Fluorine-containing ether compound, lubricant for magnetic recording medium, and magnetic recording medium
The use of a fluorine-containing ether compound with a perfluoropolyether chain and terminal polar groups addresses the challenges of corrosion resistance and spin-off in magnetic recording media, ensuring durable and reliable performance even with thinner lubricant layers.
Patent Information
- Application Number
- PCT/JP2024/015067
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-16
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional magnetic recording media lubricants face challenges in achieving sufficient corrosion resistance and preventing spin-off when the lubricant layer thickness is reduced, leading to decreased durability and recording performance.
A fluorine-containing ether compound with a perfluoropolyether chain and terminal groups containing 1 to 4 polar groups, including a 1,2-diol structure, is used to form a lubricant layer that enhances adhesion and intermolecular interactions, improving corrosion resistance and spin-off resistance while maintaining hydrophobicity.
The fluorine-containing ether compound effectively forms a lubricant layer with excellent corrosion resistance and spin-off suppression, even at reduced thickness, enhancing the durability and reliability of magnetic recording media.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Fluorine-containing ether compound, lubricant for magnetic recording medium, and magnetic recording medium
[0001] The present invention relates to a fluorine-containing ether compound, a lubricant for a magnetic recording medium, and a magnetic recording medium. This application claims priority to Japanese Patent Application No. 2023-074981, filed on April 28, 2023, the contents of which are incorporated herein by reference.
[0002] In order to improve the recording density of magnetic recording and reproducing devices, development of magnetic recording media suitable for high recording densities is progressing. Conventional magnetic recording media include those in which a recording layer is formed on a substrate and a protective layer, such as carbon, is formed on the recording layer. The protective layer protects the information recorded on the recording layer and improves the sliding properties of the magnetic head. However, simply providing a protective layer on the recording layer does not ensure sufficient durability of the magnetic recording medium. For this reason, a lubricant is generally applied to the surface of the protective layer to form a lubricating layer.
[0003] Examples of lubricants used in forming the lubricating layer of a magnetic recording medium include -CF 2 It has been proposed to use a fluorine-based polymer having a repeating structure containing -, which contains a compound having a polar group such as a hydroxyl group or an amino group at the end thereof.
[0004] For example, Patent Documents 1 and 2 disclose a method for producing a perfluoropolyether having methylene groups (-CH 2 a glycerin linking group (—O—CH 2 -CH(OH)-CH 2 The document discloses a fluorine-containing ether compound in which a terminal group, which is an organic group having a polar group, is bonded in this order.
[0005] Patent Document 3 describes a method for producing a perfluoropolyether having methylene groups (-CH) at both ends of the perfluoropolyether chain. 2 A structure in which the glycerin linking group is increased in carbon through (—O—CH 2 -CH(OH)-CH 2 - (CH 2 ) n A fluorine-containing ether compound is disclosed in which a linking group containing —O—) and a terminal group are bonded in this order.
[0006] Patent Document 4 describes a method for producing a perfluoropolyether having methylene groups (-CH) at both ends of the perfluoropolyether chain. 2 The present invention discloses a fluorine-containing ether compound having one or more glycerin structures bonded thereto via a hydroxyl group.
[0007] International Publication No. 2021 / 090940 (A) Japanese Patent No. 6804893 (B) International Publication No. 2019 / 054148 (A) International Publication No. 2009 / 013785 (A)
[0008] In recent years, in order to increase the capacity of magnetic recording media, there has been a demand for further reduction in magnetic spacing (the distance between the magnetic head and the magnetic layer of the magnetic recording medium), which has led to a demand for thinner lubricating layers in magnetic recording media.
[0009] However, generally, reducing the thickness of the lubricating layer tends to reduce the corrosion resistance of the magnetic recording medium. Furthermore, if spin-off (a phenomenon in which the lubricant scatters or evaporates due to centrifugal force and heat generated by the rotation of the magnetic recording medium) occurs when the thickness of the lubricating layer is reduced, it may become impossible to maintain a film thickness sufficient to fulfill the function of the lubricating layer. For this reason, there is a demand for a lubricating layer that has excellent corrosion resistance and can suppress spin-off even when the thickness of the lubricating layer is reduced.
[0010] The present invention has been made in view of the above circumstances, and aims to provide a fluorine-containing ether compound that has excellent corrosion resistance, can form a lubricating layer that can suppress spin-off, and can be suitably used as a material for a lubricant for a magnetic recording medium.
[0011] An object of the present invention is to provide a lubricant for magnetic recording media which contains the fluorine-containing ether compound of the present invention and is capable of forming a lubricating layer which has good corrosion resistance and is capable of suppressing spin-off.
[0012] An object of the present invention is to provide a magnetic recording medium that has a lubricating layer containing the fluorinated ether compound of the present invention, has good corrosion resistance, and is capable of suppressing spin-off.
[0013] The present invention includes the following aspects.
[0014] [1] A fluorine-containing ether compound represented by the following formula (1): 1 -CH 2 -R 2 -CH 2 -R 3 (1) (In formula (1), R 2 is a perfluoropolyether chain. 1 and R 3 is a terminal group having 1 to 4 polar groups and 1 to 50 carbon atoms. 1 and R 3 may be the same or different from each other. 1 and R 3 At least one of the groups is a terminal group represented by the following formula (2): —O—X—CH(OH)—CH 2 OH (2) (In formula (2), X is a divalent organic group having 2 to 30 carbon atoms which may contain at least one of 1 to 2 polar groups and 1 to 3 ether oxygen atoms. X contains at least one carbon atom which is not bonded to either a polar group or an ether oxygen atom.)
[0015] [2] The fluorine-containing ether compound according to [1], wherein the terminal group represented by the formula (2) is any one of the following formulae (2-1) to (2-7):
[0016] (In formula (2-1), a represents an integer of 1 to 8. b represents an integer of 1 to 7.) (In formula (2-2), c represents an integer of 1 to 7.) (In formula (2-3), d represents an integer of 1 to 6.) (In formula (2-4), e represents an integer of 1 to 6. e R a and R b each independently represents a hydrogen atom or a methyl group.) (In formula (2-5), f represents an integer of 1 to 6.) (In formula (2-6), g represents an integer of 1 to 6.) (In formula (2-7), g2 represents an integer of 1 to 6.)
[0017] [3] R in the formula (1) 1 and R 3 and each independently represent a terminal group represented by formula (2).
[0018] [4] R in the formula (1) 1 and R 3 The fluorine-containing ether compound according to any one of [1] to [3], wherein
[0019] [5] R in the formula (1) 1 and R 3 one of which is an end group represented by the formula (2), and the other is an end group represented by the following formula (3) and does not fall under formula (2):
[0020] (In formula (3), l represents an integer of 1 to 3. l m's each independently represent an integer of 1 to 6. l n's each independently represent an integer of 1 to 6. In one repeating unit, at least one of m and n is 1. B represents an alkyl group which may have only one polar group, an organic group containing a carbon-carbon unsaturated bond, or a hydrogen atom.)
[0021] [6] R in the formula (1) 1 and R 3 one of which is an end group represented by the formula (2), and the other is an end group represented by any one of the following formulas (3-1) to (3-3):
[0022] (In formula (3-1), p represents an integer of 0 to 3. q represents an integer of 0 to 2. r represents an integer of 0 to 5. The total value of p and r is 1 to 5. D represents a polar group, a vinyl group, an ethynyl group, or an aryl group which may have a substituent.) (In formula (3-2), s represents an integer of 0 to 2. t represents an integer of 1 to 5.) (In formula (3-3), u represents an integer of 1 to 3. Each of the five E's independently represents a polar group, an alkoxy group having 1 to 8 carbon atoms, a halogeno group, or a hydrogen atom. However, when a polar group is included in the five E's, the number of polar groups among the five E's is 1.)
[0023] [7] R in the formula (1) 1 and R 3 The fluorine-containing ether compound according to any one of [1] to [6], wherein the total number of polar groups is 4 to 6.
[0024] [8] R in the formula (1) 2 is a perfluoropolyether chain represented by the following formula (4): 2 ) w1 -O-(CF 2 O) w2 -(CF 2 CF 2 O) w3 -(CF 2 CF 2 CF 2 O) w4 -(CF 2 CF 2 CF 2 CF 2 O) w5 -(CF 2 ) w6 - (4) (In formula (4), w2, w3, w4, and w5 represent the average degree of polymerization, and each independently represents 0 to 20. However, w2, w3, w4, and w5 cannot all be 0 at the same time. w1 and w6 are CF 2 The repeating units in formula (4) are (CF 2 O), (CF 2 CF 2 O), (CF 2 CF 2 CF 2 O), (CF 2 CF 2 CF 2 CF 2 There are no particular restrictions on the arrangement order of O).
[0025] [9] R in the formula (1) 2 is any one selected from perfluoropolyether chains represented by the following formulas (4-1) to (4-4): 2 -(OCF 2 CF 2 ) h -(OCF 2 ) i -OCF 2- (4-1) (In formula (4-1), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.) -CF 2 CF 2 -(OCF 2 CF 2 CF 2 ) j -OCF 2 CF 2 - (4-2) (In formula (4-2), j represents the average degree of polymerization and represents 1 to 15.) -CF 2 CF 2 CF 2 -(OCF 2 CF 2 CF 2 CF 2 ) k -OCF 2 CF 2 CF 2 - (4-3) (In formula (4-3), k represents the average degree of polymerization and represents 1 to 10.) - (CF 2 ) w7 -O-(CF 2 CF 2 CF 2 O) w8 -(CF 2 CF 2 O) w9 -(CF 2 ) w10 - (4-4) (In formula (4-4), w8 and w9 represent the average degree of polymerization, each independently representing 1 to 20. w7 and w10 represent CF 2 is an average value representing the number of
[0026]
[10] The fluorinated ether compound according to any one of [1] to [9], which has a number average molecular weight in the range of 500 to 10,000.
[0027]
[11] A lubricant for magnetic recording media, comprising the fluorine-containing ether compound according to any one of [1] to
[10] .
[0028]
[12] A magnetic recording medium comprising at least a magnetic layer, a protective layer, and a lubricating layer formed in this order on a substrate, wherein the lubricating layer contains the fluorine-containing ether compound according to any one of [1] to
[10] .
[0029]
[13] The magnetic recording medium according to
[12] , wherein the lubricating layer has an average film thickness of 0.5 nm to 2.0 nm.
[0030] The fluorine-containing ether compound of the present invention is a compound represented by the above formula (1), and is therefore suitable as a material for a lubricant for a magnetic recording medium.
[0031] The lubricant for magnetic recording media of the present invention contains the fluorine-containing ether compound of the present invention, and therefore can form a lubricating layer that has good corrosion resistance and can suppress spin-off.
[0032] The magnetic recording medium of the present invention has a lubricating layer containing the fluorine-containing ether compound of the present invention. Therefore, the magnetic recording medium of the present invention has good corrosion resistance, can suppress spin-off, and is excellent in reliability and durability. Therefore, the magnetic recording medium of the present invention can have a thinner lubricating layer, which can contribute to reducing magnetic spacing and further reduce the flying height of the magnetic head.
[0033] 1 is a schematic cross-sectional view showing an embodiment of a magnetic recording medium of the present invention.
[0034] The present inventors have conducted extensive research to solve the above problems, as described below. Conventionally, fluorine-containing ether compounds having a terminal group containing a polar group such as a hydroxyl group have been preferably used as materials for lubricants for magnetic recording media (hereinafter sometimes abbreviated as "lubricants") that are applied to the surface of protective layers.
[0035] However, when a thin lubricating layer is formed on a protective layer using a conventional fluorine-containing ether compound having a terminal group containing a polar group, it is difficult to realize a lubricating layer that has good corrosion resistance and can suppress spin-off, as shown below. That is, the polar group in the fluorine-containing ether compound bonds with the active site on the protective layer, improving the adhesion of the lubricating layer to the protective layer. If the adhesion of the lubricating layer to the protective layer is insufficient, the lubricating layer will not cover the protective layer properly, and water, which causes corrosion, will be easily absorbed into the protective layer, resulting in insufficient corrosion resistance.
[0036] In addition, the polar groups in the fluorine-containing ether compound not only bond with the active sites on the protective layer and participate in the interaction with the protective layer, but also participate in intramolecular and intermolecular interactions. If the polar groups participating in the intermolecular interactions between fluorine-containing ether compounds are insufficient, the fluorine-containing ether compound in the lubricating layer will easily scatter as the magnetic recording medium rotates, making spin-off more likely to occur.
[0037] Therefore, the fluorine-containing ether compound must contain a sufficient number of polar groups that are involved in the interaction with the protective layer and intermolecular interactions so as to form a lubricating layer that has good corrosion resistance and is suppressed from spin-off. However, if the number of polar groups in the fluorine-containing ether compound is increased, the hydrophobicity of the lubricating layer containing it will decrease, and sufficient corrosion resistance will not be obtained.
[0038] Therefore, the present inventors conducted extensive research focusing on the strength of polar groups contained in fluorinated ether compounds and the interactions between polar groups. As a result, they concluded that it would be sufficient if at least a portion of the polar groups in the fluorinated ether compound were hydroxyl groups of a 1,2-diol structure located at the end of the perfluoropolyether chain. In this case, as shown below, it is possible to ensure hydroxyl groups that can interact with the protective layer and hydroxyl groups that can participate in intermolecular interactions while suppressing the decrease in hydrophobicity caused by the hydroxyl groups contained in the 1,2-diol structure.
[0039] 1,2-diol structure (-CH(OH)-CH 2 In the 1,2-diol structure (OH), the carbon atoms to which the hydroxyl groups are bonded are bonded, so the distance between the hydroxyl groups is short, and steric and electrostatic repulsion between the hydroxyl groups is likely to occur. For this reason, the two hydroxyl groups contained in the 1,2-diol structure are in an opposite conformation to the carbon atoms to which they are bonded in the 1,2-diol structure. Therefore, the dipole moments generated by the two hydroxyl groups contained in the 1,2-diol structure cancel each other out, and an increase in the polarity of the entire fluorine-containing ether compound molecule is suppressed.
[0040] Furthermore, the distance between active sites on the protective layer is sufficiently greater than the distance between hydroxyl groups contained in the 1,2-diol structure. Moreover, the two hydroxyl groups contained in the 1,2-diol structure are in the opposite conformation with respect to the carbon atom to which the 1,2-diol structure is bonded. Therefore, the two hydroxyl groups contained in the 1,2-diol structure are not simultaneously oriented toward the protective layer, and only one of the two hydroxyl groups can interact with the active site on the protective layer. Therefore, the other of the two hydroxyl groups can participate in the intermolecular interaction between the fluorine-containing ether compounds.
[0041] In the past, the structure of fluorine-containing ether compounds used in lubricants has been studied so that as many polar groups as possible in the compound are positioned to easily interact with the active sites on the protective layer in order to improve adhesion to the protective layer. Therefore, structures in which the carbon atoms to which hydroxyl groups are bonded are bonded, resulting in adjacent hydroxyl groups having opposite conformations on the protective layer, have tended to be avoided. However, the present inventors deliberately made some of the polar groups in the fluorine-containing ether compound hydroxyl groups of a 1,2-diol structure, thereby ensuring polar groups that can participate in intermolecular interactions between fluorine-containing ether compounds. Based on this, they considered it possible to adjust the number of polar groups that can interact with the active sites on the protective layer as needed.
[0042] Furthermore, the present inventors have conducted extensive research into fluorine-containing ether compounds having 1,2-diol structures at one or both ends of a perfluoropolyether chain to improve the corrosion resistance of a lubricating layer containing the compound and suppress spin-off. As a result, they have found that a fluorine-containing ether compound in which terminal groups having 1 to 50 carbon atoms and 1 to 4 polar groups are located at both ends of the perfluoropolyether chain, at least one of the two terminal groups contains at least one carbon atom that is not bonded to either a polar group or an ether oxygen atom, and is an terminal group represented by formula (2) having a 1,2-diol structure, is sufficient, and have arrived at the present invention.
[0043] In such a fluorinated ether compound, the number of polar groups is appropriate, and some of the polar groups are hydroxyl groups of a 1,2-diol structure located at the terminals of the perfluoropolyether chain. This prevents a decrease in hydrophobicity due to the polar groups, while ensuring sufficient hydroxyl groups capable of interacting with the protective layer and participating in intermolecular interactions. Furthermore, the terminal group represented by formula (2) located at at least one terminal contains at least one carbon atom that is not bonded to either a polar group or an ether oxygen atom. This carbon atom has extremely low affinity for water, strongly impeding the interaction between the fluorinated ether compound molecule and water. Therefore, sufficient hydrophobicity can be achieved even if multiple polar groups are contained in the fluorinated ether compound. Furthermore, the restricted movement of this carbon atom imparts appropriate rigidity to the fluorinated ether compound molecule, suppressing intramolecular interactions between polar groups and making the polar groups more likely to participate in intermolecular interactions between fluorinated ether compounds.
[0044] Thus, the above-mentioned fluorine-containing ether compound can maintain low polarity while ensuring the number of polar groups involved in the interaction with protective layer, and has sufficient hydrophobicity.Therefore, the lubricant containing it is less likely to absorb water that causes corrosion, and has excellent corrosion resistance.In addition, the above-mentioned fluorine-containing ether compound can easily generate polar groups that are not involved in the interaction with protective layer or the interaction within a molecule, and the polar groups can easily form intermolecular interactions.Therefore, the fluorine-containing ether compound is less likely to scatter when magnetic recording medium rotates, and can form a lubricating layer that is excellent in spin-off resistance.
[0045] On the other hand, for example, if the fluorine-containing ether compound is too flexible, the polar groups contained in the fluorine-containing ether compound tend to form intramolecular interactions, making it difficult for the polar groups to participate in intermolecular interactions. Furthermore, if all of the multiple polar groups contained in the fluorine-containing ether compound are arranged with a sufficient distance between adjacent polar groups, all of the polar groups tend to participate in interactions with the protective layer, making it difficult to obtain sufficient interactions between the fluorine-containing ether compounds due to the polar groups.
