Laminate, method for manufacturing laminate, and method for manufacturing semiconductor device

The laminate structure with a laser-absorbing temporary adhesive layer and protective layer, combined with laser lift-off technology, addresses the inefficiencies and damage issues in existing semiconductor chip mounting techniques, enabling faster and more reliable transfer and mounting of semiconductor devices.

WO2024225363A1PCT designated stage expired Publication Date: 2024-10-31TORAY INDUSTRIES INC

Patent Information

Application Number
PCT/JP2024/016178
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current semiconductor chip mounting techniques, such as flip-chip bonder and stamping methods, face challenges including long processing times, damage to brittle thin film crystals during transfer, and limitations in transferring multiple devices simultaneously due to inadequate heat resistance and adhesive residue issues with existing adhesives.

Method used

A laminate structure comprising a laser-absorbing temporary adhesive layer, a protective layer, and a semiconductor layer laminated on a laser-transparent substrate, utilizing laser lift-off (LLO) technology for efficient transfer and mounting of semiconductor devices, which reduces processing time and minimizes damage to the semiconductor layer.

Benefits of technology

This method enables faster semiconductor device manufacturing with reduced damage and allows for mass production of epitaxially grown crystals without an underlying base material, improving processing margins and reducing the need for expensive base material reuse.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016178_31102024_PF_FP_ABST
    Figure JP2024016178_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a laminate in which a laser-absorbing temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmissive substrate 1.
Need to check novelty before this filing date? Find Prior Art

Description

Stacked body, manufacturing method of stacked body, and manufacturing method of semiconductor device

[0001] The present invention relates to a laminate, a method for manufacturing the laminate, and a method for manufacturing a semiconductor device using the laminate. More specifically, the present invention relates to a laminate including a laser-absorbent temporary adhesive layer suitable for use in mounting a semiconductor element by laser transfer, a laminate including an adhesive layer that is an adherend for the semiconductor element after laser transfer, a method for manufacturing the laminate, and a method for manufacturing a semiconductor device that mounts a semiconductor element using the laminate.

[0002] Generally, semiconductor elements incorporated into semiconductor devices are transferred and mounted on circuit boards, etc., by a pick-and-place method using a flip-chip bonder, etc. In recent years, semiconductor devices have become more sophisticated and smaller, and accordingly, the semiconductor elements incorporated into semiconductor devices have also become smaller and thinner, and the number of elements mounted has also increased.

[0003] In recent years, devices using III-V group compound semiconductor chips such as gallium arsenide and indium phosphide have been facing the problem of heat generation during device operation. Therefore, in order to improve heat dissipation, studies have been conducted to directly bond the chip to a substrate with different heat dissipation properties, such as a silicon substrate, to promote heat dissipation and improve drive performance (Patent Document 1). Furthermore, in silicon photonics, a III-V group compound semiconductor laser chip is directly bonded to an SOI (Silicon On Insulator) wafer with an optical waveguide formed thereon, in an attempt to achieve miniaturization and cost reduction through integration (Patent Document 2, Non-Patent Documents 1, 2, and 3).

[0004] In this context, a chip transfer and mounting method using a stamp method has been implemented as a technology for processing a large number of semiconductor elements at once. With this method, a pattern sheet made of a silicone rubber material or an adhesive resin such as polydimethylsiloxane resin is mounted on a stamp head, making it possible to transfer and mount a large number of semiconductor elements at once (Patent Documents 3 and 4, Non-Patent Documents 2 and 3).

[0005] On the other hand, such adhesive resins are also used as adhesive layers for bonding substrates together, in addition to semiconductor element transfer and mounting technologies. For example, in the field of power semiconductors, a support substrate is attached to the device substrate during thinning processing to prevent warping and cracking. It has been disclosed that using a polyimide copolymer containing siloxanes of different chain lengths in its structure as an adhesive layer to bond the support substrate can suppress the generation of voids during high-temperature processing such as ion implantation, which is essential for the manufacture of power semiconductors, and can also be easily removed with a solvent after processing (Patent Document 5). It has also been disclosed that adding a crosslinking agent to a polyimide copolymer containing siloxanes in its structure improves chemical resistance, allowing it to be used as a copper-clad substrate for tape automated bonding (TAB) (Patent Document 6).

[0006] Japanese Patent Publication No. 2006-108556 Japanese Patent Publication No. 2017-500735 Japanese Patent Publication No. 2015-140372 Japanese Patent Publication No. 2020-129638 International Publication No. 2016 / 021646 Japanese Patent Publication No. 10-226778

[0007] Alexander W. Fang et al., Electrically pumped hybrid AlGaInAs-silicon evanescent laser, OPTICS EXPRESS, 2006, Vol.14, No.20, p9203Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803LUO et al., Wafer-scale dies-transfer bonding technology for hybrid III / V-on-silicon photonic integrated circuit, IEEE JOURNAL OF SELECTED TOPICS IN QUANTUM ELECTRONICS, 2016, Vol.22, No.6, 8200612

[0008] In the technologies of Patent Documents 1 and 2, the semiconductor element and the heat dissipation substrate are directly bonded, requiring high temperatures and pressures for bonding. This requires the semiconductor elements to be transferred and mounted one by one using a flip-chip (hereinafter also referred to as "FC") bonder capable of high-temperature bonding (transfer / mounting speed: 0.1 to 1 element / second), resulting in the issue of time-consuming transfer / mounting. Furthermore, in Non-Patent Documents 1 and 2, high-temperature bonding is performed on a wafer as a whole, shortening the process, but still requiring the semiconductor elements to be transferred and mounted one by one. Both Non-Patent Documents 1 and 2 aim to transfer epitaxially grown thin-film crystals, but the thin-film crystals are fragile and prone to breakage during transport. Therefore, a process of transporting the substrate together with the substrate and then peeling off the substrate is required.

[0009] On the other hand, while the technologies described in Patent Documents 3 and 4 and Non-Patent Document 2 can transfer and mount many semiconductor elements at once, the stamp size depends on the wafer size, which limits the number of semiconductor elements that can be simultaneously transferred. Furthermore, stamps must be created each time according to the circuit board design, which poses issues such as the possibility of transferring defective chips at the same time. Another issue is that the resin used in the stamp head has insufficient heat resistance, making it inapplicable to technologies that require high-temperature mounting, such as direct bonding.

[0010] Furthermore, although the polyimide copolymers disclosed in Patent Documents 5 and 6 have high heat resistance, they are specialized for processability after being bonded to a substrate or copper foil, and therefore have very high adhesiveness. Therefore, when attempting to apply them to the transfer of minute devices such as semiconductor elements, the transfer itself is difficult, and there is a large amount of adhesive residue left on the chip surface after transfer, making their application difficult.

[0011] In other words, the problems are that the process time for mounting semiconductor chips using an FC bonder is long, and that thin-film semiconductor chips are damaged when they are transferred and mounted, and the inability to achieve both of these problems at the same time is a further problem.

[0012] The present inventors have discovered that the above-mentioned problems can be solved by manufacturing a semiconductor device by laser lift-off (LLO) technology using a laminate 1 in which a laser-absorbent temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transparent substrate 1, and a laminate 2 in which an adhesive layer is laminated on a support substrate 2.

[0013] In order to solve the above problems, the present invention is characterized by the following (1) to (14). (1) A laminate in which a laser-absorbing temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmitting substrate 1. (2) The laminate according to (1) above, in which the semiconductor layer 1 is a compound semiconductor. (3) The laminate according to (2) above, in which the compound semiconductor is AlGaInAs, InGaAs, InP, InGaAsP, AlAs, InAs, GaAs, AlN, AlP, GaN, InN, or SiC. (4) The laminate according to any one of (1) to (3) above, in which the protective layer 1 is at least one of an oxide film and a nitride film. (5) The protective layer 1 is SiO 2(6) A method for producing a laminate, comprising the steps of: (I) using a laminate 1 in which a laser-absorbent temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmissive substrate 1; and (II) using a laminate 2 in which an adhesive layer is laminated on a support substrate 2, the step of opposing a surface of the laminate 1 on the semiconductor layer 1 side to a surface of the laminate 2 on the adhesive layer side, and (II) irradiating the laser-absorbent temporary adhesive layer 1 with a laser from the surface of the laminate 1 opposite to the surface on the semiconductor layer 1 side while transmitting through the laser-transmissive substrate 1, thereby transferring a structure in which the protective layer 1 and the semiconductor layer 1 are laminated to the laminate 2, and forming a laminate 3 in which the adhesive layer, the semiconductor layer 1, and the protective layer 1 are laminated in this order on the support substrate 2. (7) The method for producing a laminate according to (6), wherein in the step (II), the structure 1 is a structure 2 in which the laser-absorbent temporary adhesive layer 1, the protective layer 1, and the semiconductor layer 1 are laminated, and the laminate 3 is a laminate 4 in which the adhesive layer, the semiconductor layer 1, the protective layer 1, and the laser-absorbent temporary adhesive layer 1 are laminated in this order on the support substrate 2. (8) The method for producing a laminate according to (6), further comprising a step (III) of removing a portion of the adhesive layer of the laminate 3 and patterning the adhesive layer. (9) The method for producing a laminate according to (7), further comprising a step (III') of removing a portion of the adhesive layer of the laminate 4 and patterning the adhesive layer. (10) The method for producing a laminate according to (8), further comprising a step (III-A) of dry-etching or wet-etching the adhesive layer of the laminate 3 using the semiconductor layer 1 or the protective layer 1 of the laminate 3 as a mask in the step (III). (11) The method for producing a laminate according to (9) above, further comprising a step (III'-A) of dry-etching or wet-etching the adhesive layer of the laminate 4 using the semiconductor layer 1, the protective layer 1, or the laser-absorbing temporary adhesive layer 1 of the laminate 4 as a mask in the step (III'). (12) The method for producing a laminate according to (6), (8), or (10) above, further comprising a step (IV) of removing the protective layer 1 from the laminate 3.(13) The method for producing a laminate according to (7), (9), or (11), further comprising a step (IV') of removing the laser-absorbing temporary adhesive layer 1 and the protective layer 1 from the laminate 4. (14) A method for producing a semiconductor device, comprising a step (V) of placing the surface of the laminate obtained by the method for producing a laminate according to (12) on the semiconductor layer 1 side opposite a surface of a circuit board on which a circuit is formed, and bonding the semiconductor layer 1 of the laminate to the circuit board by thermocompression bonding. (15) The method for producing a semiconductor device according to (14), further comprising a step (VI) of removing a support substrate 2 with an adhesive layer from a structure in which the semiconductor layer 1 of the laminate and the circuit board are bonded, after the step (V). (16) The method for producing a semiconductor device according to (14), wherein the semiconductor device is a silicon photonics semiconductor device. (17) A laminate in which a support substrate 2, an adhesive layer, a semiconductor layer 1, and a protective layer 1 are laminated in this order, and the adhesive layer has a patterned shape.

[0014] The method for manufacturing a laminate and a semiconductor device of the present invention uses laser lift-off (LLO) technology, which allows semiconductor devices to be manufactured in a shorter time than conventional methods. Furthermore, by protecting the semiconductor layer with a protective layer during manufacturing, damage to the semiconductor layer can be prevented.

[0015] According to the laminate of the present invention, the transfer of an epitaxially grown crystal film to a semiconductor chip using laser lift-off (LLO) technology can be performed without damaging the semiconductor chip and with a wide processing margin, i.e., a wide range of processing conditions, which can contribute to mass production. Furthermore, unlike conventional technology, transfer is possible without a base substrate for the epitaxially grown crystal, which eliminates the need to remove the substrate after transfer and allows the reuse of expensive substrates. Furthermore, the mounting time per chip is significantly shortened, which has the advantage of significantly reducing the number of mounting devices required compared to FC mounting.

[0016] FIG. 1A is a schematic cross-sectional view showing an example of laminate 1. FIG. 1B is a schematic cross-sectional view showing an example of laminate 1. FIG. 1C is a schematic cross-sectional view showing an example of laminate 1. FIG. 2A is a schematic cross-sectional view showing an example of laminate 2. FIG. 2B is a schematic cross-sectional view showing an example of laminate 2. FIG. 3A is a schematic cross-sectional view showing examples of laminate 1 and laminate 3, illustrating an example of manufacturing laminate 3 by laser transfer. FIG. 3B is a schematic cross-sectional view showing examples of laminate 1 and laminate 4, illustrating an example of manufacturing laminate 4 by laser transfer. FIG. 4A is a schematic cross-sectional view showing an example of a state after patterning and removing protective layer 1 from laminate 3. FIG. 4B is a schematic cross-sectional view showing an example of a state after patterning and removing protective layer 1 from laminate 3. FIG. 5 is a schematic cross-sectional view showing an example of transferring semiconductor layer 1 to a circuit board. FIG. 6A is a schematic cross-sectional view showing an example of a manufacturing process for laminate 0″ having a Terther structure. FIG. 6B is a schematic cross-sectional view showing an example of a manufacturing process for laminate 0″ having a Terther structure. FIG. 6C is a schematic cross-sectional view showing an example of a manufacturing process of a stack 0" having a Terther structure. FIG. 6D is a schematic cross-sectional view showing an example of a manufacturing process of a stack 0" having a Terther structure. FIG. 6E is a schematic cross-sectional view showing an example of a manufacturing process of a stack 0" having a Terther structure. FIG. 6F is a schematic cross-sectional view showing an example of a manufacturing process of a stack 1' from a stack 0" having a Terther structure. 6G is a schematic cross-sectional view showing an example of a process for producing a laminate 1' from a laminate 0" having a Terther structure. FIG. 7A is a schematic cross-sectional view showing an example of a process for producing a laminate 1 from a laminate 0 having a Terther structure. FIG. 7B is a schematic cross-sectional view showing an example of a process for producing a laminate 1 from a laminate 0 having a Terther structure. FIG. 8A is a schematic cross-sectional view showing an example of a laminate 4. FIG. 8B is a schematic cross-sectional view showing an example of a state in which the laser-absorbent temporary adhesive layer 1 has been removed from the laminate 4. FIG. 9A is a schematic cross-sectional view showing an example of a laminate 3 in which patterning of the adhesive layer has been performed. FIG. 9B is a schematic cross-sectional view showing an example of a laminate 3 in which patterning of the adhesive layer has been performed. FIG. 10A is a schematic cross-sectional view showing an example of a process for removing a support substrate 2 in step (VI). FIG. 10B is a schematic cross-sectional view showing an example of a process for removing a support substrate 2 in step (VI).FIG. 10C is a schematic cross-sectional view showing an example of the process of removing the support substrate 2 in step (VI).

[0017] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited thereto. The numerical range "to" means a range including the numerical values ​​before and after it, for example, "0 to 100" means a range of 0 or more and 100 or less.

[0018] The method for producing a laminate according to this embodiment includes the following steps, in this order: a laminate 1 in which a laser-absorbent temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmissive substrate 1; and a laminate 2 in which an adhesive layer is laminated on a support substrate 2. The method includes the following steps: (I) of arranging the surface of the laminate 1 on the semiconductor layer 1 side and the surface of the laminate 2 on the adhesive layer side, and (II) of irradiating the laser-absorbent temporary adhesive layer 1 with a laser from the surface of the laminate 1 opposite to the surface on the semiconductor layer 1 side while transmitting the laser through the laser-transmissive substrate 1, thereby transferring the structure in which the protective layer 1 and the semiconductor layer 1 are laminated to the laminate 2, and forming a laminate 3 in which the adhesive layer, the semiconductor layer 1, and the protective layer 1 are laminated in this order on the support substrate 2.

[0019] Each component of the laminate of this embodiment will be described below.

[0020] [Laminate 1] First, a laminate 1 (reference numeral 100) will be described, in which a laser-absorbent temporary adhesive layer 1 (reference numeral 12), a protective layer 1 (reference numeral 13), and a semiconductor layer 1 (reference numeral 14) are laminated in this order on a laser-transmitting substrate 1 (reference numeral 11), for example, as shown in FIG. 1A.

[0021] (Laser-Transmittable Substrate 1) First, the laser-transmittable substrate 1 contained in the laminate 1 will be described. The laser-transmittable substrate 1 is preferably a substrate having an absorbance of 0.1 or less at at least one wavelength of 248 nm, 266 nm, and 355 nm. Examples of substrates having such absorbance include inorganic substrates such as quartz, sapphire, alkali glass, alkali-free glass, and borosilicate glass. When an inorganic substrate is used, the thickness of the substrate can be selected within a range that does not impair the absorbance, and is preferably 0.1 mm to 5.0 mm. From the viewpoint of substrate strength, the thickness of the substrate is more preferably 0.3 mm or more, and from the viewpoint of substrate handling, for example, limitations on the mass and substrate thickness of the device, the thickness of the substrate is more preferably 2.0 mm or less.

[0022] Alternatively, an organic substrate such as PET, aramid, polyester, polypropylene, or cycloolefin may be used as the laser-transmittable substrate 1. When an organic substrate is used, the thickness of the substrate can be selected within a range that does not impair the absorbance, and is preferably 0.05 mm to 3.0 mm. From the viewpoint of ease of handling of the substrate, the thickness of the substrate is more preferably 0.1 mm or more, and from the viewpoint of suppressing light scattering during laser irradiation, the thickness of the substrate is more preferably 1.0 mm or less.

