Block copolymer, block copolymer modified silicon dioxide nano-particles as well as preparation method and application of block copolymer modified silicon dioxide nano-particles

Through the addition reaction of block copolymer and amino surface modified silica nanoparticles, block copolymer modified silica nanoparticles with amphipathicity and stability are formed, and nanosilicon dioxide in low-permeability oil reservoir is solved. The problem of low recovery rate has achieved a reduction in oil-water interface tension and an improvement in recovery rate.

CN118930768AActive Publication Date: 2024-11-12DAQING OILFIELD CO LTD +1

Patent Information

Application Number
CN202310524776.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12
Estimated Expiration
2043-05-10

AI Technical Summary

Technical Problem

Existing nanosilicon dioxide is difficult to accurately regulate hydrophilic and lipophilic properties, and its structure is unstable, resulting in low recovery rate of low permeability reservoirs and insufficient reduction of oil-water interface tension.

Method used

The addition reaction of block copolymer and amino surface modified silica nanoparticles is formed by forming block copolymer modified silica nanoparticles with -NHCONH-linking groups, which have amphiphilicity, stability and solvent responsiveness. , can reduce the oil-water interface tension, realize automatic oil search, capture and expand the volume of oil droplets in the reservoir.

Benefits of technology

It significantly improves the crude oil recovery rate and has a stable structure, which can greatly reduce the oil-water interface tension, improves oil-driving efficiency and emulsifying crude oil capacity, and is suitable for the third oil recovery and chemical recovery rate of low-permeability reservoirs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930768A_ABST
    Figure CN118930768A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of improvement of crude oil recovery in oil fields, and discloses a block copolymer, block copolymer modified silicon dioxide nano-particles and a preparation method and application of the block copolymer modified silicon dioxide nano-particles. The block copolymer contains a structural unit A as shown in a formula I, a structural unit B as shown in a formula II or III and a structural unit C as shown in a formula IV, and R1, R3, R5 and R6 are respectively and independently hydrogen or methyl; r2 is a linear chain or branched chain alkyl group or phenyl group of C1-C12; r4 is a C1-C5 straight chain or branched chain alkylene group; r7 is # imgabs0 # imgabs1 # x, and y and z are integers from 1 to 10. The-NCO contained in the structural unit C of the block copolymer and the amino contained in the surface modified silicon dioxide nanoparticles are subjected to an addition reaction to be connected through-NHCONH-to obtain the block copolymer modified silicon dioxide nanoparticles, and the block copolymer modified silicon dioxide nanoparticles are finally applied to an oil displacement agent. The block copolymer modified silicon dioxide nanoparticles have amphipathicity, stability and solvent responsiveness, and can reduce the oil-water interfacial tension and improve the crude oil recovery rate. # imgabs2 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of improving crude oil recovery in oil fields, and in particular to block copolymers and block copolymer-modified silicon dioxide nanoparticles, and preparation methods and applications thereof. Background Art

[0002] How to effectively improve the recovery rate of low permeability reservoirs and achieve economic and efficient development of low permeability oil fields has become an important direction for domestic and foreign oil field development technology research. Therefore, the existing tertiary oil recovery technology can no longer meet the current situation of increasingly inferior oil and gas resources. It is urgent to develop new technologies to improve recovery rates, rely on technological innovation to solve new problems in the oil field development process, and meet the production and technical needs of oil fields.

[0003] In recent years, theoretical breakthroughs and technological innovations in nanotechnology have provided new ways for the development of new technologies to improve oil recovery, and more and more research teams have applied the surface effects of nanomaterials to the technology of improving oil recovery. Silica nanoparticles have become the first choice of nano oil-displacing materials due to their low cost, environmental protection, good compatibility with formations, high surface activity, high hydroxyl content, and easy surface modification. Among them, most of them adopt the "selective surface modification method" to prepare amphiphilic nano silica particles by modifying the surface of the same nanoparticle. Since hydrophilic and lipophilic modifications are both carried out on the basis of the same silica particle, the two modifications may affect each other, and the hydrophilicity and lipophilicity of silica particles cannot be regulated separately, which will affect the optimization of the amphiphilic performance of silica particles. CN107416844B couples hydrophilic nano silica particles and lipophilic nano silica particles through chemical bonds to obtain double spherical amphiphilic nano silica particles with a particle size of less than 100nm. Although hydrophilicity and lipophilicity can be regulated separately, they are easily blocked when applied to the migration process of porous reservoir media. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems of the prior art that nano-silica is difficult to accurately control the hydrophilic and oleophilic properties, has unstable structure, and does not significantly reduce the oil-water interfacial tension, as well as low recovery rate of low permeability oil reservoirs. A block copolymer and block copolymer modified silica nanoparticles and preparation methods and applications thereof are provided. The block copolymer modified silica nanoparticles are obtained by addition reaction of a block copolymer containing -NCO structural units with amino surface modified silica nanoparticles, the connecting group is -NHCONH-, has amphiphilicity, stability and solvent responsiveness, can reduce the oil-water interfacial tension, has the oil displacement functions of automatically finding oil in the reservoir, capturing and aggregating oil droplets, and intelligently expanding the swept volume along the way, thereby greatly improving the crude oil recovery rate.