[0046] Furthermore, the present inventors have confirmed that by using a lubricant containing the above-mentioned fluorine-containing ether compound, it is possible to form a lubricating layer that has good corrosion resistance and can suppress spin-off even when the thickness is thin, and have arrived at the present invention.
[0047] The fluorine-containing ether compound, the lubricant for a magnetic recording medium, and the magnetic recording medium of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments.
[0048] [Fluorine-containing ether compound] The fluorine-containing ether compound of the present embodiment is represented by the following formula (1): 1 -CH 2 -R 2 -CH 2 -R 3 (1) (In formula (1), R 2 is a perfluoropolyether chain. 1 and R 3 is a terminal group having 1 to 4 polar groups and 1 to 50 carbon atoms. 1 and R 3 may be the same or different from each other. 1 and R 3 At least one of the groups is a terminal group represented by the following formula (2): —O—X—CH(OH)—CH 2 OH (2) (In formula (2), X is a divalent organic group having 2 to 30 carbon atoms which may contain at least one of 1 to 2 polar groups and 1 to 3 ether oxygen atoms. X contains at least one carbon atom which is not bonded to either a polar group or an ether oxygen atom.)
[0049] The fluorine-containing ether compound of the present embodiment is, as represented by formula (1), 2 One end of the skeleton of a perfluoropolyether chain (hereinafter sometimes referred to as a PFPE chain) is connected via a methylene group to R 1 and the other end of the skeleton is connected via a methylene group to an end group represented by R 3 The terminal group shown in is attached.
[0050] (R 1 and R3 Terminal group represented by R 1 and R 3 is a terminal group having 1 to 4 polar groups and 1 to 50 carbon atoms. 1 and R 3 At least one of the groups is a terminal group represented by the above formula (2).
[0051] R 1 and R 3 is a terminal group that does not fall under formula (2), R 1 and R 3 The number of polar groups contained in the terminal groups that do not fall under formula (2) among the above is one or more. In addition, the number of polar groups contained in the terminal groups represented by formula (2) is two or more. Therefore, when a lubricating layer is formed on a protective layer using a lubricant containing a fluorine-containing ether compound, a favorable interaction occurs between the lubricating layer and the protective layer. R 1 and R 3 The number of polar groups contained in each of R is preferably two or more. 1 and R 3 When the number of polar groups contained therein is two or more, the fluorine-containing ether compound has excellent adhesion to the protective layer, and furthermore, intermolecular interactions between the polar groups are suitably formed, thereby enabling the formation of a lubricating layer that can suppress spin-off.
[0052] R 1 and R 3 The number of polar groups contained in each of R is 4 or less. Therefore, in a lubricating layer containing a fluorine-containing ether compound, the polarity of the fluorine-containing ether compound is too high, and the fluorine-containing ether compound aggregates to form lumps, which causes the lubricating layer to lose its smoothness. 1 and R 3 The number of polar groups contained in each of R is preferably 3 or less. 1 and R 3 When the number of polar groups contained in each of the above is 3 or less, the hydrophilicity of the fluorine-containing ether compound becomes too high, which can prevent water, which causes corrosion, from being taken into the magnetic recording medium, and the fluorine-containing ether compound can form a lubricating layer with high corrosion resistance.
[0053] R in formula (1)1 and R 3 The total number of polar groups contained in R is preferably 3 to 6, and more preferably 4 to 6. When the total number of polar groups is 3 or more, R 1 and R 3 The interaction between the polar group and the protective layer is effectively obtained. As a result, a fluorine-containing ether compound can be obtained that can form a lubricating layer with high adhesion to the protective layer. Therefore, a lubricating layer with better spin-off resistance can be obtained. Furthermore, if the total number of polar groups is 6 or less, the polarity of the fluorine-containing ether compound is too high, which can prevent the fluorine-containing ether compound from taking in water, which causes corrosion. Therefore, a lubricating layer with better corrosion resistance can be formed.
[0054] R 1 and R 3 The polar groups contained in each of R may be the same in part or in whole, or may be different from each other. 1 The number of polar groups in R 3 The number of polar groups in R may be the same or different. 1 The number of polar groups in R 3 and the number of polar groups therein are preferably the same, since this results in a more uniform coating state of the fluorine-containing ether compound on the protective layer and allows the formation of a lubricating layer with better adhesion.
[0055] R 1 and R 3 The polar groups contained in the hydroxyl group (-OH), carboxyl group (-COOH), formyl group (-(C=O)H), carbonyl group (-(C=O)R 7 ;R 7 is an organic group, a sulfo group (-SO 3 H), a cyano group (—CN), and a group having an amide bond (—NR 8 COR 9 or -CONR 10 R 11 ;R 8 , R 9 , R 10 and R 11 are each independently a hydrogen atom or an organic group; an amino group (—NR 12 R13 ;R 12 and R 13 are each independently a hydrogen atom or an organic group.) The group having an amide bond is preferably a group bonded at a carbon atom constituting the amide bond as shown in the above formula (for example, a carboxamide group (-C(=O)NH 2 )) and a group bonding at a nitrogen atom constituting an amide bond (for example, an acetamide group (—NHC(═O)CH 3 In the group having an amide bond, the R 8 and R 9 may be bonded to each other to form a ring, 10 and R 11 may be bonded to each other to form a ring. 8 , R 9 , R 10 and R 11 are preferably each independently selected from the group consisting of a hydrogen atom, a methyl group, an ethyl group, a propyl group, and a butyl group. In this specification, the term "polar group" does not include a halogeno group (such as -F, -Cl, or -Br) or an ether bond (-O-).
[0056] R 1 and R 3 Preferably, each independently contains at least one polar group selected from the group consisting of a hydroxyl group, a cyano group, and a group having an amide bond. This is because the hydroxyl group, the cyano group, and the group having an amide bond are chemically stable, and the lubricating layer containing the fluorine-containing ether compound having these polar groups will not deteriorate over the long term. In addition, the hydroxyl group, the cyano group, and the group having an amide bond are not too acidic and will not corrode the substrate.
[0057] R in formula (1) 1 and R 3 Each of the polar groups R preferably contains at least one hydroxyl group. 1 and R 3 It is more preferable that all of the polar groups in R are hydroxyl groups. 1 and R 3When all of the polar groups of are hydroxyl groups, the fluorine-containing ether compound can be more uniformly coated on the protective layer.
[0058] R 1 and R 3 The number of carbon atoms in the terminal group represented by R is 1 to 50, preferably 3 to 20, and more preferably 4 to 15. 1 and R 3 When the number of carbon atoms in the terminal group represented by R is 1 or more, the hydrophobicity of the terminal group can be ensured, so that water, which causes corrosion, can be prevented from being attracted to the lubricating layer, resulting in a lubricating layer with good corrosion resistance. 1 and R 3 When the number of carbon atoms in the terminal group represented by the formula (I) is 50 or less, the terminal group has a flexible structure, and the adhesion between the lubricating layer containing the fluorine-containing ether compound and the protective layer is improved. As a result, a lubricating layer capable of suppressing spin-off can be obtained.
[0059] R 1 and R 3 At least one of the terminal groups represented by the formula (2) is a terminal group represented by the formula (2). 2 A methylene group (-CH 2 The oxygen atom located at the end of the terminal group represented by formula (2) forms an ether bond (-O-) with the atoms bonded to both sides of it. This ether bond imparts appropriate flexibility to the fluorine-containing ether compound represented by formula (1) and increases the affinity between the polar group of the terminal group represented by formula (2) and the protective layer. As a result, the fluorine-containing ether compound represented by formula (1) can form a lubricating layer that has excellent adhesion to the protective layer.
[0060] The terminal group represented by formula (2) has a 1,2-diol structure (—CH(OH)—CH 2 Therefore, a lubricating layer containing the fluorine-containing ether compound represented by formula (1) has good corrosion resistance and can suppress spin-off.
[0061] The terminal group represented by formula (2) has a divalent organic group represented by X having 2 to 30 carbon atoms. Since the organic group represented by X has 2 or more carbon atoms, it is moderately rigid, and can suppress intramolecular interactions while simultaneously achieving sufficient hydrophobicity. Furthermore, since it has 30 or less carbon atoms, it is possible to prevent the terminal group represented by formula (2) from becoming too bulky, which would hinder the movement of the polar group and inhibit the interaction with the protective layer. The number of carbon atoms in the organic group represented by X is preferably 2 to 15, and more preferably 3 to 10.
[0062] The organic group represented by X contains at least one carbon atom that is not bonded to either a polar group or an ether oxygen atom. Examples of carbon atoms that are not bonded to either a polar group or an ether oxygen atom include carbon atoms of a methylene group, a methine group, or a fluorinated group of these that are not bonded to either a polar group or an ether oxygen atom. As mentioned above, fluoro groups are not included in the polar group. When the organic group represented by X contains a polar group containing a carbon atom (e.g., a carboxy group, a formyl group, a carbonyl group, a cyano group, or a group having an amide bond), the carbon atom contained in the polar group is not included in the "carbon atom that is not bonded to either a polar group or an ether oxygen atom."
[0063] The number of carbon atoms that are not bonded to either a polar group or an ether oxygen atom may be 1 or more, for example, 1 to 6, or may be 1 to 4. When the number of carbon atoms that are not bonded to either a polar group or an ether oxygen atom is 1 or more, the hydrophobicity of the lubricating layer containing the fluorine-containing ether compound is improved. Furthermore, when the number of carbon atoms that are not bonded to either a polar group or an ether oxygen atom is 6 or less, the ratio of the number of carbon atoms to the number of polar groups is appropriate, the polarity of the molecule is appropriate, and the ratio of the number of carbon atoms to the number of ether oxygen atoms is appropriate, resulting in a fluorine-containing ether compound with appropriate molecular flexibility. Furthermore, when the compound contains multiple carbon atoms that are not bonded to either a polar group or an ether oxygen atom, the carbon atoms that are not bonded to either a polar group or an ether oxygen atom may be bonded to each other. In this case, the fluorine-containing ether compound molecule becomes more rigid, the intramolecular interaction between the polar groups is suppressed, and the polar groups are more likely to be involved in the intermolecular interaction between the fluorine-containing ether compounds.
[0064] The organic group represented by X may contain one or two polar groups. In this case, the adhesion of the fluorine-containing ether compound represented by formula (1) to the protective layer is improved, and it is easy to form a lubricating layer that can provide a sufficient coating state even if the thickness is thin. When the organic group represented by X contains a polar group, it is preferable that the number of polar groups is one. In this case, it is possible to further suppress the fluorine-containing ether compound represented by formula (1) from being too hydrophilic and inducing water that causes corrosion.
[0065] When the organic group represented by X contains a polar group, the polar group may be R 1 and R 3 Examples of the polar group contained in the above formula (1) include those exemplified above, and it is more preferable that the polar group is selected from the group consisting of a hydroxyl group, a cyano group, and a group having an amide bond.
[0066] The organic group represented by X in formula (2) may contain 1 to 3 ether oxygen atoms. In this case, the ether oxygen atoms impart appropriate flexibility to the fluorinated ether compound represented by formula (1) and increase the affinity between the polar group and the protective layer. When the organic group represented by X contains an ether oxygen atom, the number of ether oxygen atoms is preferably 1 or 2. In this case, the fluorinated ether compound represented by formula (1) can be further prevented from becoming too flexible and causing intramolecular interactions.
[0067] The organic group represented by X in formula (2) may be partially fluorinated. In this case, the hydrophilicity of the organic group represented by X in formula (2) is reduced compared with that of a non-fluorinated organic group. As a result, the fluorine-containing ether compound can be obtained, which can suppress the induction of water that causes corrosion and can form a lubricating layer with good corrosion resistance.
[0068] In formula (2), the organic group represented by X is preferably an acyclic organic group. When the organic group represented by X is acyclic, it becomes too bulky compared to when X has a cyclic structure, which can prevent the movement of the polar group from being hindered and the interaction with the protective layer from being inhibited. The acyclic organic group may be linear or branched.
[0069] In formula (2), the organic group represented by X preferably does not contain an unsaturated carbon-carbon bond. When the organic group represented by X does not contain an unsaturated carbon-carbon bond, the molecular orientation is restricted, the movement of the polar group is hindered, and the inhibition of interaction with the protective layer can be suppressed, compared to when X contains an unsaturated carbon-carbon bond.
[0070] The terminal group represented by formula (2) is preferably any one of the following formulae (2-1) to (2-7).
[0071] (In formula (2-1), a represents an integer of 1 to 8. b represents an integer of 1 to 7.) (In formula (2-2), c represents an integer of 1 to 7.) (In formula (2-3), d represents an integer of 1 to 6.) (In formula (2-4), e represents an integer of 1 to 6. e R a and R beach independently represents a hydrogen atom or a methyl group.) (In formula (2-5), f represents an integer of 1 to 6.) (In formula (2-6), g represents an integer of 1 to 6.) (In formula (2-7), g2 represents an integer of 1 to 6.)
[0072] The terminal group represented by formula (2-1) is an organic group represented by X in formula (2) that is —CH 2 -CH(OH)-(CH 2 ) a -O-(CH 2 ) b -CH 2 a represents an integer of 1 to 8. b represents an integer of 1 to 7.
[0073] The terminal group represented by formula (2-1) has a glycerin structure (—O—CH 2 -CH(OH)-CH 2 OH) with b methylene groups. The structure with increased carbon atoms in the glycerin structure has moderate rigidity, and therefore can suppress the formation of intramolecular interactions between the terminal group represented by formula (2-1). In addition, the ether bond in the structure with increased carbon atoms in the glycerin structure imparts moderate mobility to the terminal group represented by formula (2-1). Therefore, when one of the two hydroxyl groups at the terminal portion interacts with the protective layer, the other hydroxyl group becomes more likely to participate in the intermolecular interactions between the fluorine-containing ether compounds. Therefore, the polar group in the fluorine-containing ether compound represented by formula (1) can more easily form intermolecular interactions. As a result, a lubricating layer containing the fluorine-containing ether compound represented by formula (1) is less likely to scatter the fluorine-containing ether compound as the magnetic recording medium rotates, and has even better spin-off resistance.
[0074] Since a in formula (2-1) is 1 or more, the terminal group represented by formula (2-1) has sufficient hydrophobicity. Furthermore, since a is 8 or less, the terminal group represented by formula (2-1) does not become too bulky due to the number of a being too large, and it is possible to suppress the movement of the hydroxyl group in the terminal group represented by formula (2-1) being hindered and the interaction with the protective layer being inhibited. a is preferably 1 to 6, and more preferably 1 to 4.
[0075] Since b in formula (2-1) is 1 or more, the terminal group represented by formula (2-1) has sufficient hydrophobicity. Furthermore, since b is 7 or less, the terminal group represented by formula (2-1) does not become too bulky due to the number of b being too large, and it is possible to suppress the movement of the hydroxyl group in the terminal group represented by formula (2-1) being hindered and the interaction with the protective layer being inhibited. b is preferably 1 to 5, and more preferably 1 to 3.
[0076] The sum of a and b in formula (2-1) is preferably 9 or less. In this case, the terminal group represented by formula (2-1) does not become too bulky, and the movement of the hydroxyl group in the terminal group represented by formula (2-1) is hindered, which further prevents the interaction with the protective layer from being hindered. The sum of a and b is more preferably 6 or less, and even more preferably 4 or less.
[0077] The terminal group represented by formula (2-2) is an organic group represented by X in formula (2) that is —CH 2 -CH(OH)-CH 2 - (CH 2 ) c -O-CH 2 -, and c represents an integer of 1 to 7.
[0078] The terminal group represented by formula (2-2) has a glycerin structure (—O—CH 2 -CH(OH)-CH 2 OH). Because the glycerin structure has high mobility, when one of the two hydroxyl groups at the terminal portion interacts with the protective layer, the other hydroxyl group is more likely to interact intermolecularly with a polar group in another fluorine-containing ether compound. Therefore, the polar group in the fluorine-containing ether compound represented by formula (1) can more easily form an intermolecular interaction. As a result, a lubricant containing the fluorine-containing ether compound represented by formula (1) is less likely to scatter the fluorine-containing ether compound as the magnetic recording medium rotates, and has even more excellent spin-off resistance.
[0079] Since c in formula (2-2) is 1 or more, the terminal group represented by formula (2-2) has sufficient hydrophobicity. Furthermore, since c is 7 or less, the terminal group represented by formula (2-2) does not become too bulky due to an excessively large number of c, and this can prevent the movement of the hydroxyl group in the terminal group represented by formula (2-2) from being hindered, thereby preventing the interaction with the protective layer from being inhibited. c is preferably 1 to 5, and more preferably 1 to 3.
[0080] The terminal group represented by formula (2-3) is an organic group represented by X in formula (2) that is —CH 2 -CH(OH)-(CH 2 ) d -, and d represents an integer of 1 to 6.
[0081] The terminal group represented by formula (2-3) does not contain an ether oxygen atom, which is a hydrophilic moiety, in X. Therefore, the terminal group represented by formula (2-3) has low affinity for water. Therefore, a lubricating layer containing a fluorinated ether compound represented by formula (1) is less likely to absorb water, which causes corrosion, and has better corrosion resistance.
[0082] The terminal group represented by formula (2-3) does not contain an ether oxygen atom in X in formula (2), and d is 1 or more, so it is moderately rigid. Therefore, intramolecular interactions between polar groups are more effectively suppressed, and intermolecular interactions are more easily formed, resulting in the formation of a lubricating layer with even better spin-off resistance. Furthermore, since d is 6 or less, the terminal group represented by formula (2-3) does not become too bulky due to an excessively large number of d, and the movement of the hydroxyl group in the terminal group represented by formula (2-3) is hindered, thereby preventing the interaction with the protective layer from being hindered. d is preferably 1 to 4, and more preferably 2 to 4.