[0023] (Laser-absorbent temporary adhesive layer 1) Next, the laser-absorbent temporary adhesive layer 1 contained in the laminate 1 will be described. The laser-absorbent temporary adhesive layer 1 is a resin film that is absorptive to laser and has adhesive properties that allow an article to be held on the surface of the resin film. The laser-absorbent temporary adhesive layer 1 can be imparted with laser-absorbent additives such as ultraviolet absorbers and dyes, or laser-absorbent resins. The adhesive properties for holding an article in the laser-absorbent temporary adhesive layer 1 can be imparted by adding an adhesive resin, which may be imparted in combination with a laser-absorbent resin or component, or a resin or component specialized for adhesive properties. In addition, the laser-absorbent temporary adhesive layer 1 may contain components that increase flexibility and flexibility, crosslinking agents, additives, curing accelerators, silane compounds, etc. The laser-absorbent temporary adhesive layer 1 may also be formed by forming a film from a solution-like resin composition that further contains a solvent.

[0024] The laser-absorbent temporary adhesive layer 1 preferably has an absorbance of 0.4 or more and 6.0 or less at a film thickness of 1.0 μm at at least one wavelength of 248 nm, 266 nm, and 355 nm. By having the absorbance of 0.4 or more, in the step (II), when a laser is irradiated from the laser-transparent substrate 1 side to the laser-absorbent temporary adhesive layer 1 side to transfer the semiconductor element to the opposing substrate (also referred to as laser lift-off (LLO)), the irradiated laser is concentratedly absorbed by the laser-absorbent temporary adhesive layer 1, allowing the semiconductor element to be efficiently transferred. Since the laser can be particularly absorbed near the interface between the laser-absorbent temporary adhesive layer 1 and the laser-transparent substrate 1, and transfer is possible with low-energy laser irradiation, the absorbance is more preferably 0.6 or more. Furthermore, from the viewpoint of material design, the absorbance is preferably 6.0 or less, more preferably 5.0 or less, and more preferably 4.0 or less, since versatile resins can be used.

[0025] From the viewpoint of transferability in LLO, the thickness of the laser-absorbent temporary adhesive layer 1 is preferably 1.0 μm to 15 μm, more preferably 3.0 μm to 10 μm. When the laser-absorbent temporary adhesive layer 1 is 1.0 μm or thicker, the laser is completely absorbed by the laser-absorbent temporary adhesive layer 1, preventing the protective layer 1 and the semiconductor layer 1 from being directly ablated by the laser and being damaged. When the laser-absorbent temporary adhesive layer 1 is 15 μm or thicker, the force generated by laser irradiation is sufficiently transmitted to the semiconductor layer 1, improving the yield of laser transfer. When the laser-absorbent temporary adhesive layer 1 is 3.0 μm or thicker, the laser-absorbent temporary adhesive layer 1 absorbs excessive impact caused by laser irradiation, preventing damage to the semiconductor layer 1. Furthermore, when the laser-absorbent temporary adhesive layer 1 is 10 μm or thicker, the semiconductor layer 1 can be transferred with high positional accuracy. The thickness of the laser-absorbent temporary adhesive layer 1 can be measured by cutting a laminate including this layer and observing the cross section with a scanning electron microscope.

[0026] Resins contained in the laser-absorbent temporary adhesive layer 1 include, but are not limited to, polyimide-based resins such as polyimide, polyimide precursor, polybenzoxazole, and polybenzoxazole precursor, as well as urethane resin, novolac resin, polyhydroxystyrene, polyester resin, acrylic resin, aramid resin, polysiloxane, and polyimidesiloxane. From the viewpoint of heat resistance, it is preferable that the above resins are contained in an amount of 10 to 100% by mass in the laser-absorbent temporary adhesive layer 1. It is also preferable that the laser-absorbent temporary adhesive layer 1 contains an acrylic resin, polysiloxane, or polyimidesiloxane for the purpose of imparting adhesiveness to the laser-absorbent temporary adhesive layer 1.

[0027] In addition, it is preferable that these resins have a conjugated structure in their structure. By having the above resin have a conjugated structure, the absorbance of the laser-absorbent temporary adhesive layer 1 at a film thickness of 1.0 μm at at least one wavelength of 248 nm, 266 nm, and 355 nm can be adjusted to a range of 0.4 to 6.0. Examples of structures having a conjugated structure include aromatic structures, and among them, it is preferable to have at least one structure of biphenyl, imide, benzoxazole, and benzophenone. The above absorbance can be achieved by making 60 mol % or more of the monomer residues in the resin contained in the laser-absorbent temporary adhesive layer 1 have a conjugated structure, relative to 100 mol % of all monomer residues. Only one type of these resins may be contained in the laser-absorbent temporary adhesive layer 1, or multiple types may be contained.

[0028] From the viewpoint of heat resistance during laser irradiation, the resin contained in the laser-absorbable temporary adhesive layer 1 preferably contains a resin (X) having one or more structures selected from the group consisting of a polyimide having the structure of the following formula (1), a polyimide precursor having the structure of the following formula (2), a polybenzoxazole having the structure of the following formula (3), a polybenzoxazole precursor having the structure of the following formula (4), and copolymers thereof. From the viewpoint of temporary adhesion, it is preferable that the resin (X) is contained in the laser-absorbable temporary adhesive layer 1 in an amount of 10 to 100% by mass. In this specification, "temporary adhesion" refers to a state in which an article is temporarily held on the surface of the laser-absorbable temporary adhesive layer 1 by the adhesive properties of the laser-absorbable temporary adhesive layer 1. At this time, the held article can be finally detached from the surface of the laser-absorbable temporary adhesive layer 1 using a peeling method such as laser irradiation, as described below.

[0029]

[0030] In the above formulas (1) to (4), R 1 , R 3 , R 7 and R 9 each independently represents a tetravalent organic group having 6 to 40 carbon atoms; R 2 , R 4 , R 6 and R 8 R each independently represents a divalent organic group having 2 to 40 carbon atoms. 5 represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0031] Polyimide and polybenzoxazole are resins having a cyclic structure of an imide ring or an oxazole ring within the main chain structure. Their precursors, polyimide precursors and polybenzoxazole precursors, are resins that form an imide ring or a benzoxazole ring structure by dehydration and ring closure. It is preferable that one or more structures selected from the group consisting of formulas (1) to (4) above are contained as repeating units in 10 to 100,000 units per molecule of resin (X). Within this range, the laser-absorbent temporary adhesive layer 1 can be applied with an appropriate film thickness.

[0032] Polyimides can be obtained by reacting tetracarboxylic acids, corresponding tetracarboxylic dianhydrides, tetracarboxylic diester dichlorides, etc. with diamines, corresponding diisocyanate compounds, trimethylsilylated diamines, etc., and preferably contain tetracarboxylic acid residues and diamine residues. For example, polyamic acids, which are polyimide precursors obtained by reacting tetracarboxylic dianhydrides with diamines, can be obtained by dehydrating and cyclizing the polyimides through heat treatment. During this heat treatment, a solvent that forms an azeotrope with water, such as m-xylene, can be added. Alternatively, polyimides can be obtained by adding a dehydrating condensation agent such as a carboxylic anhydride or dicyclohexylcarbodiimide, or a ring-closing catalyst such as a base such as triethylamine, followed by chemical heat treatment to dehydrate and cyclize the polyimides. Alternatively, polyimides can be obtained by adding a weakly acidic carboxylic acid compound and then heat treating the polyimides at a low temperature of 100°C or below to dehydrate and cyclize the polyimides.

[0033] Polybenzoxazole can be obtained by reacting a bisaminophenol compound with a dicarboxylic acid, a corresponding dicarboxylic acid chloride, a dicarboxylic acid activated ester, or the like, and preferably has a dicarboxylic acid residue and a bisaminophenol residue. For example, it can be obtained by dehydrating and cyclizing polyhydroxyamide, which is one of the polybenzoxazole precursors obtained by reacting a bisaminophenol compound with a dicarboxylic acid, through a heat treatment. Alternatively, it can be obtained by adding phosphoric anhydride, a base, a carbodiimide compound, or the like and dehydrating and cyclizing it through a chemical treatment.

[0034] In the above formula (1) and formula (2), R 1 and R 3 (COOR 5 ) 2 preferably represents a tetracarboxylic acid residue. 1 or R 3 (COOR 5 ) 2Examples of the tetracarboxylic acid residue constituting the compound include aromatic tetracarboxylic acid residues such as pyromellitic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 3,3',4,4'-benzophenonetetracarboxylic acid, 2,2-bis(3,4-dicarboxyphenyl)hexafluoropropane, bis(3,4-dicarboxyphenyl)sulfone, and bis(3,4-dicarboxyphenyl)ether, as well as aliphatic tetracarboxylic acid residues such as 1,2,3,4-cyclopentanetetracarboxylic acid. The compound may also contain two or more of these tetracarboxylic acid residues. From the viewpoint of absorbance, aromatic tetracarboxylic acid residues are preferred.

[0035] In the above formula (1) and formula (2), R 2 and R 4 R preferably represents a diamine derivative residue. 2 and R 4 Examples of diamine derivative residues constituting the formula include hydroxyl group-containing diamine residues such as 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4-hydroxyphenyl)sulfone, and 2,2-bis(3-amino-4-hydroxyphenyl)propane; sulfonic acid group-containing diamine residues such as 3-sulfonic acid-4,4'-diaminodiphenyl ether; thiol group-containing diamine residues such as dimercaptophenylenediamine; aromatic diamine residues such as 3,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl sulfone, p-phenylenediamine, and 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl; compounds in which a portion of the hydrogen atoms of these aromatic rings are substituted with alkyl groups or fluoroalkyl groups having 1 to 10 carbon atoms, halogen atoms, or the like; and alicyclic diamine residues such as cyclohexyldiamine and methylenebiscyclohexylamine. Two or more of these diamine residues may be contained in combination. From the viewpoint of absorbance, the aromatic diamine residues in the laser-absorbent temporary adhesive layer 1 preferably account for 30 mol % or more of the total diamine residues.

[0036] In the above formula (2), R 5represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. Examples of the organic group having 1 to 20 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a pentyl group, a hexyl group, a cyclohexyl group, an octyl group, a dodecyl group, and a phenyl group. In view of the ease of availability of raw materials for polymerization, a methyl group or an ethyl group is preferred.

[0037] In the above formulas (3) and (4), R 6 and R 8 preferably represents a dicarboxylic acid residue, a tricarboxylic acid residue, or a tetracarboxylic acid residue. Examples of dicarboxylic acid residues include residues of terephthalic acid, isophthalic acid, diphenyl ether dicarboxylic acid, bis(carboxyphenyl)hexafluoropropane, biphenyl dicarboxylic acid, benzophenone dicarboxylic acid, and triphenyl dicarboxylic acid. Examples of tricarboxylic acid residues include residues of trimellitic acid, trimesic acid, diphenyl ether tricarboxylic acid, and biphenyl tricarboxylic acid. Examples of tetracarboxylic acid residues include residues of R 1 and R 3 (COOR 5 ) 2 These are the same as the examples of the tetracarboxylic acid residues given as examples. Two or more of these may be used.

[0038] In the above formulas (3) and (4), R 7 and R 9 (OH) 2 preferably represents a residue of a bisaminophenol derivative. Specific examples of the residue of a bisaminophenol derivative include, but are not limited to, residues of bis(3-amino-4-hydroxyphenyl)propane, bis(3-amino-4-hydroxyphenyl)sulfone, 2,2-bis(3-amino-4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-amino-3-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane, etc., and these compounds may be contained alone or in combination of two or more.

[0039] Furthermore, by capping the terminals of the resins represented by formulas (1) to (4) with a monoamine, acid anhydride, acid chloride, or monocarboxylic acid having an acidic group, a resin having an acidic group at the terminal of the main chain can be obtained.

[0040] Preferred examples of such monoamines include 2-aminophenol, 3-aminophenol, and 4-aminophenol. Two or more of these may be used. Preferred examples of such acid anhydrides, acid chlorides, and monocarboxylic acids include known compounds such as phthalic anhydride, maleic anhydride, and nadic anhydride. Di-tert-butyl dicarbonate is also preferably used as a reactive terminal. Two or more of these may be used.

[0041] The resin (X) preferably has one or more structures selected from the group consisting of a dimethylsiloxane structure represented by formula (5), a diphenylsiloxane structure represented by formula (6), an alkylene glycol structure represented by formula (7), and an alkylene structure represented by formula (8). By having these flexible structures, temporary adhesive properties can be expected to be exhibited.

[0042]

[0043] In the above formulas (5) to (8), R 10 ~R 13 each independently represents a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. l, m, and n each independently represent an integer of 4 to 40. p represents an integer of 10 to 40. o represents an integer of 1 to 16.

[0044] By having one or more structures selected from the group consisting of the structures represented by the above formulas (5) to (8) in the structure of the resin (X), the flexibility and adhesive strength of the laser-absorbent temporary adhesive layer 1 can be improved. 10 ~R 13 is R 5 This is the same as the explanation above.

[0045] Specific examples of at least one structure selected from the group consisting of structures represented by the above formula (5), formula (6), formula (7), and formula (8) include aliphatic diamine residues, such as diamine residues containing a polyethylene oxide group as in JEFFAMINE (registered trademark) KH-511, JEFFAMINE (registered trademark) ED-600, JEFFAMINE (registered trademark) ED-900, and polyoxypropylene diamines D-400 and D-2000 (manufactured by Huntsman Japan Co., Ltd.); diamine residues having a polyalkylene oxide group as in Elasmer (registered trademark) 250P, Elasmer (registered trademark) 1000P, and Porea (registered trademark) SL100A (manufactured by Kumiai Chemical Industry Co., Ltd.); and siloxane diamine residues such as propylamine-terminated siloxane diamines LP-7100, KF-8010, KF-8012, and X22-161A (manufactured by Shin-Etsu Chemical Co., Ltd.). Two or more of these diamine residues may also be used in combination.

[0046] Furthermore, the resin (X) is more preferably a polyimidesiloxane. A polyimidesiloxane is a resin having a siloxane structure in a polyimide repeating unit, and the polyimidesiloxane of the resin (X) particularly preferably has a siloxanediamine residue represented by formula (9) in the structure.

[0047]

[0048] In the above formula (9), q is a natural number from 1 to 50. 14 and R 15 may be the same or different and represent an alkylene group or a phenylene group having 1 to 30 carbon atoms. 16 ~R 19 may be the same or different and represent an alkyl group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group.

[0049] Examples of the siloxane diamine residue represented by the above formula (9) include those derived from the following diamines. Specific examples include residues of α,ω-bis(3-aminopropyl)polydimethylsiloxane, α,ω-bis(3-aminopropyl)polydiphenoxysiloxane, α,ω-bis(4-aminophenyl)polydimethylsiloxane, and α,ω-bis(4-aminophenyl)polydiphenoxysiloxane. Only one type of the siloxane diamine residue may be contained, or two or more types may be contained. Polyimide siloxanes are characterized by high adhesive strength and high absorbance derived from polyimides, and can particularly increase absorbance at 355 nm, etc.

[0050] In the laminate 1 of this embodiment, the 1% mass loss temperature of at least one of the resins contained in the laser-absorbent temporary adhesive layer 1 is preferably 300 ° C. or higher, and the 1% mass loss temperature of all of the resins contained in the laser-absorbent temporary adhesive layer 1 is more preferably 300 ° C. or higher. In this specification, the 1% mass loss temperature is defined as the temperature at which the resin is heat-treated at 250 ° C. for 30 minutes, and then heated at 100 ° C. / min using thermogravimetric analysis (TGA). The mass at 100 ° C. is defined as 100%, and the temperature at which 1% of the mass is lost is defined as the 1% mass loss temperature. For resins that have already been heat-treated, this can also be confirmed by further heat-treating them at 250 ° C. for 30 minutes. By having a 1% mass loss temperature of 300 ° C. or higher, deterioration of the entire laser-absorbent temporary adhesive layer 1 due to the heat generated during laser irradiation can be suppressed. This makes it possible to prevent the deteriorated laser-absorbent temporary adhesive layer 1 from scattering and soiling the device, etc. Such fragments generated by scattering of the laser-absorbent temporary adhesive layer 1 will be hereinafter referred to as "debris."

[0051] To achieve a 1% mass loss temperature of 300 ° C or higher, the resin preferably contains a component with high thermal stability. Specific examples of components with high thermal stability include rigid components such as aromatic rings, siloxanes with relatively high thermal stability even among flexible structures, or combinations thereof. The 1% mass loss temperature can be set to 300 ° C or higher by having 50% or more of the monomer residues with high thermal stability relative to 100 mol% of all monomer residues constituting the resin contained in the laser-absorbing temporary adhesive layer 1. From the viewpoint of versatility of the resin, the 1% mass loss temperature is preferably 600 ° C or lower.

