Composition, polymer, cured product, molded body, and method for producing polymethyl methacrylate

The use of a composition with methyl methacrylate and 4-carbon alcohol in specific concentrations addresses storage stability and quality issues in polymethyl methacrylate production, achieving enhanced heat resistance and optical properties for long-term use.

WO2024224922A1PCT designated stage expired Publication Date: 2024-10-31SUMITOMO CHEM CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012193
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-03-27
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Polymethyl methacrylate products face challenges in storage stability and quality deterioration, particularly during long-term storage, which affects their heat resistance and optical properties, necessitating improved methods for producing high-quality polymers with enhanced storage stability.

Method used

A composition comprising methyl methacrylate and an alcohol with 4 carbon atoms, such as n-butanol, in specific concentration ranges, along with optional additives like (meth)acrylic esters and polymerization regulators, is used to produce polymethyl methacrylate, ensuring excellent storage stability and maintaining heat resistance and transparency.

Benefits of technology

The proposed method results in polymethyl methacrylate products with improved storage stability, heat resistance, and optical properties, as demonstrated by suppressed polymerization reactions and high total light transmittance even after accelerated aging, making them suitable for various applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

The present invention addresses the problem of providing: a composition excellent in storage stability; a polymer, a cured product, and a molded body obtained by using the composition; and a method for producing polymethyl methacrylate using the composition. The present invention relates to a composition containing methyl methacrylate and an alcohol having 4 carbon atoms, wherein the concentration of the alcohol having 4 carbon atoms is 5-10000 mass ppm of the total composition.
Need to check novelty before this filing date? Find Prior Art

Description

Composition, polymer, cured product, molded product, and method for producing polymethyl methacrylate

[0001] The present disclosure relates to a composition, a polymer, a cured product, a molded article, and a method for producing polymethyl methacrylate.

[0002] Polymethyl(meth)acrylate obtained by polymerizing methyl(meth)acrylate is used in various fields as a resin material with excellent transparency and weather resistance. In recent years, with the rise in resource prices and growing awareness of environmental issues, products (molded articles) containing polymethyl(meth)acrylate used for various applications as described above are being collected and recycled.

[0003] Methods for recycling polymethyl(meth)acrylate include, for example, material recycling, in which recovered molded bodies are subjected to a molding process again to produce new molded bodies; chemical recycling, in which recovered molded bodies are heat-treated to thermally decompose (depolymerize) the polymethyl(meth)acrylate to recover methyl (meth)acrylate, and new molded bodies are produced using the recovered methyl (meth)acrylate (sometimes referred to as recycled MMA or recycled MA); and thermal recycling, in which recovered molded bodies are burned as fuel and the combustion energy is used directly as a heat source and further used to generate electricity.

[0004] Furthermore, in response to the recent diversification of applications of polymethyl(meth)acrylate, techniques for improving the quality of polymethyl(meth)acrylate have been investigated. For example, as a polymerization apparatus suitable for obtaining high-quality polymethyl(meth)acrylate, a polymerization apparatus that suppresses the formation of gelled products in a reaction vessel in which raw material monomers and a polymerization initiator are reacted has been proposed (see Patent Document 1).

[0005] JP 2012-102190 A

[0006] In addition to improving the polymerization process of raw material monomers as described in Patent Document 1, measures to improve the quality of polymethyl(meth)acrylate include measures to suppress deterioration in quality of raw material monomers during storage. In view of the above circumstances, an object of one embodiment of the present disclosure is to provide a composition that has excellent storage stability, particularly storage stability when stored for a long period of time, a polymer, a cured product, and a molded article obtained using this composition, and a method for producing polymethyl methacrylate using this composition.

[0007] Means for solving the above problems include the following embodiments. <1> A composition containing methyl methacrylate and a C4 alcohol, wherein the concentration of the C4 alcohol is 5 ppm by mass to 10,000 ppm by mass based on the total composition. <2> The composition according to <1>, wherein the content of methyl methacrylate is 85% by mass or more based on the total composition. <3> The composition according to <1> or <2>, wherein the content of methyl methacrylate is 90% by mass or more based on the total composition. <4> The composition according to any one of <1> to <3>, wherein the concentration of the C4 alcohol is 5 ppm by mass to 6,000 ppm by mass based on the total composition. <5> The composition according to any one of <1> to <4>, wherein the concentration of the C4 alcohol is 50 ppm by mass to 6,000 ppm by mass based on the total composition. <6> The composition according to any one of <1> to <5>, wherein the C4 alcohol is n-butanol. <7> The composition according to any one of <1> to <6>, wherein the methyl methacrylate includes recycled methyl methacrylate or bio-derived methyl methacrylate. <8> The composition according to any one of <1> to <7>, further including a (meth)acrylic acid ester other than methyl methacrylate. <9> The composition according to any one of <1> to <7>, further including a polymer including structural units derived from methyl methacrylate. <10> A polymer including structural units derived from methyl methacrylate contained in the composition according to any one of <1> to <9>. <11> A molded article including the polymer according to <10>. <12> A cured product of the composition according to any one of <1> to <9>. <13> A molded article including the cured product according to <12>. <14> A method for producing polymethyl methacrylate, comprising a step of polymerizing methyl methacrylate contained in the composition according to any one of <1> to <9>.

