Resin composition for sintering binder

The resin composition with a polymer derived from a specific compound addresses the limitations of existing binders by achieving lower firing temperatures and reduced residue, enhancing energy efficiency and sustainability in inorganic powder compact production.

WO2024225225A1PCT designated stage expired Publication Date: 2024-10-31NIPPON SHOKUBAI CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015729
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-22
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current resin compositions for fired binders, such as those using polyvinyl acetal resin, fail to adequately lower firing temperatures and reduce residue, especially when used in the production of inorganic powder compacts, which is a challenge in energy-saving and sustainable manufacturing processes.

Method used

A resin composition containing a polymer with a structural unit derived from a specific compound, represented by formula (a1), which includes linear or branched alkyl groups and has a glass transition temperature of 0°C or lower, is used as a binder. This composition allows for lower firing temperatures and reduced residue, with preferred compounds like 2-octyl (meth)acrylate, enhancing the flexibility and handleability of green sheets.

Benefits of technology

The resin composition effectively lowers firing temperatures and reduces residue, improving the energy efficiency and environmental sustainability of inorganic powder compact production by facilitating faster thermal decomposition and minimizing organic content after firing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015729_31102024_PF_FP_ABST
    Figure JP2024015729_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a resin composition, for a sintering binder, capable of lowering the sintering temperature and reducing residues. The problem can be solved by including, in a resin composition for a sintering binder, a polymer having a structural unit derived from a compound represented by formula (a1). [In formula (a1), Ra1 represents a hydrogen atom or a methyl group. Ra2 and Ra3 each represent a linear or branched alkyl group, the total number of carbon atoms in the alkyl groups of Ra2 and Ra3 is 2-20, and number of carbon atoms in Ra2 ≤ number of carbon atoms in Ra3 is satisfied.]
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition for baked binder

[0001] The present invention relates to a resin composition for a baked binder.

[0002] Inorganic powder compacts such as ceramic compacts are generally produced by preparing a green sheet from a slurry containing an inorganic powder and a binder, processing the green sheet into a desired shape, and then firing it at a high temperature to remove organic components such as the binder.

[0003] For example, Patent Document 1 describes the use of a polyvinyl acetal resin as the binder.

[0004] Japanese Patent Application Laid-Open No. 2001-106580

[0005] In recent years, energy conservation has been required from the viewpoint of the SDGs (Sustainable Development Goals) and the like, and lowering the sintering temperature is also required in the production of inorganic powder moldings. Furthermore, there is also a need for low residual carbonization even when sintered at low temperatures. However, when the binder of Patent Document 1 is used, the above requirements could not be fully satisfied. Therefore, an object of the present invention is to provide a resin composition for a sintered binder that allows for lower sintering temperatures and low residues.

[0006] As a result of extensive research to solve the above problems, the present inventors have found that by using a resin composition containing a polymer having structural units derived from a specific compound, it is possible to provide a resin composition for a sintered binder that can be sintered at a lower temperature and with less residue, and have thus completed the present invention.

[0007] That is, the present invention is as follows: [1] A resin composition for a baked binder, comprising a polymer having a structural unit derived from a compound represented by formula (a1). [In formula (a1), R a1 represents a hydrogen atom or a methyl group. a2 and R a3 represents a linear or branched alkyl group, R a2 and R a3 The total number of carbon atoms in the alkyl groups of R is 2 to 20, and a2The number of carbon atoms in ≦R a3 The number of carbon atoms satisfies the following formula.] [2] The resin composition according to [1], wherein the compound represented by formula (a1) is a compound whose homopolymer has a glass transition temperature of 0°C or lower. [3] The resin composition according to [1] or [2], wherein the compound represented by formula (a1) is 2-octyl(meth)acrylate. [4] The resin composition according to any one of [1] to [3], wherein, when heated at a rate of 10°C / min, the difference (b-a) between the temperature a at which the weight loss rate of the solid content of the resin composition is 5% and the temperature b at which the weight loss rate of the solid content of the resin composition is 90% is 200°C or lower. [5] The resin composition according to any one of [1] to [4], wherein the weight loss rate of the solid content of the resin composition is 95% or higher at 400°C. [6] The resin composition according to any one of [1] to [5], wherein the polymer contains a structural unit derived from the compound represented by formula (a1) in an amount of 50% by mass or higher. [7] The resin composition according to any one of [1] to [6], wherein the glass transition temperature of the polymer is -100 to 30°C. [8] The resin composition according to any one of [1] to [7], wherein the weight average molecular weight of the polymer is 10,000 to 1,000,000. [9] A slurry containing the resin composition according to any one of [1] to [8] and an inorganic powder.

[10] A green sheet formed from the slurry according to [9].

[11] A method of using a resin composition containing a polymer having a structural unit derived from a compound represented by formula (a1) as a sintered binder. [In formula (a1), R a1 represents a hydrogen atom or a methyl group. a2 and R a3 represents a linear or branched alkyl group, R a2 and R a3 The total number of carbon atoms in the alkyl groups of R is 2 to 20, and a2 The number of carbon atoms in ≦R a3The number of carbon atoms satisfies the following formula.]

[12] The method according to

[11] , wherein the compound represented by formula (a1) is a compound whose homopolymer has a glass transition temperature of 0°C or less.

[13] The method according to

[11] or

[12] , wherein the compound represented by formula (a1) is 2-octyl(meth)acrylate.

[14] The method according to any one of

[11] to

[13] , wherein, when heated at a rate of 10°C / min, the difference (b-a) between the temperature a at which the weight loss rate of the solid content of the resin composition is 5% and the temperature b at which the weight loss rate of the solid content of the resin composition is 90% is 200°C or less.

[15] The method according to any one of

[11] to

[14] , wherein the weight loss rate of the solid content of the resin composition at 400°C is 95% or more.

[16] The method according to any one of

[11] to

[15] , wherein the content of structural units derived from the compound represented by formula (a1) in the polymer is 50% by mass or more.

[17] The method according to any one of

[11] to

[16] , wherein the glass transition temperature of the polymer is -100 to 30°C.

[18] The method according to any one of

[11] to

[17] , wherein the weight average molecular weight of the polymer is 10,000 to 1,000,000.

[19] The method according to any one of

[11] to

[18] , wherein the resin composition and an inorganic powder are mixed to form a slurry.

[20] The method according to any one of

[11] to

[19] , wherein the slurry is formed into a green sheet.

[0008] According to the present invention, it is possible to provide a resin composition for a sintered binder that can be sintered at a lower temperature and with less residue.

[0009] An embodiment of the present invention will be described below, but the present invention is not limited thereto. Unless otherwise specified in this specification, "A to B" representing a numerical range means "greater than or equal to A and less than or equal to B." Furthermore, "(meth)acrylic acid" means acrylic acid or methacrylic acid, and "(meth)acrylate" means acrylate or methacrylate. The same applies to terms such as "(meth)acryloxy" and "(meth)acryloyl." Furthermore, a "structural unit derived from a specific monomer" corresponds to a structure in which the ethylenically unsaturated double bond of a specific monomer is opened (a structure in which the double bond (C═C) becomes a single bond (—C—C—)). This structure may not only be a structure obtained by polymerizing a specific monomer, but may also be a structural unit derived from a specific monomer obtained by post-modification of a structure obtained by polymerizing a different monomer.

[0010] The resin composition for a baked binder of the present invention is characterized by containing a polymer having a structural unit derived from a compound represented by formula (a1).

[0011] [Polymer] Each component constituting the polymer will be described below.

[0012] [Compound Represented by Formula (a1)] The polymer has a structural unit derived from a compound represented by the following formula (a1), i.e., the polymer has a structural unit represented by the following formula (a1'): When the polymer has a structural unit derived from a compound represented by formula (a1), the calcination temperature of the obtained calcined binder can be lowered and the residue can be reduced.

[0013] [In formulas (a1) and (a1′), R a1 represents a hydrogen atom or a methyl group. a2 and R a3 represents a linear or branched alkyl group, R a2 and R a3 The total number of carbon atoms in the alkyl groups of R is 2 to 20, and a2 The number of carbon atoms in ≦R a3 The number of carbon atoms is as follows.

[0014] The compound represented by formula (a1) corresponds to an ester of (meth)acrylic acid with an alcohol (hereinafter referred to as a secondary alkyl alcohol) in which two linear or branched alkyl groups and one hydrogen atom are bonded to a carbon atom directly bonded to a hydroxy group. Such a specific ester of secondary alkyl alcohol and (meth)acrylic acid tends to be easily thermally decomposed, which is thought to enable the resulting fired binder to be fired at a lower temperature and with less residue.

[0015] R a2 and R a3 Specific examples of the linear alkyl group represented by R include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, and an n-dodecyl group. a2 and R a3 Examples of the branched alkyl group represented by the formula (I) include an isopropyl group, an isobutyl group, a tert-butyl group, a 2-methylbutyl group, an isopentyl group, a neopentyl group, a 2,3-dimethyl-2-butyl group, a 3-methylheptyl group, a 4-methylheptyl group, and a 2-ethylhexyl group.

[0016] R a2 and R a3 is preferably a linear alkyl group.

[0017] R a2 and R a3 The total number of carbon atoms in the alkyl groups of R is preferably 3 to 20, more preferably 3 to 15, and even more preferably 5 to 14. a2 The number of carbon atoms in the alkyl group of R is preferably 1 to 4, and more preferably 1 or 2. a3 The alkyl group preferably has 4 to 12 carbon atoms, and more preferably 4 to 10 carbon atoms.

