Epoxy resin composition, prepreg, fiber-reinforced composite material, and method for producing epoxy resin composition

The epoxy resin composition with a specific structure and reaction process enhances the mechanical properties of fiber-reinforced composites by improving elastic modulus and viscosity stability, addressing the challenges of conventional compositions in high temperature and humid environments.

WO2024225092A1PCT designated stage expired Publication Date: 2024-10-31TORAY INDUSTRIES INC
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014941
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional epoxy resin compositions for fiber-reinforced composite materials face challenges in achieving high temperature/wet elastic modulus, rubber state elastic modulus, and viscosity stability, leading to insufficient tensile and compressive strength under severe conditions, particularly in aerospace and vehicle applications.

Method used

An epoxy resin composition with specific components, including an epoxy resin with two or more epoxy groups and a phenolic hydroxyl group, combined with a curing agent and a monofunctional phenol, undergoes an addition reaction to create a low crosslinking density structure, enhancing elastic modulus and viscosity stability, while a prepreg is formed by impregnating reinforcing fibers with this composition.

Benefits of technology

The resulting fiber-reinforced composite material exhibits superior mechanical properties, including high compressive and tensile strength under high temperature/humid conditions, along with improved viscosity stability and reduced volatile content, effectively addressing the limitations of previous compositions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

In the present invention, an epoxy resin composition contains an epoxy resin obtained by means of an addition reaction of one or two epoxy groups contained in one molecule of an epoxy resin having four or more epoxy groups per molecule (constituent component [A']) and a phenolic hydroxyl group contained in a monofunctional phenol compound (constituent component [B]). Provided are: an epoxy resin composition having characteristics that are superior to those of the prior art in terms of high temperature / high humidity elastic modulus of a cured product, elastic modulus in a rubbery state, and viscosity stability when used as a matrix resin; a fiber-reinforced composite material obtained using this epoxy resin composition; and a prepreg obtained by impregnating a fiber substrate with this resin composition.
Need to check novelty before this filing date? Find Prior Art

Description

Epoxy resin composition, prepreg and fiber-reinforced composite material, and method for producing epoxy resin composition

[0001] The present invention relates to an epoxy resin composition that provides a fiber-reinforced composite material with excellent mechanical properties, and to a prepreg and a fiber-reinforced composite material that use the epoxy resin composition.

[0002] Fiber-reinforced composite materials, consisting of reinforcing fibers such as carbon fiber or glass fiber and thermosetting resins such as epoxy resin or phenolic resin, have traditionally been used in a wide range of fields, including aerospace, automobiles, railway vehicles, ships, civil engineering and construction, and sporting goods, due to their lightweight construction and excellent mechanical properties, including strength and rigidity, as well as heat and corrosion resistance. In particular, applications requiring high performance require fiber-reinforced composite materials using continuous reinforcing fibers. These materials are typically made of carbon fiber, which has excellent specific strength and specific modulus, and thermosetting resins, particularly epoxy resins, which have excellent adhesion to carbon fiber, heat resistance, modulus of elasticity, and chemical resistance, and minimize cure shrinkage. As the use of fiber-reinforced composite materials has increased in recent years, their performance requirements have become increasingly stringent. Particularly for aerospace applications and vehicle structural materials, they must be able to maintain distinct physical properties, such as tensile strength and compressive strength, even under demanding conditions. To meet these physical property requirements, improvements have been made to the matrix resin. It is known that increasing the modulus of elasticity of the cured matrix resin is effective in suppressing buckling of the reinforcing fibers under compressive loads to improve the compressive strength of reinforced fiber composite materials under high-temperature / humid conditions. On the other hand, improving tensile strength requires increasing the tensile strength utilization rate of the reinforcing fibers, and it is known that decreasing the modulus of elasticity of the cured matrix resin in its rubbery state improves the tensile strength utilization rate. It is also known that decreasing the modulus of elasticity of the cured matrix resin in its rubbery state is effective in decreasing the density of crosslinking points (hereinafter sometimes referred to as crosslink density) of the cured matrix resin.

[0003] Patent Document 1 proposes an epoxy resin composition using a multifunctional epoxy resin and naphthol glycidyl ethers. Patent Document 2 proposes an epoxy resin composition using a pendant epoxy resin. Patent Document 3 proposes an epoxy resin composition using a predetermined amount of a phenol compound having a specific functional group.

[0004] International Publication No. WO 2020 / 058766 International Publication No. WO 2010 / 109929 International Publication No. WO 2018 / 159574

[0005] However, although the cured product of the epoxy resin composition described in Patent Document 1 exhibits a high modulus under high-temperature / humid conditions, its high crosslink density structure also results in a high modulus in the rubbery state, resulting in no significant improvement in tensile strength utilization. On the other hand, the cured product of the epoxy resin composition described in Patent Document 2 exhibits a superior high-temperature / humid modulus compared to epoxy resin compositions using conventional epoxy resins, and although it may also exhibit a lower rubbery-state modulus, it is still insufficient. Furthermore, the cured product of the epoxy resin composition described in Patent Document 3 also falls short in terms of high-temperature / humid modulus and rubbery-state modulus. Furthermore, sufficient consideration was not given to the possibility that the phenolic compound may promote the reaction between the epoxy resin and the curing agent when the resin composition is used as a matrix resin, resulting in a loss of viscosity stability and a deterioration in resin impregnation, or the possibility of voids occurring due to partial volatilization of the epoxy resin composition, during fiber impregnation or curing molding.

[0006] Therefore, the present invention provides an epoxy resin composition that exhibits superior properties compared to conventional techniques in terms of the high-temperature / wet elastic modulus and rubber-state elastic modulus of the cured product, and viscosity stability when used as a matrix resin; a fiber-reinforced composite material using the epoxy resin composition; and a prepreg obtained by impregnating a fiber substrate with the resin composition.

[0007] In order to solve the above problems, the present invention provides an epoxy resin composition having the following components: 1. An epoxy resin composition containing an epoxy resin (component [A]) having two or more epoxy groups in one molecule, and one or two terminals in one molecule having the following structure: -CH(OH)-CH 2 -O-Y (In the above structure, Y represents an unfunctional aryl group.) 2. An epoxy resin composition comprising an epoxy resin in which one or two of the epoxy groups contained in one molecule of an epoxy resin (constituent element [A']) having four or more epoxy groups per molecule have undergone an addition reaction with a phenolic hydroxyl group contained in a monofunctional phenol (constituent element [B]). 3. An epoxy resin composition according to 1 or 2 above, further comprising an epoxy resin (constituent element [A']) having four or more epoxy groups per molecule and a curing agent (constituent element [C]). 4. An epoxy resin composition according to 1 above, in which the epoxy resin (constituent element [A]) is represented by any of general formulas (VI), (VII), and (VIII) described below. 5. An epoxy resin composition according to any of 2 to 4 above, in which the component [A'] accounts for 50% by mass or more and 84% by mass or less of the component and the component [A] accounts for 16% by mass or more and 50% by mass or less of the component, when the total amount of epoxy resins contained in the resin composition is taken as 100% by mass. 6. 6. The epoxy resin composition according to any one of the above 2 to 5, wherein component [B] is a hydroxyphenyl compound, a naphthol compound, or a hydroxybiphenyl compound. 7. The epoxy resin composition according to any one of the above 1 and 3 to 6, wherein the structure of Y is represented by general formula (IX), general formula (X), general formula (XI), or general formula (XII) described below. 8. The epoxy resin composition according to any one of the above 3 to 6, wherein component [C] is an aromatic polyamine.

[0008] The prepreg according to the present invention is obtained by impregnating reinforcing fibers with the epoxy resin composition according to any one of 1 to 8 above.

[0009] Furthermore, a fiber-reinforced composite material according to the present invention comprises a cured epoxy resin obtained by curing the epoxy resin composition according to any one of 1 to 8 above, and reinforcing fibers.

[0010] The method for producing an epoxy resin composition according to the present invention involves addition reaction of component [A'] and component [B] at 100 to 180°C in the presence of a curing accelerator (component [D]), followed by cooling to below 100°C and adding component [C]. [A']: epoxy resin having four or more epoxy groups per molecule; [B]: monofunctional phenol; [C]: curing agent; [D]: curing accelerator

[0011] The present invention provides an epoxy resin composition that provides a cured epoxy resin product with both an excellent elastic modulus and a low rubbery state elastic modulus under high-temperature / humid conditions. Fiber-reinforced composite materials and prepregs that use the epoxy resin composition of the present invention together with a fiber substrate exhibit excellent compressive strength and tensile properties under high-temperature / humid conditions due to the excellent properties of the epoxy resin composition.

