Titanium porous body, and titanium porous body manufacturing method
The production of titanium porous bodies with a high number of fine surface pores using a specific paste composition and processing method addresses the risk of electrolyte membrane damage in PEM type water electrolyzers, improving permeability and performance.
Patent Information
- Application Number
- PCT/JP2024/005338
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-31
AI Technical Summary
Titanium porous bodies used in PEM type water electrolyzers face the risk of electrolyte membrane damage due to large pores, which can lead to deformation and reduced performance, and existing manufacturing methods may result in uneven powder aggregation and large surface pores.
A titanium porous body is produced using a paste with titanium powder of small particle size, alcohol as an organic solvent, and a dispersant containing coal tar naphtha, which suppresses agglomeration and ensures a large number of fine pores on the surface, with a method involving drying and sintering to achieve a sheet-like structure with controlled pore size and distribution.
The resulting titanium porous body has a high number of fine pores on its surface, reducing the risk of electrolyte membrane damage and enhancing air and liquid permeability, making it suitable for use in PEM type water electrolysis devices.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Titanium porous body and method for producing titanium porous body
[0001] The present invention relates to a porous titanium body and a method for producing the porous titanium body.
[0002] Porous titanium bodies produced by sintering titanium powder or the like have air or liquid permeability due to their fine pores, electrical conductivity, and also high corrosion resistance due to the formation of a passivation film on the surface.
[0003] Porous titanium having such properties is being considered for use in porous transport layers (PTLs) in polymer electrolyte membrane (PEM)-type water electrolysis devices, which are in environments where corrosion may occur. In particular, hydrogen produced in PEM-type or other water electrolysis devices using electricity derived from renewable energy is called "green hydrogen," and great expectations are being placed on it in recent years as efforts to realize a decarbonized society accelerate.
[0004] As a related technique, Patent Document 1 proposes, for the purpose of "providing a titanium porous plate that can be brought into sufficient contact with other adjacent members and that allows good circulation and diffusion of fluids such as liquids and gases, as well as a water electrolysis electrode and a water electrolysis apparatus made of this titanium porous plate," and proposes "a titanium porous plate made of a sintered body of titanium or a titanium alloy, the titanium porous plate having a three-dimensional network structure with communicating pores that are open on the surface of the titanium porous plate and communicate with internal pores, the opening rate of one main surface being smaller than the opening rate of the other main surface, and the difference between the opening rates of the one main surface and the other main surface being 10% or more." The document states that in the "titanium-containing slurry formation step" during the manufacture of this "titanium porous plate," "raw material powder is mixed with a water-soluble resin binder (methyl cellulose), an organic solvent (neopentane, hexane, and butane), a plasticizer (glycerin and ethylene glycol), water as a solvent, a foaming agent, and, in some cases, a surfactant (alkylbenzene sulfonate) to produce a titanium-containing slurry."
[0005] Furthermore, Patent Document 2, for the same purpose as above, discloses "a titanium porous plate made of a sintered body of titanium or a titanium alloy, the titanium porous plate having a three-dimensional mesh structure with communicating pores that open on the surface of the titanium porous plate and communicate with internal pores, the titanium porous plate having a structure in which a first layer and a second layer are laminated in the thickness direction, and the average pore diameter of the second layer is larger than the average pore diameter of the first layer." In Patent Document 2, to manufacture such a "porous titanium plate material," a "first titanium-containing slurry" is used, in which "raw material powder is mixed with a water-soluble resin binder (methyl cellulose), an organic solvent (neopentane, hexane, and butane), a plasticizer (glycerin and ethylene glycol), water as a solvent, and in some cases a surfactant (alkylbenzene sulfonate)," and a "second titanium-containing slurry" is used, in which "raw material powder is mixed with a water-soluble resin binder (methyl cellulose), an organic solvent (neopentane, hexane, and butane), a plasticizer (glycerin and ethylene glycol), water as a solvent, and in some cases a surfactant (alkylbenzene sulfonate), and in addition a foaming agent."