[0018] Specific examples of the compound represented by formula (a1) include isopropyl(meth)acrylate, 2-butyl(meth)acrylate, 2-pentyl(meth)acrylate, 3-pentyl(meth)acrylate, 2-hexyl(meth)acrylate, 2-heptyl(meth)acrylate, 3-heptyl(meth)acrylate, 2-octyl(meth)acrylate, 3-octyl(meth)acrylate, 4-octyl(meth)acrylate, 3-methyl-2-butyl(meth)acrylate, 3,3-dimethyl-2-butyl(meth)acrylate, 3-methyl-2-pentyl(meth)acrylate, 4 ...4 methyl-2-pentyl(meth)acrylate, 2,4-dimethyl-3-pentyl(meth)acrylate, 2-methyl-3-hexyl(meth)acrylate, 5-methyl-2-hexyl(meth)acrylate, 2,2-dimethyl-3-hexyl(meth)acrylate, 2,5-dimethyl-3-hexyl(meth)acrylate, 5-methyl-2-heptyl(meth)acrylate, 5-methyl-3-heptyl(meth)acrylate, 6-methyl-2-heptyl(meth)acrylate, 6-methyl-3-heptyl(meth)acrylate, and the like.

[0019] The compound represented by formula (a1) is a compound whose homopolymer has a glass transition temperature (Tg) of preferably 0°C or lower, more preferably -10°C or lower, and even more preferably -15°C or lower. By adjusting the Tg within the above range, the flexibility and handleability of the green sheet are improved. If the Tg is too low, the adhesiveness of the resulting green sheet increases, which in turn reduces handleability. Therefore, the Tg is, for example, -100°C or higher, preferably -80°C or higher. That is, the Tg of the homopolymer of the compound represented by formula (a1) is preferably -100 to 0°C, more preferably -80 to -10°C, and even more preferably -80 to -15°C.

[0020] In this specification, the "Tg of a homopolymer" may be, for example, a value described in "POLYMER HANDBOOK THIRD EDITION" (by J. BRANDRUP and E. H. IMMERGUT, published by John Wiley & Sons, Inc., 1989, pages VI / 209 to VI / 277) (when multiple Tg values ​​are described, the lowest value). For compounds not described in "POLYMER HANDBOOK THIRD EDITION," a value calculated by a computer using commercially available glass transition temperature calculation software (for example, "MATERIALS STUDIO" manufactured by Accelrys Software Inc., version: 4.0.0.0, module: Synthia, conditions: calculation with a weight average molecular weight of 100,000) can also be used, or a value obtained by measuring a homopolymer obtained by polymerization using a DSC (differential scanning calorimetry) according to a measurement method in accordance with JIS-K7121 can also be used.

[0021] From the viewpoint of lowering the firing temperature, the compound represented by formula (a1) is preferably 2-octyl(meth)acrylate, more preferably 2-octyl methacrylate. Furthermore, these compounds can be synthesized using biomass materials as raw materials, and are therefore preferred from the viewpoint of reducing the environmental load.

[0022] For example, 2-octyl (meth)acrylate can be obtained by cracking ricinoleic acid derived from castor oil collected and extracted from castor bean seeds, followed by esterification of 2-octanol obtained by distilling a mixture containing sebacic acid as a by-product with (meth)acrylic acid. The (meth)acrylic acid used in the production of 2-octyl (meth)acrylate may be bio-derived or petroleum-derived.

[0023] The structural unit derived from the compound represented by formula (a1) may be contained in the polymer either alone or in combination of two or more.

[0024] The proportion of structural units derived from the compound represented by formula (a1) in the polymer (preferably the total of structural units derived from the monomer components described below) is, for example, 30 to 100% by mass, preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, still more preferably 80% by mass or more, and particularly preferably 90% by mass or more. The upper limit of this proportion may be, for example, 98% by mass or less. By adjusting the proportion of structural units derived from the compound represented by formula (a1) within the above range, the effects of lowering the firing temperature and reducing residue of the resulting fired binder tend to be further enhanced.

[0025] [Compound Represented by Formula (a2)] The polymer may further contain a structural unit derived from the compound represented by formula (a2), i.e., the polymer may have a structural unit represented by the following formula (a2'): By containing a structural unit derived from the compound represented by formula (a2), the handleability of the polymer can be improved without impairing the effects of lowering the firing temperature and reducing residue of the resulting fired binder.

[0026] [In formulas (a2) and (a2′), R a4 represents a hydrogen atom or a methyl group. a5 and R a6 represents an alkyl group, and R a5 and R a6 The total number of carbon atoms in the alkyl group of R is 2 to 20. a5 and R a6 are bonded to each other to form a ring.

[0027] R a5 and R a6 The alkyl group represented by the formula (I) may be linear or branched.

[0028] R a5 and R a6Specific examples of the alkyl group represented by the formula (I) include linear alkyl groups such as a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, and an n-dodecyl group; and branched alkyl groups such as an isopropyl group, an isobutyl group, a tert-butyl group, a 2-methylbutyl group, an isopentyl group, a neopentyl group, a 2,3-dimethyl-2-butyl group, a 3-methylheptyl group, a 4-methylheptyl group, and a 2-ethylhexyl group.

[0029] R a5 and R a6 The total number of carbon atoms in the alkyl groups is preferably 3 to 20, more preferably 6 to 15, and even more preferably 8 to 14.

[0030] R a5 and R a6 The ring formed by bonding together may be a hydrocarbon ring having one cyclic moiety such as a cycloalkyl group, or may be a hydrocarbon ring having two cyclic moieties. Examples of hydrocarbon rings having two cyclic moieties include a bridged ring structure in which the two rings share three or more atoms, such as a norbornyl group, a fused ring structure in which the two rings share two atoms, such as a decalin-1-yl group, and a spiro ring structure in which the two rings share one atom, such as a spiro[2.2]pentan-1-yl group, and among these, a bridged ring structure is preferred.

[0031] Specific examples of the compound represented by formula (a2) include cyclopropyl(meth)acrylate, cyclopentyl(meth)acrylate, cyclohexyl(meth)acrylate, cycloheptyl(meth)acrylate, cyclooctyl(meth)acrylate, and isobornyl(meth)acrylate, with isobornyl(meth)acrylate being preferred. Isobornyl(meth)acrylate can be obtained by isomerizing α-pinene obtained from pine resin or pine essential oil to camphene, and then reacting the camphene with (meth)acrylic acid. In other words, it can be synthesized using biomass materials as part of the raw materials, and is therefore preferred from the perspective of reducing environmental impact.

[0032] The structural unit derived from the compound represented by formula (a2) may be contained in the polymer either alone or in combination of two or more.

[0033] When the polymer contains structural units derived from the compound represented by formula (a2), the proportion of the structural units derived from the compound represented by formula (a2) in the polymer (preferably the sum of structural units derived from the monomer components described below) is, for example, 5 to 50% by mass, preferably 10 to 40% by mass. Adjusting this proportion to be equal to or greater than the lower limit further improves the handleability of the polymer, while adjusting this proportion to be equal to or less than the upper limit further enhances the effect of lowering the firing temperature and reducing residue of the fired binder. It is not necessary for the polymer to essentially contain structural units derived from the compound represented by formula (a2); the proportion may be 5% by mass or less, 3% by mass or less, or even 0% by mass. Furthermore, when the polymer contains structural units derived from the compound represented by formula (a2), the content of the structural units derived from the compound represented by formula (a2) is, for example, 5 to 100 parts by mass, preferably 10 to 50 parts by mass, based on 100 parts by mass of the structural units derived from the compound represented by formula (a1). The content may be 5 parts by mass or less, 3 parts by mass or less, or 0 part by mass.

[0034] [(Meth)acrylic acid alkyl ester (a3)] The polymer may further contain a structural unit derived from a (meth)acrylic acid alkyl ester other than the compounds represented by formula (a1) and formula (a2) (hereinafter, may be referred to as a (meth)acrylic acid alkyl ester (a3)).

[0035] Specific examples of the (meth)acrylic acid alkyl ester (a3) ​​include esters of (meth)acrylic acid with primary alkyl alcohols (i.e., alcohols in which one alkyl group and two hydrogen atoms are bonded to the carbon atom directly bonded to the hydroxy group), such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, tridecyl (meth)acrylate, dodecyl (meth)acrylate, stearyl (meth)acrylate, heneicosyl (meth)acrylate, and tetracosyl (meth)acrylate; Esters of tertiary alkyl alcohols (that is, alcohols having three alkyl groups bonded to the carbon atom directly bonded to the hydroxy group) and (meth)acrylic acid, such as tert-butyl (meth)acrylate; and the like.

[0036] The number of carbon atoms in the alkyl group constituting the (meth)acrylic acid alkyl ester (a3) ​​is not particularly limited, but is preferably 1 to 20, and more preferably 1 to 10.

[0037] Among the (meth)acrylic acid alkyl esters (a3), (meth)acrylic acid alkyl esters having a homopolymer Tg of −20° C. or less and methacrylic acid C 1-5 At least one selected from alkyl esters is also preferred. 1-5 By appropriately adjusting the content of structural units derived from alkyl esters, it becomes easy to adjust the Tg of the polymer to the range described below.

[0038] The Tg of the low Tg (meth)acrylic acid alkyl ester is preferably −100 to −20° C., more preferably −80 to −30° C. Among the low Tg (meth)acrylic acid alkyl esters, n-butyl acrylate, n-octyl acrylate, and 2-ethylhexyl acrylate are preferred.

[0039] Also, methacrylic acid C 1-5 Examples of alkyl esters include methacrylic acid C 1-4 Alkyl esters are preferred.

[0040] The structural unit derived from the (meth)acrylic acid alkyl ester (a3) ​​may be contained in the polymer either alone or in two or more types.