[0012] The epoxy resin (component [A]) contained in the epoxy resin composition according to the present invention has two or more epoxy groups in one molecule, and one or two of the terminal groups in one molecule have the following structure: —CH(OH)—CH 2 -O-Y In the above structure, Y represents a non-functional aryl group. The aryl group referred to in the present invention includes the substituent represented by general formula (IX), a naphthyl group (general formula (X)), and a biphenyl group (general formula (XI)), in addition to the substituent represented by general formula (XII) containing a phenyl group, a tolyl group, a xylyl group, etc., and is preferably a substituent represented by general formula (IX) described below, a naphthyl group (general formula (X) described below), or a biphenyl group (general formula (XI) described below). Furthermore, the non-functional group refers to a group that cannot undergo an addition reaction with the epoxy groups in the epoxy resin (component [A]) described below or the component [A'] described below, or other epoxy resins. Furthermore, the epoxy resin (component [A]) preferably has five or fewer epoxy groups, more preferably four or fewer epoxy groups, per molecule. A preferred specific structure of the epoxy resin (component [A]) is as described below.

[0013] The above-mentioned epoxy resin (constituent element [A]) is preferably produced by addition reaction of one or two of the epoxy groups contained in one molecule of an epoxy resin (constituent element [A′]) having four or more epoxy groups in one molecule with a phenolic hydroxyl group contained in a monofunctional phenol (constituent element [B]).

[0014] Each of the constituent elements suitable for use in producing the epoxy resin composition of the present invention will be described in detail below. In the present invention, "aromatic" refers to a compound containing an aromatic hydrocarbon or a conjugated unsaturated heterocyclic compound in its chemical structure. Furthermore, the term "epoxy resin" may also include the above-mentioned epoxy resin (constituent element [A]). Furthermore, when the above-mentioned epoxy resin constitutes the epoxy resin composition of the present invention together with other constituent elements, the above-mentioned epoxy resin is referred to as constituent element [A].

[0015] The component [A'] used in the present invention is an epoxy resin having four or more epoxy groups per molecule. Specific examples of epoxy resins include diaminodiphenylmethane-, diaminodiphenylsulfone-, metaxylenediamine-, phenol novolac-, tetraphenylolethane-, naphthalene-, biphenyl-, and isocyanurate-type epoxy resins, as well as their halogen-substituted, alkyl-substituted, and hydrogenated derivatives. In the present invention, component [A'] contains a molecular structure in which one or two of the four or more epoxy groups per molecule have undergone an addition reaction with a phenolic hydroxyl group contained in a monofunctional phenol (component [B]) described below. This allows the cured product of the epoxy resin composition (hereinafter sometimes referred to as the cured resin product) to exhibit a high elastic modulus under high-temperature / humid conditions, despite having a structure with a low density of crosslinking points (i.e., a structure that can result in a low rubber-state elastic modulus). Note that high-temperature / humid conditions refer to both high-temperature and humid conditions. In the case of resin compositions according to conventional techniques, a low crosslink density usually means a large free volume in the cured resin, resulting in a low elastic modulus under the above conditions. However, in the case of the epoxy resin composition of the present invention, although the cured resin has a low crosslink density, the free volume that would normally be generated is filled by using residues of monofunctional phenols derived from component [B]. As a result, the cured resin does not have a low elastic modulus under high-temperature / humid conditions. That is, in at least a portion of component [A'], one or two of the four or more epoxy groups do not function as crosslinking points but rather fill the free volume in the cured resin, while the remaining epoxy groups react with component [C], the curing agent, to function as crosslinking points and ensure heat resistance. From the viewpoints of suppressing a decrease in heat resistance due to such reactions and forming a crosslinked structure with sufficient strength, it is important that component [A'] be an epoxy resin having four or more epoxy groups per molecule. It is preferable that component [A'] have six or fewer epoxy groups per molecule, because this prevents the density of crosslinking points in the cured resin from becoming too high and results in a structure with a low rubber-state elastic modulus.As described above, the epoxy resin used in the present invention can be obtained by previously adding one or two of the four or more epoxy groups in component [A'] to phenolic hydroxyl groups contained in a monofunctional phenol (component [B]). However, since this addition reaction increases the resin viscosity, from the viewpoint of moldability of the epoxy resin composition, an epoxy resin that is liquid at 20°C is preferred as component [A']. Here, "liquid at 20°C" is defined as an epoxy resin that is liquid when a metal piece with a specific gravity of 7 or more, which is at the same temperature as the epoxy resin being measured, is placed on the epoxy resin and is instantly buried under gravity. Examples of metal pieces with a specific gravity of 7 or more include iron (steel), cast iron, and copper.

[0016] In the present invention, from the viewpoint of the heat resistance and elastic modulus of the cured resin product, the epoxy equivalent of the component [A'] that can be used as a raw material is preferably 90 g / eq or more and 300 g / eq or less, and more preferably 100 g / eq or more and 200 g / eq or less. An epoxy equivalent of 300 g / eq or less is preferred because the crosslink density of the cured resin product is not too low, resulting in excellent heat resistance and elastic modulus. Furthermore, an epoxy equivalent of 90 g / eq or more is preferred because the crosslink density of the cured resin product is not too high, resulting in a low rubber-state elastic modulus.

[0017] The specific chemical structure of the component [A'] is preferably a compound represented by the following general formula (I): 2 The - or -O- group is preferable from the viewpoint of handling since the epoxy resin has a low viscosity.

[0018]

[0019] (In the above general formula (I), R 1 , R 2 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 1 , m 2are each an integer from 0 to 4. 1 or m 2 When R is 2 or more, a plurality of R 1 , R 2 may be the same or different. X is —O—, —S—, —CO—, —C(═O)O—, —SO 2 -, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-.) Examples of epoxy resins represented by the general formula (I) above include tetraglycidyl-4,4'-diaminodiphenylmethane, tetraglycidyl-3,4'-diaminodiphenylmethane, tetraglycidyl-3,3'-diaminodiphenylmethane, tetraglycidyl-4,4'-diaminodiphenyl ether, tetraglycidyl-3,4'-diaminodiphenyl ether, tetraglycidyl-3,3'-diaminodiphenyl ether, tetraglycidyl-4,4'-diaminodiphenyl sulfone, tetraglycidyl-3,4'-diaminodiphenyl sulfone, and tetraglycidyl-3,3'-diaminodiphenyl sulfone. For example, commercially available products of tetraglycidyl-4,4′-diaminodiphenylmethane can be used, such as “Sumiepoxy” (registered trademark) ELM-434 (manufactured by Sumitomo Chemical Co., Ltd.), “jER” (registered trademark) 604 (manufactured by Mitsubishi Chemical Corporation), and “Araldite” (registered trademark) MY721 (manufactured by Huntsman Advanced Materials).

[0020] In the present invention, epoxy resins other than the component [A'] and the component [A] may be contained within the scope that does not impair the effects of the invention.

[0021] The component [B] used in the present invention is a monofunctional phenol. Here, the monofunctional phenol is a phenol compound that does not have any functional groups capable of addition-reacting with the epoxy group in the component [A'] other than one phenolic hydroxyl group bonded to an aromatic ring in the molecule. By not having two or more functional groups reactive with the epoxy group in the component [A'] in one molecule, the residue of the monofunctional phenol that has undergone addition reaction with the epoxy group does not function as a crosslinking point, and the free volume in the cured product is filled, thereby exhibiting a high elastic modulus under high temperature / humid conditions. If the compound contains two or more functional groups, including the phenolic hydroxyl group, capable of addition-reacting with the epoxy group-containing functional group in the component [A'] in one molecule, these functional groups react with the component [A'] in the cured resin and function as crosslinking points, so the ability to fill the free volume in the cured product is very small, and the high elastic modulus under high temperature / humid conditions shown in the present invention is not generally exhibited.