[0005] In order to achieve the above object, the first aspect of the present invention provides a block copolymer, wherein the block copolymer comprises a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV,

[0006]

[0007] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are integers from 1-10.

[0008] A second aspect of the present invention provides a method for preparing a block copolymer, wherein the preparation method comprises the following steps:

[0009] (1) in a nitrogen atmosphere and in the presence of a first initiator, a chain transfer agent, and an organic solvent, subjecting the monomer represented by formula (1) and the monomer represented by formula (2) or methacryloyl isocyanate to a first polymerization reaction to obtain a first polymer product;

[0010] (2) in a nitrogen atmosphere and in the presence of a second initiator, subjecting the first polymerization product to a second polymerization reaction with the monomer represented by formula (3) to obtain the block copolymer;

[0011]

[0012] Wherein, R1, R3 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are integers from 1-10.

[0013] The third aspect of the present invention provides a block copolymer modified silica nanoparticle, wherein the modified silica nanoparticle comprises: a core from a surface-modified silica nanoparticle, a coating layer from a block copolymer, and a connecting group connecting the core and the coating layer, wherein the block copolymer comprises a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV;

[0014] Wherein, the connecting group is -NHCONH-, which is obtained by the addition reaction of -NCO contained in the structural unit B with the amino group contained in the surface-modified silica nanoparticles;

[0015]

[0016] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are integers from 1-10.

[0017] A fourth aspect of the present invention provides a method for preparing block copolymer modified silica nanoparticles, wherein the preparation method comprises the following steps:

[0018] The block copolymer is reacted with the silane coupling agent modified silica nanoparticles to obtain the block copolymer modified silica nanoparticles; wherein the block copolymer is the block copolymer mentioned above or the block copolymer prepared by the above preparation method;

[0019] Wherein, the mass ratio of the block copolymer to the silane coupling agent modified silica nanoparticles is 0.3-10:1.

[0020] The fifth aspect of the present invention provides block copolymer-modified silica nanoparticles prepared by the preparation method of the fourth aspect.

[0021] The sixth aspect of the present invention provides the use of the block copolymer modified silica nanoparticles according to the third aspect and / or the fifth aspect in improving crude oil recovery.

[0022] A seventh aspect of the present invention provides an oil displacing agent, wherein the oil displacing agent comprises: 99.5%-99.9% by weight of water and 0.1%-0.5% by weight of the block copolymer modified silica nanoparticles of the third aspect and / or the fifth aspect.

[0023] The eighth aspect of the present invention provides use of the oil displacement agent of the seventh aspect in improving crude oil recovery.

[0024] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:

[0025] (1) The present invention obtains block copolymer-modified silica nanoparticles having a connecting group of -NHCONH- by an addition reaction between a block copolymer containing -NCO structural units and surface-modified silica nanoparticles containing amino groups. The block copolymer-modified silica nanoparticles have a stable structure.

[0026] (2) The block copolymer modified silica nanoparticles prepared by the present invention connect the triblock copolymer having a hydrophilic segment and a lipophilic segment at both ends to the surface of the silica nanoparticles through the middle segment, and have a spontaneous conformational transformation function for water / oil solvents, which can greatly reduce the oil-water interfacial tension, thereby improving the capillary action, improving the oil washing efficiency of the oil displacement system and the ability to emulsify crude oil.

[0027] (3) The oil displacing agent provided by the present invention can further improve the recovery rate on the basis of water flooding, and has great application value in further improving the recovery rate after tertiary oil recovery in low permeability reservoirs and chemical flooding. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is the infrared spectrum (FTIR) of the silicon dioxide nanoparticles before and after the block copolymer modification in Example 1;

[0029] Figure 2 This is the infrared spectrum (FTIR) of the silicon dioxide nanoparticles before and after the block copolymer modification in Comparative Example 1. DETAILED DESCRIPTION

[0030] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0031] The first aspect of the present invention provides a block copolymer, wherein the block copolymer comprises a structural unit A represented by formula I, a structural unit B represented by formula II or III, and a structural unit C represented by formula IV.

