Oriented body manufacturing device
The fixed-position oriented body manufacturing apparatus addresses deformation and versatility issues by generating a temporally varying magnetic field, ensuring precise control and improved alignment in the manufacturing process.
Patent Information
- Application Number
- PCT/JP2024/016569
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-27
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional oriented body manufacturing techniques suffer from deformation and reduced versatility due to material rotation and difficulties in adjusting the magnetic field state during the manufacturing process.
A fixed-position oriented body manufacturing apparatus with a magnetic field generation unit that generates a temporally varying magnetic field, allowing for precise control of the magnetic field state without rotating the material, using a drive device to adjust the magnetic field conditions based on the intended use of the oriented body.
This approach suppresses deformation and enhances the versatility of the manufacturing process by allowing for the precise control of magnetic field states, enabling the production of oriented bodies with improved alignment properties and adaptability to various applications.
Smart Images

Figure JP2024016569_31102024_PF_FP_ABST
Abstract
Description
Orientation manufacturing equipment
[0001] The present invention relates to an apparatus for manufacturing an oriented body.
[0002] The techniques disclosed in Patent Documents 1 and 2 are known as prior art in this technical field. In the techniques described in Patent Documents 1 and 2, a material (slurry) obtained by dispersing a material powder containing microcrystalline particles in a solvent (solution) is subjected to casting while a magnetic field is applied to the material. In Patent Document 1, a holder holding the material is rotated in a static magnetic field to apply a relative rotating magnetic field to the material. In Patent Document 2, a permanent magnet is rotated or linearly moved relative to the material to apply a rotating magnetic field to a fixedly disposed material.
[0003] International Publication No. 2010 / 073712 Japanese Patent Application Laid-Open No. 2019-192668
[0004] In the technology of Patent Document 1, the material itself is rotated, which makes it easy for deformation such as distortion to occur in the oriented body produced. In the technology of Patent Document 2, a driving device is used to rotate or linearly move a permanent magnet, making it difficult to adjust the state of the rotating magnetic field applied to the material. The state of the rotating magnetic field applied to the material during the manufacturing process varies depending on the application of the oriented body to be produced. Therefore, the technology described in Patent Document 2 has reduced versatility.
[0005] Therefore, an object of the present invention is to provide an oriented body manufacturing apparatus that can suppress deformation during the manufacturing process and has greater versatility.
[0006] [1] An oriented body manufacturing apparatus according to one aspect of the present invention comprises a magnetic field generating unit that generates a magnetic field and is fixed in position relative to a material placement area in which an oriented body material whose orientation is controlled by a magnetic field is placed, and a driving device that drives the magnetic field generating unit to generate a time-varying magnetic field in the material placement area.
[0007] In the oriented body manufacturing apparatus, the magnetic field generating unit is fixed in position relative to the material placement area. The magnetic field generating unit, whose position is fixed in this manner, generates a time-varying magnetic field in the material placement area. Therefore, a time-varying magnetic field can be applied to the oriented body material placed in the material placement area even when the oriented body material is stationary, thereby suppressing deformation (e.g., distortion) of the oriented body during the manufacturing process. In the above configuration, the time-varying magnetic field is generated by driving the magnetic field generating unit with a driving device. Therefore, by changing the driving conditions of the magnetic field generating unit with the driving device, the state of the magnetic field required depending on the application of the oriented body to be manufactured can be easily adjusted. Therefore, the above configuration improves the versatility of the oriented body manufacturing apparatus.
[0008] [2] In the oriented body manufacturing apparatus according to [1] above, the magnetic field generating unit may generate the magnetic field so that the magnetic flux density in the material placement region is greater than 0.5 T.
[0009] [3] In the apparatus for producing an oriented body according to the above [1], the magnetic field generating unit may generate a rotating magnetic field. In this case, it is possible to produce an oriented body that is controlled to be oriented in the direction of the rotation axis of the rotating magnetic field.
[0010] [4] In the oriented body manufacturing apparatus described in [3] above, the magnetic field generating unit may generate the magnetic field so that the magnetic flux density in the material placement region is greater than 0.5 T, and the rotation speed of the rotating magnetic field may be greater than 60 rpm. Under such conditions, for example, an oriented body containing biaxial crystals can be manufactured. Therefore, the oriented body manufacturing apparatus is effective for manufacturing an oriented body containing biaxial crystals.
[0011] [5] In the oriented body manufacturing apparatus described in [3] or [4] above, the magnetic field generating unit has N electromagnet pairs (N is an integer of 2 or more), and when one of the N electromagnet pairs is referred to as the i-th electromagnet pair (i is any one of 1 to N), the directions of the magnetic fields generated by each of the two electromagnets in the i-th electromagnet pair are the same, and the two electromagnets in the i-th electromagnet pair may be arranged on either side of the material placement area.
