Bonded body and method for producing bonded body
By bonding piezoelectric and support substrates with an inclined outer peripheral portion and subsequent polishing, the method addresses unbonded area issues, preventing cracks and improving yield by ensuring a smooth interface.
Patent Information
- Application Number
- PCT/JP2023/045490
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2023-12-19
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional methods for bonding piezoelectric and support substrates often result in unbonded areas at the outer periphery, leading to peeling and cracking issues during processing, which decreases yield due to the formation of corners on the substrate's periphery.
A bonded body is created by bonding a piezoelectric material substrate and a support substrate with an outer peripheral portion that is inclined, followed by a polishing process to form a sloped surface, eliminating corners and reducing the likelihood of cracks.
The method prevents corner formation and subsequent cracking on the outer periphery, enhancing the yield and stability of the bonded body by ensuring a smooth, continuous interface between the piezoelectric and support substrates.
Smart Images

Figure JP2023045490_31102024_PF_FP_ABST
Abstract
Description
Joint and method for manufacturing the joint
[0001] The present invention relates to a bonded body and a method for manufacturing the bonded body.
[0002] To achieve high-performance semiconductor devices, for example, structures in which a piezoelectric material substrate and a support substrate are bonded together have been investigated. In recent years, structures including intermediate layers and structures using support substrates made of difficult-to-process materials have been proposed to achieve even higher performance devices. To achieve this structure, both the piezoelectric material substrate and the support substrate must be bonded together. However, bonding these substrates results in an unbonded area (unbonded portion) on the periphery. The unbonded portion arises due to the shape of the periphery of the substrates before bonding. This shape is known as sagging or roll-off. Furthermore, the occurrence of an unbonded portion on the periphery makes the piezoelectric material more susceptible to peeling during processing. Furthermore, peeling can produce fragments, which can damage the piezoelectric material. To avoid this, a processing method has been proposed to remove the unbonded portion on the periphery.
[0003] Patent Document 1 discloses a composite substrate used in an acoustic wave device, which includes a support substrate, a piezoelectric substrate, and an adhesive layer that bonds the support substrate and the piezoelectric substrate. In this composite substrate, when the surface of the piezoelectric substrate that is bonded to the support substrate is defined as a first surface and the surface opposite the first surface is defined as a second surface, the piezoelectric substrate is formed so that when the first surface is projected onto the second surface in a direction perpendicular to the second surface, the first surface is located inside the second surface. In other words, the outer periphery of the piezoelectric substrate is formed so that the circumference increases toward the outer periphery.
[0004] International Publication No. 2011 / 013553
[0005] However, while conventional methods can prevent problems caused by unbonded areas in the outer periphery, they result in an unusual shape in which corners are formed on the substrate. This can lead to breakage or cracks in the outer periphery in later processes, resulting in a decrease in yield. The present invention aims to provide a bonded body and a method for manufacturing a bonded body in which corners are not formed in the outer periphery and breakage or cracks are less likely to occur in the outer periphery in later processes.
[0006] In order to solve the above problems, the present invention provides a bonded body having a piezoelectric material substrate, a support substrate bonded to the piezoelectric material substrate, and a peripheral processed portion inclined at the outer peripheries of the piezoelectric material substrate and the support substrate with respect to the main surface of the piezoelectric material substrate, wherein the peripheral processed portion includes a first inclined surface facing the piezoelectric material substrate, and a second inclined surface facing the support substrate, which is on a plane extending from the first inclined surface toward the outer periphery.
[0007] The present invention also provides a method for manufacturing a bonded body, which includes a bonding step of bonding a piezoelectric material substrate and a support substrate, and a polishing step of polishing the outer peripheries of the bonded piezoelectric material substrate and support substrate, wherein the polishing step polishes the outer periphery of the bonded piezoelectric material substrate so as to form an outer periphery processed portion that is inclined with respect to the main surface of the piezoelectric material substrate and includes a first inclined surface facing the piezoelectric material substrate and a second inclined surface facing the support substrate, which is on a plane extending from the first inclined surface toward the outer periphery.
[0008] According to the present invention, it is possible to provide a bonded body in which no corners are formed on the outer periphery and in which breakage or cracks are unlikely to occur on the outer periphery in a later process, and a method for manufacturing the bonded body.