[0083] The terminal group represented by formula (2-4) is a group in which the organic group represented by X in formula (2) is —CH 2 -CH(OH)-CH 2 -O-CH 2 - (CR a R b ) e -CH 2 -O-CH 2-. e represents an integer of 1 to 6. e R a and R b each independently represents a hydrogen atom or a methyl group.
[0084] e -CR in the terminal group represented by formula (2-4) a R b - is -CH 2 -, -CH(CH 3 ) -, -C(CH 3 ) 2 - may be either.
[0085] In the terminal group represented by formula (2-4), the organic group represented by X in formula (2) has a linear structure, that is, R a and R b When X is a hydrogen atom, the terminal group does not become too bulky compared to when X has a branch. This prevents the movement of the hydroxyl group from being hindered, thereby preventing the interaction with the protective layer. As a result, when one of the two hydroxyl groups forming the terminal 1,2-diol structure interacts with the protective layer, the other hydroxyl group can more easily form an intermolecular interaction with a polar group in another fluorinated ether compound. This makes it more difficult for the fluorinated ether compound to scatter as the magnetic recording medium rotates, resulting in even more excellent spin-off resistance.
[0086] In the terminal group represented by formula (2-4), the organic group represented by X in formula (2) has a branched structure, i.e., -CH(CH 3 )- and / or -C(CH 3 ) 2 When X contains -, X becomes suitably rigid, and the intramolecular interaction between the hydroxyl groups of the terminal groups can be effectively suppressed. Therefore, the polar groups in the fluorinated ether compound represented by formula (1) can more easily form intermolecular interactions. As a result, a lubricant containing the fluorinated ether compound represented by formula (1) is less likely to scatter the fluorinated ether compound as the magnetic recording medium rotates, and has even better spin-off resistance.
[0087] Since e in formula (2-4) is 1 or more, the terminal group represented by formula (2-4) has sufficient hydrophobicity. Furthermore, since e is 6 or less, the terminal group represented by formula (2-4) does not become too bulky, and it is possible to prevent the movement of the hydroxyl group from being hindered and the interaction with the protective layer from being inhibited. e is preferably 1 to 4, and more preferably 1 to 2.
[0088] The terminal group represented by formula (2-5) is a group in which the organic group represented by X in formula (2) is —CH 2 -CH(OH)-CH 2 -O-CH 2 -(CF 2 ) f -CH 2 -O-CH 2 f represents an integer of 1 to 6.
[0089] The terminal group represented by formula (2-5) contains a linear perfluoroalkylene chain having 1 to 6 carbon atoms, which reduces the affinity for water. When the terminal group represented by formula (2-5) is present, the saturated hydrocarbon group containing the perfluoroalkylene chain (-CH 2 -(CF 2 ) f -CH 2 -) reduces the polarity of the entire molecule and improves hydrophobicity. This reduces the affinity between the fluorine-containing ether compound and water, which causes corrosion. As a result, the lubricating layer containing the fluorine-containing ether compound represented by formula (1) is inhibited from taking in water, which causes corrosion, and has even better corrosion resistance.
[0090] Since f in formula (2-5) is 1 or more, the terminal group represented by formula (2-5) becomes appropriately rigid, and intramolecular interactions can be suppressed. Furthermore, since f is 6 or less, the terminal group represented by formula (2-5) does not become too bulky, and it is possible to suppress the movement of the hydroxyl group being hindered and the inhibition of interaction with the protective layer. In formula (2-5), f is preferably 1 to 4, and more preferably 2 to 4.
[0091] The terminal group represented by formula (2-6) is an organic group represented by X in formula (2) that is -(CH 2 ) g -CH2 g represents an integer of 1 to 6.
[0092] The terminal group represented by formula (2-6) does not contain a polar group or an ether oxygen atom, which are hydrophilic moieties, in X. Therefore, the terminal group represented by formula (2-6) has low affinity with water. Therefore, a lubricating layer containing a fluorine-containing ether compound represented by formula (1) is less likely to absorb water, which causes corrosion, and has better corrosion resistance.
[0093] Since g in formula (2-6) is 1 or more, formula (2-6) becomes moderately rigid, making it difficult for the hydroxyl groups in the 1,2-diol structure to form intramolecular interactions. Furthermore, since g in formula (2-6) is 6 or less, the terminal group represented by formula (2-6) does not become too bulky, preventing the movement of the hydroxyl groups from being hindered, thereby preventing the interaction with the protective layer from being inhibited. g is preferably 1 to 5, and more preferably 1 to 3.
[0094] The terminal group represented by formula (2-7) is an organic group represented by X in formula (2) that is -(CH 2 ) g2 -CH 2 -CH(OH)-CH 2 -O-CH 2 g2 represents an integer of 1 to 6. The terminal group represented by formula (2-7) has a glycerin structure (—O—CH 2 -CH(OH)-CH 2 OH). Because the glycerin structure has high mobility, when one of the two hydroxyl groups at the terminal portion interacts with the protective layer, the other hydroxyl group is more likely to interact intermolecularly with a polar group in another fluorine-containing ether compound. Therefore, the polar group in the fluorine-containing ether compound represented by formula (1) can more easily form an intermolecular interaction. As a result, a lubricant containing the fluorine-containing ether compound represented by formula (1) is less likely to scatter the fluorine-containing ether compound as the magnetic recording medium rotates, and has even more excellent spin-off resistance.
[0095] Since g2 in formula (2-7) is 1 or more, formula (2-7) becomes moderately rigid, making it difficult for the hydroxyl groups in the 1,2-diol structure to form intramolecular interactions. Furthermore, since g2 in formula (2-7) is 6 or less, the terminal group represented by formula (2-7) does not become too bulky, preventing the movement of the hydroxyl groups from being hindered, thereby preventing the interaction with the protective layer from being inhibited. g2 is preferably 1 to 5, and more preferably 1 to 3.
[0096] Of the terminal groups represented by formulae (2-1) to (2-7), the terminal groups represented by formulae (2-3), (2-5) and (2-6) have better corrosion resistance.
[0097] Of the terminal groups represented by formulas (2-1) to (2-7), the terminal groups represented by formulas (2-1), (2-2), (2-4), and (2-7) have better spin-off resistance when the sum of a and b in formula (2-1) is 4 or less, c in formula (2-2) is 3 or less, e in formula (2-4) is 2 or less, and g2 in formula (2-7) is 3 or less.
[0098] In the fluorine-containing ether compound represented by formula (1), R 1 and R 3 may be the same or different. 1 and R 3 In this case, the fluorine-containing ether compound can be produced easily and efficiently. 1 and R 3 "The same" means that R 1 Atoms contained in and R 3 and the atoms contained in -CH 2 -R 2 -CH 2 - means that they are arranged symmetrically with respect to each other.
[0099] In the fluorine-containing ether compound represented by formula (1), R 1 and R 3 If different from 1 and R 3 may each independently be a terminal group represented by formula (2), or R 1 and R 3One of the groups may be an end group represented by formula (2), and the other may be an end group that does not fall under formula (2). The end group that does not fall under formula (2) may be, as described above, an end group having 1 to 4 polar groups and 1 to 50 carbon atoms.
[0100] R 1 and R 3 is a terminal group represented by formula (2) and the other is a terminal group not corresponding to formula (2), the terminal group not corresponding to formula (2) is preferably represented by the following formula (3):
[0101] (In formula (3), l represents an integer of 1 to 3. l m's each independently represent an integer of 1 to 6. l n's each independently represent an integer of 1 to 6. In one repeating unit, at least one of m and n is 1. B represents an alkyl group which may have only one polar group, an organic group containing a carbon-carbon unsaturated bond, or a hydrogen atom.)
[0102] The terminal group represented by formula (3) is R 2 A methylene group (-CH 2 The oxygen atom located at the end of the terminal group represented by formula (3) forms an ether bond (-O-) with the atoms bonded to both sides of it. This ether bond imparts appropriate flexibility to the fluorine-containing ether compound represented by formula (1) and increases the affinity between the polar group of the terminal group represented by formula (3) and the protective layer. As a result, the fluorine-containing ether compound represented by formula (1) can form a lubricating layer that has excellent adhesion to the protective layer.
[0103] In formula (3), l is an integer of 1 to 3, preferably an integer of 1 or 2, and more preferably 1. If l in formula (3) is 3 or less, the number of hydroxyl groups in the terminal groups represented by formula (3) is too large, which can prevent water, which causes corrosion, from being attracted to the lubricating layer, and a lubricating layer with good corrosion resistance can be obtained.
[0104] When l in formula (3) is 2 or 3, two or three repeating units (-(CH 2 ) m -CH(OH)-(CH2 ) n The combinations of m and n in —O—) may be different from one another, or some or all of them may be the same.
[0105] In formula (3), l m's each independently represent an integer of 1 to 6. l n's each independently represent an integer of 1 to 6. One repeating unit (-(CH 2 ) m -CH(OH)-(CH 2 ) n In the formula (I), at least one of m and n is 1. In this case, it is possible to prevent the mobility of the hydroxyl group in the repeating unit from decreasing due to the alkylene group having too many carbon atoms between the carbon atom to which the hydroxyl group is bonded and the ether oxygen atom.
[0106] In formula (3), B represents an alkyl group which may have only one polar group, an organic group containing a carbon-carbon unsaturated bond, or a hydrogen atom.
[0107] When B in formula (3) is an alkyl group having no polar group, examples of B include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group.
[0108] When B in formula (3) is an alkyl group having a polar group, the polar group is R 1 and R 3 Of the above polar groups, a polar group selected from the group consisting of a hydroxyl group, a cyano group, and a group having an amide bond is more preferred.
[0109] When B in formula (3) is an alkyl group having a polar group, examples of B include a 2-hydroxyethyl group, a 3-hydroxypropyl group, a 4-hydroxybutyl group, a 5-hydroxypentyl group, a 6-hydroxyhexyl group, a 2-aminoethyl group, a 3-aminopropyl group, a 1-carboxymethyl group, a 2-carboxyethyl group, a 3-carboxypropyl group, a 1-carbonylmethyl group, a 2-carbonylethyl group, a 3-carbonylpropyl group, a 1-acetylmethyl group, a 2-acetylethyl group, a 3-acetylpropyl group, a 2-sulfoethyl group, a 3-sulfopropyl group, a 1-cyanomethyl group, a 2-cyanoethyl group, a 3-cyanopropyl group, a 4-cyanobutyl group, a 2-acetamidoethyl group, a 3-acetamidopropyl group, a 4-acetamidobutyl group, a 1-carboxamidomethyl group, a 2-carboxamidoethyl group, a 3-carboxamidopropyl group, and a 4-carboxamidobutyl group.
[0110] Among the above alkyl groups having a polar group, any one of a 2-hydroxyethyl group, a 3-hydroxypropyl group, a 4-hydroxybutyl group, a 5-hydroxypentyl group, a 6-hydroxyhexyl group, a 1-cyanomethyl group, a 2-cyanoethyl group, a 3-cyanopropyl group, a 2-acetamidoethyl group, a 1-carboxamidomethyl group, a 2-carboxamidoethyl group, and a 3-carboxamidopropyl group is preferred, and any one of a 2-hydroxyethyl group, a 3-hydroxypropyl group, a 2-cyanoethyl group, a 3-cyanopropyl group, a 2-acetamidoethyl group, and a 1-carboxamidomethyl group is more preferred.
[0111] When B in formula (3) is an organic group containing a carbon-carbon unsaturated bond, examples of B include an organic group containing at least one selected from an aromatic hydrocarbon, an unsaturated heterocycle, an alkenyl group, and an alkynyl group.
[0112] When B in formula (3) is an organic group containing a carbon-carbon unsaturated bond, examples of B include a phenyl group, a methoxyphenyl group, a fluorinated phenyl group, an acetamidophenyl group, a carboxamidophenyl group, a cyanophenyl group, a naphthyl group, a phenethyl group, a methoxyphenethyl group, a fluorinated phenethyl group, a benzyl group, a methoxybenzyl group, a naphthylmethyl group, a methoxynaphthyl group, a pyrrolyl group, a pyrazolyl group, a methylpyrazolylmethyl group, an imidazolyl group, a furyl group, a furfuryl group, an oxazolyl group, an isoxazolyl group, a thienyl group, a thienylethyl group, a thiazolyl group, a methyl ... Examples of such alkyl groups include a methyl group, an isothiazolyl group, a pyridyl group, a pyrimidinyl group, a pyridazinyl group, a pyrazinyl group, an indolinyl group, a benzofuranyl group, a benzothienyl group, a benzimidazolyl group, a benzoxazolyl group, a benzothiazolyl group, a benzopyrazolyl group, a benzisoxazolyl group, a benzisothiazolyl group, a quinolyl group, an isoquinolyl group, a quinazolinyl group, a quinoxalinyl group, a phthalazinyl group, a cinnolinyl group, a vinyl group, an allyl group, a butenyl group, a propynyl group, a propargyl group, a butynyl group, a methylbutynyl group, a pentynyl group, a methylpentynyl group, and a hexynyl group.
[0113] Among the above-mentioned organic groups containing a carbon-carbon unsaturated bond, any one of a phenyl group, a methoxyphenyl group, an acetamidophenyl group, a carboxamidophenyl group, a cyanophenyl group, a naphthyl group, a phenethyl group, a methoxyphenethyl group, a fluorinated phenethyl group, a thienylethyl group, an allyl group, a butenyl group, and a propargyl group is preferred, and any one of a phenyl group, a methoxyphenyl group, a carboxamidophenyl group, an allyl group, and a butenyl group is particularly preferred. In this case, the terminal group represented by formula (3) has sufficient hydrophobicity and is not too bulky, so that the movement of the hydroxyl group in formula (3) is not hindered, thereby preventing the interaction with the protective layer from being inhibited.
[0114] When B in formula (3) is a hydrogen atom, B forms a hydroxyl group together with the oxygen atom in formula (3).
[0115] The terminal group represented by formula (3) is more preferably represented by any one of the following formulas (3-1) to (3-3).
[0116] (In formula (3-1), p represents an integer of 0 to 3. q represents an integer of 0 to 2. r represents an integer of 0 to 5. The total value of p and r is 1 to 5. D represents a polar group, a vinyl group, an ethynyl group, or an aryl group which may have a substituent.) (In formula (3-2), s represents an integer of 0 to 2. t represents an integer of 1 to 5.) (In formula (3-3), u represents an integer of 1 to 3. Each of the five E's independently represents a polar group, an alkoxy group having 1 to 8 carbon atoms, a halogeno group, or a hydrogen atom. However, when a polar group is included in the five E's, the number of polar groups among the five E's is 1.)
[0117] In the terminal groups represented by formulas (3-1) to (3-3), each polar group contained in the terminal group is bonded to a different carbon atom. Furthermore, the carbon atoms to which the polar groups are bonded are bonded via a linking group containing a carbon atom to which no polar group is bonded. Therefore, the terminal groups represented by formulas (3-1) to (3-3) can be oriented so that both the terminal polar group and the hydroxyl group adjacent to the terminal polar group can adhere to the protective layer due to the linking group containing a carbon atom to which no polar group is bonded. Therefore, a lubricating layer that has a strong interaction with the protective layer can be formed.
[0118] In the terminal groups represented by formulae (3-1) to (3-3), the polar groups in the terminal groups are less likely to aggregate with each other and more likely to interact with the protective layer than in terminal groups in which the carbon atoms to which polar groups are bonded are directly bonded. Therefore, in the terminal groups represented by formulae (3-1) to (3-3), the terminal portions in the fluorinated ether compound are less likely to float up, and the adhesion to the protective layer is less likely to decrease.
[0119] In the terminal group represented by formula (3-1), the linking group between the carbon atom to which D is bonded and the carbon atom to which the hydroxyl group adjacent to D at the terminal is bonded contains an ether oxygen atom. The linking group has a linear structure consisting of 2 to 7 atoms, including a carbon atom to which no polar group is bonded.
[0120] The terminal group represented by formula (3-1) has a linear structure in which the linking group is composed of two or more atoms, including a carbon atom to which no polar group is bonded. Therefore, the distance between D and the hydroxyl group adjacent to D is appropriate. Therefore, intramolecular interaction between D and the hydroxyl group adjacent to D can be suppressed, allowing the polar group to efficiently adhere to the protective layer. Furthermore, since the terminal group represented by formula (3-1) has the above structure, a fluorine-containing ether compound having good hydrophobicity can be obtained even if it contains an ether oxygen atom. Furthermore, the molecular mobility is appropriate, intramolecular aggregation is unlikely to occur, and the compound has excellent adhesion to the protective layer.
[0121] The terminal group represented by formula (3-1) has a linear structure in which the linking group contains an ether oxygen atom and is composed of 7 or less atoms, including a carbon atom to which no polar group is bonded. Therefore, the adhesion between the lubricating layer containing the fluorine-containing ether compound and the protective layer is not impaired due to excessive hydrophobicity of the linking group.
[0122] From these facts, the fluorine-containing ether compound having a terminal group represented by formula (3-1) can form a lubricating layer that has excellent adhesion to a protective layer, exhibits high corrosion resistance, and can suppress spin-off.
[0123] In the terminal group represented by formula (3-1), the sum of p and r is 1 to 5, preferably 1 to 3. The terminal group represented by formula (3-1) has a linking group between the carbon atom to which D is bonded and the carbon atom to which the hydroxyl group adjacent to the D located at the terminal is bonded. The carbon atom contained in the linking group prevents intramolecular interactions between adjacent polar groups from occurring in preference to interactions between the polar groups and the protective layer. As a result, the carbon atom contained in the linking group improves the adhesion between the polar group in formula (3-1) and the protective layer.