[0008] According to one embodiment of the present disclosure, there are provided a composition having excellent storage stability, particularly excellent storage stability when stored for a long period of time, a polymer, a cured product, and a molded article obtained using this composition, and a method for producing polymethyl methacrylate using this composition.

[0009] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to the following embodiments. In this specification, numerical ranges indicated using "to" include the numerical values ​​before and after "to" as the minimum and maximum values, respectively. In numerical ranges described in stages in this specification, the upper or lower limit value described in one numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in numerical ranges described in this specification, the upper or lower limit value of that numerical range may be replaced with a value shown in an example.

[0010] <Composition> The composition of the present disclosure contains methyl methacrylate and an alcohol having 4 carbon atoms, wherein the concentration of the alcohol having 4 carbon atoms is 5 ppm by mass to 10,000 ppm by mass based on the total mass of the composition. As shown in the examples described below, the composition of the present disclosure has excellent storage stability.

[0011] (Methyl methacrylate) The composition of the present disclosure contains methyl methacrylate. In the present disclosure, "methyl methacrylate" refers to methyl methacrylate that is essentially free of impurities such as by-products generated during the synthesis of methyl methacrylate. However, the methyl methacrylate in the present disclosure is not limited thereto, provided that the purpose of the invention is not impaired. In other words, "methyl methacrylate" may contain impurities that cannot be completely removed by conventional purification methods, or may contain impurities at a level that cannot be detected by conventional detection methods.

[0012] The content of methyl methacrylate in the composition is not particularly limited and can be selected depending on the application of polymethyl methacrylate obtained using the composition. The content of methyl methacrylate may be, for example, 85% by mass or more, 90% by mass or more, 95% by mass or more, or 99% by mass or more of the total composition. A content of methyl methacrylate in the composition within the above range is preferable in terms of at least the heat resistance or surface hardness of a polymer obtained by polymerizing the composition and a molded article containing the same.

[0013] The methyl methacrylate contained in the composition may be synthesized by a known synthesis method. The synthesis method is not particularly limited, and may be the ACH method, the C4 direct acid method, or the alpha method.

[0014] The methyl methacrylate contained in the composition may include recycled methyl methacrylate. In this disclosure, recycled methyl methacrylate refers to methyl methacrylate obtained by depolymerization of polymethyl methacrylate (a reaction in which a polymer decomposes to produce monomers). Depolymerization of polymethyl methacrylate can be achieved, for example, by heat-treating polymethyl methacrylate. The source of polymethyl methacrylate, which is the raw material for recycled methyl methacrylate, is not particularly limited as long as methyl methacrylate can be recovered. For example, the source of polymethyl methacrylate may be a molded product containing polymethyl methacrylate.

[0015] The methyl methacrylate contained in the composition may include bio-derived methyl methacrylate. In the present disclosure, bio-derived methyl methacrylate refers to methyl methacrylate synthesized from a biologically derived raw material. The biologically derived raw material may be a plant-derived raw material or an animal-derived raw material, and is preferably a raw material derived from vegetable oil.

[0016] (C4 Alcohol) The composition of the present disclosure contains a C4 alcohol. The C4 alcohol contained in the composition may be at least one selected from the group consisting of n-butanol, isobutyl alcohol, sec-butyl alcohol, and tert-butyl alcohol. From the viewpoint of storage stability of the composition, the C4 alcohol is preferably n-butanol.

[0017] The concentration of the C4 alcohol contained in the composition is 5 ppm by mass to 10,000 ppm by mass of the total composition. From the viewpoint of long-term storage stability of the composition, the concentration of the C4 alcohol contained in the composition is preferably 10 ppm by mass or more of the total composition, more preferably 20 ppm by mass or more, and even more preferably 50 ppm by mass or more. From the viewpoint of optical stability of the composition, the concentration of the C4 alcohol contained in the composition is preferably 8,000 ppm by mass or less of the total composition, more preferably 6,000 ppm by mass or less, and even more preferably 5,000 ppm by mass or less. Furthermore, from the viewpoint of the heat resistance of the polymer, cured product, and molded article formed from the composition described below, the concentration of the C4 alcohol contained in the composition is preferably 10 ppm by mass or more of the total composition, more preferably 20 ppm by mass or more, and even more preferably 50 ppm by mass or more, and is preferably 6,000 ppm by mass or less of the total composition.