[0041] When the polymer contains a structural unit derived from a (meth)acrylic acid alkyl ester (a3), the proportion of the structural unit derived from the (meth)acrylic acid alkyl ester (a3) ​​in the polymer (preferably the total of structural units derived from the monomer components described below) (particularly, the proportion of the structural unit derived from the low Tg (meth)acrylic acid alkyl ester and methacrylic acid C 1-5 The total proportion of structural units derived from alkyl esters) is, for example, 5 to 50% by mass, preferably 10 to 40% by mass. The polymer does not necessarily need to contain structural units derived from (meth)acrylic acid alkyl ester (a3), and the proportion may be 5% by mass or less, 3% by mass or less, or even 0% by mass. When the polymer contains structural units derived from (meth)acrylic acid alkyl ester (a3), the content of the structural units derived from (meth)acrylic acid alkyl ester (a3) ​​(particularly, the content of the low Tg (meth)acrylic acid alkyl ester and methacrylic acid C 1-5 The total content of structural units derived from alkyl esters is, for example, 5 to 100 parts by mass, preferably 10 to 55 parts by mass or 10 to 50 parts by mass, relative to 100 parts by mass of the content of structural units derived from the compound represented by formula (a1). The content may be 5 parts by mass or less, 3 parts by mass or less, or even 0 parts by mass.

[0042] [Acid Group-Containing Monomer] The polymer may further contain a structural unit derived from an acid group-containing monomer. By containing the structural unit derived from an acid group-containing monomer, the dispersibility of the inorganic powder can be improved when preparing a slurry containing the resin composition for a fired binder described below and the inorganic powder.

[0043] The acid group-containing monomer may have at least one acid group and at least one polymerizable unsaturated group in the molecule. Examples of the acid group include a sulfo group and a carboxy group, with a carboxy group being preferred. Specific examples of the acid group-containing monomer include unsaturated monocarboxylic acids such as (meth)acrylic acid, cinnamic acid, and crotonic acid; unsaturated dicarboxylic acids such as maleic acid, fumaric acid, itaconic acid, and citraconic acid; monoesters of unsaturated dicarboxylic acids such as maleic acid monomethyl ester, maleic acid monobutyl ester, itaconic acid monomethyl ester, and itaconic acid monobutyl ester; anhydrides of unsaturated dicarboxylic acids such as maleic anhydride; 2-acryloyloxyethyl succinic acid, 2-acryloyloxyethyl phthalic acid, and 2-acryloyloxyethyl hexahydrophthalic acid. Among these, unsaturated monocarboxylic acids are preferred, with (meth)acrylic acid being more preferred.

[0044] The structural unit derived from the acid group-containing monomer may be contained in the polymer either alone or in combination of two or more.

[0045] When the polymer contains structural units derived from acid group-containing monomers, the proportion of structural units derived from the acid group-containing monomers in the polymer (preferably the sum of structural units derived from the monomer components described below) is, for example, 0.01 to 10% by mass, preferably 0.05 to 3% by mass, more preferably 0.1 to 1% by mass, and may be 0.1 to 10% by mass, 0.3 to 8% by mass, or 0.8 to 5% by mass. Adjusting the proportion to be equal to or greater than the lower limit can further improve the dispersibility of the inorganic powder during slurry preparation, while adjusting the proportion to be equal to or less than the upper limit can further enhance the effects of lowering the firing temperature and reducing residue of the resulting fired binder. Note that the polymer does not necessarily need to contain structural units derived from acid group-containing monomers, and the proportion may be 0.8% by mass or less, 0.1% by mass or less, or even 0% by mass. Furthermore, when the polymer contains a structural unit derived from an acid group-containing monomer, the content of the structural unit derived from the acid group-containing monomer is, for example, 0.01 to 10 parts by mass, preferably 0.1 to 1 part by mass, or may be 0.1 to 10 parts by mass or 0.8 to 5 parts by mass, relative to 100 parts by mass of the structural unit derived from the compound represented by Formula (a1). Furthermore, the content may be 0.8 parts by mass or less, 0.1 parts by mass or less, or even 0 part by mass.

[0046] [Hydroxyl Group-Containing Monomer] The polymer may further contain a structural unit derived from a hydroxyl group-containing monomer. By including a structural unit derived from a hydroxyl group-containing monomer, the dispersibility of the inorganic powder during slurry preparation can be improved.

[0047] The hydroxyl group-containing monomer may be any monomer having at least one hydroxyl group and at least one polymerizable unsaturated group in the molecule. Specific examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; halogen-substituted hydroxyalkyl (meth)acrylates such as 3-chloro-2-hydroxypropyl (meth)acrylate; modified hydroxyalkyl (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate and 2-(meth)acryloyloxyethyl 2-hydroxyethyl phthalate; oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate; and hydroxyl group-containing vinyl monomers such as vinyl alcohol and allyl alcohol. Among these, hydroxyalkyl (meth)acrylates are preferred, and hydroxy C 2-4 Alkyl (meth)acrylates are more preferred.

[0048] The structural unit derived from the hydroxyl group-containing monomer may be contained in the polymer either alone or in combination of two or more.

[0049] When the polymer contains structural units derived from hydroxyl group-containing monomers, the proportion of structural units derived from hydroxyl group-containing monomers in the polymer (preferably the sum of structural units derived from the monomer components described below) is, for example, 0.1 to 15% by mass, preferably 0.3 to 10% by mass, more preferably 0.8 to 5% by mass, even more preferably 1.0 to 5% by mass, and may be 0.8 to 3% by mass. By adjusting the proportion to be equal to or greater than the lower limit, the dispersibility of the inorganic powder during slurry preparation can be further improved. By adjusting the proportion to be equal to or less than the upper limit, the effect of lowering the firing temperature of the fired binder and reducing residue can be further enhanced. Note that the polymer does not necessarily need to contain structural units derived from hydroxyl group-containing monomers, and the proportion may be 0.8% by mass or less, 0.1% by mass or less, or even 0% by mass. Furthermore, when the polymer contains structural units derived from hydroxyl group-containing monomers, the content of the structural units derived from hydroxyl group-containing monomers is, for example, 0.1 to 20 parts by mass, preferably 1.5 to 10 parts by mass, or may be 0.8 to 5 parts by mass, relative to 100 parts by mass of the structural units derived from the compound represented by Formula (a1). Furthermore, the content may be 0.8 parts by mass or less, 0.1 parts by mass or less, or even 0 part by mass.

[0050] [Styrene-based Monomer] The polymer may further contain a structural unit derived from a styrene-based monomer. By containing a structural unit derived from a styrene-based monomer, the Tg of the polymer can be easily adjusted to the range described below without impairing the effects of lowering the firing temperature and reducing residue of the resulting fired binder.

[0051] The styrene-based monomers include those having a halogen atom (for example, a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), an alkyl group (for example, a C group such as a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, or a tert-butyl group). 1-4 alkyl group), vinyl group, alkoxysilyl group (e.g., trimethoxysilyl group, triethoxysilyl group, etc.) 1-4and styrene which may have one or more substituents such as a halogen atom and an alkyl group.

[0052] Specific examples of the styrene-based monomer include styrene, α-methylstyrene, p-methylstyrene, tert-butylstyrene, chlorostyrene, chloromethylstyrene, divinylbenzene, p-styryltrimethoxysilane, and 2-styrylethyltrimethoxysilane, with styrene being preferred.

[0053] The structural unit derived from a styrene-based monomer may be contained in the polymer either alone or in combination of two or more.

[0054] When the polymer contains structural units derived from styrene-based monomers, the proportion of structural units derived from styrene-based monomers in the polymer (preferably the total of structural units derived from the monomer components described below) is, for example, 5 to 50% by mass, preferably 10 to 40% by mass. The polymer does not necessarily need to contain structural units derived from styrene-based monomers, and the proportion may be 5% by mass or less, 3% by mass or less, or even 0% by mass. When the polymer contains structural units derived from styrene-based monomers, the content of the structural units derived from styrene-based monomers is, for example, 5 to 100 parts by mass, preferably 10 to 50 parts by mass, based on 100 parts by mass of the content of structural units derived from the compound represented by Formula (a1). The content may be 5 parts by mass or less, 3 parts by mass or less, or even 0 parts by mass.

[0055] [Nitrogen-Containing Monomer] The polymer may further have a structural unit derived from a nitrogen-containing monomer. By including the structural unit derived from a nitrogen-containing monomer, the dispersibility of the inorganic powder can be improved when preparing a slurry containing the resin composition for a fired binder described below and the inorganic powder.

[0056] The nitrogen atom-containing monomer may be any monomer having at least a substituent containing a nitrogen atom as a constituent and a polymerizable unsaturated group in the molecule. The nitrogen atom-containing monomer does not include compounds having at least one of a styrene structure, an acid group, and a hydroxyl group. Examples of the nitrogen atom-containing monomer include nitrogen-based heterocycle-containing monomers, amino group-containing monomers, and amide group-containing monomers. In this specification, amino group-containing monomers and amide group-containing monomers containing a nitrogen-based heterocycle are referred to as nitrogen-based heterocycle-containing monomers.

[0057] Specific examples of nitrogen-based heterocycle-containing monomers include vinyllactam-based monomers such as N-methylvinylpyrrolidone, N-vinylpiperidone, N-vinylcaprolactam, N-vinylpyrrolidone, N-vinyl-2-pyrrolidone, and N-(meth)acryloylpyrrolidone; maleimide-based monomers such as maleimide, N-phenylmaleimide, and N-cyclohexylmaleimide; piperidyl (meth)acrylic monomers such as 2,2,6,6-tetramethyl-4-piperidyl (meth)acrylate and 1,2,2,6,6-pentamethyl-4-piperidyl (meth)acrylate; aziridinyl group-containing (meth)acrylic monomers such as (meth)acryloylaziridine and 2-aziridinylethyl (meth)acrylate; Addition-polymerizable oxazolines such as 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline, 2-isopropenyl-5-methyl-2-oxazoline, and 2-isopropenyl-5-ethyl-2-oxazoline; and the like.

[0058] Specific examples of the amino group-containing monomer include amino group-containing (meth)acrylic monomers such as N,N-dimethylaminomethyl (meth)acrylate and N,N-dimethylaminoethyl (meth)acrylate.

