Optical film, display device, and composition for forming ultraviolet absorbing layer
The optical film with a specific ultraviolet absorbing layer and functional layers addresses adhesion issues and enhances durability, ensuring high adhesion and resistance to outdoor conditions.
Patent Information
- Application Number
- PCT/JP2024/015736
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional ultraviolet absorbing layers in optical films face challenges with adhesion to resin layers, leading to reduced durability and increased stress due to volumetric contraction during curing, which affects their performance in outdoor applications.
An optical film comprising a first functional layer with an ultraviolet absorbing layer containing an active energy ray-curable resin and an ultraviolet absorber, featuring a structural unit with specific repeating units, which enhances adhesion and provides antistatic, antifouling, and antiglare properties, along with a second functional layer that can be an oxygen barrier or antireflection layer, improving the film's overall performance.
The solution achieves high adhesion and durability of the ultraviolet absorbing layer, maintaining optical properties and resistance to degradation, even without surface treatment or a primer layer, ensuring excellent light resistance and reflection suppression in outdoor conditions.
Smart Images

Figure JP2024015736_31102024_PF_FP_ABST
Abstract
Description
Optical film, display device, and composition for forming ultraviolet absorbing layer
[0001] The present invention relates to an optical film. It also refers to a display device using the optical film and a composition for forming an ultraviolet absorbing layer related to the optical film. This application claims priority to Japanese Patent Application No. 2023-070822, filed on April 24, 2023, the contents of which are incorporated herein by reference.
[0002] Hard coat films are widely used to protect display screens of displays, touch panels, mobile phones, etc. Mobile products such as mobile phones and smartphones are increasingly being used outdoors. Hard coat films for such outdoor applications are required to have excellent light resistance, such as not turning yellow even when exposed to ultraviolet rays for a long period of time and not causing peeling between the hard coat layer and the substrate film.
[0003] Patent Document 1 proposes adding an ultraviolet absorber or a light stabilizer to a hard coat layer for the purpose of imparting weather resistance. Patent Document 2 proposes a method of preventing light degradation of not only the substrate but also a colorable layer by using a hard coat layer containing an ultraviolet absorber together with a primer layer.
[0004] Japanese Patent Application Publication No. 9-157315 International Publication No. 2019 / 065833
[0005] It is generally known that photocurable layers containing UV absorbers (UV-absorbing layers) often exhibit poor adhesion to the resin layer they contact. To increase the hardness of UV-absorbing layers, the exposure dose and initiator must be increased, which is thought to result in greater volumetric shrinkage and stress than normal, resulting in poor adhesion. Previous approaches to address this issue have included modifying the formulation of the underlayer, which serves as the base for the UV-absorbing layer, to adjust the surface condition and flexibility, applying surface treatments to the underlayer, and applying a primer layer to the underlayer and curing it together with the UV-absorbing layer. However, depending on the type of UV-absorbing layer and underlayer, these approaches may not result in improved adhesion. Therefore, a UV-absorbing layer with good adhesion is needed to reduce the number of processes.
[0006] In view of the above circumstances, an object of the present invention is to provide an optical film in which an ultraviolet-absorbing layer has high adhesion. Another object of the present invention is to provide a composition for forming an ultraviolet-absorbing layer, which can form an ultraviolet-absorbing layer having high adhesion.
[0007] [1] An optical film according to a first aspect of the present invention comprises a first functional layer, an ultraviolet absorbing layer located on a first surface of the first functional layer, and a transparent substrate located on a second surface of the first functional layer. The ultraviolet absorbing layer contains an active energy ray-curable resin and an ultraviolet absorber. The active energy ray-curable resin contains a copolymer of a structural unit represented by the following formula (i) and a structural unit having any of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit. This optical film has an ultraviolet ray blocking rate of 90% or more as measured in accordance with JIS L1925, and a pencil hardness of H or more under a 500 g load on the surface of the first surface side. [In formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.] [2] The optical film according to [1], wherein the ultraviolet absorbing layer has one or more functions of antistatic property, antifouling property, and antiglare property. [3] The optical film according to [1] or [2], further comprising a second functional layer provided on the first surface side of the first functional layer and having a function different from that of the first functional layer. [4] The optical film according to [3], wherein the second functional layer has at least one of an antireflection function and an antiglare function. [5] The optical film according to [3], wherein the second functional layer is an antistatic layer or an antifouling layer. [6] The optical film according to [3], wherein the second functional layer has an oxygen permeability of 10 cm 3 / (m 2The optical film according to [3], wherein the first functional layer contains at least one of a first coloring material, a second coloring material, and a third coloring material, wherein the first coloring material has an absorption maximum wavelength in the range of 470 to 530 nm and a half-width of an absorption spectrum of 15 to 45 nm, the second coloring material has an absorption maximum wavelength in the range of 560 to 620 nm and a half-width of an absorption spectrum of 15 to 55 nm, and the third coloring material has a wavelength at which the transmittance is lowest in the wavelength range of 380 to 780 nm and is 650 to 780 nm. [8] The optical film according to [7], wherein the first functional layer contains a copolymer of the structural unit represented by formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit. [9] The optical film according to [7] or [8], wherein the first functional layer contains at least one of a radical scavenger, a peroxide decomposer, and a singlet oxygen quencher.
[10] The optical film according to [9], wherein the singlet oxygen quencher contains any one of dialkyl phosphate, dialkyl dithiocarbamate, benzenedithiol, and transition metal complexes thereof.
[11] The optical film according to any one of [7] to
[10] , wherein at least one of the first color material, the second color material, and the third color material contained in the first functional layer contains at least one compound selected from the group consisting of compounds having any one of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, and an indigo structure, and metal complexes thereof.
[0008]
[12] A display device according to a second aspect of the present invention includes the optical film according to any one of [1] to
[11] .
[0009]
[13] A composition for forming an ultraviolet absorbing layer according to a third aspect of the present invention contains an ultraviolet absorber, an active energy ray-curable resin, a photopolymerization initiator, and a solvent. The active energy ray-curable resin contains a copolymer of a structural unit represented by the above formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit. When a film having a thickness of 5 μm is formed from this composition, the film has an ultraviolet shielding rate of 90% or more as measured according to the method described in JIS L1925.
[0010] According to the present invention, an optical film can be provided in which the ultraviolet absorbing layer has high adhesion.
[0011] 1 is a schematic cross-sectional view of an optical film according to a first embodiment of the present invention; FIG. 2 is a schematic cross-sectional view of an optical film according to a second embodiment of the present invention; FIG. 3 is a schematic cross-sectional view of an optical film according to a third embodiment of the present invention; FIG. 4 is a schematic cross-sectional view of an optical film according to a fourth embodiment of the present invention; FIG. 5 is a graph showing the spectrum of a white display output through an organic EL light source and a color filter in an example; and FIG. 6 is a graph of the spectra of red, green, and blue displayed through an organic EL light source and a color filter in an example.
[0012] A first embodiment of the present invention will be described with reference to FIG.
[0013] [Optical Film] Fig. 1 is a schematic cross-sectional view of an optical film 1 according to a first embodiment of the present invention. As shown in Fig. 1, the optical film 1 is a laminate comprising a transparent substrate 10, a hard coat layer (first functional layer) 20, and an ultraviolet absorbing layer 30, and is formed by laminating the hard coat layer 20 and the ultraviolet absorbing layer 30 in this order on the transparent substrate 10. That is, the ultraviolet absorbing layer 30 is located on one surface (first surface) of the hard coat layer 20, and the transparent substrate 10 is located on the other surface (second surface).
[0014] The thickness of the optical film 1 is, for example, preferably 10 to 140 μm, more preferably 15 to 120 μm, and even more preferably 20 to 100 μm. When the thickness of the optical film 1 is equal to or greater than the above lower limit, the strength of the optical film 1 can be further increased. When the thickness of the optical film 1 is equal to or less than the above upper limit, not only can the optical film 1 be made lighter, but it is also advantageous for making the display device thinner. Each layer constituting the optical film 1 will now be described.