[0009] 1 is a diagram showing a bonded body according to the present embodiment; and FIG. 2 is a flowchart illustrating a method for manufacturing a bonded body. (A) to (E) are diagrams illustrating the states of the respective steps shown in FIG. 2. (A) to (D) are diagrams illustrating step 106 (grinding step) and step 107 (polishing step) in FIG. 2. (A) to (B) are diagrams comparing polishing according to the polishing step of the present embodiment with polishing according to a conventional method. (A) to (D) are diagrams comparing the states before and after the grinding step and the polishing step.
[0010] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0011] 1 is a diagram showing a bonded body 1 according to the present embodiment. The bonded body 1 shown in the figure has a structure in which a piezoelectric layer 11a, a dielectric layer 12, and a support substrate 13 are stacked in this order from the top in the figure.
[0012] The piezoelectric layer 11a is a layer made of a piezoelectric material. The piezoelectric material is selected depending on the application of the bonded body 1. For example, the piezoelectric material is LiNbO 3 (LN) and LiTaO 3 (LT), but is not limited to this, and silicon (Si), gallium arsenide (GaAs), silicon carbide (SiC), gallium nitride (GaN), zinc oxide (ZnO), solid solution ceramics (PZT), etc. may be appropriately selected.
[0013] The dielectric layer 12 is a layer disposed under the piezoelectric layer 11a. In this embodiment, the dielectric layer 12 is made of SiO 2 That is, the dielectric layer 12 is mainly composed of SiO 2 Film and SiO 2 It can also be said to be a layer.
[0014] The support substrate 13 serves as a support for the entire bonded structure 1. The support substrate 13 is bonded to the piezoelectric layer 11a via the dielectric layer 12. Any appropriate substrate can be used as the support substrate 13. The support substrate 13 may be made of a single crystal or a polycrystalline material. It may also be made of a metal.
[0015] The material constituting the support substrate 13 is preferably selected from the group consisting of silicon, sialon, sapphire, cordierite, mullite, glass, quartz, crystal, alumina, SUS, iron-nickel alloy (42 alloy), and brass. The thickness of the support substrate 13 is, for example, 0.2 to 1 mm, but any other appropriate thickness can be adopted.
[0016] The silicon may be single crystal silicon, polycrystalline silicon, or high-resistivity silicon, and the support substrate 13 may be SOI (Silicon on Insulator).
[0017] Typically, the sialon is a ceramic obtained by sintering a mixture of silicon nitride and alumina, and for example, Si 6-w Al w O w N 8-wSpecifically, sialon has a composition in which alumina is mixed in silicon nitride, and w in the formula indicates the mixing ratio of alumina. w is preferably 0.5 or more and 4.0 or less.
[0018] Typically, the sapphire is Al 2 O 3 The alumina is a single crystal having a composition of Al 2 O 3 The alumina is preferably a translucent alumina.
[0019] Typically, the cordierite is 2MgO.2Al 2 O 3 5SiO 2 The mullite is a ceramic having a composition of 3Al 2 O 3 2SiO 2 ~2Al 2 O 3 SiO 2 It is a ceramic having a composition in the range of
[0020] <Device> The structure of the bonded body 1 shown in the figure can be used as the structure of various devices, such as high-frequency devices, power semiconductors, semiconductor lasers, surface acoustic wave (SAW) filters, thin-film piezoelectric MEMS (Micro Electro Mechanical Systems), etc.
[0021] <Description of Manufacturing Method of Bonded Body 1> Next, a manufacturing method of the bonded body 1 will be described. FIG. 2 is a flowchart illustrating the manufacturing method of the bonded body 1. FIGS. 3A to 3E are diagrams illustrating the respective processes of steps 101 to 105 shown in FIG. 2. First, a piezoelectric material substrate 11 is prepared, and a dielectric layer 12a is formed on the surface of the piezoelectric material substrate 11 (step 101). A support substrate 13 is prepared, and a dielectric layer 12b is formed on the surface of the support substrate 13 (step 102). By steps 101 and 102, dielectric layers 12a and 12b are formed on the surfaces of the piezoelectric material substrate 11 and the support substrate 13 (dielectric layer forming step: FIG. 3A). The order of steps 101 and 102 may be reversed, and it is not necessary to form the dielectric layers 12a and 12b on the surfaces of the piezoelectric material substrate 11 and the support substrate 13 in steps 101 and 102. Here, the "surface" refers to the main surface of the piezoelectric material substrate 11 and the support substrate 13, not the side surface.