[0006] International Publication No. WO 2022 / 210421 International Publication No. WO 2022 / 210681
[0007] When a porous titanium body is used as a porous transport layer in a PEM-type water electrolysis device, the porous titanium body may be pressed against an electrolyte membrane when assembled. If the pores in the porous titanium body are large, the electrolyte membrane pressed against the porous titanium body may partially enter the pores, causing significant deformation in areas adjacent to the pores and potentially damaging the electrolyte membrane.
[0008] Therefore, to prevent damage to the electrolyte membrane, it is desirable that the porous titanium body have small pores that open to the surface facing the electrolyte membrane, and that a large number of such pores be present on that surface. A porous titanium body with a large number of pores is less likely to damage the electrolyte membrane as described above, and can serve as a porous transport layer with good air and liquid permeability.
[0009] In the techniques described in Patent Documents 1 and 2, it is believed that the titanium powder in the paste may aggregate during the production of the porous titanium body. If the titanium powder aggregates in the paste, the resulting uneven distribution of the titanium powder may result in the formation of large pores on the surface of the porous titanium body after production.
[0010] An object of the present invention is to provide a porous titanium body having a surface on which a relatively large number of fine pores are formed, and a method for producing the porous titanium body.
[0011] As a result of extensive research, the inventors have found that by mixing titanium powder with a relatively small particle size to form a paste containing no water but an organic solvent alcohol, and using a dispersant containing coal tar naphtha, it is possible to obtain a porous titanium body with numerous fine pores formed on the surface after drying, debinding, and sintering the paste. This is thought to be because the specific dispersant effectively suppresses the aggregation or uneven distribution of the titanium powder in the paste.
[0012] The porous titanium body of the present invention is a sheet-like body having pores, and the average area of the pores that are open to the surface on at least one surface is 10 μm 2 More than 17 μm 2 The standard deviation of the area of the pores is 20 μm or less. 2 or less, and the area is 40,000 μm 2 The number of pores present within a rectangular region having an aspect ratio of 4:5 is 250 or more.
[0013] The thickness of the porous titanium body is preferably 40 μm or more and 500 μm or less.
[0014] The surface of the titanium porous body has an average pore area of 10 μm 2 More than 14 μm 2 It is preferable that:
[0015] The surface of the titanium porous body has a standard deviation of the pore area of 17 μm 2 It is preferable that:
[0016] The surface of the titanium porous body has an area of 40,000 μm 2 Preferably, the number of pores present within a rectangular region having an aspect ratio of 4:5 is 300 or more. The titanium porous body may have a titanium content of 97 mass % or more.
[0017] The method for producing a porous titanium body of this invention is a method for producing a sheet-like porous titanium body having pores, and comprises the following steps: a drying step in which a paste containing titanium powder having an average particle size of 25 μm or less, an organic binder, and an organic solvent, but not containing water as a solvent, is dried to obtain a sheet-like molded body; a binder removal step in which the molded body is heated to volatilize the organic binder; and a sintering step in which the molded body after the binder removal step is heated to sinter the titanium powder, wherein the organic solvent in the paste is alcohol, and the paste contains a dispersant containing coal tar naphtha.
[0018] In the above manufacturing method, it is preferable that the content of the dispersant in the paste is 0.01% by mass or more and 0.3% by mass or less.
[0019] The above manufacturing method can produce a porous titanium body having a thickness of 40 μm or more and 500 μm or less. In the above manufacturing method, it is preferable that the average particle size of the titanium powder is 18 μm or less. In the above manufacturing method, it is preferable that the drying temperature in the drying step is 90° C. or more and 165° C. or less.
[0020] The porous titanium body of the present invention has a surface on which a relatively large number of fine pores are formed, and the method for producing the porous titanium body of the present invention is suitable for producing such a porous titanium body.
[0021] The porous titanium body according to one embodiment of the present invention is a sheet-like body having pores. When the area and number of pores opening to at least one surface of the porous titanium body are checked, the average area of the pores is 10 μm 2 More than 17 μm 2The standard deviation of the area of the pores is 20 μm or less. 2 or less, and the area is 40,000 μm 2 The number of pores present within a rectangular region having an aspect ratio of 4:5 is 250 or more.