[0032]

[0033] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are integers from 1-10.

[0034] In some embodiments, R2 is a C1-C8 straight chain or branched alkyl or phenyl group, preferably a methyl or ethyl group; R4 is a C1-C3 straight chain or branched alkylene group, preferably a methylene or ethylene group; x, y and z are integers of 1-6, and x, y and z are preferably 1 or 2.

[0035] In some embodiments, the molar ratio of the structural unit A, the structural unit B and the structural unit C is 1:0.02-3:0.05-20.

[0036] In some embodiments, the block copolymer has a weight average molecular weight of 15,000-160,000 g / mol, preferably 20,000-60,000 g / mol.

[0037] A second aspect of the present invention provides a method for preparing a block copolymer, wherein the preparation method comprises the following steps:

[0038] (1) in a nitrogen atmosphere and in the presence of a first initiator, a chain transfer agent, and an organic solvent, subjecting the monomer represented by formula (1) and the monomer represented by formula (2) or methacryloyl isocyanate to a first polymerization reaction to obtain a first polymer product;

[0039] (2) in a nitrogen atmosphere and in the presence of a second initiator, subjecting the first polymerization product to a second polymerization reaction with the monomer represented by formula (3) to obtain the block copolymer;

[0040]

[0041] Wherein, R1, R3 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are integers from 1-10.

[0042] In some embodiments, the molar ratio of the monomer represented by formula (1), the monomer represented by formula (2), and the monomer represented by formula (3) is 1:0.05-0.5:0.05-50.

[0043] In some embodiments, in step (1), the conditions of the first polymerization reaction include: reaction temperature of 60-80° C., and reaction time of 3-24 h.

[0044] In some embodiments, the first initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.

[0045] In some embodiments, the chain transfer agent is benzyl dithiobenzoate or cumyl dithiobenzoate.

[0046] In some embodiments, R2 is a C1-C8 straight chain or branched alkyl or phenyl group, preferably a methyl or ethyl group; R4 is a C1-C3 straight chain or branched alkylene group, preferably a methyl or ethyl group; x, y and z are integers of 1-6, and x, y and z are preferably 1 or 2.

[0047] In some embodiments, the monomer represented by formula (1) is selected from methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-ethylhexyl acrylate or styrene.

[0048] In some embodiments, the monomer represented by formula (2) is isocyanoethyl methacrylate or isocyanoethyl acrylate.

[0049] In some embodiments, the monomer represented by formula (3) is selected from methoxyethyl methacrylate, dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, 4-hydroxybutyl 2-methacrylate, 4-hydroxybutyl acrylate or 2-methoxyethyl 2-acrylate.

[0050] In some embodiments, the organic solvent is benzene.

[0051] In some embodiments, the molar ratio of the initiator, the chain transfer agent and the monomer represented by formula (1) is 1:1-5:50-500.

[0052] In some embodiments, the volume ratio of the monomer represented by formula (1) to the monomer represented by formula (2) is 1:0.06-0.46.

[0053] In some embodiments, step (1) further comprises: dissolving the first polymerization product in tetrahydrofuran, adding the first precipitant to precipitate, repeating 3-6 times, filtering and drying at 30-50° C. for 36-48 hours.

[0054] In some embodiments, the first precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:1-4.

[0055] In some embodiments, in step (2), the conditions of the second polymerization reaction include: reaction temperature of 60-80° C., and reaction time of 5-24 h.

[0056] In some embodiments, the second initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate.

[0057] In some embodiments, the molar ratio of the first polymer product, the monomer of formula (3), and the second initiator is 1:10-1000:0.5-1.0.

[0058] In some embodiments, step (2) further comprises: dissolving the block copolymer in tetrahydrofuran, adding the block copolymer into a second precipitant for precipitation, repeating the process 3-6 times, filtering and drying at 30-50° C. for 36-48 hours.

[0059] In some embodiments, the second precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:5-10.

[0060] The third aspect of the present invention provides a block copolymer modified silica nanoparticle, wherein the modified silica nanoparticle comprises: a core from a surface-modified silica nanoparticle, a coating layer from a block copolymer, and a connecting group connecting the core and the coating layer, wherein the block copolymer comprises a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV;

[0061] Wherein, the connecting group is -NHCONH-, which is obtained by the addition reaction of -NCO contained in the structural unit B with the amino group contained in the surface-modified silica nanoparticles;

[0062]

[0063] Wherein, R1, R3, R5 and R6 are each independently hydrogen or methyl; R2 is C1-C 12 R4 is a C1-C5 straight chain or branched chain alkylene; R7 is x, y and z are integers from 1-10.

