Negative electrode for lithium secondary battery, and lithium secondary battery
The integration of an intermetallic copper-magnesium compound at the interface between the copper current collector and the magnesium-containing lithium alloy layer in lithium secondary batteries addresses adhesion issues, enhancing cycle characteristics and capacity retention.
Patent Information
- Application Number
- PCT/JP2024/015310
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-17
- Publication Date
- 2024-10-31
AI Technical Summary
Lithium secondary batteries with lithium alloy negative electrodes face deterioration in cycle characteristics due to low adhesion between the lithium alloy layer and the current collector, leading to poor performance and capacity retention.
A negative electrode with a copper current collector and a lithium alloy layer containing magnesium, where an intermetallic compound of copper and magnesium is formed at the interface, enhancing adhesion and cycle characteristics.
The introduction of the intermetallic compound improves the adhesion between the lithium alloy layer and the current collector, resulting in better cycle characteristics and capacity retention in lithium secondary batteries.
Smart Images

Figure JP2024015310_31102024_PF_FP_ABST
Abstract
Description
Negative electrode for lithium secondary battery and lithium secondary battery
[0001] The present disclosure relates to a negative electrode for a lithium secondary battery and a lithium secondary battery.
[0002] Lithium secondary batteries (also called lithium metal secondary batteries) that use lithium metal as the negative electrode active material have a high theoretical capacity density. In lithium secondary batteries, lithium metal is deposited on the negative electrode current collector during charging, and the deposited lithium metal dissolves in the non-aqueous electrolyte during discharging. A negative electrode containing a lithium alloy may also be used in lithium secondary batteries. Various proposals have been made for the negative electrode of non-aqueous electrolyte secondary batteries.
[0003] Claim 1 of Patent Document 1 (JP 2018-63872 A) describes, "A lithium-ion secondary battery comprising: a negative electrode current collector foil; and a negative electrode active material layer formed on the negative electrode current collector foil, wherein the negative electrode active material layer contains a graphite-based negative electrode active material; the negative electrode current collector foil is copper foil having a copper alloy coating formed on its surface; and the volume resistivity of the copper alloy coating is higher than that of copper and the thermal conductivity of the copper alloy coating is lower than that of copper."
[0004] Claim 1 of Patent Document 2 (JP 2014-120399 A) states that "an active material-containing layer and a substrate not carrying the active material-containing layer and having a surface roughness of Ra 1 and the active material-containing layer, and the surface roughness is 2 and a second region on the surface, the first region having a surface roughness Ra 1 The surface roughness Ra of the second region 2 and a current collector smaller than 1000 nm.
[0005] JP 2018-63872 A JP 2014-120399 A
[0006] It has been proposed to use a negative electrode including a lithium alloy layer as the negative electrode of a lithium secondary battery. However, the present inventors have found that the use of a negative electrode including a lithium alloy layer may result in a decrease in cycle characteristics. One object of the present disclosure is to provide a negative electrode including a lithium alloy layer containing magnesium, which can be used to manufacture a lithium secondary battery with good cycle characteristics.
[0007] One aspect of the present disclosure relates to a negative electrode for a lithium secondary battery, the negative electrode for the lithium secondary battery including a current collector containing copper and a lithium alloy layer disposed on the current collector, the lithium alloy layer containing magnesium, and an intermetallic compound of copper and magnesium present at the interface between the current collector and the lithium alloy layer.
[0008] Another aspect of the present disclosure relates to a lithium secondary battery including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein the negative electrode is a lithium secondary battery negative electrode according to the present disclosure, and lithium metal precipitates in the negative electrode during charging and dissolves during discharging.
[0009] According to the present disclosure, a negative electrode including a magnesium-containing lithium alloy layer can be obtained, which can be used to manufacture a lithium secondary battery having good cycle characteristics. The novel features of the present invention are set forth in the appended claims, but the present invention, both in terms of structure and content, together with other objects and features of the present invention, will be better understood from the following detailed description taken in conjunction with the drawings.
[0010] FIG. 1 is a longitudinal cross-sectional view schematically showing a lithium secondary battery according to an embodiment of the present disclosure. FIG. 2 is a cross-sectional view schematically showing a negative electrode according to an embodiment of the present disclosure. FIG. 3A is a top view schematically showing an example of a separator on which a spacer is formed. FIG. 3B is a view schematically showing a cross section taken along line IIIA-IIIA in FIG. 3A. FIG. 4 shows an example of an X-ray diffraction pattern measured in an example. FIG. 5 shows evaluation results in an example.
[0011] The following describes embodiments of the present disclosure using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials may be exemplified, but other numerical values and other materials may be applied as long as the effects of the present disclosure are obtained. In this specification, the term "numerical value A to numerical value B" includes numerical value A and numerical value B and can be read as "numerical value A or greater and numerical value B or less." In the following description, when lower and upper limits of numerical values related to specific physical properties or conditions are exemplified, any of the exemplified lower limits and any of the exemplified upper limits can be arbitrarily combined, as long as the lower limit is not greater than the upper limit. In the following description, when examples of components or methods are listed, only one of the listed examples may be used, or multiple of the listed examples may be used in combination, unless otherwise specified.
[0012] (Negative electrode for lithium secondary battery) The negative electrode according to this embodiment may be referred to as "negative electrode (N)" hereinafter. The negative electrode (N) is a negative electrode for a lithium secondary battery. The negative electrode (N) includes a current collector containing copper and a lithium alloy layer disposed on the current collector. The lithium alloy layer contains magnesium. An intermetallic compound of copper and magnesium is present at the interface between the current collector and the lithium alloy layer.