[0015] <Transparent Substrate> The transparent substrate 10 is a sheet-like member. A translucent resin film can be used as the material for the transparent substrate 10. Transparent resins and inorganic glass can be used as the material for the transparent substrate 10. Examples of transparent resins include polyolefins, polyesters, polyacrylates, polyamides, polyimides, polyarylates, polycarbonates, triacetyl cellulose, polyvinyl alcohol, polyvinyl chloride, cycloolefin copolymers, norbornene-containing resins, polyethersulfones, and polysulfones. Examples of polyolefins include polyethylene and polypropylene. Examples of polyesters include polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate. Examples of polyacrylates include polymethyl methacrylate. Examples of polyamides include nylon 6 and nylon 66. Among these, films made of polyethylene terephthalate (PET), triacetyl cellulose (TAC), polymethyl methacrylate (PMMA), and films made of polyesters other than PET are preferably used. The thickness of the transparent substrate 10 is not particularly limited, but is preferably 10 to 100 μm, for example. The transmittance of the transparent substrate 10 is preferably 90% or more, for example.
[0016] The transparent substrate 10 may be provided with ultraviolet absorbing ability. By adding an ultraviolet absorbing agent to the resin that is the raw material of the transparent substrate 10, the transparent substrate 10 can be provided with ultraviolet absorbing ability.
[0017] Examples of the ultraviolet absorber include salicylic acid ester-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, benzotriazine-based ultraviolet absorbers, cyanoacrylate-based ultraviolet absorbers, etc. These ultraviolet absorbers may be used alone or in combination of two or more.
[0018] When the transparent substrate 10 is provided with ultraviolet absorbing ability, the ultraviolet shielding rate is preferably 85% or more. Here, the ultraviolet shielding rate is a value measured in accordance with JIS L1925 and calculated by the following formula: ultraviolet shielding rate (%) = 100 - average transmittance (%) of ultraviolet light with a wavelength of 290 to 400 nm.
[0019] <Hard Coat Layer> The hard coat layer 20 is formed on the transparent substrate 10 and is in contact with the transparent substrate 10. The hard coat layer 20 is a layer that functions as a reinforcing layer in the optical film 1 to prevent scratches and the like. Examples of the hard coat layer 20 include a layer formed of a hard coat agent containing a monofunctional, difunctional, trifunctional or higher functional (meth)acrylate or urethane (meth)acrylate. In this specification, "(meth)acrylate" means both or either one of "acrylate" and "methacrylate."
[0020] <<Ultraviolet Absorbing Layer>> The ultraviolet absorbing layer 30 is formed on the hard coat layer 20 and is in contact with the hard coat layer 20. The ultraviolet absorbing layer 30 contains an active energy ray-curable resin and an ultraviolet absorber.
[0021] The active energy ray-curable resin is a resin that is polymerized and cured by irradiation with active energy rays such as ultraviolet rays, electron beams, etc. The active energy ray-curable resin according to this embodiment contains a copolymer of a radical scavenger and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit.
[0022] The radical scavenger according to this embodiment is an amine structure-containing polymer having radical scavenging ability, and includes a structural unit represented by the following formula (i).
[0023]
[0024] In the above formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.
[0025] R 1 R is preferably a hydrogen atom, a hydroxy group, or an alkyl group having 10 or less carbon atoms. The number of carbon atoms in the alkyl group is preferably 1 to 6, and more preferably 1 to 3. 2 is preferably a hydrogen atom or an alkyl group having 10 or less carbon atoms. The number of carbon atoms in the alkyl group is preferably 1 to 6, and more preferably 1 to 3. X is preferably a single bond or an aliphatic alkyl chain having 30 or less carbon atoms. The number of carbon atoms in the aliphatic alkyl chain is preferably 10 or less, preferably 1 to 6, and more preferably 2 to 4.
[0026] The molecular weight of the structural unit represented by formula (i) is preferably 2000 or more. When the molecular weight is 2000 or more, the deterioration suppression effect of the ultraviolet absorber is improved. This is thought to be because more molecules remain within the ultraviolet absorbing layer 30, thereby achieving a sufficient deterioration suppression effect. The upper limit of the molecular weight of the structural unit represented by formula (i) is not particularly limited, but can be, for example, about 100,000 or more. In this specification, "molecular weight" means the "mass average molecular weight" measured by gel permeation chromatography (GPC) using polystyrene as a standard substance.
[0027] Examples of repeating units of the copolymer include (meth)acrylate repeating units, olefin repeating units, halogen atom-containing repeating units, styrene repeating units, vinyl acetate repeating units, and vinyl alcohol repeating units.
[0028] Examples of the (meth)acrylate repeating unit include a repeating unit derived from a (meth)acrylate monomer having a linear or branched alkyl group on the side chain, and a repeating unit derived from a (meth)acrylate monomer having a hydroxyl group on the side chain.
[0029] Examples of the repeating unit derived from a (meth)acrylate monomer having the linear or branched alkyl group on the side chain include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, and isopropyl (meth)acrylate. Examples of monomer-derived components include octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, myristyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, and octadecyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above, (meth)acrylate-based repeating units having a linear or branched alkyl group having from 1 to 4 carbon atoms in the side chain are preferred.
[0030] Examples of the repeating unit derived from a (meth)acrylic monomer having a hydroxyl group in the side chain include components derived from monomers such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, hydroxyphenyl (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0031] Examples of the olefin repeating unit include components derived from olefin monomers such as ethylene, propylene, isoprene, butadiene, etc. These may be used alone or in combination of two or more.
[0032] Examples of the halogen atom-containing repeating unit include components derived from monomers such as vinyl chloride, vinylidene chloride, etc. These may be used alone or in combination of two or more.
[0033] Examples of styrene-based repeating units include components derived from styrene-based monomers such as styrene, α-methylstyrene, and vinyltoluene. These may be used alone or in combination of two or more. Examples of vinyl acetate-based repeating units include esters of saturated carboxylic acids and vinyl alcohol, such as vinyl acetate and vinyl propionate. These may be used alone or in combination of two or more. Examples of vinyl alcohol-based repeating units include vinyl alcohol, which may have a 1,2-glycol bond in the side chain.
[0034] The copolymer may have any of the structures of a random copolymer, an alternating copolymer, a block copolymer, and a graft copolymer. If the copolymer has a random structure, the manufacturing process and preparation with other components are easy. Therefore, a random copolymer is preferable to other copolymers.
[0035] Radical polymerization can be used as a polymerization method for obtaining the copolymer. Radical polymerization is preferred because it is easy to produce industrially. Radical polymerization may be a solution polymerization method, an emulsion polymerization method, a bulk polymerization method, a suspension polymerization method, or the like. For radical polymerization, it is preferable to use a solution polymerization method. By using a solution polymerization method, it is easy to control the molecular weight of the copolymer.
[0036] In radical polymerization, the above-mentioned monomers may be diluted with a polymerization solvent, and then a polymerization initiator may be added to polymerize the monomers. Examples of the polymerization solvent include ester-based solvents, alcohol ether-based solvents, ketone-based solvents, aromatic solvents, amide-based solvents, and alcohol-based solvents. Examples of the ester-based solvent include methyl acetate, ethyl acetate, n-butyl acetate, isobutyl acetate, t-butyl acetate, methyl lactate, and ethyl lactate. Examples of the alcohol ether-based solvent include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monoethyl ether, 3-methoxy-1-butanol, and 3-methoxy-3-methyl-1-butanol. Examples of the ketone-based solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. Examples of the aromatic solvent include benzene, toluene, and xylene. Examples of the amide solvent include formamide and dimethylformamide. Examples of the alcohol solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, s-butanol, t-butanol, diacetone alcohol, and 2-methyl-2-butanol. The above-mentioned polymerization solvents may be used alone or in combination of two or more.
[0037] The radical polymerization initiator may be, for example, a peroxide or an azo compound. The peroxide may be, for example, benzoyl peroxide, t-butyl peroxyacetate, t-butyl peroxybenzoate, di-t-butyl peroxide, etc. The azo compound may be, for example, azobisisobutyronitrile, azobisamidinopropane salt, azobiscyanovaleric acid (salt), 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], etc.
[0038] The amount of radical polymerization initiator used is preferably 0.0001 parts by mass or more and 20 parts by mass or less, more preferably 0.001 parts by mass or more and 15 parts by mass or less, and even more preferably 0.005 parts by mass or more and 10 parts by mass or less, when the total amount of monomers is set to 100 parts by mass. The radical polymerization initiator may be added to the monomers and polymerization solvent before the start of polymerization, or may be added dropwise to the polymerization reaction system. Adding the radical polymerization initiator dropwise to the monomers and polymerization solvent in the polymerization reaction system is preferred because it can suppress heat generation due to polymerization.
