Resin composition
The combination of β-methyl-δ-valerolactone and 3-hydroxyalkanoate polymers in a specific ratio and molecular weight range addresses the brittleness and impact resistance issues of 3-hydroxyalkanoate polymers, resulting in a resin composition with improved impact resistance and practicality for diverse applications.
Patent Information
- Application Number
- PCT/JP2024/016164
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-24
- Publication Date
- 2024-10-31
AI Technical Summary
Molded bodies made of 3-hydroxyalkanoate polymers are brittle and have inferior impact resistance compared to petroleum-based plastics, limiting their use as resin materials, despite efforts to improve tensile elongation and tear strength through blending with polycaprolactone resin.
A resin composition comprising a β-methyl-δ-valerolactone polymer and a 3-hydroxyalkanoate polymer, with specific molecular weight ranges and ratios, enhances impact resistance by incorporating 5 to 20 parts by mass of β-methyl-δ-valerolactone polymer with 3-hydroxyalkanoate polymer, optimizing molecular weights and distribution for improved handling and molding properties.
The resin composition achieves good impact resistance and practicality, with the β-methyl-δ-valerolactone polymer contributing to enhanced mechanical properties when blended with 3-hydroxyalkanoate polymers, making them suitable for various molded articles.
Smart Images

Figure JP2024016164_31102024_PF_FP_ABST
Abstract
Description
resin composition
[0001] The present invention relates to a resin composition containing a β-methyl-δ-valerolactone polymer and a 3-hydroxyalkanoate polymer.
[0002] From the viewpoint of global environmental conservation, there is a demand in a wide range of fields for reducing the environmental impact of plastic materials used in products. In order to reduce the environmental impact, plastic materials using 3-hydroxyalkanoate polymers, which are a type of "biodegradable plastic," have been developed. However, molded articles made from 3-hydroxyalkanoate polymers tend to be more brittle and have inferior flexibility and impact resistance compared to petroleum-based plastics, which may limit their use as resin materials.
[0003] For example, a technology relating to a resin composition containing a 3-hydroxyalkanoate polymer having a 3-hydroxybutyrate ratio of 80 mol % or more and a polycaprolactone resin (PCL) has been disclosed (Patent Document 1). Patent Document 1 describes that by mixing a 3-hydroxyalkanoate polymer with PCL, the tensile elongation and tear strength are improved compared to those of the 3-hydroxyalkanoate polymer alone.
[0004] Japanese Patent Application Laid-Open No. 2017-222791
[0005] However, although the resin composition described in Patent Document 1 has improved impact resistance compared to a resin composition containing a 3-hydroxyalkanoate polymer alone, the impact resistance is not fully satisfactory. Therefore, an object of the present invention is to provide a resin composition having good impact resistance.
[0006] As a result of intensive research to solve the above problems, the present inventors have conceived the following invention and found that the above problems can be solved.
[0007] [1] A resin composition containing a β-methyl-δ-valerolactone polymer represented by the following general formula (I-a) or (I-b) and a 3-hydroxyalkanoate polymer represented by the following general formula (II): [In general formula (I-a), n is 5 to 20. In general formula (I-b), l and m are each independently 2 to 10.] [In general formula (II), the ratio of k to p (k / p) is 70 / 30 to 99 / 1.] [2] The resin composition according to [1] above, containing 5 to 20 parts by mass of the β-methyl-δ-valerolactone polymer per 100 parts by mass of the 3-hydroxyalkanoate polymer. [3] The resin composition according to [1] or [2] above, wherein the number-average molecular weight of the β-methyl-δ-valerolactone polymer is 1,000 to 4,000. [4] The resin composition according to any one of [1] to [3] above, wherein the weight-average molecular weight of the 3-hydroxyalkanoate polymer is 50,000 to 3,000,000. [5] The resin composition according to any one of [1] to [4] above, wherein the β-methyl-δ-valerolactone polymer is represented by general formula (I-a). [6] The resin composition according to any one of [1] to [4], wherein the β-methyl-δ-valerolactone polymer is represented by the general formula (I-b).
[0008] According to the present invention, it is possible to provide a resin composition having good impact resistance.