[0013] Hereinafter, the lithium alloy layer containing magnesium may be referred to as an “Mg-containing Li alloy layer.” The Mg-containing Li alloy layer may contain elements other than lithium (Li) and magnesium (Mg).
[0014] The use of a negative electrode containing an Mg-containing Li alloy layer has the advantage of suppressing the deterioration of cycle characteristics due to the formation of an SEI film, as described below. However, the present inventors have found that the use of a negative electrode containing an Mg-containing Li alloy layer can sometimes result in a deterioration of cycle characteristics. As a result of their investigation, they have found that the deterioration of cycle characteristics may be due to poor adhesion between the Mg-containing Li alloy layer and the current collector. Because the Mg-containing Li alloy layer is hard, repeated deposition and dissolution of metal on the negative electrode is thought to reduce the adhesion between the Mg-containing Li alloy layer and the current collector. After further investigation, the present inventors have found that good cycle characteristics can be achieved by disposing a specific intermetallic compound between the Mg-containing Li alloy layer and the current collector. The present disclosure is based on this new finding.
[0015] The Mg-containing Li alloy layer is formed on at least one of the two surfaces of the negative electrode (N) that faces the positive electrode. When both surfaces of the negative electrode (N) face the positive electrode, an example of the negative electrode (N) has a laminated structure of Mg-containing Li alloy layer / intermetallic compound layer / current collector / intermetallic compound layer / Mg-containing Li alloy layer. When only one surface of the negative electrode (N) faces the positive electrode, an example of the negative electrode (N) has a laminated structure of current collector / intermetallic compound layer / Mg-containing Li alloy layer.
[0016] As an intermetallic compound, Cu 2 In this case, in the X-ray diffraction pattern obtained by X-ray diffraction analysis, the peak intensity Ic of the intermetallic compound (Cu 2The ratio Icm / Ic of the peak intensity Icm of the (111) plane of Mg may be in the range of 0.005 to 0.095. The ratio Icm / Ic may be 0.0007 or more, 0.005 or more, 0.0086 or more, 0.0191 or more, 0.0305 or more, or 0.0457 or more, or may be 0.1037 or less, 0.0958 or less, 0.095 or less, 0.075 or less, 0.0457 or less, 0.0305 or less, or 0.0191 or less. The ratio Icm / Ic may be in the range of 0.0007 to 0.1037, 0.005 to 0.1037, 0.0086 to 0.1037, 0.0191 to 0.1037, 0.0305 to 0.1037, or 0.0457 to 0.1037. Within these ranges, the upper limit may be 0.0958, 0.095, 0.075, 0.0457, 0.0305, or 0.0191, as long as the lower limit is not greater than or equal to the upper limit.
[0017] The thickness of the Mg-containing Li alloy layer may be 5 μm or more, or 10 μm or more, or may be 50 μm or less, or 100 μm or less. The intermetallic compound between the Mg-containing Li alloy layer and the current collector may be formed in the form of particles or layers.
[0018] The Mg content in the Mg-containing Li alloy layer may be 0.5 mass% or more, 1.0 mass% or more, 3.0 mass% or more, 5.0 mass% or more, or 10 mass% or less, 15 mass% or less, 20 mass% or less, or 30 mass% or less.
[0019] The Mg-containing Li alloy layer may be an alloy layer made of lithium (Li) and magnesium. Alternatively, the Mg-containing Li alloy layer may contain other metal elements in addition to lithium and magnesium. Examples of other metal elements include aluminum, indium, copper, zinc, potassium, calcium, sodium, silver, and gold. The content of the other metal elements may be 5% by mass or less (e.g., 1% by mass or less).
[0020] The current collector (negative electrode current collector) contains copper. At least the surface of the current collector is made of a metal containing copper. The copper-containing metal may be copper or a copper alloy. The content of elements other than copper contained in the copper alloy is small, for example, 30 mass % or less (e.g., 10 mass % or less). Examples of elements other than copper include zinc, tin, aluminum, beryllium, nickel, iron, manganese, etc.
[0021] The current collector may be a copper foil or a copper alloy foil. The copper alloy may be any of the above-mentioned copper alloys. The thickness of the foil may be 5 μm or more, or 7 μm or more, and may be 15 μm or less, or 30 μm or less.
[0022] The current collector may include a substrate and a metal layer disposed on the substrate. The metal layer contains copper. The substrate may be formed of stainless steel or a resin. This configuration particularly prevents breakage of the current collector. The copper-containing metal layer may be formed of copper or a copper alloy. The copper alloy may be the copper alloy described above. The resin of the substrate is not particularly limited, but a resin that is less susceptible to deterioration within the battery is preferably used. Examples of resins include polyethylene, polypropylene, polyethylene terephthalate, polyimide, polyamide, polyurethane, etc.
[0023] The thickness of the substrate may be 5 μm or more, or 10 μm or more, and may be 20 μm or less, or 50 μm or less. The thickness of the metal layer may be 0.1 μm or more, or 0.5 μm or more, and may be 2 μm or less, or 5 μm or less.