[0039] The reaction temperature for radical polymerization is appropriately selected depending on the types of radical polymerization initiator and polymerization solvent. From the viewpoints of ease of production and reaction controllability, the reaction temperature is preferably 60° C. or higher and 110° C. or lower.
[0040] The content of the radical scavenger represented by formula (i) is preferably 1 to 95 mol %, more preferably 10 to 90 mol %, based on the total molar amount of the monomers constituting the active energy ray-curable resin.
[0041] As the ultraviolet absorber, the same ones as those exemplified in the explanation of the transparent substrate can be used.
[0042] The optical film 1 of this embodiment having the above configuration exhibits sufficient UV-shielding ability, with a UV-shielding rate of 90% or more as measured in accordance with JIS L1925, due to the UV-absorbing layer 30, and the UV-absorbing layer 30 and the hard coat layer 20 are sufficiently adhered to each other. The copolymer contained in the active energy ray-curable resin improves the adhesion between the UV-absorbing layer 30 and the hard coat layer 20, and the radical scavenger represented by formula (i) suppresses deterioration of the UV absorber, improving light resistance. In the optical film 1, the UV-absorbing layer 30 has good adhesion even without performing a surface treatment on the surface in contact with the UV-absorbing layer 30 or forming a primer layer. Furthermore, due to the hardness of the hard coat layer 20 and the active energy ray-curable resin after curing, the UV-absorbing layer 30 side has a sufficient surface hardness of H or more in a pencil hardness test with a load of 500 g in accordance with JIS-K5400-1990.
[0043] The ultraviolet absorbing layer 30 according to the present invention may be imparted with antistatic properties, antifouling properties, antiglare properties, etc. by adding a specific substance. Examples of additives for imparting antistatic properties include metal oxide fine particles such as antimony-doped tin oxide (ATO) and tin-doped indium oxide (ITO), polymeric conductive compositions, and various antistatic agents such as quaternary ammonium salts. Examples of additives for imparting antifouling properties include various antifouling agents such as silicon oxide, fluorine-containing silane compounds, fluoroalkyl silazanes, fluoroalkyl silanes, fluorine-containing silicon-based compounds, and perfluoropolyether group-containing silane coupling agents.
[0044] Additives for imparting antiglare properties can include organic and inorganic particles. Organic particles are materials that form fine irregularities on the surface and provide the ability to scatter external light. Examples of organic particles include resin particles made of translucent resin materials such as acrylic resin, polystyrene resin, styrene-(meth)acrylic acid ester copolymer, polyethylene resin, epoxy resin, silicone resin, polyvinylidene fluoride, and polyethylene fluoride resin. Two or more types of resin particles with different materials (refractive indexes) may be mixed to adjust the refractive index and dispersibility of the resin particles. Inorganic particles are materials that adjust the sedimentation and aggregation of organic particles. Examples of inorganic particles that can be used include silica particles, metal oxide particles, and various mineral particles. Examples of silica particles that can be used include colloidal silica and silica particles surface-modified with reactive functional groups such as (meth)acryloyl groups. Examples of metal oxide microparticles that can be used include alumina (aluminum oxide), zinc oxide, tin oxide, antimony oxide, indium oxide, titania (titanium dioxide), and zirconia (zirconium dioxide). Examples of mineral microparticles that can be used include mica, synthetic mica, vermiculite, montmorillonite, iron-montmorillonite, bentonite, beidellite, saponite, hectorite, stevensite, nontronite, magadiite, ailalite, kanemite, layered titanic acid, smectite, and synthetic smectite. The mineral microparticles may be either natural or synthetic (including substituted or derivative) materials, or a mixture of both may be used. Among mineral microparticles, layered organic clays are more preferred. Layered organic clays refer to swelling clays in which organic onium ions are introduced between the layers. The organic onium ions are not limited as long as they can be organized by utilizing the cation exchange properties of the swelling clay. When a layered organic clay mineral is used as the mineral fine particles, the above-mentioned synthetic smectite can be suitably used.
[0045] A second embodiment of the present invention will be described with reference to Fig. 2. In the following description, components common to those already described will be assigned the same reference numerals and redundant description will be omitted.
[0046] 2 is a schematic cross-sectional view of an optical film 2 according to this embodiment. The optical film 2 has a second functional layer 40 formed on an ultraviolet absorbing layer 30.
[0047] The function exhibited by the second functional layer 40 can be varied in various ways depending on the application of the optical film, etc. Specific examples of the second functional layer include a low refractive index layer, an antiglare layer, an antistatic layer, an antifouling layer, etc., and the second functional layer may have two or more functions. The antistatic layer, the antifouling layer, and the antiglare layer can be formed using a composition in which the above-mentioned various additives are added to the base resin constituting the layer.
[0048] When the second functional layer 40 is a low refractive index layer, its refractive index can be, for example, 1.20 to 1.55. Examples of additives used to adjust the refractive index include fine particles of lithium fluoride (LiF), magnesium fluoride (MgF2), sodium hexafluoroaluminum (cryolite, cryolite, 3NaF·AlF3, Na3AlF6), aluminum fluoride (AlF3), etc., as well as silica fine particles. As the silica fine particles, those having voids inside the particles, such as porous silica fine particles and hollow silica fine particles, are suitable.
[0049] The method for forming the low refractive index layer is not limited, and examples thereof include a method in which a composition for forming a low refractive index layer is applied to the UV absorbing layer 30 and cured by irradiating it with active energy rays, vacuum deposition, sputtering, ion plating, ion beam deposition, and plasma vapor deposition. The thickness of the low refractive index layer is not particularly limited, but a thickness of 40 nm to 1 μm is preferred. By providing a low refractive index layer, the optical film 2 exhibits anti-reflection properties. Furthermore, the copolymer contained in the active energy ray-curable resin provides good adhesion to the UV absorbing layer 30 without requiring surface treatment or the formation of a primer layer on the surface in contact with the UV absorbing layer 30. Therefore, adhesion between the UV absorbing layer 30 and the second functional layer 40 can be improved without requiring surface treatment or the use of a primer layer.
[0050] A third embodiment of the present invention will be described with reference to Fig. 3. Fig. 3 is a schematic cross-sectional view of an optical film 3 according to this embodiment. The optical film 3 has a configuration in which a colored layer 50 is provided instead of the hard coat layer 20 of the optical film 1.
[0051] The colored layer 50, which is the first functional layer, is a cured product of a colored layer-forming composition and contains a dye (A), an active energy ray-curable resin (B), and a photopolymerization initiator (C). The thickness of the colored layer 50 is preferably, for example, 0.5 to 10 μm. When the thickness of the colored layer 50 is equal to or greater than the above-mentioned lower limit, the colored layer 50 can contain the dye without causing abnormalities in its appearance, and the light absorption properties of the dye can improve the reflectivity and color reproducibility. When the thickness of the colored layer 50 is equal to or less than the above-mentioned upper limit, this is advantageous for reducing the thickness of the display device. The thickness of the colored layer 50 can be determined by observing a cross section of the optical film in the thickness direction using a microscope or the like.
[0052] <Dye (A)> The dye (A) contains at least one of the first coloring material, second coloring material, and third coloring material shown below. The absorption maximum wavelength of the first coloring material is in the range of 470 nm to 530 nm, and the half-width of the absorption spectrum is 15 nm to 45 nm. If the absorption maximum wavelength is below the lower limit, the luminance efficiency of blue light emission is likely to decrease, and if it exceeds the upper limit, the luminance efficiency of green light emission is likely to decrease. If the half-width of the absorption spectrum is below the lower limit, the suppression effect on the reflectivity to external light is small, and if it exceeds the upper limit, the reflectivity to external light is likely to improve, but the luminance efficiency is likely to decrease.
[0053] The second colorant has an absorption maximum wavelength in the range of 560 nm to 620 nm, and an absorption spectrum half-width of 15 nm to 55 nm. If the absorption maximum wavelength is less than the lower limit, the luminance efficiency of green light emission is likely to decrease, while if it exceeds the upper limit, the luminance efficiency of red light emission is likely to decrease. If the absorption spectrum half-width is less than the lower limit, the effect of suppressing the reflectivity to external light is small, while if it exceeds the upper limit, the reflectivity to external light is likely to improve, but the luminance efficiency is likely to decrease.