[0022] If a relatively large number of relatively fine pores are formed on at least one surface of a titanium porous body in this way, it is believed that when the titanium porous body is used as a porous transport layer in a PEM-type water electrolysis device, damage to the electrolyte membrane pressed against the surface is effectively suppressed. This is thought to be because the pores opening to the surface are fine, making it difficult for the electrolyte membrane to partially penetrate into these pores, and because the number of pores is large, the load acting on the electrolyte membrane when the titanium porous body is pressed against it is dispersed. Therefore, it can be said that this titanium porous body can be suitably used as a porous transport layer in a PEM-type water electrolysis device.
[0023] The porous titanium body can be produced by, but is not limited to, sequentially drying a paste containing titanium powder, an organic binder, and an organic solvent, debinding the paste, and sintering the titanium powder. The organic solvent in the paste is alcohol, and the paste does not contain water as a solvent. In particular, in such a production method, it is essential to use titanium powder of a predetermined small particle size and to include a dispersant containing coal tar naphtha in the paste. It is believed that the coal tar naphtha in the dispersant adheres in small amounts to the surface of the titanium powder, facilitating the sliding of the titanium powder particles and promoting good dispersion of the titanium powder in the paste. This suppresses aggregation or uneven distribution of the titanium powder in the paste, allowing the small-particle titanium powder to be bonded in a relatively uniform arrangement during sintering. As a result, a porous titanium body having a large number of fine pores formed on at least one surface is obtained. Typically, a large number of fine pores are also formed on the surface opposite the surface of the porous titanium body.
[0024] (Composition) The titanium porous body is made of titanium. If it is made of titanium, a titanium porous body having high electrical conductivity at a certain relative density can be obtained. The titanium content of the titanium porous body is preferably 97% by mass or more, and more preferably 98% by mass or more. The upper limit of the titanium content is not limited to this, but may be, for example, 99.8% by mass or less, or 99% by mass or less. This titanium content refers to the purity of titanium taking into account not only the metal components but also impurities such as gas components such as oxygen. Therefore, the titanium content can be calculated by subtracting the total content of impurities, including metal components and gas components, from 100% by mass.
[0025] The titanium porous body may contain Fe as an impurity, and the Fe content may be, for example, 0.25 mass% or less. The titanium porous body may also contain Ni, Cr, Al, Cu, Zn, and Sn as unavoidable impurities resulting from the manufacturing process. It is preferable that the content of each of Ni, Cr, Al, Cu, Zn, and Sn is less than 0.10 mass%, and that the total content of these elements is less than 0.30 mass%.
[0026] The oxygen content of the porous titanium body is not particularly limited, but may be 0.9% by mass or more and 2.0% by mass or less. The oxygen content can be measured by inert gas fusion-infrared absorption method.
[0027] The titanium porous body may have a purity equivalent to pure titanium grades 1 to 4, typically grades 1 to 2, of JIS H 4600 (2012), excluding the oxygen content.
[0028] (Sheet Dimensions) The thickness of the sheet-shaped porous titanium body may be 40 μm or more and 500 μm or less. For example, a porous transport layer of a PEM water electrolysis device may require a porous titanium body of a certain thickness. On the other hand, if the thickness is too large, the PEM water electrolysis device may become large. The thickness of the porous titanium body may be, for example, 400 μm or less, 350 μm or less, 300 μm or less, 250 μm or less, or 200 μm or less, or may be 40 μm or more or 80 μm or more.
[0029] The thickness is measured at five points (four points on the periphery and one point in the center) of the titanium porous body using a digital thickness gauge with a flat probe having a diameter of 10 mm and a measurement accuracy of 0.001 to 0.01 mm, such as a Mitutoyo digital thickness gauge (model number 547-321), and the average of these measurements is used. When the sheet-like titanium porous body has a rectangular shape in plan view, the four peripheral points are the four corners.
[0030] The surface area of the sheet-like porous titanium body in plan view is not particularly limited and may be determined appropriately depending on the application. For example, 2 Above, 350000mm 2 Below, 40000mm 2 ~600,000mm 2 This may be the case.