[0024] The negative electrode (N) may optionally contain a second negative electrode active material other than lithium (the first negative electrode active material). Examples of the second negative electrode active material include Si-containing materials (silicon, silicon oxide, etc.), Sn-containing materials (tin, tin oxide, etc.), and carbonaceous materials (graphite, soft carbon, hard carbon, amorphous carbon, etc.). The second negative electrode active material is capable of reversibly absorbing and desorbing lithium. The negative electrode (N) may contain only one or more of these second negative electrode active materials. The negative electrode (N) may include a layer containing the second negative electrode active material. The layer containing the second negative electrode active material may optionally contain at least one selected from the group consisting of a binder, a conductive material, a thickener, and an additive. These components may be selected from the components described for the positive electrode. However, more than half of the capacity of the negative electrode (N) is due to the deposition and dissolution of lithium metal. An example negative electrode (N) does not include a second negative electrode active material.
[0025] (Manufacturing Method of Negative Electrode (N)) Manufacturing method (M), which is one example of a manufacturing method of the negative electrode (N), will be described below. However, the negative electrode (N) may be manufactured by a method other than the method described below. Since the matters described for the negative electrode (N) are applicable to the manufacturing method below, duplicated explanations will be omitted. Furthermore, the matters described in the manufacturing method below may also be applied to the negative electrode (N).
[0026] The manufacturing method (M) includes steps (i) and (ii). Step (i) is a step of disposing a Mg-containing Li alloy (e.g., a Li-Mg alloy foil) on a current collector. The Mg-containing Li alloy foil is a foil that will become the Mg-containing Li alloy layer. The current collector is the above-mentioned current collector.
[0027] In step (ii), a current collector and a Mg-containing Li alloy foil are pressed together to bond them together. Silicone oil or hydrocarbon oil is used as rolling oil when manufacturing the Mg-containing Li alloy foil. In this step, it is preferable that no oil residue remains on the surface of the Mg-containing Li alloy foil, in order to ensure that the intermetallic compound is present appropriately.
[0028] The first of the useful means for leaving no oil residue is a method for producing a Mg-containing Li alloy foil using a highly volatile oil (volatile oil). Examples of highly volatile oils include decane, dodecane, tridecane, tetradecane, pentadecane, hexadecane, and the like. The second of the useful means for leaving no oil residue is a method for removing the oil residue by vacuum drying the Mg-containing Li alloy foil before step (i). Vacuum drying can be performed, for example, by holding the Mg-containing Li alloy foil for a certain period of time under a vacuum atmosphere of 0.006 MPa (gauge pressure: -0.095 MPa) or less. The first and second methods may be used in combination.
[0029] The manufacturing method (M) may include step (a) and / or step (b) before step (i). Step (a) is a step of manufacturing a Mg-containing Li alloy foil by rolling using a highly volatile oil. Step (b) is a step of vacuum-drying the Mg-containing Li alloy foil. When both steps (a) and (b) are performed, step (b) is performed after step (a).
[0030] If the pressing pressure during compression bonding is high, deformation and wrinkles will occur in the resulting laminate (negative electrode (N)) when the Mg-containing Li alloy foil is pressed onto the current collector. Therefore, it is preferable to set the upper limit of the pressing pressure to a pressure at which deformation and wrinkles will not occur in the negative electrode (N). The pressing for compression bonding may be performed using a roll press with a linear pressure in the range of 9.8 N / cm to 490 N / cm.
[0031] After the current collector and the Mg-containing Li alloy foil are pressure-bonded, the resulting laminate (negative electrode (N)) can be held for a certain period of time in an inert atmosphere at 60°C or less (for example, in the range of 40°C to 60°C), thereby appropriately controlling the amount of intermetallic compounds. Specifically, the amount of intermetallic compounds tends to increase by extending the time for holding in an inert atmosphere at 60°C or less. Examples of inert atmospheres include an argon gas atmosphere and a vacuum atmosphere of 0.006 MPa (gauge pressure: -0.095 MPa) or less. The holding time may be in the range of 1 to 72 hours.
[0032] By appropriately controlling the removal of the oil residue, the pressure of the press, and the holding conditions after pressing, an intermetallic compound (e.g., Cu) having a predetermined ratio Icm / Ic is formed between the current collector and the Li-Mg alloy layer. 2 In this way, the negative electrode (N) can be produced.
[0033] (Lithium secondary battery) The lithium secondary battery according to the present disclosure may be referred to hereinafter as a "lithium secondary battery (B)" or a "secondary battery (B)." The secondary battery (B) includes a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte. The negative electrode is the negative electrode (N) according to the present disclosure. In the negative electrode (N), lithium metal precipitates during charging, and the lithium metal dissolves during discharging. The negative electrode (N) has been described above, so a redundant description will be omitted.
[0034] In general, in lithium secondary batteries, lithium metal precipitates on the negative electrode during charging, and the precipitated lithium metal dissolves in the non-aqueous electrolyte during discharge. In general, in lithium secondary batteries, a coating is formed on the negative electrode during charging due to decomposition and / or reaction of components contained in the non-aqueous electrolyte. This coating is called an SEI (Solid Electrolyte Interphase) coating. The SEI coating is also formed on the surface of the precipitated lithium metal. During charging, lithium metal precipitates on the negative electrode, and an SEI coating is also formed. Therefore, compared to lithium ion secondary batteries, the charging reaction of lithium secondary batteries is more likely to be uneven, which can lead to reduced capacity and poor cycle performance. Furthermore, if the charging reaction occurs locally due to the SEI coating, lithium metal precipitates in a dendrite-like form, which can easily cause the negative electrode to expand. When the negative electrode expands, the non-aqueous electrolyte contained in the positive electrode and separator is pushed out, reducing the lithium ion concentration and poor cycle performance. Furthermore, when lithium metal is precipitated in a dendrite-like form, the specific surface area of the lithium metal increases, further increasing side reactions between the lithium metal and the electrolyte, resulting in a significant decrease in cycle characteristics.