[0052] The above absorbance can also be achieved by incorporating an additive such as an ultraviolet absorber or a dye into the laser-absorbent temporary adhesive layer 1. Examples of additives that can be incorporated into the laser-absorbent temporary adhesive layer 1 include ultraviolet absorbers such as Tinuvin (registered trademark) PS (manufactured by BASF Japan Ltd.), DAINSORB (registered trademark) T-0, DAINSORB (registered trademark) T-7 (manufactured by Daiwa Kasei Co., Ltd.), and dyes such as Solvent Yellow 93 (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0053] Only one type of these additives may be contained, or multiple types may be contained, in the laser-absorbent temporary adhesive layer 1. The content of the additives to set the absorbance within the above range is preferably 0.1 parts by mass or more relative to 100 parts by mass of the entire laser-absorbent temporary adhesive layer 1, and is preferably 70 parts by mass or less from the viewpoint of stability in the varnish state before forming the laminate.

[0054] The laser-absorbent temporary adhesive layer 1 preferably has an interface adhesive strength of 0.02 N / cm or more and 0.3 N / cm or less with the adjacent photoresist or protective layer 1 described below. The adhesive strength mentioned here refers to the value obtained by removing the structure in which the photoresist, protective layer 1, and semiconductor layer 1 are laminated from the laminate 1, and performing a 90° peel test on the exposed surface of the laser-absorbent temporary adhesive layer 1 and the polyimide film. When the laminate 1 does not contain photoresist, the value obtained by removing the structure in which the protective layer 1 and semiconductor layer 1 are laminated from the laminate 1 and performing the 90° peel test described above is used. A specific measurement method involves pressing a polyimide film, Kapton (registered trademark) 100EN (manufactured by DuPont-Toray Co., Ltd.), cut to 1 cm x 9 cm onto the laser-absorbent temporary adhesive layer 1 using a vacuum laminator at 0.1 MPa and 25°C, and then performing a peel test on the pressed polyimide film in a direction perpendicular to the laser-absorbent temporary adhesive layer 1 at a constant speed of 2 mm / sec using a tensile tester.

[0055] When the adhesive strength is 0.02 N / cm or more, the structure in which the protective layer 1 and the semiconductor layer 1 are laminated can be stably held on the laser-absorbent temporary adhesive layer 1. Furthermore, when the adhesive strength is 0.3 N / cm or less, the structure in which the protective layer 1 and the semiconductor layer 1 are laminated can be transferred to the laminate 2 described below by low-energy laser irradiation. More preferably, the adhesive strength is 0.2 N / cm or less, and in this case, the laser irradiation energy during the transfer can be further suppressed, thereby reducing the risk of damage to the semiconductor element.

[0056] In order to achieve the adhesive strength of the laser-absorbent temporary adhesive layer 1 within the above range, it is preferable that the laser-absorbent temporary adhesive layer 1 contains a component that increases flexibility and flexibility. By introducing a component that increases flexibility and flexibility, the glass transition temperature is lowered, and the adhesive strength can be increased. Examples of components that increase flexibility and flexibility include flexible structures derived from aliphatic or silane groups such as alkylene groups and siloxanes; flexible structures derived from ether groups such as alkylene glycols and biphenyl ethers; alicyclic structures, flexible structures such as olefins, and the like. By containing 20 mol% or more of monomer residues having these flexibility-imparting structures relative to 100 mol% of all monomer residues constituting the resin contained in the laser-absorbent temporary adhesive layer 1, the adhesive strength can be 0.02 N / cm or more, and by making the monomer residues 70 mol% or less, the adhesive strength can be 0.3 N / cm or less.

[0057] On the other hand, for laser-absorbent temporary adhesive layers 1 with an adhesive strength exceeding 0.3 N / cm, the addition of a crosslinking agent crosslinks part of the structure, hardening the surface of the laser-absorbent temporary adhesive layer 1 and reducing the adhesive strength to the above-mentioned range. Furthermore, by crosslinking and strengthening the surface of the laser-absorbent temporary adhesive layer 1, cohesive failure of the laser-absorbent temporary adhesive layer 1 can be suppressed. This makes it possible to suppress the adhesion of residues of the laser-absorbent temporary adhesive layer 1 to the surface of the photoresist or protective layer 1 when the laser-absorbent temporary adhesive layer 1 is peeled off from the surface of the photoresist or protective layer 1. When residues of the adhesive layer or the pressure-sensitive adhesive layer described below remain on the surface of the material to be adhered, these residues are hereinafter referred to as "adhesive residue."

[0058] Examples of crosslinking agents that may be contained in the laser-absorbent temporary adhesive layer 1 include compounds having an alkoxymethyl group or a methylol group, such as NIKALAC (registered trademark) and MW-100LM (manufactured by Sanwa Chemical Co., Ltd.).

[0059] Furthermore, compounds having an epoxy group are also preferred as crosslinking agents, and examples thereof include bisphenol A type epoxy resins, bisphenol F type epoxy resins, epoxy group-containing silicones such as propylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and polymethyl(glycidyloxypropyl)siloxane, and dimer acid-modified epoxy resins, but the crosslinking agent used in this embodiment is not limited to these. Specific examples include JER (registered trademark) 871 (manufactured by Mitsubishi Chemical Corporation) and Showfree (registered trademark) PETG (Resonac Inc.).

[0060] The laser-absorbent temporary adhesive layer 1 may contain only one type of crosslinking agent, or two or more types. The crosslinking agent is preferably contained in an amount of 1 to 30 parts by mass per 100 parts by mass of the laser-absorbent temporary adhesive layer 1. Furthermore, by containing preferably 1 part by mass or more of the crosslinking agent per 100 parts by mass of the laser-absorbent temporary adhesive layer 1, adhesive residue can be reduced. More preferably, by containing 5 parts by mass or more of the crosslinking agent per 100 parts by mass of the laser-absorbent temporary adhesive layer 1, a high adhesive residue suppression effect can be obtained. Furthermore, the crosslinking agent is preferably contained in an amount of 30 parts by mass or less per 100 parts by mass of the laser-absorbent temporary adhesive layer 1. Within this range, a certain degree of flexibility is maintained in the laser-absorbent temporary adhesive layer 1. Furthermore, from the viewpoint of storage stability in the varnish state before forming the laminate, the crosslinking agent is preferably contained in an amount of 20 parts by mass or less per 100 parts by mass of the laser-absorbent temporary adhesive layer 1.

[0061] Furthermore, when the laser-absorbable temporary adhesive layer 1 contains a crosslinking agent, the laser-absorbable temporary adhesive layer 1 may also contain a curing accelerator for the purpose of accelerating curing by the crosslinking agent. Examples of curing accelerators include imidazoles, tertiary amines or their salts, and organic boron salt compounds, with imidazoles being preferred. Specific examples of imidazoles include imidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-1H-imidazole, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl-(1')]-ethyl-s-triazine, and 2-methylimidazole isocyanuric acid adduct. Preferred commercially available imidazoles include Curesol (registered trademark) 2E4MZ and Curesol (registered trademark) 2E4MZ-CN (manufactured by Shikoku Chemicals Corporation).

[0062] The content of the curing accelerator is preferably 0.1 parts by mass or more and 5.0 parts by mass or less per 100 parts by mass of the crosslinking agent. This range ensures a sufficient crosslinking acceleration effect. Furthermore, from the viewpoint of maintaining the stability of the varnish in its state before forming the laminate 1, the content of the curing accelerator is more preferably 0.5 parts by mass or more and 2.0 parts by mass or less per 100 parts by mass of the crosslinking agent.

[0063] Furthermore, the laser-absorbent temporary adhesive layer 1 may further contain a silane compound, if necessary. By containing a silane compound, the adhesion between the laser-absorbent temporary adhesive layer 1 and the laser-transparent substrate 1 can be adjusted. This prevents the laser-unirradiated portions of the laser-absorbent temporary adhesive layer 1 from peeling off from the laser-transparent substrate 1. Specific examples of silane compounds include N-phenylaminoethyltriethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, and p-styryltrimethoxysilane. The content of the silane compound is preferably 0.01 parts by mass or more and 15 parts by mass or less, relative to 100 parts by mass of the laser-absorbent temporary adhesive layer 1.

[0064] Furthermore, the laser-absorbent temporary adhesive layer 1 may contain a surfactant, if necessary, to improve wettability with the laser-transparent substrate 1 during film formation and to form a laser-absorbent temporary adhesive layer 1 with a uniform film thickness.

[0065] ((Laser absorbing layer 1, temporary adhesive layer 2)) Furthermore, since the effect of preventing damage to the semiconductor layer 1 described below is further enhanced, it is preferable that the laser absorbing temporary adhesive layer 1 has a structure of two or more layers including the laser absorbing layer 1 and the temporary adhesive layer 2. In this case, it is preferable that the laser absorbing layer 1 does not have adhesive properties. In this case, as shown in FIG. 1B, for example, the laminate 1 (reference numeral 100) is formed by laminating, in this order, on a laser-transparent substrate 1 (reference numeral 11), a laser absorbing temporary adhesive layer 1 (reference numeral 12) including a laser absorbing layer 1 (reference numeral 17) and a temporary adhesive layer 2 (reference numeral 16), a protective layer 1 (reference numeral 13), and a semiconductor layer 1 (reference numeral 14).

[0066] The thickness of the laser absorbing layer 1 is preferably 0.1 μm to 5 μm, preferably 0.1 μm or more, more preferably 0.3 μm or more, and preferably 5 μm or less, more preferably 3 μm or less. The thickness of the temporary adhesive layer 2 is preferably 0.1 μm to 10 μm, preferably 0.1 μm or more, more preferably 0.3 μm or more, and preferably 10 μm or less, more preferably 5 μm or less. When the thickness of the temporary adhesive layer 2 is 0.1 μm or more, the protective layer 1 can be stably adhered, and when the thickness is 10 μm or less, the energy required for laser transfer of the semiconductor element can be reduced. The total film thickness of the laser absorbing layer 1 and the temporary adhesive layer 2 is preferably 1.0 μm or more and 15 μm or less. The thicknesses of the laser absorbing layer 1 and the temporary adhesive layer 2 can be measured by cutting a laminate including these layers and observing the cross section with a scanning electron microscope.

[0067] The laser absorbing layer 1 is an inorganic film or an organic film. The laser absorbing layer 1 preferably has an absorbance of 0.4 or more and 6.0 or less at a film thickness of 1.0 μm at at least one wavelength of 248 nm, 266 nm, and 355 nm. When the absorbance is 0.4 or more, in the step (II), when a laser is irradiated from the laser-transparent substrate 1 side to the laser absorbing layer 1 side to transfer the semiconductor layer 1 to the opposing substrate, the irradiated laser is intensively absorbed by the laser absorbing layer 1, and the semiconductor layer 1 can be efficiently transferred. Since the laser can be absorbed particularly near the outermost surface of the laser absorbing layer 1 and transfer is possible with low-energy laser irradiation, the absorbance is more preferably 0.6 or more. Furthermore, from the viewpoint of material design, the absorbance is preferably 6.0 or less, and more preferably 5.0 or less because a versatile inorganic film or organic film can be used.

[0068] Suitable organic films that can be contained in the laser absorbing layer 1 include polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, urethane resin, novolac resin, polyhydroxystyrene, polyester resin, acrylic resin, and aramid resin. These may also be contained in the temporary adhesive layer 2.

[0069] As the inorganic film contained in the laser absorbing layer 1, for example, one or more inorganic substances selected from the group consisting of metals, metal compounds, and carbon can be suitably used.

[0070] The metal is preferably at least one selected from gold, silver, copper, iron, nickel, aluminum, titanium, chromium, and alloys thereof. The alloy is preferably silver-tin. The metal compound refers to a compound containing a metal atom, and may be, for example, a metal oxide or a metal nitride. Note that carbon is a concept that may also include allotropes of carbon, and may be, for example, diamond, fullerene, diamond-like carbon, carbon nanotubes, etc. Examples of such inorganic substances include, but are not limited to, metals such as gold, platinum, palladium, cobalt, rhodium, iridium, calcium, ruthenium, osmium, manganese, molybdenum, tungsten, niobium, tantalum, bismuth, antimony, lead, silver, copper, iron, nickel, aluminum, titanium, chromium, tin, and alloys thereof; SiO 2 , SiN, Si 3 N 4 , metal compounds such as TiN, and carbon.

[0071] By having the organic film have a conjugated structure, the absorbance of the laser absorbing layer 1 at a film thickness of 1.0 μm at at least one of wavelengths of 248 nm, 266 nm, and 355 nm can be adjusted to a range of 0.4 to 6.0. Examples of structures having a conjugated structure include aromatic structures, and among these, at least one structure selected from biphenyl, imide, benzoxazole, and benzophenone is preferred. The absorbance can be adjusted to the above range by using monomer residues having a conjugated structure in an amount of 60 mol % or more of the monomer residues relative to 100 mol % of all monomer residues of the resin contained in the laser absorbing layer 1. Only one type of these resins may be contained in the laser absorbing layer 1, or multiple types may be contained.

[0072] The above absorbance can also be achieved by incorporating an additive such as an ultraviolet absorber or a dye. Examples of the additive incorporated in the laser absorbing layer 1 include ultraviolet absorbers such as Tinuvin (registered trademark) 477, Tinuvin (registered trademark) 479 (manufactured by BASF Japan Ltd.), Tinuvin (registered trademark) 400, and DAINSORB (registered trademark, manufactured by Daiwa Chemical Industry Co., Ltd.), and dyes such as Violet 36 (manufactured by Tokyo Chemical Industry Co., Ltd.).

[0073] Only one type of these additives may be contained, or multiple types may be contained, in the laser absorbing layer 1. The content of the additives to bring the absorbance into the above range is preferably 0.1 parts by mass or more per 100 parts by mass of the laser absorbing layer 1, and from the viewpoint of stability in the varnish state before forming the laminate, preferably 50 parts by mass or less.

[0074] Furthermore, the laser-absorbing layer 1 may further contain a silane compound, if necessary. By containing a silane compound, it is possible to adjust the adhesion between the laser-absorbing layer 1 and the laser-transmittable substrate 1. This makes it possible to prevent the laser-unirradiated portion of the laser-absorbing layer 1 from peeling off from the laser-transmittable substrate 1. Specific examples of the silane compound include the silane compounds exemplified as those that can be contained in the laser-absorbent temporary adhesive layer 1, and an equivalent content is preferred.

[0075] Furthermore, the laser absorbing layer 1 may contain a surfactant, if necessary, for the purpose of improving wettability with the laser transmissive substrate 1 during film formation and forming a laser absorbing layer 1 with a uniform thickness. The laser absorbing layer 1 preferably does not have pressure-sensitive adhesive properties, and preferably can be easily removed from the support substrate 2 when the laser absorbing layer 1 moves toward the support substrate 2 together with the semiconductor layer 1 and the like after the LLO in step (II).

[0076] The temporary adhesive layer 2 may be a layer having the same composition and physical properties as the laser-absorbing temporary adhesive layer 1 defined above, a layer not having laser absorption properties, or a layer having the same composition and physical properties as the adhesive layer described below. When the temporary adhesive layer 2 contains a resin (X), it is preferable that the resin (X) contains the structure of the above formula (9). In the step (III) of patterning the adhesive layer, from the viewpoint of removing the temporary adhesive layer 2 simultaneously with the adhesive layer when partially removing the adhesive layer, it is preferable that the temporary adhesive layer 2 is a layer having the same composition and physical properties as the adhesive layer described below.

[0077] (Semiconductor Layer 1) Next, the semiconductor layer 1 contained in the laminate 1 will be described. The semiconductor layer 1 preferably includes an epitaxially grown crystal film. The epitaxially grown crystal film is preferably made of a compound semiconductor, particularly a III-V group compound semiconductor. Examples of preferred epitaxially grown crystal films include compound semiconductors such as AlGaInAs, InGaAs, InP, InGaAsP, AlAs, InAs, GaAs, AlN, AlP, GaN, InN, SiC, and AlGaS. A semiconductor device using these epitaxially grown crystal films may contain only one type of compound semiconductor, or may contain two or more types of compound semiconductors, or may further contain different types of semiconductors stacked together, or may contain a semiconductor substrate, electrode material, a sapphire substrate, a glass substrate, wiring, etc. stacked together. The size of the semiconductor layer 1 is preferably such that the maximum side is 5 μm or more and 5.0 mm or less, more preferably 1.0 mm or less. The thickness of the epitaxially grown crystalline film is preferably 0.005 μm or more and 10 μm or less. If the thickness of the epitaxially grown crystalline film is less than 0.005 μm, there is a risk of breakage during transfer, and if it is more than 10 μm, it takes an enormous amount of time to form the epitaxially grown crystalline film, which is not practical. The size of the epitaxially grown crystalline film can be adjusted, for example, by the method described in Non-Patent Document 2 (Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803).

[0078] (Photoresist) Next, the photoresist that may be contained in the laminate 1 will be described. The laminate 1 preferably has a photoresist between the laser-absorbent temporary adhesive layer 1 and the protective layer 1. In this case, for example, as shown in FIG. 1C, the laminate 1 (reference numeral 100) is a laser-transparent substrate 1 (reference numeral 11) on which a laser-absorbent temporary adhesive layer 1 (reference numeral 12), a photoresist layer (reference numeral 54), a protective layer 1 (reference numeral 13), and a semiconductor layer 1 (reference numeral 14) are laminated. A photoresist is a substance that is photosensitive and can be patterned by imagewise exposure and development to form an image layer on its surface, and contains a photosensitizer and a resin. Either a positive or negative type can be used. Non-Patent Document 2 (Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803) describes the use of photoresist as "tether" to hold the wafer and epitaxially grown crystalline film in the air. In this embodiment, photoresist is also used as tether. This photoresist can also be used as the protective layer 1 itself.