[0012] In this case, the magnetic field generating unit has first to Nth pairs of electromagnets. By adjusting the magnetic fields generated by the first to Nth pairs of electromagnets, a rotating magnetic field can be generated.
[0013] [6] In the apparatus for manufacturing an oriented body according to the above [5], the driving device may apply voltages to the N electromagnet pairs with a phase shift so that the magnetic field generated by the N electromagnet pairs changes over time. This allows a rotating magnetic field to be generated.
[0014] [7] In the oriented body manufacturing apparatus described in [5] or [6] above, the N electromagnet pairs may be three electromagnet pairs, and the driving device may apply voltages of each phase of a three-phase alternating current to each of the three electromagnet pairs so as to generate the rotating magnetic field.
[0015] [8] In the alignment body manufacturing apparatus described in any one of [5] to [7] above, the cooling method for cooling the magnetic field generation unit may be a boiling cooling method. In this case, the magnetic field generation unit can be cooled by utilizing the boiling latent heat as well as the sensible heat difference due to direct cooling. Therefore, the magnetic field generation unit can be cooled efficiently.
[0016] [9] The alignment body manufacturing apparatus described in [8] above may include a housing having the material placement area and accommodating the magnetic field generation unit, and within the housing, the magnetic field generation unit may be disposed in an insulating liquid having a boiling point lower than that of water. In this case, insulation of the magnetic field generation unit is easy.
[0017]
[10] The oriented body manufacturing apparatus described in [9] above may further include a heat exchanger disposed within the housing and configured to return the vaporized insulating liquid to a liquid phase, and the heat exchanger may be supplied with a refrigerant from outside the housing. In this case, the vaporized boiling refrigerant can be returned to a liquid phase by the heat exchanger, eliminating the need to circulate the insulating liquid using a circulator or the like. Furthermore, the refrigerant is supplied to the heat exchanger from outside the housing. Therefore, a configuration of the oriented body manufacturing apparatus including the heat exchanger can improve quietness within the oriented body manufacturing apparatus.
[0018] According to the present invention, it is possible to provide an oriented body manufacturing apparatus that can suppress deformation during the manufacturing process and has greater versatility.
[0019] FIG. 1 is a schematic diagram illustrating an oriented body manufacturing apparatus according to one embodiment. FIG. 2 is a diagram illustrating a material to be placed in a material placement region and a holding unit that holds the material. FIG. 3 is a diagram illustrating an example of a coil. FIG. 4 is a diagram illustrating another example of a coil. FIG. 5 is a diagram illustrating an example of the temporal change in the magnitude of a magnetic field generated by an electromagnet pair. FIG. 6 is a diagram illustrating the temporal change in the magnetic field in the X and Y directions at the center of the material placement region. FIG. 7 is a diagram illustrating the direction of the magnetic field at the center of the material placement region. FIG. 8 is a schematic diagram of an example of a specific configuration of the oriented body manufacturing apparatus shown in FIG. 1. FIG. 9 is a diagram illustrating an example of a prototype of a magnetic field generation unit. FIG. 10 is a diagram illustrating the relationship between the current flowing through the coil and the magnetic flux density at the center of the magnetic field generation unit in the magnetic field generation unit shown in FIG. 9. FIG. 11 is a diagram of an oriented body manufactured using the oriented body manufacturing apparatus shown in FIG. 8, viewed from the central axis. FIG. 12 is a side view of the oriented body shown in FIG. 11. FIG. 13 is a graph showing the results of analyzing the sintered oriented body shown in FIGS. 10 and 11 using an X-ray diffraction method after sintering the oriented body.
[0020] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings. In the description of the drawings, the same or equivalent elements will be designated by the same reference numerals, and redundant description will be omitted. The dimensional proportions of the drawings do not necessarily correspond to those in the description.
[0021] Fig. 1 is a schematic diagram illustrating an oriented body manufacturing apparatus according to one embodiment. The oriented body manufacturing apparatus 1 shown in Fig. 1 is an apparatus for manufacturing an oriented body by slip casting while applying a time-varying magnetic field to an oriented body material (hereinafter simply referred to as "material") 3 placed in a material placement area 2.
[0022] The oriented body manufactured by the oriented body manufacturing apparatus 1 is a microcrystalline molded body with controlled orientation. The oriented body is a molded body that can be used as a ceramic (polycrystalline body) by being fired. In this embodiment, the oriented body manufacturing apparatus 1 will be described using as an example a case where the oriented body is a molded body that can be used as a ceramic laser medium by being fired.
[0023] FIG. 2 is a diagram for explaining the material 3 to be placed in the material placement area 2 and the holding portion 30 that holds the material 3.