[0022] Furthermore, the reaction between the phenolic hydroxyl group and the epoxy group typically begins at a relatively low temperature of around 100°C in the presence of the curing accelerator [D] (described below). The monofunctional phenols react with the epoxy groups of the component [A'] before volatilizing, allowing them to be incorporated into the composition as an epoxy resin. Therefore, the volatile content (mass %) during the curing process of the epoxy resin composition of the present invention is kept low compared to epoxy resin compositions using conventional epoxy resins, such as pendant epoxy resins. High volatile content during the curing process can lead to the formation of voids in the cured product, which can become the starting point for fracture and reduce the resin strength. Therefore, the volatile content is preferably as low as possible. As a guideline for the volatile content, when the epoxy resin composition is allowed to stand in a hot air oven at 160°C for 30 minutes, it is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0.2% by mass or less.

[0023] As described above, from the viewpoint of filling the free volume in the crosslinked structure in the cured product and reducing the volatile content during the curing process of the epoxy resin composition, the monofunctional phenol (component [B]) preferably has an active hydrogen equivalent derived from the phenolic hydroxyl group (equivalent to the average molecular weight, since it is a monofunctional phenol) of 100 g / eq or more and 400 g / eq or less, more preferably 120 g / eq or more and 300 g / eq or less, and even more preferably 130 g / eq or more and 260 g / eq or less. The number of aromatic rings contained in one molecule of the monofunctional phenol is not limited, but includes those having two or more aromatic rings, and among these, those having two aromatic rings are preferably used. However, the number of aromatic rings contained in one molecule may be one. Examples include hydroxyphenyl compounds, naphthol compounds, and hydroxybiphenyl compounds. Specific examples include 4-hydroxybiphenyl, 3-hydroxybiphenyl, 2-hydroxybiphenyl, α-naphthol, β-naphthol, p-cumylphenol, m-cumylphenol, o-cumylphenol, 4-phenoxyphenol, 3-phenoxyphenol, 4-benzylphenol, 3-benzylphenol, styrenated phenol, tribenzylphenol, 2,6-di-tert-butyl-4-methylphenol, 3-methyl-6-tert-butylphenol, and 2,3,6-trimethylphenol.

[0024] The hydroxyphenyl compound is preferably a compound represented by the following general formula (II) or (V), the naphthol compound is preferably a compound represented by the following general formula (III), and the hydroxybiphenyl compound is preferably a compound represented by the following general formula (IV). In particular, hydroxyphenyl compounds and naphthol compounds are preferred from the viewpoint of ease of reaction due to their excellent solubility in epoxy resins and general-purpose organic solvents. In particular, the naphthol compound represented by general formula (III) is preferred from the viewpoint of excellent room-temperature elastic modulus in the dry state of the cured resin.

[0025] In the following general formulas (II), (III), and (IV), m 3 +m 4 , m5 , m 6 +m 7 Preferably, each of m is 2 or less, 3 ~m 7 In the following general formula (V), it is preferable that at least one or all of m 8 is preferably 1 or more and 4 or less, and more preferably 2 or more and 3 or less.

[0026]

[0027] (In the above general formula (II), R 3 , R 4 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 3 is an integer from 0 to 4, and m 4 is an integer from 0 to 5. 3 or m 4 When R is 2 or more, a plurality of R 3 , R 4 may be the same or different. A is —O—, —S—, —CO—, —C(═O)O—, —SO 2 -, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-, or any of the structures represented by the formula:

[0028]

[0029] (In the above general formula (III), R 5 represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 5 is an integer from 0 to 7. 5When R is 2 or more, a plurality of R 5 may be the same or different.)

[0030]

[0031] (In the above general formula (IV), R 6 , R 7 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 6 is an integer from 0 to 4, and m 7 is an integer from 0 to 5. 6 or m 7 When R is 2 or more, a plurality of R 6 , R 7 may be the same or different.)

[0032]

[0033] (In the above general formula (V), R 8 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 8 is an integer from 0 to 5. 8 When R is 2 or more, a plurality of R 8may be the same or different.) The epoxy resin composition of the present invention preferably contains a curing agent as component [C]. The curing agent described here is a curing agent for the epoxy resin contained in the epoxy resin composition of the present invention, and is a compound having at least two active groups capable of reacting with epoxy groups in one molecule. Specific examples of curing agents include dicyandiamide, aromatic polyamines, and various acid anhydrides. By using an aromatic polyamine as a curing agent, a cured epoxy resin product with good heat resistance can be obtained. In particular, among aromatic polyamines, various isomers of diaminodiphenyl sulfone are suitable curing agents from the viewpoint of not only being able to obtain a cured epoxy resin product with good heat resistance and elastic modulus due to their rigid chemical structure, but also being able to obtain a cured epoxy resin product with good heat resistance and elastic modulus due to their electron-withdrawing functional groups, which appropriately suppress the nucleophilicity of the amine, thereby providing a good pot life in resin preparation processes and processes for producing intermediate substrates such as prepregs. Furthermore, among aromatic polyamines, compounds in which an alkyl group is substituted on the diaminodiphenylmethane skeleton are suitable curing agents from the viewpoint that the cured resin has a low water absorption rate due to the effect of the substituted alkyl group, and therefore has an excellent elastic modulus under high temperature / humid conditions.

[0034] Commercially available aromatic polyamine curing agents include Seikacure-S (manufactured by Wakayama Seika Kogyo Co., Ltd.), "JER Cure" (registered trademark) W (manufactured by Japan Epoxy Resins Co., Ltd.), and 3,3'-DAS (manufactured by Mitsui Chemicals, Inc.), "PrimaCure" (registered trademark) M-DEA (manufactured by Arcsada Japan Co., Ltd.), "PrimaCure" (registered trademark) M-DIPA (manufactured by Arcsada Japan Co., Ltd.), "PrimaCure" (registered trademark) M-MIPA (manufactured by Arcsada Japan Co., Ltd.), and "PrimaCure" (registered trademark) DETDA (manufactured by Arcsada Japan Co., Ltd.). These aromatic polyamines may be used alone or in a suitable mixture of two or more types. Furthermore, when mixed with other components, they may be in either a solid (powder) or liquid form, or a mixture of both may be used.

[0035] When used together with component [B], the preferred amount of component [C] is an amount such that the ratio of the total number of moles of active hydrogen, including the number of moles of active hydrogen in component [B] and component [C], to the number of moles of epoxy groups derived from all epoxy resins blended in the epoxy resin composition is 0.6 to 1.4 times, which is preferable from the viewpoint of obtaining a cured epoxy resin product that exhibits good mechanical properties. A molar ratio of 0.8 to 1.2 times is more preferable because it provides excellent heat resistance. A molar ratio of 1.1 to 1.5 times is preferable because it provides excellent fast-curing properties.

[0036] In the method for producing an epoxy resin composition of the present invention, it is preferable to produce the composition by blending a curing accelerator as component [D]. Specifically, component [D] can act as an accelerator for the addition reaction between the epoxy resin and a monofunctional phenol, and accelerates the reaction between component [A'] and component [B]. On the other hand, it may also accelerate the reaction between component [A'] and component [C], which is preferable. From the viewpoint of achieving both storage stability and reactivity of the epoxy resin composition, it is preferable to use at least one curing accelerator selected from the group consisting of aromatic urea compounds, imidazole derivatives, and phosphorus compounds.

[0037] Examples of the aromatic urea compound include 3-phenyl-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, toluenebisdimethylurea, etc. Commercially available aromatic urea compounds include DCMU-99 (manufactured by Hodogaya Chemical Co., Ltd.) and "Omicure" (registered trademark) 24 (manufactured by PTI Japan, Inc.).

[0038] Examples of the imidazole derivatives include 1-benzyl-2-methylimidazole, 1-benzyl-2-ethylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, etc. Commercially available imidazole derivatives include "Cureduct" (registered trademark) P-0505, 1B2MZ, 1B2PZ, 2MZ-CN, 2E4MZ-CN, and 2PZ-CN (all manufactured by Shikoku Chemicals Corporation).

[0039] Examples of the phosphorus compound include triphenylphosphine, tri-o-tolylphosphine, tris(p-methoxyphenyl)phosphine, triphenylphosphine, triphenylborane, tetraphenylphosphonium tetraphenylborate, etc. Commercially available phosphorus compounds include "Hokuko TPP" (registered trademark), "TOTP" (registered trademark), "TPP-K" (registered trademark), and "TPP-MK" (registered trademark) (all manufactured by Hokko Chemical Industry Co., Ltd.).