[0009] The following is a description based on one example of an embodiment of the present invention. However, the embodiment shown below is an example for embodying the technical idea of the present invention, and the present invention is not limited to the following description. Furthermore, although preferred embodiments are shown in this specification, a combination of two or more of the individual preferred embodiments is also a preferred embodiment. For matters shown as numerical ranges, when there are several numerical ranges, the lower limit and upper limit can be selectively combined to form a preferred embodiment. Furthermore, in this specification, when a numerical range is described as "XX to YY," it means "XX or more and YY or less."
[0010] <Resin Composition> The resin composition of this embodiment contains a β-methyl-δ-valerolactone polymer represented by general formula (I-a) or (I-b) and a 3-hydroxyalkanoate polymer containing a structure represented by general formula (II). By containing a β-methyl-δ-valerolactone polymer represented by general formula (I-a) or (I-b) and a 3-hydroxyalkanoate polymer containing a structure represented by general formula (II), the resin composition has good impact resistance.
[0011] [β-Methyl-δ-valerolactone Polymer] The β-methyl-δ-valerolactone polymer of this embodiment is represented by the following general formula (Ia) or (Ib).
[0012]
[0013] <n, m, l> In general formulas (I-a) and (I-b), n, m, and l represent the average number of repeating units. n is 5 to 20, and in one embodiment of the present invention, it is preferably 5 to 18, more preferably 5 to 15, and in another embodiment of the present invention, it is preferably 10 to 20, more preferably 12 to 20. m is 2 to 10, preferably 2 to 9, more preferably 2 to 7. l is 2 to 10. It is preferably 2 to 9, more preferably 2 to 7. m+l is preferably 4 to 18, more preferably 4 to 14. In this specification, "n, m, and l" represent the following: 1 It is a value calculated from the ratio of the integrated value of the proton number of the initiator structure to the integrated value of the proton number of the repeating unit structure, which are determined by H-NMR measurement. The detailed measurement method can be according to the method described in the Examples.
[0014] <Number Average Molecular Weight (Mn)> The number average molecular weight of the β-methyl-δ-valerolactone polymer is preferably 1,000 to 4,000, more preferably 1,500 to 3,000, and even more preferably 1,800 to 2,500. When the number average molecular weight of the β-methyl-δ-valerolactone polymer is within the above range, the viscosity of the resin composition does not become too low, resulting in good handleability and productivity during molding. All "number average molecular weights" described in this specification are number average molecular weights calculated in terms of standard polystyrene as determined by gel permeation chromatography (GPC). Detailed measurement methods can be performed according to the methods described in the Examples.
[0015] <Weight Average Molecular Weight (Mw)> The weight average molecular weight of the β-methyl-δ-valerolactone polymer is preferably 1,500 to 8,000, more preferably 1,500 to 6,000, and even more preferably 2,000 to 5,000. When the weight average molecular weight of the β-methyl-δ-valerolactone polymer is within the above range, the viscosity of the resin composition does not become too low, resulting in good handling during molding and improved productivity. All "weight average molecular weights" described in this specification are weight average molecular weights calculated in terms of standard polystyrene as determined by gel permeation chromatography (GPC). Detailed measurement methods can be performed according to the methods described in the Examples.
[0016] <Molecular Weight Distribution (Mw / Mn)> The molecular weight distribution (Mw / Mn) of the β-methyl-δ-valerolactone polymer is preferably 1.0 to 3.0, more preferably 1.0 to 2.6, even more preferably 1.1 to 2.5, still more preferably 1.1 to 2.0, and even more preferably 1.2 to 1.8. All "molecular weight distributions" described in this specification are values calculated from the number average molecular weight and weight average molecular weight in terms of standard polystyrene determined by gel permeation chromatography (GPC) measurement. Detailed methods for measuring the number average molecular weight and weight average molecular weight can be according to the methods described in the Examples.