[0079] (Protective Layer 1) Next, the protective layer 1 contained in the laminate 1 will be described. The protective layer 1 is a layer formed adjacent to the semiconductor layer 1 in order to protect the semiconductor layer 1. The semiconductor layer 1, which may include an epitaxially grown crystal film, is formed on a semiconductor wafer, and then the protective layer 1 is formed. The protective layer 1 may be an organic film or an inorganic film. Examples of organic films include the above-mentioned photoresist and soluble polyimide resin. A photoresist is preferable because it allows for easy formation of the laminate 1 and is also preferable because it can be used as the above-mentioned Tether. The inorganic film may be a film formed by vapor phase growth or a film formed by a coating method. Silicon, titanium, tungsten, oxides, and nitrides are preferable as inorganic films in terms of heat resistance. The protective layer 1 is preferably at least one of an oxide film and a nitride film from the viewpoint of ease of film formation, and a layer containing at least one of silicon oxide and silicon nitride is more preferable from the viewpoint of workability when partially removing the adhesive layer described below. Silicon dioxide (SiO 2 ) is particularly preferably contained.

[0080] From the viewpoint of protecting the semiconductor layer 1, the thickness of the protective layer 1 is preferably 0.1 μm or more and less than 5 μm, preferably 0.1 μm or more, and more preferably 0.3 μm or more. When the thickness of the protective layer 1 is 0.1 μm or more, it becomes easier to obtain the effect of preventing damage to the semiconductor layer 1 when laminating a layer including the semiconductor layer 1 on the laser-absorbent temporary adhesive layer 1. Furthermore, when the thickness of the protective layer 1 is 0.3 μm or more, the effect of suppressing damage to the semiconductor layer 1 when laser transferring the semiconductor layer 1 from the laminate 1 to the laminate 2 is enhanced. In addition, the thickness of the protective layer 1 is preferably thinner than 5 μm, and particularly when the protective layer 1 is an inorganic film, the time required for film formation can be shortened. When the protective layer 1 is produced as an inorganic film, it can be produced by a known method such as CVD technology.

[0081] [Characteristics of the laminate 1] The number of small pieces of the semiconductor layer 1 mounted on the laminate 1 of this embodiment is 5 pieces / cm 2 ~50,000 pieces / cm 2 is preferable, and 5 pieces / cm 2 More preferably, 10 particles / cm2 The number of semiconductor layers 1 is set to 5 / cm 2 By doing so, the effect of improving throughput by using laser transfer is enhanced. In addition, since the laser can be accurately irradiated onto each small piece of the semiconductor layer 1, the number of small pieces of the semiconductor layer 1 mounted on the laminate 1 of this embodiment can be increased to 50,000 pieces / cm. 2 Preferably, it is equal to or less than 10,000 particles / cm, and more preferably 10,000 particles / cm 2 The following is the result.

[0082] The laminate 1 of this embodiment may have another layer between them, as long as the laser-absorbent temporary adhesive layer 1, protective layer 1, and semiconductor layer 1 are laminated in this order on the laser-transparent substrate 1. The laminate 1 preferably has the above-mentioned photoresist between the laser-absorbent temporary adhesive layer 1 and the protective layer 1. However, the protective layer 1 is formed adjacent to the semiconductor layer 1, and the laser-transparent substrate 1 and the semiconductor layer 1 are located on the outermost surfaces of the laminate 1.

[0083] [Method for manufacturing laminate 1] Next, a detailed description will be given of a method for manufacturing laminate 1. The laminate 1 can be formed by forming a laser-absorbent temporary adhesive layer 1 on a laser-transparent substrate 1, and then pressure-bonding the laser-absorbent temporary adhesive layer 1 and the semiconductor layer 1 with the protective layer 1 described above.

[0084] An example of a manufacturing method for the laminate 1 will be described. A varnish prepared by dissolving the material components of the laser-absorbent temporary adhesive layer 1 in a solvent is applied to a laser-transmissive substrate 1, followed by heat curing to produce the laser-absorbent temporary adhesive layer 1. A laminate having a single layer of the laser-absorbent temporary adhesive layer 1 on a laser-transmissive substrate 1 will be referred to as laminate α hereinafter. When preparing the laser-absorbent temporary adhesive layer 1 by a coating method, any coating method can be selected, including spin coating using a spinner, spray coating, roll coating, and slit die coating. After coating, the laser-absorbent temporary adhesive layer 1 is preferably dried at a temperature ranging from 50°C to 150°C for 1 minute to several tens of minutes using a hot plate, drying oven, infrared radiation, or the like. Thereafter, if necessary, the layer is heated and cured at a temperature ranging from 100°C to 500°C for several minutes to several hours. The thickness of the laser-absorbent temporary adhesive layer 1 at this time is preferably 1.0 μm to 30 μm. The thickness can be measured using a scanning electron microscope, an optical film thickness gauge, a step gauge, or the like. When the laser-absorbing temporary adhesive layer 1 includes a laser-absorbing layer 1 and a temporary adhesive layer 2, the laser-absorbing layer 1 and the temporary adhesive layer 2 can be manufactured using a varnish in which the material components of the laser-absorbing layer 1 are dissolved in a solvent, and a varnish in which the material components of the temporary adhesive layer 2 are dissolved in a solvent, in the same manner as for the laser-absorbing temporary adhesive layer 1. A laminate having a laser-absorbing temporary adhesive layer 1 consisting of two layers, the laser-absorbing layer 1 and the temporary adhesive layer 2, on a laser-transparent substrate 1 in this manner will hereinafter be referred to as laminate β.

[0085] The semiconductor layer 1 with the protective layer 1 can be directly stacked on the laser-absorbing temporary adhesive layer 1 or temporary adhesive layer 2 on the laminate α, β using a mounter, a flip-chip mounting machine, etc., but if necessary, it can also be pressed using a vacuum laminator, a wafer bonder, or a press.

[0086] Alternatively, there is a lamination method as described in the aforementioned Non-Patent Document 2 (Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803), which is as follows. This lamination method is described using FIGS. 6A, 6B, 6C, 6D, 6E, 6F, and 6G. A sacrificial layer (52) and a semiconductor layer 1 (14) are formed in this order on a semiconductor wafer (51) (FIG. 6A). After the semiconductor layer 1 (14) and the sacrificial layer (52) are separated into small pieces (FIG. 6B), a photoresist layer (54) is formed to cover the small pieces consisting of the semiconductor layer 1 (14) and the sacrificial layer (52) (FIG. 6C). At this time, the photoresist layer (54) is partially patterned so that the sacrificial layer can be removed (FIG. 6D). Thereafter, the sacrificial layer (reference numeral 52) is removed with a chemical solution, and the photoresist layer (reference numeral 54) is left as it is, and a laminate 0″ (reference numeral 501) can be formed, which is a bridge structure in which the semiconductor layer 1 (reference numeral 14) and the semiconductor wafer (reference numeral 51) are connected by a hollow (reference numeral 55) (FIG. 6E). After that, the laser absorption of a laminate α (reference numeral 502) which is formed by laminating a laser-absorbent temporary adhesive layer 1 (reference numeral 12) on a laser-transparent substrate 1 (reference numeral 11) which has been separately prepared, is performed. By pressing the photoresist layer (reference numeral 54) side of the laminate 0 ″ (reference numeral 501) onto the temporary adhesive layer 1 (reference numeral 12) side (FIG. 6F), the bridge structure of the photoresist layer (reference numeral 54) is broken, the bridge structure of the photoresist layer (reference numeral 54) and the semiconductor wafer (reference numeral 51) are separated, and the photoresist layer (reference numeral 54) and the semiconductor layer 1 (reference numeral 14) are stacked in this order on the laminate α (reference numeral 502). A laminate 1 ′ (reference numeral 101) can be obtained (FIG. 6G). In the process illustrated in FIGS. 6F and 6G, a laminate β may be used instead of the laminate α. In this case, by pressing the photoresist side of the laminate 0 ″ onto the temporary adhesive layer 2 side of the laminate β, the bridge structure of the photoresist is broken and separated, and a laminate 1 ′ in which the photoresist and the semiconductor layer 1 are stacked in this order on the laminate β is obtained.

[0087] In the process of obtaining the above-mentioned laminate 0", a sacrificial layer (reference numeral 52), a semiconductor layer 1 (reference numeral 14), and a protective layer 1 (reference numeral 13) are formed in this order on a semiconductor wafer (reference numeral 51), and the semiconductor layer 1 (reference numeral 14), the sacrificial layer (reference numeral 52), and the protective layer 1 (reference numeral 13) are divided into small pieces. After that, a photoresist layer (reference numeral 54) is formed so as to cover the small pieces consisting of the semiconductor layer 1 (reference numeral 14), the sacrificial layer (reference numeral 52), and the protective layer 1 (reference numeral 13). In this manner, a laminate 0 (reference numeral 503), which is a bridge structure prior to obtaining the laminate 1 of the present invention, can be produced (FIG. 7A), as shown in FIGS. 7A and 7B, by the same method as above (FIG. 7A). Then, by using laminate 0 (reference numeral 503) instead of laminate 0″, and pressing the photoresist layer (reference numeral 54) side of laminate 0 (reference numeral 503), which is the bridge structure, to the laser-absorbing temporary adhesive layer 1 (reference numeral 12) side of laminate α (reference numeral 502), the bridge structure of the photoresist layer (reference numeral 54) is broken, the bridge structure of the photoresist layer (reference numeral 54) is separated from the semiconductor wafer (reference numeral 51), and a laminate 1 (reference numeral 100) can be obtained in which the photoresist layer (reference numeral 54), protective layer 1 (reference numeral 13), and semiconductor layer 1 (reference numeral 14) are stacked in this order on laminate α (reference numeral 502) ( FIG. 7B ).

[0088] When dry etching is used to pattern the adhesive layer described below, the protective layer 1 can be used as a dry etching mask. In this case, if the protective layer 1 is a photoresist, the selectivity of the dry etching rate will be insufficient, so the protective layer 1 preferably includes an inorganic film having a dry etching selectivity with the adhesive layer. The inorganic film is preferably formed immediately after the formation of the semiconductor layer 1 including the epitaxial crystal growth film. On the other hand, when wet etching is used to pattern the adhesive layer, the protective layer 1 is not limited to the above.

[0089] The pressure applied when laminating the semiconductor layer 1 with the protective layer 1 can be optimally selected depending on the adhesive strength of the laser-absorbent temporary adhesive layer 1, and is selected from the range of 0.05 MPa to 5.0 MPa. The pressure is preferably 2.0 MPa or less, as this can avoid damage to the semiconductor layer 1 and prevent the semiconductor layer 1 from being embedded in the laser-absorbent temporary adhesive layer 1. Furthermore, when laminating the semiconductor layer 1, it is also possible to apply pressure while heating as necessary. Heating increases the flexibility of the laser-absorbent temporary adhesive layer 1, allowing the semiconductor element to be pressure-bonded at a lower pressure.

[0090] Furthermore, by providing alignment marks on the laminate 1 in advance, it becomes easier to adjust the transfer position in the subsequent operations.

[0091] [Laminate 2] Next, a laminate 2 (reference numeral 200) in which an adhesive layer (reference numeral 22) is laminated on a support substrate 2 (reference numeral 21), as shown in FIG. 2A, for example, will be described.

[0092] (Support Substrate 2) First, the support substrate 2 included in the laminate 2 will be described. The support substrate 2 is not particularly limited, but substrates such as glass, quartz, silicon wafer, sapphire substrate, ceramic substrate, metal substrate, semiconductor substrate, ceramic substrate, and further, circuit substrates in which circuit constituent materials are disposed on these substrates are used. From the viewpoint of handling the substrate, the thickness of the support substrate 2 is preferably 0.3 mm to 5 mm.

[0093] (Adhesive Layer) Next, we will explain the adhesive layer included in the laminate 2. The adhesive layer retains adhesiveness even after undergoing heat curing or a curing treatment in which a crosslinking agent or a curing agent reacts, and an article held by the adhesive layer can be reversibly held and released.

[0094] The adhesive layer is an adhesive resin layer. Resins that can be contained in the adhesive layer include, but are not limited to, polyimide, polyimide precursor, polybenzoxazole, polybenzoxazole precursor, urethane resin, novolac resin, polyhydroxystyrene, polyester resin, acrylic resin, aramid resin, silicone, and polyimide silicone resin, each having a glass transition temperature of 100° C. or less.

[0095] The adhesive layer adheres to the semiconductor layer 1 when the laminate 3 is formed. During the subsequent manufacturing of the semiconductor device, the adhesive layer preferably has heat resistance and mechanical properties that allow the semiconductor layer 1 to be directly bonded to a circuit board while the adhesive layer and semiconductor layer 1 are in an adhered state. The heat resistance is preferably 200°C or higher, and more preferably 250°C or higher. The heat resistance refers to the temperature at which the film obtained by curing the adhesive layer loses 1% mass. Possessing mechanical properties means that when the semiconductor layer 1 is directly bonded to the circuit board at high temperatures, protrusion due to melting of the adhesive layer does not adversely affect the direct bond.

[0096] The adhesive layer preferably has a modulus of elasticity at 200°C of 0.1 MPa or more, more preferably 0.3 MPa or more, and even more preferably 0.5 MPa or more. Since solvent etching of the semiconductor layer 1, removal of the photoresist, or removal of the protective layer 1 may be performed while the adhesive layer and the semiconductor layer 1 are in adhesion, the adhesive layer preferably has chemical resistance. Examples of solvents that can be used include etching solvents such as hydrofluoric acid, buffered hydrofluoric acid, hydrochloric acid, sulfuric acid, iron chloride, and SC-2 (aqueous hydrochloric acid / hydrogen peroxide solution), resist solvents, developer (2.38% TMAH), SC-1 (aqueous ammonia / hydrogen peroxide solution), and resist stripping solvents.

[0097] The elastic modulus can be calculated by dynamic mechanical analysis (DMA) measurement, the details of which are as described in the Examples below.

[0098] In view of the above-mentioned properties, the adhesive layer preferably contains a polyimide resin. The polyimide resin preferably contains a polyimide copolymer (A) having at least an acid dianhydride residue and a diamine residue. The diamine residue preferably contains a diamine residue (A0) represented by formula (10), where n is preferably a natural number of 1 or more and 100 or less, more preferably 1 or more and 50 or less. The diamine residue (A0) preferably accounts for 50.0 to 95.0 mol % of the total diamine residues in the polyimide copolymer (A), ie, 100.0 mol %.

[0099] Furthermore, the polyimide copolymer (A) preferably contains a diamine residue (A3) having a phenolic hydroxyl group, and the polyimide copolymer (A) preferably contains 1.0 to 30.0 mol % of the diamine residue (A3) relative to 100.0 mol % of all diamine residues in the polyimide copolymer (A).

[0100]

[0101] In formula (10), R 21 and R 22 may be the same or different and represent an alkylene group or a phenylene group having 1 to 30 carbon atoms. 23 ~R 26 may be the same or different and represent an alkyl group having 1 to 30 carbon atoms, a phenyl group, or a phenoxy group.

[0102] The polyimide copolymer (A) has an acid dianhydride residue and a diamine residue, and can be produced by copolymerizing them. In order to impart adhesiveness at room temperature, the polyimide copolymer (A) can be produced by copolymerizing a diamine residue (A0) as a diamine component. Alternatively, the polyimide copolymer (A) may be produced by copolymerizing a diamine having the diamine residue (A0) with a diamine having the diamine residue (A3).

[0103] Furthermore, copolymerization of the diamine residue (A0) with the diamine residue (A3) allows the polyimide copolymer (A) to be crosslinked with a crosslinking agent described later. In addition, the effect of hydrogen bonding of the hydroxyl groups of the diamine residue (A3) is effective in maintaining a constant modulus of elasticity when the pressure-sensitive adhesive layer is heated.

[0104] The polyimide copolymer (A) constituting the adhesive layer preferably contains 50.0 to 95.0 mol% of diamine residues (A0) relative to 100.0 mol% of all diamine residues. By containing 50.0 mol% or more of diamine residues (A0), the adhesive layer exhibits good adhesion, and the semiconductor layer 1 can be laminated to the adhesive layer with a high probability. By containing 95.0 mol% or less of diamine residues (A0) relative to 100 mol% of all diamine residues, the stability of the adhesive layer over time is improved, and displacement of the semiconductor layer 1 when stored in the state of the laminate 3 described below can be reduced. More preferably, the polyimide copolymer (A) preferably contains 80.0 to 93.0 mol% of diamine residues relative to 100.0 mol% of all diamine residues. By containing 80 mol% or more, the adhesive layer exhibits good flexibility, and when the semiconductor layer 1 is transferred from the laminate 1 described below with a laser, the semiconductor layer 1 can be laminated with high positional accuracy. Furthermore, by having a content of 93 mol % or less, the material can be passed through a process that involves heat and pressure, such as direct bonding.