[0040] The content of the curing accelerator as component [D] is preferably 0.1 to 8.0 parts by mass, and more preferably 0.5 to 5.0 parts by mass, relative to 100 parts by mass of the total epoxy resin contained in the resin composition. By containing component [D] in this range, an epoxy resin composition can be obtained that has an excellent balance between storage stability and reaction rate and gives a cured resin product with excellent physical properties.

[0041] The epoxy resin composition of the present invention may also preferably contain, as component [E], a thermoplastic resin that dissolves in one of the epoxy resins constituting the composition at room temperature, dissolved in the epoxy resin, as long as the effects of the present invention are not impaired. Such a thermoplastic resin can be added to control the tackiness of the resulting prepreg, control the fluidity of the matrix resin when the prepreg is heat-cured, and impart toughness to the resulting fiber-reinforced composite material without impairing its heat resistance or elastic modulus. Preferred examples of such thermoplastic resins include thermoplastic resins having a polyaryl ether skeleton, such as polysulfone, polyphenylsulfone, polyethersulfone, polyetherimide, polyphenylene ether, polyetheretherketone, and polyetherethersulfone. These thermoplastic resins having a polyaryl ether skeleton may be used alone or in combination as appropriate. Among these, polyethersulfone and polyetherimide are preferred because they can impart toughness to the resulting fiber-reinforced composite material without impairing its heat resistance or mechanical properties.

[0042] The thermoplastic resin for component [E] may be a commercially available product. Examples include "Sumikaexcel" (registered trademark) 5003P, 5003PS, 5900P, 5400P, 5200P, 4800P, 4100P, 3600P, and 2603MP (manufactured by Sumitomo Chemical Co., Ltd.), PET, and PBT (manufactured by KDA Corporation), "J-POVAL" (registered trademark) JC-25, JM-17, and JP-03 (manufactured by Nippon Vinyl Acetate & Poval Co., Ltd.), "S-LEC" (registered trademark) BX-L, KS-1, and KS-10 (manufactured by Sekisui Chemical Co., Ltd.), "Ultrasene" (registered trademark) 515 and 530 (manufactured by Tosoh Corporation), JPH-3800 (manufactured by Johoku Chemical Industry Co., Ltd.), and YS Polystar UH130 (manufactured by Yasuhara Chemical Co., Ltd.).

[0043] The blending amount of the thermoplastic resin is preferably 1 to 50 parts by mass, based on 100 parts by mass of the total epoxy resin, from the viewpoint of ease of forming a resin film and the tackiness of a prepreg produced by impregnating a fiber substrate with the resin film, and more preferably 2 to 20 parts by mass.

[0044] When preparing a prepreg using the epoxy resin composition of the present invention as a matrix resin, the epoxy resin composition is usually heated to about 60°C to 80°C, a resin film is prepared, and the obtained resin film is impregnated into reinforcing fibers at a temperature of about 80°C to 130°C. Therefore, the viscosity of the epoxy resin composition of the present invention after being held at 80°C for 3 hours is preferably 4.0 times or less, more preferably 3.0 times or less, of the initial viscosity at 80°C. The lower limit is not particularly limited, but is usually 1.1 to 1.3 times. Here, the viscosity increase ratio after being held at 80°C for 3 hours is calculated by the viscosity (initial viscosity at 80°C) η after being held at 80°C for 1 minute. * 1 , viscosity η when kept at 80°C for 3 hours * 180 Measure η * 180 ÷η * 1 Here, viscosity refers to the complex viscosity η measured using a dynamic viscoelasticity measuring device, ARES rheometer (manufactured by TA Instruments), with a flat parallel plate having a diameter of 25 mm as the upper measuring jig and a diameter of 40 mm as the lower measuring jig, at a frequency of 0.5 Hz and a gap of 1 mm. * This refers to the following.

[0045] The viscosity increase ratio when maintained at 80°C for 3 hours can be used as an indicator of the pot life of the epoxy resin composition during the kneading process of the epoxy resin composition and the prepreg production process. That is, the smaller the viscosity increase ratio when maintained at 80°C for 3 hours, the better the pot life. When the viscosity increase ratio of an epoxy resin composition when maintained at 80°C for 3 hours is 4.0 times or less, the epoxy resin composition has high thermal stability, and a resin film with a stable resin basis weight is easily obtained in the prepreg production process, resulting in stable prepreg quality. Additionally, a good pot life prevents a decrease in the resin's impregnation into the reinforcing fibers, and reduces the occurrence of voids in the molded product.

[0046] In the present invention, the above-mentioned epoxy resin is used, and such an epoxy resin can be obtained as component [A] by reacting component [A'] with component [B] in advance, specifically by adding one or two of the four or more epoxy groups in component [A'] with phenolic hydroxyl groups contained in component [B]. By producing component [A] in advance, it becomes easy to adjust the thickening ratio of the epoxy resin composition to the above-mentioned preferred range. That is, the reaction between component [A'] and component [B] in the presence of component [D] can cause an increase in viscosity when the epoxy resin composition is maintained at 80°C for 3 hours. Therefore, for example, in the epoxy resin composition preparation process, in the absence of component [C], component [A'] and component [B] are heat-treated in advance in the presence of component [D] at a higher temperature, 100°C to 180°C, while being kneaded for 1 hour. This allows the epoxy groups and phenolic hydroxyl groups to react in advance. This makes it possible to obtain an epoxy resin (component [A]) in which component [A'] and component [B] have reacted while suppressing the viscosity increase ratio of the epoxy resin composition at 80°C. The heat treatment temperature is more preferably in the range of 100°C to 160°C, and even more preferably in the range of 100°C to 150°C. Setting the reaction temperature at 100°C or higher tends to shorten the time until the reaction is completed. On the other hand, setting the reaction temperature at 180°C or lower tends to reduce the amount of volatile components and the possibility of gelation.

[0047] In the step of preparing the epoxy resin composition, following the heat treatment, the component [C] is preferably kneaded with the other epoxy resin compositions containing the component [A] at a temperature lowered to less than 100°C, with the temperature being more preferably 90°C or lower, and even more preferably 80°C or lower. If the temperature at which the component [C] is kneaded is less than 100°C, the reaction between the component [A] and the component [C] is suppressed, thereby reducing the increase in viscosity of the epoxy resin composition during kneading. Furthermore, the lower limit of the temperature at which the component [C] is kneaded is preferably 50°C or higher. Generally, at a temperature of 50°C or higher, the viscosity of the resin composition is not excessively high, and the component [C] can be sufficiently dispersed in the epoxy resin composition by kneading.

[0048] From the viewpoint of reducing the viscosity increase ratio when maintained at 80°C for 3 hours, it is preferable that the reaction between the phenolic hydroxyl groups and the epoxy groups contained in component [B] in component [A] is completed, and that it is considered that substantially no unreacted monofunctional phenols remain in the epoxy resin composition. The absence of substantially unreacted monofunctional phenols can be determined, for example, by using a differential scanning calorimeter (DSC) to measure the exothermic peak resulting from the reaction between the epoxy groups and the phenolic hydroxyl groups when the temperature is increased from 20°C to 180°C at a rate of 5°C / min in a nitrogen atmosphere. Typically, the exothermic peak of the reaction between the epoxy groups and the phenolic hydroxyl groups is observed around 100 to 150°C, but after the heat treatment at 100 to 180°C, this exothermic peak is significantly smaller than before the heat treatment or disappears. For the reaction peak between the epoxy group and the phenolic hydroxyl group, if the ratio of the heat release amount after the heat treatment to the heat release amount before the heat treatment is 0.05 or less, the reaction rate of the phenolic hydroxyl group of the component [B] can be considered to be 95% or more, and it can be determined that there are substantially no unreacted monofunctional phenols. Another method for determining the presence or absence of unreacted monofunctional phenols is a method using HPLC measurement, which can be calculated by determining the presence or absence of a peak derived from the component [B] after the heat treatment or the ratio of the area value of the peak derived from the component [B] after the heat treatment to the area value of the peak derived from the component [B] before the heat treatment. If this ratio is 0.05 or less, it can be determined that there are substantially no unreacted monofunctional phenols.

