubular furnace or a hot plate. In addition to these atmospheric (pressless) heat treatments, pressurized heat treatments such as hot pressing and HIP, or a combination of atmospheric and pressurized heat treatments, can also be used. The heat treatment atmosphere is preferably a nitrogen-containing inert gas atmosphere. The nitrogen-containing inert gas is preferably a mixed gas containing nitrogen and argon. The nitrogen flow rate is, for example, 0.5 to 15 L / min, and the argon flow rate is, for example, 3 to 100 L / min. The heat treatment temperature is preferably 1700 to 2700°C. Increasing the temperature facilitates the growth of the orientation precursor layer 40 while oriented along the c-axis and a-axis, using the SiC single crystal substrate 20 as a seed crystal. Therefore, the heat treatment temperature is preferably 1700°C or higher, more preferably 1800°C or higher, even more preferably 1900°C or higher, and particularly preferably 2200°C or higher. On the other hand, excessively high temperatures can result in partial loss of SiC due to sublimation or plastic deformation of the SiC, resulting in defects such as warping. Therefore, the heat treatment temperature is preferably 2700°C or lower, more preferably 2500°C or lower. However, because the heat treatment conditions affect the content of rare earth elements in the biaxially oriented SiC layer, it is preferable to appropriately control the conditions (e.g., heat treatment temperature and holding time). From this perspective, the heat treatment temperature is preferably 1900 to 2700°C, more preferably 2200 to 2600°C, and even more preferably 2400 to 2500°C. Furthermore, the holding time is preferably 2 to 30 hours, more preferably 4 to 20 hours. Furthermore, the heat treatment temperature and holding time are related to the thickness of the SiC substrate 30 produced by epitaxial growth, and can be adjusted as appropriate.
[0035] However, when a pre-formed compact is used as the orientation precursor layer 40, it is necessary to sinter it during the heat treatment, and high-temperature atmospheric pressure firing, hot pressing, HIP, or a combination thereof is suitable. For example, when using hot pressing, the surface pressure is 50 kgf / cm. 2 More preferably, 100 kgf / cm 2 More preferably, 200 kgf / cm 2 The firing temperature is not particularly limited, as long as sintering and epitaxial growth occur. However, since firing conditions affect the content of rare earth elements in the biaxially oriented SiC layer, it is preferable to appropriately control the firing conditions (e.g., firing temperature and holding time). From this perspective, the firing temperature is preferably 1700 to 2700°C. The holding time is preferably 2 to 18 hours. The firing atmosphere can be selected from vacuum, nitrogen, inert gas, or a mixture of nitrogen and inert gas. Furthermore, firing may be performed in multiple stages, with the firing temperature and total holding time preferably within the above ranges. The raw SiC powder may be composed of at least one of α-SiC and β-SiC, but is preferably composed of β-SiC. The SiC powder is preferably composed of SiC particles having an average particle size of 0.01 to 100 μm. The average particle size refers to the average value obtained by observing the powder with a scanning electron microscope and measuring the maximum diameter in a specific direction for 100 primary particles.
[0036] During the heat treatment process, the crystals in the orientation precursor layer 40 grow from the crystal growth surface of the SiC single crystal substrate 20 while being oriented in the c-axis and a-axis, so that the orientation precursor layer 40 gradually changes from the crystal growth surface into the SiC substrate 30. The SiC composite substrate including the resulting SiC substrate 30 has a controlled Raman shift value, which indicates a peak corresponding to the shear wave acoustic branch of the Raman spectrum, and has reduced warpage. While the exact mechanism behind this is unclear, it is thought that, for example, increasing the flow rate of nitrogen during heat treatment increases the uniformity of the nitrogen concentration and heat distribution, resulting in reduced warpage.
[0037] 2(c) Grinding and / or Polishing Step As shown in Fig. 2(c), in the grinding step, the orientation precursor layer 40 remaining on the SiC substrate 30 after the heat treatment step is ground and removed to expose the surface of the SiC substrate 30, and the exposed surface is then ground and / or polished to obtain the SiC composite substrate 10.
[0038] It should be noted that the present invention is not limited to the above-described embodiment, and may be embodied in various forms as long as it falls within the technical scope of the present invention. For example, in the above-described embodiment, only one SiC substrate 30 is provided on the SiC single crystal substrate 20, but two or more layers may be provided. Specifically, a second SiC substrate 30 can be provided on the SiC substrate 30 by stacking an orientation precursor layer 40 on the SiC substrate 30 of the SiC composite substrate 10, performing heat treatment, and then grinding and / or polishing in this order.
[0039] The present invention will be further illustrated by the following examples.
[0040] Example 1 (1) Preparation of Textured Precursor Layer A raw material powder containing 93.0 wt.% of commercially available fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 7.0 wt.% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was prepared. This raw material powder was mixed in ethanol using SiC balls in a ball mill for 24 hours and then dried to obtain a mixed powder. A commercially available SiC single crystal substrate (n-type 4H-SiC, diameter 100 mm (4 inches), Si-face, (0001) plane, off-angle 4°, thickness 0.35 mm, no orientation flat) was prepared as the SiC single crystal layer. The mixed powder was sprayed onto the SiC single crystal substrate using the AD device 50 shown in FIG. 3 to form an AD film (textured precursor layer).