[0018] If necessary, the composition may contain a component other than methyl methacrylate and an alcohol having a carbon number of 4. For example, the composition may contain a (meth)acrylic acid ester other than methyl methacrylate, a polymer containing a structural unit derived from methyl methacrylate, a low-content component, or an additive, as described below.

[0019] ((Meth)acrylic acid ester) In addition to methyl methacrylate, the composition may contain a (meth)acrylic acid ester other than methyl methacrylate (hereinafter simply referred to as a (meth)acrylic acid ester). Specific examples of the (meth)acrylic acid ester include methyl acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, and cyclopentanyl (meth)acrylate. Among these, methyl acrylate or ethyl acrylate is preferred, and methyl acrylate is more preferred. These may be used alone or in combination of two or more. In the present disclosure, the term "(meth)acrylic acid ester" indicates that the compound may be an acrylic acid ester or a methacrylic acid ester. The (meth)acrylic acid ester may be contained in the composition as a by-product produced during the production of methyl methacrylate or during the regeneration treatment of polymethyl methacrylate, or may be intentionally mixed into the composition.

[0020] When the composition contains a (meth)acrylic acid ester, the concentration thereof is preferably 50,000 ppm by mass or less, more preferably 40,000 ppm by mass or less, and even more preferably 30,000 ppm by mass or less, based on the total composition. When the composition contains another (meth)acrylic acid ester, the concentration thereof may be 1 ppm by mass or more, 2 ppm by mass or more, or 5 ppm by mass or more, based on the total composition.

[0021] The composition may contain, in addition to methyl methacrylate, a polymer containing structural units derived from methyl methacrylate. This polymer may be a homopolymer of methyl methacrylate or a copolymer of methyl methacrylate with another (meth)acrylic acid ester polymerizable with methyl methacrylate. Examples of the other (meth)acrylic acid ester polymerizable with methyl methacrylate include the same as those described above.

[0022] (Low Content Component) The composition may contain a low content component other than the alcohol having 4 carbon atoms. The low content component may be contained in the composition as a by-product generated during the production of methyl methacrylate or the regeneration treatment of polymethyl methacrylate. In the present disclosure, the low content component means a component contained in the composition at a concentration of 10,000 ppm by mass or less.

[0023] Examples of the low content component other than the alcohol having 4 carbon atoms that the composition may contain include carboxylic acid esters, aromatic hydrocarbon compounds, aliphatic hydrocarbon compounds, alcohols other than the alcohol having 4 carbon atoms, butyl acrylate, etc. The low content component other than the alcohol having 4 carbon atoms contained in the composition may be one type only, or two or more types.

[0024] Specific examples of carboxylic acid esters include methyl isobutyrate, methyl propionate, methyl 2,4-dimethyl-4-pentenoate, methyl 2-methyl-3-butenoate, methyl tiglate, methyl 3-methyl-3-butenoate, methyl 3-methyl-2-butenoate, dimethyl itaconate, and dimethyl 2-methyl-5-methylenehexanedioate. Specific examples of aromatic hydrocarbon compounds include toluene and styrene. Specific examples of aliphatic hydrocarbon compounds include 1-octene and 1-octadecene.

[0025] When the composition contains low-content components other than the C4 alcohol, the concentration of each low-content component is preferably 8000 ppm by mass or less, more preferably 6000 ppm by mass or less, and even more preferably 5000 ppm by mass or less, of the total composition. When the composition contains low-content components other than the C4 alcohol, the concentration of each low-content component may be 1 ppm by mass or more, 2 ppm by mass or more, or 5 ppm by mass or more, of the total composition.

[0026] (Additives) The composition may contain additives as needed. Specific examples of additives include a release agent, a polymerization regulator, a polymerization initiator, an ultraviolet absorber, and a colorant. The composition may contain one or more additives.

[0027] Examples of the release agent that can be contained in the composition include higher fatty acid esters, higher fatty alcohols, higher fatty acids, higher fatty acid amides, higher fatty acid metal salts, and fatty acid derivatives. Specific examples of the release agent include sodium di-(2-ethylhexyl)sulfosuccinate, stearyl alcohol, methyl stearate, and stearic acid amide.

[0028] The composition may contain one or more types of release agents. The content of the release agent in the composition may be, for example, 0.01% by mass to 1.0% by mass of the total composition.

[0029] As the polymerization regulator (an additive that regulates the polymerization rate in a polymerization reaction) that may be contained in the composition, any suitable polymerization regulator known in the art can be used. Examples of such polymerization regulators that can be used include compounds that can regulate the polymerization rate in a direction that slows down the polymerization rate. Specific examples of polymerization regulators include mercaptan compounds such as n-butyl mercaptan and n-octyl mercaptan, terpenoid compounds such as limonene, myrcene, α-terpinene, β-terpinene, γ-terpinene, terpinolene, β-pinene, and α-pinene, and α-methylstyrene dimer.

[0030] The composition may contain one or more polymerization regulators, and the content of the polymerization regulator in the composition may be, for example, 0.001% by mass to 0.5% by mass of the total composition.