[0064] In some embodiments, R2 is a C1-C8 straight chain or branched alkyl or phenyl group, preferably a methyl or ethyl group; R4 is a C1-C3 straight chain or branched alkylene group, preferably a methylene or ethylene group; x, y and z are integers of 1-6, and x, y and z are preferably 1 or 2.

[0065] In some embodiments, the molar ratio of the structural unit A, the structural unit B and the structural unit C is 1:0.02-0.3:0.05-20.

[0066] In some embodiments, the content of the silica nanoparticles is 15-85 wt %, preferably 35-75 wt %, based on the total weight of the block copolymer-modified silica nanoparticles.

[0067] In some embodiments, the average particle size of the silica nanoparticles is 20-80 nm.

[0068] A fourth aspect of the present invention provides a method for preparing block copolymer modified silica nanoparticles, wherein the preparation method comprises the following steps:

[0069] The block copolymer is reacted with the silane coupling agent modified silica nanoparticles to obtain the block copolymer modified silica nanoparticles; wherein the block copolymer is the block copolymer mentioned above or the block copolymer prepared by the above preparation method;

[0070] Wherein, the mass ratio of the block copolymer to the silane coupling agent modified silica nanoparticles is 0.3-10:1.

[0071] In some embodiments, the reaction conditions include: ultrasonically dispersing the block copolymer and the silane coupling agent modified silica nanoparticles in toluene; reacting at 20-30°C for 4-12 hours using a reflux method; separating the precipitate, washing it, and drying it at 60-100°C for 12-36 hours to obtain block copolymer modified nano silica nanoparticles.

[0072] In some embodiments, the silane coupling agent is selected from 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, anilinemethyltrimethoxysilane or anilinemethyltriethoxysilane.

[0073] In some embodiments, the preparation method of the silane coupling agent modified silica nanoparticles includes: mixing anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate for a first reaction, adding a silane coupling agent for a second reaction for 2-5 hours to obtain the silane coupling agent modified silica nanoparticles.

[0074] In some embodiments, the molar ratio of anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate is 25-80:2-5:0.25-3.9:1; the molar ratio of tetraethyl orthosilicate to silane coupling agent is 1:0.01-0.2.

[0075] In some embodiments, the conditions of the first reaction are: under stirring conditions, the reaction time is 12-24 hours; the reaction temperature is 20-30°C; the conditions of the second reaction are: under stirring conditions, the reaction time is 2-5 hours; the reaction temperature is 60-70°C.

[0076] In some embodiments, the preparation method further comprises: washing the silane coupling agent modified silica nanoparticles in a dispersant, filtering and drying at 70-90° C. for 12-24 hours, and the dispersant is deionized water and / or ethanol.

[0077] The fifth aspect of the present invention provides block copolymer-modified silica nanoparticles prepared by the preparation method of the fourth aspect.

[0078] The sixth aspect of the present invention provides the use of the block copolymer modified silica nanoparticles according to the third aspect and / or the fifth aspect in improving crude oil recovery.

[0079] A seventh aspect of the present invention provides an oil displacing agent, wherein the oil displacing agent comprises: 99.5%-99.9% by weight of water and 0.1%-0.5% by weight of the block copolymer modified silica nanoparticles of the third aspect and / or the fifth aspect.

[0080] Compared with commercially available nano oil-displacing agents, the oil-displacing agent comprising the block copolymer-modified silicon dioxide nanoparticles prepared in the present invention can significantly reduce the oil / water interfacial tension, thereby improving the crude oil recovery rate.

[0081] The eighth aspect of the present invention provides use of the oil displacement agent of the seventh aspect in improving crude oil recovery.

[0082] The present invention will be described in detail below by way of examples, but the protection scope of the present invention is not limited to the following description.

[0083] In the following examples and comparative examples, if no specific conditions are specified, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used, if no manufacturer is specified, are all conventional products that can be obtained through commercial channels.

[0084] Test for reducing water / crude oil interfacial tension performance, test method reference standard SY / T 5370-2018:

[0085] The test oil was a simulated oil prepared from crude oil from a block of Daqing Oilfield and aviation kerosene, and the test water was deep treated sewage from the same block after being filtered through a filter membrane with a pore size of 0.45μm.