[0024] The material 3 is a slurry (suspension) formed by dispersing a material powder containing single crystal particles in a solvent (solution). The single crystal particles are either uniaxial single crystal particles whose axis of easy magnetization is the a-axis (crystal minor axis) or biaxial single crystal particles. Examples of uniaxial single crystal particles include single crystal particles formed by an apatite compound to which Tb, Dy, Ho, Er, Tm or Yb is added as a rare earth element (for example, Yb:FAP(Ca 5 (P.O. 4 ) 3 F), single crystal particles formed by vanadate-based compounds to which Ce, Pr, Nd, or Sm is added as a rare earth element (for example, Nd:YVO 4 ), LiYF containing rare earth elements (Ce, Pr, Nd, Sm, Tb, Dy, Ho, Er, Tm or Yb) 4 , LiLuF 4 , LiSrAlF 6 , LiCaAlF 6 , LiSrGaF 6 Examples of biaxial single crystal fine particles include LiYF doped with rare earth elements (Ce, Pr, Nd, Sm, Tb, Dy, Ho, Er, Tm, or Yb). 4 , YAlO 3 , KY(WO 4 )2, KGd(WO 4 )2, CaYAlO 4 , GdCa 4 O(BO 3 ) 3 , YCa 4 O(BO 3 ) 3 , Y 2SiO 4 , Gd 2 SiO 4 Examples of single crystal particles include:
[0025] The rare earth element-doped single crystal particles can be prepared by uniformly dispersing the rare earth element in a predetermined oxide powder, for example, by a solid-state reaction such as premixing and calcination, or by a wet synthesis method.
[0026] The suspension can be prepared, for example, by mixing the oxide powder of single crystal particles doped with a rare earth element prepared as described above with another predetermined oxide powder, and adding the resulting material powder to water (solvent) together with a polymeric dispersant. The type of solvent and polymeric dispersant, as well as the concentration of the polymeric dispersant, can be appropriately determined depending on the state of the material powder. When preparing the suspension, multiple types of oxide powder of single crystal particles doped with a rare earth element may be used.
[0027] The holding unit 30 includes a cylindrical portion 31 and a filter portion 32 that closes one of the openings at both ends of the cylindrical portion 31. An example of the material for the cylindrical portion 31 is glass, and in this case, the cylindrical portion 31 is a glass tube. The shape and size of the cylindrical portion 31 are set according to the shape and size of the oriented body to be manufactured. In this embodiment, unless otherwise specified, the cylindrical portion 31 is a cylinder. An example of the diameter of the cylindrical portion 31 is 10 mm or more and 254 mm (10 inches) or less. A diameter of the cylindrical portion 31 of 10 mm or more allows for the manufacture of a molded body (oriented body) that is effective for the intended application. A diameter of 254 mm or less facilitates high-temperature firing. An example of the diameter of the cylindrical portion 31 is 12 mm. The length of the cylindrical portion 31 in the central axis direction depends on the amount of material 3 (slurry), but is, for example, 10 cm or more and 125 cm or less. A length of the cylindrical portion 31 in the central axis direction of 10 cm or more ensures a sufficient thickness for the molded body (oriented body). A length of 125 cm or less facilitates slip casting. The upper limit of the length of the cylindrical portion 31 in the central axis direction also depends on the size of the coil, which will be described later. An example of the length of the cylindrical portion 31 in the central axis direction is 25 cm. The filter portion 32 is configured to pass the liquid portion contained in the suspension (material 3). In this case, the liquid portion of the material 3 in the holding portion 30 is discharged through the filter portion 32, so that the single crystal particles are solidified. The material of the cylindrical portion 31 of the holding portion 30 is not limited to the glass described above. For example, the material of the cylindrical portion 31 may be plaster. In this case, the holding portion 30 may have a bottom formed of plaster instead of the filter portion 32.
[0028] In this embodiment, for convenience of explanation, unless otherwise specified, the suspension will be referred to as material 3. However, as described above, the liquid portion of the suspension is removed in the manufacturing process of the oriented body, and therefore the single crystal particles to which the rare earth is added are the substantial material of the oriented body.
[0029] Returning to Fig. 1, an outline of the oriented body manufacturing apparatus 1 will be described. The oriented body manufacturing apparatus 1 has a magnetic field generating unit 10 and a driving device 20. Fig. 1 shows the magnetic field generating unit 10 as viewed from a direction perpendicular to the X direction and Y direction shown in Fig. 1. The X direction and Y direction are perpendicular to each other.
[0030] In this embodiment, the magnetic field generator 10 generates a rotating magnetic field as a time-varying magnetic field with a rotation axis perpendicular to the X and Y directions. The magnetic field generator 10 has N (N is an integer of 2 or greater) electromagnet pairs. If one of the N electromagnet pairs is referred to as the ith electromagnet (i is any value from 1 to N), the magnetic field generator 10 has first to Nth electromagnet pairs.
[0031] In this embodiment, a case will be described in which there are three electromagnet pairs 101, 102, and 103. The electromagnet pair (first electromagnet pair) 101, the electromagnet pair (second electromagnet pair) 102, and the electromagnet pair (third electromagnet pair) 103 are arranged around the material placement area 2. Specifically, the three electromagnet pairs 101, 102, and 103 are arranged at 120-degree intervals around the center O of the material placement area 2.