[0035] On the other hand, since the negative electrode (N) of the secondary battery (B) contains magnesium, which has a higher standard electrode potential than lithium, it is thought that the reductive decomposition reaction of the non-aqueous electrolyte is suppressed, and the growth of the SEI film is suppressed. Therefore, in the secondary battery (B), the negative electrode (N) contains a Mg-containing Li alloy layer, which can suppress the deterioration of cycle characteristics due to the formation of the SEI film.
[0036] Furthermore, the negative electrode (N) of the secondary battery (B) contains the above-mentioned intermetallic compound, which can particularly suppress the deterioration of cycle characteristics.
[0037] In the secondary battery (B), lithium in the positive electrode can be deposited as lithium metal on the negative electrode (N) during charging. The deposited lithium metal can be dissolved in the non-aqueous electrolyte during discharging. Charging and discharging are carried out in this manner. When charging and discharging are repeated, the Mg-containing Li alloy layer can be utilized for charging and discharging.
[0038] The secondary battery (B) may include a spacer (protrusion) formed on either the positive electrode or the separator. The use of the spacer can suppress volumetric changes in the electrode assembly, particularly suppressing deterioration in cycle characteristics. When a spacer is formed on the positive electrode, the spacer is formed on one of both surfaces of the positive electrode, facing the negative electrode (N) via the separator. When a spacer is formed on the separator, the spacer is usually formed on one surface of the separator.
[0039] The spacers have a convex shape. The spacers may be linear convex portions and / or dot-shaped convex portions. The material of the spacers is not particularly limited, and insulating resin and / or insulating inorganic material can be used. The insulating resin can be an insulating resin that is less likely to deteriorate in the secondary battery (B), and the insulating resin used in the separator can also be used. The spacers may also be formed from a mixture of insulating resin and insulating inorganic material. Examples of insulating resin materials include polyethylene, polypropylene, polyethylene terephthalate, polyimide, polyamide, polyurethane, etc. The insulating inorganic material can be an inorganic material that does not affect the characteristics of the secondary battery (B). Examples of insulating inorganic materials include Al. 2 O 3, MgO, ZnO, ZrO 2 , SiO 2 , TiO 2 These include:
[0040] The width of the spacer may be 100 μm or more, or 500 μm or more, and may be 1000 μm or less, or 2000 μm or less. The height of the spacer may be 10 μm or more, or 20 μm or more, and may be 50 μm or less, or 100 μm or less. The spacer may include an insulating inorganic material and have a height of 10 μm or more.
[0041] The spacers can be formed in a predetermined pattern. For example, the spacers may have a mesh-like shape. Examples of mesh-like shapes include shapes that combine polygons, such as a honeycomb shape. The spacers may include a plurality of linear protrusions extending in a stripe pattern. The spacers may also include a plurality of dot-like protrusions arranged at regular intervals.
[0042] The spacer can be formed by applying a spacer material to a predetermined member (a positive electrode or a separator). The method for applying the spacer material is not particularly limited, and the spacer material may be applied by screen printing or by a method using a dispenser.
[0043] The method for producing the secondary battery (B) is not particularly limited except for the use of the negative electrode (N), and the secondary battery (B) may be produced using a known method. In one example of the production method, first, an electrode group is produced using a positive electrode, a negative electrode (N), and a separator. Next, the electrode group and a non-aqueous electrolyte are sealed in an outer casing. In this manner, the secondary battery (B) can be produced.
[0044] Examples of components of the secondary battery (B) are described below. Components other than those characteristic of the secondary battery (B) of the present disclosure are not particularly limited, and components used in known lithium secondary batteries may be applied.
[0045] (Negative electrode) The above-described negative electrode (N) is used as the negative electrode. The shape of the negative electrode is selected depending on the form of the secondary battery (B). For example, when the secondary battery (B) is a cylindrical battery, a strip-shaped negative electrode can be used.
[0046] (Positive Electrode) The positive electrode includes, for example, a positive electrode current collector and a positive electrode composite layer formed on the surface of the positive electrode current collector. The positive electrode current collector may be in a sheet form (for example, a foil or a film) or may be porous. The positive electrode composite layer may be formed on both main surfaces of the positive electrode current collector, or may be formed on only one main surface. The positive electrode composite layer may be formed in a state where it is filled into a mesh-shaped positive electrode current collector.
[0047] Examples of materials for the positive electrode current collector include metal materials such as Al, Al alloys, Ti, Ti alloys, and Fe alloys. The Fe alloy may be stainless steel.
[0048] The positive electrode mixture layer includes a positive electrode active material. In addition to the positive electrode active material, the positive electrode mixture layer may include at least one selected from the group consisting of a binder, a conductive material, a thickener, and an additive. If necessary, a conductive carbonaceous material may be disposed between the positive electrode current collector and the positive electrode mixture layer.
[0049] The positive electrode active material is a material that electrochemically absorbs and releases lithium ions. Examples of such materials include at least one selected from the group consisting of lithium-containing transition metal oxides, transition metal fluorides, polyanions, fluorinated polyanions, and transition metal sulfides. From the viewpoints of high average discharge voltage and cost advantage, the positive electrode active material may be a lithium-containing transition metal oxide.
[0050] Examples of transition metal elements contained in the lithium-containing transition metal oxide include Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Y, Zr, W, etc. The lithium-containing transition metal oxide may contain only one transition metal element, or may contain two or more transition metal elements. The transition metal element may be at least one selected from the group consisting of Co, Ni, and Mn. The lithium-containing transition metal oxide may contain one or more typical metal elements as needed. Examples of typical metal elements include Mg, Al, Ca, Zn, Ga, Ge, Sn, Sb, Pb, Bi, etc. The typical metal element may be Al, etc.