[0086] Add a certain mass of the sample to be tested into the on-site water of the corresponding mass concentration, ultrasonically disperse for 30 minutes, and mechanically stir for 30 minutes for standby. The test instrument is a TEXAS-500 rotating drop interfacial tension meter. The main test steps are as follows: start the constant temperature system and control the temperature between 45±0.2℃; fill the measuring tube with the sample of the nano-oil displacement system; use a micro-syringe to draw simulated oil and inject it into the measuring tube to form a suitable droplet, and there must be no bubbles in the measuring tube; start the interfacial tension meter and set the speed at 4500RPM; try to keep the oil drop in the middle position of the capillary during the entire measurement process, and record the experimental data every 15 minutes; the entire measurement time is 2 hours.

[0087] The oil displacement experiment operation method refers to the standard SY / T 6424-2014, and the main steps are as follows:

[0088] 1. Vacuum a square-section 4.5 cm × 4.5 cm × 30 cm Bailey core continuously for more than 4 hours and saturate the core with filtered in-situ water;

[0089] 2. Heat the core to the formation temperature of 45°C, use the prepared simulated oil to drive water, and stop when the water volume in the outlet scale tube no longer changes. Measure the cumulative saturated oil volume to obtain the bound water saturation;

[0090] 3. The core saturated with oil was placed in a 45℃ constant temperature box for aging for 12 hours, and then the saturated oil process was changed to a water flooding process. When the water content reached more than 98% in the continuous water flooding 0.5 times pore volume (0.5PV) stage, the water flooding was stopped;

[0091] 4. Switch to the nano-oil-displacing agent injection process, continuously inject 0.3 PV of the nano-oil-displacing system slug at a rate of 0.3 mL / min, and record the oil and water production at that stage;

[0092] 5. Switch to subsequent water drive until the water content of the produced fluid at the outlet reaches more than 98% for consecutive 0.5PV. Then end the experiment and calculate the stage recovery factor and total recovery factor respectively.

[0093] Example 1

[0094] (1) Preparation of block copolymers

[0095] 0.05 g of azobisisobutyronitrile, 0.1 g of isopropyl dithiobenzoate and 2.0 g of ethyl methacrylate (as shown in formula (1), R1 is methyl and R2 is ethyl) are added to 10 mL of benzene, and the reaction is carried out for 1.5 h at 65° C. under a nitrogen atmosphere; then 1.2 g of isocyanoethyl methacrylate (as shown in formula (2), R3 is methyl and R4 is ethylene) is added, and the reaction is continued for 1.5 h under a nitrogen atmosphere, the product is dissolved and diluted with tetrahydrofuran, and slowly added dropwise to a first precipitant (toluene and petroleum ether in a volume ratio of 1:1) in an ice bath for precipitation, and the reaction is repeated 3 times, and then vacuum dried to obtain a first polymerization product;

[0096] 1.5 g of the first polymerization product and 9.1 g of dimethylaminoethyl acrylate (as shown in formula (3), R6 is hydrogen, R7 is x is 2) and 0.02g of azobisisobutyronitrile are added to 15mL of benzene, and the reaction is carried out for 5h under a nitrogen atmosphere at a temperature of 65°C. The product is dissolved and diluted with tetrahydrofuran, and slowly added dropwise to a second precipitant (toluene and petroleum ether volume ratio of 1:5) in an ice bath for precipitation, and the reaction is repeated 3 times. Then, the block copolymer is obtained, wherein the structural unit A (as shown in Formula I, R1 is methyl and R2 is ethyl), the structural unit B (as shown in Formula II, R3 is methyl and R4 is ethylene) and the structural unit C (as shown in Formula IV, R6 is hydrogen and R7 is The molar ratio of x being 2) is 1:0.29:3.9.

[0097] (2) Preparation of surface-modified silica nanoparticles

[0098] 200 g of ethanol, 5 g of deionized water and 10 g of ammonia water (25 wt%) were mixed, stirred for 15 min, and then 15 g of tetraethyl orthosilicate was added, and the mixture was stirred and reacted at room temperature for 12 h; the temperature was raised to 65° C., 1 g of 3-aminopropyltriethoxysilane was added dropwise, and the mixture was stirred and reacted for 2 h; the solid product was collected by centrifugation, dispersed and washed with ethanol and deionized water for 3 times, and vacuum dried at 80° C. for 12 h to obtain surface-modified silica nanoparticles.