[0105] In addition, the polyimide copolymer (A) constituting the adhesive layer of this embodiment preferably contains a diamine residue (A3) having a phenolic hydroxyl group. When the polyimide copolymer (A) contains the diamine residue (A3), the hydroxyl groups of the diamine (A3) hydrogen bond, thereby maintaining a constant modulus of elasticity at high temperatures and suppressing extrusion of the adhesive layer during the direct bonding process. Furthermore, when a crosslinking agent is added, the resin on the surface of the adhesive layer is crosslinked, reducing cohesive failure of the adhesive layer when the semiconductor layer 1 laminated on the adhesive layer is separated from the adhesive layer, thereby preventing adhesive residue on the surface of the semiconductor layer 1. In this case, adhesive residue refers to the adhesive layer remaining on the surface of the semiconductor layer 1 after the semiconductor layer 1 is separated.

[0106] The content of the diamine residue (A3) having a phenolic hydroxyl group is preferably 1.0 mol to 30.0 mol % relative to 100.0 mol % of all diamine residues in the polyimide copolymer (A). This stabilizes the elastic modulus at high temperatures, thereby stably holding the semiconductor element, and further improves the adhesive transfer suppression effect when crosslinked with a crosslinking agent.

[0107] The content of the diamine residue (A3) having a phenolic hydroxyl group is more preferably 5.0 mol% to 20.0 mol% relative to 100.0 mol% of all diamine residues in the polyimide copolymer (A). When the polyimide copolymer (A) contains 5.0 mol% or more of the diamine residue (A3) having a phenolic hydroxyl group relative to 100.0 mol% of all diamine residues in the polyimide copolymer (A), crosslinking on the film surface proceeds uniformly, further suppressing adhesive residue and improving chemical resistance. Furthermore, when the polyimide copolymer (A) contains 20.0 mol% or less of the diamine residue (A3) relative to 100.0 mol% of all diamine residues in the polyimide copolymer (A), semiconductor elements can be stably held.

[0108] Specific examples of the diamine residue (A3) having a phenolic hydroxyl group include those represented by the formulas (3) and (4) shown in the description of the laser-absorbent temporary adhesive layer 1, where R 7 and R 9 (OH) 2 When represents a bisaminophenol derivative residue, specific examples thereof include the bisaminophenol derivative residues listed above.

[0109] Furthermore, the polyimide copolymer (A) may contain diamine residues other than the diamine residue (A0) and the diamine residue (A3) having a phenolic hydroxyl group. The diamine residues other than the diamine residue (A0) and the diamine residue (A3) having a phenolic hydroxyl group are preferably contained in an amount of 0.1 mol % or more and 40.0 mol % or less, based on 100.0 mol % of all diamine residues in the polyimide copolymer (A).

[0110] Specific examples of diamine residues other than the diamine residue (A0) and the diamine residue (A3) include residues of p-phenylenediamine, 9,9-bis(4-aminophenyl)fluorene, 4'-bis(4-aminophenoxy)biphenyl, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl sulfone, 4,4'-diaminobenzophenone, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, etc. The polyimide copolymer (A) may contain only one type of diamine residue other than the diamine residue (A0) and the diamine residue (A3), or may contain two or more types.

[0111] The polyimide copolymer (A) contains an acid dianhydride residue, preferably an aromatic tetracarboxylic dianhydride residue. The acid dianhydride residue may contain a residue of a known acid dianhydride. Specific examples of the aromatic tetracarboxylic dianhydride residue include those represented by the formulas (1) and (2) described above in the description of the laser-absorbent temporary adhesive layer 1, such as R 1 or R 3 (COOR 5 ) 2 The polyimide copolymer (A) may contain only one type of aromatic tetracarboxylic dianhydride residue or two or more types of aromatic tetracarboxylic dianhydride residues.

[0112] Furthermore, the polyimide copolymer (A) may contain a residue of a tetracarboxylic dianhydride having an aliphatic ring to the extent that the heat resistance of the polyimide copolymer (A) is not impaired. Specific examples of the residue of a tetracarboxylic dianhydride having an aliphatic ring include residues of 1,2,3,4-cyclobutanetetracarboxylic dianhydride and 1,2,3,4-cyclopentanetetracarboxylic dianhydride. The polyimide copolymer (A) may contain only one type of residue of the tetracarboxylic dianhydride, or may contain two or more types.

[0113] From the viewpoint of adhesiveness, the weight average molecular weight of the polyimide copolymer (A) is preferably 500 to 1,000,000. This weight average molecular weight is a value measured by gel permeation chromatography (hereinafter sometimes abbreviated as GPC) and converted into polystyrene.

[0114] The molecular weight of the polyimide copolymer (A) can be adjusted by using equimolar amounts of the acid dianhydride component and the diamine component used in the synthesis, or by using an excess of either one. Either the acid dianhydride component or the diamine component can be used in excess, and the polymer chain ends can be blocked with an end-capping agent such as an acid component or an amine component. Dicarboxylic acids or their anhydrides are preferably used as end-capping agents for the acid component, and monoamines are preferably used as end-capping agents for the amine component. In this case, it is preferable to use equimolar amounts of the acid equivalent of the tetracarboxylic acid component, including the end-capping agent for the acid component or the amine component, and the amine equivalent of the diamine component.

[0115] Known monoamines can be used as the end-capping agent for the amine component, and among them, aniline, aminophenol, etc. are preferred. Two or more of these may be used as the end-capping agent for the amine component.

[0116] Preferred examples of the acid component end-capping agent include monocarboxylic acids, monoacid chloride compounds, and monoactive ester compounds, such as acid anhydrides such as phthalic anhydride, maleic anhydride, nadic anhydride, and cyclohexanedicarboxylic anhydride, monocarboxylic acids such as 3-carboxyphenol, and monoacid chloride compounds in which the carboxyl group of these monocarboxylic acids is converted to an acid chloride, monoacid chloride compounds in which only one carboxyl group of dicarboxylic acids such as phthalic acid and maleic acid is converted to an acid chloride, and active ester compounds obtained by reacting a monoacid chloride compound with N-hydroxybenzotriazole. Two or more of these acid component end-capping agents may be used.

[0117] The molar ratio of the acid dianhydride component / diamine component in the polyimide copolymer (A) can be adjusted appropriately so that the viscosity of the resin composition falls within a range that makes it easy to use in coating, etc., and the molar ratio of the acid dianhydride component / diamine component is generally adjusted within a range of 100 / 100 to 100 / 95, or 100 / 100 to 95 / 100. If the molar ratio of the acid dianhydride component / diamine component in the polyimide copolymer (A) is outside the above range, the molecular weight of the resin decreases, the mechanical strength of the formed film decreases, and uneven adhesion tends to occur, so it is preferable to adjust the molar ratio within a range that stabilizes adhesion.

[0118] The polyimide copolymer (A) may be a polyimide precursor that undergoes ring closure upon heating to become a polyimide copolymer, a polyimide copolymer that has undergone ring closure upon heating, or a polyimide precursor in which a portion of a polyimide copolymer has undergone ring closure upon heating.

[0119] There are no particular limitations on the method for polymerizing the polyimide copolymer (A). For example, when polymerizing polyamic acid, which is a polyimide precursor, an acid dianhydride and a diamine are stirred in a solvent at 0 to 100°C for 1 to 100 hours to obtain a polyamic acid resin solution. If the polyimide resin is soluble in the solvent, the polyamic acid is polymerized, and then the temperature is raised to 120 to 300°C and the mixture is stirred for 1 to 100 hours to convert it to polyimide, thereby obtaining a polyimide resin solution. At this time, toluene, o-xylene, m-xylene, p-xylene, or the like may be added to the reaction solution, and the water produced by the imidization reaction may be removed by azeotropy with the solvent.

[0120] The adhesive layer may contain a crosslinking agent. Examples of crosslinking agents include polyfunctional acrylics, polyfunctional epoxies, polyfunctional methylol compounds, and polyfunctional styrene compounds. A particularly preferred crosslinking agent is a dimer acid-modified epoxy resin. A dimer acid-modified epoxy resin has a structure in which the terminals of the dimer acid are epoxidized and has a flexible skeleton. Therefore, even when crosslinked with the phenolic hydroxyl groups contained in the polyimide copolymer (A), the adhesive layer can be improved in chemical resistance and heat resistance without losing its flexibility, which is preferable.

[0121] Dimer acid-modified epoxy resins are those in which a glycidyl group has been introduced into a dibasic acid obtained by dimerizing an unsaturated fatty acid. Examples of dimer acid-modified epoxy resins include oleic acid, elaidic acid, octadecenoic acid, linoleic acid, palmitoleic acid, myristoleic acid, linolenic acid, isooleic acid, eicosenoic acid, docosenoic acid, branched octadecenoic acid, branched hexadecenoic acid, and undecylenic acid. Examples of dimer acid-modified epoxy resins include, but are not limited to, JER (registered trademark) 871 and JER (registered trademark) 872 (manufactured by Mitsubishi Chemical Corporation) and ERISYSGS-120 (manufactured by CVC Corporation), in which a glycidyl group has been introduced into a linolenic acid dimer.

[0122] The amount of the crosslinking agent added is preferably 0.1 to 20 parts by mass relative to 100 parts by mass of the polyimide copolymer (A). When the amount is 0.1 part by mass or more, chemical resistance can be imparted to the adhesive layer. When the amount is 20 parts by mass or less, the adhesive layer can maintain appropriate adhesiveness and flexibility, and the semiconductor layer 1 can be stably held in the state of the laminates 3 and 4 described below.

[0123] The adhesive layer may contain a curing accelerator, if necessary, to accelerate the curing of the polyimide copolymer (A) and the crosslinking agent.

[0124] Examples of the curing accelerator include imidazoles, tertiary amines or their salts, and organic boron salt compounds, with imidazoles being preferred. Specific examples of imidazoles include imidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenyl-1H-imidazole, 2,4-diamino-6-[2'-ethyl-4-methylimidazolyl-(1')]-ethyl-s-triazine, and 2-methylimidazole isocyanuric acid adduct. Preferred commercially available imidazoles include Curesol (registered trademark) 2E4MZ and Curesol (registered trademark) 2E4MZ-CN (manufactured by Shikoku Chemicals Corporation).

[0125] The amount of the curing accelerator added is preferably 0.1 to 5.0 parts by mass per 100 parts by mass of the polyimide copolymer (A). The amount of the curing accelerator added is more preferably 0.3 to 1.0 part by mass per 100 parts by mass of the polyimide copolymer (A). When the amount of the curing accelerator added is within this range, a sufficient crosslinking promoting effect is obtained, and the stability of the adhesive layer is improved.

[0126] The adhesive layer may also contain an imidization accelerator. When the polyimide copolymer (A) is a polyamic acid resin, the imidization accelerator can convert it into a polyimide resin by heating at a low temperature for a short time. The conversion of the polyamic acid resin into a polyimide resin improves heat resistance.

[0127] Specific examples of the imidization accelerator include, but are not limited to, pyridine, β-picoline, quinoline, imidazole, 2-methylimidazole, 1,2-dimethylimidazole, 2-phenylimidazole, triethylamine, m-hydroxybenzoic acid, 4-hydroxyphenylpropionic acid, p-phenolsulfonic acid, p-aminophenol, and p-aminobenzoic acid.

[0128] The content of the imidization accelerator is preferably 3 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the polyimide copolymer (A). If the content of the imidization accelerator is within this range, imidization can be completed even with heat treatment at a lower temperature, and the amount of imidization accelerator remaining in the adhesive layer after heat treatment can be minimized, thereby suppressing the generation of volatile components. The imidization accelerator may be added during or after polymerization of the polyimide copolymer (A).

[0129] The adhesive layer may contain an ultraviolet absorber or a dye. This enables the substrate to be peeled off using a laser in the substrate peeling step (VI) described below. Preferred examples of the ultraviolet absorber or dye used in the adhesive layer are the same as those described above for the laser-absorbent temporary adhesive layer 1.

[0130] The thickness of the adhesive layer formed on the support substrate 2 is preferably 1.0 to 30 μm. When the thickness of the adhesive layer is 1.0 μm or more, the transferred semiconductor layer 1 can be laminated on the adhesive layer in the semiconductor layer 1 transfer step by laser irradiation, which will be described later. Furthermore, when the thickness of the adhesive layer is 30 μm or less, unevenness in the in-plane uniformity of the adhesive layer is reduced, allowing the semiconductor element to be held uniformly. A more preferred range for the thickness of the adhesive layer is 2.5 to 10 μm. When the thickness of the adhesive layer is 2.5 μm or more, the semiconductor layer 1 can be laminated on the adhesive layer with good positional accuracy in the laser transfer step of the semiconductor layer 1. Furthermore, when the thickness of the adhesive layer is 10 μm or less, poor bonding due to protrusion of the adhesive layer and misalignment of the semiconductor layer 1 due to flow of the adhesive layer can be reduced in the direct bonding step, which will be described later.

[0131] The thickness of the adhesive layer can be measured using a scanning electron microscope, an optical film thickness meter, a step gauge, a laser microscope, or the like.

[0132] The above-mentioned laser absorbing layer 2 may be present between the support substrate 2 and the adhesive layer. In this case, for example, as shown in FIG. 2B , the laminate 2 (reference numeral 200) is obtained by laminating the laser absorbing layer 2 (reference numeral 23) and the adhesive layer (reference numeral 22) in this order on the support substrate 2 (reference numeral 21). This makes it possible to apply a peeling method using a laser in the substrate peeling step in step (VI) described below. The detailed description of the laser absorbing layer 2 is the same as that of the laser absorbing layer 1 described above.

[0133] An example of a method for forming an adhesive layer on the support substrate 2 is a method in which a varnish prepared by dissolving the above-mentioned components that can be contained in the adhesive layer in a solvent is applied to the support substrate 2. After application, the varnish may be cured by heating.

[0134] [Method for Manufacturing Laminate 2] Next, a detailed description will be given of a method for manufacturing the laminate 2. The laminate 2 can be manufactured by forming an adhesive layer on the support substrate 2.

[0135] An example of a method for producing the laminate 2 will be described. The adhesive layer can be formed by applying a varnish, in which the components that can be contained in the adhesive layer are dissolved in a solvent, to the support substrate 2 and then heat-curing the varnish. When preparing the adhesive layer by coating, any coating method can be selected, including spin coating using a spinner, spray coating, roll coating, and slit die coating. After coating, the adhesive layer is preferably dried at a temperature between 50°C and 150°C for 1 minute to several tens of minutes using a hot plate, drying oven, infrared radiation, or the like. Thereafter, if necessary, the adhesive layer is further heat-cured at a temperature between 100°C and 500°C for several minutes to several hours. The thickness of the adhesive layer at this time is preferably 1.0 μm to 30 μm. The thickness can be measured using a scanning electron microscope, an optical film thickness gauge, a step gauge, or the like.

[0136] When the laser absorbing layer 2 is provided between the support substrate 2 and the adhesive layer, the laser absorbing layer 2 can be formed on the support substrate 2, and then an adhesive layer can be further formed thereon.

[0137] [Method for manufacturing laminate 3] Next, as shown in FIG. 3A , for example, a laminate 3 (reference numeral 300) according to one embodiment of the present invention will be described, in which an adhesive layer (reference numeral 22), a semiconductor layer 1 (reference numeral 14), and a protective layer 1 (reference numeral 13) are laminated in this order on a support substrate 2 (reference numeral 21).

[0138] The laminate 3 is preferably a laminate in which a support substrate 2, an adhesive layer, a semiconductor layer 1, and a protective layer 1 are laminated in this order, and the adhesive layer has a patterned shape.

[0139] An example of a method for manufacturing the laminate 3 will be described, but the present invention is not limited to this example. For example, as shown in Fig. 3A, a laminate 1 (reference numeral 100) is formed by laminating a laser-absorbent temporary adhesive layer 1 (reference numeral 12), a protective layer 1 (reference numeral 13), and a semiconductor layer 1 (reference numeral 14) in this order on a laser-transmitting substrate 1 (reference numeral 11), and a laminate 2 (reference numeral 200) is formed by laminating an adhesive layer (reference numeral 22) on a support substrate 2 (reference numeral 21), and the laminate 1 (reference numeral 100) is used, and the surface of the semiconductor layer 1 (reference numeral 14) side of the laminate 1 (reference numeral 100) and the surface of the adhesive layer (reference numeral 22) side of the laminate 2 (reference numeral 200) are made to face each other; The laser-absorbent temporary adhesive layer 1 (symbol 12) is irradiated with a laser (symbol 15) from the surface opposite to the surface of the semiconductor layer 1 (symbol 14) of the laminate 1 (symbol 100) while transmitting through the laser-transparent substrate 1 (symbol 11), and the protective layer 1 (symbol 13) and the semiconductor layer 1 (symbol 14) are laminated. The structure 1 is transferred to the laminate 2 (symbol 200) to form the laminate 3 (symbol 300). By performing this in this order, a laminate 3 (symbol 300) in which the support substrate 2 (symbol 21), adhesive layer (symbol 22), semiconductor layer 1 (symbol 14), and protective layer 1 (symbol 13) are laminated in this order is obtained.

[0140] In step (I), it is preferable to fix the laminate 1 and laminate 2 prepared by the above-mentioned method so that the surface of laminate 1 facing the semiconductor layer 1 and the surface of laminate 2 facing the adhesive layer are opposed to each other, and the laminates 1 and 2 are parallel to each other. In order to prevent misalignment due to the weight of the semiconductor layer 1 during transfer, the opposed laminates 1 and 2 are preferably arranged with the laminate 1 facing upward. The laminates 1 and 2 are arranged at a constant distance, and the distance between the semiconductor layer 1 of laminate 1 and the adhesive layer of laminate 2 can be selected depending on the size and thickness of the semiconductor layer 1, and is preferably in the range of 0 μm to 100 μm.