[0059] Examples of the amide group-containing monomer include (meth)acrylamide-based monomers such as (meth)acrylamide, N-monomethyl(meth)acrylamide, N-monoethyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-n-propyl(meth)acrylamide, N-isopropyl(meth)acrylamide, methylenebis(meth)acrylamide, N-butoxymethyl(meth)acrylamide, dimethylaminoethyl(meth)acrylamide, N,N-dimethylaminopropylacrylamide, and diacetone acrylamide.

[0060] As the nitrogen atom-containing monomer, a nitrogen-based heterocycle-containing monomer is preferred, a vinyl lactam monomer or a piperidyl(meth)acrylic monomer is more preferred, and N-vinyl-2-pyrrolidone, 2,2,6,6-tetramethyl-4-piperidyl(meth)acrylate, and 1,2,2,6,6-pentamethyl-4-piperidyl(meth)acrylate are even more preferred. Furthermore, from the viewpoint of improving light stability, a nitrogen atom-containing monomer having a hindered amine structure is preferred. As such a monomer, a monomer having a 2,2,6,6-tetraalkylpiperidine ring structure and a polymerizable unsaturated group in the molecule is preferred, a monomer having a 2,2,6,6-tetramethylpiperidine ring structure and a polymerizable unsaturated group is more preferred, and 2,2,6,6-tetramethyl-4-piperidyl(meth)acrylate and 1,2,2,6,6-pentamethyl-4-piperidyl(meth)acrylate are even more preferred.

[0061] In addition, from the viewpoint of further improving the dispersibility of the inorganic powder when preparing the slurry, the nitrogen atom-containing monomer is preferably an amino group-containing (meth)acrylic monomer, and diC 1-4 Alkylamino C 1-4 Alkyl (meth)acrylates are more preferred.

[0062] The structural unit derived from the nitrogen atom-containing monomer may be contained in the polymer either alone or in combination of two or more.

[0063] When the polymer contains structural units derived from nitrogen-atom-containing monomers, the proportion of the structural units derived from the nitrogen-atom-containing monomers in the polymer (preferably the sum of structural units derived from the monomer components described below) is, for example, 0.05 to 10% by mass, preferably 0.1 to 1% by mass, and may be 0.1 to 10% by mass or 0.5 to 5% by mass. The polymer does not necessarily need to contain structural units derived from nitrogen-atom-containing monomers, and the proportion may be 0.5% by mass or less, 0.1% by mass or less, or even 0% by mass. Adjusting the proportion to be equal to or greater than the lower limit can further enhance the dispersibility of the inorganic powder during slurry preparation, while adjusting the proportion to be equal to or less than the upper limit can further enhance the effects of lowering the firing temperature and reducing residue of the resulting fired binder. Furthermore, when the polymer contains a structural unit derived from a nitrogen atom-containing monomer, the content of the structural unit derived from the nitrogen atom-containing monomer is, for example, 0.05 to 10 parts by mass, preferably 0.1 to 1 part by mass, and may be 0.1 to 10 parts by mass or 0.5 to 5 parts by mass, relative to 100 parts by mass of the structural unit derived from the compound represented by Formula (a1). Furthermore, the content may be 0.5 parts by mass or less, 0.1 parts by mass or less, or even 0 part by mass.

[0064] [Crosslinkable Monomer] The polymer may further contain a structural unit derived from a crosslinkable monomer. By including a structural unit derived from a crosslinkable monomer, toughness during processing of the green sheet can be improved.

[0065] The crosslinkable monomer may be any monomer that does not have a styrene structure, an acid group, a hydroxyl group, or a substituent containing a nitrogen atom as a constituent, and that has a crosslinkable functional group and a polymerizable unsaturated group in the molecule. Examples of the crosslinkable functional group include a polymerizable unsaturated group, an epoxy group, and a hydrolyzable silyl group. The hydrolyzable silyl group refers to a silyl group to which a hydrolyzable group (e.g., an alkoxy group, a halogen atom, etc.) is bonded.

[0066] Examples of crosslinkable monomers include monomers having two or more polymerizable unsaturated groups, silane coupling agents having a hydrolyzable silyl group and a polymerizable unsaturated group, and epoxy group-containing crosslinkable monomers having an epoxy group and a polymerizable unsaturated group (but excluding hydrolyzable silyl groups).

[0067] Specific examples of the monomer having two or more polymerizable unsaturated groups include di(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, ethylene oxide-modified 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, and propylene oxide-modified neopentyl glycol di(meth)acrylate; polyalkylene glycol di(meth)acrylates having an added mole number of alkylene oxide groups of 2 to 4 carbon atoms of 2 to 50, such as polyethylene glycol di(meth)acrylate having an added mole number of ethylene oxide of 2 to 50, and polypropylene glycol di(meth)acrylate having an added mole number of propylene oxide of 2 to 50; Tri(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as ethoxylated glycerin tri(meth)acrylate, propylene oxide-modified glycerol tri(meth)acrylate, ethylene oxide-modified trimethylolpropane tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, and trimethylolpropane triethoxytri(meth)acrylate; tetra(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, and ditrimethylolpropane tetra(meth)acrylate; penta(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as dipentaerythritol penta(meth)acrylate; hexa(meth)acrylates of polyhydric alcohols having 1 to 10 carbon atoms, such as dipentaerythritol hexa(meth)acrylate; 2-(2'-vinyloxyethoxyethyl)(meth)acrylate; and the like.

[0068] Specific examples of the silane coupling agent include (meth)acryloyl group-containing silane coupling agents such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and 3-(meth)acryloxyethoxypropyltrimethoxysilane; vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane; and epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0069] Specific examples of the epoxy group-containing crosslinkable monomer include epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate, α-methylglycidyl (meth)acrylate, and 2-glycidyloxyethyl (meth)acrylate; and epoxy group-containing vinyl monomers such as allyl glycidyl ether.

[0070] The structural unit derived from the crosslinkable monomer may be contained in the polymer either alone or in combination of two or more kinds.

[0071] When the polymer contains structural units derived from crosslinkable monomers, the proportion of the structural units derived from the crosslinkable monomers in the polymer (preferably the total of structural units derived from the monomer components described below) is, for example, 0.05 to 5% by mass, preferably 0.1 to 3% by mass. The polymer does not necessarily need to contain structural units derived from crosslinkable monomers, and the proportion may be 0.05% by mass or less, or even 0% by mass. When the polymer contains structural units derived from crosslinkable monomers, the content of the structural units derived from the crosslinkable monomers is, for example, 0.05 to 5 parts by mass, preferably 0.1 to 3 parts by mass, based on 100 parts by mass of the structural units derived from the compound represented by formula (a1). The content may be 0.1 parts by mass or less, or even 0 parts by mass.

[0072] [Other Monomers] The polymer may further have a structural unit derived from a monomer other than the compound represented by formula (a1), the compound represented by formula (a2), the (meth)acrylic acid alkyl ester (a3), the acid group-containing monomer, the hydroxyl group-containing monomer, the styrene-based monomer, the nitrogen atom-containing monomer, and the crosslinkable monomer. The other monomer may be a monomer other than the above-mentioned monomers and have at least one polymerizable unsaturated group in the molecule.

[0073] Specific examples of the other monomers include: fluoroalkyl (meth)acrylates such as trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, and octafluoropentyl (meth)acrylate; alkoxyalkyl group-containing (meth)acrylates such as methoxyethyl (meth)acrylate, methoxybutyl (meth)acrylate, ethoxybutyl (meth)acrylate, and trimethylolpropane tripropoxy (meth)acrylate; carbonyl group-containing (meth)acrylates such as (meth)acryloxyalkyl propenal, acetonyl (meth)acrylate, diacetone (meth)acrylate, 2-hydroxypropyl (meth)acrylate acetylacetate, butanediol-1,4-acrylate acetylacetate, and 2-(acetoacetoxy)ethyl (meth)acrylate; vinyl-based monomers such as vinyl acetate, vinyl chloride, and vinyl benzoate; and olefin-based monomers such as ethylene and propylene.

[0074] The structural unit derived from the other monomer may be contained in the polymer either alone or in combination of two or more kinds.

[0075] When the polymer contains structural units derived from other monomers, the proportion of the structural units derived from other monomers in the polymer (preferably the total of structural units derived from the monomer components described below) is, for example, 0.1 to 20% by mass, preferably 1 to 10% by mass. Note that the polymer does not necessarily need to contain structural units derived from other monomers, and the proportion may be 10% by mass or less, 5% by mass or less, or even 0% by mass.

[0076] [Physical Properties of Polymer] The glass transition temperature (Tg) of the polymer is not particularly limited, but is preferably −100 to 0°C, more preferably −80 to −10°C, and even more preferably −70 to −15°C. Adjusting the Tg to the upper limit or less improves the flexibility and handleability of the green sheet. Furthermore, setting the Tg to the lower limit or more can prevent the resulting green sheet from becoming too sticky, which would otherwise result in a decrease in handleability. From the perspective of the handleability of the slurry before green sheet preparation, the Tg of the polymer is preferably −70 to 30°C, more preferably −60 to 25°C, and even more preferably −50 to 20°C. Adjusting the Tg to the upper limit or less ensures that the slurry has fluidity that allows it to be handled at room temperature. Furthermore, setting the Tg to the lower limit or more can prevent a decrease in yield due to adhesion to containers and equipment during handling of the slurry. That is, the Tg of the polymer is preferably −100 to 30° C., more preferably −80 to 25° C., even more preferably −70 to 20° C., still more preferably −60 to 0° C., particularly preferably −50 to −10° C., and most preferably −50 to −15° C.

[0077] The glass transition temperature (Tg) of the polymer can be measured by differential scanning calorimetry (AST D3418-08), and the Tg can be calculated from the Fox equation shown in the following formula (1): A It may be converted from (K).