[0049] In the epoxy resin composition of the present invention, when the total amount of epoxy resin contained in the resin composition is taken as 100% by mass, the component [A] is preferably contained in an amount of 16% by mass to 50% by mass, more preferably 19% by mass to 45% by mass, and even more preferably 22% by mass to 41% by mass. Meanwhile, the component [A'] is preferably contained in an amount of 50% by mass to 84% by mass, more preferably 55% by mass to 81% by mass, and even more preferably 59% by mass to 78% by mass. Within these ranges, the cured product of the epoxy resin composition easily exhibits excellent flexural modulus and glassy state modulus under high-temperature / humid conditions while suppressing a decrease in heat resistance. Furthermore, by including the component [A] in the epoxy resin composition of the present invention, in addition to the effect of reducing the viscosity increase ratio when maintained at 80°C for 3 hours, the composition can also exhibit the effect of excellent impregnation in the resin impregnation step of a reinforcing fiber substrate during prepreg production, while simultaneously achieving a prepreg surface tackiness suitable for the prepreg lamination step. In recent years, automated lamination has become increasingly common in prepreg lamination processes to improve production efficiency. To achieve the required surface tackiness of prepregs in these automated lamination processes, the viscosity at room temperature (20°C) where prepreg lamination is performed is generally increased by, for example, dissolving a large amount of thermoplastic resin in the epoxy resin. However, dissolving a large amount of thermoplastic resin significantly increases the viscosity at high temperatures, such as in the resin film production process (usually carried out at 60 to 80°C) and the resin impregnation process for reinforcing fiber substrates (usually carried out at 80 to 130°C). This makes it difficult to simultaneously improve the viscosity at room temperature (20°C) and reduce the viscosity in the resin impregnation process. The use of an epoxy resin composition containing component [A] of the present invention not only achieves both a high elastic modulus and a low rubber-state elastic modulus under high-temperature / humid conditions, but also significantly improves the viscosity at 20°C while slightly suppressing the increase in viscosity at 100°C relative to the viscosity of component [A'] alone. Therefore, prepregs using such epoxy resin compositions can exhibit the aforementioned resin impregnation properties and surface tackiness. Furthermore, by reacting the component [B] with the component [A'] in advance to form the component [A], there is also the advantage that the volatile content during curing of the epoxy resin composition can be further reduced.

[0050] The viscosity of an epoxy resin composition containing the above-mentioned component [A] is significantly affected by the viscosity of the component [A'] alone, and therefore, the component [A'] is preferably liquid at 20° C., and more preferably has a viscosity of 1.0 Pa s or less at 100° C. Specifically, a structure represented by general formula (I) is preferred.

[0051] As the component [A], structures represented by general formulas (VI) to (VIII) are preferred. In particular, a cured product of an epoxy resin composition using an epoxy mixture containing general formula (VI) is preferred because it is excellent in terms of heat resistance.

[0052]

[0053]

[0054]

[0055] (In the above general formulas (VI), (VII), and (VIII), Y represents a non-functional aryl group, and R 1 , R 2 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 1 , m 2 are each an integer from 0 to 4. 1 , m 2 When R is 2 or more, a plurality of R 1 , R 2 may be the same or different. X is —O—, —S—, —CO—, —C(═O)O—, —SO 2 -, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2-, -N=N-, or -N=N-.) Furthermore, the unfunctional aryl group Y in the structures of general formulas (VI) to (VIII) preferably has a formula weight of 83 g / mol to 383 g / mol, more preferably 103 g / mol to 283 g / mol, and even more preferably 113 g / mol to 243 g / mol from the viewpoints of achieving high heat resistance and reducing the rubber-state elastic modulus of the cured product. Here, the formula weight refers to the sum of the atomic weights of Y, and is generally the value obtained by subtracting the formula weight of the hydroxyl group, 17 g / mol, from the active hydrogen equivalent derived from the phenolic hydroxyl group of component [B]. Structures listed in general formulas (IX) to (XII) are preferred. In particular, epoxy resin compositions containing component [A] of general formulas (VI) to (VIII) in which Y is represented by general formula (X) are preferred from the viewpoint of achieving an excellent room-temperature elastic modulus in the dry state of the cured resin.

[0056]

[0057] (In the above general formula (IX), R 3 , R 4 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 3 is an integer from 0 to 4, and m 4 is an integer from 0 to 5. 3 or m 4 When R is 2 or more, a plurality of R 3 , R 4 may be the same or different. A is —O—, —S—, —CO—, —C(═O)O—, —SO 2 -, -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-, or any of the structures represented by the formula:

[0058]

[0059] (In the above general formula (X), R 5represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 5 is an integer from 0 to 7. 5 When R is 2 or more, a plurality of R 5 may be the same or different.)

[0060]

[0061] (In the above general formula (XI), R 6 , R 7 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 6 is an integer from 0 to 4, and m 7 is an integer from 0 to 5. 6 or m 7 When R is 2 or more, a plurality of R 6 , R 7 may be the same or different.)

[0062]

[0063] (In the above general formula (XII), R 8 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 8 is an integer from 0 to 5. 8 When R is 2 or more, a plurality of R 8may be the same or different.) In the present invention, it is also suitable to contain particles whose main component is a thermoplastic resin (hereinafter, sometimes referred to as thermoplastic resin particles). In the prepreg of the present invention, such thermoplastic resin particles do not dissolve in other components such as epoxy resin and maintain their particulate form. Furthermore, even when heated at a temperature typically used for preparing fiber-reinforced composite materials (e.g., 180°C), they do not dissolve in the fiber-reinforced composite material and maintain their particulate form. By containing such thermoplastic resin particles, when the prepreg of the present invention is laminated to prepare a fiber-reinforced composite material, the toughness of the resin layer formed between adjacent reinforcing fiber layers is improved, thereby improving impact resistance.

[0064] The resin type of the thermoplastic resin particles can be any type that can be mixed into an epoxy resin composition. Among these, polyamides are most preferred, and among polyamides, polyamide 12, polyamide 6, polyamide 11, polyamide 6 / 12 copolymers, and polyamides that have been semi-IPN (polymer interpenetrating network structure) with epoxy compounds (semi-IPN polyamides) described in Examples 1 to 7 of JP-A-2009-221460 provide particularly good adhesive strength with epoxy resins.

[0065] The shape and form of the thermoplastic resin particles may be spherical or non-spherical, and porous particles may also be used. Spherical particles are preferred in terms of shape, as they do not reduce the flow properties of the resin, have excellent viscoelasticity, have no starting points for stress concentration, and provide high impact resistance.

[0066] Commercially available polyamide particles include SP-500, SP-10, TR-1, TR-2, 842P-48, and 842P-80 (manufactured by Toray Industries, Inc.), and ORGASOL (registered trademark) 1002D, 2001UD, 2001EXD, 2002D, 3202D, 3501D, and 3502D (manufactured by Arkema Co., Ltd.). These polyamide particles may be used alone or in combination.

[0067] The epoxy resin composition of the present invention may contain a coupling agent, thermosetting resin particles, or an inorganic filler such as silica gel, carbon black, clay, carbon nanotubes, graphene, carbon particles, or metal powder, as long as the effects of the present invention are not impaired.

[0068] The prepreg of the present invention is obtained by impregnating reinforcing fibers with the epoxy resin composition of the present invention. That is, the prepreg of the present invention is obtained by using the above-described epoxy resin composition as a matrix resin and compounding this epoxy resin composition with reinforcing fibers. Preferred examples of reinforcing fibers include carbon fibers, graphite fibers, aramid fibers, and glass fibers. Of these, carbon fibers are particularly preferred. The carbon fibers preferably have a tensile modulus in the range of 200 to 440 GPa. This range is preferred because the carbon fiber reinforced composite material has a high level of balance between rigidity and strength. The tensile elongation of the carbon fibers is preferably in the range of 0.8 to 3.0%. Here, the tensile modulus and tensile elongation are values ​​measured in accordance with JIS R 7601-2006.

[0069] Commercially available carbon fibers include "TORAYCA" (registered trademark) T800G-24K, "TORAYCA" (registered trademark) T800S-24K, "TORAYCA" (registered trademark) T700G-24K, "TORAYCA" (registered trademark) T300-3K, and "TORAYCA" (registered trademark) T700S-12K (all manufactured by Toray Industries, Inc.).