[0141] When the semiconductor layer 1 is a thin film having a thickness of 10 μm or less, even a slight impact generated during laser irradiation may damage the thin semiconductor layer 1. Therefore, the laser-absorbing temporary adhesive layer 1 preferably has a two-layer or more structure including the laser-absorbing layer 1 and the temporary adhesive layer 2.

[0142] For the purpose of transfer alignment, the laser transparent substrate 1 and the support substrate 2 may have alignment marks.

[0143] Next, step (II) will be described. In the laminate 1 and laminate 2 arranged in the above step (I), a laser is irradiated onto the laser-absorbent temporary adhesive layer 1 from the surface of the laminate 1 opposite to the surface on the semiconductor layer 1 side, while transmitting the laser through the laser-transmitting substrate 1.

[0144] The laminate 3 produced in step (II) may contain layers other than the protective layer 1, the semiconductor layer 1, the adhesive layer, and the support substrate 2. In particular, in step (II), when transferring the structure 1 in which the protective layer 1 and the thin-film semiconductor layer 1 are laminated, for example, as shown in FIG. 3B, at least the laser-absorbent temporary adhesive layer 1 (symbol 12), the protective layer 1 (symbol 13), and the semiconductor layer 1 (symbol 14) are integrated and transferred simultaneously, and the adhesive layer (symbol 22), the semiconductor layer 1 (symbol 14), the protective layer 1 (symbol 13), and the laser-absorbent temporary adhesive layer 1 (symbol 12) are laminated in this order on the support substrate 2 (symbol 21) to form a laminate 4 (symbol 600) is preferably formed because the thin-film semiconductor layer 1 (symbol 14) can be transferred without damage.

[0145] The type of laser can be selected depending on the wavelength to be used, and includes solid-state lasers such as YAG laser, YVO4 laser, fiber laser, and semiconductor laser, and gas lasers such as carbon dioxide laser, excimer laser, and argon laser. The beam shape of the irradiated laser is not limited, and the laser spot size may be smaller than the size of the semiconductor layer 1. However, it is preferable that the laser spot size is such that the laser does not hit the semiconductor layer 1 adjacent to the semiconductor layer 1 to be transferred. The laser can be selected with any energy amount. From the viewpoint of stability of the laser energy amount, the laser energy amount is 1 mJ / cm. 2 The above is preferable, and from the viewpoint of preventing damage to the semiconductor layer 1 and shortening the processing time, 1000 mJ / cm 2 More preferably, the laser energy amount is 10 mJ / cm or less. 2 Above, 500mJ / cm 2 The following is the result.

[0146] By using the laminate 1 according to one embodiment of the present invention, transfer is possible even with low laser irradiation energy, and further, even when the amount of laser irradiation energy is changed, the influence of positional accuracy can be reduced.

[0147] Furthermore, in step (II), when the structure in which the protective layer 1 and the semiconductor layer 1 are laminated is transferred to the laminate 2, the laminate 2 may be heated. Heating the laminate 2 improves the retention of the semiconductor layer 1 on the adhesive layer after transfer. When heating the laminate 2, the heating temperature is preferably 100° C. or less, as this prevents warping of the laminate 2 due to heat and enables transfer with high positional accuracy.

[0148] In step (II), the transfer of the structure in which the protective layer 1 and the semiconductor layer 1 are stacked onto the laminate 2 is preferably performed while adjusting the position to match the actual mounting location of the semiconductor layer 1 in the semiconductor device to be fabricated. For example, when fabricating a device for Si photonics, the semiconductor layer 1 is transferred onto the laminate 2 while shifting the pitch to match the waveguide size and arrangement of the optical circuit board. Next, the laminate 3 to which the semiconductor layer 1 has been transferred and the optical circuit board are placed opposite each other, and the semiconductor layer 1 is pressure-bonded and transferred to the circuit board, thereby fabricating an optical circuit board on which the semiconductor layer 1 is mounted.

[0149] In step (II), as shown in FIG. 8A, the laser-absorbent temporary adhesive layer 1 (symbol 12), the protective layer 1 (symbol 13), and the semiconductor layer 1 (symbol 14) are laminated to form a laminate 2 (symbol 200) on a support substrate 2 (symbol 21). The adhesive layer (symbol 22), the semiconductor layer 1 (symbol 14), the protective layer 1 (symbol 13), and the laser-absorbent temporary adhesive layer 1 (symbol 12) are laminated in this order to form a laminate 4 (symbol 600). Then, the laser-absorbent temporary adhesive layer 1 (symbol 12) is removed from the laminate 4 (symbol 600) (FIG. 8B). The laser-absorbent temporary adhesive layer 1 may be removed by wet cleaning with a solvent or a stripping solution, or by dry etching. At this time, it is preferable to also perform the step (III ') of removing and patterning a portion of the adhesive layer described below in one go, as this simplifies the process.

[0150] A method for producing a laminate 3 according to one embodiment of the present invention preferably includes a step (III) of removing a portion of the adhesive layer of the laminate 3 obtained in the step (II) of forming the laminate 3, and patterning the adhesive layer.

[0151] The laminate 3 preferably has a patterned shape in which a portion of the adhesive layer has been removed. The patterning here refers to, as shown in FIG. 9A , a difference in the thickness of the adhesive layer (22) between the semiconductor layer 1 (14) and the support substrate 2 (21) and the thickness of the adhesive layer (25) on the support substrate 2 (21) in a region where the semiconductor layer 1 (14) is not present. In this case, the difference in thickness between the adhesive layer (24) between the semiconductor layer 1 (14) and the support substrate 2 (21) and the adhesive layer (25) on the support substrate 2 (21) in a region where the semiconductor layer 1 (14) is not present is preferably at least 0.5 μm or more. In particular, as shown in FIG. 9B , the laminate 3 (300) preferably has only the adhesive layer (24) between the semiconductor layer 1 (14) and the support substrate 2 (21) as the adhesive layer. That is, it is preferable that the adhesive layer is removed from the laminate 3 except for the portion between the semiconductor layer 1 and the support substrate 2. Simultaneously with or after removing the adhesive layer, it is preferable to remove the protective layer 1 from the laminate 3 to expose the surface of the semiconductor layer 1. This is to facilitate bonding of the laminate 3 to a circuit board and removal of the support substrate 2 with the adhesive layer in the subsequent steps (V) and (VI). The step of removing a portion of the adhesive layer of the laminate 4 and patterning the adhesive layer is also referred to as step (III').

[0152] In one embodiment of the present invention, the method for producing a laminate 3 preferably includes a step (III-A) of dry-etching or wet-etching the adhesive layer of the laminate 3 using the semiconductor layer 1 or protective layer 1 of the laminate 3 as a mask in the step (III) of removing a portion of the adhesive layer of the laminate 3 and patterning the adhesive layer. When the laminate 3 is a laminate 4, the method for producing a laminate 3 preferably includes a step (III'-A) of dry-etching or wet-etching the adhesive layer of the laminate 4 using the semiconductor layer 1, protective layer 1, or laser-absorbent temporary adhesive layer 1 of the laminate 4 as a mask. There are no other limitations on the dry etching and wet etching, as long as the adhesive layer can be removed. In dry etching, in order to suppress damage to the semiconductor layer 1, it is preferable to perform dry etching while the protective layer 1 remains on the semiconductor layer 1.

[0153] The type of gas used for dry etching preferably has a selectivity ratio of the dry etching rate to the protective layer 1. For example, a fluorine-based gas such as a CF or SF gas, or oxygen is preferred, and more preferably, a fluorine-based gas, especially CF, is preferred because it can provide a high selectivity and a high dry etching rate. 4 or CHF 3 A mixture of at least one of the above with oxygen is preferred. As the ratio of fluorine-based gas to oxygen, the oxygen concentration (volume %) in the entire gas is preferably 5 to 98%, more preferably 50 to 95%, and even more preferably 75 to 90%. If the oxygen concentration is less than 5 volume %, the etching rate of the organic resin-based components of the protective layer 1 may be insufficient, while if it is more than 98 volume %, the etching rate of the inorganic components (particularly silicon, siloxane, and silicone-based compositions) may be insufficient.

[0154] The chemical solution used for wet etching is not particularly limited as long as it dissolves the adhesive layer and does not damage the semiconductor layer 1. Specific examples include solvents used as a solvent for the resin component of the adhesive layer when forming the adhesive layer, resist stripping solutions, etc. In this case, if the laminate 3 has a structure including the laser-absorbent temporary adhesive layer 1 and a photoresist, these may be removed at the same time.

[0155] The laminate manufacturing method of one embodiment of the present invention preferably includes a step (IV) of removing the protective layer 1 from the laminate 3. As described above, after removing the adhesive layer by dry etching or wet etching in step (III-A), removing the protective layer 1 on the semiconductor layer 1 is preferable in order to proceed with the direct bonding process of the semiconductor layer 1 in the next step. Here, if the laminate 3 has a photoresist, it is preferable to remove the photoresist together with the protective layer 1. Note that, when the laminate 3 is the laminate 4, the laminate manufacturing method of one embodiment of the present invention preferably includes a step of removing the laser-absorbent temporary adhesive layer 1 and the protective layer 1 from the laminate 4, and this step is also referred to as step (IV'). The laser-absorbent temporary adhesive layer 1 and the photoresist can be removed all at once during the dry etching or wet etching of the adhesive layer in step (III-A). Furthermore, the photoresist can be stripped using a resist stripper designed for photoresist. The protective layer 1 can be removed with an etchant solution that dissolves the protective layer 1. Examples of etchant solutions include hydrofluoric acid and phosphoric acid.

[0156] 5 , a method for manufacturing a semiconductor device according to one aspect of the present invention includes a step (V) of stacking an adhesive layer (22) and a semiconductor layer 1 (14) in this order on a support substrate 2 (21) from which the protective layer 1 has been removed from the laminate 3 obtained in the step (IV), with the surface of the semiconductor layer 1 (14) facing the surface of a circuit board (41) on which a circuit has been formed, and bonding the semiconductor layer 1 (14) of the stack to the circuit board (41) by thermocompression bonding, thereby manufacturing a semiconductor device (400). The method for manufacturing a semiconductor device preferably includes a step (VI) of removing the support substrate 2 (21) with the adhesive layer (22) from the bonded structure of the semiconductor layer 1 of the stack and the circuit board, after the step (V).

[0157] As described above, by patterning the adhesive layer in the laminate 3 in step (III) and removing the protective layer 1 in step (IV), the adhesive layer can be improved in step (V) by thermocompression bonding of the semiconductor layer 1 to the circuit board, and the peelability of the adhesive layer and the semiconductor layer 1 can be improved in step (VI). That is, by thinning or completely removing the adhesive layer other than the adhesive layer directly below the semiconductor layer 1 from the laminate 3 in step (III), only the semiconductor layer 1 can be brought into contact with and bonded to the opposing circuit board during thermocompression bonding in step (V). A schematic cross-sectional view of the laminate 3 from which the adhesive layer has been patterned and the protective layer has been removed has a patterned adhesive layer (reference numeral 22) and a semiconductor layer 1 (14) on a support substrate 2 (reference numeral 21), as shown in, for example, FIGS. 4A and 4B .

[0158] After step (V), in the next step (VI), the adhesive layer-attached support substrate 2 is peeled off and removed from the semiconductor layer 1. Prior to removal, the adhesive layer is immersed in a solvent to swell or dissolve, which facilitates peeling and removal of the adhesive layer-attached support substrate 2 from the semiconductor layer 1. In order to accelerate the swelling or dissolution of the adhesive layer due to this solvent immersion, it is preferable to pattern the adhesive layer in step (III). This is because patterning the adhesive layer allows the solvent to easily enter the space from which the adhesive layer has been removed, facilitating swelling of the adhesive layer.

[0159] Furthermore, if the adhesive layer is laser-absorbent, as shown in FIG. 10A , laser irradiation (15) may be performed from the support substrate 2 (21) side to peel the support substrate 2 (21) from the semiconductor layer 1 (14) ( FIG. 10B ). In this case, too, by patterning the adhesive layer in (III), the support substrate 2 can be peeled off by irradiating only the semiconductor layer 1 with a laser, without irradiating the entire surface of the support substrate 2 with a laser. After removing the support substrate 2, the adhesive layer can be removed to obtain a semiconductor device (400) in which the semiconductor layer 1 (14) is bonded to a circuit board (41) ( FIG. 8C ). Similarly, if the adhesive layer is not laser-absorbent but has a laser-absorbing layer 2 between it and the support substrate 2, the support substrate 2 with the adhesive layer can be peeled off from the semiconductor layer 1 by irradiating a laser from the support substrate 2 side. In this case, after removing the support substrate 2, the laser-absorbing layer 2 is removed together with the adhesive layer.

[0160] As described above, a semiconductor device can be fabricated by joining the semiconductor layer 1 to a circuit board by thermocompression bonding. The circuit board may be an SOI wafer on which an optical waveguide is formed, as shown in Non-Patent Documents 1 to 3 (Alexander W. Fang et al., Electrically pumped hybrid AlGaInAs-silicon evanescent laser, OPTICS EXPRESS, 2006, Vol. 14, No. 20, p. 9203; Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803; LUO et al., Wafer-scale die-transfer bonding technology for hybrid III / V-on-silicon photonic integrated circuit, IEEE JOURNAL OF SELECTED TOPICS IN QUANTUM ELECTRONICS, 2016, Vol. 22, No. 6, 8200612), or may be a substrate of Si, Cu, Al, or the like in order to prioritize heat dissipation. As shown in Non-Patent Documents 1 and 2 (Alexander W. Fang et al., Electrically pumped hybrid AlGaInAs-silicon evanescent laser, OPTICS EXPRESS, 2006, Vol. 14, No. 20, p. 9203; Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803), after the semiconductor layer 1 is transferred, multiple semiconductor layers 1 can be processed simultaneously on a circuit board.

[0161] The circuit board with the semiconductor layer 1 can be suitably used as a semiconductor device. Examples of the semiconductor device include semiconductor communication elements, image pickup elements, and amplifier elements. These are suitable for silicon photonics semiconductor devices that apply silicon photonics technology, such as for high-speed communication and high-speed processing in data centers and machine learning, distance sensors (lidar), healthcare (health monitors mounted on smart watches), and gas detection sensors.

[0162] In the above-described semiconductor device, after bonding the semiconductor layer 1 and the circuit board in step (V), it is preferable to remove the adhesive layer remaining after step (VI), but it does not have to be removed. Because the above-described adhesive layer is insulating, if it remains on the semiconductor device, it can prevent short circuits in the circuit board. When removing the adhesive layer, it can be removed by dissolving the adhesive layer in a solvent or by dry etching.

[0163] When transfer is performed by thermocompression bonding using the laminate of one embodiment of the present invention, transfer can be performed with high positional accuracy, so that the semiconductor layer 1 can be transferred without being misaligned from the circuit of the substrate on which it will ultimately be mounted, thereby reducing mounting defects caused by misalignment.

[0164] The present invention relates to a silicon photonics semiconductor device manufactured by transferring a compound semiconductor chip using a laser transfer method, and a method for manufacturing the same.

[0165] As explained above, the present specification discloses the following. [1] A laminate comprising a laser-absorbing temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 laminated in this order on a laser-transparent substrate 1. [2] The laminate according to the above [1], wherein the semiconductor layer 1 is a compound semiconductor. [3] The laminate according to the above [2], wherein the compound semiconductor is AlGaInAs, InGaAs, InP, InGaAsP, AlAs, InAs, GaAs, AlN, AlP, GaN, InN, or SiC. [4] The laminate according to any one of the above [1] to [3], wherein the protective layer 1 is at least one of an oxide film and a nitride film. [5] The protective layer 1 is SiO 2[6] A method for producing a laminate, comprising the steps of: (I) using a laminate 1 in which a laser-absorbent temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmissive substrate 1; and (II) using a laminate 2 in which an adhesive layer is laminated on a support substrate 2, the step of arranging a surface of the laminate 1 on the semiconductor layer 1 side and a surface of the laminate 2 on the adhesive layer side, and (II) irradiating the laser-absorbent temporary adhesive layer 1 with a laser from the surface of the laminate 1 opposite to the surface on the semiconductor layer 1 side while transmitting a laser through the laser-transmissive substrate 1 to transfer a structure in which the protective layer 1 and the semiconductor layer 1 are laminated to the laminate 2, thereby forming a laminate 3 in which the adhesive layer, the semiconductor layer 1, and the protective layer 1 are laminated in this order on the support substrate 2. [7] The method for producing a laminate according to [6] above, wherein in the step (II), the structure 1 is a structure 2 in which the laser-absorbent temporary adhesive layer 1, the protective layer 1, and the semiconductor layer 1 are laminated, and the laminate 3 is a laminate 4 in which the adhesive layer, the semiconductor layer 1, the protective layer 1, and the laser-absorbent temporary adhesive layer 1 are laminated in this order on the support substrate 2. [8] The method for producing a laminate according to [6] or [7] above, further comprising a step (III) of removing a portion of the adhesive layer of the laminate 3 and patterning the adhesive layer. [9] The method for producing a laminate according to [7] or [8] above, further comprising a step (III') of removing a portion of the adhesive layer of the laminate 4 and patterning the adhesive layer.