[0041] The AD film formation conditions were as follows. First, the carrier gas was He, and the film was formed using a ceramic nozzle with a slit of 5 mm long x 0.4 mm short. The nozzle scanning conditions were a scan speed of 0.5 mm / s, moving 105 mm in a direction perpendicular to the long side of the slit and advancing, moving 5 mm in the long side direction of the slit, moving 105 mm in a direction perpendicular to the long side of the slit and returning, and moving 5 mm in the long side direction of the slit and in the opposite direction from the initial position, and repeating the following scans. When the nozzle had moved 105 mm from the initial position in the long side direction of the slit, it scanned in the opposite direction from before, and returned to the initial position. This cycle was repeated 4000 times. The thickness of the AD film formed in this way was approximately 400 μm.
[0042] (2) Heat Treatment of the Orientation Precursor Layer The SiC single crystal substrate on which the AD film, which is the orientation precursor layer, was formed was removed from the AD device and annealed in a mixed gas of argon and nitrogen at 2400°C for 10 hours. That is, the orientation precursor layer was heat-treated to form a heat-treated layer. At this time, the flow rate of argon was 4.5 L / min and the flow rate of nitrogen was 0.5 L / min.
[0043] (3) Grinding (3a) Surface Grinding The (0001) surface of the SiC single crystal substrate on which the heat treatment layer was formed was surface-ground to a predetermined thickness using a grinder (a diamond wheel with a grit of 1000 to 6000) to achieve the target thickness and surface condition.
[0044] (3b) Backside Grinding The (000-1) surface of the SiC single crystal substrate on which the heat treatment layer had been formed was surface-ground to a predetermined thickness using a grinder (a diamond wheel with a grit of 1000 to 6000) to achieve the target thickness and surface condition.
[0045] (4) Polishing The (0001) and (000-1) faces of the SiC single crystal substrate on which the heat treatment layer was formed were polished with diamond abrasive grains, and then the (0001) face was finished by chemical mechanical polishing (CMP) to achieve the target thickness and surface condition. In this way, a SiC substrate was obtained.
[0046] (5) Raman Spectroscopic Measurement Raman shift values showing peaks corresponding to the shear wave acoustic branch of the Raman spectrum were measured at 1 mm intervals on two mutually orthogonal lines passing through the center point of the (0001) plane (i.e., Si plane) of the obtained SiC substrate. In addition, Raman shift values showing peaks corresponding to the shear wave acoustic branch of the Raman spectrum were measured at 1 mm intervals on two mutually orthogonal lines passing through the center point of the (000-1) plane (i.e., C plane) of the obtained SiC substrate. The measurement conditions at this time are as follows. Of the Raman shift values measured on these four lines, the maximum value k max and the minimum value k min The difference (k max -k min The results are shown in Table 1. The Raman shift value showing the peak corresponding to the shear wave acoustic branch in the Raman spectrum is FTA(2 / 4)E 2 (wave number 200cm -1 The Raman shift value indicates a peak in the vicinity of the Raman peak.
[0047] <Raman spectroscopy measurement conditions> Measurement device: LabRAM HR Evolution manufactured by Horiba, Ltd. Light source: semiconductor pumped solid state laser (DPSS, 532 nm, 100 mW) Diffraction grating: 1800 gr / mm Optical system: backscattering configuration Objective lens: 100x magnification Laser irradiation time: 5 seconds
[0048] (6) Warpage Measurement The degree of warpage, i.e., the amount of warpage, was measured for the surface of the obtained SiC substrate using a high-precision laser measuring instrument (LT-9010M manufactured by Keyence Corporation). As shown in Fig. 4, in a plan view diagram when the (0001) plane of SiC substrate 10 is viewed in plan, two lines X and Y that are perpendicular to each other and pass through point G, which is the center of gravity of the plan view diagram, were drawn, and two points A and B, each 45 mm away from point G on line X, and two points C and D, each 45 mm away from point G on line Y, were determined. Next, as shown in FIG. 5 , among line segments extending perpendicular to the line segment AB from any point on the curve AB between points A and B on the surface of the SiC substrate 10, point P on the curve AB was determined as the longest line segment (for example, in FIG. 5 , points P, O, etc. are arbitrary points on the curve AB, and among line segments extending perpendicular to the line segment AB from each of these points, the line segment extending from point P is the longest line segment). The distance between the line segment AB and point P was determined as the amount of warpage α. Furthermore, as shown in FIG. 6 , among line segments extending perpendicular to the line segment CD from any point on the curve CD between points C and D on the surface of the SiC substrate 10, point R on the curve CD was determined as the longest line segment (for example, in FIG. 6 , points R, O, etc. are arbitrary points on the curve CD, and among line segments extending perpendicular to the line segment CD from each of these points, the line segment extending from point R is the longest line segment). The distance between the line segment CD and the point R was defined as the amount of warpage β. The average value of these amounts of warpage α and β was defined as the amount of warpage of the SiC substrate. The results were as shown in Table 1. The amount of warpage can be measured by the above-described measurement method whether the SiC substrate 10 warps in a convex shape or a concave shape.