[0070] The form and arrangement of the carbon fibers can be appropriately selected from unidirectionally aligned long fibers, woven fabrics, and the like. To obtain a lightweight, highly durable carbon fiber-reinforced composite material, the carbon fibers are preferably in the form of continuous fibers, such as unidirectionally aligned long fibers (fiber bundles) or woven fabrics. The prepreg of the present invention can be produced by various known methods. For example, the prepreg can be produced by a wet method in which a matrix resin is dissolved in an organic solvent to reduce its viscosity and then impregnated into the reinforcing fibers, or a hot melt method in which a matrix resin is heated to reduce its viscosity without using an organic solvent and then impregnated into the reinforcing fibers. In the wet method, the reinforcing fibers are immersed in a liquid containing the matrix resin, then removed, and the organic solvent is evaporated using an oven or the like to obtain the prepreg.

[0071] In addition, in the hot melt method, a matrix resin whose viscosity has been reduced by heating is directly impregnated into the reinforcing fibers, or a method in which the matrix resin is first coated on release paper or the like to produce a release paper sheet with a resin film, and then a resin film is placed on both sides or one side of the reinforcing fibers, and the reinforcing fibers are impregnated with the matrix resin by heating and pressurizing can be used.

[0072] The method for producing the prepreg of the present invention is preferably a hot melt method in which the matrix resin is impregnated into the reinforcing fibers without using an organic solvent, since this method results in substantially no organic solvent remaining in the prepreg.

[0073] The prepreg of the present invention has a reinforcing fiber amount per unit area of ​​30 to 2,000 g / m 2 It is preferable that the amount of reinforcing fibers is 30 g / m 2 When the amount of reinforcing fibers is 2,000 g / m or more, the number of layers to be laminated to obtain a predetermined thickness during molding of the fiber-reinforced composite material can be reduced, and the work tends to be simplified. 2 If it is less than this, the drapeability of the prepreg is likely to be improved.

[0074] The fiber mass content of the prepreg of the present invention is preferably 30 to 90% by mass, more preferably 35 to 85% by mass, and even more preferably 40 to 80% by mass. When the fiber mass content is 30% by mass or more, the amount of resin is not too large, making it easier to obtain the advantages of a fiber-reinforced composite material, such as excellent specific strength and specific modulus, and also making it less likely that the amount of heat generated during curing will be too high when the fiber-reinforced composite material is molded. Furthermore, when the fiber mass content is 90% by mass or less, poor resin impregnation is less likely to occur, and the resulting fiber-reinforced composite material is more likely to have fewer voids.

[0075] A first embodiment of the fiber-reinforced composite material of the present invention is obtained by curing the prepreg of the present invention. This fiber-reinforced composite material can be produced, for example, by laminating the prepregs of the present invention described above in a predetermined form and then applying pressure and heat to cure the resin. Examples of methods for applying heat and pressure include press molding, autoclave molding, bagging molding, tape wrapping, and internal pressure molding.

[0076] A second embodiment of the fiber-reinforced composite material of the present invention comprises a cured epoxy resin obtained by curing the epoxy resin composition of the present invention, and reinforcing fibers. This fiber-reinforced composite material can be produced by impregnating reinforcing fibers directly with the epoxy resin composition of the present invention without going through a prepreg-forming step, followed by heat curing, for example, by a molding method such as hand layup, filament winding, pultrusion, resin injection molding, or resin transfer molding.

[0077] The upper and lower limits of the above-described ranges of values ​​can be combined in any manner.

[0078] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to these examples. The unit "parts" in the composition ratios means parts by mass unless otherwise noted. Furthermore, measurements of various characteristics (physical properties) were carried out in an environment of a temperature of 23°C and a relative humidity of 50% unless otherwise noted.

[0079] <Raw materials used in the examples and comparative examples> (1) Component [A'] "Sumiepoxy" (registered trademark) ELM434 (tetraglycidyl-4,4'-diaminodiphenylmethane, manufactured by Sumitomo Chemical Co., Ltd.), epoxy equivalent: 122 g / eq, epoxy resin having four epoxy groups in one molecule 3,4'-TGDDE (tetraglycidyl-3,4'-diaminodiphenyl ether, manufactured by Toray Fine Chemical Co., Ltd.), epoxy equivalent: 106 g / eq, epoxy resin having four epoxy groups in one molecule 4,4'-TGDDE (tetraglycidyl-4,4'-diaminodiphenyl ether, manufactured by Toray Fine Chemical Co., Ltd.), epoxy equivalent: 106 g / eq, epoxy resin having four epoxy groups in one molecule (2) Epoxy resins other than component [A'] "Denacol" (registered trademark) EX-142 (o-phenylphenol glycidyl ether, manufactured by Nagase ChemteX Corporation), epoxy equivalent: 240 g / eq, monofunctional epoxy resin having one epoxy group in one molecule. TOREPA-204E (N,N-diglycidyl-p-phenoxyaniline, manufactured by Toray Fine Chemicals Co., Ltd.), epoxy resin having two epoxy groups in one molecule, epoxy equivalent: 162 g / eq, epoxy resin having two epoxy groups in one molecule. "EPICLON" (registered trademark) HP4770 (bisnaphthalene-type epoxy resin, manufactured by DIC Corporation), epoxy equivalent: 205 g / eq, epoxy resin having two epoxy groups in one molecule. (3) Component [B] p-cumylphenol (manufactured by Mitsui Chemicals Fine Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl group: 212 g / eq, hydroxyphenyl compound. β-naphthol (manufactured by Mitsui Fine Chemicals, Inc.), active hydrogen equivalent derived from phenolic hydroxyl group: 144 g / eq, naphthol compound ANTAGE SP (styrenated phenol, manufactured by Kawaguchi Chemical Industry Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl group: 308 g / eq, hydroxyphenyl compound TBP (tribenzylphenol, manufactured by Kawaguchi Chemical Industry Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl group: 348 g / eq, hydroxyphenyl compound 2,3,6-TMP (2,3,6-trimethylphenol, manufactured by Honshu Chemical Industry Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl group: 136 g / eq, hydroxyphenyl compound 3M6B (3-methyl-6-tert-butylphenol, manufactured by Honshu Chemical Industry Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl group: 164 g / eq, hydroxyphenyl compound (4) Phenols other than component [B] Bisphenol F (manufactured by Tokyo Chemical Industry Co., Ltd.), active hydrogen equivalent derived from phenolic hydroxyl group: 100 g / eq, phenol compound having two phenolic hydroxyl groups in one molecule (5) Component [C] Seikacure-S (4,4'-diaminodiphenyl sulfone, melting point 178 ° C, manufactured by Wakayama Seika Co., Ltd.), active hydrogen equivalent derived from amino group: 62 g / eq (6) Component [D] "TPP-MK" (registered trademark) (tetraphenylphosphonium tetra-p-tolylborate, manufactured by Hokko Chemical Industry Co., Ltd.) "Hokuko TPP" (registered trademark) (triphenylphosphine, manufactured by Hokko Chemical Industry Co., Ltd.) (7) Component [E] "Sumikaexcel" (registered trademark) PES2603MP (polyethersulfone, manufactured by Sumitomo Chemical Co., Ltd.) (8) Component [F] Carbon fiber "TORAYCA" (registered trademark) T800SC-24k-10E fiber (tensile strength: 5.9 GPa, tensile modulus: 294 GPa, elongation: 2.0%, manufactured by Toray Industries, Inc.)