[0031] The polymerization initiator that the composition may contain includes a radical polymerization initiator, a diacyl peroxide initiator, a dialkyl peroxide initiator, a peroxyester initiator, a percarbonate initiator, and a peroxyketal initiator.

[0032] Specific examples of radical polymerization initiators include azo compounds such as 1,1′-azobis(cyclohexane-1-carbonitrile), 2,2′-azobis(2,4,4-trimethylpentene), 2,2′-azobis(2-methylpropane), 2-cyano-2-propylazoformamide, 2,2′-azobis(2-hydroxymethylpropionate), 2,2′-azobis(2-methylbutyronitrile), 2,2′-azobisisobutyronitrile, 2,2′-azobis[2-(2-imidazolin-2-yl)propane], and dimethyl 2,2′-azobis(2-methylpropionate).

[0033] Specific examples of diacyl peroxide initiators and dialkyl peroxide initiators include dicumyl peroxide, tert-butylcumyl peroxide, di-tert-butyl peroxide, benzoyl peroxide, and lauroyl peroxide.

[0034] Specific examples of peroxyester initiators include tert-butylperoxy-3,3,5-trimethylhexanoate, tert-butylperoxylaurate, tert-butylperoxyisobutyrate, tert-butylperoxyacetate, di-tert-butylperoxyhexahydroterephthalate, di-tert-butylperoxyazelate, tert-butylperoxy-2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, and tert-amylperoxy-2-ethylhexanoate.

[0035] Specific examples of percarbonate initiators include tert-butylperoxyallyl carbonate and tert-butylperoxyisopropyl carbonate.

[0036] Specific examples of peroxyketal initiators include 1,1-di-tert-butylperoxycyclohexane, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, and 1,1-di-tert-hexylperoxy-3,3,5-trimethylcyclohexane.

[0037] The composition may contain one or more polymerization initiators, and the content of the polymerization initiator in the composition may be, for example, 0.01% by mass to 5% by mass of the total composition.

[0038] Examples of UV absorbers that the composition may contain include benzophenone UV absorbers, cyanoacrylate UV absorbers, benzotriazole UV absorbers, malonic acid ester UV absorbers, and oxalanilide UV absorbers.

[0039] Specific examples of ultraviolet absorbers include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-hydroxy-4-n-octylbenzophenone, 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole, 2-(2-hydroxy-3,5-di-tert-pentylphenyl)benzotriazole, and 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate.

[0040] The composition may contain one or more types of ultraviolet absorbers. The content of the ultraviolet absorbers in the composition may be, for example, 0.001% by mass to 1% by mass of the total composition.

[0041] Colorants that the composition may contain include perylene dyes, perinone dyes, pyrazolone dyes, methine dyes, coumarin dyes, quinophthalone dyes, quinoline dyes, anthraquinone dyes, asdolapyridone dyes, thioindigo dyes, coumarin dyes, isoindolinone pigments, sichetopyrrolopyrrole pigments, condensed azo pigments, benzimidazolone pigments, dioxazine pigments, copper phthalocyanine pigments, and quinacridone pigments.

[0042] The colorant contained in the composition may be one kind or two or more kinds. The content of the colorant in the composition is, for example, 1.0 × 10 -8 It can be 0.5% by mass to 0.5% by mass.

[0043] When the composition contains additives, the total content thereof may be 15% by mass or less, 10% by mass or less, 5% by mass or less, or 1% by mass or less of the total composition. When the composition contains additives, the total content thereof may be 0.01% by mass or more, 0.05% by mass or more, or 0.1% by mass or more of the total composition.

[0044] The storage conditions for the composition of the present disclosure are not particularly limited, and can be, for example, 0° C. to 35° C. From the viewpoint of ensuring good quality, the storage temperature is preferably selected from the range of 0° C. to 39° C., more preferably selected from the range of about 25° C.±10° C., and even more preferably selected from the range of about 25 to 30° C.

[0045] The composition of the present disclosure has excellent storage stability. Specifically, the composition can maintain a state in which the polymerization reaction is suppressed during storage. In the present disclosure, the storage stability of the composition was evaluated by checking whether or not a polymer was formed in the composition stored under accelerated conditions, and by measuring the total light transmittance of the composition stored under accelerated conditions. The methods for evaluating storage stability and measuring total light transmittance are described below.

[0046] In the examples described later, the storage stability of a composition was evaluated by (1) preparing a composition containing methyl methacrylate and an alcohol, (2) conducting a storage test including the following steps 1 to 7 in this order, and (3) visually observing the appearance of the solution of the composition after the storage test when it was dropped into a poor solvent.