[0124] If the linking group contains too many carbon atoms, the flexibility of the terminal group represented by formula (3-1) decreases, making it difficult to uniformly coat the entire surface of the protective layer. In the terminal group represented by formula (3-1), the total value of p and r is 5 or less, so the alkylene chain in the main chain portion of formula (3-1) is not too long. Therefore, the long rigid alkylene chain reduces the flexibility of the terminal portion, weakening the interaction with the protective layer and preventing the terminal portion from lifting up. p is an integer of 0 to 3, preferably 0 or 1, and more preferably 0. r is an integer of 0 to 5, preferably 1 or 2, and more preferably 1.
[0125] In formula (3-1), D represents a polar group, a vinyl group, an ethynyl group, or an aryl group which may have a substituent. When D is a polar group, D is R 1 and R 3 Among the above polar groups, a polar group selected from the group consisting of a hydroxyl group, a cyano group, and a group having an amide bond is more preferred. When D is an aryl group which may have a substituent, an aryl group which may have a substituent that is included in the organic group which can be used when B in the above formula (3) is an organic group containing a carbon-carbon unsaturated bond can be used.
[0126] In formula (3-1), q represents an integer of 0 to 2. The number of polar groups in formula (3-1) is q+2 when D is a polar group, and q+1 when D is a vinyl group or an ethynyl group. As described above, R 1 and R 3 The number of polar groups contained in each of the formulas is preferably 2 or 3. Therefore, q in formula (3-1) is preferably 0 or 1 when D is a polar group, and is preferably 1 or 2 when D is a vinyl group or an ethynyl group. When D is an aryl group which may have a substituent, it is preferable to select q so that the number of polar groups in formula (3-1) is 2 or 3.
[0127] In the terminal group represented by formula (3-2), the linking group between the carbon atom to which the terminal hydroxyl group is bonded and the carbon atom to which the hydroxyl group adjacent to the terminal hydroxyl group is bonded does not contain an oxygen atom, and therefore, intramolecular interaction is small and intramolecular aggregation is unlikely to occur, resulting in excellent adhesion to the protective layer.
[0128] The terminal group represented by formula (3-2) has a linear structure in which the linking group is composed of 1 to 5 atoms including a carbon atom not bonded to a hydroxyl group. Because the linking group has a linear structure composed of one or more atoms including a carbon atom not bonded to a hydroxyl group, the distance between the terminal hydroxyl group and the hydroxyl group adjacent to the terminal hydroxyl group is appropriate. Therefore, intramolecular aggregation is unlikely to occur, and a fluorinated ether compound having good hydrophobicity can be obtained.
[0129] The terminal group represented by formula (3-2) has a linear structure in which the linking group does not contain an oxygen atom and is composed of five or less atoms including a carbon atom to which no hydroxyl group is bonded. Therefore, the linking group is not too hydrophobic to impair adhesion to the protective layer, and the linking group is not too bulky to hinder the movement of the hydroxyl group.
[0130] In the terminal group represented by formula (3-2), t is an integer of 1 to 5. In the terminal group represented by formula (3-2), similar to the terminal group represented by formula (3-1), if the linking group disposed between the carbon atoms bonded to the polar group contains too many carbon atoms, the flexibility of the terminal group represented by formula (3-2) decreases, making it difficult to uniformly coat the entire surface of the protective layer. In the terminal group represented by formula (3-2), t is 5 or less, so the alkylene chain in the main chain portion of formula (3-2) is not too long. Therefore, a long rigid alkylene chain reduces the flexibility of the terminal portion, preventing a decrease in the interaction between the terminal hydroxyl group and the protective layer. t is preferably 1 or 2, and more preferably 1.
[0131] From these facts, the fluorine-containing ether compound having an end group represented by formula (3-2) can form a lubricating layer that has excellent adhesion to a protective layer, high corrosion resistance, and can suppress spin-off, because the linking group in formula (3-2) does not contain an oxygen atom and has a linear structure consisting of 1 to 5 atoms including a carbon atom to which no hydroxyl group is bonded.
[0132] In formula (3-2), s represents an integer of 0 to 2. The number of polar groups in formula (3-2) is s+2, and as described above, R 1 and R 3 The number of polar groups contained in each of the formulas is preferably 2 or 3. Therefore, s in formula (3-2) is preferably 0 or 1.
[0133] In the terminal group represented by formula (3-3), five E's each independently represent a polar group, an alkoxy group having 1 to 8 carbon atoms, a halogeno group, or a hydrogen atom. When a polar group is included in the five E's, the number of polar groups among the five E's is one.
[0134] In the terminal group represented by formula (3-3), when the five E's contain polar groups, the linking group between the carbon atom to which the polar group represented by E is bonded and the carbon atom to which the hydroxyl group adjacent to the polar group represented by E is bonded contains an oxygen atom forming an ether bond. The linking group has a structure consisting of 3 to 5 atoms, including a carbon atom to which no polar group is bonded. The number of atoms in the linking group refers to the number of atoms in the shortest distance between the carbon atom to which the polar group included in E is bonded and the carbon atom to which the hydroxyl group adjacent to the polar group included in E is bonded.
[0135] In the terminal group represented by formula (3-3), when the five E's contain polar groups, the linking group contains an oxygen atom forming an ether bond, and has a structure consisting of three or more atoms including a carbon atom not bonded to a polar group. Therefore, the distance between the polar group represented by E and the hydroxyl group adjacent to the polar group represented by E is appropriate. In addition, since the benzene ring is rigid, free rotation is difficult. Therefore, it is possible to suppress interaction between the polar group represented by E, which is a substituent bonded to the benzene ring, and the hydroxyl group adjacent to the polar group represented by E.
[0136] In formula (3-3), u represents an integer of 1 to 3. When u in formula (3-3) is 2 or 3, -(CH 2 CH(OH)CH 2 O) u The linking group between carbon atoms to which adjacent hydroxyl groups are bonded contains an oxygen atom forming an ether bond and has a linear structure consisting of three atoms including a carbon atom to which no hydroxyl group is bonded. Because the linking group has a linear structure consisting of three atoms including a carbon atom to which no hydroxyl group is bonded, the distance between adjacent hydroxyl groups is appropriate. This makes it possible to suppress interactions between hydroxyl groups within the molecule.
[0137] For these reasons, the fluorine-containing ether compound having a terminal group represented by formula (3-3) can suppress interactions between polar groups within the molecule, and therefore the lubricating layer containing the fluorine-containing ether compound having a terminal group represented by formula (3-3) has excellent adhesion to the protective layer and a high spin-off suppressing effect.
[0138] In the terminal group represented by formula (3-3), when none of the five E's contains a polar group, the hydrophobicity of the molecule is higher than when one of the five E's is a polar group. Therefore, a lubricating layer containing a fluorine-containing ether compound having an terminal group represented by formula (3-3) can further suppress the induction of water, which causes corrosion, and has higher corrosion resistance.
[0139] In the terminal group represented by formula (3-3), when E is a polar group, E is R 1 and R 3 Among the above polar groups, E is more preferably a polar group selected from the group consisting of a cyano group and a group having an amide bond, and is preferably a cyano group, an acetamide group (—NHC(═O)CH 3 ) or a carboxamide group (—C(═O)NH 2) is more preferable. When the polar group is a cyano group, an acetamide group, or a carboxamide group, the resulting fluorine-containing ether compound can form a lubricating layer with stronger interaction with the protective layer. In addition, since the acidity of a cyano group, an acetamide group, or a carboxamide group is not too high, a fluorine-containing ether compound having these groups hardly corrodes the substrate. When E is not a polar group, it is preferable that each E is independently a methoxy group, a fluoro group, or a hydrogen atom.
[0140] The number of polar groups in formula (3-3) is u+1 when the five E's contain polar groups, and is u when the five E's do not contain polar groups. 1 and R 3 The number of polar groups contained in each of the above is preferably 2 or 3. Therefore, u in formula (3-3) is preferably 1 or 2 when a polar group is contained in the five E's, and is preferably 2 or 3 when a polar group is not contained in the five E's.
[0141] When the five E's in formula (3-3) contain polar groups, the four E's other than the polar groups may be partially or completely the same, or may be different from each other. When the five E's contain polar groups, it is preferable that the four E's other than the polar groups are all the same. When the five E's do not contain polar groups, the five E's may be partially or completely the same, or may be different from each other.
[0142] When a polar group is included in the five E's in formula (3-3), the polar group may be located at any position of the five E's.
[0143] (R 2 In the fluorine-containing ether compound represented by formula (1), R 2 is a perfluoropolyether chain. 2 When a lubricating layer is formed by applying a lubricant containing the fluorine-containing ether compound of this embodiment onto a protective layer, the PFPE chain represented by the formula (R) coats the surface of the protective layer and imparts lubricity to the lubricating layer, thereby reducing the frictional force between the magnetic head and the protective layer. 2The PFPE chain represented by the formula (I) is appropriately selected depending on the performance required of the lubricant containing the fluorine-containing ether compound.
[0144] R 2 Examples of the PFPE chain represented by the formula (1) include those made of a polymer or copolymer of perfluoroalkylene oxide. Examples of perfluoroalkylene oxide include perfluoromethylene oxide, perfluoroethylene oxide, perfluoro-n-propylene oxide, perfluoroisopropylene oxide, and perfluorobutylene oxide.
[0145] R in formula (1) 2 is preferably a PFPE chain represented by the following formula (4) derived from a polymer or copolymer of perfluoroalkylene oxide: -(CF 2 ) w1 -O-(CF 2 O) w2 -(CF 2 CF 2 O) w3 -(CF 2 CF 2 CF 2 O) w4 -(CF 2 CF 2 CF 2 CF 2 O) w5 -(CF 2 ) w6 - (4) (In formula (4), w2, w3, w4, and w5 represent the average degree of polymerization, and each independently represents 0 to 20. However, w2, w3, w4, and w5 cannot all be 0 at the same time. w1 and w6 are CF 2 The repeating units in formula (4) are (CF 2 O), (CF 2 CF 2 O), (CF 2 CF 2 CF 2 O), (CF 2 CF 2 CF 2 CF 2 There are no particular restrictions on the arrangement order of O).
[0146] In formula (4), w2, w3, w4, and w5 represent average degrees of polymerization, each independently representing 0 to 20, preferably 0 to 15, and more preferably 0 to 10. In formula (4), w1 and w6 represent CF 2 The values of w1 and w6 are determined depending on the structure of the repeating units located at the ends of the chain structure in the PFPE chain represented by formula (4). 2 O), (CF 2 CF 2 O), (CF 2 CF 2 CF 2 O), (CF 2 CF 2 CF 2 CF 2 O) is a repeating unit. There is no particular limitation on the arrangement order of the repeating units in formula (4). There is also no particular limitation on the number of types of repeating units in formula (4).
[0147] R in formula (1) 2 is preferably any one selected from PFPE chains represented by the following formulas (4-1) to (4-4): 2 -(OCF 2 CF 2 ) h -(OCF 2 ) i -OCF 2 - (4-1) (In formula (4-1), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.) -CF 2 CF 2 -(OCF 2 CF 2 CF 2 ) j -OCF 2 CF 2 - (4-2) (In formula (4-2), j represents the average degree of polymerization and represents 1 to 15.) -CF 2 CF 2 CF 2 -(OCF 2 CF 2 CF 2 CF 2 )k -OCF 2 CF 2 CF 2 - (4-3) (In formula (4-3), k represents the average degree of polymerization and represents 1 to 10.) - (CF 2 ) w7 -O-(CF 2 CF 2 CF 2 O) w8 -(CF 2 CF 2 O) w9 -(CF 2 ) w10 - (4-4) (In formula (4-4), w8 and w9 represent the average degree of polymerization, each independently representing 1 to 20. w7 and w10 represent CF 2 is an average value representing the number of
[0148] R 2 When R is any one selected from the PFPE chains represented by formulas (4-1) to (4-4), the resulting fluorine-containing ether compound provides a lubricating layer having good lubricity. 2 is any one selected from the PFPE chains represented by formulas (4-1) to (4-4), the ratio of the number of oxygen atoms (the number of ether bonds (-O-)) to the number of carbon atoms in the PFPE chain is appropriate. Therefore, the fluorine-containing ether compound has an appropriate hardness. Therefore, the fluorine-containing ether compound applied on the protective layer is less likely to aggregate on the protective layer, and a thinner lubricating layer can be formed with a sufficient coverage. In addition, R 2 A lubricating layer containing a fluorine-containing ether compound in which R is any one selected from the PFPE chains represented by formulas (4-1) to (4-4) is more dense and can further suppress spin-off, and is therefore preferred.
[0149] In formula (4-1), the repeating unit (OCF 2 CF 2 ) and (OCF 2 In formula (4-1), there is no particular limitation on the arrangement order of (OCF 2 CF 2 ) and the number h (OCF 2The number i of (OCF 2 CF 2 The PFPE chain represented by formula (4-1) may be a polymer of (OCF 2 CF 2 ) and (OCF 2 ) may be any of a random copolymer, a block copolymer, and an alternating copolymer.
[0150] In formulas (4-1) to (4-3), h, which indicates the average degree of polymerization, is 1 to 20, i, which is 0 to 20, j, which is 1 to 15, and k, which is 1 to 10, so that the fluorine-containing ether compound can provide a lubricating layer with good lubricity. Furthermore, in formulas (4-1) to (4-3), h and i, which indicate the average degree of polymerization, are 20 or less, j is 15 or less, and k is 10 or less, so that the viscosity of the fluorine-containing ether compound does not become too high, and a lubricant containing the fluorine-containing ether compound is easily applied, which is preferable. h, i, j, and k, which indicate the average degree of polymerization, are preferably 1 to 10, more preferably 1.5 to 8, and even more preferably 2 to 7, so that the fluorine-containing ether compound can easily wet and spread on the protective layer and provide a lubricating layer with a uniform thickness.
[0151] In formula (4-4), the repeating unit (CF 2 CF 2 CF 2 O) and (CF 2 CF 2 In formula (4-4), the order of the groups (CF) representing the average degree of polymerization is not particularly limited. 2 CF 2 CF 2 O) number w8 and (CF 2 CF 2 The number w9 of monomer units (CF 2 CF 2 CF 2 O) and (CF 2 CF 2 O) may be a random copolymer, a block copolymer, or an alternating copolymer.
[0152] In formula (4-4), w8 and w9, which represent the average degree of polymerization, are each independently 1 to 20, preferably 1 to 15, and more preferably 1 to 10. w7 and w10 in formula (4-4) are each independently 1 to 20, more preferably 1 to 15, and even more preferably 1 to 10. 2 and each independently represents 1 to 2. w7 and w10 are determined depending on the structure of the repeating unit located at the end of the chain structure in the PFPE chain represented by formula (4-4).
[0153] Specifically, the fluorine-containing ether compound represented by formula (1) is preferably any one of the compounds represented by the following formulae (AA) to (AS), (BA) to (BH), and (CA) to (CK): When the compound represented by formula (1) is any one of the compounds represented by the following formulae (AA) to (AS), (BA) to (BH), and (CA) to (CK), the raw materials are easily available, and a lubricating layer can be formed that has even better corrosion resistance and can suppress spin-off, even if it is thin.
[0154] In the compounds represented by the following formulae (AA) to (AS), (BA) to (BH), and (CA) to (CK), Rf representing a PFPE chain 1 , Rf 2 , Rf 3 That is, in the compounds represented by the following formulae (AA) to (AS), (BA) to (BF), (CA), (CB), and (CE), Rf 1 is a PFPE chain represented by the above formula (4-1). In the compounds represented by the following formulae (BG), (CC), (CF) to (CK), Rf 2 is a PFPE chain represented by the above formula (4-2). In the compounds represented by the following formulas (BH) and (CD), Rf 3 is a PFPE chain represented by the above formula (4-3). Rf 1 h and i in Rf 2 j and Rf in 3 Since k in the above formula is a value indicating the average degree of polymerization, it is not necessarily an integer.
[0155]
[0156] The compounds represented by the following formulas (AA) to (AS) can be prepared by adding R 1 and R 3 is a terminal group represented by any one of the above formulas (2-1) to (2-6). 2 is the PFPE chain represented by the above formula (4-1).
[0157] The compounds represented by the following formulas (BA) to (BE) are each a compound represented by the formula (1) R 1 and R 3 One of the R groups is a terminal group represented by the above formula (2-1), and the other is a terminal group represented by either the above formula (3-1) or (3-2). 2 is the PFPE chain represented by the above formula (4-1).
[0158] The compound represented by the following formula (BF) is a compound represented by the formula (1) 1 and R 3 One of the groups is a terminal group represented by the above formula (2-1), and the other is a terminal group represented by the formula (3). 2 is the PFPE chain represented by the above formula (4-1). The terminal group represented by formula (3) does not correspond to any of the above formulae (3-1) to (3-3).
[0159] The compounds represented by the following formulas (BG) and (BH) can be prepared by the reaction of R 1 and R 3 is the terminal group represented by the above formula (2-1). 2 is a PFPE chain represented by the above formula (4-2) or (4-3).
[0160] (Rf in formula (AA) 1 In the formula (AB), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AC), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AD), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula, h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.
[0161] (Rf in formula (AE) 1 In the formula (AF), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AG), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AH), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula, h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.
[0162] (Rf in formula (AI) 1 In the formula (AJ), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AK), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AL), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula, h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.
[0163] (Rf in formula (AM) 1 In the formula (AN), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AO), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (AP), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula, h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.
[0164] (Rf in formula (AQ) 1 In the formula (AR), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1In the formula (AS), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula, h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.
[0165] (Rf in formula (BA) 1 In the formula (BB), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (BC), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (BD), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula, h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.
[0166] (Rf in formula (BE) 1 In the formula (BF), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 1 In the formula (BG), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 2 In the formula (BH), j represents the average degree of polymerization, and represents 1 to 15. 3 In the formula, k represents the average degree of polymerization and is a number ranging from 1 to 10.
[0167] The compounds represented by the following formulas (CA) to (CK) are each a compound represented by R 1 and R 3 is a terminal group represented by any one of the above formulas (2-1) to (2-7). 2 is a PFPE chain represented by any one of the above formulas (4-1) to (4-3).