[0022] The dielectric layers 12a and 12b are made of SiO 2 The dielectric layers 12a and 12b are integrated by bonding in a later step, and the dielectric layers 12a and 12b are made of SiO 2 The dielectric layers 12a and 12b can be formed by reactive sputtering using a reactive sputtering device. Specifically, the piezoelectric material substrate 11 and the support substrate 13 are placed in the reactive sputtering device. A target made of silicon (Si) is also placed in the reactive sputtering device. Argon (Ar) gas and oxygen radicals are then introduced into the reactive sputtering device. The silicon that constitutes the target is then sputtered using a sputtering power supply to form a silicon film on the piezoelectric material substrate 11 and the support substrate 13, which is then oxidized by the oxygen radicals to form silicon oxide (SiO 2 As a result, the surfaces of the piezoelectric material substrate 11 and the support substrate 13 are coated with SiO 2 The dielectric layers 12a and 12b can be formed by polishing and planarizing the dielectric layers 12a and 12b. This improves the bonding strength when they are bonded in a later step.
[0023] Next, the surfaces of the dielectric layers 12a and 12b are activated by plasma (step 103: activation step) (FIG. 3B). 2 Plasma can be used, and as a result, the SiO 2 constituting the dielectric layers 12a and 12b can be removed as shown in FIG. 2 is activated, and a hydroxyl group (OH group) is generated as a hydrophilic functional group. Therefore, this process can also be considered as a hydrophilization process in which the surfaces of the dielectric layers 12a and 12b are made hydrophilic by plasma.
[0024] Furthermore, the surfaces of the dielectric layers 12a and 12b after the activation step are bonded together (step 104: bonding step) ( FIG. 3(D) ). Bonding is performed, for example, by bringing the surfaces of the dielectric layers 12a and 12b into contact with each other and pressing them together with a predetermined pressure. This bonds the piezoelectric material substrate 11 and the support substrate 13 via the dielectric layers 12a and 12b. If the dielectric layers 12a and 12b are not provided on the piezoelectric material substrate 11 and the support substrate 13 in steps 101 and 102, activation may be performed by irradiating the surfaces of the piezoelectric material substrate 11 and the support substrate 13 with a fast atom beam (hereinafter referred to as FAB) using an inert gas such as Ar as the atomic species for a predetermined period of time. After activation, the piezoelectric material substrate 11 and the support substrate 13 are bonded together in the same manner as in the bonding step.
[0025] Then, the bonded piezoelectric material substrate 11 and support substrate 13 are heated (step 105: heating step) (FIG. 3(E)). Heating is performed, for example, by placing the bonded piezoelectric material substrate 11 and support substrate 13 in a heating device such as an oven at a predetermined temperature and for a predetermined time. Hydroxy groups generated on the surfaces of the dielectric layers 12a and 12b are covalently bonded by heating. The dielectric layers 12a and 12b are then integrated to form the dielectric layer 12. As a result, the piezoelectric material substrate 11 and support substrate 13 are firmly bonded via the dielectric layer 12. At this time, the following reaction occurs: [Si-OH] + [OH + Si] → [Si-O-Si] + H 2 O reacts to form water (H 2O) is generated. This water is released outside the dielectric layer 12. The heating step can also be considered as a step of annealing the bonded piezoelectric material substrate 11 and support substrate 13 (annealing step).
[0026] Next, the piezoelectric material substrate 11 is ground into a thin film (step 106: grinding step). This forms the piezoelectric layer 11a shown in FIG. 1. Grinding can be performed by a known method using a grinding machine. Then, the outer peripheries of the piezoelectric material substrate 11 and the support substrate 13 are polished (step 107: polishing step). Polishing can be performed by pressing a polishing film against the edge of the outer periphery of the bonded body 1 and rotating the bonded body 1 and the polishing film. The bonded body 1 can be manufactured through the above steps. These grinding and polishing steps will be described in detail below.
[0027] 4A to 4D are diagrams illustrating step 106 (grinding step) and step 107 (polishing step) in FIG. 2. Among these, FIG. 4A shows the piezoelectric material substrate 11 (LiTaO in the illustrated example) after bonding through step 104 (bonding step) and step 105 (heating step). 3 1, a dielectric layer 12 is not provided, but may be provided.
[0028] 4B shows the piezoelectric material substrate 11 and the support substrate 13 after grinding in step 106 (grinding step). As shown in the figure, the piezoelectric material substrate 11 is thinned by grinding, and a piezoelectric layer 11a is formed.