[0078] [In formula (1), Tg A : Tg (K) of polymer, Tg n : Tg (K), W of the homopolymer of each monomer used n : Mixing ratio of each monomer used (mass%)]

[0079] As will be described later, the polymer may be present in the form of emulsion particles, and the emulsion particles may have a single layer or a multilayer structure. When the emulsion particles have a multilayer structure, the glass transition temperature of the entire polymer constituting the multilayer emulsion particles may be calculated from the above formula using the blending ratio of each monomer in all the monomer components used in the multistage emulsion polymerization and the glass transition temperature of the corresponding homopolymer of each monomer.

[0080] The weight-average molecular weight (Mw) of the polymer is not particularly limited, but is preferably 10,000 to 1,000,000, and more preferably 20,000 to 700,000. By adjusting the Mw to a predetermined value or less, the flexibility and handleability of the green sheet can be improved. Furthermore, by adjusting the Mw to a predetermined value or more, the resulting green sheet can be made more resistant to deformation under its own weight (shape retention) and stronger.

[0081] [Method for Producing Polymer] The polymer can be obtained by polymerizing the compound represented by the above-mentioned formula (a1), the compound represented by formula (a2) used as needed, (meth)acrylic acid alkyl esters other than the compounds represented by formula (a1) and formula (a2), acid group-containing monomers, hydroxyl group-containing monomers, styrene-based monomers, nitrogen atom-containing monomers, crosslinkable monomers, and other monomers (hereinafter, these monomers are collectively referred to as monomer components). As the polymerization method, known polymerization methods can be used, such as solution polymerization, bulk polymerization, suspension polymerization, and emulsion polymerization. Among these, solution polymerization and emulsion polymerization are preferred. The types, combinations, and blending ratios of preferred monomer components used in each polymerization method are similar to those described above for the preferred monomers for forming the polymer. Preferred production methods are described in detail below, but are not limited thereto.

[0082] Specific means and conditions for carrying out the solution polymerization method can be appropriately selected and adopted from means and techniques used in conventionally known solution polymerization methods. For example, any method can be adopted, such as a method of charging the monomer components all at once and polymerizing them, a method of polymerizing the monomer components while adding them dropwise, or a method of charging some of the monomer components all at once and polymerizing the remaining monomer components while adding them dropwise. When charging the monomer components all at once and polymerizing them, it is more preferable to charge a polymerization initiator together with the monomer components so as to produce a polymer with a high molecular weight. When polymerizing the monomer components while adding them dropwise, it is more preferable to add a mixture of the monomer components and the polymerization initiator dropwise in order to keep the ratio of the monomer components to the polymerization initiator as constant as possible during polymerization.

[0083] Specific examples of the polymerization initiator used in the solution polymerization method include known polymerization initiators such as peroxide-based polymerization initiators such as methyl ethyl ketone peroxide, benzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, t-butyl hydroperoxide, cumene hydroperoxide, t-butyl peroxyoctoate, t-butyl peroxybenzoate, and lauroyl peroxide; and azo-based polymerization initiators such as azobisisobutyronitrile, 2,2-azobis(2-methylbutyronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2-diaminopropane) hydrochloride, 4,4-azobis(4-cyanovaleric acid), and 2,2-azobis(2-methylpropionamidine). One type of polymerization initiator may be used alone, or two or more types may be used in combination.

[0084] The amount of the polymerization initiator used in the solution polymerization method is preferably 0.01 to 3 parts by mass per 100 parts by mass of the monomer components. If the amount of the polymerization initiator is outside the above range, a polymer having the desired weight average molecular weight may not be obtained.

[0085] The solvent used in the solution polymerization method is preferably an organic solvent, and specific examples thereof include aliphatic hydrocarbon solvents such as n-hexane and n-heptane; alicyclic hydrocarbon solvents such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, trimethylcyclohexane, ethylcyclohexane, diethylcyclohexane, decahydronaphthalene, bicycloheptane, tricyclodecane, hexahydroindenecyclohexane, cyclooctane, α-pinene, terpinolene, and limonene; aromatic hydrocarbon solvents such as toluene, xylene, benzene, and solvent naphtha; aliphatic ester solvents such as ethyl acetate and butyl acetate; ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, and ethylene glycol monobutyl ether. Examples of suitable solvents include (poly)alkylene glycol monoalkyl ether acetate solvents such as ethylene glycol monophenyl ether acetate, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether acetate, and propylene glycol monopropyl ether acetate; (poly)alkylene glycol monophenyl ether acetate solvents such as ethylene glycol monophenyl ether acetate and propylene glycol monophenyl ether acetate; and diesters of one molecule of (poly)alkylene glycol with two molecules of dicarboxylic acid such as ethylene glycol diadipate and ethylene glycol disuccinate. Among these, aliphatic ester solvents and / or aromatic hydrocarbon solvents are preferred, and aliphatic ester solvents are more preferred. These solvents may be used alone or in combination of two or more.

[0086] The amount of the solvent used in the solution polymerization method may be appropriately determined depending on the reaction conditions, the composition of the monomer components, and the like so as to obtain a polymer having desired physical properties. For example, the amount of the solvent used is preferably 10 to 300 parts by mass, more preferably 30 to 250 parts by mass, and even more preferably 50 to 200 parts by mass, relative to 100 parts by mass of the monomer components.

[0087] The reaction conditions in the solution polymerization method, such as the reaction temperature and reaction time, are not particularly limited. Specifically, they can be appropriately determined depending on the composition of the monomer components and the properties required of the resulting polymer, and the reaction temperature is, for example, 0 to 100°C, preferably 50 to 95°C, and more preferably 60 to 90°C, and the reaction time is, for example, 0.5 to 30 hours, preferably 1 to 20 hours, and more preferably 3 to 10 hours. The reaction pressure is also not particularly limited, and may be normal pressure (atmospheric pressure), reduced pressure, or increased pressure. It is desirable to carry out the polymerization reaction in an atmosphere of an inert gas such as nitrogen gas.

[0088] In the emulsion polymerization method, a method of emulsion polymerizing the monomer components in an aqueous solvent in the presence of an emulsifier and a polymerization initiator is preferably mentioned. Note that the specific means and conditions for carrying out the emulsion polymerization can be appropriately selected and adopted from means and techniques in conventionally known emulsion polymerization methods.

[0089] The emulsifier used in the emulsion polymerization is not limited, but includes nonionic emulsifiers, anionic emulsifiers, cationic emulsifiers, amphoteric emulsifiers, etc., and conventionally known emulsifiers can be used. These emulsifiers may be used alone or in combination of two or more. Among the emulsifiers, nonionic emulsifiers or anionic emulsifiers are preferred, and anionic emulsifiers are more preferred. Furthermore, an emulsifier containing a polymerizable unsaturated group in the molecule may also be used. Examples of the polymerizable unsaturated group include a group having an ethylenically unsaturated double bond. Incidentally, an emulsifier containing a polymerizable unsaturated group is also referred to as a reactive emulsifier. Furthermore, a polymeric emulsifier can also be used as the emulsifier.

[0090] Examples of the anionic emulsifier include alkyl sulfate salts such as ammonium dodecyl sulfate and sodium dodecyl sulfate; alkyl sulfonate salts such as ammonium dodecyl sulfonate, sodium dodecyl sulfonate and sodium alkyl diphenyl ether disulfonate; alkyl aryl sulfonate salts such as ammonium dodecyl benzene sulfonate, sodium dodecyl benzene sulfonate and sodium dodecyl naphthalene sulfonate; polyoxyethylene alkyl sulfonate salts; polyoxyethylene alkyl ether sulfate salts; polyoxyethylene alkyl aryl ether sulfate salts; polyoxyethylene polycyclic phenyl ether sulfate ester salts; dialkyl sulfosuccinate salts; arylsulfonic acid-formalin condensates; fatty acid salts such as ammonium laurate and sodium stearylate; sulfates or salts thereof having an allyl group such as bis(polyoxyethylene polycyclic phenyl ether) methacrylate sulfonate salts, propenyl-alkyl sulfosuccinate ester salts, (meth)acrylic acid polyoxyethylene sulfonate salts, (meth)acrylic acid polyoxyethylene phosphonate salts, and sulfonate salts of allyloxymethyl alkyloxy polyoxyethylene; sulfate ester salts of allyloxymethyl alkoxyethyl polyoxyethylene, and polyoxyalkylene alkenyl ether ammonium sulfate salts.

[0091] Examples of nonionic emulsifiers include polyoxyethylene alkyl ethers, polyoxyethylene alkylaryl ethers, condensates of polyethylene glycol and polypropylene glycol, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, fatty acid monoglycerides, condensates of ethylene oxide and aliphatic amines, and polyoxyalkylene alkenyl ethers.

[0092] Examples of polymer emulsifiers include poly(meth)acrylates such as sodium polyacrylate; polyvinyl alcohol; polyvinylpyrrolidone; polyhydroxyalkyl(meth)acrylates such as polyhydroxyethyl acrylate; and copolymers containing one or more of the monomers constituting these polymers as copolymerization components.

[0093] Examples of reactive emulsifiers include propenyl-alkyl sulfosuccinate salts, (meth)acrylic acid polyoxyethylene sulfonate salts, (meth)acrylic acid polyoxyethylene phosphonate salts (e.g., Sanyo Chemical Industries, Ltd., trade name: Eleminol RS-30, etc.), polyoxyethylene alkylpropenylphenyl ether sulfonate salts (e.g., Dai-ichi Kogyo Seiyaku Co., Ltd., trade name: Aqualon HS-10, etc.), allyloxymethyl alkyloxy polyoxyethylene sulfonate salts (e.g., Dai-ichi Kogyo Seiyaku Co., Ltd., trade name: Aqualon KH-10, etc.), and polyoxyethylene styrenated propenyl phenyl ether sulfate ammonium esters. anionic emulsifiers having a polymerizable unsaturated group, such as hydroxypropyl methyl acrylate (e.g., trade name: Aqualon AR-10, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), sulfonate salts of allyloxymethyl nonylphenoxyethyl hydroxypolyoxyethylene (e.g., trade name: Adeka Reasop SE-10, manufactured by ADEKA Corporation), allyloxymethyl alkoxyethyl hydroxypolyoxyethylene sulfate ester salts (e.g., trade name: Adeka Reasop SR-10, SR-30, manufactured by ADEKA Corporation), and bis(polyoxyethylene polycyclic phenyl ether) methacrylated sulfonate salts (e.g., trade name: Antox MS-60, manufactured by Nippon Nyukazai Co., Ltd.); nonionic emulsifiers having a polymerizable unsaturated group, such as polyoxyethylene styrenated propenyl phenyl ether (for example, trade name: Aqualon AN-10, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), allyloxymethyl alkoxyethyl hydroxypolyoxyethylene (for example, trade name: Adeka Reasop ER-20, manufactured by ADEKA Corporation), polyoxyethylene alkylpropenyl phenyl ether (for example, trade name: Aqualon RN-20, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.), and allyloxymethyl nonylphenoxyethyl hydroxypolyoxyethylene (for example, trade name: Adeka Reasop NE-10, manufactured by ADEKA Corporation); and the like.