[0054] The third coloring material has a wavelength of 650 to 780 nm at which the transmittance is lowest within the wavelength range of 380 to 780 nm. If the wavelength of 400 to 780 nm at which the transmittance is lowest is less than the lower limit, the luminance efficiency of red light emission is likely to decrease. If the wavelength is greater than the upper limit, the effect of suppressing the reflectivity of external light is reduced.
[0055] The dye (A) preferably contains a compound having a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, or an indigo structure, or a metal complex thereof. In particular, it is more preferable to use a metal complex having a porphyrin structure, a pyrromethene structure, or a phthalocyanine structure, or a compound having a squarylium structure, because of its excellent reliability. The dye (A) may contain one of these compounds or metal complexes thereof alone, or two or more of them. These compounds or metal complexes thereof may be contained in the first coloring material, the second coloring material, the third coloring material, or two or more of these coloring materials.
[0056] <Energy ray-curable compound (B)> The energy ray-curable compound (B) is a resin that is polymerized and cured by irradiation with active energy rays such as ultraviolet rays, electron beams, etc. For example, a monofunctional, difunctional, trifunctional or higher functional (meth)acrylate monomer, urethane (meth)acrylate, etc. can be used.
[0057] Examples of monofunctional (meth)acrylate compounds that can be contained in the energy ray-curable compound (B) include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, glycidyl (meth)acrylate, acryloylmorpholine, N-vinylpyrrolidone, tetrahydrofurfuryl acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and methyl acrylate. Sil (meth)acrylate, isobornyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, benzyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phosphate (meth)acrylate, ethylene oxide-modified phosphate (meth)acrylate, phenoxy (meth)acrylate, ethylene oxide Oxide-modified phenoxy (meth)acrylate, propylene oxide-modified phenoxy (meth)acrylate, nonylphenol (meth)acrylate, ethylene oxide-modified nonylphenol (meth)acrylate, propylene oxide-modified nonylphenol (meth)acrylate, methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypropylene glycol (meth)acrylate, 2-(meth)acryloyloxyethyl-2-hydroxypropyl phthalate, 2-hydroxypropyl acrylate hydroxy-3-phenoxypropyl (meth)acrylate, 2-(meth)acryloyloxyethyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hydrogen phthalate, 2-(meth)acryloyloxypropyl hexahydrohydrogen phthalate, 2-(meth)acryloyloxypropyl tetrahydrohydrogen phthalate, dimethylaminoethyl (meth)acrylate, trifluoroethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate,Examples include adamantane derivative mono(meth)acrylates such as octafluoropropyl(meth)acrylate, 2-adamantane, and adamantyl acrylate having a monovalent mono(meth)acrylate derived from adamantanediol. Here, "(meth)acryloyl" means both or either "acryloyl" and "methacryloyl."
[0058] Examples of bifunctional (meth)acrylate compounds that can be contained in the energy ray-curable compound (B) include di(meth)acrylates such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, nonanediol di(meth)acrylate, ethoxylated hexanediol di(meth)acrylate, propoxylated hexanediol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, ethoxylated neopentyl glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, and hydroxypivalic acid neopentyl glycol di(meth)acrylate.
[0059] Examples of trifunctional or higher functional (meth)acrylate compounds that can be contained in the energy ray curable compound (B) include tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, ethoxylated trimethylolpropane tri(meth)acrylate, propoxylated trimethylolpropane tri(meth)acrylate, tris-2-hydroxyethyl isocyanurate tri(meth)acrylate, and glycerin tri(meth)acrylate, and trifunctional (meth)acrylates such as pentaerythritol tri(meth)acrylate, dipentaerythritol tri(meth)acrylate, and ditrimethylolpropane tri(meth)acrylate. Examples of the (meth)acrylate compound include tri- or higher functional (meth)acrylate compounds such as pentaerythritol tetra(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and ditrimethylolpropane hexa(meth)acrylate, as well as polyfunctional (meth)acrylate compounds in which a portion of these (meth)acrylates is substituted with an alkyl group or ε-caprolactone.
[0060] Another resin that can be contained in the energy ray-curable compound (B) is a urethane (meth)acrylate. Examples of the urethane (meth)acrylate include those obtained by reacting a polyester polyol with an isocyanate monomer or a prepolymer, and then reacting the resulting product with a (meth)acrylate monomer having a hydroxyl group.
[0061] Examples of urethane (meth)acrylates include pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate hexamethylene diisocyanate urethane prepolymer, pentaerythritol triacrylate toluene diisocyanate urethane prepolymer, dipentaerythritol pentaacrylate toluene diisocyanate urethane prepolymer, pentaerythritol triacrylate isophorone diisocyanate urethane prepolymer, and dipentaerythritol pentaacrylate isophorone diisocyanate urethane prepolymer.
[0062] The monofunctional, difunctional, trifunctional or higher functional (meth)acrylate monomers, urethane (meth)acrylates, etc. that can be contained in the other energy ray-curable compound (B) described above may be used alone or in combination of two or more. They may also be partially polymerized oligomers. Copolymers containing various repeating units used in the ultraviolet absorbing layer 30 may also be contained in the energy ray-curable compound (B).
[0063] The content of the energy ray-curable compound (B) is preferably 20 to 80 mass %, more preferably 30 to 70 mass %, relative to the total mass of the color layer-forming composition. When the content of the energy ray-curable compound (B) is equal to or greater than the above-mentioned lower limit, the effect of inhibiting discoloration can be further enhanced. When the content of the energy ray-curable compound (B) is equal to or less than the above-mentioned upper limit, the handleability of the color layer-forming composition can be further improved.
[0064] <Photopolymerization initiator (C)> When ultraviolet rays are used as the active energy rays, the photopolymerization initiator (C) generates radicals when irradiated with ultraviolet rays. Examples of the photopolymerization initiator (C) include benzoins (benzoin alkyl ethers such as benzoin, benzoin methyl ether, benzoin ethyl ether, and benzoin isopropyl ether), phenyl ketones [for example, alkyl phenyl ketones such as acetophenones (for example, acetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, and 1,1-dichloroacetophenone) and 2-hydroxy-2-methylpropiophenone; cycloalkyl phenyl ketones such as 1-hydroxycyclohexyl phenyl ketone], aminoacetophenones {2-methyl-1-[4-(methylthio)phenyl] [4-morpholinophenyl]-2-morpholinoaminopropanone-1, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, etc.}, anthraquinones (anthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-t-butylanthraquinone, 1-chloroanthraquinone, etc.), thioxanthones (2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone, etc.), ketals (acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.), benzophenones (benzophenone, etc.), xanthones, phosphine oxides (for example, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, etc.), etc. These photopolymerization initiators may be used alone or in combination of two or more.
[0065] The content of the photopolymerization initiator (C) is preferably 0.01 to 20% by mass, more preferably 0.01 to 5% by mass, based on the solid content of the color layer-forming composition. If the content of the photopolymerization initiator (C) is less than the above lower limit, curability will be insufficient. If the content of the photopolymerization initiator (C) is more than the above upper limit, unreacted photopolymerization initiator (C) will remain, deteriorating reliability such as heat resistance.
[0066] The colored layer 50 may contain a solvent (D) and an additive (E). These are described in detail below. <Solvent (D)> The solvent (D) is necessary when forming the colored layer. While most of it disappears from the colored layer by volatilization or other means during drying after application, some remains in the colored layer, and therefore its components will be described below. Examples of the solvent (D) include ethers, ketones, esters, and cellosolves. Examples of ethers include dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, 1,4-dioxane, 1,3-dioxolane, 1,3,5-trioxane, tetrahydrofuran, anisole, and phenetole. Examples of ketones include acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, methylcyclohexanone, and ethylcyclohexanone. Examples of esters include ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, and γ-butyrolactone. Examples of cellosolves include methyl cellosolve, cellosolve (ethyl cellosolve), butyl cellosolve, and cellosolve acetate. The solvent (D) may be used alone or in combination of two or more.
[0067] The content of the solvent (D) is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, based on the total mass of the colored layer-forming composition containing the above (A) to (C). When the content of the solvent (D) is equal to or greater than the above lower limit, the handleability of the colored layer-forming composition can be further improved. When the content of the solvent (D) is equal to or less than the above upper limit, the time required to form the colored layer can be shortened.
[0068] <Additive (E)> Examples of additive (E) include a compound having at least a structure represented by the following formula (ii) (hereinafter referred to as "compound A"), a radical scavenger, a singlet oxygen quencher, a peroxide decomposer, and the like.