[0032] When distinguishing between the two electromagnets in the electromagnet pair 101, they are referred to as electromagnet 101A and electromagnet 101B. Electromagnet 101A has a magnetic core 111a and a coil 121 wound around magnetic core 111a. Electromagnet 101B has a magnetic core 111b disposed opposite magnetic core 111a with respect to material placement region 2, and a coil 121 wound around magnetic core 111b. The coil 121 of electromagnet 101A and the coil 121 of electromagnet 101B are connected. That is, electromagnets 101A and 101B have a pair of magnetic cores 111a and 111b facing each other with respect to material placement region 2, and a coil 121 wound continuously around the pair of magnetic cores 111a and 111b. Coil 121 is wound so that when a current flows through coil 121, the magnetic fields generated by electromagnets 101A and 101B are oriented in the same direction.
[0033] When distinguishing between the two electromagnets in the electromagnet pair 102, they are referred to as electromagnet 102A and electromagnet 102B. Electromagnet 102A has a magnetic core 111c and a coil 122 wound around magnetic core 111c. Electromagnet 102B has a magnetic core 111d disposed opposite magnetic core 111c with respect to material placement region 2, and a coil 122 wound around magnetic core 111d. The coil 122 in electromagnet 102A and the coil 122 in electromagnet 102B are connected. That is, the electromagnet pair 102 has a pair of magnetic cores 111c, 111d facing each other with respect to material placement region 2, and a coil 122 wound continuously around the pair of magnetic cores 111c, 111d. The coil 122 is wound so that when a current flows through the coil 122, the magnetic fields generated by the electromagnets 102A and 102B are oriented in the same direction.
[0034] When distinguishing between the two electromagnets of the electromagnet pair 103, they are referred to as electromagnet 103A and electromagnet 103B. Electromagnet 103A has a magnetic core 111e and a coil 123 wound around magnetic core 111e. Electromagnet 103B has a magnetic core 111f disposed opposite magnetic core 111e with respect to material placement region 2, and a coil 123 wound around magnetic core 111f. The coil 123 of electromagnet 103A and the coil 123 of electromagnet 103B are connected. That is, electromagnet pair 103 has a pair of magnetic cores 111e, 111f facing each other with respect to material placement region 2, and a coil 123 wound continuously around the pair of magnetic cores 111e, 111f. Coil 123 is wound so that when a current flows through coil 123, the magnetic fields generated by electromagnets 103A and 103B are oriented in the same direction.
[0035] The material of the pair of magnetic cores 111a and 111b, the pair of magnetic cores 111c and 111d, and the pair of magnetic cores 111e and 111f is, for example, iron.
[0036] In one embodiment, the outer ends (ends opposite the material placement area 2) and inner ends (ends on the material placement area 2 side) of the pair of magnetic cores 111a, 111b, the pair of magnetic cores 111c, 111d, and the pair of magnetic cores 111e, 111f may be connected by a first connecting portion 111g and a second connecting portion 111h. The material of the first connecting portion 111g and the second connecting portion 111h is the same as that of the pair of magnetic cores 111a, 111b, the pair of magnetic cores 111c, 111d, and the pair of magnetic cores 111e, 111f. In other words, the magnetic field generator 10 may include a magnetic body 111 that includes a first connecting portion 111g, a second connecting portion 111h that is disposed inside the first connecting portion 111g and concentric with the first connecting portion 111g, and magnetic cores 111a to 111f that connect the first connecting portion 111g and the second connecting portion 111h. Below, unless otherwise specified, a configuration in which the magnetic field generator 10 includes the first connecting portion 111g and the second connecting portion 111h (in other words, a configuration that includes the magnetic body 111) will be described. The magnetic body 111 is, for example, a plate-shaped magnetic body.
[0037] The first end 121a of the coil 121, the first end 122a of the coil 122, and the first end 123a of the coil 123 of the magnetic field generating unit 10 are electrically connected to the driving device 20. The second end 121b of the coil 121, the second end 122b of the coil 122, and the second end 123b of the coil 123 of the magnetic field generating unit 10 are electrically connected to each other and to the driving device 20.
[0038] The driving device 20 applies voltages to the three electromagnet pairs 101, 102, and 103 with a phase shift so that the magnetic fields generated by the three electromagnet pairs 101, 102, and 103 change periodically. In this embodiment, the driving device 20 applies voltages of each phase of a three-phase AC current to the coils 121, 122, and 123. In this case, for example, the coil 121 functions as a U-phase coil, the coil 122 functions as a V-phase coil, and the coil 123 functions as a W-phase coil.
[0039] The driving device 20 includes a power supply unit 21 and a control unit 22 .
[0040] The power supply unit 21 includes, for example, an AC inverter circuit having three transistor pairs connected in parallel, and three gate drivers corresponding to the three transistor pairs. Each transistor pair is configured by three transistors connected in series. Each driver sends a drive signal to the gates of the upper arm transistor and the lower arm transistor of the corresponding transistor pair to drive the transistor pair.