[0094] The amount of the emulsifier used is not limited, but is, for example, preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 5 parts by mass, relative to 100 parts by mass of the monomer component. If necessary, protective colloids can also be used alone or together with the emulsifier.

[0095] The polymerization initiator used in carrying out the emulsion polymerization is not limited, but examples thereof include azo-based polymerization initiators such as azobisisobutyronitrile, 2,2-azobis(2-methylbutyronitrile), 2,2-azobis(2,4-dimethylvaleronitrile), 2,2-azobis(2-diaminopropane) hydrochloride, 4,4-azobis(4-cyanovaleric acid), and 2,2-azobis(2-methylpropionamidine); persulfates such as ammonium persulfate and potassium persulfate; and peroxide-based polymerization initiators such as hydrogen peroxide, benzoyl peroxide, parachlorobenzoyl peroxide, lauroyl peroxide, and ammonium peroxide. These polymerization initiators may be used alone, or two or more types may be used in combination.

[0096] The amount of the polymerization initiator used in the emulsion polymerization is preferably 0.01 to 3 parts by mass, more preferably 0.05 to 2 parts by mass, and even more preferably 0.1 to 1 part by mass, per 100 parts by mass of the monomer components. When a peroxide-based polymerization initiator is used as the polymerization initiator, if it is necessary to increase the polymerization rate or lower the reaction temperature, a reducing agent such as a soluble sulfite or ascorbic acid, or a metal compound that generates heavy metal ions in water, such as ferrous sulfate, can be combined with the polymerization initiator to form a redox-based initiator.

[0097] The reaction temperature during the emulsion polymerization can be appropriately set taking into consideration the weight-average molecular weight of the resulting polymer, the blending ratio of the monomer components, the type of polymerization initiator, and the like. The reaction temperature is, for example, 0 to 100°C, preferably 50 to 95°C, and more preferably 60 to 90°C, and the reaction time is, for example, 0.5 to 30 hours, preferably 1 to 20 hours, and more preferably 3 to 10 hours. The reaction pressure is also not particularly limited and may be normal pressure (atmospheric pressure), reduced pressure, or increased pressure. The polymerization reaction is desirably carried out under an atmosphere of an inert gas such as nitrogen gas.

[0098] Examples of aqueous solvents used in the emulsion polymerization include water and mixed solvents of water and water-soluble organic solvents. Examples of water that can be used include tap water, ion-exchanged water (deionized water), distilled water, and pure water. The water content in the aqueous solvent is preferably 10 to 100% by mass, more preferably 25% by mass or more, even more preferably 60% by mass or more, and particularly preferably 90% by mass or more. The remainder is preferably a water-soluble organic solvent. In this specification, a water-soluble organic solvent refers to an organic solvent that dissolves in water at a concentration of 0.01% by mass or more at 25°C and 1 atmosphere.

[0099] Examples of the water-soluble organic solvent include: lower alcohols having 1 to 4 carbon atoms, such as methyl alcohol, ethyl alcohol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, and tert-butyl alcohol; glycols, such as propylene glycol, 1,3-propanediol, glycerin, dipropylene glycol, tripropylene glycol, diethylene glycol, triethylene glycol, and tetraethylene glycol; monoalkyl ethers of monoethylene glycol, such as monoethylene glycol monomethyl ether, monoethylene glycol monoethyl ether, monoethylene glycol monopropyl ether, monoethylene glycol monoisopropyl ether, monoethylene glycol monobutyl ether, and monoethylene glycol monoisobutyl ether; monoalkyl ethers of monopropylene glycol, such as monopropylene glycol monomethyl ether, monopropylene glycol monoethyl ether, monopropylene glycol monopropyl ether, monopropylene glycol monoisopropyl ether, monopropylene glycol monobutyl ether, and monopropylene glycol monoisobutyl ether; Monoalkyl ethers of diethylene glycol, such as diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, and diethylene glycol monoisobutyl ether; monoalkyl ethers of dipropylene glycol, such as dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoisopropyl ether, dipropylene glycol monobutyl ether, and dipropylene glycol monoisobutyl ether;monoalkyl ethers of polyethylene glycol, such as monomethyl ether of polyethylene glycol (number of moles of added EO=2 to 10, preferably 2 to 4), monoethyl ether of polyethylene glycol (number of moles of added EO=2 to 10, preferably 2 to 4), monopropyl ether of polyethylene glycol (number of moles of added EO=2 to 10, preferably 2 to 4), monoisopropyl ether of polyethylene glycol (number of moles of added EO=2 to 10, preferably 2 to 4), monobutyl ether of polyethylene glycol (number of moles of added EO=2 to 10, preferably 2 to 4), and monoisobutyl ether of polyethylene glycol (number of moles of added EO=2 to 10, preferably 2 to 4); Monoalkyl ethers of polypropylene glycol such as monomethyl ether of polypropylene glycol (number of moles of PO added=2 to 10, preferably 2 to 4), monoethyl ether of polypropylene glycol (number of moles of PO added=2 to 10, preferably 2 to 4), monopropyl ether of polypropylene glycol (number of moles of PO added=2 to 10, preferably 2 to 4), monoisopropyl ether of polypropylene glycol (number of moles of PO added=2 to 10, preferably 2 to 4), monobutyl ether of polypropylene glycol (number of moles of PO added=2 to 10, preferably 2 to 4), and monoisobutyl ether of polypropylene glycol (number of moles of PO added=2 to 10, preferably 2 to 4); heterocyclic rings such as 2-pyrrolidone and N-methyl-2-pyrrolidone; ketones having 1 to 6 carbon atoms such as acetone and methyl ethyl ketone;

[0100] These water-soluble organic solvents may be used alone or in combination of two or more kinds.

[0101] Among these, propylene glycol, glycerin, diethylene glycol, triethylene glycol, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monoisobutyl ether, monobutyl ether of polyethylene glycol (number of moles of EO added=2 to 4), and 2-pyrrolidone are preferred, and propylene glycol, triethylene glycol, monobutyl ether of polyethylene glycol (number of moles of EO added=2 to 4), and 2-pyrrolidone are more preferred.

[0102] The amount of the aqueous solvent used in carrying out the emulsion polymerization is not limited, but is preferably 20 to 300 parts by mass, more preferably 30 to 200 parts by mass, and even more preferably 40 to 150 parts by mass, per 100 parts by mass of the monomer components.

[0103] Specific examples of the emulsion polymerization include monomer dropping polymerization, pre-emulsion dropping polymerization, seed polymerization, and multi-stage polymerization.

[0104] In the reaction system of the solution polymerization or emulsion polymerization, additives such as chain transfer agents, e.g., compounds having a thiol group, e.g., tert-dodecyl mercaptan, n-dodecyl mercaptan, pH buffers, chelating agents, etc., may be added in appropriate amounts as needed. The amount of the additive varies depending on the type and cannot be determined in general, but is usually preferably 0.01 to 5 parts by mass, more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the monomer components.

[0105] [Resin composition for sintered binder] The resin composition of the present invention contains the polymer, and is suitably used as a resin composition for sintered binder. A method of using the resin composition as a sintered binder is also included in the present invention.

[0106] The content of the polymer in the resin composition for a sintered binder is not particularly limited, but when the amount of solid content (non-volatile content) in the resin composition for a sintered binder is taken as 100% by mass, it is, for example, 60% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more, or may be 100% by mass or less or 99.5% by mass or less. In this specification, the solid content (non-volatile content) refers to components excluding the solvent.

[0107] The nonvolatile content can be calculated by a known method. It may be calculated according to the following formula 1 as the mass of the resin composition for a calcined binder minus the mass of volatile components contained in the polymer and various additives from the resin composition for a calcined binder. Alternatively, it may be calculated according to the following formula 2 by weighing 1 g of the resin composition for a calcined binder and drying it in a hot air dryer at a temperature of 150°C for 15 minutes, and using the resulting residue as the nonvolatile content. Formula 1: [Amount of nonvolatile content (mass %) in the resin composition for a calcined binder] = ([Total mass of the resin composition for a calcined binder - Mass of volatile components] / [Total mass of the resin composition for a calcined binder]) x 100 Formula 2: [Amount of nonvolatile content (mass %) in the resin composition for a calcined binder] = ([Mass of residue] / [Mass of 1 g of the resin composition for a calcined binder]) x 100

[0108] The resin composition for a sintered binder of the present invention preferably further contains a solvent. The solvent acts as a diluent that adjusts the viscosity of the resin composition for a sintered binder and improves its handleability. An organic solvent or an aqueous solvent can be suitably used as the solvent. Hereinafter, a resin composition for a sintered binder containing an organic solvent as the main component may be referred to as a "solvent-based resin composition," and a resin composition for a sintered binder containing an aqueous solvent as the main component may be referred to as an "aqueous resin composition." The content of the organic solvent in the solvent contained in the solvent-based resin composition is preferably 70% by mass or more, more preferably 85% by mass or more, even more preferably 95 or 98% by mass or more, and may even be 100% by mass. The content of the aqueous solvent in the solvent contained in the aqueous resin composition is preferably 70% by mass or more, more preferably 85% by mass or more, even more preferably 95 or 98% by mass or more, and may even be 100% by mass.