[0069]
[0070] In formula (ii), R 1 each independently represents an alkyl group, an alkenyl group, an aryl group, a heterocyclic group, R 9 CO-, R 10 SO 2 -, and R 11 NHCO— (R 9 , R 10 , R 11 are each independently any one of an alkyl group, an alkenyl group, an aryl group, and a heterocyclic group. 2 and R 3 R are each independently any one of a hydrogen atom, a halogen atom, an alkyl group, an alkenyl group, an alkoxy group, and an alkenyloxy group. 4 ~R 8 are each independently a hydrogen atom, an alkyl group, an alkenyl group, or an aryl group.
[0071] Examples of the radical scavenger include hindered amine light stabilizers such as 4-isopropylaminodiphenylamine, N-phenyl-1-naphthylamine, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate, and phenolic antioxidants such as 2,6-di-t-butyl-p-cresol and 6,6'-di-t-butyl-4,4'-butylidene-m-cresol.
[0072] Examples of singlet oxygen quenchers include transition metal complexes, dyes, amines, phenols, and sulfides. Particularly preferred materials include transition metal complexes of dialkyl phosphate, dialkyl dithiophosphate, dialkyl dithiocarbamate, or benzenedithiol or similar dithiols, and nickel, zinc, copper, or cobalt is preferably used as the central metal of these transition metal complexes.
[0073] Peroxide decomposers have the function of decomposing peroxides generated when dyes are oxidized and deteriorated, stopping the autoxidation cycle and suppressing dye deterioration (fading). Phosphorus-based antioxidants and sulfur-based antioxidants can be used as peroxide decomposers.
[0074] Examples of phosphorus-based antioxidants include 2,2'-methylenebis(4,6-di-t-butyl-1-phenyloxy)(2-ethylhexyloxy)phosphorus, 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane, and 6-[3-(3-t-butyl-4-hydroxy-5-methylphenyl)propoxy]-2,4,8,10-tetra-t-butyldibenz[d,f][1,3,2]dioxaphosphepine.
[0075] Examples of sulfur-based antioxidants include 2,2-bis({[3-(dodecylthio)propionyl]oxy}methyl)-1,3-propanediyl-bis[3-(dodecylthio)propionate], 2-mercaptobenzimidazole, dilauryl-3,3′-thiodipropionate, dimyristyl-3,3′-thiodipropionate, distearyl-3,3′-thiodipropionate, pentaerythrityl-tetrakis(3-laurylthiopropionate), and 2-mercaptobenzothiazole.
[0076] By incorporating these additives into the colored layer 50, the light resistance and heat resistance of the dye (A) can be improved.
[0077] The additive (E) may contain other additives such as a leveling agent, an antifoaming agent, an antioxidant, an ultraviolet absorber, a light stabilizer, a photosensitizer, and a conductive material.
[0078] The optical film 3 according to this embodiment includes a colored layer 50, and when attached to various display devices, it can achieve both reflection suppression and brightness efficiency, thereby contributing to improved display quality. Furthermore, by attaching the ultraviolet absorbing layer 30 positioned on the side where external light is incident, deterioration of the colored layer can be suppressed, and the effect can be maintained for a long period of time. Furthermore, the copolymer contained in the active energy ray-curable resin ensures good adhesion of the ultraviolet absorbing layer 30 without performing surface treatment or forming a primer layer on the surface that comes into contact with the ultraviolet absorbing layer 30. Therefore, the adhesion between the ultraviolet absorbing layer 30 and the colored layer 50 can be improved without using surface treatment or a primer layer.
[0079] A fourth embodiment of the present invention will be described with reference to Fig. 4. Fig. 4 is a schematic cross-sectional view of an optical film 4 according to this embodiment. The optical film 4 has the same configuration as the optical film 3, except that an oxygen barrier layer (second functional layer) 60 is provided between the ultraviolet absorbing layer 30 and the colored layer 50.
[0080] The oxygen barrier layer 60 is a transparent layer having optical transparency, and is one embodiment of the second functional layer. The oxygen permeability of the oxygen barrier layer 60 is 10 cm 3 / m 2 ・day・atm or less, 5cm 3 / (m 2 ·day·atm) or less, and 3 / (m 2 When the oxygen permeability of the oxygen barrier layer 60 is equal to or less than the above upper limit, sufficient oxygen barrier properties can be exhibited. The lower limit of the oxygen permeability of the oxygen barrier layer 60 is not particularly limited, and is preferably 0 cm 3 / (m 2 The oxygen barrier layer 60 may have a pressure of 1000 psi (1000 psi, ...
[0081] Furthermore, inorganic particles (particles made of an inorganic compound) may be dispersed in the oxygen barrier layer 60. The inorganic particles can further reduce oxygen permeability and further suppress oxidative deterioration (fading) of the colored layer 50. The size and content of the inorganic particles are not particularly limited and may be appropriately set depending on the thickness of the oxygen barrier layer 60, etc. The size (maximum length) of the inorganic particles dispersed in the oxygen barrier layer 60 is preferably less than the thickness of the oxygen barrier layer 60, and the smaller the size, the more advantageous it is. The size of the inorganic particles dispersed in the oxygen barrier layer 60 may be uniform or non-uniform. Specific examples of inorganic particles dispersed in the oxygen barrier layer 60 include silica particles, alumina particles, silver particles, copper particles, titanium particles, zirconia particles, and tin particles.
[0082] The optical film 4 according to this embodiment includes an oxygen barrier layer 60. Therefore, by attaching the oxygen barrier layer 60 to a display device so that it is closer to the viewer than the colored layer 50, oxygen contained in the ambient air does not reach the colored layer 50 unless it passes through the oxygen barrier layer 60. As a result, deterioration of the coloring material contained in the colored layer 50 due to oxygen is suppressed, and the color correction function can be maintained for a longer period of time. Furthermore, the copolymer contained in the active energy ray-curable resin ensures good adhesion of the ultraviolet absorbing layer 30 without performing surface treatment or forming a primer layer on the surface in contact with the ultraviolet absorbing layer 30. Therefore, the adhesion between the ultraviolet absorbing layer 30 and the oxygen barrier layer 60 can be improved without using surface treatment or a primer layer. In this embodiment, the number and position of the oxygen barrier layer 60 can be appropriately determined.
[0083] [Method for Manufacturing Optical Film] The optical film according to each embodiment of the present invention can be manufactured by a conventionally known method. For example, in the case of the optical film 1, a hard coat layer 20 is formed by first applying a hard coat agent to one surface of the transparent substrate 10 and curing it. Note that a colored layer 50 may be formed instead of the hard coat layer 20. Furthermore, an oxygen barrier layer 60 may be formed on the colored layer 50. Thereafter, a composition for forming an ultraviolet absorbing layer is applied and cured by irradiation with active energy rays, thereby obtaining the ultraviolet absorbing layer 30. A second functional layer 40 may be formed on the ultraviolet absorbing layer 30.
[0084] The ultraviolet absorbing layer-forming composition according to the present invention contains an ultraviolet absorber, an active energy ray-curable resin, a photopolymerization initiator, and a solvent. The active energy ray-curable resin contains a copolymer of a structural unit represented by formula (i) and a structural unit having any of a (meth)acrylate repeating unit, an olefin repeating unit, a halogen atom-containing repeating unit, a styrene repeating unit, a vinyl acetate repeating unit, and a vinyl alcohol repeating unit. The photopolymerization initiator may be any of those described above for photopolymerization initiator (C). The light source used to form the ultraviolet absorbing layer 30 can be any light source that generates active energy rays. Examples of active energy rays that can be used include radiation (gamma rays, X-rays, etc.), ultraviolet rays, visible light, and electron beams (EB). UV rays and electron beams are typically used. For example, lamps that emit ultraviolet rays include low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, and electrodeless discharge tubes. The irradiation condition is that the ultraviolet irradiation dose is usually 100 to 1000 mJ / cm 2 A film having a thickness of 5 μm formed from this composition for forming an ultraviolet absorbing layer has an ultraviolet shielding rate of 90% or more as measured in accordance with the method described in JIS L1925.