[0031] The term "sheet-like" in relation to the titanium porous body means a plate-like or foil-like body having a thickness smaller than the dimensions in a plan view, and the shape in a plan view is not particularly limited.
[0032] (Pores) Porous titanium bodies are formed by bonding titanium powder particles together, and have a three-dimensional network structure in which pores are formed between the bonded titanium powder particles. As an example, porous titanium bodies may have a skeleton with a three-dimensional network structure similar to that of titanium sponge. Note that porous titanium bodies manufactured using titanium fibers tend to have a three-dimensional network structure similar to that of nonwoven fabric. In many cases, the skeleton of porous titanium bodies, which is made up of bonded titanium powder particles, is solid rather than hollow.
[0033] Among the pores formed in the titanium porous body, the average area of a large number of pores that are open to at least one surface of the porous body is 10 μm 2 More than 17 μm 2 The standard deviation of the surface pore area is 20 μm or less. 2 In this way, if the majority of pores on at least one surface have a relatively small area, the surface can be said to be generally smooth, and damage to the electrolyte membrane in a PEM-type water electrolysis device can be effectively suppressed. From this perspective, the average area of the pores on the surface is 10 μm or less.2 More than 14 μm 2 From the same viewpoint, it is preferable that the standard deviation of the area of the pores on the surface is 17 μm or less. 2 It is preferable that the average pore area is less than 1 / 2 mm. If the average pore area is too small, the air permeability or liquid permeability may decrease. However, it is acceptable for a small number of pores with a relatively large area to exist on the surface.
[0034] In addition, the surface area is 40,000 μm 2 The number of pores present within a rectangular region having an aspect ratio of 4:5 is 250 or more, preferably 300 or more. The presence of many fine pores on the surface makes it easier to ensure the required breathability or liquid permeability, while also achieving surface smoothness. The number of pores within the rectangular region is not limited to this, but may be, for example, 500 or less.
[0035] The average value and standard deviation of the area of the pores opening to the surface as described above, and the number of pores within a predetermined rectangular area, are measured using a scanning electron microscope (Keyence Ultra-Deep Multi-Angle Lens VHX-D510). 2An SEM image was acquired at 1500x magnification for a rectangular region with an aspect ratio of 4:5. The SEM image was then analyzed using a scanning electron microscope. Half the maximum detected brightness value for the SEM image was used as a threshold, and closed regions with brightness ranging from 0 to the threshold were considered to be individual pores. If necessary, the SEM image may be binarized. After the binarization process, a process for removing small particles of 50 pixels or less (processing to convert black pixels after binarization) is performed, followed by a process for filling 50 pixels or less (processing to convert white pixels after binarization). The number and area of each pore were calculated using this data, and the standard deviation was determined as the square root of the variance. This SEM image analysis was performed for five rectangular regions on the surface of the titanium porous body, each at least partially offset from the others. The average area, standard deviation, and number of pores in these rectangular regions were used as the average area and standard deviation of the pores in the titanium porous body, and the number of pores in the rectangular regions, respectively. In the case of a titanium porous body that is a square or rectangular in plan view, the five rectangular regions are the five rectangular regions at the center and four corners.
[0036] (Applications) The porous titanium body can be particularly suitably used for the porous transport layer of a PEM-type water electrolysis device. A PEM-type water electrolysis device may include an anode, a cathode, an electrolyte membrane such as a perfluorocarbon sulfonic acid membrane disposed between the anode and the cathode and having electrode catalyst layers of a platinum group metal or the like on both sides, and a porous transport layer disposed between each electrode catalyst layer of the electrolyte membrane and the anode or cathode.
[0037] In the PEM water electrolysis device, when water is supplied to the anode and a voltage is applied, the water moves through the porous transport layer on the anode side and reaches the electrode catalyst layer, where it decomposes to produce oxygen and protons (H + The protons pass through the anode electrolyte membrane to move from the anode to the cathode, where they acquire electrons at the cathode catalyst layer, generating hydrogen at the cathode. Meanwhile, oxygen passes through the porous transport layer to the discharge channel and is discharged outside the device.