[0017] In one embodiment of the present invention, the β-methyl-δ-valerolactone polymer is preferably represented by general formula (Ia): In another embodiment of the present invention, the β-methyl-δ-valerolactone polymer is preferably represented by general formula (Ib):
[0018] <Production Method> The β-methyl-δ-valerolactone polymer of this embodiment is preferably produced by a production method including a step of adding a terminal modifier to a reaction solution obtained by reacting β-methyl-δ-valerolactone, an alcohol compound, and a base catalyst to perform a terminal modification reaction (hereinafter also referred to as the "reaction step"). This production method is characterized by adding the terminal modifier directly to the reaction solution obtained by reacting β-methyl-δ-valerolactone, an alcohol compound, and a base catalyst. That is, after ring-opening polymerization of β-methyl-δ-valerolactone, the terminal modifier can be added to the reactor in which the ring-opening polymerization was performed without first removing the ring-opened polymer, thereby performing terminal modification of the ring-opened polymer. Because the reaction step involves performing the ring-opening polymerization reaction and the terminal modification reaction in one pot, this production method can be considered a simplified process. It should be noted that the β-methyl-δ-valerolactone polymer of this embodiment is not limited to the production method described above.
[0019] (Alcohol Compound) The alcohol compounds that can be used in this embodiment are isoamyl alcohol and ethylene glycol. When isoamyl alcohol is used as the alcohol compound, a β-methyl-δ-valerolactone polymer represented by general formula (I-a) can be obtained, and when ethylene glycol is used as the alcohol compound, a β-methyl-δ-valerolactone polymer represented by general formula (I-b) can be obtained.
[0020] (Base Catalyst) Examples of base catalysts that can be used in this embodiment include metal catalysts such as alkali metals and alkali metal compounds, as well as organic base compounds. A single base catalyst may be used alone, or two or more may be used in combination. Examples of alkali metal compounds include organic alkali metal compounds, alkali metal hydroxide compounds, and alkali metal hydrides, with organic lithium compounds such as butyllithium being preferred. Examples of organic base compounds include amine compounds having an amidine skeleton or a guanidine skeleton. Metal catalysts such as organomagnesium compounds and organozinc compounds can also be used as base catalysts. In the reaction step, it is preferable to add 0.005 to 1.5 molar equivalents of the base catalyst relative to the hydroxyl groups of the alcohol compound.
[0021] (β-Methyl-δ-valerolactone) The β-methyl-δ-valerolactone that can be used in this embodiment can be produced by a known method. For example, it can be produced by a known method using 2-hydroxy-4-methyltetrahydropyran or the like as a raw material (Japanese Patent Publication No. 6-53691, etc.). In addition, commercially available β-methyl-δ-valerolactone can be used, and it can be derived from either petroleum or biomass. In the reaction step, it is preferable to add 5 to 50 molar equivalents of β-methyl-δ-valerolactone relative to the hydroxyl groups of the alcohol compound.
[0022] (Terminal Modifier) In this embodiment, acetic anhydride is used as the terminal modifier. In the reaction step, it is preferable to add 1.0 to 20.0 molar equivalents of acetic anhydride as the terminal modifier relative to the hydroxyl groups of the alcohol compound.
[0023] (Co-catalyst) In the reaction step, a co-catalyst may be added as necessary. Examples of the co-catalyst that can be used include amine compounds such as triethylamine, tributylamine, trioctylamine, imidazole, pyridine, aminopyridine, and 4-dimethylaminopyridine. In the reaction step, the co-catalyst can be added in an amount of 0.001 to 10 molar equivalents relative to the hydroxyl groups of the alcohol compound.
[0024] (Solvent) The reaction step can be carried out in the presence of a solvent inert to the ring-opening polymerization reaction. Examples of the solvent include aliphatic hydrocarbons such as cyclohexane, methylcyclohexane, n-hexane, and n-pentane; and aromatic hydrocarbons such as benzene, toluene, and xylene.
[0025] (Reaction Conditions) In the reaction step, the reaction temperature when reacting β-methyl-δ-valerolactone, the alcohol compound, and the base catalyst may usually be 20 to 100°C, and the reaction time may usually be 1 minute to 24 hours. In addition, in the reaction step, the reaction temperature when carrying out the terminal modification reaction after adding the terminal modifying agent to the reaction solution may usually be 20 to 80°C, and the reaction time may usually be 1 minute to 24 hours.
[0026] (Post-treatment step) The polymer of this embodiment can be produced by going through the above reaction step. If necessary, a post-treatment step may be carried out to isolate the produced polymer. As the post-treatment step, a suitable method can be adopted from known methods. For example, the reaction mixture after the reaction step can be washed with a reaction solvent or water, concentrated, and purified by a method typically used for separating and purifying organic compounds, such as distillation.