[0041] The control unit 22 has a function of controlling the period, amplitude, etc. of the three-phase AC voltage generated in the power supply unit 21 in accordance with the rotating magnetic field generated in the material placement region 2. The control unit 22 is, for example, a microcomputer. When the power supply unit 21 has an AC inverter circuit and a gate driver as described above, the control unit 22 generates a control signal for controlling the period, amplitude, etc. of the three-phase AC voltage and transmits it to the gate driver. The control signal is, for example, a pulse width modulated (PWM) signal.
[0042] A description will be given of an example of how to wind the coils 121, 122, and 123 of the magnetic field generating unit 10. Since the example of how to wind the coils 121, 122, and 123 is the same, an example of how to wind the coil 121 will be described as a representative example.
[0043] Fig. 3 is a diagram illustrating an example of the coil 121. In Fig. 3, the conductor that constitutes the coil 121 is illustrated as conductor 12a. The conductor 12a may be wound to form multiple layers as shown in Fig. 3. In this case, all adjacent layers may be in contact with each other as shown in Fig. 3.
[0044] Figure 4 is a diagram illustrating another example of the coils 121 to 123. In Figure 4, as in Figure 3, the conductors constituting the coils 121 to 123 are illustrated as conductors 12a. The coils 121 to 123 shown in Figure 4 differ from the coils 121 to 123 shown in Figure 3 in that an insulating spacer 12b is disposed between at least one adjacent layer in the multilayer structure. An example of the spacer 12b is a resin film.
[0045] In the oriented body manufacturing apparatus 1 shown in FIG. 1, three magnetic fields with different directions are generated by electromagnet pairs 101, 102, and 103. In this embodiment, as shown in FIG. 1, the angle between the directions of two adjacent magnetic fields among the three magnetic fields around the center O of the material placement area 2 is 120 degrees. The magnitudes of the three magnetic fields change over time as shown in FIG. 5 depending on the three-phase AC voltage applied to the electromagnet pairs 101 to 103. FIG. 5 is a diagram showing an example of the temporal change in the magnitude of the magnetic fields generated by the electromagnet pairs 101, 102, and 103. The horizontal axis represents time, and the vertical axis represents the magnetic flux density at the center O. The solid line, dashed line, and dashed line in FIG. 5 represent the temporal change in the magnetic field (magnetic flux density) generated by the electromagnet pair 101, the electromagnet pair 102, and the electromagnet pair 103, respectively.
[0046] As shown in FIG. 5, the magnitude of the magnetic field generated by the electromagnet pairs 101, 102, and 103 changes over time, and therefore the magnetic flux density in the X and Y directions at the center O changes over time as shown in FIG. 6. As a result, the direction of the magnetic field M at the center O rotates over time, as shown in FIG. 7. FIG. 6 is a diagram schematically showing the temporal changes in the magnetic fields in the X and Y directions at the center O. FIG. 7 is a diagram schematically showing the direction of the magnetic field M at the center O. The magnetic field M is a composite magnetic field of the three magnetic fields generated by the electromagnet pairs 101, 102, and 103. In FIG. 7, M(t0) represents the magnetic field M at time t0 in FIG. 5, and M(t1) represents the magnetic field M at time t1 in FIG. 5. Similarly, M(t2) to M(t7) in FIG. 6 represent the magnetic field M from time t2 to t7 in FIG. 5.
[0047] 7, the magnetic field M generated by the magnetic field generating unit 10 rotates around a center O. Therefore, the magnetic field M is also referred to as a rotating magnetic field M.
[0048] The outline of the oriented body manufacturing apparatus 1 has been explained above using Figures 1 to 6. Next, a more specific configuration example of the oriented body manufacturing apparatus 1 will be explained using Figure 8. As shown in Figure 8, the oriented body manufacturing apparatus 1 according to one embodiment has a housing 40 that houses a magnetic field generation unit 10.
[0049] The housing 40 has a top wall 41, a bottom wall 42, and a side wall 43. In the embodiment shown in Fig. 8, the bottom wall 42 and the side wall 43 are integrated. The side wall 43 rises continuously from the periphery of the bottom wall 42. The top wall 41 is fixed to the end of the side wall 43 opposite the bottom wall 42. An example of a material for the housing 40 is an aluminum alloy such as A5052.
[0050] The housing 40 is provided with a material placement tube 44. Examples of materials for the material placement tube 44 include resin, such as engineering plastics and super engineering plastics. The material placement tube 44 is formed of, for example, polyether ether ketone (PEEK). The material placement tube 44 passes through an opening 41a in the top wall 41 and extends to the bottom wall 42. A hole 44a, through which a holding portion 30 (see FIG. 2 ) holding the material 3 passes, is formed in the material placement tube 44 in the extension direction of the material placement tube 44. The hole 44a is connected to an opening 42a in the bottom wall 42. In this embodiment, the cross section of the material placement tube 44 perpendicular to the extension direction is circular.