[0099] (3) Preparation of block copolymer modified silica nanoparticles

[0100] 1.5 g of block copolymer and 0.5 g of surface-modified silica nanoparticles were ultrasonically dispersed in 20 mL of tetrahydrofuran solvent and refluxed at room temperature for 4 h. The solid product was separated by centrifugation, washed with tetrahydrofuran three times, and then vacuum dried at 80° C. for 24 h to obtain block copolymer modified silica nanoparticles 1.

[0101] Example 2

[0102] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the monomer represented by formula (2) was replaced by methacryloyl isocyanate, to obtain block copolymer modified silica nanoparticles 2.

[0103] Example 3

[0104] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the molar ratio of ethyl methacrylate, isocyanoethyl methacrylate and dimethylaminoethyl methacrylate was 1:0.25:0.33, to obtain block copolymer modified silica nanoparticles 3.

[0105] Example 4

[0106] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the molar ratio of ethyl methacrylate, isocyanoethyl methacrylate and dimethylaminoethyl methacrylate was 1:0.03:0.67, to obtain block copolymer modified silica nanoparticles 4.

[0107] Example 5

[0108] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the chain transfer agent was benzyl dithiobenzoate, to obtain block copolymer modified silica nanoparticles 5.

[0109] Comparative Example 1

[0110] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that no silane coupling agent was used to modify the silica nanoparticles. The specific steps are as follows:

[0111] (1) preparing a block copolymer according to the method of Example 1;

[0112] (2) 1.2 g of the block copolymer and 0.4 g of silica nanoparticles were ultrasonically dispersed in 20 mL of tetrahydrofuran solvent and refluxed at room temperature for 5 h. The solid product was separated by centrifugation, washed with tetrahydrofuran three times, and then vacuum dried at 80° C. for 24 h to obtain block copolymer modified silica nanoparticles D1.

[0113] Comparative Example 2

[0114] Block copolymer modified silica nanoparticles were prepared according to the method of Example 1, except that the structural unit B was derived from glycidyl methacrylate, to obtain block copolymer modified silica nanoparticles D2.

[0115] Comparative Example 3

[0116] Commercially available nano oil displacement agent D3

[0117] Test Case

[0118] The block copolymer modified silica nanoparticles 1-5, D1, D2 and D3 were tested for their ability to reduce water / crude oil interfacial tension. The results are shown in Table 1.

[0119] The block copolymer modified silica nanoparticles 1-5, D1, D2 and D3 were used to prepare an oil displacement agent system, and core flooding experiments were carried out. The results are shown in Table 2.

[0120] Table 1

[0121]

[0122]

[0123] Table 2

[0124]

[0125] It can be seen from the results in Table 1 that the interfacial tension of Examples 1-5 of the present invention is significantly reduced, and the interfacial tension of Example 1-3 can reach 10 when the mass concentration is higher than 0.3%. -2 The mN / m level indicates that the block copolymer modified silica nanoparticles provided by the present invention have good performance in reducing oil-water interfacial tension.

[0126] It can be seen from the results in Table 2 that the core permeabilities of Examples 1-5 and Comparative Examples 1-2 are all less than or equal to 50 mD, which are natural Berea cores in the low permeability range. The water drive recovery rate fluctuates within the normal range of ±2%. The nano-drive recovery rate of Examples 1-5 of the present invention is significantly improved on the basis of water drive, and the total recovery rate is also significantly improved. Moreover, the nano-drive recovery rate of Example 1-3 can be increased by more than 8 percentage points on the basis of water drive. Compared with commercially available nano oil-displacing agents, the block copolymer modified silica nanoparticles provided by the present invention can significantly improve the crude oil recovery rate.

[0127] Figure 1 By comparing the infrared spectra of Example 1 with those of the silicon dioxide nanoparticles not modified by the block copolymer of the present invention, it can be clearly seen that Example 1 has a 1600-1850 cm -1 The characteristic peak of carbon-oxygen double bond stretching vibration indicates that the block copolymer and the silica nanoparticles are connected via -NHCONH- in Example 1 to obtain block copolymer-modified silica nanoparticles.

[0128] Figure 2 By comparing the infrared spectra of Example 1 with those of the silica nanoparticles, it can be seen that there is no obvious change in the characteristic peaks, and the silica nanoparticles of D1 are not modified by the block copolymer.

[0129] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A block copolymer, It is characterized in that The block copolymer contains a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV. Among them, R 1 , R 3 , R 5 and R 6 are each independently hydrogen or methyl; R 2 C 1 -C 12 A straight chain or branched alkyl or phenyl group; R 4 C 1 -C 5 A straight chain or branched alkylene group; R 7 for x, y and z are each independently an integer of 1-10.