[0027] [3-Hydroxyalkanoate Polymer] The 3-hydroxyalkanoate polymer of the present embodiment is represented by the following general formula (II).
[0028]
[0029] <k / p> The ratio of k to p (k / p) represents the ratio of each structural unit and is 70 / 30 to 99 / 1. When k / p is 70 / 30 or more, molded articles produced using the resin composition have sufficient strength and are highly practical, while when k / p is 99 / 1 or less, the resin composition exhibits good impact resistance. In this specification, "k and p" are values determined by gas chromatography measurement using the following method. 2 ml of a sulfuric acid-methanol mixture (15:85) and 2 ml of chloroform are added to 20 mg of a 3-hydroxyalkanoate polymer, the container is sealed, and heated at 100°C for 140 minutes to obtain a methyl ester of a 3-hydroxyalkanoate polymer decomposition product. After cooling, 1.5 g of sodium bicarbonate is added little by little to neutralize the mixture, and the mixture is left to stand until carbon dioxide generation ceases. Subsequently, 4 ml of diisopropyl ether was added and mixed thoroughly, followed by centrifugation, and the monomer unit composition ratio of the polyester decomposition product in the supernatant was analyzed under the following measurement conditions: (Measurement Conditions) Apparatus: Gas chromatograph GC-17A (Shimadzu Corporation) Capillary column: NEUTRA BOND-1 (GL Sciences Inc., column length 25 m, column inner diameter 0.25 mm, liquid film thickness 0.4 μm)
[0030] <Number Average Molecular Weight (Mn)> The number average molecular weight of the 3-hydroxyalkanoate polymer is preferably 20,000 to 1,000,000, and more preferably 50,000 to 700,000. When the number average molecular weight is within the above range, the viscosity of the resin composition is prevented from becoming too low or too high, improving the handleability and productivity during molding.
[0031] <Weight-average molecular weight (Mw)> The weight-average molecular weight of the 3-hydroxyalkanoate polymer is preferably 50,000 to 3,000,000, and more preferably 100,000 to 1,500,000. When the weight-average molecular weight is within the above range, the viscosity of the resin composition is prevented from becoming too low or too high, improving the handling properties and productivity during molding.
[0032] <Molecular Weight Distribution (Mw / Mn)> The molecular weight distribution (Mw / Mn) of the 3-hydroxyalkanoate polymer is preferably 1.0 to 3.0, more preferably 1.1 to 2.0, and even more preferably 1.2 to 1.8.
[0033] <Production Method> The 3-hydroxyalkanoate polymer of this embodiment is preferably produced by a microorganism, i.e., obtained by a fermentation synthesis method. Microorganisms that can be used in this fermentation synthesis method are not particularly limited as long as they are capable of producing a 3-hydroxyalkanoate polymer. Known examples of bacteria that produce 3-hydroxyalkanoate polymers include Aeromonas caviae and Alcaligenes eutrophus, which produces poly(3-hydroxybutyrate-co-4-hydroxybutyrate). From the viewpoint of productivity, Alcaligenes eutrophus AC32 strain (FERM BP-6038) (J. Bateriol., 179, pp. 4821-4830 (1997)) into which genes of a group of synthetic enzymes have been introduced is more preferred, and microbial cells obtained by culturing these microorganisms under appropriate conditions and allowing 3-hydroxyalkanoate polymers to accumulate in the cells may also be used.
[0034] Carbon sources and culture conditions used in culturing microorganisms capable of producing 3-hydroxyalkanoate polymers are described in, for example, Japanese Patent Application Laid-Open Nos. 5-93049 and 2001-340078. For example, fats and oils such as vegetable oils and fish oils are used as carbon sources, and the culture is carried out under limited nutrients other than the carbon source, such as nitrogen, phosphorus, and minerals, to produce 3-hydroxyalkanoate polymers as storage substances inside the microbial cells. Culture conditions such as pH, temperature, aeration, and culture time are appropriately adjusted.
[0035] The resin composition of this embodiment preferably contains 5 to 20 parts by mass, more preferably 10 to 20 parts by mass, of the β-methyl-δ-valerolactone polymer per 100 parts by mass of the 3-hydroxyalkanoate polymer. This content ratio allows the resin composition to have better impact resistance.