[0029] FIG. 4(C) is a diagram illustrating the state of FIG. 4(B) in more detail, showing the state before the polishing process of step 107. This can be said to be the state before the edge polishing (polishing of the periphery) of the piezoelectric material substrate 11 and the support substrate 13. In this case, the unbonded portion X, which is the portion where the piezoelectric material substrate 11 and the support substrate 13 are not bonded, is 0.7 mm to 1.5 mm. In this embodiment, the unbonded portion X is eliminated and the piezoelectric material substrate 11 (LiTaO in the illustrated example) is polished.3 Polishing is performed along a polishing plane P indicated by the dotted line so that the piezoelectric material substrate 11 and the support substrate 13 (a Si substrate in the illustrated example) have a smoothly continuous structure, thereby forming a peripheral processed portion R on the outer periphery of the piezoelectric material substrate 11 and the support substrate 13. In practice, polishing is performed along the polishing plane P, for which the polishing angle and the range of the unbonded portion X are specified. Specifically, in the polishing process, polishing is performed to form a polishing plane P having an angle θ of 3.5° to 12.0° with respect to the main surface H of the piezoelectric material substrate 11 and the support substrate 13. This can also be said to be polishing at a polishing angle θ of 3.5° to 12.0° with respect to the main surface H of the piezoelectric material substrate 11 and the support substrate 13. In addition, in the polishing process, polishing is performed so that the length, as viewed from above, of the second inclined plane P2, where the support substrate 13 is exposed as a result of the removal of the piezoelectric material substrate 11 by polishing, in the direction from the center of the support substrate 13 to the outer periphery, is 0.7 mm to 1.5 mm when viewed from above. As a result, a polished surface P is formed which is composed of a first inclined surface P1 facing the piezoelectric material substrate 11 and a second inclined surface P2 facing the support substrate 13, with the first inclined surface P1 and the second inclined surface P2 being continuous. Therefore, the polishing process can also be said to be a process of polishing to form a peripheral processed portion R which is inclined with respect to the main surface H of the piezoelectric material substrate 11 and which is composed of the first inclined surface P1 facing the piezoelectric material substrate 11 and the second inclined surface P2 facing the support substrate 13, with the first inclined surface P1 and the second inclined surface P2 being continuous.
[0030] When the angle is 3.5° or more, an area that can be used sufficiently for the bonded body 1 is preferably provided. When the angle is 12.0° or less, the risk of forming a corner that may cause breakage or cracks on the outer periphery in a later process is suppressed, which is preferable. When the length is 0.7 mm or more, a structure in which the piezoelectric material substrate 11 and the support substrate 13 are smoothly connected is sufficiently ensured. When the length is 1.5 mm or less, an area that can be used sufficiently for the bonded body 1 is preferably provided.
[0031] FIG. 4(D) shows the state after the polishing process of step 107. That is, it shows the state after polishing has been performed at the polishing plane P specified in FIG. 4(C), when the outer peripheral processed portion R has been formed. This can be said to be the state after edge polishing (polishing of the outer periphery) of the piezoelectric material substrate 11 and the support substrate 13. Furthermore, this can also be said to be configured as a bonded body 1 that includes the piezoelectric material substrate 11, the support substrate 13 bonded to the piezoelectric material substrate 11, and the outer peripheral processed portion R, which is formed by processing the outer peripheral portions of the piezoelectric material substrate 11 and the support substrate 13 so as to be inclined with respect to the main surface H of the piezoelectric material substrate 11. The outer peripheral processed portion R is composed of a first inclined surface P1 facing the piezoelectric material substrate 11 and a second inclined surface P2 facing the support substrate 13, and the first inclined surface P1 and the second inclined surface P2 are continuous. The bonded body 1 can also be configured such that the first inclined surface P1 and the second inclined surface P2 of the outer peripheral processed portion R are inclined at an angle of 3.5° to 12.0° with respect to the main surface H of the piezoelectric material substrate 11. The bonded body 1 can also be configured such that the length of the second inclined surface P2 as viewed from above is 0.7 mm to 1.5 mm.
[0032] If a dielectric layer 12 is present between the piezoelectric material substrate 11 and the support substrate 13, the first inclined surface P1 and the second inclined surface P2 will no longer be continuous. This case can also be included in the form that the outer periphery processed portion R includes the first inclined surface P1 that the piezoelectric material substrate 11 faces, and the second inclined surface that is located on a plane extending from the first inclined surface P1 toward the outer periphery and that the support substrate 13 faces. That is, although the first inclined surface P1 and the second inclined surface P2 are not continuous, they exist on the same plane, and the surface of the dielectric layer 12 exists between them. The surface of the dielectric layer 12 also exists on this plane.
