Fishing line guide and method for producing fishing gear item

A ribbed fiber-containing resin composition for fishing line guides, combining 3D printing and heating/pressurizing techniques, addresses the need for lightweight and high-strength guides, improving mechanical strength and ease of manufacturing while maintaining lightness.

WO2024224717A1PCT designated stage expired Publication Date: 2024-10-31DAIWA SEIKO CORPORATION +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/001718
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-01-22
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional metal fishing line guides are heavy and lack flexibility, making them unsuitable for lightweight fishing rods, while existing fiber-reinforced plastic guides do not meet the requirements for both lightness and high mechanical strength.

Method used

A fishing line guide made from a fiber-containing resin composition with a ribbed structure, featuring a combination of a ring-shaped and Y-shaped portion, where the inner part of the branch is thin-walled and the outer part is thick-walled, with carbon fibers and a thermosetting resin, manufactured using 3D printing and a heating/pressurizing process to achieve the desired properties.

Benefits of technology

The solution results in a lightweight fishing line guide with enhanced mechanical strength, allowing for easy manufacturing and integration with fishing rods without compromising weight or performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024001718_31102024_PF_FP_ABST
    Figure JP2024001718_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a light-weight fishing gear item with high mechanical strength. This fishing gear item is a fishing line guide of which a body part is composed of a fiber-containing resin composition, the body part having a rib.
Need to check novelty before this filing date? Find Prior Art

Description

Fishing line guide and fishing tackle manufacturing method

[0001] The present invention relates to, for example, a fishing line guide.

[0002] A fishing line guide for guiding a fishing line is known. The fishing line guide comprises a frame and a guide ring. The frame comprises a ring holder and a fixed portion. The ring holder and the fixed portion are integrally formed. The ring holder holds the guide ring. The fixed portion is attached to the outer periphery of the fishing rod. The fishing line is passed through the guide ring. The frame is made by pressing a metal plate. Examples of such metals include stainless steel and titanium. Metal fishing line guides are heavy and have poor flexibility. If multiple metal fishing line guides are attached along the axial length of the fishing rod, the entire rod becomes particularly heavy. Fishing rods that require lightweight construction cannot achieve the desired performance.

[0003] From this perspective, fishing line guides made of fiber-reinforced plastics have been proposed (Patent Nos. 5460441 and 5514061).

[0004] Patent No. 5460441 Patent No. 5514061

[0005] The fishing line guides disclosed in the aforementioned patent documents were excellent. However, there was a demand for fishing line guides that were even lighter and had greater mechanical strength. There was also a demand for a technology that could easily manufacture fishing line guides with the aforementioned characteristics.

[0006] The problem that the present invention aims to solve is to provide a fishing line guide that is lightweight and has excellent mechanical strength, and to provide a technique for easily manufacturing the fishing line guide with the above features.

[0007] The present invention provides a fishing line guide, wherein a main body of the fishing line guide is made of a fiber-containing resin composition, and the main body is provided with ribs.

[0008] The present invention proposes a fishing line guide in which the main body preferably comprises an approximately ring-shaped portion and an approximately Y-shaped portion, the tip of the branched portion of the approximately Y-shaped portion is connected to the approximately ring-shaped portion, and a rib is formed on the branched portion.

[0009] The present invention proposes a fishing line guide as described above, wherein the inner portion of the branched portion is thin-walled and the outer portion of the branched portion is thick-walled, and the thick-walled portion is a rib.

[0010] The present invention proposes a fishing line guide in which the main body preferably comprises an approximately ring-shaped portion and an approximately Y-shaped portion, the tip of the branch of the approximately Y-shaped portion is connected to the approximately ring-shaped portion, and a rib is formed on the approximately ring-shaped portion at a position sandwiched between the branch portions.

[0011] The present invention proposes a fishing line guide as described above, wherein preferably the outer ring portion of the approximately ring-shaped portion sandwiched between the branching portions is thin-walled and the inner ring portion of the approximately ring-shaped portion is thick-walled, and the thick-walled portion is a rib.

[0012] The present invention proposes a fishing line guide as described above, preferably in which the direction in which the branched portion of the substantially Y-shaped portion extends is a direction substantially tangent to the substantially ring-shaped portion.

[0013] The present invention proposes a fishing line guide as described above, preferably in which the width of the branched portion of the substantially Y-shaped portion is wider than the width of the substantially ring-shaped portion.

[0014] The present invention proposes a fishing line guide as described above, wherein the thickness of the rib portion at the branched portion of the substantially Y-shaped portion is preferably substantially the same as the thickness of the substantially ring-shaped portion.

[0015] The present invention proposes a fishing line guide as described above, wherein preferably the width of the base of the substantially Y-shaped portion decreases monotonically from the tip end to the base end.

[0016] The present invention proposes a fishing line guide as described above, wherein the thickness of the base of the substantially Y-shaped portion preferably increases monotonically from the tip end toward the bent position.

[0017] The present invention proposes a fishing line guide as described above, wherein the thickness of the base of the substantially Y-shaped portion preferably becomes thinner from a position past the bent position toward the base end.

[0018] The present invention proposes a fishing line guide as described above, wherein the fiber preferably exists across the substantially ring-shaped portion and the substantially Y-shaped portion.

[0019] The present invention proposes a fishing line guide as described above, wherein the fibers are preferably carbon fibers.

[0020] The present invention proposes a fishing line guide as described above, wherein the fibers preferably have a fiber length of 1 cm or more.

[0021] The present invention proposes a fishing line guide as described above, wherein the resin is preferably a thermosetting resin.

[0022] The present invention proposes a fishing line guide as described above, wherein the resin composition preferably has a ratio of (amount of resin) / (amount of resin+amount of fiber)=30 / 100 to 60 / 100.

[0023] The present invention proposes a fishing line guide, preferably a fishing tackle having a water absorption rate of 2.0% or less.

[0024] The present invention proposes a method for manufacturing fishing tackle, the method comprising: a molding process in which a resin composition containing fibers is molded using a 3D printer; and a heating and pressurizing process in which the molded object obtained in the molding process is heated and pressurized.

[0025] The present invention proposes a method for manufacturing a fishing tackle whose main body is made of a fiber-containing resin composition, the method comprising: a molding process in which a 3D printer is used to mold the resin composition containing fibers; and a heating and pressurizing process in which the molded object obtained in the molding process is heated and pressurized.

[0026] The present invention proposes a method for manufacturing the fishing tackle item, wherein a mold is preferably used in the pressurizing step, the mold comprising mold half A and mold half B, mold half A and mold half B each have a recess with no corners on the concave surface formed on the opposing surfaces of mold half A and mold half B, and after the shaped object is placed in the recess of mold half A, mold half B is placed over it and heated and pressurized.