[0036] The total content of the β-methyl-δ-valerolactone polymer and the 3-hydroxyalkanoate polymer in the resin composition of this embodiment is preferably 80% by mass or more, more preferably 85% by mass or more, even more preferably 90% by mass or more, still more preferably 95% by mass or more, still more preferably 98% by mass or more, and may be 100% by mass. At this content, the effects of the present invention are more significantly exhibited.
[0037] The content of the β-methyl-δ-valerolactone polymer in the resin composition of this embodiment is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 20% by mass or less, more preferably 18% by mass or less. That is, the content of the β-methyl-δ-valerolactone polymer in the resin composition of this embodiment is preferably 5 to 20% by mass, more preferably 10 to 18% by mass. With the above content, the effects of the present invention are more significantly exhibited.
[0038] The content of the 3-hydroxyalkanoate polymer in the resin composition of this embodiment is preferably 80% by mass or more, more preferably 82% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less. That is, the content of the 3-hydroxyalkanoate polymer in the resin composition of this embodiment is preferably 80 to 95% by mass, more preferably 82 to 90% by mass. With this content, the effects of the present invention are more significantly exhibited.
[0039] [Additives] The resin composition of this embodiment may contain additives other than the β-methyl-δ-valerolactone polymer and the 3-hydroxyalkanoate polymer. Examples of additives include inorganic fillers, softeners, heat aging inhibitors, antioxidants, hydrolysis resistance inhibitors, light stabilizers, antistatic agents, release agents, flame retardants, foaming agents, pigments, dyes, brighteners, UV absorbers, and lubricants. These may be used alone or in combination of two or more. When using the above additives, the content of the additives in the resin composition may be determined appropriately depending on the desired physical properties of the resin composition.
[0040] [Method for Producing Resin Composition] The method for producing the resin composition of this embodiment is not particularly limited; it is sufficient to uniformly mix the β-methyl-δ-valerolactone polymer, the 3-hydroxyalkanoate polymer, and, if necessary, additives. Examples of mixing methods include melt-kneading using a single-screw extruder, multi-screw extruder, Banbury mixer, heated roll, Brabender, various kneaders, etc., or melt-kneading by feeding each component through separate inlets. Pre-blending may also be performed before melt-kneading. Examples of pre-blending methods include using a mixer such as a Henschel mixer, high-speed mixer, V-blender, ribbon blender, tumbler blender, or conical blender. The temperature during melt-kneading is preferably limited to approximately 185°C, taking into account the melting point and decomposition temperature of the 3-hydroxyalkanoate polymer. Therefore, the temperature may be, for example, approximately 100 to 185°C, or may be selected arbitrarily within the range of 120 to 180°C.
[0041] <Molded Article> By using the resin composition of this embodiment, a molded article having good impact resistance can be obtained. The shape of the molded article may be any molded article that can be produced using the resin composition of this embodiment. Examples of molded articles include molded articles of various shapes such as pellets, films, sheets, plates, pipes, tubes, bottles, fibrous bodies, rod-shaped bodies, fine particles, particulate bodies, and foams. The method for producing this molded article is not particularly limited, and it can be molded by various known molding methods, such as injection molding, blow molding, press molding, extrusion molding, calendar molding, and molding using a 3D printer.
[0042] <Applications> The β-methyl-δ-valerolactone polymer represented by the above general formula (I-a) or (I-b) can be mixed with a 3-hydroxyalkanoate polymer to form a resin composition having improved impact resistance. Therefore, the β-methyl-δ-valerolactone polymer represented by the above general formula (I-a) or (I-b) is useful as a modifier for 3-hydroxyalkanoate polymers.
[0043] The present invention will be specifically explained below with reference to examples and comparative examples, but the present invention is not limited to these.
[0044] <Measurement and Evaluation Methods> Various physical properties were measured or evaluated by the following methods.