[0168] (Rf in formula (CA) 1 In the formula (CB), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0. 1 In the formula (CC), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0.2 In the formula (CD), j represents the average degree of polymerization, and represents 1 to 15. 3 In the formula (CE), k represents the average degree of polymerization and represents 1 to 10. 1 In the formula (CF), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20. 2 In the formula (CG), j represents the average degree of polymerization, and represents 1 to 15. 2 In the formula (CH), j represents the average degree of polymerization, which is 1 to 15. 2 In the formula (CI), j represents the average degree of polymerization, which is 1 to 15. 2 In the formula (CJ), j represents the average degree of polymerization, and represents 1 to 15. 2 In the formula (CK), j represents the average degree of polymerization, which is 1 to 15. 2 In the formula, j represents the average degree of polymerization and is a number ranging from 1 to 15.
[0169] The fluorine-containing ether compound of this embodiment preferably has a number average molecular weight (Mn) in the range of 500 to 10,000, particularly preferably in the range of 1,000 to 5,000. When the number average molecular weight is 500 or more, a lubricating layer made of a lubricant containing the fluorine-containing ether compound of this embodiment will have excellent heat resistance. The number average molecular weight of the fluorine-containing ether compound is more preferably 1,000 or more. Furthermore, when the number average molecular weight is 10,000 or less, the viscosity of the fluorine-containing ether compound becomes appropriate, and by applying a lubricant containing this, a thin lubricating layer can be easily formed. The number average molecular weight of the fluorine-containing ether compound is preferably 5,000 or less, so that the viscosity becomes easy to handle when applied to a lubricant.
[0170] The number average molecular weight (Mn) of the fluorine-containing ether compound was measured by AVANCEIII400 manufactured by Bruker Biospin. 1 H-NMR and 19 This is a value measured by F-NMR. 19The number of repeating units of the PFPE chain is calculated from the integrated value measured by F-NMR to determine the number average molecular weight. In the NMR (nuclear magnetic resonance) measurement, the sample is diluted in a hexafluorobenzene / d-acetone (4 / 1 v / v) solvent and measured. 19 The reference for F-NMR chemical shifts is the hexafluorobenzene peak at −164.7 ppm. 1 The reference for H-NMR chemical shifts is the acetone peak at 2.2 ppm.
[0171] The fluorine-containing ether compound of this embodiment is preferably subjected to molecular weight fractionation by an appropriate method to make the molecular weight dispersity (ratio of weight average molecular weight (Mw) / number average molecular weight (Mn)) 1.3 or less. In this embodiment, the method for molecular weight fractionation is not particularly limited, and for example, molecular weight fractionation by silica gel column chromatography, gel permeation chromatography (GPC), or the like, molecular weight fractionation by supercritical extraction, or the like can be used.
[0172] "Production Method" The production method of the fluorinated ether compound of this embodiment is not particularly limited, and the compound can be produced using a conventionally known production method. The fluorinated ether compound of this embodiment can be produced, for example, using the production method shown below.
[0173] (R 1 and R 3 In formula (1), R 1 and R 3 and R in formula (1) are the same as each other. 2 At both ends of the perfluoropolyether chain corresponding to 2 A fluorine-based compound in which a hydroxyl group (OH) is arranged is prepared.
[0174] Next, the hydroxyl groups of the hydroxymethyl groups located at both ends of the fluorine-based compound and the R 1 A group (=R 3 The epoxy group of the epoxy compound having R 2 At both ends of the perfluoropolyether chain corresponding to1 A group corresponding to (=R 3 A compound having a group corresponding to
[0175] R in formula (1) 1 A group (=R 3 As the epoxy compound having a group (which is a group represented by the formula (5-1) to (5-16) and the formula (5-24), for example, compounds represented by the following formulas (5-1) to (5-16) and the following formula (5-24) can be used. In the above reaction, instead of the epoxy compound, compounds represented by the formula (1) 1 A group (=R 3 and a compound having a leaving group (hereinafter, sometimes simply referred to as a "compound having a leaving group"). As the compound having a leaving group, compounds represented by the following formulas (5-25) to (5-27) can be used. MOM in formulas (5-25) and (5-26) represents a methoxymethyl group. Ts in formulas (5-25) to (5-27) represents a tosyl group.
[0176]
[0177]
[0178] When a fluorine-based compound is reacted with an epoxy compound (or a compound having a leaving group), the hydroxyl group of the epoxy compound (or a compound having a leaving group) may be protected with an appropriate protecting group before the reaction with the fluorine-based compound.
[0179] An epoxy compound (for example, an epoxy compound represented by formula (5-1)) can be produced by a method of reacting an alcohol compound, which may be appropriately protected, with a halogen compound having an epoxy group, as shown in the following formula (6-1).
[0180]
[0181] An epoxy compound (e.g., an epoxy compound represented by formula (5-5)) may be produced, for example, as shown in formula (6-2) below, by a method in which an alcohol compound having a vinyl group is reacted with a halogen compound having an alcohol which may be appropriately protected, and then the resulting compound is oxidized by the action of m-chloroperbenzoic acid (mCPBA).
[0182]
[0183] An epoxy compound (e.g., an epoxy compound represented by formula (5-10)) may be produced by, for example, reacting a diol compound with a halogen compound having an alcohol which may be appropriately protected and a halogen compound having an epoxy group in that order, as shown in the following formula (6-3):
[0184]
[0185] The epoxy compound (or compound having a leaving group) may be a commercially available product.
[0186] By carrying out the above steps, R 1 and R 3 A compound in which
[0187] In formula (1), R 1 and R 3 To prepare a compound in which
[0188] First, R in formula (1) 2 At both ends of the perfluoropolyether chain corresponding to 2 A fluorine-based compound having a vinyl group at both ends is prepared. The hydroxyl groups of the hydroxymethyl groups at both ends of the fluorine-based compound are reacted with a halogen compound having a vinyl group at the end. This results in a compound having a vinyl group at both ends of a chain structure containing a perfluoropolyether chain.
[0189] Subsequently, the vinyl groups at both ends of the obtained compound are oxidized to obtain a compound having epoxy groups at both ends of a chain structure containing a perfluoropolyether chain. The epoxy groups at both ends are subjected to a ring-opening reaction to convert to a 1,2-diol. By carrying out the above steps, the compound represented by R 1 and R 3 A compound in which
[0190] (R 1 and R 3In formula (1), R 1 and R 3 To produce a compound different from 2 At both ends of the perfluoropolyether chain corresponding to 2 A fluorine-based compound in which a hydroxyl group (OH) is arranged is prepared.
[0191] Next, the hydroxyl group of the hydroxymethyl group located at one end of the fluorine-based compound and the R 1 By this, the epoxy group of the epoxy compound having the group R 2 At one end of the perfluoropolyether chain corresponding to 1 An intermediate compound 1 is obtained (first reaction) having a group corresponding to
[0192] Next, the intermediate compound 1 and R 3 In the first reaction and / or the second reaction, a compound having a leaving group may be used in place of the epoxy compound.
[0193] R 1 and R 3 and (5-23) are different, one of which is an end group represented by formula (2) and the other is an end group not corresponding to formula (2), the epoxy compounds corresponding to the end group not corresponding to formula (2) can be, for example, epoxy compounds represented by the following formulas (5-17) to (5-23). In formulas (5-17), (5-18), and (5-21) to (5-23), THP represents a tetrahydropyranyl group.
[0194]
[0195] By carrying out the above steps, R 1 and R 3 A compound different from the above is obtained.
[0196] [Lubricant for magnetic recording media] The lubricant for magnetic recording media of this embodiment contains a fluorine-containing ether compound represented by the above formula (1). The lubricant of this embodiment can be used by mixing, as needed, with known materials used as lubricant materials, as long as the properties resulting from the inclusion of the fluorine-containing ether compound represented by the above formula (1) are not impaired.
[0197] Specific examples of known materials include FOMBLIN (registered trademark) ZDIAC, FOMBLIN ZDEAL, FOMBLIN AM-2001 (all manufactured by Solvay Solexis), Moresco A20H (manufactured by Moresco), etc. The known material to be mixed with the lubricant of this embodiment preferably has a number average molecular weight of 1,000 to 10,000.
[0198] When the lubricant of the present embodiment contains a material other than the fluorinated ether compound represented by the above formula (1), the content of the fluorinated ether compound represented by the above formula (1) in the lubricant of the present embodiment is preferably 70% by mass or more, more preferably 90% by mass or more, and even more preferably 95% by mass or more.
[0199] The lubricant of this embodiment contains the fluorine-containing ether compound represented by the above formula (1), and therefore can form a lubricating layer that has excellent corrosion resistance and can suppress spin-off.
[0200] [Magnetic Recording Medium] The magnetic recording medium of this embodiment has at least a magnetic layer, a protective layer, and a lubricating layer sequentially provided on a substrate. In the magnetic recording medium of this embodiment, one or more underlayers can be provided between the substrate and the magnetic layer as needed. In addition, at least one of an adhesive layer and a soft magnetic layer can be provided between the underlayer and the substrate.
[0201] 1 is a schematic cross-sectional view showing one embodiment of a magnetic recording medium of the present invention. The magnetic recording medium 10 of this embodiment has a structure in which an adhesive layer 12, a soft magnetic layer 13, a first underlayer 14, a second underlayer 15, a magnetic layer 16, a protective layer 17, and a lubricating layer 18 are sequentially provided on a substrate 11.
[0202] "Substrate" The substrate 11 may be, for example, a non-magnetic substrate in which a film made of NiP or a NiP alloy is formed on a base made of a metal or alloy material such as Al or an Al alloy. Alternatively, the substrate 11 may be a non-magnetic substrate made of a non-metallic material such as glass, ceramics, silicon, silicon carbide, carbon, or resin, or a non-magnetic substrate in which a film of NiP or a NiP alloy is formed on a base made of such a non-metallic material.
[0203] "Adhesion Layer" The adhesion layer 12 prevents the progress of corrosion of the substrate 11, which occurs when the substrate 11 and the soft magnetic layer 13 provided on the adhesion layer 12 are disposed in contact with each other. The material of the adhesion layer 12 can be appropriately selected from, for example, Cr, Cr alloy, Ti, Ti alloy, CrTi, NiAl, AlRu alloy, etc. The adhesion layer 12 can be formed by, for example, a sputtering method.
[0204] "Soft Magnetic Layer" The soft magnetic layer 13 preferably has a structure in which a first soft magnetic film, an intermediate layer made of a Ru film, and a second soft magnetic film are laminated in this order. That is, the soft magnetic layer 13 preferably has a structure in which the intermediate layer made of a Ru film is sandwiched between two soft magnetic films, and the soft magnetic films above and below the intermediate layer are anti-ferro-coupling (AFC).
[0205] Examples of materials for the first and second soft magnetic films include CoZrTa alloys and CoFe alloys. It is preferable to add Zr, Ta, or Nb to the CoFe alloy used for the first and second soft magnetic films. This promotes the amorphization of the first and second soft magnetic films. As a result, it is possible to improve the orientation of the first underlayer (seed layer) and reduce the flying height of the magnetic head. The soft magnetic layer 13 can be formed, for example, by sputtering.
[0206] "First Underlayer" The first underlayer 14 is a layer that controls the orientation and crystal size of the second underlayer 15 and magnetic layer 16 that are provided thereon. Examples of the first underlayer 14 include a Cr layer, a Ta layer, a Ru layer, or a CrMo alloy layer, a CoW alloy layer, a CrW alloy layer, a CrV alloy layer, and a CrTi alloy layer. The first underlayer 14 can be formed by, for example, a sputtering method.
[0207] "Second Underlayer" The second underlayer 15 is a layer that controls the orientation of the magnetic layer 16 so that it is favorable. The second underlayer 15 is preferably a layer made of Ru or a Ru alloy. The second underlayer 15 may be a layer consisting of a single layer, or may be made of multiple layers. When the second underlayer 15 consists of multiple layers, all of the layers may be made of the same material, or at least one layer may be made of a different material. The second underlayer 15 can be formed, for example, by a sputtering method.
[0208] "Magnetic Layer" The magnetic layer 16 is made of a magnetic film whose axis of easy magnetization is oriented perpendicular or horizontal to the substrate surface. The magnetic layer 16 is a layer containing Co and Pt. To improve the SNR characteristics, the magnetic layer 16 may be a layer containing oxides, Cr, B, Cu, Ta, Zr, etc. Examples of oxides contained in the magnetic layer 16 include SiO 2 , SiO, Cr 2 O 3 , CoO, Ta 2 O 3 , TiO 2 etc.
[0209] The magnetic layer 16 may be composed of a single layer, or may be composed of multiple magnetic layers made of materials with different compositions. For example, when the magnetic layer 16 is composed of three layers, a first magnetic layer, a second magnetic layer, and a third magnetic layer stacked in this order from the bottom, the first magnetic layer preferably has a granular structure made of a material containing Co, Cr, and Pt and further containing an oxide. As the oxide contained in the first magnetic layer, it is preferable to use an oxide of, for example, Cr, Si, Ta, Al, Ti, Mg, Co, or the like. Among them, TiO is particularly preferable. 2 , Cr 2 O3 , SiO 2 The first magnetic layer is preferably made of a composite oxide containing two or more kinds of oxides. 2 O 3 -SiO 2 , Cr 2 O 3 -TiO 2 , SiO 2 -TiO 2 The first magnetic layer may contain, in addition to Co, Cr, Pt, and oxides, one or more elements selected from B, Ta, Mo, Cu, Nd, W, Nb, Sm, Tb, Ru, and Re.
[0210] The second magnetic layer can be made of the same material as the first magnetic layer. The second magnetic layer preferably has a granular structure. The third magnetic layer preferably has a non-granular structure made of a material containing Co, Cr, and Pt and not containing oxides. In addition to Co, Cr, and Pt, the third magnetic layer can contain one or more elements selected from B, Ta, Mo, Cu, Nd, W, Nb, Sm, Tb, Ru, Re, and Mn.
[0211] When the magnetic layer 16 is formed of multiple magnetic layers, it is preferable to provide a non-magnetic layer between adjacent magnetic layers. When the magnetic layer 16 is formed of three layers, namely, a first magnetic layer, a second magnetic layer, and a third magnetic layer, it is preferable to provide a non-magnetic layer between the first magnetic layer and the second magnetic layer and between the second magnetic layer and the third magnetic layer.
[0212] The non-magnetic layer provided between adjacent magnetic layers of the magnetic layer 16 can be suitably made of, for example, Ru, a Ru alloy, a CoCr alloy, or a CoCrX1 alloy (X1 represents one or more elements selected from Pt, Ta, Zr, Re, Ru, Cu, Nb, Ni, Mn, Ge, Si, O, N, W, Mo, Ti, V, and B).
[0213] The non-magnetic layer provided between adjacent magnetic layers of the magnetic layer 16 is preferably made of an alloy material containing an oxide, a metal nitride, or a metal carbide. Specifically, the oxide may be, for example, SiO 2 , Al2 O 3 , Ta 2 O 5 , Cr 2 O 3 , MgO, Y 2 O 3 , TiO 2 Examples of metal nitrides that can be used include AlN and Si. 3 N 4 , TaN, CrN, etc. can be used as the metal carbide. TaC, BC, SiC, etc. can be used as the metal carbide. The non-magnetic layer can be formed by, for example, sputtering.
[0214] To achieve higher recording density, the magnetic layer 16 is preferably a magnetic layer for perpendicular magnetic recording, in which the axis of easy magnetization is oriented perpendicular to the substrate surface. The magnetic layer 16 may also be a magnetic layer for in-plane magnetic recording. The magnetic layer 16 may be formed by any conventionally known method, such as vapor deposition, ion beam sputtering, or magnetron sputtering. The magnetic layer 16 is usually formed by sputtering.
[0215] "Protective Layer" The protective layer 17 protects the magnetic layer 16. The protective layer 17 may be composed of a single layer or multiple layers. A carbon-based protective layer is preferably used as the protective layer 17, and an amorphous carbon protective layer is particularly preferred. If the protective layer 17 is a carbon-based protective layer, the interaction with the polar groups (particularly hydroxyl groups) contained in the fluorine-containing ether compound in the lubricating layer 18 is further enhanced, which is preferable.
[0216] The adhesion between the carbon-based protective layer and the lubricating layer 18 can be controlled by using hydrogenated carbon and / or nitrogenated carbon for the carbon-based protective layer and adjusting the hydrogen and / or nitrogen contents in the carbon-based protective layer. The hydrogen content in the carbon-based protective layer is preferably 3 atomic % to 20 atomic % as measured by hydrogen forward scattering (HFS). The nitrogen content in the carbon-based protective layer is preferably 4 atomic % to 15 atomic % as measured by X-ray photoelectron spectroscopy (XPS).
[0217] The hydrogen and / or nitrogen contained in the carbon-based protective layer does not need to be uniformly contained throughout the carbon-based protective layer. The carbon-based protective layer is preferably a compositionally graded layer, for example, in which nitrogen is contained on the lubricating layer 18 side of the protective layer 17 and hydrogen is contained on the magnetic layer 16 side of the protective layer 17. In this case, the adhesion between the magnetic layer 16 and the lubricating layer 18 and the carbon-based protective layer is further improved.
[0218] The thickness of the protective layer 17 is preferably 1 nm to 7 nm. When the thickness of the protective layer 17 is 1 nm or more, sufficient performance as the protective layer 17 can be obtained. When the thickness of the protective layer 17 is 7 nm or less, it is preferable from the viewpoint of making the protective layer 17 thinner.
[0219] The protective layer 17 can be formed by sputtering using a target material containing carbon, chemical vapor deposition (CVD) using a hydrocarbon raw material such as ethylene or toluene, ion beam deposition (IBD), or the like. When a carbon-based protective layer is formed as the protective layer 17, it can be formed by DC magnetron sputtering, for example. In particular, when a carbon-based protective layer is formed as the protective layer 17, it is preferable to form an amorphous carbon protective layer by plasma CVD. An amorphous carbon protective layer formed by plasma CVD has a uniform surface with little roughness.