[0027] The present invention proposes a method for manufacturing a fishing tackle, wherein the heating and pressurizing step is preferably a step in which the shaped object is placed in a mold and heated and pressurized.

[0028] The present invention proposes a method for manufacturing fishing tackle, preferably wherein the heating and pressurizing step comprises a first pressurizing step and a second pressurizing step, and the second pressurizing step is a step in which the product obtained through the first pressurizing step is pressurized under heat, and the volume of the obtained product is smaller than the volume of the product obtained by the first pressurizing step.

[0029] The present invention proposes a method for manufacturing fishing tackle, preferably in which the molding process is a process for obtaining a product in which not all of the fibers are integrally bonded by the resin, but the fibers are partially separated.

[0030] The present invention proposes a method for manufacturing fishing tackle, wherein preferably the first pressurizing step is a step in which the product obtained through the molding step is pressurized, and most of the fibers are integrally bonded by the resin to obtain a product having a curved portion.

[0031] The present invention proposes a method for manufacturing a fishing tackle, wherein the first pressurizing step is preferably a step in which a plurality of products obtained through the shaping step are stacked and pressed.

[0032] The present invention provides a method for manufacturing a fishing tackle, wherein the pressure in the first pressurizing step is preferably lower than the pressure in the second pressurizing step.

[0033] The present invention proposes a method for manufacturing the fishing tackle, preferably, wherein (volume of the product obtained after the first pressurizing step) / (volume of the product obtained after the second pressurizing step) is ≦2.5.

[0034] The present invention proposes a method for manufacturing the fishing tackle, preferably, wherein 1.0<(volume of the product obtained after the first pressurizing step) / (volume of the product obtained after the second pressurizing step)≦2.5.

[0035] The present invention proposes a method for manufacturing the fishing tackle, wherein preferably the first pressurizing step is a step of applying pressure at a temperature equal to or higher than the melting temperature of the resin by the 1 / 2 method using a flow tester CFT-500D (manufactured by Shimadzu Corporation).

[0036] The present invention proposes a method for manufacturing the fishing tackle, wherein preferably the second pressurizing step is a step of pressurizing at a temperature equal to or higher than the melting temperature of the resin by the 1 / 2 method using a flow tester CFT-500D (manufactured by Shimadzu Corporation).

[0037] The present invention proposes a method for manufacturing a fishing tackle, wherein the heating method in the first pressurizing step is preferably a non-contact heating method.

[0038] The present invention proposes a method for manufacturing a fishing tackle, wherein the non-contact heating method is preferably an induction heating method.

[0039] The present invention proposes a method for manufacturing a fishing tackle, preferably in which a mold made of a non-magnetic material is used in the first pressurizing step.

[0040] The present invention proposes a method for manufacturing a fishing tackle, wherein the heating method in the second pressurizing step is preferably a contact heating method.

[0041] The present invention provides a method for manufacturing a fishing tackle, preferably in which a mold made of a metal material is used in the second pressurizing step.

[0042] The present invention proposes a method for manufacturing the fishing tackle, wherein the fibers preferably include fibers having a fiber length of 1 cm or more.

[0043] The present invention proposes a method for manufacturing the fishing tackle, preferably in which the fibers are conductive fibers.

[0044] The present invention proposes a method for manufacturing the fishing tackle, preferably in which the conductive fibers are carbon fibers.

[0045] The present invention proposes a method for manufacturing the fishing tackle, wherein the resin composition preferably has a ratio of (amount of the fibers) / (amount of the resin+amount of the fibers)=30 / 100 to 60 / 100.

[0046] The present invention proposes a method for manufacturing fishing tackle, preferably in which the ratio of the fiber to the resin used in the molding process is (volume of the resin) / (volume of the fiber+volume of the resin)=30 / 100 to 55 / 100.

[0047] The present invention proposes a method for manufacturing the fishing tackle, preferably in which the resin is a thermosetting resin.

[0048] The present invention proposes a method for manufacturing the fishing tackle, preferably wherein the resin is a thermoplastic resin.

[0049] The present invention proposes a method for manufacturing the fishing tackle, wherein the resin composition preferably has a water absorption rate of 2.0% or less.

[0050] The present invention proposes a method for manufacturing the fishing tackle, wherein the first pressurizing step uses a mold having at least a lower mold, a middle mold, and an upper mold, wherein the lower mold has a curved surface portion, the upper mold has a curved surface portion, and the curved surface portion of the upper mold corresponds to the curved surface portion of the lower mold, and the middle mold has a guide portion that guides the product obtained through the additive manufacturing technology step toward the lower mold, wherein the middle mold is placed relative to the lower mold, the product obtained through the additive manufacturing technology step is placed relative to the guide portion of the middle mold, and the upper mold is placed relative to the product placed relative to the guide portion, and pressure is applied between the lower mold and the upper mold, so that a curved portion corresponding to the curved surface portion is formed in the product located between the curved surface portion of the lower mold and the curved surface portion of the upper mold.

[0051] The present invention proposes a method for manufacturing the fishing tackle, wherein the middle mold preferably has a flat surface on its upper surface and a curved surface on its lower surface that corresponds to the curved surface of the lower mold, the guide portion being a gap provided in the vertical direction of the middle mold, and the gap being connected to the curved surface of the lower mold.

[0052] The present invention proposes a method for manufacturing fishing tackle, wherein the second pressurizing step preferably uses a mold having at least a lower mold and an upper mold, the upper mold and the lower mold have a cavity corresponding to the shape of the final product when the upper mold is placed relative to the lower mold, the cavity being composed of a groove formed on the surface of the upper mold and a groove formed on the surface of the lower mold, the groove having a substantially U-shaped cross section, the product obtained through the first pressurizing step being placed on the lower mold, the upper mold being placed on top of the product placed on the lower mold, and pressure being applied between the lower mold and the upper mold.

[0053] The fishing tackle obtained by the above manufacturing method is, for example, a fishing line guide.

[0054] The fishing tackle of the present invention was lightweight and had excellent mechanical strength. Fishing tackle with the above features could be easily manufactured.

[0055] A perspective view of the fishing line guide according to the present invention from one side (front side) A perspective view of the fishing line guide according to the present invention from the other side (back side) A cross-sectional view of the fishing line guide according to the present invention A cross-sectional view of the fishing line guide according to the present invention A perspective view of the lower half of the mold A perspective view of the upper half of the mold in an upside-down state

[0056] Embodiments of the present invention will now be described.