2. The block copolymer according to claim 1, in, R 2 C 1 -C 8 A straight or branched alkyl or phenyl group, preferably a methyl or ethyl group; R 4 C 1 -C 3 A straight chain or branched alkylene group, preferably a methylene group or an ethylene group; x, y and z are each independently an integer of 1 to 6, and x, y and z are preferably each independently 1 or 2; Preferably, the molar ratio of the structural unit A, the structural unit B and the structural unit C is 1:0.02-0.3:0.05-20; Preferably, the block copolymer has a weight average molecular weight of 15,000-160,000 g / mol, preferably 20,000-60,000 g / mol.

3. A method for preparing a block copolymer, It is characterized in that The preparation method comprises the following steps: (1) in a nitrogen atmosphere and in the presence of a first initiator, a chain transfer agent, and an organic solvent, subjecting the monomer represented by formula (1) and the monomer represented by formula (2) or methacryloyl isocyanate to a first polymerization reaction to obtain a first polymer product; (2) in a nitrogen atmosphere and in the presence of a second initiator, subjecting the first polymerization product to a second polymerization reaction with the monomer represented by formula (3) to obtain the block copolymer; Among them, R 1 , R 3 and R 6 are each independently hydrogen or methyl; R 2 C 1 -C 12 A straight chain or branched alkyl or phenyl group; R 4 C 1 -C 5 A straight chain or branched alkylene group; R 7 for x, y and z are each independently an integer of 1-10.

4. The preparation method according to claim 3, in, The molar ratio of the monomer represented by formula (1), the monomer represented by formula (2) and the monomer represented by formula (3) is 1:0.05-0.5:0.05-50.

5. The preparation method according to claim 3 or 4, in, In step (1), the conditions of the first polymerization reaction include: reaction temperature of 60-80° C., reaction time of 3-24 h; Preferably, the first initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate; Preferably, the chain transfer agent is benzyl dithiobenzoate or cumyl dithiobenzoate; Preferably, the R 2 C 1 -C 8 A straight chain or branched alkyl or phenyl group, preferably a methyl group or an ethyl group; 4 C 1 -C 3 A straight chain or branched alkylene group is preferably a methyl group or an ethyl group; x, y and z are each independently an integer of 1 to 6, and x, y and z are preferably each independently 1 or 2; Preferably, the monomer represented by formula (1) is selected from methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, isooctyl methacrylate, 2-ethylhexyl acrylate or styrene; Preferably, the monomer represented by formula (2) is isocyanoethyl methacrylate or isocyanoethyl acrylate; Preferably, the monomer represented by formula (3) is selected from methoxyethyl methacrylate, dimethylaminoethyl methacrylate, dimethylaminoethyl acrylate, poly(ethylene glycol) methacrylate, poly(ethylene glycol) acrylate, hydroxyethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl methacrylate, hydroxypropyl acrylate, 4-hydroxybutyl 2-methacrylate, 4-hydroxybutyl acrylate or 2-methoxyethyl 2-acrylate; Preferably, the organic solvent is benzene; Preferably, the molar ratio of the initiator, the chain transfer agent and the monomer represented by formula (1) is 1:1-5:50-500; Preferably, the volume ratio of the monomer represented by formula (1) to the monomer represented by formula (2) is 1:0.06-0.

46.

6. The preparation method according to any one of claims 3 to 5, in, Step (1) further comprises: dissolving the first polymer product in tetrahydrofuran, adding the first precipitant to precipitate, repeating 3-6 times, filtering and drying at 30-50° C. for 36-48 hours; Preferably, the first precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:1-4.

7. The preparation method according to any one of claims 3 to 6, in, In step (2), the conditions of the second polymerization reaction include: reaction temperature of 60-80° C., reaction time of 5-24 h; Preferably, the second initiator is an azo initiator, preferably one of azobisisobutyronitrile, azobisisoheptanenitrile and dimethyl azobisisobutyrate; Preferably, the molar ratio of the first polymer product, the monomer described in formula (3) and the second initiator is 1:10-1000:0.5-1.0; Preferably, step (2) further comprises: dissolving the block copolymer in tetrahydrofuran, adding the block copolymer into a second precipitant for precipitation, repeating 3-6 times, filtering and drying at 30-50° C. for 36-48 hours; Preferably, the second precipitant is a mixed solution of toluene and petroleum ether in a volume ratio of 1:5-10.