[0047] Step 1: Inject 25 mL of the composition into the bottom of a pressure vessel (TVS-N2 type manufactured by Taiatsu Glass Industry Co., Ltd.). Step 2: Place a gasket between the top and bottom of the pressure vessel and seal the pressure vessel. Step 3: Feed nitrogen into the top tip of the pressure vessel and seal it at an internal pressure of 0.2 MPa, then check for one minute to see if the internal pressure changes. Step 4: Remove the internal pressure from the pressure vessel and attach a stopcock to the top tip of the pressure vessel. Step 5: Place the pressure vessel in an oil bath set to 60°C. Step 6: Store in the oil bath for 72 hours. Step 7: After 72 hours, remove the pressure vessel from the oil bath and place it in ice-cold water to rapidly cool it.

[0048] In the above (3), the poor solvent may be selected from any suitable solvent that does not dissolve the polymer formed in the composition. In the examples described below, normal hexane is used. The lower the degree of cloudiness or precipitation in the solution, the more the polymerization reaction of methyl methacrylate is inhibited.

[0049] In the examples described below, the total light transmittance of a composition stored under accelerated conditions is measured by measuring the total light transmittance of the composition after storage. Specifically, the total light transmittance Tt (%) of the composition after storage is measured for light in the wavelength range of 500 nm to 780 nm when the optical path length is 10 mm. A spectrophotometer (Hitachi Spectrophotometer U-4000, manufactured by Hitachi High-Tech Fielding Corporation) is used for the measurement, but any suitable commercially available spectrophotometer may also be used. The higher the total light transmittance, the more the optical properties, such as transparency, of the composition can be determined to be maintained. The total light transmittance of a composition stored under accelerated conditions is preferably greater than 97%, and more preferably 98% or greater.

[0050] <Polymer, Cured Product, and Molded Product> The polymer of the present disclosure is a polymer containing structural units derived from methyl methacrylate contained in the composition of the present disclosure described above. Here, the polymer is obtained by polymerizing components involved in polymerization contained in the composition, and has structural units derived from the components involved in polymerization. The polymer of the present disclosure may contain structural units derived from methyl methacrylate contained in the composition of the present disclosure and structural units derived from other polymerization components. The weight-average molecular weight of the polymer of the present disclosure is not particularly limited and can be selected depending on the application of the polymer. The cured product of the present disclosure is a cured product of the composition of the present disclosure described above. Here, the cured product is a cured composition and may also contain components not involved in polymerization. However, depending on the method for curing the composition, it may be considered the same as the above-mentioned polymer (i.e., not containing components not involved in polymerization). The molded product of the present disclosure includes the polymer or cured product of the present disclosure described above. If the cured product can be considered the same as a polymer, the molded product will contain a polymer of the composition of the present disclosure. Preferably, the molded product contains a cured product obtained by curing only the composition of the present disclosure. The molded article may be an object obtained by molding a polymer or a cured product into any shape.

[0051] (Physical Properties of Polymer and Cured Product) The polymer and cured product of the present disclosure have excellent heat resistance and optical properties. Specifically, compared to a polymer or cured product obtained from a composition containing methyl methacrylate but not containing a C4 alcohol, the Vicat softening temperature is approximately the same, and the total light transmittance for light having a wavelength in the range of 380 nm to 780 nm after accelerated aging treatment tends to be less likely to decrease.

[0052] The Vicat softening temperature indicates the heat resistance of polymers and cured products. Specifically, it is an index of resistance to deformation in high-temperature environments. If the Vicat softening temperature is high, for example, when a polymer or cured product is used outdoors, it is less likely to deform even when exposed to high temperatures such as direct sunlight, making it possible to use it. In the present disclosure, the Vicat softening temperature can be measured using any suitable conventionally known device and any suitable conventionally known method. In the examples described below, the Vicat softening temperature was measured using a heat distortion tester ("148-6-barrel model" manufactured by Yasuda Seiki Seisakusho Co., Ltd.) in accordance with JIS K7206 (B50 method). As the test piece used for the measurement, for example, a cast plate as described below can be used.

[0053] A specific method for measuring the Vicat softening temperature is described below. First, a 25 mm × 25 mm × 3 mm test piece prepared from the cast plate is stored at 83°C for 16 hours, and then subjected to a conditioning treatment in which the test piece is allowed to cool in a desiccator at 23±5°C for at least 1 hour. After the conditioning treatment, the Vicat softening temperature (°C) of the test piece is measured using a heat distortion tester ("148-6-barrel model" manufactured by Yasuda Seiki Seisakusho Co., Ltd.) in accordance with JIS K7206 (B50 method).

[0054] Optical properties, more specifically, total light transmittance, indicate the transparency of a polymer and a cured product. In the present disclosure, the measurement of total light transmittance may be performed after subjecting the polymer or the cured product to an accelerated aging treatment. This method can efficiently evaluate the transparency of the polymer or the cured product after long-term use.

[0055] In the examples described below, the molded articles after the accelerated aging treatment were used to measure the total light transmittance Tt (%) for light in the wavelength range of 380 nm to 780 nm using a commercially available spectrophotometer (Hitachi Spectrophotometer U-4000, manufactured by Hitachi High-Tech Fielding Corporation).