[0085] [Display Device] The display device of the present invention comprises the optical film of the present invention. Specific examples of the display device include televisions, monitors, mobile phones, portable game machines, personal digital assistants, personal computers, electronic books, video cameras, digital still cameras, head-mounted displays, navigation systems, audio playback devices (car audio, digital audio players, etc.), copiers, facsimiles, printers, multi-function printers, vending machines, automated teller machines (ATMs), personal authentication devices, optical communication devices, and IC cards. In particular, the optical film of the present invention is preferably used in display devices equipped with self-luminous elements such as LEDs, organic electroluminescent devices, inorganic phosphors, and quantum dots, which are susceptible to the influence of external light reflection due to metal electrodes and wiring.
[0086] Each embodiment of the present invention has been described above in detail with reference to the drawings, but the specific configuration is not limited to this embodiment, and configuration changes, combinations, etc. are also included within the scope that does not deviate from the gist of the present invention.
[0087] The present invention will be described in more detail below using examples, but the technical scope of the present invention is not limited solely by the specific content of these examples.
[0088] [Examples 1 to 13, Comparative Examples 1 to 5] In the following Examples and Comparative Examples, optical films A to R were prepared with the layer structures shown in Tables 1 and 2. In the tables, "-" indicates that the corresponding layer was not present.
[0089]
[0090]
[0091] Tables 3 and 4 show the layer configurations for each example.
[0092]
[0093]
[0094] <<Preparation of Optical Film>> Hereinafter, each layer constituting the optical film will be described in detail.
[0095] <Transparent substrate> Details of the materials listed in Tables 1 and 2 are as follows: TAC: triacetyl cellulose film (manufactured by Fujifilm Corporation, TG60UL, substrate thickness 60 μm, UV shielding rate 92.9%) PMMA: polymethyl methacrylate film (manufactured by Sumitomo Chemical Co., Ltd., W002N80, substrate thickness 80 μm, UV shielding rate 13.9%)
[0096] <Hard Coat Layer and Ultraviolet Absorbing Layer> Details of the materials listed in Table 3 are shown below. Active energy ray curable resin Resin 1: A polymer containing a structural unit represented by formula (i), R 1 is CH 3 , R 2 is CH 3, X is a single bond, and the resin has an amine structure (molecular weight 120,000). UA-306H: Pentaerythritol triacrylate hexamethylene diisocyanate urethane prepolymer (Kyoeisha Chemical Co., Ltd., UA-306H) DPHA: Dipentaerythritol hexaacrylate PETA: Pentaerythritol triacrylate (Example of production of resin 1) 2.4 g of 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate (Showa Denko Materials Co., Ltd., FA-711MM), 5.6 g of methyl methacrylate (Kanto Chemical Co., Ltd.), 31 g of cyclohexanone (Kanto Chemical Co., Ltd.), and 0.11 g of 2,2'-azobis(isobutyronitrile) (Fujifilm Wako Pure Chemical Industries, Ltd.) were placed in a reaction vessel and heated and stirred at 70 ° C. for 8 hours under a nitrogen gas atmosphere. Thereafter, a polymer solution was obtained by heating and stirring at 100 ° C. for 1 hour. This polymer solution was poured into 400 mL of methanol (Kanto Chemical Co., Ltd.), and the resulting precipitate was filtered and dried to obtain Resin 1, which was copolymerized with 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate and methyl methacrylate at a ratio of 15:85 [mol %]. Photopolymerization initiator: Omnirad 819: acylphosphine oxide photopolymerization initiator (manufactured by IGM Resins B.V.). Ultraviolet (UV) absorber: Tinuvin 477: hydroxyphenyltriazine-based ultraviolet absorber, Tinuvin (registered trademark) 477 (manufactured by BASF Japan Ltd.). Tinuvin 479: hydroxyphenyltriazine-based ultraviolet absorber, Tinuvin (registered trademark) 479 (manufactured by BASF Japan Ltd.). Tinuvin 970: hydroxyphenyltriazine-based ultraviolet absorber, Tinuvin (registered trademark) 970 (manufactured by BASF Japan Ltd.).Additives (anti-fouling agent) OPTOOL (registered trademark) AR-110 (manufactured by Daikin Industries, Ltd., solid content 15%, solvent: methyl isobutyl ketone) (HALS agent (hindered amine light stabilizer)) ADK STAB LA-82 (manufactured by ADEKA Corporation, molecular weight 239) Anti-glare property-imparting particles (resin particles) styrene-methyl methacrylate copolymer particles (refractive index 1.515, average particle size 2.0 μm) (inorganic fine particles) Inorganic fine particles 1: synthetic smectite Inorganic fine particles 2: alumina nanoparticles (average particle size 40 nm) Solvents MEK: methyl ethyl ketone Methyl acetate: methyl acetate Toluene: toluene IPA: isopropyl alcohol.
[0097] [Formation of Hard Coat Layer / UV Absorbing Layer] In each example, a composition for forming a hard coat layer or an ultraviolet absorbing layer shown in Table 3 was applied onto the corresponding layer and dried in an oven at 80°C for 60 seconds. Thereafter, an ultraviolet irradiation device was used to apply an irradiation dose of 150 mJ / cm. 2 The coating film was cured by irradiating it with ultraviolet light using a light source H bulb manufactured by Fusion UV Systems Japan Co., Ltd., to form a hard coat layer and an ultraviolet absorbing layer so that the film thickness after curing was 5.0 μm. The amounts added in Table 3 are mass ratios (mass %), and "-" indicates that the component is not contained.
[0098] <Low Refractive Index Layer> Details of the composition for forming the low refractive index layer are shown below. Refractive index adjuster: porous silica fine particles (average particle size 75 nm, solid content 20%) dispersion in methyl isobutyl ketone 8.5 parts by mass Antifouling agent: Optool (registered trademark) AR-110 5.6 parts by mass Active energy ray curable resin: PETA 0.4 parts by mass Photopolymerization initiator: Omnirad TPO (manufactured by IGM Resins B.V.) 0.07 parts by mass Leveling agent: RS-77 (manufactured by DIC Corporation) 1.7 parts by mass Solvent: methyl isobutyl ketone 83.73 parts by mass
[0099] [Formation of low refractive index layer] The composition for forming a low refractive index layer was applied onto the ultraviolet absorbing layer and dried in an oven at 80°C for 60 seconds. Thereafter, an ultraviolet irradiation device was used to apply an irradiation dose of 200 mJ / cm 2The coating was cured by irradiating it with ultraviolet light (H bulb light source, manufactured by Fusion UV Systems Japan Co., Ltd.) to form a low refractive index layer having a thickness of 100 nm after curing.
[0100] <Antiglare Layer> Details of the composition for forming an antiglare layer are shown below. - Active energy ray curable resin: Pentaerythritol triacrylate, Light Acrylate PE-3A (manufactured by Kyoeisha Chemical Co., Ltd., refractive index 1.52) 43.7 parts by mass - Photopolymerization initiator: Omnirad TPO 4.55 parts by mass - Resin particles: Styrene-methyl methacrylate copolymer particles (refractive index 1.515, average particle size 2.0 μm) 0.5 parts by mass - Inorganic fine particles: Synthetic smectite 0.25 parts by mass, Alumina nanoparticles (average particle size 40 nm) 1.0 part by mass - Solvent: Toluene 15 parts by mass, Isopropyl alcohol 35 parts by mass [Formation of Antiglare Layer] In the corresponding example, the composition for forming an antiglare layer was applied onto the ultraviolet absorbing layer and dried in an oven at 80°C for 60 seconds. Thereafter, an irradiation dose of 150 mJ / cm was applied using an ultraviolet irradiation device. 2 The coating was cured by irradiating it with ultraviolet light (H bulb light source, manufactured by Fusion UV Systems Japan Co., Ltd.) to form an antiglare layer having a thickness of 5.0 μm after curing.
[0101] <Antistatic and Antifouling Layer> Details of the composition for forming the antistatic and antifouling layer are shown below. Antifouling agent: Optool (registered trademark) AR-110 5.6 parts by mass. Active energy ray curable resin: PETA 0.4 parts by mass. Photopolymerization initiator: Omnirad TPO 0.07 parts by mass. Leveling agent: RS-77 1.7 parts by mass. Solvent: Methyl isobutyl ketone 91.6 parts by mass. [Formation of Antistatic and Antifouling Layer] In the corresponding example, the composition for forming the antistatic and antifouling layer was applied onto the ultraviolet absorbing layer and dried in an oven at 80°C for 60 seconds. Thereafter, the composition was exposed to an ultraviolet ray using an ultraviolet ray irradiation device at an irradiation dose of 200 mJ / cm. 2 The coating was cured by irradiating it with ultraviolet light (H bulb light source, manufactured by Fusion UV Systems Japan Co., Ltd.) to form an antistatic and antifouling layer having a thickness of 100 nm after curing.