[0220] "Lubricant Layer" The lubricant layer 18 prevents contamination of the magnetic recording medium 10. The lubricant layer 18 also reduces the frictional force of the magnetic head of the magnetic recording and reproducing device sliding on the magnetic recording medium 10, thereby improving the durability of the magnetic recording medium 10. As shown in FIG. 1 , the lubricant layer 18 is formed on and in contact with the protective layer 17. The lubricant layer 18 is formed by applying the magnetic recording medium lubricant of the above-mentioned embodiment onto the protective layer 17. Therefore, the lubricant layer 18 contains the above-mentioned fluorine-containing ether compound.
[0221] When the protective layer 17 disposed below the lubricating layer 18 is a carbon-based protective layer, the lubricating layer 18 bonds with the protective layer 17 with particularly high bonding strength. As a result, even if the thickness of the lubricating layer 18 is thin, it becomes easier to obtain a magnetic recording medium 10 in which the surface of the protective layer 17 is covered with a high coverage, and contamination of the surface of the magnetic recording medium 10 can be effectively prevented.
[0222] The average thickness of the lubricating layer 18 is preferably 0.5 nm (5 Å) to 2.0 nm (20 Å), and more preferably 0.5 nm (5 Å) to 1.2 nm (12 Å). When the average thickness of the lubricating layer 18 is 0.5 nm or more, the lubricating layer 18 is formed with a uniform thickness without forming an island or mesh-like structure. This allows the lubricating layer 18 to cover the surface of the protective layer 17 with a high coverage. Furthermore, by setting the average thickness of the lubricating layer 18 to 2.0 nm or less, the lubricating layer 18 can be made sufficiently thin, and the flying height of the magnetic head can be sufficiently reduced.
[0223] "Method for forming lubricating layer" As a method for forming the lubricating layer 18, for example, a method is given in which a magnetic recording medium in the middle of manufacture in which each layer up to the protective layer 17 is formed on the substrate 11, and a solution for forming a lubricating layer is applied to the protective layer 17 and dried.
[0224] The lubricant layer-forming solution can be obtained by dispersing and dissolving the magnetic recording medium lubricant of the above-described embodiment in a solvent as needed, and adjusting the viscosity and concentration to suit the coating method. Examples of solvents used in the lubricant layer-forming solution include fluorine-based solvents such as Vertrel (registered trademark) XF (trade name, manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd.) and Asahiklin (registered trademark) AE-3000 (trade name, manufactured by AGC).
[0225] The method for applying the lubricant layer-forming solution is not particularly limited, and examples thereof include spin coating, spraying, paper coating, and dipping. When using the dipping method, the following method can be used, for example. First, the substrate 11 on which each layer up to the protective layer 17 has been formed is immersed in the lubricant layer-forming solution placed in the immersion tank of a dip coating device. Next, the substrate 11 is pulled out of the immersion tank at a predetermined speed. In this way, the lubricant layer-forming solution is applied to the surface of the protective layer 17 of the substrate 11. By using the dipping method, the lubricant layer-forming solution can be applied uniformly to the surface of the protective layer 17, and the lubricant layer 18 can be formed on the protective layer 17 with a uniform film thickness.
[0226] In this embodiment, it is preferable to subject the substrate 11 on which the lubricating layer 18 is formed to a heat treatment. By subjecting the substrate 11 to a heat treatment, the adhesion between the lubricating layer 18 and the protective layer 17 is improved, and the adhesive strength between the lubricating layer 18 and the protective layer 17 is also improved. The heat treatment temperature is preferably 100°C to 180°C, and more preferably 100°C to 160°C. A heat treatment temperature of 100°C or higher sufficiently improves the adhesion between the lubricating layer 18 and the protective layer 17. Furthermore, by setting the heat treatment temperature to 180°C or lower, thermal decomposition of the lubricating layer 18 due to the heat treatment can be prevented. The heat treatment time can be adjusted appropriately depending on the heat treatment temperature, and is preferably 10 minutes to 120 minutes.
[0227] In this embodiment, in order to further improve the adhesion of the lubricating layer 18 to the protective layer 17, the lubricating layer 18 may be irradiated with ultraviolet (UV) rays before or after the heat treatment.
[0228] The magnetic recording medium 10 of this embodiment has at least a magnetic layer 16, a protective layer 17, and a lubricating layer 18 sequentially formed on a substrate 11. In the magnetic recording medium 10 of this embodiment, a lubricating layer 18 containing the above-mentioned fluorine-containing ether compound is formed on and in contact with the protective layer 17. This lubricating layer 18 has good corrosion resistance and can suppress spin-off, even though it is thin. Therefore, the magnetic recording medium 10 of this embodiment has excellent reliability, particularly corrosion resistance and spin-off suppression, and durability. As a result, the magnetic recording medium 10 of this embodiment can contribute to reducing magnetic spacing, reduce the magnetic head flying height (e.g., 10 nm or less), and operate stably for long periods of time, even in harsh environments associated with diverse applications. Therefore, the magnetic recording medium 10 of this embodiment is particularly suitable as a magnetic disk to be installed in a magnetic disk device using the LUL (Load Unload) method.
[0229] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0230] [Example 1] The compound represented by the above formula (AA) was obtained by the following method. 2 CF2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 5 g of a compound (number average molecular weight: 1000, molecular weight distribution: 1.1) represented by formula (5-1), 2.70 g of the compound represented by formula (5-1), and 5 mL of t-butanol were charged and stirred at room temperature until homogenous to obtain a mixture. 0.30 g of potassium tert-butoxide was added to this mixture, and the mixture was reacted at 70°C for 16 hours with stirring.
[0231] The compound represented by formula (5-1) was synthesized by protecting the 1,2-diol moiety of 1,2,4-butanetriol with acetone, and then reacting the hydroxyl group at the 4-position with epibromohydrin.
[0232] After the reaction, the reaction solution obtained was returned to room temperature, and 10 g of a 10% hydrogen chloride-methanol solution (hydrogen chloride-methanol reagent (5-10%), manufactured by Tokyo Chemical Industry Co., Ltd.) was added, followed by stirring at room temperature for 4 hours. Thereafter, the reaction solution was transferred little by little to a separatory funnel containing 25 mL of saturated aqueous sodium bicarbonate, and extracted twice with 50 mL of ethyl acetate. The organic layer was washed with 25 mL of brine, 25 mL of saturated aqueous sodium bicarbonate, and 25 mL of brine in that order, and dehydrated with anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (AA) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0233] The obtained compound (AA) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0234] [Example 2] A compound represented by the above formula (AB) was obtained by the method shown below. The same procedure as in Example 1 was carried out, except that a compound represented by formula (5-2) was used instead of a compound represented by formula (5-1), to obtain compound (AB) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0235] The compound represented by formula (5-2) was synthesized by protecting the 1,2-diol moiety of 1,2,6-hexanetriol with acetone, and then reacting the hydroxyl group at the 6-position with epibromohydrin.
[0236] The obtained compound (AB) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (12H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0237] [Example 3] A compound represented by the above formula (AC) was obtained by the method shown below. Compound (AC) (Rf in formula (AC)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-3) was used instead of a compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0238] The compound represented by formula (5-3) was synthesized by protecting the 1,2-diol moiety of 1,2,8-octanetriol with acetone, and then reacting the hydroxyl group at the 8-position with epibromohydrin.
[0239] The obtained compound (AC) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (20H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0240] [Example 4] A compound represented by the above formula (AD) was obtained by the method shown below. Compound (AD) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0241] The compound represented by formula (5-4) was synthesized by the following method. After protecting the 1,2-diol moiety of 1,2,4-butanetriol with acetone, the hydroxyl group at the 4-position was brominated and reacted with 3-buten-1-ol to obtain the compound. The vinyl group of the obtained compound was then oxidized with m-chloroperbenzoic acid (mCPBA) to synthesize the compound.
[0242] The obtained compound (AD) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6): δ [ppm] = 1.65-1.85 (8H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0243] [Example 5] A compound represented by the above formula (AE) was obtained by the method shown below. Compound (AE) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0244] The compound represented by formula (5-5) was synthesized by reacting a compound obtained by brominating the hydroxyl group of solketal (2,2-dimethyl-1,3-dioxolane-4-methanol) with 3-buten-1-ol, and oxidizing the vinyl group of the resulting compound with m-chloroperbenzoic acid (mCPBA).
[0245] The obtained compound (AE) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0246] [Example 6] A compound represented by the above formula (AF) was obtained by the method shown below. Compound (AF) (Rf in formula (AF)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-6) was used instead of a compound represented by formula (5-1).1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0247] The compound represented by formula (5-6) was synthesized by reacting a compound obtained by brominating the hydroxyl group of solketal with 5-hexen-1-ol, and then oxidizing the vinyl group of the resulting compound with m-chloroperbenzoic acid (mCPBA).
[0248] The obtained compound (AF) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (12H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0249] [Example 7] A compound represented by the above formula (AG) was obtained by the method shown below. Compound (AG) (Rf in formula (AG)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-7) was used instead of a compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0250] The compound represented by formula (5-7) was synthesized by reacting a compound obtained by brominating the hydroxyl group of solketal with 7-octen-1-ol, and then oxidizing the vinyl group of the resulting compound with m-chloroperbenzoic acid (mCPBA).
[0251] The obtained compound (AG) 1 H-NMR and 19F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (20H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0252] [Example 8] A compound represented by the above formula (AH) was obtained by the method shown below. Compound (AH) (Rf in formula (AH)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-8) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0253] The compound represented by formula (5-8) was synthesized by the following method. The epoxy group of 1,2-epoxy-5-hexene was ring-opened using dilute sulfuric acid. The 1,2-diol moiety generated by the ring-opening was protected with acetone, and the vinyl group of the resulting compound was oxidized using m-chloroperbenzoic acid (mCPBA).
[0254] The obtained compound (AH) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (8H), 3.40-3.85 (18H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0255] [Example 9] A compound represented by the above formula (AI) was obtained by the method shown below. Compound (AI) (Rf in formula (AI)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-9) was used instead of a compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0256] The compound represented by formula (5-9) was synthesized by the following method. One of the vinyl groups of 1,7-octadiene was oxidized using m-chloroperbenzoic acid (mCPBA). The epoxy group generated by the oxidation was ring-opened using dilute sulfuric acid. The 1,2-diol moiety generated by the ring-opening was protected with acetone, and the vinyl group of the resulting compound was oxidized using mCPBA.
[0257] The obtained compound (AI) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (16H), 3.40-3.85 (18H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0258] [Example 10] A compound represented by the above formula (AJ) was obtained by the method shown below. Compound (AJ) (Rf in formula (AJ)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-10) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0259] The compound represented by formula (5-10) was synthesized by reacting one of the hydroxyl groups of 1,3-propanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0260] The obtained compound (AJ) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (34H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0261] [Example 11] A compound represented by the above formula (AK) was obtained by the method shown below. Compound (AK) (Rf in formula (AK)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-11) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0262] The compound represented by formula (5-11) was synthesized by reacting one of the hydroxyl groups of 2,2-dimethyl-1,3-propanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0263] The obtained compound (AK) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.20-1.25 (12H), 3.40-3.85 (34H), 3.85-4.10 (4H) 19 F-NMR (acetone-D6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0264] [Example 12] A compound represented by the above formula (AL) was obtained by the method shown below. Compound (AL) (Rf in formula (AL)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-12) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0265] The compound represented by formula (5-12) was synthesized by reacting one of the hydroxyl groups of 1,4-butanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0266] The obtained compound (AL) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (8H), 3.40-3.85 (34H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0267] [Example 13] A compound represented by the above formula (AM) was obtained by the method shown below. Compound (AM) (Rf in formula (AM)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-13) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0268] The compound represented by formula (5-13) was synthesized by reacting one of the hydroxyl groups of 2,3-dimethyl-1,4-butanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0269] The obtained compound (AM) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.20-1.25 (12H), 1.65-1.85 (4H), 3.40-3.85 (34H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0270] [Example 14] A compound represented by the above formula (AN) was obtained by the method shown below. Compound (AN) (Rf in formula (AN)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-14) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0271] The compound represented by formula (5-14) was synthesized by reacting one of the hydroxyl groups of 1,8-octanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0272] The obtained compound (AN) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (24H), 3.40-3.85 (34H), 3.85-4.10 (4H)19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0273] [Example 15] A compound represented by the above formula (AO) was obtained by the method shown below. The same procedure as in Example 1 was carried out, except that a compound represented by formula (5-15) was used instead of the compound represented by formula (5-1), to obtain compound (AO) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0274] The compound represented by formula (5-15) was synthesized by reacting one of the hydroxyl groups of 2,2,3,3-tetrafluoro-1,4-butanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0275] The obtained compound (AO) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 3.40-3.85 (26H), 3.85-4.10 (12H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F), -128.5 to 130.0 (8F)
[0276] [Example 16] A compound represented by the above formula (AP) was obtained by the method shown below. Compound (AP) (Rf in formula (AP)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-16) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0277] The compound represented by formula (5-16) was synthesized by reacting one hydroxyl group of 2,2,3,3,4,4,5,5,6,6,7,7-dodecafluoro-1,8-octanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin.
[0278] The obtained compound (AP) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 3.40-3.85 (26H), 3.85-4.10 (12H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F), -122.5 to -124.5 (16F), -128.5 to 130.0 (8F)
[0279] [Example 17] The compound represented by the above formula (AQ) was obtained by the following method. HOCH 2 CF 2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 5 g of a compound (number average molecular weight: 1000, molecular weight distribution: 1.1) represented by the formula OH (where h, representing the average degree of polymerization, is 4.5, and i, representing the average degree of polymerization, is 4.5), 4.50 g of 1-bromo-4-pentene, and 10 mL of N,N-dimethylformamide were charged and stirred at room temperature until homogeneous to obtain a mixture. 1.20 g of sodium hydride (purity: 60%, containing mineral oil) was added to this mixture, and the mixture was reacted with stirring at 70°C for 16 hours.
[0280] The reaction product obtained after the reaction was cooled to 25°C, transferred to a separatory funnel containing 50 mL of water, and extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated over anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 4.76 g of the compound represented by the following formula (7-1) as an intermediate compound.
[0281] (Rf in formula (7-1) 1 is the PFPE chain represented by the above formula (4-1). 1 In the formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0282] Subsequently, under a nitrogen gas atmosphere, 4.76 g of the compound represented by formula (7-1), which is the intermediate compound obtained above, 20 mL of methylene chloride, and 3.15 g of m-chloroperbenzoic acid (mCPBA (purity 73%, water-containing)) were placed in a 100 mL recovery flask, and the mixture was stirred at room temperature for 16 hours to cause a reaction.
[0283] After the reaction, 50 mL of an aqueous solution of 3.18 g of sodium sulfite was added to the reaction solution obtained to deactivate excess mCPBA. The resulting solid was filtered off, transferred to a separatory funnel, and extracted three times with 100 mL of methylene chloride. The organic layer was washed with water and dehydrated over anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 4.21 g of the compound represented by the following formula (7-2) as an intermediate compound.
[0284] (Rf in formula (7-2) 1 is the PFPE chain represented by the above formula (4-1). 1 In the formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0285] Subsequently, in a nitrogen gas atmosphere, 4.21 g of the compound represented by formula (7-2), which is the intermediate compound obtained above, 20 mL of acetone, and 20 mL of 10% diluted sulfuric acid were placed in a 100 mL recovery flask, and the mixture was stirred at room temperature for 16 hours to cause a reaction.
[0286] After the reaction, 20 mL of saturated aqueous sodium bicarbonate solution was added to the reaction solution obtained to neutralize it, and the resulting solid was filtered off. Thereafter, the solution was transferred to a separatory funnel and extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated with anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (AQ) (Rf in formula (AQ) 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0287] The obtained compound (AQ) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (8H), 3.40-3.85 (14H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0288] [Example 18] A compound represented by the above formula (AR) was obtained by the following method. The same procedure as in Example 17 was carried out except that 1-bromo-7-octene was used instead of 1-bromo-4-pentene, to obtain compound (AR) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0289] The obtained compound (AR) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (20H), 3.40-3.85 (14H), 3.85-4.10 (4H) 19F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0290] Example 19 The compound represented by the above formula (AS) was obtained by the method shown below.
[0291] (First reaction) HOCH was placed in a 100 mL recovery flask under a nitrogen gas atmosphere. 2 CF 2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 12.5 g of a compound (number average molecular weight: 1000, molecular weight distribution: 1.1) represented by formula (5-1), 2.70 g of the compound represented by formula (5-1), and 12 mL of t-butanol were charged and stirred at room temperature until homogenous to obtain a mixture. 1.10 g of potassium tert-butoxide was added to this mixture, and the mixture was reacted at 70°C for 16 hours with stirring.
[0292] The reaction product obtained after the reaction was cooled to 25°C, transferred to a separatory funnel containing 100 mL of water, and extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated over anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain 7.21 g of a compound represented by the following formula (8) as intermediate compound 1.
[0293] (Rf in formula (8) 1 is the PFPE chain represented by the above formula (4-1). 1 In the formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0294] (Second Reaction) Subsequently, under a nitrogen gas atmosphere, 7.21 g of the compound represented by formula (8), which is intermediate compound 1 obtained above, 2.70 g of the compound represented by formula (5-5), and 20 mL of t-butanol were placed in a 100 mL recovery flask and stirred at room temperature until a homogeneous mixture was obtained. 0.55 g of potassium tert-butoxide was added to this mixture, and the mixture was allowed to react with stirring at 70°C for 16 hours.