[0033] Furthermore, in this case, the polishing process can also be said to polish the piezoelectric material substrate 11 so as to form an outer peripheral processed portion R including the first inclined surface P1 and the second inclined surface P2, which is inclined with respect to the main surface H of the piezoelectric material substrate 11 and is composed of a first inclined surface P1 facing the piezoelectric material substrate 11 and a second inclined surface P2 facing the support substrate 13 and is located on a surface extending from the first inclined surface P1 toward the outer periphery.
[0034] FIGS. 5A and 5B compare the results of polishing using the polishing process of the present embodiment with those of polishing using a conventional method. FIG. 5A shows a bonded body 1 polished using the polishing process of the present embodiment. In contrast, FIG. 5B shows a bonded body 1 polished using a conventional polishing method. In FIG. 5A, the polishing plane P indicated by the dotted line is designated, and the first inclined plane P1 and the second inclined plane P2 forming this polishing plane P are continuous, resulting in a smoothly continuous structure between the piezoelectric layer 11a and the support substrate 13. In contrast, in FIG. 5B, the polishing plane P is designated by the dotted line, and in this case, two corners K are formed in the piezoelectric layer 11a and the support substrate 13. In the bonded body 1 of FIG. 5B, there is no unbonded portion X, but the presence of the corners K makes it more likely that breaks or cracks will occur in the outer periphery during a subsequent polishing process of the piezoelectric material substrate 11. This results in a reduced yield. On the other hand, in the bonded body 1 shown in FIG. 5A, the polished surface P formed by polishing is inclined at a predetermined angle relative to the main surface H. At this time, the piezoelectric layer 11a and the support substrate 13 are smoothly connected. This prevents corners K from being formed, making it less likely for breaks or cracks to occur in the outer periphery. Note that the entire edge of the bonded body 1 after edge polishing does not need to have the same angle; it is sufficient that the support substrate 13 side of the piezoelectric layer 11a and the piezoelectric layer 11a side of the support substrate 13 are continuously inclined. Furthermore, if a dielectric layer 12 is present between the piezoelectric layer 11a and the support substrate 13 side, the dielectric layer 12 and the support substrate 13 side may also be continuously inclined.
[0035] (Example 1) A piezoelectric material substrate 11 was made of 42Y-cut black LiTaO with a thickness of 0.25 mm and mirror-polished on both sides. 3 A 0.23 mm thick high-resistivity (≧2 kΩ·cm) Si substrate was prepared as the support substrate 13. Next, SiO 2 films were formed on the LT substrate and Si substrate as the dielectric layers 12a and 12b. 2 The SiO2 film of the LT substrate and the Si substrate were formed to a thickness of 0.5 μm (dielectric layer forming step), and the surface was polished and flattened by about 0.1 μm by CMP (Chemical Mechanical Polishing). 2The film surfaces were exposed to N discharges of 100 W (LT substrate side) and 65 W (Si substrate side). 2 After activation with plasma (activation process), the substrates were bonded (bonding process). The vacuum time in the bonding process was 120 seconds. To increase the bonding strength, the bonded substrates were placed in an oven at 130°C and heated for 4 hours (heating process). The LT surfaces of the bonded substrates removed from the oven were thinned to 2 μm by grinding (grinding process). Then, a polishing film GC#2000 was contacted with the outer periphery and polished for 120 seconds to remove the unbonded portions (polishing process). The head angle for fixing the polishing film was 79°. The film feed rate was 100 mm / min. Finally, the LT surfaces were polished to a thickness of 1 μm, but no abnormalities such as peeling, scratches, chipping, or cracks occurred in the LT substrate. The finished shape of the outer periphery was then confirmed. The inclination was 8.1°, the processing width (from the edge of the Si substrate to the edge of the LT substrate) was 786 μm (0.786 mm), and there were no unbonded portions. That is, the polished surface P has an angle of 8.1° with respect to the surfaces of the LT substrate and the Si substrate.
[0036] Example 2 The width of the unbonded portion X is determined by the sagging of the wafer. When a bonded body is produced using a commercially available wafer, the width of the unbonded portion X is 0.8 mm to 1.2 mm. In Example 2, a bonded body 1 having a width of the unbonded portion X of 1.2 mm was used, and the inclination angle θ, which is the polishing angle of the first inclined surface P1 and the second inclined surface P2, was set to 12°. When the edges were polished, the unbonded portion X was completely removed.
[0037] In Example 3, the inclination angle was set to 13° and the edge was polished. In this case, the unbonded portion X was removed, but the area that could be used as a device was smaller than when the inclination angle was 12°.