[0102] <Oxygen Barrier Layer> As a composition for forming the oxygen barrier layer, an 80% by mass aqueous solution of PVA (Kuraray Poval (registered trademark) PVA-117 (manufactured by Kuraray Co., Ltd.)) was used. In the corresponding example, this was applied onto the colored layer and dried to form a film having an oxygen permeability of 1 cm 3 / (m 2 An oxygen barrier layer having a specific oxygen content (.times.day.atm) was formed.
[0103] <Colored Layer> Details of the materials used in the colored layer are shown below. Note that the absorption maximum wavelength, half-width, and minimum transmittance wavelength in the specified wavelength range of the colorant are values for a cured coating film with a thickness of 5 μm. <Dye (A)> First Colorant Dye-1: Pyrromethene cobalt complex dye (absorption maximum wavelength 493 nm, half-width 26 nm) <Production Example of Dye-1> 5-formyl-2,4-dimethyl-1H-pyrrole-3-ethyl carboxylate (2.5 g) was sealed in a reaction vessel and dissolved in methanol (50 mL), after which 47% hydrobromic acid (45 g) was added and refluxed for 1 hour. The precipitated solid was filtered off to obtain 3,3',5,5'-tetramethyl-4,4'-diethoxycarbonyl-2,2'-dipyrromethene hydrobromide (2.6 g). 3,3',5,5'-Tetramethyl-4,4'-diethoxycarbonyl-2,2'-dipyrromethene hydrobromide (0.6 g) was placed in a reaction vessel, and methanol (5 mL), triethylamine (0.17 g), and cobalt acetate tetrahydrate (0.18 g) were added, followed by refluxing for 2 hours. The precipitated solid was separated by filtration to obtain Dye-1 (0.42 g). Second coloring material Dye-2: tetraazaporphyrin copper complex dye (manufactured by Yamamoto Chemical Industry Co., Ltd., PD-311S, maximum absorption wavelength 586 nm, half width 22 nm) Dye-3: tetraazaporphyrin copper complex dye (manufactured by Yamada Chemical Industry Co., Ltd., FDG-007, maximum absorption wavelength 595 nm, half width 22 nm) Third coloring material Dye-4: phthalocyanine copper complex dye (manufactured by Yamada Chemical Industry Co., Ltd., FDN-002, minimum transmittance wavelength in the 380 to 780 nm range 780 nm)
[0104] <Energy ray-curable compound (B)> Resin 1: same as that used in the ultraviolet absorbing layer UA-306H DPHA PETA <Photopolymerization initiator (C)> Omnirad 819 <Solvent (D)> MEK: methyl ethyl ketone Methyl acetate <Additive (E)> D1781: singlet oxygen quencher (bis(dibutyldithiocarbamate)nickel(II), manufactured by Tokyo Chemical Industry Co., Ltd.)
[0105] [Formation of Colored Layer] In the corresponding example, the colored layer-forming composition was applied to a transparent substrate and dried in an oven at 80° C. for 60 seconds. Thereafter, an ultraviolet irradiation device was used to apply an irradiation dose of 150 mJ / cm 2 The coating was cured by irradiating it with ultraviolet light (light source H bulb, manufactured by Fusion UV Systems Japan Co., Ltd.), to form an antistatic and antifouling layer having a thickness of 5.0 nm after curing.
[0106] The optical film according to each example was evaluated as follows. [Film Property Evaluation] <UV Shielding Ratio of UV-Absorbing Layer> A layer structure of a layer above the first functional layer in each example was formed on a glass substrate, and the layer was peeled off using cellophane tape conforming to the JIS-K5600 adhesion test. The transmittance of the peeled cellophane tape was measured using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.), with the cellophane tape alone used as a reference. Using the obtained transmittance, the average transmittance [%] in the ultraviolet range (290 nm to 400 nm) was calculated, and the UV Shielding Ratio [%] was calculated by subtracting the average transmittance [%] in the ultraviolet range (290 nm to 400 nm) from 100%. The UV Shielding Ratio is preferably 90% or more, more preferably 95% or more, and may be 100%.
[0107] <Adhesion Test> In accordance with JIS K-5600 5-6:1999, 10 × 10 cross-cuts were made at 1 mm intervals on the surface of the first surface side (the side on which the functional layer was formed) of the optical film according to each example, and then an adhesive tape adhesion test was carried out to visually evaluate the remaining rate of the coating film. When the evaluation corresponded to Class 0, Class 1, or Class 2 as specified in the JIS, it was recorded as "○ (pass)", and when it corresponded to Class 3, Class 4, or Class 5, it was recorded as "× (fail)".
[0108] <Pencil Hardness Test> A pencil hardness test was conducted in accordance with JIS-K5600-5-4:1999 using a pencil (UNI, pencil hardness H, manufactured by Mitsubishi Pencil Co., Ltd.) to which a load of 500 gf (4.9 N) was applied, on the surface of the first surface of the optical film according to each example, using a Clemens scratch hardness tester (HA-301, manufactured by Tester Sangyo Co., Ltd.). Changes in appearance due to scratches were evaluated visually, and a rating of "○ (pass)" was given when no scratches were observed, and a rating of "× (fail)" was given when scratches were observed.
[0109] <Lightfastness Test> The lightfastness of the obtained optical film was tested using a xenon weather meter tester (X75, manufactured by Suga Test Instruments Co., Ltd.) at a xenon lamp illuminance of 60 W / m 2 (300 nm to 400 nm), the test was conducted for 120 hours under conditions of a temperature of 45°C and a humidity of 50% RH inside the tester. Transmittance measurements were performed before and after the test using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.), and the difference in ultraviolet shielding rate ΔT (290-400 nm) before and after the test was calculated. The closer the difference in ultraviolet shielding rate is to zero, the better, with |ΔT (290-400 nm) | ≦ 10 being preferred, and |ΔT (290-400 nm) | ≦ 5 being even more preferred. For Examples and Comparative Examples including a colored layer, the difference in transmittance ΔTλ1 before and after the test at wavelength λ1, which indicates the minimum transmittance before the test in the wavelength range of 470 nm to 530 nm, and the difference in transmittance ΔTλ2 before and after the test at wavelength λ2, which indicates the minimum transmittance before the test in the wavelength range of 560 nm to 620 nm, were also calculated. The transmittance difference is better when it is close to zero, and it is preferable that |ΔTλN|≦20 (N=1 to 2), and more preferably that |ΔTλN|≦10 (N=1 to 2).
[0110] [Evaluation of Display Device Characteristics] <White Display Transmittance Characteristics> The transmittance of the obtained optical film was measured using an automatic spectrophotometer (U-4100, manufactured by Hitachi, Ltd.), and the efficiency of light transmitted through the optical film during white display was calculated using this transmittance, which was evaluated as the white display transmittance characteristics. As a standard, the efficiency of the spectrum during white display output through a white organic EL light source and a color filter, whose spectrum is shown in FIG. 5, was set to 100. The closer to 100, the higher the white display transmittance and the more excellent the luminance efficiency. <Display Device Reflectance Characteristics> The transmittance T(λ) and surface reflectance R2(λ) of the obtained optical film were measured using an automatic spectrophotometer (U-4100). For the measurement of surface reflectance R2(λ), a matte black dye was applied to the surface of the transparent substrate on which no ultraviolet absorbing layer or the like was formed to perform an anti-reflection treatment, and the spectral reflectance at an incident angle of 5° was measured and used as the surface reflectance R2(λ). Electrode reflectance R E The relative reflectance value was calculated based on the following formulas (1) to (4) when the reflectance value of the display device for the D65 light source (CIE (International Commission on Illumination) standard light source D65) without the optical film was taken as 100, and the surface reflectance R(λ) of the outermost layer on the observer side was used to evaluate the display device's reflectance characteristics. The lower the reflectance value of the display device, the more external light reflection can be reduced and the better the reflectance characteristics. In formulas (1) to (4), R1(λ) represents the internal reflection component, Y represents one of the tristimulus values at the white point of the D65 light source, and P D65 (λ) represents the spectrum of the D65 light source, and the overline y(λ) represents the CIE1931 color matching function.