[0295] After the reaction, the reaction solution obtained was returned to room temperature, and 50 g of a 10% hydrogen chloride-methanol solution (hydrogen chloride-methanol reagent (5-10%), manufactured by Tokyo Chemical Industry Co., Ltd.) was added, followed by stirring at room temperature for 4 hours. Thereafter, the reaction solution was transferred little by little to a separatory funnel containing 100 mL of saturated aqueous sodium bicarbonate, and extracted twice with 200 mL of ethyl acetate. The organic layer was washed with 100 mL of brine, 100 mL of saturated aqueous sodium bicarbonate, and 100 mL of brine in that order, and dehydrated with anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (AS) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0296] The obtained compound (AS) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0297] [Example 20] A compound represented by the above formula (BA) was obtained by the method shown below. Compound (BA) (Rf in formula (BA)) was obtained by the same procedure as in Example 19, except that a compound represented by formula (5-17) was used instead of the compound represented by formula (5-5).1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0298] The compound represented by formula (5-17) was synthesized by protecting the hydroxyl group of ethylene glycol monoallyl ether with dihydropyran, and then oxidizing the vinyl group with m-chloroperbenzoic acid (mCPBA).
[0299] The obtained compound (BA) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (2H), 3.40-3.85 (24H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0300] [Example 21] A compound represented by the above formula (BB) was obtained by the method shown below. Compound (BB) (Rf in formula (BB)) was obtained by the same procedure as in Example 19, except that a compound represented by formula (5-18) was used instead of the compound represented by formula (5-5). 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0301] The compound represented by formula (5-18) was synthesized by the following method. Epichlorohydrin was reacted with 3-buten-1-ol in a molar amount twice that of the epichlorohydrin. The hydroxyl group generated by the reaction was protected with dihydropyran. One of the vinyl groups of the compound obtained by the reaction was oxidized with m-chloroperbenzoic acid (mCPBA).
[0302] The obtained compound (BB) 1 H-NMR and19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (27H), 3.85-4.10 (4H), 5.20-5.80 (3H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0303] [Example 22] A compound represented by the above formula (BC) was obtained by the method shown below. Compound (BC) (Rf in formula (BC)) was obtained by the same procedure as in Example 19, except that a compound represented by formula (5-19) was used instead of the compound represented by formula (5-5). 1 is the PFPE chain represented by the above formula (4-1). 1 In this example, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0304] The compound represented by formula (5-19) was synthesized by reacting the hydroxyl group of 2-acetamidoethanol with epibromohydrin.
[0305] The obtained compound (BC) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (2H), 1.90 (3H), 3.40-3.85 (23H), 3.85-4.10 (4H), 6.70-6.80 (1H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0306] [Example 23] A compound represented by the above formula (BD) was obtained by the method shown below. Compound (BD) (Rf in formula (BD)) was obtained by the same procedure as in Example 19, except that a compound represented by formula (5-20) was used instead of the compound represented by formula (5-5). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0307] The compound represented by formula (5-20) was synthesized by reacting the hydroxyl group of 3-cyanopropanol with epibromohydrin.
[0308] The obtained compound (BD) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 1.90-2.00 (2H), 3.40-3.85 (21H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0309] [Example 24] A compound represented by the above formula (BE) was obtained by the method shown below. Compound (BE) (Rf in formula (BE)) was obtained by the same procedure as in Example 19, except that a compound represented by formula (5-21) was used instead of the compound represented by formula (5-5). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0310] The compound represented by formula (5-21) was synthesized by protecting the hydroxyl group of 3-buten-1-ol with dihydropyran, and then oxidizing the vinyl group with m-chloroperbenzoic acid (mCPBA).
[0311] The obtained compound (BE) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (20H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0312] [Example 25] A compound represented by the above formula (BF) was obtained by the method shown below. Compound (BF) (Rf in formula (BF)) was obtained by the same procedure as in Example 19, except that a compound represented by formula (5-22) was used instead of the compound represented by formula (5-5). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0313] The compound represented by formula (5-22) was synthesized by protecting the two hydroxyl groups of 3-allyloxy-1,2-propanediol with dihydropyran, and then oxidizing the vinyl group with m-chloroperbenzoic acid (mCPBA).
[0314] The obtained compound (BF) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (2H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0315] [Example 26] The compound represented by the above formula (BG) was obtained by the method shown below. 2 CF 2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 Instead of the compound represented by OH, 2 CF 2 CF 2 O (CF 2 CF 2 CF 2 O) j CF 2 CF 2 CH 2 The same procedure as in Example 1 was carried out to obtain compound (BG) (Rf in formula (BG)) except that a compound (number average molecular weight: 1,000, molecular weight distribution: 1.1) represented by the formula OH (where j, representing the average degree of polymerization, is 4.5) was used. 2 is the PFPE chain represented by the above formula (4-2). 2 In this formula, j, which indicates the average degree of polymerization, is 4.5.
[0316] The obtained compound (BG) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0317] [Example 27] A compound represented by the above formula (BH) was obtained by the method shown below. 2 CF 2 O (CF 2 CF 2 O) h (CF 2 O)i CF 2 CH 2 Instead of the compound represented by OH, 2 CF 2 CF 2 CF 2 O (CF 2 CF 2 CF 2 CF 2 O) k CF 2 CF 2 CF 2 CH 2 The same procedure as in Example 1 was carried out to obtain a compound (BH) (Rf in formula (BH)) (number average molecular weight: 1,000, molecular weight distribution: 1.1) represented by the formula OH (where k, representing the average degree of polymerization, is 3.0) was used. 3 is the PFPE chain represented by the above formula (4-3). 3 In this example, k, which indicates the average degree of polymerization, is 3.0.
[0318] The obtained compound (BH) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (16F), -122.5 (4F), -126.0 (12F), -129.0 to -128.0 (4F)
[0319] [Example 28] A compound represented by the above formula (CA) was obtained by the method shown below. 2 CF 2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 OH (where h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5),2 CF 2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 The same procedure as in Example 1 was carried out, except that a compound represented by the formula (CA) (Rf 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 7.0, and i representing the average degree of polymerization is 0. 3.15 g of compound (CA) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -78.5 (4F), -91.0 to -88.5 (28F)
[0320] [Example 29] A compound represented by the above formula (CB) was obtained by the method shown below. Compound (CB) (Rf in formula (CB)) was obtained by the same procedure as in Example 28, except that a compound represented by formula (5-5) was used instead of a compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the above formula, h representing the average degree of polymerization is 7.0, and i representing the average degree of polymerization is 0. 3.08 g of compound (CB) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D6 ): δ [ppm] = -78.5 (4F), -91.0 to -88.5 (28F)
[0321] [Example 30] A compound represented by the above formula (CC) was obtained by the method shown below. Compound (CC) (Rf in formula (CC)) was obtained by the same procedure as in Example 26, except that a compound represented by formula (5-5) was used instead of a compound represented by formula (5-1). 2 is the PFPE chain represented by the above formula (4-2). 2 In the above formula, j, which indicates the average degree of polymerization, is 4.5. 3.24 g of compound (CC) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0322] [Example 31] A compound represented by the above formula (CD) was obtained by the method shown below. Compound (CD) (Rf in formula (CD)) was obtained by the same procedure as in Example 27, except that a compound represented by formula (5-5) was used instead of a compound represented by formula (5-1). 3 is the PFPE chain represented by the above formula (4-3). 3 In the above formula, k, which indicates the average degree of polymerization, is 3.0. 2.95 g of the compound (CD) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6): δ [ppm] = -84.0 to -83.0 (16F), -122.5 (4F), -126.0 (12F), -129.0 to -128.0 (4F)
[0323] [Example 32] A compound represented by the above formula (CE) was obtained by the method shown below. Compound (CE) (Rf in formula (CE)) was obtained by the same procedure as in Example 1, except that a compound represented by formula (5-24) was used instead of the compound represented by formula (5-1). 1 is the PFPE chain represented by the above formula (4-1). 1 In the formula (5-24), h, which indicates the average degree of polymerization, is 4.5, and i, which indicates the average degree of polymerization, is 4.5. 3.35 g of compound (CE) was obtained. The compound represented by formula (5-24) was synthesized by reacting one hydroxyl group of 2-methyl-1,3-propanediol with a compound obtained by brominating the hydroxyl group of solketal, and then reacting the other hydroxyl group with epibromohydrin. The compound (CE) obtained was 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.20-1.25 (6H), 1.25-1.35 (2H), 3.40-3.85 (34H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -55.5 to -51.5 (9F), -78.5 (2F), -80.5 (2F), -91.0 to -88.5 (18F)
[0324] [Example 33] The compound represented by the above formula (CF) was obtained by the following method. HOCH 2 CF 2 CF 2 O (CF 2 CF 2 CF 2 O) j CF 2 CF 2 CH 25 g of a compound (number average molecular weight 1000, molecular weight distribution 1.1) represented by formula (5-25) (where j, representing the average degree of polymerization, is 4.5), 4.83 g of the compound represented by formula (5-25), and 20 mL of N,N-dimethylformamide were charged and stirred at room temperature until homogeneous to form a mixture. 7.14 g of cesium carbonate was added to this mixture, and the mixture was stirred at 70°C for 16 hours to allow the reaction to proceed. The compound represented by formula (5-25) was synthesized by the following method. First, the hydroxyl group of 3-buten-1-ol was protected with dihydropyran, and then the alkenyl group was oxidized with m-chloroperbenzoic acid. The resulting compound was then reacted with solketal, and the secondary hydroxyl group of the resulting compound was protected with chloromethyl methyl ether. The resulting compound represented by the following formula (5-25A) was treated with an acid to selectively deprotect the THP group, and then the primary hydroxyl group was reacted with p-toluenesulfonyl chloride to obtain a compound represented by formula (5-25). The selective deprotection of the THP group was carried out by adding 0.52 g (2.07 mmol) of pyridinium p-toluenesulfonate as an acid catalyst to a mixture of 3.60 g (10.3 mmol) of the compound represented by formula (5-25A) and a mixed solvent of 16 g of 2-propanol and 16 g of acetone, and stirring the mixture in an air atmosphere at a reaction temperature of 55°C for 7 hours.
[0325]
[0326] The reaction solution obtained after the reaction of the fluorine-based compound with the compound represented by formula (5-25) was returned to room temperature, and 10 g of a 10% hydrogen chloride-methanol solution (hydrogen chloride-methanol reagent (5-10%), manufactured by Tokyo Chemical Industry Co., Ltd.) was added, followed by stirring at room temperature for 4 hours. Thereafter, the reaction solution was transferred little by little to a separatory funnel containing 25 mL of saturated aqueous sodium bicarbonate, and extracted twice with 50 mL of ethyl acetate. The organic layer was washed with 25 mL of brine, 25 mL of saturated aqueous sodium bicarbonate, and 25 mL of brine in that order, and dehydrated with anhydrous sodium sulfate. After filtering off the desiccant, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (CF) (Rf in formula (CF) 1 is the PFPE chain represented by the above formula (4-1). 1In the above formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5. 2.81 g of compound (CF) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0327] [Example 34] A compound represented by the above formula (CG) was obtained by the method shown below. Compound (CG) (Rf in formula (CG)) was obtained by the same procedure as in Example 33, except that a compound represented by formula (5-26) was used instead of a compound represented by formula (5-25). 2 is the PFPE chain represented by the above formula (4-2). 2 In the formula (5-26), j, which indicates the average degree of polymerization, is 4.5. 2.92 g of a compound represented by formula (5-26) was obtained. The compound represented by formula (5-26) was synthesized by the following method. First, the hydroxyl groups of 5-hexen-1-ol were protected using dihydropyran, and then the alkenyl groups were oxidized with m-chloroperbenzoic acid. Then, the obtained compound was reacted with solketal, and the secondary hydroxyl groups of the resulting compound were protected using chloromethyl methyl ether. The obtained compound was reacted with an acid to selectively deprotect the THP groups, and then the primary hydroxyl groups were reacted with paratoluenesulfonyl chloride to obtain a compound represented by formula (5-26). The obtained compound (CG) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (12H), 3.40-3.85 (26H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0328] [Example 35] The compound represented by the above formula (CH) was obtained by the following method. HOCH 2 CF 2 CF 2 O (CF 2 CF 2 CF 2 O) j CF 2 CF 2 CH 2 12 g of a compound (number average molecular weight: 1000, molecular weight distribution: 1.1) represented by OH (where j, representing the average degree of polymerization, is 4.5), 1.81 g of a compound represented by the above formula (5-27), and 20 mL of N,N-dimethylformamide were charged and stirred at room temperature until homogeneous to form a mixture. 5.51 g of cesium carbonate was added to this mixture, and the mixture was stirred at 50°C for 16 hours to allow the reaction to proceed. The compound represented by formula (5-27) was synthesized by protecting the 1,2-diol moiety of 1,2,6-hexanetriol with acetone, followed by reaction of the hydroxyl group at the 6-position with paratoluenesulfonyl chloride. The reaction product obtained after the reaction was cooled to 25°C, transferred to a separatory funnel containing 100 mL of water, and extracted three times with 100 mL of ethyl acetate. The organic layer was washed with water and dehydrated over anhydrous sodium sulfate. After filtering off the drying agent, the filtrate was concentrated and the residue was purified by silica gel column chromatography to obtain 5.96 g of a compound represented by the following formula (9) as intermediate compound 1. (Rf in formula (9) 2 is the PFPE chain represented by the above formula (4-2). 2In this formula, j, which indicates the average degree of polymerization, is 4.5.) Next, under a nitrogen gas atmosphere, 5.96 g of the compound represented by formula (9), which is the intermediate compound 1 obtained above, 2.76 g of the compound represented by formula (5-26), and 20 mL of N,N-dimethylformamide were charged into a 100 mL recovery flask and stirred at room temperature until a homogeneous mixture was obtained. 3.65 g of cesium carbonate was added to this mixture, and the mixture was allowed to react with stirring at 50°C for 16 hours. After the reaction, the resulting reaction solution was returned to room temperature, and 50 g of a 10% hydrogen chloride-methanol solution (hydrogen chloride-methanol reagent (5-10%), manufactured by Tokyo Chemical Industry Co., Ltd.) was added and stirred at room temperature for 4 hours. The reaction solution was then transferred little by little to a separatory funnel containing 100 mL of saturated aqueous sodium bicarbonate and extracted twice with 200 mL of ethyl acetate. The organic layer was washed sequentially with 100 mL of brine, 100 mL of saturated aqueous sodium bicarbonate, and 100 mL of brine, and then dehydrated using anhydrous sodium sulfate. After filtering off the drying agent, the filtrate was concentrated, and the residue was purified by silica gel column chromatography to obtain compound (CH) (Rf 2 is the PFPE chain represented by the above formula (4-2). 2 In the above formula, j, which indicates the average degree of polymerization, is 4.5. 2.41 g of the compound (CH) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (12H), 3.40-3.85 (20H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0329] [Example 36] A compound represented by the above formula (CI) was obtained by the method shown below. Compound (CI) (Rf in formula (CI)) was obtained by the same procedure as in Example 26, except that a compound represented by formula (5-8) was used instead of a compound represented by formula (5-1). 2 is the PFPE chain represented by the above formula (4-2). 2In the above formula, j, which indicates the average degree of polymerization, is 4.5. 3.13 g of the compound (CI) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (8H), 3.40-3.85 (18H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0330] [Example 37] A compound represented by the above formula (CJ) was obtained by the method shown below. Compound (CJ) (Rf in formula (CJ)) was obtained by the same procedure as in Example 26, except that a compound represented by formula (5-10) was used instead of a compound represented by formula (5-1). 2 is the PFPE chain represented by the above formula (4-2). 2 In this example, j, which indicates the average degree of polymerization, is 4.5. 3.52 g of compound (CJ) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 1.65-1.85 (4H), 3.40-3.85 (34H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0331] [Example 38] A compound represented by the above formula (CK) was obtained by the method shown below. Compound (CK) (Rf in formula (CK)) was obtained by the same procedure as in Example 26, except that a compound represented by formula (5-15) was used instead of a compound represented by formula (5-1). 2 is the PFPE chain represented by the above formula (4-2). 2In the above formula, j, which indicates the average degree of polymerization, is 4.5. 3.61 g of the compound (CK) was obtained. 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6 ): δ [ppm] = 3.40-3.85 (26H), 3.85-4.10 (12H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -128.5 (17F)
[0332] The compounds (AA) to (AS), (BA) to (BH), and (CA) to (CK) of Examples 1 to 38 thus obtained were each applied to the formula (1) to obtain R 1 , R 2 , R 3 The structures of the compounds are shown in Tables 1 and 2.
[0333]
[0334]
[0335] Comparative Example 1 A compound represented by the following formula (ZA) was synthesized by the method described in Patent Document 1.
[0336] (Rf in formula (ZA) 2 is the PFPE chain represented by the above formula (4-2). 2 In this case, j, which indicates the average degree of polymerization, is 4.5.
[0337] Comparative Example 2 A compound represented by the following formula (ZB) was synthesized by the method described in Patent Document 2.
[0338] (Rf in formula (ZB) 2 is the PFPE chain represented by the above formula (4-2). 2 In this case, j, which indicates the average degree of polymerization, is 4.5.
[0339] Comparative Example 3 A compound represented by the following formula (ZC) was synthesized by the method described in Patent Document 3.
[0340] (Rf in formula (ZC) 1 is the PFPE chain represented by the above formula (4-1). 1 In the formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0341] Comparative Example 4 A compound represented by the following formula (ZD) was synthesized by the following method.
[0342] (Rf in formula (ZD) 2 is the PFPE chain represented by the above formula (4-2). 2 In this case, j, which indicates the average degree of polymerization, is 4.5.
[0343] Instead of the compound represented by formula (5-1), a compound represented by formula (5-23) was used. 2 CF 2 O (CF 2 CF 2 O) h (CF 2 O) i CF 2 CH 2 Instead of the compound represented by OH, 2 CF 2 CF 2 O (CF 2 CF 2 CF 2 O) j CF 2 CF 2 CH 2 The same operation as in Example 1 was performed except that a compound (number average molecular weight: 1,000, molecular weight distribution: 1.1) represented by the formula OH (where j, representing the average degree of polymerization, is 4.5) was used, thereby obtaining 2.81 g of compound (ZD).