[0038] In Example 4, a bonded body having a width of the unbonded portion X of 0.8 mm was used, and the inclination angle was set to 3°, and the edge was polished. In this case, processing was possible, but precise control was required.
[0039] Figures 6(A) to 6(D) are diagrams comparing the states of the LT substrate and the Si substrate before the grinding and polishing processes. Figure 6(A) is a diagram showing the state of the LT substrate and the Si substrate from above before the grinding and polishing processes, and Figure 6(B) is a cross-sectional view of Figure 6(A). Figure 6(C) is a diagram showing the state of the LT substrate and the Si substrate from above after the grinding and polishing processes, and Figure 6(D) is a cross-sectional view of Figure 6(C). That is, Figures 6(B) and 6(D) are views of the LT substrate and the Si substrate viewed from the same direction as Figures 4 and 5. Figure 6(A) corresponds to the case of Figure 4(A), and there is an unbonded portion (length 0.800 mm) where the LT substrate and the Si substrate are separated. Furthermore, as shown in Figure 6(B), the outer periphery of the LT substrate at this time had an angle of 23.8°. Figure 6(C) corresponds to the case of Figure 4(D), and shows the state after polishing. In Fig. 6(C), the polished portion is shown as the outer peripheral processed portion. As shown in Fig. 6(B), the outer peripheral portion of the LT substrate at this time had an angle of 8.1° as described above.
[0040] Although the present embodiment has been described above, the technical scope of the present invention is not limited to the scope of the above embodiment. It is clear from the claims that various modifications and improvements to the above embodiment are also included in the technical scope of the present invention.
[0041] 1...bonded body, 11...piezoelectric material substrate, 11a...piezoelectric layer, 12, 12a, 12b...dielectric layer, 13...support substrate, P...polished surface, P1...first inclined surface, P2...second inclined surface, R...periphery processed portion
Claims
1. A joint comprising a piezoelectric material substrate, a support substrate bonded to the piezoelectric material substrate, and an outer periphery processed portion inclined at the outer periphery of the piezoelectric material substrate and the support substrate with respect to the main surface of the piezoelectric material substrate, the outer periphery processed portion including a first inclined surface facing the piezoelectric material substrate, and a second inclined surface facing the support substrate, the second inclined surface being on a surface extending from the first inclined surface toward the outer periphery.
2. The bonded body according to claim 1, wherein the first inclined surface and the second inclined surface of the outer peripheral processed portion are inclined at an angle of 3.5° or more and 12.0° or less with respect to the main surface of the piezoelectric material substrate.
3. A bonded body as described in claim 1 or 2, wherein the length of the second inclined surface as viewed from above, in the direction from the center of the supporting substrate toward the outer periphery, is 0.7 mm or more and 1.5 mm or less.
4. The bonded body according to claim 1, wherein the supporting substrate is a substrate made of Si.
5. The piezoelectric material substrate and the support substrate are made of SiO 2 5. The bonded body according to claim 4, wherein bonding is performed via a layer.
6. A method for manufacturing a bonded body, comprising: a bonding step of bonding a piezoelectric material substrate and a support substrate; and a polishing step of polishing the outer periphery of the bonded piezoelectric material substrate and support substrate, wherein the polishing step polishes the substrate to form an outer periphery processed portion that is inclined with respect to a main surface of the piezoelectric material substrate and includes a first inclined surface facing the piezoelectric material substrate, and a second inclined surface facing the support substrate, which is on a plane extending from the first inclined surface toward the outer periphery.
7. The method for producing a bonded body according to claim 6, further comprising a grinding step between said bonding step and said polishing step, for grinding said piezoelectric material substrate into a thin film.
8. SiO 2 The method further includes a step of activating, by plasma, the respective surfaces of the piezoelectric material substrate and the support substrate, the surfaces of which are mainly composed of SiO. 2 The method for producing a bonded body according to claim 6 or 7, wherein bonding is performed via a layer.
9. The method for producing a bonded body according to claim 8, further comprising a heating step of heating the bonded piezoelectric material substrate and the supporting substrate.
Citation Information
Patent Citations
Bonded semiconductor substrate
JP1991083320A
Manufacture of laminated wafer
JP1993226305A
Pasted silicon wafers and manufacturing method therefor
JP1999251277A
Chamfering device and chamfering method
JP2017177251A
Wafer chamfering device and wafer chamfering method
JP2019166598A
Cited By
Composite substrate, device, and method for manufacturing composite substrate
WO2026204128A1