[10] The method for producing a laminate according to [8] above, further comprising a step (III-A) of dry-etching or wet-etching the adhesive layer of the laminate 3 or the laminate 4 using the semiconductor layer 1 or the protective layer 1 of the laminate 3 as a mask.

[11] In the step (III '), the semiconductor layer 1, the protective layer 1 or the laser-absorbent temporary adhesive layer 1 of the laminate 4 is used as a mask to dry-etch or wet-etch the adhesive layer of the laminate 4. The method for producing the laminate according to the above [9], comprising the step (III '-A).

[12] The method for producing a laminate according to any one of [6] to

[11] above, further comprising a step (IV) of removing the protective layer 1 from the laminate 3.

[13] The method for producing a laminate according to any one of [7] to

[12] above, further comprising a step (IV') of removing the laser-absorbing temporary adhesive layer 1 and the protective layer 1 from the laminate 4.

[14] A method for producing a semiconductor device, comprising a step (V) of placing the surface of the laminate obtained by the method for producing a laminate according to

[12] or

[13] above, facing the surface of the semiconductor layer 1 side, and a surface of a circuit board on which a circuit is formed, and bonding the semiconductor layer 1 of the laminate to the circuit board by thermocompression bonding.

[15] The method for producing a semiconductor device according to

[14] above, further comprising a step (VI) of removing a support substrate 2 with an adhesive layer from a structure in which the semiconductor layer 1 of the laminate and the circuit board are bonded, after the step (V).

[16] The method for producing a semiconductor device according to

[14] or

[15] above, wherein the semiconductor device is a silicon photonics semiconductor device.

[17] A laminate in which a support substrate 2, an adhesive layer, a semiconductor layer 1, and a protective layer 1 are laminated in this order, and the adhesive layer has a patterned shape.

[0166] The present invention will be described below with reference to examples, but the present invention is not limited to these examples.

[0167] (1) Preparation of laminate α and laminate β in laminate 1 A 4-inch quartz substrate with a thickness of 0.5 mm and an alignment mark was coated with varnish a prepared by the method described below using a spinner, pre-baked on a hot plate at 120 ° C. for 3 minutes, and then heated and cured at 225 ° C. for 5 minutes to produce a laminate α-1 in which a laser-absorbent temporary adhesive layer 1 was laminated on a quartz substrate (laser-transmitting substrate 1). In addition, varnish b prepared by the method described below was applied to another quartz substrate using a spinner, pre-baked on a hot plate at 120 ° C. for 3 minutes, and heated and cured at 250 ° C. for 30 minutes, and a laser-absorbing layer 1 was laminated on the quartz substrate. Furthermore, varnish c prepared by the method described below was applied onto the laser absorbing layer 1 using a spinner, pre-baked on a hot plate at 120°C for 3 minutes, and then subsequently heated and cured at 225°C for 5 minutes to prepare a laminate β-1 in which the laser absorbing layer 1 and the temporary adhesive layer 2 were laminated in this order on the quartz substrate (laser-transmitting substrate 1).

[0168] The film thickness of the laser-absorbing temporary adhesive layer 1 of the laminate α-1, and the laser-absorbing layer 1 and temporary adhesive layer 2 of the laminate β-1 were measured by cutting each laminate and observing the cross section with a scanning electron microscope (Hitachi High-Tech Corporation, S-4800). Furthermore, laminates α-2 to α-6 were prepared by changing the type of varnish and film thickness of the laminate α-1, and laminates β-2 to β-11 were prepared by changing the type of varnish and film thickness of the laminate β-1. The measurement results for each composition and film thickness are summarized in Tables 1 and 2.

[0169]

[0170]

[0171] (2)-1 Fabrication of Stack 1 from Stack 0 Having a Tether Structure Separately, as described in Non-Patent Document 2 (Jing Zhang et al., III-V-on-Si photonic integrated circuits realized using micro-transfer-printing, APL Photon., 2019, 4, 110803) and other known techniques, a sacrificial layer was formed on an InP substrate, and an epitaxially grown crystal film of InGaAsP (thickness: 0.5 μm, multiple quantum well (MQW (= Multiple Quantum Well structure))) (hereinafter also referred to as MQW) was formed on the sacrificial layer as semiconductor layer 1. A SiO 2 layer was then formed on the sacrificial layer as protective layer 1 using CVD technology. 2 After forming a film of 0.3 μm, SiO 2 The attached MQW was separated into small pieces (size: 50 μm × 400 μm). The distance between the small pieces was 200 μm. Subsequently, photoresist was formed to cover the small pieces, and the sacrificial layer was removed to form a stack 0-1 having a bridge structure in which the photoresist served as a tether, connecting the InP substrate and the epitaxially grown crystalline film. That is, as illustrated in FIG. 7A , the bridge structure described above has a structure in which, on the InP substrate, i.e., semiconductor wafer (reference numeral 51), there is a space, i.e., a hollow (reference numeral 55), where the sacrificial layer had been located, and the semiconductor layer 1 (reference numeral 14) (epitaxially grown crystalline film) and protective layer 1 (reference numeral 13) stacked thereon are supported from the sides by a photoresist layer (reference numeral 54). The small pieces consisting of the semiconductor layer 1 (reference numeral 14) and protective layer 1 (reference numeral 13) are covered on the top and side surfaces by the photoresist layer (reference numeral 54). At this time, the thickness of the photoresist on the top surface of the MQW layer was 2 μm. Thereafter, the bridge structure is cut along with the InP substrate, and the SiO 2 A stack 0-1 was prepared in which 100 small pieces of MQW with a GaN layer were mounted on an InP substrate.

[0172] In the fabrication of the stack 0-1, the thickness of the MQW was set to 2.0 μm, and SiO 2A Tether structure was formed after forming a photoresist layer without forming a protective layer 1 on the top surface of the MQW. The photoresist on the top surface of the MQW was then removed by dry etching, so that the photoresist layer was formed only on the side surfaces of the sacrificial layer and semiconductor layer 1 (MQW), and no photoresist remained on the MQW. The sacrificial layer was then removed and the substrate was cleaved to create 100 small pieces of MQW on the InP substrate. This resulted in the creation of stack 0-3, which did not have a protective layer 1 on the top surface of the MQW.

[0173] In the production of the laminate 0-1, the inorganic protective layer 1 (SiO 2 A laminate 0-4 having only 2 μm of photoresist as the protective layer 1 was prepared in the same manner as the laminate 0-1, except that the protective layer 1 was not prepared.

[0174] In the production of the laminate 0-1, SiO 2 A 0.08 μm SiN layer was created instead of the layer. Subsequently, after creating a photoresist layer, the photoresist layer on the SiN layer was removed by dry etching, so that the photoresist layer was formed only on the side surfaces of the insulating layer, semiconductor layer 1 (MQW), and protective layer 1 (SiN), and no photoresist remained on the SiN. After that, the sacrificial layer was removed and the substrate was fractured, resulting in 100 small pieces of MQW with SiN on the InP substrate. Stack 0-5 was created, having a 0.08 μm SiN as protective layer 1 on the top surface of the MQW.

[0175] In the preparation of the laminate 0-5, the type and thickness of the protective layer 1 were changed according to Table 3 below to prepare laminates 0-6 to 0-8. The configurations of the prepared laminates 0 are summarized in Table 3.

[0176]

[0177] The laminate 0-1 was placed on the temporary adhesive layer 2 side of the laminate β-1 with the photoresist side on the protective layer 1 of the laminate 0-1 facing each other, and then they were pressed and temporarily bonded using a vacuum laminator. Thereafter, the InP substrate of the laminate 0-1 was peeled off, and the quartz substrate, laser absorbing layer 1, temporary adhesive layer 2, photoresist, and protective layer 1 (SiO 2), and semiconductor layer 1 (MQW) were stacked in this order to produce stack 1-1. The MQW on stack 1-1 was observed with an optical microscope, and the number of small pieces of semiconductor layer 1 (MQW) that could be stacked on temporary adhesive layer 2 and the presence or absence of cracks in each chip were confirmed. In other words, the number of small pieces of semiconductor layer 1 (MQW) is the number on a 4-inch quartz substrate.

[0178] Furthermore, for each combination of the stack 0-1, stack 0-3 to 0-6, and the aforementioned stacks α-1 to α-6, and β-1 to β-11, the semiconductor layer 1 was temporarily bonded in the same manner to prepare stacks 1-3 to 1-25. The combinations of each stack and the results of temporary bonding of the semiconductor layer 1 are summarized in Tables 4 and 5.

[0179]

[0180]

[0181] (2)-2 Fabrication of laminate 1 using laminate 0' fabricated using dicing tape On a GaAs substrate (thickness 150 μm) on a dicing tape, an epitaxially grown crystal film (thickness: 0.5 μm in total) of GaAs and AlGaS for a high-frequency device HEMT (High Electron Mobility Transistor) was formed as a semiconductor layer 1, and a SiO 2 protective layer was formed thereon. 2 The substrate was diced on a dicing tape to form chips (size: 1.1 x 1.1 mm), and a laminate 0'-2 was produced in which 100 HEMT pieces were mounted on the dicing tape. The configuration of the laminate 0'-2 is summarized in Table 3 above.

[0182] SiO of laminate 0'-2 2 The surface of the dicing tape was then irradiated with UV light to reduce the adhesiveness of the surface of the dicing tape that contacted the GaAs substrate, and the dicing tape was removed from the laminate (reverse mounting method). Then, the quartz substrate, the laser-absorbent temporary adhesive layer 1, and the protective layer 1 (SiO 2), semiconductor layer 1 (HEMT), and GaAs substrate were stacked in this order to produce stack 1-2. The semiconductor layer 1 on stack 1-2 was visually observed with an optical microscope from the quartz substrate side, and the number of small pieces of semiconductor layer 1 (MQW) that had been stacked on temporary adhesive layer 2 and the presence or absence of cracks in each chip were confirmed. In other words, the number of small pieces of semiconductor layer 1 (MQW) is the number on a 4-inch quartz substrate. The configuration and evaluation results of stack 1-2 are summarized in Table 4 above.

[0183] (3) Measurement of absorbance of laser-absorbent temporary adhesive layer 1 and laser-absorbing layer 1 Varnishes a and f used for laminates α-1 to α-6 were applied to a quartz substrate in the same manner as in (1) above, prebaked, and heat-cured to prepare a quartz substrate with laser-absorbent temporary adhesive layer 1 for absorbance measurement. In addition, varnish b used for laser-absorbing layer 1 in the preparation of laminates β-1 to β-11 in (1) was similarly formed into a film, prebaked, and heat-cured to prepare a quartz substrate with laser-absorbing layer 1 for absorbance measurement. The film thickness was also measured in the same manner as in (1) above.

[0184] The absorbance of the quartz substrate with the laser-absorbing temporary adhesive layer 1 for absorbance measurement and the quartz substrate with the laser-absorbing layer 1 obtained as described above was continuously measured from 200 nm to 400 nm using an ultraviolet-visible spectrophotometer (U-2910, manufactured by Hitachi, Ltd.). From these, values ​​at 248 nm, 266 nm, and 355 nm were read, and the respective absorbances per μm were calculated using the following formula (1). The results are summarized in Tables 1 and 2 above. Absorbance per μm = actual absorbance obtained in measurement / measured film thickness (μm)... formula (1)

[0185] (4) Measurement of adhesive strength of the surface where the laser-absorbent temporary adhesive layer 1 or temporary adhesive layer 2 contacts the protective layer 1 In the laminates 1-1, 1 to 3 to 1-24 produced in (2)-1 above, a dicing tape (UDT-1025MC) was attached to the surface of the semiconductor layer 1 and then peeled off, thereby peeling off the semiconductor layer 1 with the protective layer 1 and the photoresist from the temporary adhesive layer 2. Similarly, in the laminate 1-2 produced in (2)-2 above, the semiconductor layer 1 with the protective layer 1 was peeled off from the laser-absorbent temporary adhesive layer 1.

[0186] After peeling off the semiconductor layer 1 with the protective layer 1, the temporary adhesive layer 2 and the laser-absorbent temporary adhesive layer 1 were subjected to pressure bonding using a vacuum laminator at 0.1 MPa and 25 ° C. to a polyimide film cut into a 1 cm x 9 cm strip, Kapton (registered trademark) 100EN (registered trademark) (manufactured by DuPont-Toray Co., Ltd.). The sample was placed in a tensile tester (manufactured by Nidec-Shimpo Corporation, FGS-VC), and the bonded Kapton film was peeled off in the vertical direction at a constant speed of 2 mm / sec. The peel strength at this time was measured using a digital force gauge (manufactured by Nidec-Shimpo Corporation, FGJN-5). The measurement was performed three times using different samples, and the average value was taken as the adhesive strength. The adhesive strength measured for each laminate 1 is summarized in Tables 4 and 5 above.

[0187] (6) Laser Transfer (LLO) Test of Semiconductor Layer 1 (6)-1 Preparation of Laminate 2 The adhesive layer varnish d described below was applied to a 0.5 mm thick 4-inch quartz substrate with an alignment mark, which was used as the support substrate 2, using a spinner, and pre-baked on a hot plate at 120 ° C. for 3 minutes, and then further heated and cured at 225 ° C. for 10 minutes to form an adhesive layer with a thickness of approximately 5 μm on the quartz substrate, producing a support substrate 2 with an adhesive layer (laminate 2-1). The film thickness of the adhesive layer after thermal curing was measured using an optical film thickness meter (Lambda Ace, manufactured by SCREEN Holdings Co., Ltd., refractive index = 1.543). Laminates 2-2 to 2-11 were prepared using the same method as above, but using different varnishes and film thicknesses for the adhesive layer. The configuration of laminate 2 is summarized in Table 6.

[0188]

[0189] (6)-2 Production of Laminate 4 by Laser Transfer of Semiconductor Layer 1 with Protective Layer 1 (Application of Laminate 1-1) Next, a laser light source, the laminate 1-1 produced by the above-described method, and laminate 2-1 were arranged in this order. At this time, the surface of laminate 1-1 on which semiconductor layer 1 was held and the surface of laminate 2-1 on which the adhesive layer was formed were held facing each other so that the distance between the surface of semiconductor layer 1 and the surface of the adhesive layer was 50 μm. The laminate 1-1 and laminate 2-1 were aligned using their respective alignment marks. The laser spot size was a square shape measuring 90 μm × 440 μm, and the positions of the laser light source and laminate 1-1 were adjusted so that one MQW piece was located in the center of the laser spot, and the laser was not irradiated onto the adjacent semiconductor layer 1.

[0190] A laser with a wavelength of 355 nm was applied to the MQW placed at the laser irradiation position at 100 mJ / cm 2 The irradiation was performed with an energy irradiation amount of 1000 W, and the support substrate 2, adhesive layer, semiconductor layer 1 (MQW), and protective layer 1 (SiO 2 ), a photoresist, a temporary adhesive layer 2, and a laser absorbing layer 1 were laminated in this order to prepare a laminate 4-1. The LLO of the semiconductor layer 1 was carried out on 10 samples for each sample, and then the samples were observed with an optical microscope to determine whether the MQW and SiO 2 The presence or absence of cracks or damage to the layer was confirmed. In addition, the positions of the small pieces of the semiconductor layer 1 before and after transfer were calculated from the alignment marks and compared with the positions in the laminate 1. Those in which the deviation in both the short axis direction and the long axis direction of the MQW chip was less than ±2 μm were evaluated as A, those in which the deviation was ±2 μm or more and ±5 μm or less were evaluated as B, those in which the deviation was greater than ±5 μm were evaluated as C, those in which transfer was not possible were evaluated as D, and those in which transfer was possible but cracks or chips occurred were evaluated as E, and the numbers of each are summarized in Table 7.

[0191] (6)-3 Production of laminate 3 by transferring semiconductor layer 1 with protective layer 1 (application of laminate 1-2) The same procedure as in (6)-2 above was carried out except that laminate 1-2 was used instead of laminate 1-1, and a support substrate 2, adhesive layer, GaAs, semiconductor layer 1 (HEMT), protective layer 1 (SiO 2), and the laser-absorbing temporary adhesive layer 1 were laminated in this order to prepare a laminate 3-2. When observed with an optical microscope, the transferred GaAs, HEMT, SiO 2 No debris or adhesive residue from the laser-absorbent temporary adhesive layer 1 was observed on the upper or peripheral adhesive layer surface. The evaluation method for the presence or absence of damage to the transferred HEMT and its positional accuracy was the same as in (6)-2. The evaluation results are summarized in Table 7.

[0192]

[0193] (7)-1 Dry Etching of Adhesive Layer The laminate 4-1 prepared in (6)-2 was dry-etched using a high-throughput ashing and etching apparatus (MAS-8220AT; manufactured by Canon Inc.) under the following conditions to remove the protective layer 1 (SiO 2 ) as a mask, the temporary adhesive layer 2, the laser absorbing layer 1, the photoresist and the protective layer 1 (SiO 2 The adhesive layer was removed from areas other than the area where the adhesive layer was formed. The removal of the adhesive layer and the temporary adhesive layer 2 thereon, the laser absorbing layer 1, and the photoresist was confirmed by confirming with a microscopic IR spectrophotometer that the peaks of the temporary adhesive layer 2, the laser absorbing layer 1, the photoresist, and the adhesive layer had disappeared. Similarly, the protective layer 1 (SiO 2 ) as a mask, laser-absorbent temporary adhesive layer 1 and protective layer 1 (SiO 2 The adhesive layer was removed from areas other than the above. Removal of the adhesive layer was confirmed by confirming with a microscopic IR spectrophotometer that the peaks of the laser-absorbent temporary adhesive layer 1 and the adhesive layer had disappeared.