[0344] The obtained compound (ZD) 1 H-NMR and 19 F-NMR measurement was carried out, and the structure was identified from the following results. 1 H-NMR (acetone-D 6): δ [ppm] = 3.40-3.85 (14H), 3.85-4.10 (4H) 19 F-NMR (acetone-D 6 ): δ [ppm] = -84.0 to -83.0 (18F), -86.4 (4F), -124.3 (4F), -130.0 to -129.0 (9F)
[0345] Comparative Example 5 A compound represented by the following formula (ZE) was synthesized by the method described in Patent Document 4.
[0346] (Rf in formula (ZE) 1 is the PFPE chain represented by the above formula (4-1). 1 In the formula, h representing the average degree of polymerization is 4.5, and i representing the average degree of polymerization is 4.5.
[0347] The number average molecular weights (Mn) of the compounds thus obtained in Examples 1 to 38 and Comparative Examples 1 to 5 were measured by the above-mentioned method. The results are shown in Tables 3 and 4.
[0348] Next, solutions for forming lubricating layers were prepared by the method described below using the compounds obtained in Examples 1 to 38 and Comparative Examples 1 to 5. Then, using the obtained solutions for forming lubricating layers, lubricating layers for magnetic recording media were formed by the method described below, thereby obtaining the magnetic recording media of Examples 1 to 38 and Comparative Examples 1 to 5.
[0349] "Lubricant Layer-Forming Solution" The compounds obtained in Examples 1 to 38 and Comparative Examples 1 to 5 were each dissolved in a fluorine-based solvent, Vertrel (registered trademark) XF (trade name, manufactured by DuPont-Mitsui Fluorochemicals Co., Ltd.), and diluted with Vertrel XF so that the film thickness when applied to the protective layer would be 9.0 Å to 9.5 Å, to prepare a lubricant layer-forming solution.
[0350] "Magnetic Recording Medium" A magnetic recording medium was prepared by sequentially depositing an adhesive layer, a soft magnetic layer, a first underlayer, a second underlayer, a magnetic layer, and a protective layer on a substrate with a diameter of 65 mm. The protective layer was made of carbon. The lubricant layer-forming solutions of Examples 1 to 38 and Comparative Examples 1 to 5 were applied by dipping onto the protective layer of the magnetic recording medium on which each layer up to the protective layer had been formed. The dipping was performed under the following conditions: an immersion speed of 10 mm / sec, an immersion time of 30 seconds, and a pull-up speed of 1.2 mm / sec.
[0351] The magnetic recording medium coated with the lubricating layer-forming solution was then placed in a thermostatic chamber, and a heat treatment was performed at 120°C for 10 minutes to remove the solvent in the lubricating layer-forming solution and improve the adhesion between the protective layer and the lubricating layer, thereby forming a lubricating layer on the protective layer and obtaining a magnetic recording medium.
[0352] [Film Thickness Measurement] The film thickness of the lubricating layer of each of the magnetic recording media thus obtained in Examples 1 to 38 and Comparative Examples 1 to 5 was measured using a Fourier transform infrared spectrophotometer (FT-IR, product name: Nicolet iS50, manufactured by Thermo Fisher Scientific). The results are shown in Tables 3 and 4.
[0353] Next, the following corrosion resistance test and spin-off characteristic test were carried out on the magnetic recording media of Examples 1 to 38 and Comparative Examples 1 to 5. The results are shown in Tables 3 and 4.
[0354] [Corrosion Resistance Test] The magnetic recording medium was exposed to conditions of a temperature of 85° C. and a relative humidity of 90% for 48 hours. After that, the number of corrosion spots with a diameter of 5 μm or more that appeared on the surface of the magnetic recording medium was counted using an optical surface analyzer (Candela 7140 manufactured by KLA Tencor Corporation), and evaluated based on the following evaluation criteria.
[0355] "Corrosion resistance evaluation criteria" A+: Number of corrosion spots less than 100 A: Number of corrosion spots 100 or more but less than 300 B: Number of corrosion spots 300 or more but less than 500 C: Number of corrosion spots 500 or more but less than 1000 D: Number of corrosion spots 1000 or more
[0356] [Spin-off property test] A magnetic recording medium was mounted on a spin stand and rotated at a rotation speed of 10,000 rpm in an environment of 80°C for 72 hours. Before and after this operation, the film thickness of the lubricating layer at a position 20 mm radius from the center of the magnetic recording medium was measured using FT-IR, and the film thickness reduction rate of the lubricating layer before and after the test was calculated. The spin-off property was evaluated using the calculated film thickness reduction rate according to the evaluation criteria shown below.
[0357] "Evaluation criteria for spin-off characteristics" A+: Film thickness reduction rate less than 2% A: Film thickness reduction rate 2% or more but less than 3% B: Film thickness reduction rate 3% or more but less than 5% C: Film thickness reduction rate 5% or more but less than 10% D: Film thickness reduction rate 10% or more
[0358] [Overall Evaluation] From the results of the corrosion resistance test and the spin-off property test, an overall evaluation was made based on the following criteria.
[0359] "Overall evaluation criteria" A: Both the evaluation of the corrosion resistance test and the evaluation of the spin-off characteristics test are A+ or A. B: One of the evaluation of the corrosion resistance test and the evaluation of the spin-off characteristics test is B, and the other is A+, A, or B. C: One of the evaluation of the corrosion resistance test and the evaluation of the spin-off characteristics test is C, and the other is A+, A, B, or C. D: At least one of the evaluation of the corrosion resistance test and the evaluation of the spin-off characteristics test is D.
[0360]
[0361]
[0362] As shown in Tables 3 and 4, R 1 and R 3 The magnetic recording media of Examples 1 to 38, which used fluorine-containing ether compounds (AA) to (AS), (BA) to (BH), and (CA) to (CK) satisfying formula (1), at least one of which is an end group represented by formula (2), were all rated A+, A, or B in the corrosion resistance test and spin-off characteristics test, and the overall rating was A or B. This confirmed that the lubricating layers of the magnetic recording media of Examples 1 to 38 had good corrosion resistance and were able to suppress spin-off.
[0363] R1 and R 3 In Examples 8, 9, 15 to 18, 35, 36, and 38, which used compounds (AH), (AI), (AO) to (AR), (CH), (CI), and (CK), each of which has a terminal group represented by formula (2-3), (2-5), (2-6), or (2-7), the corrosion resistance test was evaluated as A+, which showed good results.
[0364] R 1 and R 3 is a terminal group represented by formula (2-1), and the sum of a and b is 4 or less. 1 and R 3 is a terminal group represented by formula (2-2), and c is 3 or less. 1 and R 3 is a terminal group represented by formula (2-4), and e is 2 or less, 1 and R 3 Compound (AS) in which one of R is a terminal group represented by formula (2-1) and the sum of a and b is 4 or less, and the other is a terminal group represented by formula (2-2) and c is 3 or less, 1 and R 2 In Examples 1, 2, 4 to 6, 10 to 13, 19, 26 to 34, and 37, which used compounds (CF) and (CG) in which is a terminal group represented by formula (2-7) and g2 is 3 or less, the evaluation of the spin-off characteristics test was A+, which was good.
[0365] In contrast, as shown in Tables 3 and 4, in Comparative Examples 1 to 5 in which compounds (ZA) to (ZE) were used, the corrosion resistance test and the spin-off property test were all evaluated as B, C, or D, and the overall evaluation was either C or D.
[0366] In the compound (ZA) used in Comparative Example 1, the terminal group does not contain a 1,2-diol structure and a carbon atom that is not bonded to either a polar group or an ether oxygen atom.
[0367] The terminal group of compound (ZA) does not contain a 1,2-diol structure, and all hydroxyl groups contribute greatly to increasing the polarity of the entire molecule. Furthermore, since the terminal group of compound (ZA) does not contain a carbon atom that is not bonded to either a polar group or an ether oxygen atom, the molecule does not have sufficient hydrophobicity. For these reasons, it is thought that in Comparative Example 1, the fluorine-containing ether compound is more likely to absorb water, which causes corrosion, and the result of the corrosion resistance test was D.
[0368] In compound (ZA), the distance between hydroxyl groups is greater than the distance between hydroxyl groups in a 1,2-diol structure, so all of the hydroxyl groups tend to interact with the protective layer. As a result, the interaction between hydroxyl groups in the molecules is reduced, making it easier for the lubricant to scatter as the magnetic recording medium rotates, which is thought to be why the spin-off characteristics test was rated C.
[0369] The compound (ZB) used in Comparative Example 2 and the compound (ZC) used in Comparative Example 3 each contain a carbon atom whose terminal group is not bonded to either a polar group or an ether oxygen atom, but do not contain a 1,2-diol structure.
[0370] Compound (ZB) and compound (ZC) contain carbon atoms in their terminal groups that are not bonded to either polar groups or ether oxygen atoms, resulting in increased hydrophobicity of the molecules. Furthermore, the total number of hydroxyl groups possessed by compounds (ZB) and (ZC) is 4. Therefore, the total number of hydroxyl groups possessed by compounds (ZB) and (ZC) is smaller than the total number of hydroxyl groups possessed by compound (ZA) used in Comparative Example 1, which is 6. Therefore, in compounds (ZB) and (ZC), the fluorine-containing ether compounds are less likely to absorb water, which is the cause of corrosion, and the results of the corrosion resistance tests of Comparative Examples 2 and 3 were better than those of Comparative Example 1.
[0371] In compounds (ZB) and (ZC), the distance between hydroxyl groups is greater than the distance between hydroxyl groups in a 1,2-diol structure, so all hydroxyl groups are likely to interact with the protective layer. Furthermore, the total number of hydroxyl groups in compounds (ZB) and (ZC) is four, which is relatively small, so there are almost no hydroxyl groups that can contribute to intermolecular interactions. As a result, the intermolecular interactions of the fluorine-containing ether compound are small, making the lubricant more likely to scatter as the magnetic recording medium rotates, and it is believed that this is why Comparative Examples 2 and 3 received a D rating in the spin-off characteristics test.
[0372] In the compound (ZD) used in Comparative Example 4 and the compound (ZE) used in Comparative Example 5, the terminal group contains a 1,2-diol structure, but does not contain a carbon atom that is not bonded to either a polar group or an ether oxygen atom.
[0373] The compounds (ZD) and (ZE) have no carbon atoms in their end groups that are not bonded to either polar groups or ether oxygen atoms, so the hydrophobicity of the molecules is reduced.As a result, the fluorine-containing ether compounds are more likely to absorb water, which is the cause of corrosion, and it is considered that the result of the corrosion resistance test in Comparative Example 4 is C, and the result of the corrosion resistance test in Comparative Example 5 is D.The reason why the results of the corrosion resistance test in Comparative Example 4 are C and in Comparative Example 5 are D is considered to be that the total number of hydroxyl groups in the compound (ZD) is 4, and the total number of hydroxyl groups in the compound (ZE) is 8, so that Comparative Example 5, which has a larger total number of hydroxyl groups, is more likely to absorb water.
[0374] Because compounds (ZD) and (ZE) do not contain a carbon atom at their terminal that is not bonded to either a polar group or an ether oxygen atom, it is difficult to impart a suitable degree of rigidity to the molecule. This makes it easier for the two hydroxyl groups that make up the 1,2-diol structure to interact within the molecule. As a result, it is thought that the hydroxyl groups in the fluorine-containing ether compound are less likely to interact with each other intermolecularly, making the lubricant more likely to scatter as the magnetic recording medium rotates, which is why the spin-off characteristics tests for Comparative Examples 4 and 5 received a C rating.
[0375] By using a lubricant for magnetic recording media containing the fluorine-containing ether compound of the present invention, it is possible to form a lubricating layer that has good corrosion resistance and is capable of suppressing spin-off even if it is thin.
[0376] REFERENCE SIGNS LIST 10 magnetic recording medium 11 substrate 12 adhesive layer 13 soft magnetic layer 14 first underlayer 15 second underlayer 16 magnetic layer 17 protective layer 18 lubricating layer
Claims
1. A fluorine-containing ether compound represented by the following formula (1): 1 -CH 2 -R 2 -CH 2 -R 3 (1) (In formula (1), R 2 is a perfluoropolyether chain. 1 and R 3 is a terminal group having 1 to 4 polar groups and 1 to 50 carbon atoms. 1 and R 3 may be the same or different. 1 and R 3 At least one of the above is a terminal group represented by the following formula (2): —O—X—CH(OH)—CH 2 OH (2) (In formula (2), X is a divalent organic group having 2 to 30 carbon atoms which may contain at least one of 1 to 2 polar groups and 1 to 3 ether oxygen atoms. X contains at least one carbon atom which is not bonded to any of the polar groups and the ether oxygen atoms.) 2. The fluorine-containing ether compound according to claim 1, wherein the terminal group represented by the formula (2) is any one of the following formulae (2-1) to (2-7): (In formula (2-1), a represents an integer of 1 to 8. b represents an integer of 1 to 7.) (In formula (2-2), c represents an integer of 1 to 7.) (In formula (2-3), d represents an integer of 1 to 6.) (In formula (2-4), e represents an integer of 1 to 6. e R a and R b each independently represents a hydrogen atom or a methyl group.) (In formula (2-5), f represents an integer of 1 to 6.) (In formula (2-6), g represents an integer of 1 to 6.) (In formula (2-7), g2 represents an integer of 1 to 6.) 3. R in the above formula (1) 1 and R 3 and each independently represent a terminal group represented by formula (2).
4. R in the above formula (1) 1 and R 3The fluorine-containing ether compound according to claim 1 or 2, wherein 5. R in the above formula (1) 1 and R 3 one of the above is an end group represented by formula (2), and the other is an end group represented by formula (3) below not corresponding to formula (2): (In formula (3), l represents an integer of 1 to 3. l's m each independently represents an integer of 1 to 6. l's n each independently represents an integer of 1 to 6. In one repeating unit, at least one of m and n is 1. B represents an alkyl group which may have only one polar group, an organic group containing a carbon-carbon unsaturated bond, or a hydrogen atom.) 6. R in the above formula (1) 1 and R 3 one of the above is an end group represented by formula (2), and the other is an end group represented by any one of the following formulas (3-1) to (3-3): (In formula (3-1), p represents an integer of 0 to 3. q represents an integer of 0 to 2. r represents an integer of 0 to 5. The sum of p and r is 1 to 5. D represents a polar group, a vinyl group, an ethynyl group, or an aryl group which may have a substituent.) (In formula (3-2), s represents an integer of 0 to 2. t represents an integer of 1 to 5.) (In formula (3-3), u represents an integer of 1 to 3. Each of the five E's independently represents a polar group, an alkoxy group having 1 to 8 carbon atoms, a halogeno group, or a hydrogen atom. However, when the five E's include a polar group, the number of polar groups among the five E's is 1.) 7. R in the above formula (1) 1 and R 3 The fluorine-containing ether compound according to claim 1 or 2, wherein the total number of polar groups is 4 to 6.
8. R in the above formula (1) 2 The fluorine-containing ether compound according to claim 1 or 2, wherein -(CF 2 ) w1 -O-(CF 2 O) w2 -(CF2 CF 2 O) w3 -(CF 2 CF 2 CF 2 O) w4 -(CF 2 CF 2 CF 2 CF 2 O) w5 -(CF 2 ) w6 In formula (4), w2, w3, w4, and w5 each independently represent an average degree of polymerization, and each independently represent a value of 0 to 20. However, w2, w3, w4, and w5 cannot all be 0 at the same time. w1 and w6 are each independently a value of 0 to 20. 2 is an average value representing the number of repeating units in formula (4), each of which independently represents 1 to 3. 2 O), (CF 2 CF 2 O), (CF 2 CF 2 CF 2 O), (CF 2 CF 2 CF 2 CF 2 There is no particular restriction on the order of arrangement of O).
9. R in the above formula (1) 2 is any one selected from perfluoropolyether chains represented by the following formulas (4-1) to (4-4): 2 - (OCF 2 CF 2 ) h - (OCF 2 ) i - OCF 2 - (4-1) (In formula (4-1), h and i represent the average degree of polymerization, h represents 1 to 20, and i represents 0 to 20.) -CF 2 CF 2 - (OCF 2 CF 2 CF 2 ) j - OCF 2 CF 2 - (4-2) (In formula (4-2), j represents an average degree of polymerization and is 1 to 15.) -CF2 CF 2 CF 2 - (OCF 2 CF 2 CF 2 CF 2 ) k - OCF 2 CF 2 CF 2 (In formula (4-3), k represents the average degree of polymerization and is 1 to 10.) -(CF 2 ) w7 -O-(CF 2 CF 2 CF 2 O) w8 -(CF 2 CF 2 O) w9 -(CF 2 ) w10 In formula (4-4), w8 and w9 represent the average degree of polymerization, each independently representing 1 to 20. w7 and w10 represent CF 2 is an average value representing the number of, each independently representing 1 to 2.) 10. The fluorine-containing ether compound according to claim 1 or 2, which has a number average molecular weight in the range of 500 to 10,000.
11. A lubricant for magnetic recording media, comprising the fluorine-containing ether compound according to claim 1 or 2.
12. A magnetic recording medium comprising at least a magnetic layer, a protective layer, and a lubricating layer provided in that order on a substrate, the lubricating layer comprising the fluorine-containing ether compound according to claim 1 or 2.
13. The magnetic recording medium according to claim 12, wherein the average thickness of the lubricating layer is 0.5 nm to 2.0 nm.
Citation Information
Patent Citations
Magnetic recording medium
JP1994309654A
Fluoropolyether compound, lubricant, magnetic disk, and method for producing fluoropolyether compound
JP2024052300A
Polyfluoro lubricant compositions
US20200002640A1
Perfluoropolyether derivatives
WO2004035656A1
Fluoropolyether compound
WO2005068534A1