[0080] <Various Production and Evaluation Methods> (9) Preparation of Epoxy Resin Compositions (Comparative Examples 1 to 13, Comparative Examples 15 to 22, No Heat Treatment Step for Preliminarily Reacting Constituent Element [A'] and Constituent Element [B]) In the blending ratios shown in Tables 2-1 and 2-2 (units in the tables: parts by mass), predetermined amounts of components other than constituent element [C] and constituent element [D] were added without preliminarily reacting constituent element [A'] and constituent element [B] by heat treatment, and the mixture was heated to 130°C while kneading, and then kneaded at 130°C for 30 minutes to obtain a viscous liquid. Next, the temperature was lowered to 70°C while kneading, and then predetermined amounts of constituent element [C] and constituent element [D] were added, and the mixture was further kneaded to obtain an epoxy resin composition. (10) Preparation of Epoxy Resin Compositions (Examples 1 to 25, Comparative Example 14, Heat Treatment Step for Preliminarily Reacting Component [A'] and Component [B]: Present) A viscous liquid was obtained by adding predetermined amounts of components other than component [C] to the blending ratios shown in Tables 1-1, 1-2, 1-3, and 2-2 (units in the tables: parts by mass), raising the temperature to 130°C while kneading, and then performing a heat treatment by kneading at 130°C for 1 hour. Because the epoxy groups in component [A'] used as a raw material were in excess relative to the phenolic hydroxyl groups in component [B], it is believed that it was the phenolic hydroxyl groups derived from component [B], rather than the epoxy groups, that were almost completely consumed. It can be determined that the products (Examples 1 to 25 in Tables 1-1, 1-2, and 1-3) contain substantially no unreacted component [B], and therefore the products obtained by such heat treatment are referred to as epoxy resin compositions (the "compositions after pre-heat treatment" shown in Tables 1 and 2). 1Analysis by H-NMR measurement confirmed that the product contained an epoxy resin (corresponding to component [A], particularly a structure represented by general formulas (VI) to (VIII)) in which one or two of the four or more epoxy groups in component [A'] had reacted with the phenolic hydroxyl groups of component [B]. DSC measurement was performed on the composition before and after this heat treatment from 20°C to 180°C at a heating rate of 5°C / min. The exothermic peak observed before the heat treatment, resulting from the reaction between the epoxy groups in component [A'] and the phenolic hydroxyl groups in component [B], disappeared after the heat treatment. In all Examples, the ratio of the heat release amount after the heat treatment to that before the heat treatment was 0.05 or less (the reaction rate of component [B] was 95% or more). Furthermore, the contents of component [A'] and component [A] were determined using HPLC measurement, and the results are shown in Tables 1-1, 1-2, 1-3, and 2-2.

[0081] Next, the temperature was lowered to 70°C while kneading, and then a predetermined amount of component [C] was added and further kneaded to obtain an epoxy resin composition. (11) Preparation of Epoxy Resin Compositions in Which Component [E] Was Dissolved in Component [A'] (Comparative Examples 23 to 27) Predetermined amounts of each component were added at the blending ratios shown in Table 3 (units in the table: parts by mass), and the mixture was heated to 150°C while kneading, and kneaded at 150°C for 1 hour to obtain a viscous liquid. (12) Preparation of Cured Epoxy Resin Products The epoxy resin compositions prepared according to (9) and (10) above were degassed in a vacuum, and then heated from 30°C to 180°C at a rate of 1.7°C / min in a mold set to a thickness of 2 mm using a 2 mm thick Teflon (registered trademark) spacer, and cured at 180°C for 2 hours to obtain a 2 mm thick plate-shaped cured resin product. (13) Measurement of flexural modulus of cured resin under room temperature / dry conditions Rectangular test pieces 10 mm wide and 60 mm long were cut out from the cured resin products prepared according to (12) above, and three-point bending was performed using an Instron universal testing machine (manufactured by Instron Corporation) at a span of 32 mm, a crosshead speed of 2.5 mm / min, sample number n=6, and a load range for obtaining elastic modulus of 5-30 N according to JIS K 7171 (1994). The average value of the elastic modulus was taken as the flexural modulus of the cured resin under room temperature / dry conditions. (14) Measurement of flexural modulus of cured resin under high-temperature / humid conditions: Rectangular test pieces 10 mm wide and 60 mm long were cut from the cured resin prepared according to (12) above, and immersed in boiling water at 98°C for 24 hours. After that, three-point bending was performed using an Instron universal testing machine (manufactured by Instron) under the same conditions as in (13), except that the measurement temperature was 82°C. The average value of the modulus was taken as the flexural modulus of the cured resin under high-temperature / humid conditions. A flexural modulus of 2.8 GPa or more, which is considered to be sufficient to improve the compressive strength of fiber-reinforced composite materials under high-temperature / humid conditions, was deemed to be acceptable. (15) Measurement of rubber-state modulus of cured resin: Rectangular test pieces 10 mm wide and 35 mm long were cut from the cured resin prepared according to (12) above to obtain test pieces. The storage modulus G' was measured using a bending DMA (Q800: manufactured by TA Instruments) under the conditions of a measurement frequency of 1.0 Hz, a heating rate of 5°C / min, a strain of 0.1%, and single cantilever mode, with a distance between chucks of 17.8 mm, and the temperature was raised from 30°C to 320°C.In a storage modulus change curve with log G' on the vertical axis and temperature on the horizontal axis, the temperature at the intersection of the extensions of two linear regions that can be considered as straight lines before and after the sudden drop in log G' with increasing temperature was taken as the glass transition temperature, and the rubber-state modulus was taken as G' at a temperature 50°C or more above the glass transition temperature where log G' can be considered as a flat section. The linear regions of the two regions refer to the region before the sudden drop in storage modulus with increasing temperature and the linear or nearly linear region that appears during the process of the sudden drop in storage modulus. A rubber-state modulus of 24 MPa or less, which is sufficient to improve fiber strength utilization, was considered to be acceptable. (16) Measurement of Water Absorption of Cured Resin Product Three rectangular pieces, 10 mm wide and 35 mm long, were cut out of the cured resin product prepared according to (12) above to obtain test pieces. The mass of each test piece was measured before and after immersion in boiling water at 98°C for 48 hours, and the water absorption of the cured resin was calculated using the following formula: The average value of the three test pieces was taken as the water absorption of the cured resin.

[0082] Water absorption (%) = (mass of test piece after immersion - mass of test piece before immersion) / (mass of test piece before immersion) x 100 (17) Viscosity measurement of epoxy resin composition when held at 80°C for 1 minute and 3 hours The viscosity of the epoxy resin composition was measured using a dynamic viscoelasticity analyzer ARES-G2 (manufactured by TA Instruments). Using flat parallel plates with a diameter of 25 mm as the upper measuring jig and a diameter of 40 mm as the lower measuring jig, the parallel plates were heated to 70°C, and the epoxy resin composition was placed between the upper and lower jigs so that the distance between the jigs was 1 mm. The measurement was then performed at an angular frequency of 10 rad / s. "The temperature was raised from 70°C to 80°C at a rate of 2.0°C / min, and the viscosity 1 minute after reaching 80°C" was calculated as η * 1 "The viscosity after the temperature was raised from 70°C to 80°C at a rate of 2.0°C / min and the temperature was maintained at 80°C for 3 hours" was defined as η * 180 , and the thickening factor is defined as η * 180 ÷η * 1 Here, viscosity is the complex viscosity η in dynamic viscoelasticity measurement. *(18) Measurement of volatile content of epoxy resin composition Aluminum cup (exact mass of aluminum cup is W 0 Onto the mixture, about 5 g of the epoxy resin composition prepared according to the above (8) and (9) (the exact mass of the resin composition is W 1 The aluminum cup was then placed in a hot air dryer set at 160°C for 30 minutes, and cooled to 25°C in a desiccator. The total mass W of the aluminum cup and the epoxy resin composition was then measured. 2 was measured. 2 -W 0 The mass W of the resin composition after standing at 160°C for 30 minutes was 3 The volatile content (mass%) of the epoxy resin composition was calculated using the following formula.

[0083] Volatile content (mass%) = (W 1 -W 3 ) / W 1 ×100 (19) Viscosity measurement of epoxy resin composition before kneading with component [C] at 20°C and 100°C The viscosities of the epoxy resin composition without added component [C], obtained by the preliminary heat treatment in (10) above, at 20°C and 100°C were measured using a dynamic viscoelasticity analyzer ARES-G2 (manufactured by TA Instruments). Using the same measuring jig as in (17), the epoxy resin composition was placed between the upper and lower jigs so that the distance between the jigs was 1 mm, and then the dynamic viscoelasticity was measured from 15°C to 105°C while increasing the temperature at an angular frequency of 10 rad / s and a rate of 2.0°C / min, and the viscosities at 20°C and 100°C were determined. (Examples 1 to 25, Comparative Examples 1 to 22) Epoxy resin compositions were prepared according to the blending ratios in Tables 1-1, 1-2, 1-3, 2-1, and 2-2 by the procedure (9) or (10) above, and cured resin products were obtained by the procedure (12) above. The epoxy resin compositions were subjected to the measurements described in (17) and (18), and the cured epoxy resin products were subjected to the measurements described in (13) to (16).

[0084] The results of various measurements are shown in Tables 1-1, 1-2, 1-3, 2-1 and 2-2.