[0049] (7) Measurement of the concentration of N and rare earth elements in the heat-treated layer The center of the (0001) plane of the SiC substrate was used as the evaluation point, and dynamic secondary ion mass spectrometry (D-SIMS) was performed. For rare earth elements (Y in this example), an IMS-7f manufactured by CAMECA was used as the analyzer, and the primary ion species was O 2 + The measurement was carried out at an acceleration voltage of 11.0 kV. For N, the analyzer used was an IMS-7f manufactured by CAMECA, and the primary ion species was Cs+ The measurement was carried out at an acceleration voltage of 15.0 kV. RE (atoms / cm 3 ) and the concentration of N C N (atoms / cm 3 The results are shown in Table 1.
[0050] (8) Evaluation of Biaxial Orientation of Heat-Treated Layer Using EBSD (Electron Backscatter Diffraction Patterns) under the conditions shown below, inverse pole figure mapping of the surface (plate surface) of the obtained heat-treated layer and a cross section perpendicular to the plate surface was measured. As a result, the tilt angle distribution was 0.01° or less in both the approximately normal direction and the approximately plate surface direction. Therefore, it was determined that the heat-treated layer was a biaxially oriented SiC layer oriented along the c-axis and a-axis, and had an off angle similar to that of the SiC single crystal substrate.
[0051] <EBSD measurement conditions> Measurement device: SEM (SU-5000, manufactured by Hitachi High-Technologies Corporation) equipped with an electron backscatter diffraction device (EBSD) (Nordlys Nano, manufactured by Oxford Instruments) Acceleration voltage: 15 kV Spot intensity: 70 Working distance: 22.5 mm Step size: 0.5 μm Specimen tilt angle: 70° Measurement program: Aztec (version 3.3)
[0052] Example 2: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, the argon flow rate was set to 45 L / min and the nitrogen flow rate was set to 5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0053] Example 3: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, the argon flow rate was set to 90 L / min and the nitrogen flow rate was set to 10 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0054] Example 4: A SiC substrate was fabricated and evaluated in the same manner as in Example 1, except that in (2) above, the argon flow rate was set to 5 L / min and the nitrogen flow rate was set to 0.5 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0055] Example 5: A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a raw material powder containing 91.7 wt% of commercially available fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 8.3 wt% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was used. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0056] Example 6: A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a raw material powder containing 95.2 wt% of commercially available fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 4.8 wt% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was used. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0057] Example 7: A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (1) above, a raw material powder containing 93.0 wt% of commercially available fine β-SiC powder (volume-based D50 particle size: 0.7 μm) and 7.0 wt% of yttrium oxide powder (volume-based D50 particle size: 0.1 μm) was used. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0058] Example 8 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (2) above, the argon flow rate was 2.7 L / min and the nitrogen flow rate was 0.3 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0059] Example 9 (Comparative) A SiC substrate was produced and evaluated in the same manner as in Example 1, except that in (2) above, the argon flow rate was set to 0.9 L / min and the nitrogen flow rate was set to 0.1 L / min. The obtained heat-treated layer was confirmed to be a biaxially oriented SiC layer. The results are shown in Table 1.
[0060]
Claims
1. A SiC substrate having a biaxially oriented SiC layer, wherein the maximum Raman shift value k is within the Si surface and the C surface of the SiC substrate. max and the minimum value k min The difference is 0.50 cm -1 the Raman shift value is a value obtained by measuring Raman shift values showing peaks corresponding to shear wave acoustic branches of a Raman spectrum at 1 mm intervals on two straight lines passing through a center point of the Si-face and perpendicular to each other, within the Si-face of the SiC substrate, and measuring Raman shift values showing peaks corresponding to shear wave acoustic branches of a Raman spectrum at 1 mm intervals on two straight lines passing through a center point of the C-face and perpendicular to each other, within the C-face of the SiC substrate.
2. The maximum value k max and the minimum value k min The difference is 0.20 cm -1 The SiC substrate according to claim 1 , wherein:
3. The N concentration of the biaxially oriented SiC layer is 5.0×10 18 atoms / cm 3 The SiC substrate according to claim 1 or 2.
4. The rare earth element concentration of the biaxially oriented SiC layer is 1.0×10 14 ~5.0 x 10 15 atoms / cm 3 The SiC substrate according to claim 1 or 2.
5. A SiC composite substrate comprising a SiC single crystal substrate and the SiC substrate according to claim 1 or 2 on the SiC single crystal substrate.
Citation Information
Patent Citations
Silicon carbide single crystal wafer
JP2016164120A
Silicon carbide substrate and method for manufacturing silicon carbide substrate
WO2021111835A1
Internal stress evaluation method of silicon carbide single crystal wafer, and prediction method of warp of silicon carbide single crystal wafer
JP2015059073A
Silicon carbide substrate
JP2017075074A
Silicon carbide substrate and silicon carbide epitaxial substrate
JP2022120059A