[0038] In such a PEM-type water electrolysis device, the space where the porous transport layer is placed, particularly on the anode side, is subject to strongly acidic and strongly oxidizing conditions, but a titanium porous body with high corrosion resistance can be used successfully as a porous transport layer in such an extremely harsh environment. Furthermore, as described above, the titanium porous body of the present invention has a large number of fine pores formed on at least one surface, which can prevent damage to the electrolyte membrane when the titanium porous body is placed in a PEM-type water electrolysis device with its surface pressed against the electrolyte membrane.
[0039] In addition to the PEM-type water electrolysis devices described above, the use of porous titanium materials in organic electrolysis synthesis using PEM-type reactors is also being considered. In such devices, electrolysis is carried out by passing protons through a proton exchange membrane. The porous titanium materials described here may also be well suited for organic electrolysis synthesis using PEM-type reactors, and are considered to be usable as a porous transport layer (PTL) on the anode side of electrolysis devices that use proton exchange membranes.
[0040] (Manufacturing Method) The above-described porous titanium body can be manufactured, for example, by carrying out the following steps in this order: paste preparation, paste application, drying, binder removal, and sintering. However, if the paste has already been prepared or applied in sheet form, the paste preparation and paste application steps may be omitted.
[0041] First, in a paste preparation step, a paste containing titanium powder, an organic binder, and an organic solvent is prepared.
[0042] The average particle size of the titanium powder contained in the paste can be 25 μm or less, preferably 18 μm or less. By using titanium powder with such a small particle size and further using a predetermined dispersant as described below, it is possible to achieve a smooth surface of the final porous titanium body. If the average particle size of the titanium powder exceeds 25 μm, the pores on the surface of the porous titanium body tend to become large even when a predetermined dispersant is used. From the perspective of using relatively inexpensive titanium powder to suppress increases in production costs and to facilitate handling of the titanium powder, the average particle size of the titanium powder may be 5 μm or more, or even 10 μm or more. The average particle size refers to the particle size at which the cumulative volume distribution in the particle size distribution obtained by laser diffraction scattering is 50%.
[0043] High-purity titanium powder is preferred, and pure titanium powder can be used. The titanium powder may have a titanium content of 99% by mass or more. The titanium powder can be a pulverized powder, a spherical powder such as atomized powder, or any other powder. Titanium hydride powder obtained by hydrogenating and pulverizing a titanium raw material such as sponge titanium can also be used. In this case, the hydrogen content of the titanium hydride powder is preferably 5% by mass or less. When using titanium hydride powder, it may be subjected to a dehydrogenation treatment at a temperature range of 500°C or higher and 650°C or lower in a reduced pressure atmosphere such as vacuum between the binder removal step and the sintering step described below. Hydrogenated and dehydrogenated titanium powder (HDH powder) obtained by dehydrogenating titanium hydride powder can also be used.
[0044] The organic binder used in the paste can be selected from a variety of materials, including methyl cellulose, polyvinyl alcohol, ethyl cellulose, acrylic, and polyvinyl butyral. Hydrophobic organic binders are preferred. However, they are not limited to the materials listed here. The organic solvent is alcohol (ethanol, isopropanol, terpineol, butyl carbitol, etc.). For example, the organic binder may be polyvinyl butyral and the organic solvent may be isopropyl alcohol. The paste may further contain a plasticizer (glycerin, ethylene glycol, etc.) or a surfactant (alkylbenzene sulfonate, etc.).
[0045] The paste does not contain water as a solvent. It is also preferable that the paste does not contain a foaming agent. This is because, if the paste contains water, aggregation of the titanium powder in the paste due to the difference in drying behavior between organic solvents and water during drying and the generation of pinholes on the surface of the titanium porous body are suppressed. Furthermore, if the paste does not contain a foaming agent, large localized voids caused by foaming of the foaming agent are not formed in the titanium porous body. As a result, the titanium porous body is likely to have a smooth surface and is less likely to crack during handling. Therefore, a foaming treatment that generates bubbles in the paste is not performed here. It is sufficient that the paste does not contain water as a solvent, and the inclusion of water that may be unintentionally mixed into the paste due to moisture absorption or the like is permitted.