[0056] A specific method for measuring total light transmittance in the present disclosure is described below. First, a 50 mm x 50 mm x 3 mm test piece made from a polymer or a cured product is subjected to accelerated aging treatment by leaving it in an incubator ("Vacuum Oven VOS-301SD" manufactured by Tokyo Rikakikai Co., Ltd.) set to 80°C for 200 hours. Next, using the test piece after the accelerated aging treatment, the total light transmittance Tt (%) for light rays in the wavelength range of 380 nm to 780 nm when the optical path length is set to 50 mm is measured. The measurement is performed using a spectrophotometer ("Hitachi Spectrophotometer U-4000" manufactured by Hitachi High-Tech Fielding Corporation). From the perspective of optical properties, the total light transmittance of the polymer or cured product after the accelerated aging treatment is preferably 81% or more, and more preferably 81.5% or more.

[0057] Whether the polymer and cured product of the present disclosure contain methyl methacrylate, a C4 alcohol, or other components can be determined by known analytical methods. Examples of known analytical methods include gas chromatography and liquid chromatography.

[0058] <Method for producing polymethyl methacrylate> The method for producing polymethyl methacrylate of the present disclosure is a method for producing polymethyl methacrylate, including a step of polymerizing the methyl methacrylate contained in the composition of the present disclosure described above. Here, the polymethyl methacrylate of the present disclosure corresponds to a polymer obtained from the composition of the present disclosure, and also corresponds to a cured product obtained from the composition.

[0059] The method for polymerizing methyl methacrylate contained in the composition is not particularly limited, and may be carried out by a known method, such as bulk polymerization, cell cast polymerization, solution polymerization, suspension polymerization, or emulsion polymerization.

[0060] Specifically, the composition of the present disclosure can be used, for example, by bulk polymerization to form a methyl methacrylate polymer into a sheet (molded product). Furthermore, in cell-cast polymerization, the composition is heated under predetermined heating conditions to promote the polymerization reaction, thereby forming a cured product (molded product) from the composition.

[0061] In the method for polymerizing methyl methacrylate contained in the composition of the present disclosure or the method for producing a molded article, the heating conditions, that is, the heating temperature and heating time, can be set taking into consideration, for example, the type and content of the selected polymerization regulator, polymerization initiator, and / or other components.

[0062] In cell cast polymerization, the heating temperature for producing a cured product and its molded article can be, for example, 50°C to 120°C. The heating time for production can be, for example, 1 hour to 20 hours. The heat treatment can be a heat treatment including multiple steps with different heating temperatures and / or heating times.

[0063] The cured product obtained by cell cast polymerization and its molded article can be produced, for example, by carrying out a heat treatment under heating conditions including the following steps 1 to 7.

[0064] Step 1: Raise the temperature from room temperature to 68°C over 20 minutes. Step 2: Hold at 68°C for 90 minutes. Step 3: Lower the temperature from 68°C to 64°C over 20 minutes. Step 4: Hold at 64°C for 90 minutes. Step 5: Raise the temperature from 64°C to 123°C over 10 minutes. Step 6: Hold at 123°C for 120 minutes. Step 7: Lower the temperature from 123°C to room temperature over 78 minutes.

[0065] In the method for producing a cured product and a molded article thereof, by carrying out the above steps 1 to 7 in this order, heat generation during the polymerization reaction can be suppressed and the polymerization can be completed stably.

[0066] When the composition of the present disclosure is subjected to a heat treatment, for example, a cell casting method (cell cast polymerization) using a cell capable of defining an enclosed space of a predetermined shape inside can be applied to form a molded article of a predetermined shape. The method for producing a molded article by the cell casting method will be specifically described below.

[0067] To produce a molded body by the cell casting method, a cell is first prepared. Here, an example of forming a plate-shaped molded body (sometimes called a cast plate) is described. Such a cell can be composed of at least two flat plate-shaped members and a sealing material (gasket) that is sandwiched between the two flat plate-shaped members and can seal the gap between the two opposing flat plate-shaped members as an airtight space.

[0068] The flat plate-like member may be in the form of a sheet or a belt. The flat plate-like member is made of a material that is not dissolved by the composition of the present disclosure, does not inhibit the polymerization reaction of the composition, and has sufficient heat resistance to the heating temperature in the heat treatment. Examples of suitable materials for the flat plate-like member include glass and metal.

[0069] Any suitable conventional sealing material can be used as the sealing material. The sealing material is composed of a material that is not dissolved by the composition of the present disclosure, does not inhibit the polymerization reaction of the composition, and has sufficient heat resistance to the heating temperature in the heat treatment. A specific example of a suitable sealing material is a gasket made of vinyl chloride resin.