[0051] Examples of the binder include fluororesin, polyacrylonitrile, polyimide resin, acrylic resin, polyolefin resin, rubber polymer, etc. Examples of the fluororesin include polytetrafluoroethylene, polyvinylidene fluoride, etc.
[0052] The conductive material may be, for example, a conductive carbonaceous material. Examples of the conductive carbonaceous material include carbon black, carbon nanotubes, graphite, etc. Examples of carbon black include acetylene black and ketjen black.
[0053] The thickener may be, for example, a cellulose derivative such as cellulose ether. Examples of cellulose derivatives include carboxymethyl cellulose (CMC) and its modified forms, methyl cellulose, etc. Examples of modified CMC include salts of CMC. Examples of salts include alkali metal salts (e.g., sodium salts), ammonium salts, etc.
[0054] The carbonaceous material disposed between the positive electrode current collector and the positive electrode mixture layer can be, for example, at least one selected from the conductive carbonaceous materials exemplified as the conductive material.
[0055] The positive electrode can be obtained, for example, by applying or filling a slurry containing the components of the positive electrode composite layer and a dispersion medium onto a positive electrode current collector, and then drying and compressing the coating. If necessary, a conductive carbonaceous material may be applied to the surface of the positive electrode current collector. The dispersion medium can be at least one selected from the group consisting of water and organic media (e.g., N-methyl-2-pyrrolidone).
[0056] (Separator) A porous sheet having ion permeability and insulating properties is used for the separator. Examples of the form of the porous sheet include a microporous film, a woven fabric, and a nonwoven fabric. The separator may be made of a polymer material. Examples of the polymer material include an olefin resin, a polyamide resin, and cellulose. Examples of the olefin resin include polyethylene, polypropylene, and a copolymer of ethylene and propylene. The separator may contain additives as needed. Examples of the additives include inorganic fillers.
[0057] The separator may include multiple layers that differ in at least one of form and composition, such as a laminate of a polyethylene microporous film and a polypropylene microporous film, or a laminate of a nonwoven fabric containing cellulose fibers and a nonwoven fabric containing thermoplastic resin fibers.
[0058] (Non-aqueous electrolyte) The non-aqueous electrolyte (non-aqueous electrolyte solution) contains a solvent (non-aqueous solvent) and a solute dissolved in the solvent. Examples of the solute include lithium salts. Various additives may be added to the electrolyte solution.
[0059] Known materials can be used as the solvent. Examples of solvents that can be used include cyclic carbonates, chain carbonates, cyclic carboxylic acid esters, chain carboxylic acid esters, chain ethers, fluorinated chain ethers, cyclic ethers, and fluorinated cyclic ethers. Examples of cyclic carbonates include propylene carbonate (PC), ethylene carbonate (EC), fluoroethylene carbonate (FEC), and vinylene carbonate (VC). Examples of chain carbonates include diethyl carbonate (DEC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC). Examples of cyclic carboxylic acid esters include γ-butyrolactone (GBL) and γ-valerolactone (GVL). Examples of chain carboxylic acid esters include non-aqueous solvents such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP). Examples of chain ethers include dimethyl ether, ethyl methyl ether, diethyl ether, ethyl propyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,1-dimethoxymethane, 1,1-diethoxyethane, and the like. The chain ether preferably includes a chain ether having two or more ether bonds. Examples of such chain ethers include 1,2-dimethoxyethane (DME), 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol ethyl methyl ether, diethylene glycol dibutyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol ethyl methyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, and tetraethylene glycol ethyl methyl ether.Examples of cyclic ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, and crown ethers. Fluorinated chain ethers have a structure in which one or more hydrogen atoms of the above-mentioned chain ethers are substituted with fluorine atoms. Examples of fluorinated chain ethers include bis(2,2,2-trifluoroethyl)ether, 1,1,2,2-tetrafluoroethyl 2,2,2-trifluoroethyl ether, and 1,1,2,2-tetrafluoroethyl 2,2,3,3-tetrafluoropropyl ether. Fluorinated cyclic ethers have a structure in which one or more hydrogen atoms of the above-mentioned cyclic ethers are substituted with fluorine atoms. An example of fluorinated cyclic ethers is 3,3,4,4-tetrafluorotetrahydrofuran. The non-aqueous solvent may be used alone or in combination of two or more.
[0060] Examples of lithium salts include lithium salts of chlorine-containing acids (LiClO 4 , LiAlCl 4 , LiB 10 Cl 10 etc.), lithium salts of fluorine-containing acids (LiPF 6 , LiPF 2 O 2 , LiBF 4 , LiSbF 6 , LiAsF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 etc.), lithium salt of fluorine-containing acid imide (LiN(FSO 2 ) 2 , LiN(CF 3 SO 2 ) 2 , LiN(CF 3 SO 2 ) (FSO 2 ), LiN(CF 3 SO 2 ) (C 4 F 9 SO 2), LiN(C 2 F 5 SO 2 ) 2 etc.), lithium halides (LiCl, LiBr, LiI etc.), lithium salts containing oxalate complexes (LiB(C 2 O 4 ) 2 , LiBF 2 (C 2 O 4 ), LiPF 4 (C 2 O 4 ), LiPF 2 (C 2 O 4 ) 2 The lithium salts may be used alone or in combination of two or more.