[0046] The paste also contains a dispersant containing coal tar naphtha. The use of such a dispersant is believed to disperse the titanium powder in the water-free paste, suppressing its aggregation or uneven distribution, thereby preventing the formation of large pores on the surface of the porous titanium body. Furthermore, coal tar naphtha is a hydrocarbon mixture with a relatively low boiling point, and is believed to volatilize along with the organic solvent and organic binder during the drying and debinding processes, so it does not significantly affect the porous titanium body.
[0047] In particular, when the dispersant contains 20% by mass or more of coal tar naphtha, the dispersant's effect of dispersing the titanium powder can be even more effectively exerted. The dispersant may contain components other than coal tar naphtha, and typically contains a polycarboxylic acid amine salt. To further disperse the titanium powder, the content of the dispersant in the paste is preferably 0.01% by mass or more and 0.3% by mass or less, more preferably 0.01% by mass or more and 0.1% by mass or less, and particularly preferably 0.05% by mass or more and 0.1% by mass or less.
[0048] The paste can be prepared by mixing the titanium powder, organic binder, organic solvent, and the like as described above using, for example, a mixer with an agitator, a rotary mixer, a triple roll mill, etc. At this time, the mixture may be pulverized using a vibration mill, a bead mill, or other pulverizing mixer, etc.
[0049] In the paste application step, the paste is applied relatively thinly onto a substrate. A release layer may be provided on the substrate in advance. In this case, the paste is applied onto the substrate via the release layer. When a release layer is provided on the substrate, it becomes easier to separate the molded body obtained by drying the paste from the substrate after the drying step.
[0050] As the substrate, a resin substrate is preferable because it is relatively inexpensively available. Resin substrates also have the advantage of being flexible and therefore easy to handle. Specific materials for the resin substrate include polyesters such as PET (polyethylene terephthalate) and PEN (polyethylene naphthalate), and polyvinyls such as polyethylene, polypropylene, polystyrene, and polyvinyl alcohol. Of these, PET is preferable because it is inexpensive and allows the molded body to be easily separated from the substrate after the drying process.
[0051] It is optional to provide a release layer on the substrate. If a release layer is provided, a silicone coating or the like can be used as the release layer. For example, a release layer can be provided on the substrate by selecting a substrate pre-coated with such a material, such as Cerapeel (registered trademark) manufactured by Toray Industries, Inc. By providing a release layer on the substrate, the thin sheet-like molded product obtained after the drying process can be easily separated from the substrate.
[0052] In the drying step, the paste is dried on the substrate in, for example, a furnace or a dryer, etc. This causes the organic solvent in the paste to evaporate, and a sheet-like molded body is obtained on the substrate.
[0053] The drying temperature can be set to 90°C or higher and 165°C or lower. By heating and drying the paste at a temperature within this range, it is possible to complete drying in a relatively short time while suppressing boiling of components such as the organic solvent in the paste. As a result, localized surface roughness and pinhole formation due to boiling of organic solvent components and prolonged heating are suppressed, making it easier to obtain a porous titanium body with a smooth surface.
[0054] The drying time is not particularly limited and may be determined as appropriate, and may be, for example, 5 minutes or more and 300 minutes or less. From the viewpoint of effectively removing the organic solvent from the paste, it is desirable to perform the drying while discharging gas from the furnace, dryer, etc. When discharging gas from the furnace or dryer, the inside of the furnace or dryer may be made into a reduced pressure atmosphere, or the inside of the furnace or dryer may be made into a pressure equivalent to the outside by supplying a gas such as atmospheric air.
[0055] After the drying step is completed, the green body obtained by drying the paste may be separated from the substrate, for example, by peeling it off, before the binder removal step. Separating the green body from the substrate at this stage can prevent the porous titanium body from being deformed, resulting in poor sheet shape, or contamination of the porous titanium body due to the substrate material, when the green body is subjected to the subsequent binder removal step or sintering step together with the substrate. When a resin substrate is used, separation of the green body from the substrate becomes easier. When a metal substrate is used, it can be difficult to separate the green body from the substrate.
[0056] Next, in the binder removal step, the compact is heated in a furnace to volatilize and remove the organic binder in the compact. In the binder removal step, for example, the compact can be heated to a temperature of 300° C. or higher and 450° C. or lower for a time of 3 hours or higher and 12 hours or lower.