[0070] Next, the composition of the present disclosure is injected into the gap (void) defined by the prepared cells by any suitable conventional method. The cells are then heat-treated under the heating conditions already described. The method of heat-treating the cells into which the composition of the present disclosure has been injected is not particularly limited. The heat-treating method for the cells may be, as in the conventionally known cell casting method, a method in which the cells are directly heat-treated from the outside using a hot air circulating oven, an infrared heater, or the like, or a method in which a conventionally known jacket is further provided outside the cells and a heat medium such as hot air, hot water, or steam is introduced into the jacket.

[0071] <Applications of Polymethyl Methacrylate and Molded Articles Thereof> Polymethyl methacrylate and molded articles thereof obtained from the composition of the present disclosure have excellent light transmittance, heat resistance, and weather resistance, and are therefore suitable for a variety of applications that may be exposed to the external environment and further to heat and light sources, such as lighting fixtures, automobile parts, signs, and building materials.

[0072] Hereinafter, embodiments of the present disclosure will be described based on examples, but the present disclosure is not limited to the following examples.

[0073] Example 1 0.001% by mass of n-butanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as an alcohol was added to and mixed with 99.999% by mass of methyl methacrylate to prepare composition 1. The resulting composition 1 was in the form of a solution.

[0074] Examples 2 to 5 and Comparative Examples 1 to 6 Compositions were prepared in the same manner as in Example 1, except that the alcohol and its concentration (ppm by mass) added to methyl methacrylate were changed from Example 1 as shown in Table 1. All of the obtained compositions were in the form of a solution. As the alcohol, n-butanol, methanol, or ethanol (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was used.

[0075] (1) Evaluation of Storage Stability of Compositions A storage test including the following steps 1 to 7 in this order was carried out on the compositions prepared in Examples 1 to 5 and Comparative Examples 1 to 6. The storage test was carried out under accelerated conditions (60°C) to evaluate the stability after long-term storage.

[0076] Step 1: Inject 25 mL of the composition into the bottom of a pressure vessel (TVS-N2 type manufactured by Taiatsu Glass Industry Co., Ltd.). Step 2: Place a gasket between the top and bottom of the pressure vessel and seal the pressure vessel. Step 3: Feed nitrogen into the top tip of the pressure vessel and seal it at an internal pressure of 0.2 MPa, then check for one minute to see if the internal pressure changes. Step 4: Remove the internal pressure from the pressure vessel and attach a stopcock to the top tip of the pressure vessel. Step 5: Place the pressure vessel in an oil bath set to 60°C. Step 6: Store in the oil bath for 72 hours. Step 7: After 72 hours, remove the pressure vessel from the oil bath and place it in ice-cold water to rapidly cool it.

[0077] After the storage test, 2 mL of the composition was added to 10 mL of normal hexane in a 25 mL bottle and allowed to stand. The appearance of the solution in the bottle was then visually observed, and the state of the solution was evaluated based on the following evaluation criteria. The lower the degree of cloudiness or precipitation in the solution, the more the polymerization reaction of methyl methacrylate was inhibited. The results are shown in Table 1.

[0078] (Evaluation criteria) A (Excellent): No clear cloudiness or precipitation was observed. B (Good): Clear cloudiness or precipitation was observed, but the degree was small. C (Unacceptable): Clear cloudiness or precipitation was observed, but the degree was large.

[0079] The composition (3 mL) after the storage test was placed in a quartz glass cell (T-1, Taiko Seisakusho Co., Ltd.) measuring 10 mm in length, 10 mm in width, and 45 mm in height. Using the composition placed in the quartz glass cell, the total light transmittance Tt (%) was measured for light in the wavelength range of 500 nm to 780 nm when the optical path length was set to 10 mm. A spectrophotometer (Hitachi Spectrophotometer U-4000, manufactured by Hitachi High-Tech Fielding Co., Ltd.) was used for the measurement. The higher the total light transmittance, the more it can be determined that optical properties such as high transparency are maintained even after storage. The results are shown in Table 1.

[0080]

[0081] As shown in Table 1, the compositions of Examples 1 to 5, in which n-butanol was added to methyl methacrylate, showed a suppressed polymerization reaction of methyl methacrylate in the storage test compared to Comparative Example 1, in which no alcohol was added to methyl methacrylate, Comparative Examples 2 to 4, in which methanol was added to methyl methacrylate, or Comparative Examples 5 and 6, in which ethanol was added to methyl methacrylate. These results demonstrate that the compositions of Examples 1 to 5 exhibit excellent storage stability.

[0082] (2) Evaluation of Physical Properties of Molded Articles Molded articles were produced using the compositions of Examples 1 to 5 and Comparative Example 1, and the following physical properties were evaluated. A composition for forming a molded article was obtained by adding and mixing the composition (99.85 parts by mass) prepared as described above, sodium di-(2-ethylhexyl)sulfosuccinate (0.05 parts by mass) as a mold release agent, terpinolene (0.01 parts by mass) as a polymerization regulator, 2,2'-azobisisobutyronitrile (0.08 parts by mass) as a polymerization initiator, and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (0.01 parts by mass) as an ultraviolet absorber to a glass container. The resulting composition was in the form of a solution.