[0109] Examples of the organic solvent include the same organic solvents as those described as solvents used in solution polymerization and the same water-soluble organic solvents as those described as solvents used in emulsion polymerization. One or more of the organic solvents may be used. Examples of the aqueous solvent include the same aqueous solvents as those described as solvents used in emulsion polymerization. One or more of the aqueous solvents may be used.

[0110] The organic solvent may be a solvent derived from the organic solvent used in solution polymerization, or may be a solvent added separately to the reaction solution of solution polymerization or the isolated polymer, and the aqueous solvent may be a solvent derived from the aqueous solvent used in emulsion polymerization, or may be a solvent added separately to the reaction solution of emulsion polymerization or the isolated polymer.

[0111] When the resin composition for a baked binder of the present invention is an aqueous resin composition, it may be a resin emulsion in which the polymer is dispersed in an aqueous solvent as emulsion particles. The shape of the emulsion particles is not particularly limited, but they are typically spherical. The shape can be measured using a transmission electron microscope or a scanning electron microscope. The emulsion particles may have a single-layer structure or a multi-layer structure (e.g., a core-shell structure). The average particle size of the emulsion particles is preferably 20 to 500 nm, more preferably 50 to 400 nm, and even more preferably 100 to 300 nm. The average particle size of the emulsion particles may be determined by the cumulant average particle size measured by dynamic light scattering.

[0112] The content of the solvent in the resin composition for a sintered binder is, for example, 10 to 95% by mass, preferably 30 to 80% by mass, and more preferably 50 to 70% by mass. In other words, the solid content of the resin composition for a sintered binder is, for example, 5 to 90% by mass, preferably 20 to 70% by mass, and more preferably 30 to 50% by mass.

[0113] The resin composition for a sintered binder of the present invention may further contain binder components other than the polymer (hereinafter, sometimes referred to as "other binder components"), such as cellulose, polyvinyl alcohol, polyvinyl butyral, polyethylene glycol, (meth)acrylic resin, etc. The content of the other binder components is, for example, 1 to 80 parts by mass, preferably 50 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 10 parts by mass or less, and particularly preferably 5 parts by mass or less, relative to 100 parts by mass of the polymer.

[0114] The resin composition for a fired binder of the present invention may further contain, if desired, one or more of various conventionally known additives, such as a dispersant (deflocculating agent), a viscosity modifier, a surfactant, a wetting agent, a thickener, a pH adjuster, a stabilizer, a polymerization initiator, a polymerization inhibitor, a leveling agent, a preservative, or an anti-mold agent.

[0115] The content of the additive varies depending on the type thereof and cannot be determined in general; however, it may be, for example, 0 to 20 parts by mass or 0.001 to 20 parts by mass relative to 100 parts by mass of the polymer, and is preferably 10 parts by mass or less, and more preferably 5 parts by mass or less.

[0116] [Physical Properties of Resin Composition for Sintered Binder] The resin composition for a sintered binder of the present invention can be sintered at low temperatures. For example, the weight loss rate of the solid content of the resin composition for a sintered binder at 350°C is preferably 60% or more, more preferably 80% or more, even more preferably 90% or more, particularly preferably 95% or more, and may be 100% or less. Furthermore, the weight loss rate of the solid content of the resin composition for a sintered binder at 400°C is preferably 95% or more, more preferably 99% or more, and even more preferably 100%. The weight loss rate of the solid content of the resin composition for a sintered binder can be measured by heating and drying the resin composition for a sintered binder at 150°C for 15 minutes to remove the solvent, preparing a sample, and then using a differential thermobalance to continuously measure the weight of the sample in an air atmosphere, increasing the temperature from room temperature to 500°C at a heating rate of 10°C / min.

[0117] The difference (ba) between the temperature a at which the weight loss rate of the solid content of the resin composition for baked binder is 5% and the temperature b at which the weight loss rate of the solid content of the resin composition is 90% is preferably 200°C or less, more preferably 180°C or less, even more preferably 150°C or less, and particularly preferably 120°C or less. A value of b-a in the above range means that the thermal decomposition rate is fast, which is preferable from the viewpoint of energy saving because it shortens the baking time. The lower limit of the value of b-a is not particularly limited, but from the viewpoint of suppressing the occurrence of cracks and fractures caused by excessively rapid decomposition, it may be, for example, 20°C or higher, preferably 40°C or higher. That is, the value of b-a is preferably 20 to 200°C, more preferably 40 to 180°C, even more preferably 40 to 150°C, and particularly preferably 40 to 120°C.

[0118] [Slurry] The present invention also includes a slurry containing the resin composition for a sintered binder and an inorganic powder. The resin composition for a sintered binder contained in the slurry of the present invention is as described above, and preferred embodiments are also the same.

[0119] The total content of the inorganic powder and the polymer contained in the resin composition for a calcined binder is not particularly limited, but is, for example, 60% by mass or more, preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 95% by mass or more, when the amount of solids (non-volatile content) in the slurry is taken as 100% by mass. It may also be 100% by mass or 99.5% by mass or less. Furthermore, in the slurry of the present invention, the content ratio of the resin composition for a calcined binder and the inorganic powder is not particularly limited, but the content ratio of the resin composition for a calcined binder and the inorganic powder may be adjusted so that the polymer is, for example, 1 to 100 parts by mass, preferably 5 to 50 parts by mass, and more preferably 10 to 30 parts by mass, per 100 parts by mass of the inorganic powder.

[0120] The inorganic powder is not particularly limited, and examples thereof include metal oxides, inorganic salts (metal carbonates, metal sulfates, metal silicates, metal phosphates, metal titanates, metal borates, etc.), metal nitrides, etc. The inorganic powders may be used alone or in combination of two or more.

[0121] Examples of metal oxides include diatomaceous earth, alumina, zinc oxide, titania, zirconia, calcium oxide, magnesium oxide, iron oxide, copper oxide, tin oxide, chromium oxide, antimony oxide, yttrium oxide, cerium oxide, samarium oxide, lanthanum oxide, tantalum oxide, terbium oxide, europium oxide, neodymium oxide, ferrites, lanthanum lithium zirconate (LLZ)-based materials, and lithium titanium aluminum phosphate (LATP)-based materials.

[0122] Examples of metal carbonates include heavy calcium carbonate, light calcium carbonate, zinc carbonate, barium carbonate, dawsonite, and hydrotaluisite. Examples of metal sulfates include calcium sulfate, barium sulfate, and gypsum fiber. Examples of metal silicates include silica, calcium silicate (wollastonite, xonotlite, and the like), kaolin, clay, talc, mica, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, and glass flakes. Examples of metal phosphates include tricalcium phosphate. Examples of metal titanates include potassium titanate, calcium titanate, magnesium titanate, barium titanate, and lead zirconate titanate. Examples of metal borates include zinc borate and aluminum borate.

[0123] Examples of metal nitrides include aluminum nitride, titanium nitride, boron nitride, and silicon nitride.

[0124] The volume average primary particle size of the inorganic powder is preferably 0.01 to 10 μm, more preferably 0.05 to 1 μm, and even more preferably 0.05 to 0.5 μm.

[0125] The inorganic powder can be used as a ceramic powder. The metal element contained in the ceramic powder is not particularly limited, but preferably includes Group 4 elements such as titanium (Ti), zirconium (Zr), and hafnium (Hf), Group 5 elements such as vanadium (V), niobium (Nb), and tantalum (Ta), and Group 6 elements such as chromium (Cr), Mo (molybdenum), and tungsten (W). From the viewpoint of increasing the dispersibility of the ceramic powder in the ceramic molding material, titanium and / or zirconium are preferred.

[0126] The slurry of the present invention preferably further contains a solvent. The solvent may be a solvent derived from the resin composition for the calcined binder, a solvent added separately from the resin composition for the calcined binder (hereinafter sometimes referred to as a separate solvent), or a mixed solvent thereof. When the resin composition for the calcined binder contains a solvent, some or all of the solvent contained in the resin composition for the calcined binder may be removed and then mixed with the separate solvent. Examples of the separate solvent include the same solvents as those in the resin composition for the calcined binder. Among them, lower alcohols, aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, aliphatic ester solvents, ketone solvents, and (poly)alkylene glycol monoalkyl ether acetate solvents are preferred, and lower alcohols and aromatic hydrocarbon solvents are more preferred. In the slurry of the present invention, solvents can be used alone or in combination of two or more.

[0127] The solvent content of the slurry (100% by mass) is, for example, 5 to 90% by mass, preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and even more preferably 30 to 70% by mass. By adjusting the solvent content within the above range, the viscosity of the slurry can be maintained appropriately while shortening the drying time of the solvent and reducing the amount of heat required for drying when producing a green molding material such as a green sheet. Furthermore, from the perspective of the environmental impact and working environment when producing a green molding material such as a green sheet, the solvent content of the slurry (100% by mass) is, for example, 3 to 50% by mass, preferably 3 to 40% by mass, more preferably 3 to 30% by mass, even more preferably 3 to 20% by mass, and particularly preferably 3 to 15% by mass.

[0128] The slurry of the present invention may further contain, if desired, one or more of various conventionally known additives, such as binder components other than the polymers described above, such as polyvinyl alcohol, polyvinyl butyral, polyethylene glycol, and (meth)acrylic resins, dispersants (deflocculants), viscosity modifiers, film-forming aids, wetting agents, thickeners, pH adjusters, stabilizers, ultraviolet absorbers, ultraviolet stabilizers, polymerization inhibitors, leveling agents, rheology modifiers, surfactants, adhesion promoters, fillers, thixotropic agents, plasticizers, antioxidants, antistatic agents, lubricants, opacifiers, antifoaming agents, polymerization initiators, dyes, and pigments.