[0057] The first invention relates to a fishing tackle. The fishing tackle may be, for example, a fishing line guide. The main body of the fishing line guide is made of a fiber-containing resin composition. The main body has ribs (thick portions). Previously proposed fishing line guides did not have ribs (rib structures). Conventional fishing line guides have a constant thickness. In contrast, the present invention has ribs (rib structures). The fishing line guide of the present invention has thick and thin portions. The thick portions are ribs. This improves mechanical strength. Furthermore, the fishing line guide of the present invention with ribs (rib structures) is lighter than conventional fishing line guides (without ribs (rib structures)) that have the same mechanical strength as the fishing line guide of the present invention. The thickness of the non-rib portions (thin portions) need only be thinner than the thickness of the ribs (thick portions). This alone achieves weight reduction. The thickness refers to the vertical dimension when the fishing line guide is placed with the surface of its approximately Y-shaped portion horizontal. The thickness is the dimension in the vertical direction in Figures 1, 2, and 3. The width is the dimension in the direction perpendicular to the thickness direction. The thickness direction and width direction hereinafter will also be treated in the same manner as above.

[0058] The main body preferably includes a generally ring-shaped portion. A fishing line is threaded through the generally ring-shaped portion. The main body preferably includes a support portion. The support portion is attached to the fishing rod. The support portion preferably includes a base (trunk) located on the fishing rod side. The support portion preferably includes a branch portion (branch portion: the tip of this branch portion (branch portion) connects to the ring-shaped portion) that branches off at the tip of the base (trunk). The width of the branch portion is approximately half (or less than half) the dimension of the base. The thickness of the branch portion is approximately the same as the thickness of the point where the branch portion connects to the base. The generally ring-shaped portion may be annular, and may be circular, elliptical, or polygonal, such as triangular or rectangular. The generally ring-shaped portion may be partially interrupted (open ring (generally C-shaped)). In other words, it does not necessarily have to be closed. However, it is generally a closed ring. The approximately ring-shaped portion has thin portions (thin portions). This contributes to weight reduction. The approximately ring-shaped portion has thick portions (thick portions). These thick portions are ribs. The support portion is, for example, approximately Y-shaped. The tips of the branch portions (branches) of this approximately Y-shape are connected to the approximately ring-shaped portion. The approximately Y-shaped portion supports the approximately ring-shaped portion. The approximately Y-shaped portion also includes the following cases: The tip side of the approximately Y-shaped portion is approximately V-shaped. That is, there are two wires on the tip side, but this can be three or more. The number of wires is not important, but in reality it will be two or three. This is because the more wires there are, the heavier the wire will be. When force from the fishing line acts on the approximately ring-shaped portion, this force acts on the tip of the support portion (branch portion) that supports the approximately ring-shaped portion. Since there is not one but multiple support parts (branch parts), that is, since the support parts (supporting tip parts) are roughly Y-shaped, the support parts are less likely to bend (twist). Although they are less likely to bend (twist), because the tip parts of the support parts (branch parts) are divided into, for example, two parts, the mechanical strength of each support part (branch part) is reduced. Therefore, to compensate for the reduced mechanical strength, ribs are formed on the branch parts. The inner part of the branch part is thin-walled. The outer part of the branch part is thick-walled. The thick parts are ribs. The reasons why a rib structure was preferable are as follows.This is because the rib structure (i.e., a structure in which the rib is located at an outer position than the inner position) had a higher resistance to deformation pressure such as torsion than a rib structure in which the inner portion of the branch portion is thick and the outer portion is thin. The rib structure may be configured in a location other than the branch portion (branch portion). For example, a rib is configured in the approximately ring-shaped portion at a position sandwiched between the branch portions. The outer ring portion of the approximately ring-shaped portion at a position sandwiched between the branch portions is thin-walled and the inner ring portion of the approximately ring-shaped portion is thick-walled. The thick portion is a rib. Since a rib structure is used in which the inner portion of the branch portion is thin-walled, the outer ring portion is thin-walled. If the configuration were reversed, the structure would become complicated.

[0059] The extending direction of the branch portion (branch portion) of the approximately Y-shaped portion was preferably a direction approximately tangential to the approximately ring-shaped portion. The reason for this is as follows: When the connecting direction between the branch portion and the approximately ring-shaped portion was a direction approximately tangential to the approximately ring-shaped portion, the branch portion could firmly withstand the force applied to the approximately ring-shaped portion. The width of the branch portion (branch portion) of the approximately Y-shaped portion was preferably wider than the width of the approximately ring-shaped portion. The reason for this is as follows: When the width of the branch portion (branch portion) is increased, the mechanical strength of the branch portion is increased. The branch portion could easily withstand the force applied to the approximately ring-shaped portion. The thickness of the rib of the branch portion (branch portion) of the approximately Y-shaped portion was preferably approximately the same as the thickness of the approximately ring-shaped portion. The reason for this is as follows: By making the thicknesses the same, the structure was simplified. The width of the base (trunk: the root-side portion from which the branched portions (branches) are derived) of the approximately Y-shaped portion preferably decreased almost monotonically from the tip (where the branched portions are connected) toward the base (bending position). The thickness of the base (trunk) of the approximately Y-shaped portion preferably increased almost monotonically from the tip toward the bending position. The reason for this is as follows: By increasing the thickness even when the width was narrow, the mechanical strength of the base (trunk) was ensured. In other words, the base was able to firmly withstand the force applied to the approximately ring-shaped portion. The thickness of the base (trunk) of the approximately Y-shaped portion preferably decreased from a position past the bending position toward the base. The reason for this is as follows: To make it easier to fix the base to the fishing rod, the thickness was reduced from approximately the midpoint between the bending position and the base toward the base. The fibers were present across the approximately ring-shaped portion and the approximately Y-shaped portion.

[0060] The structure of the fishing line guide may adopt the disclosures of Patent Document 1 (Japanese Patent No. 5460441) and Patent Document 2 (Japanese Patent No. 5514061) as appropriate. For example, the structure of the main body may adopt the disclosures of Patent Document 1 or Patent Document 2 as necessary. For example, the ring-shaped portion may be provided with a ring made of metal (e.g., Ti, Al, Mg, SUS, etc.) or ceramic. The base (trunk) of the Y-shaped portion may be configured to be easily attached to a fishing rod, for example, bent.