[0045] [Average Degree of Polymerization of β-methyl-δ-valerolactone Polymer] In the Production Examples, the degree of polymerization of the terminally modified β-methyl-δ-valerolactone polymer obtained was 1 The proton signal of the initiator alcohol determined by H-NMR measurement was used as a reference and the proton signal of the repeating unit of the polymer was used as a reference. The specific measurement method was as follows. (Measurement conditions) Apparatus: 400YH (manufactured by JEOL Ltd.) Solvent: deuterated chloroform (CDCl 3 ) Measurement temperature: 23°C (Method for calculating degree of polymerization) In the case of Production Example I-1, the terminal CH of isoamyl alcohol, which is the initiator, 3 (0.9-0.92 ppm, d) Proton number X and methyl branch CH of β-methyl-δ-valerolactone, which is a repeating structural unit3 Using the number of protons Y of (0.98-1.00 ppm, d), n was calculated by the following formula (1): n=2×Y / X (1) In the case of Production Example I-2, the CH 2 (4.28-4.30 ppm, m) proton number X' and the methyl branch CH of β-methyl-δ-valerolactone, which is a repeating structural unit 3 Using the number of protons Y' of (0.98-1.00 ppm, d), l+m was calculated using the following formula (2): l+m=4×Y' / (3×X') (2)
[0046] [k / p of 3-hydroxyalkanoate polymer] The k / p of the 3-hydroxyalkanoate polymer (P3HB3HH-1) was determined by gas chromatography. The specific measurement method is as follows. 2 ml of a sulfuric acid-methanol mixture (15:85) and 2 ml of chloroform were added to 20 mg of P3HB3HH-1 obtained in Production Example, and the mixture was sealed and heated at 100°C for 140 minutes to obtain a methyl ester of a 3-hydroxyalkanoate polymer decomposition product. After cooling, 1.5 g of sodium bicarbonate was added little by little to neutralize the mixture, and the mixture was left to stand until carbon dioxide gas generation ceased. Subsequently, 4 ml of diisopropyl ether was added and mixed well, followed by centrifugation, and the monomer unit composition ratio of the polyester decomposition product in the supernatant was analyzed under the following measurement conditions. (Measurement conditions) Apparatus: Gas chromatograph GC-17A (Shimadzu Corporation) Capillary column: NEUTRA BOND-1 (GL Sciences Inc., column length 25 m, column inner diameter 0.25 mm, liquid film thickness 0.4 μm)
[0047] [Number-average molecular weight and weight-average molecular weight of β-methyl-δ-valerolactone polymer] Using a polymer obtained after a terminal modification reaction of a β-methyl-δ-valerolactone polymer as a sample, the number-average molecular weight (Mn) and weight-average molecular weight (Mw) of the β-methyl-δ-valerolactone polymer were determined by gel permeation chromatography (GPC) using standard polystyrene equivalent molecular weights. The specific measurement method is as follows. A tetrahydrofuran (THF) solution was used as the eluent, and 10 mg of the sample, calculated as resin, was weighed out and dissolved in 1 mL of the eluent. The solution was passed through a 0.2 μm membrane filter to prepare a measurement sample. The specific measurement method is as follows. (Measurement conditions) Apparatus: HLC-EcoSEC8320GPC (manufactured by Tosoh Corporation) Column: Three columns, KF-803 (manufactured by Resonac Corporation), KF-802.5 (manufactured by Resonac Corporation), and KF-802 (manufactured by Resonac Corporation), were connected in series. Eluent: tetrahydrofuran Flow rate: 0.9 mL / min Sample injection amount: 30 μL Column temperature: 40°C Standard polystyrene: PSt Oligomer Kit (molecular weight 589 to 98,900) manufactured by Tosoh Corporation was used for cubic approximation. Detector: RI detector
[0048] [Weight-average molecular weight of 3-hydroxyalkanoate polymer] The weight-average molecular weight (Mw) of the 3-hydroxyalkanoate polymer was determined by gel permeation chromatography (GPC) in terms of standard polystyrene. The specific measurement method is as follows. (Measurement conditions) Apparatus: High-performance liquid chromatograph LC-20A (Shimadzu Corporation) Column: K-G 4A (1 column) and K-806M (2 columns) (Resonac Corporation) were connected in series. Eluent: Chloroform Flow rate: 1.0 mL / min Sample injection amount: 100 μL Column temperature: 40°C Standard polystyrene: Polystyrene standard (molecular weight: 2,880 to 6,570,000) manufactured by Agilent Technologies Inc. was used for quintic approximation. Detector: RI detector
[0049] [Impact Resistance Test] (1) Preparation of Test Pieces for Impact Resistance Test The resin compositions (pellets) obtained in the Examples and Comparative Examples were placed in an injection molding machine (Shibaura Machine Co., Ltd., "SI-30IV-CCH150B"), and molded into a 80 x 80 mm, 1 mm thick plate-shaped molded body at a cylinder temperature of 120 to 150 ° C (exit resin temperature 160 ° C) and a mold set temperature of 35 ° C. The obtained plate-shaped molded body was cut into a size of 40 x 40 mm to prepare a test piece. (2) Impact Resistance Test The obtained test piece was evaluated for impact resistance in accordance with JIS K 7211-1:2006 using a DuPont drop impact tester (manufactured by Yasuda Seiki Seisakusho Co., Ltd.). When a 2 kg weight was dropped from a height of 100 cm, if the test piece was not destroyed, it was evaluated as "G", and if the test piece was destroyed, it was evaluated as "NG".