[0129] The slurry can be obtained by mixing the resin composition for a sintered binder, inorganic powder, and a solvent and other additives that are used as needed.

[0130] [Green Material] The slurry can be formed into a desired shape and dried as needed to produce a green material. For example, a green sheet can be produced by forming it into a sheet, but the shape of the green material is not limited to a sheet and can be any shape depending on the intended use. The drying temperature is not particularly limited, but is, for example, 10 to 200°C, preferably 20 to 150°C.

[0131] The green molding material (preferably a green sheet) may be further subjected to shaping such as lamination, crimping, cutting, etc., as required. Furthermore, the green molding material (preferably a green sheet) may be, for example, subjected to conductor pattern printing before shaping.

[0132] [Inorganic particle molded body] By firing the green molding material to remove organic components (e.g., the polymer), etc., an inorganic particle molded body such as a ceramic molded body can be produced. As described above, the resin composition for a fired binder of the present invention can be fired at low temperatures and leaves little residue when fired at low temperatures, so it is useful for low-temperature firing of, for example, glass ceramic substrates for integrated circuits, glass substrates for plasma displays, photodegradable titanium oxide-containing tapes, etc.

[0133] This application claims the benefit of priority based on Japanese Patent Application No. 2023-072360, filed on April 26, 2023. The entire contents of the specification of Japanese Patent Application No. 2023-072360, filed on April 26, 2023, are incorporated herein by reference.

[0134] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass." In the following examples and comparative examples, various physical properties were evaluated as follows.

[0135] [Method for measuring nonvolatile content (N.V.)] 1 g of the composition was weighed and dried in a hot air dryer at 150°C for 15 minutes, and the resulting dry residue was taken as the nonvolatile content, which was calculated based on the following formula: [Amount of nonvolatile content in composition (%)] = ([mass of residue] / [mass of composition 1 g]) × 100.

[0136] [Method for calculating glass transition temperature] Tg calculated from the Fox equation shown in the following formula (1) A The glass transition temperature (calculated Tg) of the polymer was calculated by converting the temperature (K) to degrees Celsius (°C). [In formula (1), Tg A : Tg (K) of polymer, Tg n : Tg (K), W of the homopolymer of each monomer usedn : Mixing ratio of each monomer used (mass%)]

[0137] [Method for Measuring Thermal Decomposition Behavior] The (meth)acrylic polymer compositions prepared in the examples were heated and dried in an oven at 150°C for 15 minutes, and the binders obtained by volatilizing the solvent, as well as the binders of the comparative examples, were used as samples to measure the thermal decomposition behavior of each binder by the following method. Using a differential thermobalance (Rigaku Corporation, ThermoPlus2 TG-8120), a thermal decomposition test was conducted in which approximately 10 mg of a sample placed in an aluminum pan was heated from room temperature to 500°C at a heating rate of 10°C / min in an air atmosphere while continuously measuring the sample's weight, and then held at 500°C for 10 minutes. The weight loss rates were measured at 250°C, 300°C, 350°C, 400°C, and 450°C.

[0138] [Evaluation of low-temperature decomposition property] The low-temperature decomposition property of the binder was evaluated based on the weight loss rate at 400°C according to the following criteria: [Evaluation criteria] ◯: Weight loss rate of 99% or more △: Weight loss rate of 95% or more but less than 99% ×: Weight loss rate less than 95%

[0139] [Evaluation of thermal decomposition rate] In the measurement of the thermal decomposition behavior, the temperature a at which the weight loss rate was 5% and the temperature b at which the weight loss rate was 90% were determined. In addition, the difference between the temperatures b and a (ba) was calculated. The smaller the value of b-a, the faster the thermal decomposition rate.

[0140] [Evaluation of Aluminum Pan Residue] After the thermal decomposition test in the measurement of thermal decomposition behavior was completed, the residue on the aluminum pan was evaluated based on the following criteria. [Evaluation criteria] ◯: No residue remains ×: Residue remains

[0141] [Method for Evaluating Slurry Dispersibility] As in the "Method for Measuring Thermal Decomposition Behavior," binder samples of each Example and Comparative Example were prepared, and 0.5 g of each sample was weighed into a plastic container. 1.0 g of a mixed solution of toluene / ethanol = 1 / 1 (mass ratio) was added thereto and stirred with a stirring rod to obtain each binder solution. 8.5 g of barium titanate (product name: BT-03, manufactured by Sakai Chemical Industry Co., Ltd.) was added to 1.5 g of each binder solution, and the slurry dispersibility was evaluated by stirring with a stirring rod at room temperature. [Evaluation Criteria] ◎: Uniformly mixed within a few minutes of stirring, becoming a paste-like substance with high fluidity. 〇: Uniformly mixed within a few minutes of stirring, but poor fluidity (forming lumps). ×: Not uniformly mixed even when stirred, separating into powder and lumps, with some remaining as powder.

[0142] Example 1 A reaction vessel equipped with a condenser, a nitrogen gas inlet pipe, a thermometer, a dropping funnel, and a stirrer was charged with 150 parts of ethyl acetate and 100.0 parts of 2-octyl methacrylate (2-octyl methacrylate, Tg of homopolymer: -25°C). Then, 0.1 parts of an azo polymerization initiator (manufactured by Nippon Finechem Co., Ltd., product name: ABN-E) was added to the reaction vessel, and the mixture was reacted in a nitrogen gas atmosphere at 80°C for 6 hours to obtain a (meth)acrylic polymer composition with a nonvolatile content of 40%.

[0143] [Example 2] A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate was changed to the composition shown in Table 1. The evaluation result of the slurry dispersibility was ◯.

[0144] Example 3 A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate was changed to the composition shown in Table 1. The evaluation result of the slurry dispersibility was ⊚.

[0145] Example 4 A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate was changed to the composition shown in Table 1. The evaluation result of the slurry dispersibility was ◯.

[0146] Example 5 A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate in Example 1 was changed to the composition shown in Table 1 and 150 parts of ethyl acetate was changed to a mixed solvent of 100 parts of ethyl acetate and 50 parts of toluene. The evaluation result of the slurry dispersibility was ⊚.

[0147] [Example 6] A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate was changed to the composition shown in Table 1. The evaluation result of the slurry dispersibility was ◯.

[0148] Example 7 A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate was changed to the composition shown in Table 1 and 0.1 parts of n-dodecyl mercaptan was added per 100 parts of the total monomers at the start of polymerization. The evaluation result of the slurry dispersibility was ⊚.

[0149] Example 8 A (meth)acrylic polymer composition having a nonvolatile content of 40% was obtained by the same procedure as in Example 1, except that 100.0 parts of 2-octyl methacrylate was changed to the composition shown in Table 1. The evaluation result of the slurry dispersibility was ◯.

[0150] Comparative Example 1 A commercially available binder, polyvinyl butyral (product name: S-LEC BL-2H, manufactured by Sekisui Chemical Co., Ltd.), was used. The evaluation result of the slurry dispersibility was x.

[0151] Comparative Example 2 A commercially available binder, high molecular weight polycarboxylic acid (trade name: Marialim AKM-0531, manufactured by NOF Corporation), was used. The evaluation result of the slurry dispersibility was ◯.

[0152]

[0153] The abbreviations in Table 1 have the following meanings: 2OMA: 2-octyl methacrylate 2EHA: 2-ethylhexyl acrylate HPA: 2-hydroxypropyl acrylate AA: acrylic acid IBOA: isobornyl acrylate IBOMA: isobornyl methacrylate EMA: ethyl methacrylate HEMA: 2-hydroxyethyl methacrylate MMA: methyl methacrylate nBMA: normal butyl methacrylate DMMA: dimethylaminoethyl methacrylate iBMA: isobutyl methacrylate EtOAc: ethyl acetate Tol: toluene

[0154] From the above results, the compositions of the examples containing the polymer having a structural unit derived from the compound represented by formula (a1) have better thermal decomposition properties at low temperatures than the binders of the comparative examples, and can reduce the residue after firing at low temperatures. Furthermore, the compositions of the examples containing the polymer have a faster thermal decomposition rate than the comparative examples, i.e., can shorten the firing time.

Claims

1. A resin composition for a sintered binder, comprising a polymer having a structural unit derived from a compound represented by formula (a1). [In formula (a1), R a1 represents a hydrogen atom or a methyl group. a2 and R a3 represents a linear or branched alkyl group; R a2 and R a3 The total number of carbon atoms in the alkyl groups of R is 2 to 20, and a2 The number of carbon atoms in R a3 The number of carbon atoms is as follows.

2. The resin composition according to claim 1, wherein the compound represented by formula (a1) is a compound whose homopolymer has a glass transition temperature of 0° C. or lower.

3. The resin composition according to claim 1, wherein the compound represented by formula (a1) is 2-octyl (meth)acrylate.

4. The resin composition according to claim 1, wherein, when heated at a rate of 10°C / min, the difference (b-a) between the temperature a at which the weight loss rate of the solid content of the resin composition is 5% and the temperature b at which the weight loss rate of the solid content of the resin composition is 90% is 200°C or less.

5. A slurry comprising the resin composition according to any one of claims 1 to 4 and an inorganic powder.

6. A green sheet formed from the slurry of claim 5.

7. A method of using a resin composition containing a polymer having a structural unit derived from a compound represented by formula (a1) as a sintered binder. [In formula (a1), R a1 represents a hydrogen atom or a methyl group. a2 and R a3 represents a linear or branched alkyl group; R a2 and R a3 The total number of carbon atoms in the alkyl groups of R is 2 to 20, and a2 The number of carbon atoms in R a3 The number of carbon atoms is as follows.

Citation Information

Patent Citations

  • Green sheet

    JP1994080465A

  • Aluminum nitride green sheet

    JP1995089768A

  • Aluminum nitride green sheet

    JP1995144970A

  • Particulate pressure-sensitive adhesive composition

    JP2014077141A