[0061] The fibers of the fiber-containing resin composition constituting the main body of the fishing line guide are reinforcing fibers. Examples of such fibers include inorganic fibers. Organic fibers are also acceptable. A combination of both is also acceptable. The fibers need only satisfy the following requirements: (length of at least ¼ of the circumference of the generally ring-shaped portion)≦(length in the longitudinal direction of the fibers). Alternatively, (length of at least ½ of the length from the base end of the generally Y-shaped portion to the end of one branch)≦(length in the longitudinal direction of the fibers). Preferably, (length from the base end of the generally Y-shaped portion to a portion surrounding the periphery of the generally ring-shaped portion)≦(length in the longitudinal direction of the fibers). While this varies depending on the size of the main body, specific values ​​are, for example, 1 cm or more. Preferably, it is 2 cm or more. More preferably, it is 3 cm or more. Furthermore, it is 6 cm or more. There are no particular restrictions on the average fiber length of the continuous reinforcing fibers used in the present invention. However, from the viewpoint of improving moldability, a range of 0.05 to 20,000 m is preferred. More preferably, it is 100 to 10,000 m. It was more preferably 1000 to 7000 m. A combination of fiber lengths of more than 3 cm (6 cm) and fiber lengths of 3 cm (6 cm) or less may also be used. The fiber length in the present invention is the weight average fiber length, unless otherwise specified. The average fiber diameter of the fibers was preferably 3 μm or more. More preferably, it was 4 μm or more. Even more preferably, it was 5 μm or more. It was preferably 50 μm or less. More preferably, it was 20 μm or less. Even more preferably, it was 12 μm or less. The average fiber diameter is the diameter of a single yarn.

[0062] Examples of the inorganic fibers include carbon fibers, silicon carbide fibers, alumina fibers, boron fibers, glass fibers, and metal fibers. However, the present invention is not limited to these. Multiple types of fibers may be used in combination, rather than just one type. From the viewpoints of mechanical strength and lightness, carbon fibers are preferred. Examples of the carbon fibers include polyacrylonitrile (PAN)-based carbon fibers, petroleum / coal pitch-based carbon fibers, rayon-based carbon fibers, cellulose-based carbon fibers, lignin-based carbon fibers, phenol-based carbon fibers, and vapor-grown carbon fibers. One or more of these may be used as appropriate. The carbon fibers used preferably have a tensile modulus of elasticity of 100 GPa to 1000 GPa. The form of the carbon fibers is not particularly limited. They may be continuous or discontinuous. Examples of continuous fibers include those in which carbon fibers are oriented in one direction (unidirectional materials). Examples of discontinuous fibers include materials in which carbon fibers are oriented in a specific direction in the resin, and materials in which carbon fibers are randomly dispersed in the in-plane direction. Carbon fibers may be in the form of single threads, fiber bundles, or a mixture of both. Carbon fibers are generally in the form of fiber bundles, consisting of thousands to tens of thousands of filaments. When using carbon fiber bundles as carbon fibers, using the carbon fiber bundles as is can result in localized thickening of the entangled portions of the fiber bundles, making it difficult to obtain carbon fiber reinforced resin products with thin end faces. Therefore, when using carbon fiber bundles as carbon fibers, it is preferable to widen or open the carbon fiber bundles before use. Examples of metal fibers include Al fibers, Au fibers, Ag fibers, Fe fibers, and stainless steel fibers. Examples of organic fibers include aramid fibers, aromatic polyamide fibers, cellulose fibers, polyethylene fibers, and poly(paraphenylene benzobisoxazole) fibers (Zylon (manufactured by Toyobo Co., Ltd.)). The fibers may be treated with a treatment agent. Examples of the treatment agent include a bundling agent and a surface treatment agent. For example, the treatment agent disclosed in Japanese Patent No. 4,894,982 is mentioned. It is advantageous if the treating agent on the fiber surface reacts with the functional group (reactive group: polar group) of the resin.The treating agent is selected from the group consisting of, for example, epoxy resins, urethane resins, silane coupling agents, water-insoluble polyamide resins, and water-soluble polyamide resins. Preferably, it is selected from the group consisting of epoxy resins, urethane resins, water-insoluble polyamide resins, and water-soluble polyamide resins. One type or two or more types may be used.

[0063] Various resins can be used as the resin of the fiber-containing resin composition constituting the main body of the fishing line guide. The main body is produced, for example, by additive manufacturing technology, as described below. Therefore, a resin (matrix resin) that can be used in additive manufacturing technology is preferred. Examples of such resins include thermoplastic resins and thermosetting resins. Either one of these may be used alone, or they may be used in combination. One type of resin may be used, or two or more types of resins may be used. The resin may be in the form of a film (or sheet). The resin may be in the form of fibers (threads or filaments). When the resin is in the form of fibers, in the present invention, it is a so-called mixed fiber yarn (see, for example, WO 2016 / 167136 A1). In the case of mixed fiber yarn, the technology disclosed in WO 2016 / 167136 A1 can be employed. The resin preferably has a functional group (reactive group: polar group). Resins without functional groups (reactive groups: polar groups) can also be used. Thermoplastic resins may be composed solely of thermoplastic resins or may have thermoplastic resins as the main component. Either case is acceptable in the present invention. In the present invention (this specification), the term "thermoplastic resin" includes both cases consisting solely of thermoplastic resins and cases consisting primarily of thermoplastic resins, unless otherwise specified. A resin consisting primarily of thermoplastic resins refers to a resin containing 50% by mass or more of thermoplastic resin. Preferably, this is 80% by mass or more. More preferably, this is 90% by mass or more. Thermosetting resins may be composed solely of thermosetting resins or may have thermosetting resins as the main component. Either case is acceptable in the present invention. In the present specification (this specification), the term "thermosetting resin" refers to a resin containing both thermosetting resins and thermosetting resins as the main component, unless otherwise specified. A resin consisting primarily of thermosetting resins refers to a resin containing 50% by mass or more of thermosetting resin. Preferably, this is 80% by mass or more. More preferably, this is 90% by mass or more. Examples of thermosetting resins include epoxy resins, vinyl ester resins, unsaturated polyester resins, diallyl phthalate resins, phenol resins, maleimide resins, cyanate resins, benzoxazine resins, and dicyclopentadiene resins.Examples of thermoplastic resins include polyolefin resins, polystyrene resins, thermoplastic polyamide resins, polyester resins, polyacetal resins (polyoxymethylene resins), polycarbonate resins, (meth)acrylic resins, polyarylate resins, polyphenylene ether resins, polyimide resins, polyethernitrile resins, phenoxy resins, polyphenylene sulfide resins, polysulfone resins, polyketone resins, polyether ketone resins, thermoplastic urethane resins, fluorine-based resins, and thermoplastic polybenzimidazole resins. Examples of polyolefin resins include polyethylene resins, polypropylene resins, polybutadiene resins, polymethylpentene resins, vinyl chloride resins, vinylidene chloride resins, vinyl acetate resins, and polyvinyl alcohol resins. Examples of polystyrene resins include polystyrene resins, acrylonitrile-styrene resins (AS resins), and acrylonitrile-butadiene-styrene resins (ABS resins). Examples of the polyamide resin include polyamide 6 resin (nylon 6), polyamide 11 resin (nylon 11), polyamide 12 resin (nylon 12), polyamide 46 resin (nylon 46), polyamide 66 resin (nylon 66), and polyamide 610 resin (nylon 610).Nylon (hereinafter sometimes abbreviated as "PA"), which is one of the polyamide resins, includes PA6 (also called polycaproamide, polycaprolactam, or poly-ε-caprolactam), PA26 (polyethylene adipamide), PA46 (polytetramethylene adipamide), PA66 (polyhexamethylene adipamide), PA69 (polyhexamethylene azepamide), PA610 (polyhexamethylene sebacamide), PA611 (polyhexamethylene undecamide), PA612 (polyhexamethylene dodecamide), PA11 (polyundecaneamide), PA12 (polydodecanamide), PA1212 (polydodecamethylene dodecamide), PA6T (polyhexamethylene terephthalamide), PA Examples include A6I (polyhexamethylene isophthalamide), PA912 (polynonamemethylene dodecamide), PA1012 (polydecamethylene dodecamide), PA9T (polynonamemethylene terephthalamide), PA9I (polynonamemethylene isophthalamide), PA10T (polydecamethylene terephthalamide), PA10I (polydecamethylene isophthalamide), PA11T (polyundecamethylene terephthalamide), PA11I (polyundecamethylene isophthalamide), PA12T (polydodecamethylene terephthalamide), PA12I (polydodecamethylene isophthalamide), polyamide XD6 (polymetaxylylene adipamide), and polyamide XD10 (polyxylylene sebacamide). Examples of the polyester resin include polyethylene terephthalate resin, polyethylene naphthalate resin, polybutylene terephthalate resin, polytrimethylene terephthalate resin, and liquid crystal polyester. Examples of the (meth)acrylic resin include polymethyl methacrylate. Examples of the modified polyphenylene ether resin include modified polyphenylene ether. Examples of the thermoplastic polyimide resin include thermoplastic polyimide, polyamideimide resin, and polyetherimide resin. Examples of the polysulfone resin include modified polysulfone resin and polyethersulfone resin.Examples of the polyether ketone resin include polyether ketone resin, polyether ether ketone resin, and polyether ketone ketone resin. Examples of the fluorine-based resin include polytetrafluoroethylene. A thermosetting resin is preferred as the resin for the fiber-containing resin composition that constitutes the main body of the fishing line guide. A thermosetting resin with a water absorption rate of 2.0% or less is particularly preferred. The reason why a water absorption rate of 2.0% or less is preferred is as follows: Fishing line guides often come into contact with water during use. When exposed to water, water absorption occurs. As a result, the weight increases. This is not preferred from the perspective of lightweight properties.