[0057] The compact that has undergone the binder removal step is then subjected to a sintering step, in which the titanium powder in the compact is sintered. The conditions for the sintering step are not particularly limited as long as the titanium powder in the compact is sintered. For example, in the sintering step, the compact may be heated to a temperature of 700°C or higher and 1000°C or lower for a period of 1 hour or higher and 4 hours or lower. Since the titanium porous body of this embodiment is relatively thin, the titanium powder can be appropriately sintered at a relatively low temperature and for a short heating period. The atmosphere during sintering may be, for example, 1.0 x 10 -2 The atmosphere may be a vacuum of 10 Pa or less, or an inert atmosphere of Ar or He.
[0058] After the sintering step, a porous titanium body is obtained, which, as mentioned above, has a large number of fine pores formed on at least one surface.
[0059] Next, a prototype of the porous titanium body of the present invention was produced and its effects were confirmed, which will be described below. However, the description here is for illustrative purposes only and is not intended to be limiting.
[0060] Titanium powder (HDH powder) having an average particle size shown in Table 1 and a titanium content of 99% by mass or more was mixed with polyvinyl butyral as an organic binder and isopropyl alcohol as an organic solvent to prepare a paste. The paste did not contain any foaming agent.
[0061] In Examples 1 to 7 and Comparative Examples 2 and 4, the paste further contained a dispersant A. Dispersant A was SN Sparce 2190 manufactured by San Nopco Ltd., which contained 42% by mass of coal tar naphtha and 58% by mass of polycarboxylic acid amine salts and the like.
[0062] A paste containing no dispersant was used in Comparative Example 1. A paste containing Dispersant B was used in Comparative Example 3. Dispersant B was SN Sperse 70 manufactured by San Nopco Ltd., which contained 63 mass % of an aliphatic amide surfactant, 26 mass % of a nonionic surfactant, and 11 mass % of diethanolamine.
[0063] The mass ratio of titanium powder:organic binder:organic solvent was 100:9:36 in all of Examples 1 to 7 and Comparative Examples 1 to 3. The contents of dispersants in the pastes of Examples 1 to 7 and Comparative Examples 2 to 4 are shown in Table 1.
[0064] The pastes of Examples 1 to 7 and Comparative Examples 1 to 3 did not contain water, but in Comparative Example 4, the organic solvent was reduced by 10 mass% from the paste of Example 1, and 10 mass% of water was added instead.
[0065] For each of Examples 1 to 7 and Comparative Examples 1 to 3, the paste was applied in the form of a sheet onto a release layer provided on a PET sheet, and this was heated and dried in an air atmosphere at the temperatures shown in Table 1 to remove the organic solvent, thereby obtaining a molded article. Next, the molded article was peeled off from the release layer and heated at 360°C in an air atmosphere to perform a binder removal treatment. Thereafter, the molded article was subjected to a vacuum treatment (1.0 x 10 -3 The titanium powder was sintered by heating at 775°C under a pressure of 1000 Pa or less, and the surface area was 240,000 mm 2 A sheet-like porous titanium body having dimensions of approximately 600 mm x 400 mm in plan view was produced. In Comparative Example 4, the titanium powder in the paste was not dispersed but aggregated, so the steps after coating on the PET sheet were not carried out and the production of the porous titanium body was abandoned.
[0066] For each titanium porous body produced as described above, the thickness, the average value and standard deviation of the pore area on the surface that was in contact with the release layer of the PET sheet during production, and the number of pores within a rectangular region were measured using the methods described above. Here, the titanium porous body was cut into five pieces, and each sample was observed using a scanning electron microscope. A Keyence Ultra-Deep Multi-Angle Lens VHX-D510 was used as the scanning electron microscope. The results are shown in Table 1. The titanium porous bodies of all Examples had a titanium content of 97% by mass or more and an oxygen content of 0.9% by mass or more and 2.0% by mass or less.
[0067]
[0068] As can be seen from Table 1, all of the porous titanium bodies of Examples 1 to 7 had surfaces on which numerous fine pores were formed.