[0085]

[0086]

[0087]

[0088]

[0089]

[0090] Examples 1 to 25, Comparative Examples 1 to 8, 15 to 22: The cured resin products of the epoxy resin compositions containing the epoxy resin (component [A]) according to the present invention exhibit both an excellent flexural modulus of 2.8 GPa or more under high-temperature / humid conditions and an excellent rubbery-state modulus of 24 MPa or less, and are superior in terms of viscosity increase after 3 hours at 80°C and volatile content compared to Comparative Examples 1 to 8 and 15 to 22. In particular, as can be seen from Example 8, when the epoxy resin is prepared using a phenol containing a naphthalene ring as component [B], the flexural modulus under room temperature / dry conditions is excellent. Comparative Examples 9 to 12: These compositions contain the same types of components [A'], [C], and [D] as Examples 1 to 25, but do not contain component [A]. Compared to Comparative Example 9, Comparative Examples 11 and 12 showed improvements in the flexural modulus and rubbery-state modulus under high-temperature / humid conditions, but the reduction in the rubbery-state modulus was insufficient. Comparative Example 13 This composition contains the same types of components [A'], [C], and [D] as in Examples 1 to 25, but does not contain component [A]. This composition also uses "Denacol" (registered trademark) EX-142 (a monofunctional epoxy resin having one epoxy group in the molecule) as an epoxy resin other than component [A'], and aims to reduce the free volume in the cured product. However, this resin composition has a very high volatile content during the curing process, and it was determined that it was not worthy of evaluation of resin physical properties. It can be understood that EX-142 volatilized during the curing process because the reaction between the epoxy group of EX-142 and the active hydrogen in the amine contained in component [C] was slow. This suggests that an epoxy resin (component [A]) in which one or two epoxy groups of component [A'] have reacted with phenolic hydroxyl groups of component [B] is important as a monofunctional component that fills the free volume in the cured resin. Comparative Example 14 This composition contains the same components [A'], [C], and [D] as in Examples 1 to 25, but does not contain component [B], and contains bisphenol F (a phenolic compound having two phenolic hydroxyl groups in one molecule) as a phenol other than component [B]. Neither the improvement in flexural modulus under high temperature / humid conditions nor the reduction in rubbery state modulus is sufficient.In the case of bisphenol F, it is clear that even if it is incorporated into the epoxy resin crosslinked structure, it does not have the function of filling the free volume and ends up increasing the crosslink density. (Examples 1 to 5, 7 to 18, 20 to 23, Comparative Examples 23 to 27) Epoxy resin compositions were prepared according to the blending ratios in Tables 1-1, 1-2, 1-3, 2-1, 2-2, and 3 in the procedures (10) and (11) above, and viscosity measurements were carried out according to the procedure (19) above.

[0091] The results of various measurements are shown in Tables 1-1, 1-2, 1-3, 2-1, 2-2, and 3.

[0092]

[0093] Examples 1 to 25 The epoxy resin composition prepared by reacting the components [A'] and [B] in advance contains the component [A]. 1 This was confirmed by H-NMR measurement and HPLC measurement. By including component [A], the compositions after the pre-heat treatment in Examples 1 to 5, 7 to 18, and 20 to 23 had a viscosity at 100°C of about 1.7 to 10 times or less compared to the epoxy resin composition in Comparative Example 23, while the viscosity at 20°C was about 6 to 10 times higher. 42 times, i.e., it is an epoxy resin composition with an extremely large viscosity change with temperature change. When component [C] is added to this pre-heat-treated composition, the resulting cured epoxy resin composition not only exhibits an excellent improvement in flexural modulus under high-temperature / humid conditions and a reduction in rubber-state modulus, but also provides an epoxy resin composition with excellent resin impregnation into fiber substrates during prepreg preparation and excellent prepreg surface tackiness at room temperature, making this a preferred embodiment. <Comparative Examples 23 to 27> Comparative Examples 24 to 27 show mixtures in which component [E] (thermoplastic resin) is dissolved in component [A'] to increase the viscosity at 20°C. It can be seen that by blending the thermoplastic resin, the 20°C viscosity increases by about 3 to 18 times, while the 100°C viscosity increases by about 3 to 12 times, compared to Comparative Example 23. Because the viscosity change with temperature is small, it can be seen that it is difficult to achieve an epoxy resin composition that combines excellent resin impregnation into fiber substrates during prepreg preparation and excellent prepreg surface tackiness at room temperature simply by dissolving a thermoplastic resin in an epoxy resin.

Claims

1. An epoxy resin composition containing an epoxy resin (component [A]) having two or more epoxy groups in one molecule, and one or two of the terminals in one molecule having the following structure: -CH(OH)-CH 2 -O-Y (In the above structure, Y represents a non-functional aryl group.) 2. An epoxy resin composition comprising an epoxy resin in which one or two of the epoxy groups contained in one molecule of an epoxy resin (constituent element [A']) having four or more epoxy groups in one molecule have undergone an addition reaction with a phenolic hydroxyl group contained in a monofunctional phenol (constituent element [B]).

3. The epoxy resin composition according to claim 1 or 2, further comprising an epoxy resin having four or more epoxy groups in one molecule (component [A']) and a curing agent (component [C]).

4. The epoxy resin composition according to claim 1, wherein the epoxy resin (component [A]) is represented by any one of general formulas (VI), (VII) and (VIII). (In the above general formulas (VI), (VII), and (VIII), Y represents a non-functional aryl group, R 1 , R 2 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 1 , m 2 Each is an integer from 0 to 4. 1 , m 2 When R is 2 or more, multiple R 1 , R 2 may be the same or different. X is -O-, -S-, -CO-, -C(=O)O-, -SO 2 --, --CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-, or any of the structures represented by the formula:

5. An epoxy resin composition according to claim 3, comprising 50% by mass or more and 84% by mass or less of component [A'] and 16% by mass or more and 50% by mass or less of component [A], when the total amount of epoxy resins contained in the resin composition is taken as 100% by mass.

6. The epoxy resin composition according to claim 2, wherein the component [B] is a hydroxyphenyl compound, a naphthol compound or a hydroxybiphenyl compound.

7. The epoxy resin composition according to claim 1, wherein the structure of Y is represented by general formula (IX), general formula (X), general formula (XI) or general formula (XII). (In the above general formula (IX), R 3 , R 4 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 3 is an integer from 0 to 4, m 4 is an integer from 0 to 5. 3 Or m 4 When R is 2 or more, multiple R 3 , R 4 may be the same or different. A is -O-, -S-, -CO-, -C(=O)O-, -SO 2 --, --CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 -, -N=N-, or any of the structures represented by the formula: (In the above general formula (X), R 5 represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 5 is an integer from 0 to 7. 5 When R is 2 or more, multiple R 5 may be the same or different.) (In the above general formula (XI), R 6 , R 7 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 6 is an integer from 0 to 4, m 7 is an integer from 0 to 5. 6 Or m 7 When R is 2 or more, multiple R 6 , R 7 may be the same or different.) (In the above general formula (XII), R 8 Each of m represents at least one selected from the group consisting of an aliphatic hydrocarbon group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, an aromatic hydrocarbon group having 6 to 10 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, an acyl group, a trifluoromethyl group, a nitro group, a cyano group, a phenyl group, and a halogen atom. 8 is an integer from 0 to 5. 8 When R is 2 or more, multiple R 8 may be the same or different.) 8. The epoxy resin composition according to claim 3, wherein the component [C] is an aromatic polyamine.

9. A prepreg obtained by impregnating reinforcing fibers with the epoxy resin composition according to claim 1 or 2.

10. A fiber-reinforced composite material comprising a cured epoxy resin obtained by curing the epoxy resin composition according to claim 1 or 2, and reinforcing fibers.

11. A method for producing an epoxy resin composition, comprising subjecting component [A'] and component [B] to an addition reaction at 100°C to 180°C in the presence of a curing accelerator (component [D]), then lowering the temperature to less than 100°C and adding component [C]. [A']: Epoxy resin having 4 or more epoxy groups in one molecule [B]: Monofunctional phenol [C]: Curing agent [D]: Curing accelerator

Citation Information

Patent Citations

  • Polyamide fine particle, prepreg, and carbon fiber-reinforced composite material

    JP2009221460A

  • Epoxy resin composition for fiber-reinforced composite material, prepreg, and fiber-reinforced composite material

    WO2010109929A1

  • Epoxy resin composition, prepreg and fiber-reinforced composite material

    WO2018159574A1

  • Epoxy resin composition, prepreg, and fiber reinforced composite material

    WO2020058766A1

  • Preparation method of epoxy curing agent

    CN108727564A