[0051] The material placement tube 44 has a first portion 441 and a second portion 442 in the extension direction of the material placement tube 44. The first portion 441 is a portion into which the holding unit 30 holding the material 3 is introduced. The cross-sectional size of the first portion 441 is larger than the cross-sectional size of the holding unit 30. The second portion 442 is a portion for placing the material 3 introduced from the first portion 441 at a predetermined position and for removing the material 3 from the bottom wall 42 side after the oriented body is produced. The predetermined position is the position of the holding unit 30 within the rotating magnetic field generated by the magnetic field generation unit 10 (in other words, the position of the magnetic field generation unit 10). The cross-sectional size of the second portion 442 is substantially the same as or slightly larger than the cross-sectional size of the holding unit 30. In this embodiment, the inner diameter of the second portion 442 is slightly larger than the outer diameter of the holding unit 30.
[0052] Due to the relationship between the inner diameters of the first portion 441 and the second portion 442 described above, the diameter of the region of the first portion 441 in the hole 44a is larger than the diameter of the region of the second portion 442. That is, the hole 44a has a large diameter portion and a small diameter portion. The portion of the large diameter portion that connects to the small diameter portion tapers toward the small diameter portion.
[0053] When manufacturing an oriented body, the sample holder 50 shown in FIG. 8 is inserted into the second portion 442 and the hole 44a from the hole 44a side. The sample holder 50 is hollow. An example of the material for the sample holder 50 is resin. Examples of resins for constructing the sample holder 50 are the same as those for the material placement tube 44. The sample holder 50 is fixed to the bottom wall 42, for example, by screws. The sample holder 50 is a member for positioning the holding unit 30 at the predetermined position. The length of the sample holder 50 along the central axis of the material placement tube 44 is designed so that the position of the holding unit 30 supported by the stopper 51 is the predetermined position when the sample holder 50 is fixed to the bottom wall 42. A mesh-like stopper (support member) 51 for supporting the holding unit 30 is formed on the upper end 50a (the end on the top wall 41 side) of the sample holder 50.
[0054] In this embodiment, the sample holder 50 has a double-tube structure. Specifically, the sample holder 50 includes an outer tube 52 and an inner tube 53 disposed inside the outer tube 52. The diameter of the outer tube 52 may be the same as or slightly shorter than the inner diameter of the second portion 442. As shown in FIG. 8 , the outer diameter of the inner tube 53 is smaller than the inner diameter of the outer tube 52. Thus, a radial gap is formed between the outer tube 52 and the inner tube 53. The upper end of the inner tube 53 may protrude from the outer tube 52 toward the top wall 41. In this case, the upper end of the inner tube 53 corresponds to the upper end 50a of the sample holder 50. The lower end of the inner tube 53 is connected to a vacuum device (not shown). A cooling air inlet is formed at the lower end of the sample holder 50 to allow cooling air to flow through the gap between the outer tube 52 and the inner tube 53.
[0055] The magnetic field generator 10 is disposed in a state in which the second connecting portion 111h is passed through the second portion 442 of the material placement tube 44. Specifically, the magnetic field generator 10 is fixed to a support base 45. The support base 45 has a support plate 45a, a bottom plate 45b, and a plurality of connecting columns 45c. The support plate 45a is connected to the bottom plate 45b via the plurality of connecting columns 45c. The bottom plate 45b is fixed to the inner surface of the bottom wall 42, for example, by screws. The magnetic field generator 10 is fixed by, for example, screwing the magnetic body 111 to the support plate 45a. For example, openings are formed in the support plate 45a in portions corresponding to the coils 121 to 123 so that the coils 121 to 123 do not interfere with the support plate 45a.
[0056] The driving device 20 that controls the magnetic field generating unit 10 can be disposed outside the housing 40. The driving device 20 is not shown in FIG.
[0057] In this embodiment, a boiling cooling method is used to cool the coils 121, 122, and 123. That is, the heat generated by the coils 121 to 123 is cooled by utilizing the boiling latent heat of the boiling refrigerant 46. Specifically, the boiling refrigerant 46 is stored in the housing 40 so that the magnetic field generating unit 10 is located within the boiling refrigerant 46. An example of the boiling refrigerant 46 is an insulating liquid with a boiling point lower than that of water (hereinafter also referred to as a "low-boiling-point insulating liquid"). An example of the low-boiling-point insulating liquid is Fluorinert.
[0058] A heat exchanger 47 is provided on the top wall 41 side of the housing 40 to return the boiling refrigerant 46, which has been boiled and evaporated during the cooling process of the coils 121 to 123, to a liquid phase. In this embodiment, the heat exchanger 47 is a finned tube through which the refrigerant flows from outside the housing 40. For example, the heat exchanger 47 is connected to a chiller disposed outside the housing 40. FIG. 8 illustrates an example in which multiple heat exchangers 47 are provided in the housing 40.