[0083] A cell was prepared in which a 3.8 mm thick vinyl chloride resin gasket was sandwiched between two opposing glass plates, creating a space sealed by the gasket between the two glass plates. The composition for forming a molded body prepared as described above was poured into this space. The cell containing the composition was placed in an oven, and methyl methacrylate was polymerized by heat treatment under heating conditions including the following steps 1 to 7 in this order. This resulted in the production of a cast plate, a molded body measuring 250 mm x 250 mm x 3 mm.

[0084] Step 1: Raise the temperature from room temperature to 68°C over 20 minutes. Step 2: Hold at 68°C for 90 minutes. Step 3: Lower the temperature from 68°C to 64°C over 20 minutes. Step 4: Hold at 64°C for 90 minutes. Step 5: Raise the temperature from 64°C to 123°C over 10 minutes. Step 6: Hold at 123°C for 120 minutes. Step 7: Lower the temperature from 123°C to room temperature over 90 minutes.

[0085] The following test was carried out to evaluate the heat resistance of the obtained molded body. A 25 mm x 25 mm x 3 mm test piece prepared from the cast plate was subjected to a conditioning treatment in which the piece was left to stand at 83°C for 16 hours and then allowed to cool in a desiccator at 23±5°C for at least 1 hour. After the conditioning treatment, the Vicat softening temperature (°C) of the test piece was measured using a heat distortion tester ("148-6-barrel model" manufactured by Yasuda Seiki Seisakusho Co., Ltd.) in accordance with JIS K7206 (B50 method). The results are shown in Table 2.

[0086] The following test was conducted to evaluate the optical properties of the obtained molded article after accelerated aging treatment. A 50 mm x 50 mm x 3 mm test piece prepared from the cast plate was subjected to accelerated aging treatment by placing it in an incubator ("Vacuum Oven VOS-301SD" manufactured by Tokyo Rikakikai Co., Ltd.) set at 80°C for 200 hours. Using the test piece after accelerated aging treatment, the total light transmittance Tt (%) was measured for light in the wavelength range of 380 nm to 780 nm when the optical path length was set to 50 mm. A spectrophotometer ("Hitachi Spectrophotometer U-4000" manufactured by Hitachi High-Tech Fielding Corporation) was used for the measurement. A total light transmittance of 81% or more can be evaluated as good for the molded article after accelerated aging treatment. The results are shown in Table 2.

[0087]

[0088] As shown in Table 2, the molded articles produced using the compositions of Examples 1 to 5 had equivalent Vicat softening temperatures and higher total light transmittances after accelerated aging treatment compared to Comparative Example 1, in which no alcohol was added to methyl methacrylate. These results demonstrate that the molded articles produced using the compositions of Examples 1 to 5 exhibit good heat resistance and, further, excellent optical properties even after long-term use.

Claims

1. A composition comprising methyl methacrylate and an alcohol having 4 carbon atoms, wherein the concentration of the alcohol having 4 carbon atoms is 5 ppm by mass to 10,000 ppm by mass of the entire composition.

2. The composition according to claim 1, wherein the content of methyl methacrylate is 85% by mass or more of the total composition.

3. The composition according to claim 1, wherein the content of methyl methacrylate is 90% by mass or more of the total composition.

4. The composition according to claim 1, wherein the concentration of the alcohol having 4 carbon atoms is 5 ppm by mass to 6,000 ppm by mass based on the total composition.

5. The composition according to claim 1, wherein the concentration of the alcohol having 4 carbon atoms is 50 ppm by mass to 6,000 ppm by mass based on the total composition.

6. The composition of claim 1, wherein the four carbon alcohol is n-butanol.

7. The composition of claim 1, wherein the methyl methacrylate comprises recycled methyl methacrylate or bio-derived methyl methacrylate.

8. The composition of claim 1, further comprising a (meth)acrylic acid ester other than methyl methacrylate.

9. The composition of claim 1, further comprising a polymer containing structural units derived from methyl methacrylate.

10. A polymer comprising structural units derived from methyl methacrylate contained in the composition according to any one of claims 1 to 9.

11. A molded article comprising the polymer according to claim 10.

12. A cured product of the composition according to any one of claims 1 to 9.

13. A molded article comprising the cured product according to claim 12.

14. A method for producing polymethyl methacrylate, comprising the step of polymerizing the methyl methacrylate contained in the composition according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Continuous polymerization apparatus, and method for producing polymer composition

    JP2012102190A

  • Resin composition for coating material, and method for producing the same

    JP2019026768A

  • Method for separating methanol

    WO2012018007A1

  • Methyl methacrylate-containing composition

    WO2022230596A1