[0064] The resin to fiber content ratio (mixing ratio) of the fiber-containing resin composition constituting the main body of the fishing line guide was preferably as follows, from the viewpoints of light weight and mechanical strength. For example, when the amount of carbon fiber was large, the mechanical strength increased. However, light weight was lost. Conversely, when the amount of carbon fiber was small, the mechanical strength decreased. From these viewpoints, the preferable ratios of the two were as follows. Preferably, 20 / 100≦(volume of the resin) / (volume of the fiber + volume of the resin). More preferably, 25 / 100≦(volume of the resin) / (volume of the fiber + volume of the resin). Even more preferably, 30 / 100≦(volume of the resin) / (volume of the fiber + volume of the resin). Even more preferably, 35 / 100≦(volume of the resin) / (volume of the fiber + volume of the resin). Preferably, (volume of the resin) / (volume of the fiber + volume of the resin)≦55 / 100. More preferably, (volume of the resin) / (volume of the fiber + volume of the resin)≦50 / 100, even more preferably, (volume of the resin) / (volume of the fiber + volume of the resin)≦45 / 100, and even more preferably, (volume of the resin) / (volume of the fiber + volume of the resin)≦40 / 100.

[0065] A second invention is a method for manufacturing a fishing tackle. For example, the method is a method for manufacturing the fishing line guide. The method includes a molding step in which a resin composition having fibers (e.g., including fibers) is shaped using a 3D printer. The method also includes a heating and pressurizing step in which the shaped object obtained in the molding step is heated and pressurized.

[0066] Additive manufacturing (3D printer modeling technology) is well known. This technology is described as follows in the "2013 Patent Application Technology Trends Survey Report (Summary) 3D Printers": 3D printing (additive manufacturing) refers to the process of creating an object from a numerical representation of a three-dimensional shape by depositing material. This is often achieved by stacking layers on top of each other. The term 3D printer is used in contrast to the two-dimensional printout on paper. ASTM F2792-12a (Standard Terminology for Additive Manufacturing Technologies) uses the term additive manufacturing. It has been difficult to produce three-dimensional fiber-reinforced resin products (not sheet-like (flat)) using additive manufacturing alone. This has been particularly challenging when the amount of fiber is maximized (relatively reducing the amount of resin) to improve mechanical strength. Therefore, when manufacturing the fishing tackle, the object formed by additive manufacturing technology is heated and pressurized.

[0067] The shaping process (additive manufacturing process) is a process in which additive manufacturing technology is used. In the additive manufacturing process, for example, an additive manufacturing device equipped with a nozzle is used. In the process, resin (plastic) and fibers are used. In the process, the resin (matrix resin) and fibers may be supplied (discharged) from separate nozzles. The respective materials may be supplied (discharged) simultaneously. They may be supplied (discharged) with a time lag. A fiber-reinforced plastic material (a material in which fibers are dispersed in a resin) may be supplied (discharged) from a single nozzle. A fiber-reinforced plastic product of the desired shape is obtained by the process. In the additive manufacturing process, for example, additive manufacturing technology using fused deposition modeling may be used. The additive manufacturing process may use additive manufacturing techniques that do not include, for example, a coating / printing process in which uncoagulated coagulant is coated and printed on the top surface of the laminate or on the surface of a sheet to be laminated on the laminate based on laminate region data in a predetermined cross section of a three-dimensional model, and a bonding process in which the sheet coated and printed with the uncoagulated coagulant and the laminate are overlapped and bonded together while kept warm, or that do not include a bonding process in which sheets selectively coated with coagulant are stacked on the surface and the sheets are selectively bonded together by the coagulant, and that use fibers and resin for molding. The additive manufacturing process may use additive manufacturing techniques that do not include, for example, a process in which sheets coated with coagulant are stacked and bonded together, and that use fibers and resin for molding. The fishing tackle (e.g., the fishing line guide) may be molded by a single additive manufacturing process. Product A includes part A. 1 , ..., part Ak (k is an integer equal to or less than n), ..., part An (n is an integer equal to or greater than 2). 1 is one (one) additive manufacturing technology process A 1 Similarly, the part Ak is formed by one (single) additive manufacturing technology process Ak. The part An is formed by one (single) additive manufacturing technology process An. 1 , ..., Ak, ..., An 1, ..., Ak, ..., An are combined, and the combined product has the same shape as the product A. In other words, the additive manufacturing technology process may require only one (one time) or two or more (two or more times). Either method may be adopted.