[0059] In the oriented body manufacturing apparatus 1 shown in FIG. 8 , the distance L1 between the center of the magnetic field generation unit 10 in the thickness direction and the inner surface of the bottom wall 42 is, for example, 47.5 mm or more and 435 mm or less. An example of the distance L1 is 70 mm. The distance L2 between the center of the magnetic field generation unit 10 in the thickness direction and the outer surface of the bottom wall 42 is, for example, 77.5 mm or more and 615 mm or less. An example of the distance L2 is 100 mm. The distance L3 between the center of the magnetic field generation unit 10 in the thickness direction and the upper end of the second portion 442 (the connection between the first portion 441 and the second portion 442) is, for example, 77.5 mm or more and 705 mm or less. An example of the distance L3 is 115 mm. The center of the magnetic field generation unit 10 in the thickness direction is the center of the magnetic field generation unit 10 in the thickness direction of the bottom wall 42. The distance L4 between the liquid level of the boiling refrigerant 46 and the inner surface of the bottom wall 42 is, for example, 95 mm or more and 810 mm or less. An example of the distance L4 is 130 mm.
[0060] An example of a method for manufacturing an oriented body will be described using the oriented body manufacturing apparatus 1 shown in Figure 8 as an example. When manufacturing an oriented body using the oriented body manufacturing apparatus 1, first, the above-mentioned sample holder 50 is attached to the oriented body manufacturing apparatus 1. As mentioned above, the case where the sample holder 50 has an outer tube 52 and an inner tube 53 will be described. The inner tube 53 is connected to a vacuum device. A cooling air supply source is connected to the lower end of the sample holder 50 so that cooling air flows through the gap between the outer tube 52 and the inner tube 53.
[0061] The holder 30 holding the material 3 is introduced into the first portion 441 of the material placement tube 44. This moves the holder 30 from the first portion 441 to the second portion 442. The holder 30 is maintained at the position of the stopper 51 of the sample holder 50. In this state, the holder 30 is located within the magnetic field generator 10. With the holder 30 (material 3) positioned in the second portion 442, the drive unit 20 (see FIG. 1) applies a three-phase AC voltage to the coils 121-123 of the magnetic field generator 10. This causes current to flow through the coils 121-123, generating a rotating magnetic field M in the material placement region 2 that rotates around the rotation axis 4 shown in FIG. 8. For example, the rotating magnetic field M is generated so that the magnetic flux density in the material placement region 2 is greater than 0.5 T and the rotation speed is greater than 60 rpm. The rotation axis 4 extends in a direction perpendicular to the X and Y directions shown in FIG. 1.
[0062] By generating a rotating magnetic field M in the material placement area 2 as described above, the rotating magnetic field M is applied to the material 3. As a result, the a-axes of the single crystal particles contained in the material (slurry) 3 are oriented in a plane perpendicular to the rotation axis 4, and the c-axes, which are the hard magnetization axes, are oriented in the direction of the rotation axis 4. In this embodiment, the liquid portion of the material 3 is discharged through the filter portion 32 of the holding unit 30. If the material of the filter portion 32 is gypsum, at least a portion of the liquid component is absorbed by the filter portion 32. As a result, the material 3 is solidified, and an oriented body (microcrystalline molded body) in which the c-axis is oriented in the direction of the rotation axis 4 can be produced. After producing the oriented body as described above, the sample holder 50 is removed from the bottom wall 42. This allows the holding unit 30 to be removed through the opening 42a, and as a result, the oriented body can be removed from the oriented body manufacturing apparatus 1.
[0063] When applying a three-phase AC voltage to the magnetic field generator 10 to produce an oriented body as described above, a vacuum device connected to the inner tube 53 is driven to evacuate the inner tube 53, and cooling air is circulated between the outer tube 52 and the inner tube 53. Because the holder 30 is disposed above the inner tube 53, the vacuum evacuations described above facilitate the discharge of the liquid portion of the material 3 and the promotion of water absorption by the filter unit 32. The cooling air flows from the sample holder 50 into the material placement tube 44, thereby suppressing the temperature rise of the holder 30 and the material 3 (slurry).
[0064] In the above-described oriented body manufacturing apparatus 1, the position of the magnetic field generator 10 is fixed relative to the material placement area 2. That is, the magnetic field generator 10 itself does not move or rotate relative to the material placement area 2. Because the fixed magnetic field generator 10 generates the rotating magnetic field M, the material 3 may also be fixed (in other words, stationary). Because the material 3 is fixed, deformation such as distortion is unlikely to occur in the oriented body being manufactured. Because the magnetic field generator 10 is not rotated or moved relative to the material placement area 2, a mechanism for rotating or moving the magnetic field generator 10 is not required, and the rotating magnetic field M can be adjusted by controlling the magnetic field generator 10. As a result, the state of the rotating magnetic field M is easily controlled, improving versatility.