[0069] In contrast, in Comparative Example 1, no dispersant was added to the paste during production, so the standard deviation of the pore area on the surface of the titanium porous body was large and the number of pores was small. In Comparative Example 2, the average particle size of the titanium powder used in production was large, so the average value and standard deviation of the pore area on the surface of the titanium porous body were both large and the number of pores was small. In Comparative Example 3, the dispersant B added to the paste did not contain coal tar naphtha, so the average value and standard deviation of the pore area on the surface of the titanium porous body were large and the number of pores was small.
[0070] Furthermore, to confirm the breathability of each porous titanium body, the air permeability of each porous titanium body was measured using a Gurley densometer in accordance with ISO 5636. However, the size of the vent hole used in measuring the breathability was 6 mm instead of 22 mm.
[0071] Air permeability depends on the thickness of the porous titanium body, and the porous titanium body of Example 1 having a thickness of 500 μm had an air permeability of 5 μm / Pa·s or more. The porous titanium bodies of Examples 2, 4, 6 and 7 having a thickness of 100 μm had an air permeability of 50 μm / Pa·s or more. The porous titanium body of Example 3 having a thickness of 40 μm had an air permeability of 100 μm / Pa·s or more. The porous titanium body of Example 5 having a thickness of 250 μm had an air permeability of 10 μm / Pa·s or more. All of Examples 1 to 7 had excellent air permeability according to their respective thicknesses.
[0072] From the above, it has been found that according to the present invention, a porous titanium body having a surface on which a relatively large number of fine pores are formed can be obtained.
Claims
1. A sheet-shaped porous titanium body having pores, the average area of the pores opening to at least one surface being 10 μm 2 More than 17 μm 2 The standard deviation of the area of the pores is 20 μm or less. 2 and the area is 40,000 μm 2 The titanium porous body has a rectangular region having an aspect ratio of 4:5 and the number of the pores present therein is 250 or more.
2. The titanium porous body according to claim 1, which has a thickness of 40 μm or more and 500 μm or less.
3. On the surface, the average area of the pores is 10 μm 2 More than 14 μm 2 3. The titanium porous body according to claim 1 or 2, wherein:
4. The standard deviation of the area of the pores on the surface is 17 μm 2 3. The titanium porous body according to claim 1 or 2, wherein:
5. The surface has an area of 40,000 μm 2 3. The titanium porous body according to claim 1, wherein the number of pores present within a rectangular region having an aspect ratio of 4:5 is 300 or more.
6. A titanium porous body according to claim 1 or 2, having a titanium content of 97 mass% or more.
7. A method for producing a sheet-like porous titanium body having pores, comprising: a drying step of drying a paste containing titanium powder having an average particle size of 25 μm or less, an organic binder, and an organic solvent, and not containing water as a solvent, to obtain a sheet-like molded body; a binder removal step of heating the molded body to volatilize the organic binder; and a sintering step of heating the molded body after the binder removal step to sinter the titanium powder, wherein the organic solvent in the paste is alcohol, and the paste contains a dispersant containing coal tar naphtha.
8. A method for producing a porous titanium body as described in claim 7, wherein the content of the dispersant in the paste is 0.01 mass % or more and 0.3 mass % or less.
9. A method for producing a porous titanium body according to claim 7 or 8, which produces a porous titanium body having a thickness of 40 μm or more and 500 μm or less.
10. A method for producing a porous titanium body according to claim 7 or 8, wherein the average particle size of the titanium powder is 18 μm or less.
11. The method for producing a porous titanium body according to claim 7 or 8, wherein the drying temperature in the drying step is 90°C or higher and 165°C or lower.
Citation Information
Patent Citations
Titanium porous plate material, electrode for water electrolysis, and water electrolysis device
WO2022210681A1
Method of metallic component surface modification for electrochemical applications
US20160305011A1
Porous titanium-based sintered compact, method for manufacturing same, and electrode
WO2019181684A1
Titanium-based porous body and method for producing titanium-based porous body
WO2022064898A1
Titanium porous plate, electrode for water electrolysis, and water electrolysis device
WO2022210421A1