[0068] In the molding process (additive manufacturing technology process), when the resin is a thermosetting resin, from the viewpoint of moldability, the temperature was preferably 0°C or higher. More preferably, it was 10°C or higher. Even more preferably, it was 20°C or higher. Even more preferably, it was 30°C or higher. It was preferably 350°C or lower. Even more preferably, it was 150°C or lower. Even more preferably, it was 100°C or lower. When the resin is a thermoplastic resin, from the viewpoint of moldability, the temperature was preferably 30°C or higher. Even more preferably, it was 50°C or higher. Even more preferably, it was 100°C or higher. There is no particular restriction on the upper limit. However, in general, it is preferably 700°C or lower. More preferably, it is 500°C or lower. Even more preferably, it is 450°C or lower. Even more preferably, it is 400°C or lower.

[0069] The product obtained through the additive manufacturing technology process was approximately flat. It was not a three-dimensional (3D) shape. For example, it was not a 3D shape with flat surfaces and intersecting surfaces that intersect the flat surfaces. It was not easy to obtain a three-dimensional (3D) shape product using additive manufacturing technology alone. It was easy (relatively easy) to obtain an approximately flat product using additive manufacturing technology. In the product obtained through the additive manufacturing technology process, if the fiber content was high, not all of the fibers were firmly (rigidly) bonded together by the resin. The resin can also be considered a binder. Therefore, if the amount of resin was low, it would be difficult to obtain a solid (rigidly) bond between the fibers. In the product, the fibers were partially separated. The fibers were only loosely connected. This separation only meant that the product (the product obtained through the additive manufacturing technology process) did not have a fixed, single shape. For example, it only meant that the fibers would shift position if a force that bent the product into an approximately bow shape was applied. If all of the fibers are firmly bonded together by the resin, the fibers will not shift position even if the above-mentioned force is applied to the product, unless, of course, a force large enough to destroy them is applied.

[0070] The pressurizing step (heating and pressurizing step) is preferably a step in which the shaped object placed in a mold and heated is pressurized. The pressurizing step may be performed multiple times. For example, it may be performed in two stages, such as a first pressurizing step and a second pressurizing step. When the fiber content is high, it is preferable to perform the pressurizing step multiple times. The first pressurizing step is performed at a relatively low pressure. The second pressurizing step (second pressurizing step) is performed at a higher pressure than the first pressurizing step (first pressurizing step). The change in pressure from low to high in the pressurizing step may be a step function or continuous. In other words, the pressure may gradually increase. This type of pressurizing is also considered to be performed multiple times. The first pressurizing step is a step in which the product obtained through the additive manufacturing technology step is pressurized. By the first pressurizing step, most of the fibers are integrally bonded by the resin. In other words, the fibers are integrally bonded to a certain degree firmly by the resin. When the fibers are bonded together by the resin, the fibers are less likely to shift position even when a large force is applied to the product. Even when a large force is applied to a product that has undergone the first pressurization process, the product is less likely to deform. Of course, applying a force large enough to destroy the product is a different story. In contrast, applying a large force to a product obtained through the additive manufacturing process could potentially cause the fibers to shift position. The product obtained through the first pressurization process has curved portions. Therefore, the product has a three-dimensional shape. In contrast, the product obtained through the additive manufacturing process is flat. Therefore, at this stage, the product does not have curved portions (surfaces that intersect with a plane). In the first pressurization process, a two-dimensional product is molded into a three-dimensional product. If the force applied in the first pressurization process is too large, the product is more likely to lose its shape. This is because the fibers in the product obtained through the additive manufacturing process are not firmly integrated with the resin. When the fiber content is high, the product after the additive manufacturing process is often not a strong, integrated unit. Therefore, it is preferable not to apply too much force. In other words, the force applied in the first pressing step should be less than the force required to form the final product shape.In the first pressurizing process, multiple products obtained through the additive manufacturing technology process may be stacked and pressed. Of course, in some cases, only one product may be stacked. In the second pressurizing process, the product obtained through the first pressurizing process is pressed under heat. The force applied in the second pressurizing process is greater than the force applied in the first pressurizing process. That is, the force applied in the second pressurizing process is the force applied to form the final product shape. The volume of the product obtained through the second pressurizing process is smaller than the volume of the product obtained by the first pressurizing process. The pressure in the first pressurizing process is smaller than the pressure in the second pressurizing process. For example, (pressure in the first pressurizing process) / (pressure in the second pressurizing process) was 0.8 or less. For example, 0.7 or less. For example, 0.6 or less. For example, 0.5 or less. For example, 0.4 or less. For example, 0.02 or more. For example, 0.05 or more. For example, 0.1 or more. The pressure in the first pressurizing process was 0.8 kPa or more. For example, 4 kPa or more. For example, 8.0 × 10. 5 For example, 4.0 × 10 5 The pressure in the second pressurizing step was 1 kPa or more. For example, 5 kPa or more. For example, 1.0×10 6 For example, 5.0 × 10 5 kPa or less. (Volume of the product obtained through the first pressurizing step) / (Volume of the product obtained through the second pressurizing step)≦2.5. For example, 2 or less. For example, 1.5 or less. For example, 1.05 or more. For example, 1.1 or more.