[0050] [Production Example I-1] A 500 mL four-necked glass flask was purged with nitrogen, and 7.9 g (90 mmol) of isoamyl alcohol and 231 g (2.025 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 0.84 mL of n-butyllithium (1.6 M hexane solution) was added and stirred at 60°C for 60 minutes. Next, 11.0 g (108 mmol) of acetic anhydride and 0.55 g (4.5 mmol) of 4-dimethylaminopyridine dissolved in 5.5 g of β-methyl-δ-valerolactone were added to the four-necked glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a β-methyl-δ-valerolactone polymer. The reaction solution containing the obtained β-methyl-δ-valerolactone polymer was extracted with toluene and water and purified using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 155 g of β-methyl-δ-valerolactone polymer. The obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-1") is represented by the aforementioned general formula (I-a). The physical properties of the obtained PMVL-1 were also measured as described above. The results are shown in Table 1.
[0051] [Production Example I-2] A 500 mL four-neck glass flask was purged with nitrogen, and 11.3 g (183 mmol) of ethylene glycol and 184 g (1.616 mol) of β-methyl-δ-valerolactone were added and heated to 60°C. 1.18 mL of n-butyllithium (1.6 M hexane solution) was added thereto and stirred at 60°C for 60 minutes. Next, 44.2 g (433 mmol) of acetic anhydride and 2.23 g (18.3 mmol) of 4-dimethylaminopyridine dissolved in 20.8 g of β-methyl-δ-valerolactone were added to the four-neck glass flask and stirred at 60°C for 60 minutes to obtain a reaction solution containing a β-methyl-δ-valerolactone polymer. The reaction solution containing the obtained β-methyl-δ-valerolactone polymer was extracted with toluene and water and purified using a thin-film evaporator ("Molecular Distillation Apparatus MS-300" manufactured by Shibata Scientific Co., Ltd.), yielding 161 g of β-methyl-δ-valerolactone polymer. The obtained β-methyl-δ-valerolactone polymer (hereinafter sometimes referred to as "PMVL-2") is represented by the aforementioned general formula (I-b). The physical properties of the obtained PMVL-2 were also measured as described above. The results are shown in Table 1.