[0061] The concentration of the lithium salt in the electrolyte solution may be 1 mol / L or more and 5 mol / L or less, or 1 mol / L or more and 3 mol / L or less. By setting the lithium salt concentration within the above range, an electrolyte solution having excellent ionic conductivity and appropriate viscosity can be obtained.
[0062] The electrolytic solution may contain additives (for example, known additives). Examples of the additives include 1,3-propane sultone, methylbenzenesulfonate, cyclohexylbenzene, biphenyl, diphenyl ether, and fluorobenzene.
[0063] (Shape, etc.) The positive electrode, the negative electrode, and the separator constitute an electrode group. Examples of electrode groups include an electrode group in which a positive electrode and a negative electrode are wound with a separator interposed therebetween (a wound electrode group). The electrode group may have a form other than a wound type. For example, the electrode group may be an electrode group in which a positive electrode and a negative electrode are stacked with a separator interposed therebetween (a stacked electrode group). The form of the lithium secondary battery (B) is not limited, and may be cylindrical, prismatic, coin-shaped, button-shaped, laminated, or the like. The lithium secondary battery (B) includes an exterior body corresponding to these forms. The exterior body houses the electrode group and the non-aqueous electrolyte. The exterior body is not particularly limited, and an exterior body similar to that of a known lithium secondary battery may be used.
[0064] Below, examples of the lithium secondary battery (B) and the negative electrode (N) will be specifically described with reference to the drawings. However, the lithium secondary battery (B) and the negative electrode (N) are not limited to the configurations shown in the drawings. Components other than those essential to the lithium secondary battery (B) and the negative electrode (N) may be omitted. The examples described below can be modified based on the above description. Furthermore, the matters described below may be applied to the above embodiment.
[0065] (Embodiment 1) FIG. 1 is a longitudinal cross-sectional view schematically illustrating a lithium secondary battery 10 according to Embodiment 1. The lithium secondary battery 10 is a cylindrical battery. The lithium secondary battery 10 includes a cylindrical battery case and a wound electrode group 14 and a nonaqueous electrolyte (not shown) housed in the battery case. The battery case includes a cylindrical case body 15 with a bottom and a sealing body 16 that seals the opening of the case body 15. The case body 15 is made of metal. A gasket 27 is disposed between the case body 15 and the sealing body 16. The gasket 27 ensures the hermeticity of the battery case. The case body 15, the sealing body 16, and the gasket 27 form an exterior body. Within the case body 15, insulating plates 17 and 18 are disposed at both ends of the electrode group 14 in the direction of the winding axis.
[0066] The case body 15 has a step portion 21. The step portion 21 supports the sealing body 16. The sealing body 16 includes a filter 22, a lower valve body 23, an insulating member 24, an upper valve body 25, and a cap 26. The above-mentioned components constituting the sealing body 16 are electrically connected to each other except for the insulating member 24. The cap 26 functions as a positive electrode terminal. The case body 15 functions as a negative electrode terminal.
[0067] The electrode group 14 is a wound electrode group composed of a positive electrode 11, a negative electrode 12, and a separator 13. The positive electrode 11, the negative electrode 12, and the separator 13 are all strip-shaped. The negative electrode 12 is the above-mentioned negative electrode (N).
[0068] The positive electrode 11 is electrically connected to the cap 26 via a positive electrode lead 19. One end of the positive electrode lead 19 is connected to the positive electrode 11. The other end of the positive electrode lead 19 is connected to the sealing body 16 (filter 22). The negative electrode 12 is electrically connected to the case body 15 via a negative electrode lead 20. One end of the negative electrode lead 20 is connected to the negative electrode 12. The other end of the negative electrode lead 20 is connected to the case body 15.
[0069] 2 is a schematic cross-sectional view of an example of the negative electrode 12. The negative electrode 12 includes a current collector (negative electrode current collector) 12a and Mg-containing Li alloy layers 12b formed on both surfaces of the current collector 12a. The above-described intermetallic compound (not shown) is present at an interface 12i between the current collector 12a and the Mg-containing Li alloy layer 12b.
[0070] Fig. 3A shows a top view of an example of a separator on which spacers are formed. Fig. 3B shows a cross-sectional view taken along line IIIB-IIIB in Fig. 3A. In the example shown in Fig. 3A, spacers 31 are formed in a honeycomb shape on separator 13. As shown in Figs. 3A and 3B, spacers 31 have linear protrusions.
[0071] (Additional Notes) The above description discloses the following technologies: (Technology 1) A negative electrode for a lithium secondary battery, comprising: a current collector containing copper; and a lithium alloy layer disposed on the current collector, the lithium alloy layer containing magnesium, and an intermetallic compound of copper and magnesium present at the interface between the current collector and the lithium alloy layer. (Technology 2) The intermetallic compound is Cu 2The negative electrode for a lithium secondary battery according to Technical 1, wherein the intermetallic compound is Mg. (Technology 3) The negative electrode for a lithium secondary battery according to Technical 1 or 2, wherein in an X-ray diffraction pattern obtained by X-ray diffraction analysis, the ratio Icm / Ic of the peak intensity Icm of the (111) plane of the intermetallic compound to the peak intensity Ic of the (111) plane of Cu is in the range of 0.005 to 0.095. (Technology 4) The negative electrode for a lithium secondary battery according to any one of Technical 1 to 3, wherein the current collector includes a substrate and a metal layer disposed on the substrate, the metal layer containing copper, and the substrate is formed of stainless steel or resin. (Technology 5) A lithium secondary battery including a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein the negative electrode is the negative electrode for a lithium secondary battery according to any one of Technical 1 to 4, and wherein lithium metal precipitates in the negative electrode during charging and dissolves during discharging. (Technology 6) The lithium secondary battery according to Technology 5, further comprising a spacer formed on either the positive electrode or the separator, the spacer having a height of 10 μm or more.