[0071] The pressurization step is preferably carried out under heated conditions. This is because raising the temperature above room temperature (e.g., 25°C) softens the resin (resin composition). As a result, the moldability by pressurization is improved. The heating temperature only needs to satisfy the following conditions. For example, it was a temperature equal to or higher than the melting temperature in the 1 / 2 method performed using a Flow Tester CFT-500D (manufactured by Shimadzu Corporation) in accordance with the manual that came with the device. Preferably, it was a temperature equal to or higher than {the melting temperature + 10°C}. More preferably, it was a temperature equal to or higher than {the melting temperature + 20°C}. Preferably, it was a temperature equal to or lower than {the melting temperature + 60°C}. Even more preferably, it was a temperature equal to or lower than {the melting temperature + 50°C}. Even more preferably, it was a temperature equal to or lower than {the melting temperature + 40°C}. Even more preferably, it was a temperature equal to or lower than {the melting temperature + 30°C}. If the resin is a thermoplastic resin, for example, it is sufficient to heat the resin at a temperature above the melting temperature. If the resin is a thermosetting resin, for example, it is sufficient to heat the resin at a temperature lower than the curing temperature. The melting temperature is also called the softening point. This temperature was determined by the following method. A constant-load extrusion capillary rheometer (flow property evaluation device: Flow Tester CFT-500D (manufactured by Shimadzu Corporation)) was used, and the test was performed in accordance with the manual that came with the device. In this device, a constant load is applied from above the measurement sample (the sample in this case is a resin without fiber, not a resin blended with fiber) by a piston. The measurement sample filled in the cylinder is heated and melted. The molten measurement sample is extruded from a die at the bottom of the cylinder. A flow curve showing the relationship between the piston depression amount and temperature is obtained. The melting temperature in the 1 / 2 method described in the manual was calculated as follows. Half of the difference between the piston depression amount Smax at the end of outflow and the piston depression amount Smin at the start of outflow is calculated (this is designated as X; X = (Smax - Smin) / 2). The melting temperature in the 1 / 2 method is the temperature on the flow curve at the point where the piston descends by the distance X. For example, when the resin is an epoxy resin (thermosetting resin), the melting temperature (softening temperature) determined by the above method was about 70°C.When the resin was benzoxazine (thermosetting resin), the melting temperature (softening temperature) determined by the above method was approximately 80°C. When the resin was cyanate resin (thermosetting resin), the melting temperature (softening temperature) determined by the above method was approximately 80°C. When the resin was a thermosetting resin, the heating temperature was preferably a temperature of (resin curing temperature - 70°C) or higher. More preferably, it was a temperature of (resin curing temperature - 60°C) or higher. Even more preferably, it was a temperature of (resin curing temperature - 50°C) or higher. Even more preferably, it was a temperature of (resin curing temperature - 40°C) or higher. Preferably, the temperature was (resin curing temperature + 20°C) or lower. More preferably, the temperature was (resin curing temperature + 10°C) or lower. Still more preferably, the temperature was lower than the resin curing temperature. The curing temperature is the peak temperature in the DSC curve. The thermosetting temperature of epoxy resin (thermosetting resin) is about 120 to 180°C. The thermosetting temperature of benzoxazine resin (thermosetting resin) is about 120 to 200°C. The thermosetting temperature of cyanate resin (thermosetting resin) is about 150 to 250°C. When the resin is a thermosetting resin, after-cure may be performed.

[0072] A mold is used in the pressure application process. The mold comprises mold half A and mold half B. Mold half A and mold half B each have a recess (groove) with no corners on the concave surface formed on the opposing surfaces of mold half A and mold half B. The shaped object obtained in the additive manufacturing technology process is placed in the recess of mold half A. Mold half B is then placed on top and pressure is applied. When mold half A and mold half B are combined, the space (cavity) formed by the recesses of mold halves A and B is the shape of the final product. The inner surface of the recess (groove) has no corners. Therefore, the product obtained by applying pressure between mold half A and mold half B has no corners because the inner surface of the recess (groove) has no corners. If the cavity is composed only of a groove formed on the upper surface of the mold half A (if the mold half B facing the recess (groove) of the mold half A has a convex portion formed thereon or is flat), the product obtained in this manner will have corners even if the groove does not have corners.

[0073] The present invention will be described in detail below. The following examples are merely examples of the present invention. The present invention is not limited to the following examples. In other words, the present invention also includes modifications and applications that do not significantly impair the features of the present invention.

[0074] Example 1: A thermosetting resin (benzoxazine resin, manufactured by Aica Kogyo Co., Ltd.) was used. Carbon fiber (manufactured by Mitsubishi Rayon Co., Ltd., Pyrofil-TR-50S-12000-AD, 8000 dtex, 12000 filament count, 6 m fiber length) was used. The blending ratio was 40 parts by volume of the resin and 60 parts by volume of the carbon fiber.

[0075] A 3D printer (Velleman K8200) was used. Additive manufacturing technology was performed (nozzle temperature: 135°C, stage temperature: 50°C). As a result, Product X made of the composition was obtained. Product X obtained through the additive manufacturing process was approximately flat. It was not a three-dimensional shape (solid shape). Since the amount of resin in Product X was relatively small, not all of the fibers were integrally bonded by the resin. The fibers in Product X were partially separated.

[0076] The product X obtained through the additive manufacturing process was placed in a mold. 3A pressure of 100 kPa was applied. The mold was made of non-metal. Non-contact heating (induction heating) was performed in this pressurization process. A three-dimensional molded product Y was obtained. The molded product Y after pressurization was removed from the mold and placed in a metal die. The mold included a metal mold half A (see Figure 5) and a metal mold half B (see Figure 6). Grooves (recesses) 11 and 12 were formed on the surfaces of the mold halves A and B. The space (cavity) shape formed by the grooves (recesses) 11 and 12 when the mold half A and the mold half B were combined is the shape of the final product Z. The concave surfaces of the grooves (recesses) 11 and 12 have no corners. The removed molded product Y was first placed in the groove (recess) 11 of the mold half A. The mold half B was then placed over the mold half A with the molded product Y placed in it. Half of the molded product Y is located in the groove 11 of the mold half A, and the other half of the molded product Y is located in the groove 12 of the mold half B. When heated to 180° C., 4 A pressure of 100 kPa was applied to the molded product Y.

[0077] The fishing line guide Z obtained in this manner is shown in Figures 1, 2, 3, and 4. Figure 1 is a perspective view of the fishing line guide Z. Figure 2 is a perspective view of the fishing line guide Z viewed from the opposite side to that shown in Figure 1. Figure 3 is a cross-sectional view of the fishing line guide Z in the state shown in Figure 1, taken along a line connecting the apex of the approximately ring-shaped portion 1 of the fishing line guide Z to the base end 3f of the approximately Y-shaped portion 2. Figure 4 is a cross-sectional view taken along a line perpendicular to the cross-sectional line of Figure 3 that intersects the opening 6 of the fishing line guide Z. In each figure, reference numeral 1 denotes the approximately ring-shaped portion through which the fishing line will be passed (inner diameter of the ring: approximately 20.5 mm, outer diameter of the ring: approximately 23.7 mm, thickness: approximately 2.3 mm, width: approximately 1.6 mm).

[0078] Reference numeral 2 denotes a substantially Y-shaped portion. The tip side of the substantially Y-shaped portion 2 has a branched structure. That is, the substantially Y-shaped portion 2 has two branched portions (branches) 2a and 2b on the tip side. Tips 3a and 3b of the branched portions 2a and 2b are connected to the substantially ring-shaped portion 1. The extension direction of the branched portions 2a and 2b is the direction of a tangent to the substantially ring-shaped portion 1. Because the connection direction between the branched portions 2a and 2b and the substantially ring-shaped portion 1 is approximately the direction of a tangent to the substantially ring-shaped portion 1, the branched portions 2a and 2b can easily withstand the force applied to the substantially ring-shaped portion 1. The base (trunk) 2c of the substantially Y-shaped portion 2 is one trunk. The intersection position 3c of the branched portion (branch) 2a and the branched portion (branch) 2b is the tip of the base (trunk) 2c.