[0194] Dry etching conditions: Etching gas: CF 4 / O 2 = 80 / 20 (volume ratio) RF power: 300 W Etching temperature: 100°C Processing pressure: 20 Pa Gas flow rate: 50 sccm

[0195] (7)-2 Wet Etching of Adhesive Layer The laminate 4-1 prepared in (6)-2 was immersed in CHN at room temperature. After immersion, the surface was washed with acetone and then pure water, and dried on a hot plate at 150 ° C for 5 minutes. It was confirmed that the laser-absorbent temporary adhesive layer 1 laminated on the protective layer 1 had been removed. In addition, the adhesive layer in the area where the semiconductor layer 1 was not laminated was measured using an optical film thickness meter (Lambda Ace, manufactured by SCREEN Holdings Co., Ltd., refractive index = 1.543), and the amount etched was calculated by comparing the film thickness with that before treatment. The results are summarized in Table 8.

[0196] (8)-1 Transfer to circuit board by thermocompression bonding Using the laminate 4-1 or laminate 3-2 with the patterned adhesive layer prepared in (7), thermal transfer was carried out to a photonic integrated circuit using an SOI substrate described in Japanese Patent Application Laid-Open No. 2017-500735 or a Si circuit board for a power amplifier. Just before the thermal transfer, the SiO 2 The surface, photonic integrated circuit surface, and Si circuit surface are UV-O 3 The substrates were treated in a treatment machine for 5 minutes to sufficiently hydrophilize the contact interface, and then thermocompression bonded at 150°C and 1 MPa using a flip chip bonder (FC-3000, manufactured by Toray Engineering Co., Ltd.). This is called a bonded substrate. Details of each laminate are summarized in Table 8.

[0197]

[0198] (8)-2 Peeling of Support Substrate 2 and Adhesive Layer from Bonded Substrate The bonded substrate prepared in (8)-1 was mechanically peeled at the interface between the adhesive layer and semiconductor layer 1 (mechanical peeling). For laminates 4-32 and 4-33, a laser was irradiated from the support substrate 2 side to the semiconductor layer 1 with the same energy amount and spot size as in (6)-2, and the adhesive layer in contact with the semiconductor layer 1 was peeled off from the support substrate 2 (laser peeling). For laminate 4-9, the bonded substrate was thermocompression bonded without patterning the adhesive layer, and the bonded substrate was immersed in cyclohexanone overnight, and the cyclohexane was soaked in from the edge, dissolving the adhesive layer to peel off the substrate (solvent peeling). After peeling, deviations in both the minor axis and major axis directions of the semiconductor layer 1 compared to before bonding were evaluated as A, ±2 μm or more but less than ±5 μm as B, ±5 μm or more as C, and bonding was successfully completed but cracks or chips occurred as E. The results are summarized in Table 8.

[0199] (9) Evaluation of Storage Modulus at 200°C Approximately 1 g of the varnish described below was placed in an aluminum cup and dried at 120°C for 30 minutes using a hot plate. It was then heat-treated at 250°C for 2 hours using a hot plate, yielding a cured product with a film thickness of approximately 500 μm. Subsequently, a single film of the obtained cured product was cut into a length of 0.5 cm x 3 cm to prepare a strip-shaped sample. This sample was measured using a dynamic viscoelasticity measuring device (DVA-200, manufactured by IT Measurement & Control Co., Ltd.) in tension mode, at a frequency of 1 Hz, in the temperature range of 25°C to 250°C, and the storage modulus at 200°C was determined from the obtained temperature-storage modulus curve.

[0200] The abbreviations for the acid dianhydrides, diamines, additives, and solvents shown in the following production examples and formulation examples are as follows: PMDA: pyromellitic anhydride (manufactured by Daicel Corporation) BPDA: 3,3',4,4'-biphenyltetracarboxylic anhydride (manufactured by Mitsubishi Chemical Corporation) DIBOC: di-tert-butyl dicarbonate (manufactured by Tokyo Chemical Industry Co., Ltd.) PA: phthalic anhydride (manufactured by Tokyo Chemical Industry Co., Ltd.)

[0201] PDA: p-phenylenediamine (manufactured by Tokyo Chemical Industry Co., Ltd.) BAHF: 2,2-bis(3-amino-4-hydroxyphenyl)-1,1,1,3,3,3-hexafluoropropane (manufactured by Merck Ltd.) FDA: 9,9-bis(3-amino-4-hydroxyphenyl)fluorene (manufactured by Merck Ltd.) APPS2: α,ω-bis(3-aminopropyl)polydimethylsiloxane (number average molecular weight 860) APPS3: α,ω-bis(3-aminopropyl)polydimethylsiloxane (number average molecular weight 1550) APPS4: α,ω-bis(3-aminopropyl)polydimethylsiloxane (number average molecular weight 3000)

[0202] NMP: 2-methyl-1-pyrrolidone (manufactured by Mitsubishi Chemical Corporation) CHN: cyclohexanone (manufactured by Toyo Gosei Co., Ltd.) BDM: diethylene glycol butyl methyl ether (manufactured by Toho Chemical Industry Co., Ltd.) JER (registered trademark) 871: dimer acid modified epoxy resin (manufactured by Mitsubishi Chemical Corporation) PETG: pentaerythritol-based skeleton epoxy resin (manufactured by Showa Denko K.K.) 2E4MZ: 2-ethyl-4-methylimidazole (manufactured by Shikoku Chemical Industry Co., Ltd.) 100LM: crosslinking agent having a methylol group represented by the structure of the following formula (11) (product name: Nikalac (registered trademark) MW-100LM, manufactured by Sanwa Chemical Co., Ltd.)

[0203]

[0204] Tinuvin (registered trademark) 477: ultraviolet absorber (manufactured by BASF Japan Ltd.)

[0205] Production Example 1 (Polymerization of Resin Contained in Laser Absorbing Layer 1) A thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer were installed in a reaction kettle, and 11.82 g (109 mmol) of PDA and 195.80 g of NMP were charged and dissolved. A solution containing 0.48 g (2.19 mmol) of DIBOC and 26.10 g of NMP was added dropwise to the reaction kettle while stirring, and the mixture was stirred at 40 ° C. for 1 hour. Next, 12.87 g (43.7 mmol) of BPDA and 13.05 g of NMP were added, and the mixture was stirred at 60 ° C. for 30 minutes. Subsequently, 13.83 g (63 mmol) of PMDA and 13.05 g of NMP were added, and the mixture was stirred at 60 ° C. for 4 hours, to obtain a PAA-1-containing solution containing 13 parts by weight of polyimide precursor PAA-1 relative to 100 parts by weight of the total volume.

[0206] Production Example 2 (Polymerization of Resins Contained in Laser-Absorbable Temporary Adhesive Layer 1 and Temporary Adhesive Layer 2) Into a reaction vessel equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water / cooling water, and a stirrer, 344.00 g (400 mmol) of APPS2, 37.50 g (25 mmol) of APPS3, and 27.47 g (75 mmol) of BAHF were charged together with 481.40 g of CHN and dissolved. After that, 14.81 g (100 mmol) of PA and 20.00 g of CHN were added, and the mixture was stirred at 60°C for 15 minutes. Subsequently, 97.61 g (450 mmol) of PMDA and 20.00 g of CHN were added, and the mixture was stirred at 60°C for 1 hour. The mixture was then heated to 145°C and reacted for 4 hours to obtain a PIS-1-containing solution containing 50 parts by weight of polyimidesiloxane PIS-1 per 100 parts by weight of the total volume.

[0207] Production Example 3 (Polymerization of resin contained in adhesive layer) Polymerization was carried out in the same manner as in Production Example 2, except that APPS2 was 340.56 g (396 mmol), APPS3 was 44.95 g (29 mmol), BAHF was 27.47 g (75 mmol), and CHN was 482.00 g, to obtain a PIS-2-containing solution containing 50 parts by weight of polyimidesiloxane PIS-2 per 100 parts by weight of the total volume.

[0208] Production Example 4 (polymerization of the resin contained in the temporary adhesive layer 2 and the adhesive layer) Thermometer, dry nitrogen inlet, heating and cooling device using hot water and cooling water, and a reaction kettle equipped with a stirrer, APPS3 620 g (400 mmol), APPS4 150 g (50 mmol), BAHF 18.31 g (50 mmol) and CHN 856 g were charged together and stirred for 15 minutes at 60 ° C. Subsequently, PMDA 107.97 g (495 mmol) and CHN 40.00 g were added, and the mixture was stirred at 60 ° C. for 1 hour, and then heated to 145 ° C. and reacted for 4 hours, with respect to 100 parts by weight of the total volume, containing 50 parts by weight of polyimidesiloxane PIS-3, a PIS-3-containing solution was obtained.

[0209] Production Example 5 (Polymerization of Resins Contained in Laser Absorbing Layer 1 and Adhesive Layer) Into a reaction kettle equipped with a thermometer, a dry nitrogen inlet, a heating / cooling device using hot water and cooling water, and a stirrer, 736 g (475 mmol) of APPS3, 9.51 g (25 mmol) of FDA, and 821 g of BDM were charged and stirred for 60 minutes at 60° C. Subsequently, 107.97 g (495 mmol) of PMDA and 40.00 g of BDM were added, and the mixture was stirred at 60° C. for an additional hour, and then the temperature was raised to 145° C. and reacted for 4 hours to obtain a PIS-4-containing solution containing 50 parts by weight of polyimidesiloxane PIS-4 per 100 parts by weight of the total volume.

[0210] Preparation Example 1 (Preparation of Varnish a) 2.82 g of the PIS-1-containing solution (1.41 g of polyimidesiloxane PIS-1 and 1.41 g of CHN) was placed in a vial, and 0.28 g of PETG, 0.01 g of 100LM, 0.01 g of 2E4MZ, 0.28 g of Tinuvin (registered trademark) 477, and 6.59 g of CHN were added and stirred to prepare varnish a.

[0211] Preparation Example 2 (Preparation of Varnish b) 5.0 g of a PAA-1-containing solution (0.65 g of polyimide precursor PAA-1, 4.35 g of NMP) was placed in a vial, and 5.0 g of NMP was added and stirred to prepare varnish b.

[0212] Preparation Example 3 (Preparation of Varnish c) 41 g of the PIS-1-containing solution (20.5 g of polyimidesiloxane PIS-1 and 20.5 g of CHN) was placed in a vial, and 4 g of JER (registered trademark) 871, 0.2 g of 100LM, 0.2 g of 2E4EMZ, and 4.5 g of CHN were added and stirred to prepare varnish c.

[0213] Preparation Example 4 (Preparation of Varnish d) 41 g of the PIS-2-containing solution (20.5 g of polyimidesiloxane PIS-2, 20.5 g of CHN) was placed in a vial, and 4 g of JER (registered trademark) 871, 0.2 g of 100LM, 0.2 g of 2E4EMZ, and 4.5 g of CHN were added and stirred to prepare varnish d.

[0214] Varnishes e to g were then prepared according to the description in Table 9.

[0215]

[0216] All of the varnishes a to g were filtered through a polytetrafluoroethylene (PTFE) filter with a pore size of 0.2 μm. Using these varnishes, laminates α and β were produced by the above-mentioned method.

[0217] Using the above varnish, the storage modulus of the adhesive layer at 200° C. was evaluated as described in (9) Evaluation of storage modulus at 200° C. above. The results are shown in Table 10.

[0218]

[0219] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2023-072581) filed on April 26, 2023, the entirety of which is incorporated by reference. All references cited herein are incorporated in their entirety.

[0220] DESCRIPTION OF SYMBOLS 11 Laser-transmitting substrate 1 12 Laser-absorbing temporary adhesive layer 1 13 Protective layer 1 14 Semiconductor layer 1 15 Laser irradiation 16 Temporary adhesive layer 2 17 Laser absorbing layer 1 21 Support substrate 2 22 Adhesive layer 23 Laser absorbing layer 2 24 Adhesive layer present between semiconductor layer 1 and support substrate 2 25 Adhesive layer in a portion of support substrate 2 not having semiconductor layer 1 41 Circuit board 51 Semiconductor wafer 52 Sacrificial layer 54 Photoresist layer 55 Hollow 100 Laminate 1 101 Laminate 1' 200 Laminate 2 300 Laminate 3 400 Semiconductor device 501 Laminate 0" 502 Laminate α 503 Laminate 0 600 Laminate 4

Claims

1. A laminate in which a laser-absorbent temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmitting substrate 1.

2. The laminate according to claim 1, wherein the semiconductor layer 1 is a compound semiconductor.

3. The stack according to claim 2, wherein the compound semiconductor is AlGaInAs, InGaAs, InP, InGaAsP, AlAs, InAs, GaAs, AlN, AlP, GaN, InN or SiC.

4. The laminate according to any one of claims 1 to 3, wherein the protective layer 1 is at least one of an oxide film and a nitride film.

5. The protective layer 1 is made of SiO 2 The laminate of claim 4 comprising:

6. A method for producing a laminate, comprising the steps of: using a laminate 1 in which a laser-absorbent temporary adhesive layer 1, a protective layer 1, and a semiconductor layer 1 are laminated in this order on a laser-transmissible substrate 1; and a laminate 2 in which an adhesive layer is laminated on a support substrate 2, a step (I) of opposing a surface of the laminate 1 on the semiconductor layer 1 side to a surface of the laminate 2 on the adhesive layer side; and a step (II) of irradiating the laser-absorbent temporary adhesive layer 1 with a laser from the surface side of the laminate 1 opposite to the surface on the semiconductor layer 1 side while transmitting the laser through the laser-transmissive substrate 1, thereby transferring a structure 1 in which the protective layer 1 and the semiconductor layer 1 are laminated to the laminate 2, and forming a laminate 3 in which the adhesive layer, the semiconductor layer 1, and the protective layer 1 are laminated in this order on the support substrate 2.

7. A method for producing a laminate as described in claim 6, wherein in the step (II), the structure 1 is a structure 2 in which the laser-absorbent temporary adhesive layer 1, the protective layer 1 and the semiconductor layer 1 are laminated, and the laminate 3 is a laminate 4 in which the adhesive layer, the semiconductor layer 1, the protective layer 1 and the laser-absorbent temporary adhesive layer 1 are laminated in this order on the supporting substrate 2.

8. The method for producing a laminate according to claim 6, further comprising the step (III) of removing a portion of the adhesive layer of the laminate 3 and patterning the adhesive layer.

9. The method for producing a laminate according to claim 7, further comprising the step (III') of removing a portion of the adhesive layer of the laminate 4 and patterning the adhesive layer.

10. The method for producing a laminate according to claim 8, wherein in the step (III), a step (III-A) is included in which the adhesive layer of the laminate 3 is dry-etched or wet-etched using the semiconductor layer 1 or the protective layer 1 of the laminate 3 as a mask.

11. The method for producing a laminate according to claim 9, further comprising a step (III'-A) of performing dry etching or wet etching of the adhesive layer of the laminate 4 using the semiconductor layer 1, the protective layer 1 or the laser-absorbing temporary adhesive layer 1 of the laminate 4 as a mask in the step (III').

12. The method for producing a laminate according to claim 6, 8 or 10, further comprising a step (IV) of removing the protective layer 1 from the laminate 3.

13. A method for producing a laminate according to claim 7, 9 or 11, further comprising a step (IV') of removing the laser-absorbent temporary adhesive layer 1 and the protective layer 1 from the laminate 4.

14. A method for manufacturing a semiconductor device, comprising a step (V) of opposing the surface of the laminate obtained by the method for manufacturing a laminate described in claim 12 on the side of the semiconductor layer 1 to the surface of a circuit board on which a circuit is formed, and bonding the semiconductor layer 1 of the laminate to the circuit board by thermocompression bonding.

15. The method for manufacturing a semiconductor device according to claim 14, further comprising, after step (V), a step (VI) of removing a support substrate 2 with an adhesive layer from a structure formed by bonding the semiconductor layer 1 of the laminate to the circuit board.

16. The method of manufacturing a semiconductor device according to claim 14, wherein the semiconductor device is a silicon photonics semiconductor device.

17. A laminate in which a supporting substrate 2, an adhesive layer, a semiconductor layer 1, and a protective layer 1 are laminated in this order, and the adhesive layer has a patterned shape.

Citation Information

Patent Citations

  • Heat-resistant resin adhesive sheet and substrate

    JP1998226778A

  • Semiconductor device and semiconductor module

    JP2006108556A

  • Organic modified silicone resin composition

    JP2015140372A

  • Asymmetric waveguide grating resonator and dbr laser

    JP2017500735A

  • Microstructure transfer device, stamp head unit, microstructure transfer stamp component, and microstructure integrated component transfer method

    JP2020129638A

Cited By

  • Laminate, laminate manufacturing method, and semiconductor device manufacturing method

    WO2026211739A1