8. A block copolymer modified silica nanoparticle, It is characterized in that The modified silica nanoparticles comprise: a core from a surface-modified silica nanoparticle, a coating layer from a block copolymer, and a connecting group connecting the core and the coating layer, wherein the block copolymer comprises a structural unit A shown in formula I, a structural unit B shown in formula II or III, and a structural unit C shown in formula IV; Wherein, the connecting group is -NHCONH-, which is obtained by the addition reaction of -NCO contained in the structural unit B with the amino group contained in the surface-modified silica nanoparticles; Among them, R 1 , R 3 , R 5 and R 6 are each independently hydrogen or methyl; R 2 C 1 -C 12 A straight chain or branched alkyl or phenyl group; R 4 C 1 -C 5 A straight chain or branched alkylene group; R 7 for x, y and z are integers from 1-10.

9. The block copolymer modified silica nanoparticles according to claim 8, in, R 2 C 1 -C 8 A straight or branched alkyl or phenyl group, preferably a methyl or ethyl group; R 4 C 1 -C 3 A straight or branched alkylene group, preferably a methylene group or an ethylene group; x, y and z are integers of 1 to 6, and x, y and z are preferably 1 or 2; Wherein, the molar ratio of the structural unit A, the structural unit B and the structural unit C is 1:0.02-0.3:0.05-20; and / or, based on the total weight of the block copolymer modified silica nanoparticles, the content of the silica nanoparticles is 15-85wt%, preferably 35-75wt%; And / or, the average particle size of the silicon dioxide nanoparticles is 20-80 nm.

10. A method for preparing block copolymer modified silica nanoparticles, It is characterized in that The preparation method comprises the following steps: The block copolymer is reacted with silane coupling agent modified silica nanoparticles to obtain block copolymer modified silica nanoparticles; wherein the block copolymer is the block copolymer described in claims 1-2 or the block copolymer prepared by the preparation method described in any one of claims 3-7; Preferably, the mass ratio of the block copolymer to the silane coupling agent modified silica nanoparticles is 0.3-10:

1.

11. The preparation method according to claim 10, in, The reaction conditions include: ultrasonically dispersing the block copolymer and the silane coupling agent modified silica nanoparticles in tetrahydrofuran; reacting at 20-30° C. for 4-12 hours by reflux method; separating the precipitate, washing it, and drying it at 60-100° C. for 12-36 hours to obtain block copolymer modified silica nanoparticles; Preferably, the silane coupling agent is selected from 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldiethoxysilane, anilinemethyltrimethoxysilane or anilinemethyltriethoxysilane; Preferably, the preparation method of the silane coupling agent modified silica nanoparticles comprises: mixing anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate for a first reaction, adding a silane coupling agent for a second reaction for 2-5 hours to obtain the silane coupling agent modified silica nanoparticles; Preferably, the molar ratio of anhydrous ethanol, deionized water, ammonia water and tetraethyl orthosilicate is 25-80:2-5:0.25-3.9:1; Preferably, the molar ratio of the tetraethyl orthosilicate to the silane coupling agent is 1:0.01-0.2; Preferably, the conditions of the first reaction are: under stirring conditions, the reaction time is 12-24h; the reaction temperature is 20-30°C; Preferably, the conditions of the second reaction are: under stirring, the reaction time is 2-5h; the reaction temperature is 60-70°C; Preferably, the preparation method further comprises: washing the silane coupling agent modified silica nanoparticles in a dispersant, filtering and drying at 70-90° C. for 12-24 hours, wherein the dispersant is deionized water and / or ethanol.

12. Block copolymer modified nano silicon dioxide prepared by the preparation method according to claim 10 or 11.

13. Use of the block copolymer modified silica nanoparticles according to any one of claims 8 to 9 and 12 in enhancing crude oil recovery.

14. An oil displacing agent, It is characterized in that The oil displacing agent comprises: 99.5%-99.9% by weight of water and 0.1%-0.5% by weight of the block copolymer modified silicon dioxide nanoparticles according to any one of claims 8-9 and 12.

15. Use of the oil displacing agent according to claim 14 in improving crude oil recovery.

Citation Information

Patent Citations

  • Acrylic-urethane composite resin particles

    CN105849142A

  • Interface modification viscosity reducer for oil displacement as well as preparation method and application of interface modification viscosity reducer

    CN114507312A

  • Water-base polymer emulsion

    JP1996092455A

  • Pigment dispersant, pigment composition, colored composition for color filter and color filter

    JP2019210453A

  • Hair cosmetic comprising block copolymer

    WO2019230326A1

Cited By

  • Nano oil-displacing agent for oil extraction in oil field and preparation method of nano oil-displacing agent

    CN119614176A

  • Nano oil displacement agent for oil field production and preparation method thereof

    CN119614176B