[0079] The substantially ring-shaped portion 1 and the substantially Y-shaped portion 2 are integrally formed. This can be understood from the fact that the product X is obtained by additive manufacturing technology. Some of the carbon fibers dispersed in the thermosetting resin are longer than {(the circumferential length of the substantially ring-shaped portion 1) + (the length of the substantially Y-shaped portion 2)}. Therefore, some of the carbon fibers will be present straddling the substantially ring-shaped portion 1 and the substantially Y-shaped portion 2.

[0080] The branches 2a, 2b are slightly bent near a midpoint 3d of the branches 2a, 2b (e.g., approximately 2 / 3 of the way from the tips 3a, 3b) (the opening angle is, for example, approximately 160 to 175° (e.g., 170°)). The base 2c is bent at a midpoint 3e (the opening angle is, for example, approximately 125 to 145° (e.g., 135°)). The length of the branches 2a, 2b is approximately 40 mm. The width of the branches 2a, 2b is larger than the width of the approximately ring-shaped portion 1 so that the approximately ring-shaped portion 1 can be firmly supported even when the thickness of the thick portions of the branches 2a, 2b and the thickness of the approximately ring-shaped portion 1 are approximately the same. The width of the branches 2a, 2b is approximately 3.2 mm. The thickness of the thick portions of the branches 2a, 2b is approximately 2.3 mm. The thickness of the thin portions of the branches 2a, 2b is approximately 1 mm. The length of the base 2c is approximately 35 mm. The width of the base 2c at its tip 3c (the intersection of the branch 2a and branch 2b) is approximately 7 mm. The width of the base (trunk) 2c at the bending position 3e is approximately 4.6 mm. The thickness of the base 2c at its tip 3c is approximately 2.5 mm. The thickness of the base 2c at the bending position 3e is approximately 2.7 mm. The thickness of the base 2c at its base end 3f is approximately 1 mm. The width of the base 2c decreases almost monotonically from the tip 3c to the base end 3f. The thickness of the base 2c increases monotonically from the tip 3c to the bending position 3e. The reason for the increased thickness is to ensure the mechanical strength of the base 2c, as the width of the base 2c gradually narrows. The thickness decreases from the bending position 3e to the base end 3f. However, the rate of decrease from approximately the midpoint between the bending position 3e and the base end 3f toward the base end 3f increases rapidly. The thickness of the portion where the base 2c is attached to the fishing rod (from the approximately midpoint between the bending position 3e and the base end 3f to the base end 3f) is made thin to make it easier to fix to the fishing rod.

[0081] Reference numerals 4a and 4b denote thick portions (ribs) in the branch portions 2a and 2b. Reference numerals 5a and 5b denote thin portions in the branch portions 2a and 2b. The thick portions (ribs) 4a and 4b are located on the outside of the branch portions 2a and 2b. The thin portions 5a and 5b are located on the inside of the branch portions 2a and 2b (on the side of the opening 6 formed by the branch portions 2a and 2b). The "thickness" of the thick portions means that they are "thicker" than the "thickness" of the thin portions. The thickness of the thick portions (ribs) 4a and 4b is the same as the thickness of the branch portions 2a and 2b (approximately 2.3 mm). The width of the thick portions (ribs) 4a and 4b is approximately 1 mm. The width of the thin portions 5a and 5b is approximately 2.2 mm.

[0082] A thin portion is also formed in the approximately ring-shaped portion 1. A thin portion 7a is formed in the approximately ring-shaped portion 1 at a position sandwiched between the branch portions 2a and 2b. The width of the thin portion 7a is approximately 1 mm. The width of the thick portion 7b is approximately 0.6 mm. The thickness of the thick portion 7b is approximately 2.3 mm. The thickness of the thin portion 7a is approximately 1 mm.

[0083] [Comparative Example 1] In Example 1, no ribs were configured. The presence of the ribs made it possible to achieve a lighter weight while maintaining the necessary rigidity. In other words, when comparing a fishing rod equipped with the fishing line guide of Example 1 and a fishing rod equipped with the fishing line guide of Comparative Example 1, the fishing rod equipped with the fishing line guide of Example 1 was significantly easier to use.

[0084] REFERENCE SIGNS LIST 1 Approximately ring-shaped portion 2 Approximately Y-shaped portion 2a, 2b Branch portion (branch portion) 2c Base portion (trunk portion) 3a, 3b Tip portion 3c Intersection position of branch portion (branch portion) 2a and branch portion (branch portion) 2b 3e Bending position 3f Base end portion 4a, 4b, 7b Thick portion (rib) 5a, 5b, 7a Thin portion 6 Opening

Claims

1. A fishing line guide, comprising: a main body portion of said fishing line guide made of a fiber-containing resin composition; and said main body portion having a rib.

2. The fishing line guide of claim 1, wherein said main body comprises a generally ring-shaped portion and a generally Y-shaped portion, said generally Y-shaped portion has a branched portion whose tip is connected to said generally ring-shaped portion, and said branched portion is provided with a rib.

3. The fishing line guide of claim 2, wherein an inner portion of said branched portion is thin-walled and an outer portion of said branched portion is thick-walled, said thick-walled portion being a rib.

4. A fishing line guide as claimed in claim 1 or 2, wherein said main body comprises a generally ring-shaped portion and a generally Y-shaped portion, a tip of a branch of said generally Y-shaped portion is connected to said generally ring-shaped portion, and a rib is formed on said generally ring-shaped portion at a position sandwiched between said branch portions.

5. The fishing line guide according to claim 1, wherein the fibers are carbon fibers.

6. The fishing line guide of claim 1, wherein said fibers have a fiber length of 1 cm or more.

7. The fishing line guide according to claim 1, wherein said resin is a thermosetting resin.

8. The fishing line guide according to claim 1, wherein said resin composition has a ratio of (amount of said resin) / (amount of said resin+amount of said fibers)=30 / 100 to 60 / 100.

9. The fishing line guide of claim 1, wherein said fishing line guide has a water absorption rate of 2.0% or less.

10. A method for manufacturing fishing tackle, wherein the fishing tackle is a fishing line guide, a main body of the fishing line guide is made of a fiber-containing resin composition, the method comprising: a modeling process in which the resin composition having fibers is modeled using a 3D printer; and a heating and pressurizing process in which the model obtained in the modeling process is heated and pressurized.

11. The method of claim 10, wherein a mold is used in the pressurizing step, the mold comprising mold half A and mold half B, mold half A and mold half B each have a recess without corners formed on the opposing surfaces of mold half A and mold half B, and after the object is placed in the recess of mold half A, mold half B is placed over it and heated and pressurized.

Citation Information

Patent Citations

  • Fishing line guide and method for producing the same

    JP2011223920A

  • Fishing line guide and method for manufacturing the same

    JP2012070676A

  • Fishing guide frame, and manufacturing method for fishing guide frame

    JP2022131689A

  • Method for producing fiber-reinforced resin article

    WO2021112097A1