[0111]
[0112] For the Examples and Comparative Examples that included a colored layer, color reproducibility was further evaluated using the following procedure. <Color Reproducibility> The transmittance of the obtained optical film was measured using an automatic spectrophotometer (U-4100), and the red, green, and blue display spectra of FIG. 6 output through a white EL light source and a color filter were measured. The vertical axes of the graphs in FIGS. 5 and 6 represent luminous intensity [a.u.] (arbitrary unit). The NTSC (National Television System Committee) ratio was calculated from the CIE 1931 chromaticity values calculated using the measured transmittance and the red, green, and blue display spectra of FIG. 6, and the NTSC ratio was used as an index of color reproducibility for evaluation. The higher the NTSC ratio, the better the color reproducibility.
[0113] The results are shown in Tables 5 to 9. The white display transmission characteristics and the display device reflection characteristics are also shown as a ratio with Comparative Example 1, which does not have a colored layer, as the reference (100%).
[0114]
[0115]
[0116]
[0117]
[0118]
[0119] The results of Example 2, Comparative Example 1, and Comparative Example 2 demonstrated that adhesion was improved when the radical scavenging compound in the UV-absorbing layer contained a structural unit represented by formula (i). The results of Example 2 and Comparative Example 3, in which the amount of photopolymerization initiator in the UV-absorbing layer was reduced compared to Example 2, demonstrated that sufficient photopolymerization was necessary for the optical film to have sufficient surface hardness. The results of Examples 2 and 3 demonstrated that antistatic, antifouling, and antiglare properties could be imparted to the UV-absorbing layer while maintaining physical properties. The results of Examples 4 to 13 demonstrated that satisfactory physical properties could be achieved even when a second functional layer, such as a low refractive index layer, an antistatic / antifouling layer, or an antiglare layer, was provided separately from the UV-absorbing layer. The results of Example 8, Comparative Example 4, and Comparative Example 5, which included a colored layer, demonstrated that an optical film having a UV-absorbing layer containing a structural unit represented by formula (i) could improve the light resistance of the colored layer. This was thought to be due to the UV-absorbing layer in Comparative Example 5, in which the UV-absorbing layer did not contain a structural unit represented by formula (i), deteriorating more rapidly than in Example 8. The results of Examples 8 and 10 showed that providing an oxygen barrier layer as a second functional layer further improved the light resistance of the colored layer. The results of Example 8 (a sample having a colored layer), Example 11 (a sample containing Resin 1 in the colored layer), and Example 12 (a sample containing Resin 1 and a singlet oxygen quencher in the colored layer) showed that the light resistance of the colored layer improved when the colored layer contained a radical scavenger or a singlet oxygen quencher. The results of Example 8 (substrate: TAC) and Example 13 (substrate: PMMA) showed that optical films satisfying the required physical and optical properties could be produced using transparent substrates other than TAC.
[0120] In the display devices employing the optical films according to Examples 7 to 9, which have a colored layer as the first functional layer, the reflection characteristics were significantly improved compared to the display device employing the optical film according to Example 1, which does not have a colored layer. It is generally said that the transmittance is halved in display devices equipped with a circular polarizer, whereas the display devices employing the optical films according to Examples 7 to 9 exhibited excellent luminance efficiency, as indicated by the evaluation value of white display transmittance, and also improved color reproducibility. The results of Examples 7 to 9 indicated a tendency for the reflection characteristics to be excellent as the absorption wavelength band becomes wider.
[0121] 1, 2, 3, 4 Optical film 10 Transparent substrate 20 Hard coat layer (first functional layer) 30 Ultraviolet absorbing layer 40 Second functional layer 50 Colored layer (first functional layer)
Claims
1. An optical film comprising: a first functional layer; an ultraviolet absorbing layer located on a first surface of the first functional layer; and a transparent substrate located on a second surface of the first functional layer, wherein the ultraviolet absorbing layer contains an active energy ray curable resin and an ultraviolet absorber, and the active energy ray curable resin contains a copolymer of a structural unit represented by the following formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit, wherein the ultraviolet ray shielding rate measured in accordance with JIS L1925 is 90% or more, and the pencil hardness under a 500 g load of the surface on the first surface side is H or more. [In formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.
2. The optical film according to claim 1, wherein the ultraviolet absorbing layer has one or more functions of antistatic property, antifouling property and antiglare property.
3. The optical film according to claim 1, further comprising a second functional layer provided on the first surface side of the first functional layer and having a function different from that of the first functional layer.
4. The optical film according to claim 3, wherein the second functional layer has at least one of an anti-reflection function and an anti-glare function.
5. The optical film according to claim 3, wherein the second functional layer is an antistatic layer or an antifouling layer.
6. The second functional layer has an oxygen permeability of 10 cm 3 / (m 2 The optical film according to claim 3 , wherein the oxygen barrier layer has a resistance of 0.5 to 100 MPa (100 MPa) or less.
7. The optical film according to claim 1, wherein the first functional layer contains at least one of a first color material, a second color material, and a third color material, wherein the first color material has a maximum absorption wavelength in the range of 470 to 530 nm and a half-width of an absorption spectrum of 15 to 45 nm, the second color material has a maximum absorption wavelength in the range of 560 to 620 nm and a half-width of an absorption spectrum of 15 to 55 nm, and the third color material has a wavelength in the range of 380 to 780 nm with the lowest transmittance in the range of 650 to 780 nm.
8. The optical film according to claim 7, wherein the first functional layer contains a copolymer of a structural unit represented by formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit.
9. The optical film according to claim 7, wherein the first functional layer contains at least one of a radical scavenger, a peroxide decomposer, and a singlet oxygen quencher.
10. The optical film according to claim 9, wherein the singlet oxygen quencher contains any one of dialkyl phosphate, dialkyl dithiocarbamate, benzenedithiol, and transition metal complexes thereof.
11. The optical film according to claim 7, wherein at least one of the first color material, the second color material, and the third color material contained in the first functional layer comprises at least one compound selected from the group consisting of compounds having any of a porphyrin structure, a merocyanine structure, a phthalocyanine structure, an azo structure, a cyanine structure, a squarylium structure, a coumarin structure, a polyene structure, a quinone structure, a tetradiporphyrin structure, a pyrromethene structure, and an indigo structure, and metal complexes thereof.
12. A display device comprising the optical film according to any one of claims 1 to 11.
13. A composition for forming an ultraviolet absorbing layer, comprising an ultraviolet absorber, an active energy ray curable resin, a photopolymerization initiator, and a solvent, wherein the active energy ray curable resin contains a copolymer of a structural unit represented by formula (i) and a structural unit having any one of a (meth)acrylate-based repeating unit, an olefin-based repeating unit, a halogen atom-containing repeating unit, a styrene-based repeating unit, a vinyl acetate-based repeating unit, and a vinyl alcohol-based repeating unit, and when a film having a thickness of 5 μm is formed, the film has an ultraviolet ray shielding rate of 90% or more as measured in accordance with the method described in JIS L1925. [In formula (i), R 1 represents a hydrogen atom, a halogen atom, a carboxyl group, a sulfo group, a cyano group, a hydroxy group, an alkyl group having 10 or less carbon atoms, an alkoxycarbonyl group having 10 or less carbon atoms, an alkylsulfonylaminocarbonyl group having 10 or less carbon atoms, an arylsulfonylaminocarbonyl group, an alkylsulfonyl group, an arylsulfonyl group, an acylaminosulfonyl group having 10 or less carbon atoms, an alkoxy group having 10 or less carbon atoms, an alkylthio group having 10 or less carbon atoms, an aryloxy group having 10 or less carbon atoms, a nitro group, an alkoxycarbonyloxy group, an aryloxycarbonyloxy group, an acyloxy group having 10 or less carbon atoms, an acyl group having 10 or less carbon atoms, a carbamoyl group, a sulfamoyl group, an aryl group having 10 or less carbon atoms, a substituted amino group, a substituted ureido group, a substituted phosphono group, or a heterocyclic group; R 2 represents a hydrogen atom or an alkyl group having 30 or less carbon atoms, and X represents a single bond, an ester group, an aliphatic alkyl chain having 30 or less carbon atoms, an aromatic chain, a polyethylene glycol chain, or a linking group formed by combining these, any of which may contain a spirodioxane ring.
Citation Information
Patent Citations
Composition for coloring layer formation, optical film and display device
JP2023032001A
Decorative film and method for manufacturing same, and decorative molded article
WO2017051539A1