[0072] The present disclosure will be described in more detail below with reference to examples. In these examples, a plurality of lithium secondary batteries were fabricated and evaluated according to the following procedure.
[0073] (Preparation of Battery A1) (1) Preparation of Positive Electrode A positive electrode active material, acetylene black (conductive material), and polyvinylidene fluoride (binder) were mixed in a mass ratio of 95:2.5:2.5 to obtain a mixture. An appropriate amount of N-methyl-2-pyrrolidone (dispersion medium) was added to the mixture and stirred to prepare a positive electrode slurry. A lithium-containing transition metal oxide containing Ni, Co, and Al was used as the positive electrode active material.
[0074] The positive electrode slurry was applied to both sides of an aluminum foil (positive electrode current collector) and dried to form a laminate. The laminate was compressed in the thickness direction using a roller. The compressed laminate was cut to a predetermined size. In this way, a positive electrode including a positive electrode current collector and positive electrode composite layers formed on both sides of the positive electrode current collector was produced.
[0075] (2) Preparation of Negative Electrode A negative electrode was prepared by pressure-bonding a Li-Mg alloy foil (thickness: 35 μm) to both sides of a copper foil (negative electrode current collector, thickness: 14 μm) in an inert gas atmosphere. The Li-Mg alloy foil was pressure-bonded to the surface of the copper foil under the conditions of step (ii) described above. Specifically, a Li-Mg alloy foil was first produced by rolling using volatile oil (dodecane) as the rolling oil. Next, the copper foil and two Li-Mg alloy foils were pressed together using a roll press at the linear pressure shown in Table 1, thereby pressure-bonding the copper foil and the Li-Mg alloy foil. The magnesium content of the Li-Mg alloy foil was set to the value shown in Table 1. The resulting laminate was then stored in an inert atmosphere at 40°C. In this manner, the negative electrode of Battery A1 was obtained.
[0076] (3) Preparation of non-aqueous electrolyte: LiPF in a non-aqueous solvent 6 and LiBF 2 (C 2 O 4 A liquid non-aqueous electrolyte was prepared by dissolving LiPF in the non-aqueous electrolyte. 6 and LiBF 2 (C 2 O 4 The concentrations of propylene carbonate (PC) and 1,2-dimethoxyethane (DME) were 1 mol / L and 0.1 mol / L, respectively. The non-aqueous solvent used was a mixture of propylene carbonate (PC) and 1,2-dimethoxyethane (DME) in a volume ratio of 1:2.
[0077] (4) Battery Assembly One end of an aluminum positive electrode lead was attached to the positive electrode current collector by welding. One end of a nickel negative electrode lead was attached to the negative electrode current collector by welding. A wound electrode assembly was fabricated by winding the positive and negative electrodes in an inert gas atmosphere with a separator between them. A polyethylene microporous membrane was used as the separator. A honeycomb-patterned spacer (height: approximately 30 μm) was formed on the separator.
[0078] Next, the electrode group was housed in an exterior housing. A bag-shaped exterior housing formed of a laminate sheet with an Al layer was used as the exterior housing. A nonaqueous electrolyte was injected into the exterior housing, and then the exterior housing was sealed. In this manner, a battery A1 (lithium secondary battery) was assembled. When the electrode group was housed in the exterior housing, the other end of the positive electrode lead and the other end of the negative electrode lead were exposed to the outside of the exterior housing.
[0079] (Batteries A2 to A7 and Battery C1) Anodes were produced in the same manner and under the same conditions as those for the production of the negative electrode of Battery A1, except that the magnesium content of the Li—Mg alloy foil, the production conditions of the Li—Mg alloy foil, and the conditions for pressing the current collector and the Li—Mg alloy foil were changed as shown in Table 1. Batteries A2 to A7 and Battery C1 were produced in the same manner and under the same conditions as those for the production of Battery A1, except that the resulting anodes were used.
[0080] (Evaluation of Charge-Discharge Cycle Characteristics) A charge-discharge cycle test was performed on the fabricated lithium secondary batteries. Specifically, the lithium secondary batteries were charged in a thermostatic chamber at 25°C under the following charge conditions, rested for 20 minutes, and discharged under the following discharge conditions. This cycle of charge, rest, and discharge constitutes one cycle, and 50 charge-discharge cycles were performed. (Charge) Constant current charging was performed at a current of 0.2 C until the battery voltage reached 4.1 V, and then constant voltage charging was performed at a voltage of 4.1 V until the charging current reached 0.02 C. (Discharge) Constant current discharging was performed at a current of 0.2 C until the battery voltage reached 3.0 V.
[0081] The change in the capacity retention rate was evaluated by the above cycle test. The capacity retention rate was calculated by measuring the battery capacity E0 before the cycle test and the battery capacity E1 after the cycle test using the following formula: Capacity retention rate (%) = 100 × E1 / E0
[0082] (Evaluation of the ratio Icm / Ic) The negative electrodes used in the above batteries were subjected to XRD analysis. From the XRD patterns obtained by the XRD analysis, the ratio of Cu (111) plane peak intensity Ic to Cu (111) plane peak intensity Ic was calculated. 2The ratio Icm / Ic of the peak intensity Icm of the (111) plane of Mg was determined. XRD analysis was performed under the following conditions. It is believed that in XRD analysis, X-rays penetrate the Li-Mg alloy layer and can analyze the interface between the Li-Mg alloy layer and the current collector. A sample for measurement was prepared by fixing a negative electrode (N) to a sample holder. Specifically, first, a thin layer of clay was applied to a glass sample holder, and the negative electrode (N) was placed on top of it. Then, the negative electrode (N) was fixed to the sample holder by pressing it with a glass plate, and a sample for measurement was obtained.