[0052] [Production Example II] Alcaligenes eutrophus AC32 (Accession No. FERM BP-6038), into which Aeromonas caviae-derived polyhydroxyalkanoate synthase genes had been introduced, was cultured by the method described in Example 1 of JP-A 2001-340078 to produce a 3-hydroxyalkanoate polymer. That is, Alcaligenes eutrophus AC32 (Accession No. FERM BP-6038) (hereinafter abbreviated as "AC32 strain") was cultured as follows. The composition of the medium was 1 w / v% meat extract, 1 w / v% Bacto-Trypton, 0.2 w / v% yeast extract, and 0.9 w / v% Na. 2 HPO4・12H 2 O, 0.15w / v% KH 2 P.O. 4The composition of the polyester production medium was 1.1 w / v% Na 2 HPO 4 ・12H 2 O, 0.19w / v% KH 2 P.O. 4 , 0.6w / v% (NH 4 ) 2 SO 4 , 0.1w / v% MgSO 4 ・7H 2 0, 0.5 v / v% trace metal salt solution (1.6 w / v% FeCl in 0.1 N hydrochloric acid) 3 ・6H 2 O, 1w / v% CaCl 2 ・2H 2 O, 0.02w / v% CoCl 2 ・6H 2 O, 0.016w / v% CuSO 4 ・5H 2 O, 0.012w / v% NiCl 3 ・6H 2 O, 0.01w / v% CrCl 3 ・6H 2 O dissolved in water), 2 w / v% Proex AP-12 (manufactured by Banshu Seasoning Co., Ltd.), 5 × 10 -6The culture medium was oil-based, with palm oil, palm kernel oil, or coconut oil (4 w / v%) added in three separate portions. A glycerol stock of AC32 strain was inoculated into a preculture medium and cultured for 20 hours. A 10-L jar fermenter (MD-500 model, manufactured by Marubishi Bioengineering Co., Ltd.) containing 6 L of production medium was inoculated at 1.5 v / v%. The operating conditions were a culture temperature of 30°C, an agitation speed of 400 rpm, and an aeration rate of 1.8 L / min. The pH was controlled between 6.6 and 6.8. 5N sulfuric acid and sodium hydroxide were used to control the pH. Culture was continued for up to 72 hours. The cells were collected by centrifugation, washed with methanol, and then freeze-dried. A 3-hydroxyalkanoate polymer was extracted from the dried bacterial cells using chloroform, and then bacterial components were removed from the chloroform solution containing the 3-hydroxyalkanoate polymer by filtration. Methanol was added to the filtrate to precipitate the 3-hydroxyalkanoate polymer. The supernatant was then removed by centrifugation, and the resulting polymer was dried to obtain a 3-hydroxyalkanoate polymer. The resulting 3-hydroxyalkanoate polymer (hereinafter sometimes referred to as "P3HB3HH-1") is represented by the general formula (II) described above. The physical properties of the resulting P3HB3HH-1 were also measured as described above. The results are shown in Table 1.
[0053]
[0054] [Examples 1 and 2, and Comparative Example 1] The β-methyl-δ-valerolactone polymer and 3-hydroxyalkanoate polymer obtained in the Production Examples were charged into a co-rotating intermeshing twin-screw extruder ("TEM26ss" manufactured by Shibaura Machine Co., Ltd.), melt-kneaded at a cylinder temperature of 140 to 160°C and a screw rotation speed of 100 rpm, and the extruded strands were cut to produce a resin composition (pellets). The evaluation results of the resin compositions are shown in Table 2.
[0055]
[0056] It is clear from Examples 1 and 2 and Comparative Example 1 that the resin compositions obtained in the Examples are resin compositions with improved impact resistance at the above temperatures. It is also clear from Examples 1 and 2 and Comparative Example 1 that the β-methyl-δ-valerolactone polymers obtained in Production Examples 1 and 2 are useful as modifiers for 3-hydroxyalkanoate polymers.
Claims
1. A resin composition comprising a β-methyl-δ-valerolactone polymer represented by the following general formula (I-a) or (I-b) and a 3-hydroxyalkanoate polymer represented by the following general formula (II): [In general formula (I-a), n is 5 to 20. In general formula (I-b), l and m each independently are 2 to 10.] [In the general formula (II), the ratio of k to p (k / p) is 70 / 30 to 99 / 1.] 2. The resin composition according to claim 1, comprising 5 to 20 parts by mass of the β-methyl-δ-valerolactone polymer per 100 parts by mass of the 3-hydroxyalkanoate polymer.
3. The resin composition according to claim 1 or 2, wherein the β-methyl-δ-valerolactone polymer has a number average molecular weight of 1,000 to 4,000.
4. The resin composition according to any one of claims 1 to 3, wherein the 3-hydroxyalkanoate polymer has a weight average molecular weight of 50,000 to 3,000,000.
5. The resin composition according to any one of claims 1 to 4, wherein the β-methyl-δ-valerolactone polymer is represented by the general formula (I-a).
6. The resin composition according to any one of claims 1 to 4, wherein the β-methyl-δ-valerolactone polymer is represented by the general formula (I-b).
Citation Information
Patent Citations
Copolymer and its production
JP1993093049A
Electronic component mounting apparatus
JP1994053691A
Method for producing polyester
JP2001340078A
Poly-3-hydroxyalkanoate-based resin composition and molded body
JP2017222791A
Preparation method and application of polylactic acid for producing extinction biaxially oriented film
CN115057997A