[0083] The XRD analyzer used was a Miniflex 600 manufactured by Rigaku Corporation, placed in an atmosphere maintained at a dew point of -60°C or less. The radiation source was a CuKα radiation source, the tube voltage was 40 kV, and the tube current was 15 mA. The sampling width was 0.02°, the scan speed was 10° / min, the divergence slit width was 0.625°, the receiving slit width was 13 mm (OPEN), and the scattering slit width was 8 mm. The obtained XRD pattern was fitted using a split pseudo-Voigt function by the RIR method to identify Cu and Cu. 2 Mg was identified and the peak intensity was calculated.
[0084] The XRD patterns obtained by XRD analysis for the negative electrodes of the batteries A1 and C1 are shown in Figure 4. As shown in Figure 4, the negative electrode of the battery A1 contains Cu. 2 A peak on the (111) plane of Mg was observed. This indicates that Cu exists at the interface between the current collector and the Li-Mg alloy foil. 2 On the other hand, in the negative electrode of battery C1, Cu 2 No peak of the (111) plane of Mg (peak at 2θ of about 22°) was observed.
[0085] Table 1 shows some of the production conditions for the negative electrode of each battery, along with the evaluation results. In the Li-Mg alloy foil production conditions in Table 1, "volatile oil" and "non-volatile oil" refer to the type of rolling oil used during production of the Li-Mg alloy foil. Silicone oil was used as the non-volatile oil. In the Li-Mg alloy foil production conditions in Table 1, "without vacuum drying" and "with vacuum drying" refer to whether the Li-Mg alloy foil was vacuum-dried before being pressure-bonded to the copper foil. In the pressure-bonding conditions in Table 1, the linear pressure refers to the linear pressure used when pressure-bonding the copper foil and the Li-Mg alloy foil. In the pressure-bonding conditions in Table 1, "with 40°C holding" and "without 40°C holding" refer to whether the resulting laminate was held at 40°C in an inert atmosphere after pressure-bonding the copper foil and the Li-Mg alloy foil.
[0086]
[0087] Batteries A1 to A7 are secondary batteries (B) according to the present disclosure, and battery C1 is a comparative example. The results shown in Table 1 are shown in FIG. 5. As shown in Table 1 and FIG. 5, battery C1 had a lower capacity retention rate than batteries A1 to A7. As shown in FIG. 5, when the ratio Icm / Ic was in the range of 0.005 to 0.095, the decrease in the capacity retention rate was particularly suppressed. If the ratio Icm / Ic was too low, it is thought that the adhesion between the current collector and the Li-Mg alloy foil was reduced, resulting in a decrease in the capacity retention rate. On the other hand, if the ratio Icm / Ic was too high, the Cu 2 It is believed that the capacity retention rate decreases due to the high resistance of the Mg layer.
[0088] The present disclosure can be used for negative electrodes for lithium secondary batteries and lithium secondary batteries. Although the present invention has been described with reference to presently preferred embodiments, such disclosure should not be interpreted as limiting. Various modifications and alterations will undoubtedly become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. Therefore, the appended claims should be construed to cover all modifications and alterations without departing from the true spirit and scope of the present invention.
[0089] 10: Lithium secondary battery 11: Positive electrode 12: Negative electrode 12a: Current collector 12b: Mg-containing Li alloy layer 12i: Interface 13: Separator 31: Spacer
Claims
1. A negative electrode for a lithium secondary battery comprising: a current collector containing copper; and a lithium alloy layer disposed on the current collector, the lithium alloy layer containing magnesium; and an intermetallic compound of copper and magnesium is present at the interface between the current collector and the lithium alloy layer.
2. The intermetallic compound is Cu 2 2. The negative electrode for a lithium secondary battery according to claim 1, wherein Mg is used.
3. The negative electrode for a lithium secondary battery according to claim 1 or 2, wherein in an X-ray diffraction pattern obtained by X-ray diffraction analysis, the ratio Icm / Ic of the peak intensity Icm of the (111) plane of the intermetallic compound to the peak intensity Ic of the (111) plane of Cu is in the range of 0.005 to 0.
095.
4. The negative electrode for a lithium secondary battery according to claim 1 or 2, wherein the current collector includes a substrate and a metal layer disposed on the substrate, the metal layer contains copper, and the substrate is formed of stainless steel or a resin.
5. A lithium secondary battery comprising a positive electrode, a negative electrode, a separator disposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte, wherein the negative electrode is the negative electrode for a lithium secondary battery according to claim 1, and in the negative electrode, lithium metal precipitates during charging, and the lithium metal dissolves during discharging.
6. The lithium secondary battery according to claim 5, further comprising a spacer formed on either the positive electrode or the separator, the spacer having a height of 10 μm or more.
Citation Information
Patent Citations
Electrode, battery, and battery pack
JP2014120399A
Lithium ion secondary battery
JP2018063872A
Nonaqueous electrolyte secondary battery
JP1997245836A
Manufacturing method of electrochemical element
JP2004253350A
Electrode plate for battery and lithium secondary battery including the same
JP2008135376A