[0065] As exemplified in the above-mentioned oriented body manufacturing apparatus 1, in a configuration in which a rotating magnetic field M is generated by controlling the voltage applied to the coils 121 to 123 of the magnetic field generating unit 10, the magnitude of the rotating magnetic field M, the rotation speed of the rotating magnetic field M, etc. can be easily controlled.
[0066] As described above, the oriented body manufacturing apparatus 1 according to one embodiment can easily generate a rotating magnetic field M having a magnetic flux density of greater than 0.5 T (tesla) in the material placement area 2. For example, the oriented body manufacturing apparatus 1 can achieve a magnetic flux density of 0.6 T or more. The oriented body manufacturing apparatus 1 according to one embodiment can easily generate a rotating magnetic field M having a rotation speed of greater than 60 rpm in the material placement area 2. For example, the oriented body manufacturing apparatus 1 can achieve a rotation speed of 300 rpm or more. An oriented body manufacturing apparatus 1 capable of achieving such magnetic flux densities and rotation speeds of the rotating magnetic field M is effective for controlling the orientation of biaxial crystals. The upper limit of the rotation speed of the rotating magnetic field M is not limited, but may be, for example, 60 Hz (3600 rpm), which is the frequency of a typical three-phase alternating current, or 20 kHz (1.2 Mrpm), which is the switching frequency of a high-power IGBT.
[0067] In a configuration in which the rotating magnetic field M is generated by controlling the voltage applied to the coils 121 to 123 of the magnetic field generation unit 10, it is easy to control the magnetic field generated by the electromagnet pairs 101, 102, and 103. As a result, the magnetic field generation unit 10 can generate not only a rotating magnetic field M with a constant rotation speed, but also a rotating magnetic field M with a modulated rotation speed, a rotating magnetic field M with an intermittent rotation, and the like. The rotation state, such as the rotation speed of the rotating magnetic field M, differs depending on the oriented body to be manufactured. Therefore, as described above, an oriented body manufacturing apparatus 1 equipped with a magnetic field generation unit 10 that can generate not only a rotating magnetic field M with a constant rotation speed, but also a rotating magnetic field M with a modulated rotation speed, and a rotating magnetic field M with an intermittent rotation, has greater versatility.
[0068] As mentioned above, the oriented body manufacturing apparatus 1 does not require a device for rotating or moving the magnetic field generating unit 10 itself or a device for rotating the material 3. This also improves the degree of freedom in designing the size of the material placement area 2. In this respect, the oriented body manufacturing apparatus 1, which is equipped with a magnetic field generating unit 10 capable of generating a rotating magnetic field M in a fixedly placed state, is easily applicable to the manufacture of oriented bodies for various purposes.
[0069] For example, when material 3 is rotated, a pressure distribution occurs within material 3 as a slurry. When the above-described pressure distribution occurs during slip casting, non-uniform casting pressure acts on material 3. This pressure distribution is likely to induce orientation disturbance due to the shape anisotropy of the single crystal particles. As a result, it is difficult to control the orientation when material 3 is rotated at a high speed.
[0070] In contrast, in the oriented body manufacturing apparatus 1, the rotating magnetic field M is generated by the magnetic field generating unit 10 without rotating the material 3 as described above. Therefore, even when a higher rotation speed of the rotating magnetic field M is required, it is easy to appropriately control the orientation. In this respect, the oriented body manufacturing apparatus 1 equipped with the magnetic field generating unit 10 capable of generating the rotating magnetic field M is easily applicable to the manufacture of oriented bodies for various uses.
[0071] Since the oriented body manufacturing apparatus 1 does not require a device for rotating or moving the magnetic field generating unit 10 itself or a device for rotating the material 3, vibrations applied to the material 3 can be suppressed. In other words, the oriented body manufacturing apparatus 1 is quieter. Therefore, deformations such as distortions are less likely to occur in the oriented body. Since the orientation is less likely to be hindered by the influence of vibrations, it is easier to achieve the desired orientation state. As a result, it is possible to obtain an oriented body with excellent orientation characteristics.
[0072] A voltage is applied to the coils 121-123 to generate the rotating magnetic field M, causing the coils 121-123 to generate heat. In the embodiment shown in FIG. 8, a boiling cooling method is used to cool the coils 121-123. The boiling cooling method utilizes boiling latent heat as well as the sensible heat difference caused by direct cooling using a boiling refrigerant in contact with the coils 121-123. It is known that boiling latent heat is about twice as great as sensible heat. Therefore, the boiling cooling method can cool the coils 121-123 more efficiently than a cooling method that utilizes only the sensible heat difference, such as a water cooling method.
[0073] In the embodiment shown in FIG. 8 , the boiling refrigerant that has evaporated during the cooling process of the coils 121-123 is returned to its liquid phase by the heat exchanger 47, which is cooled by an external drive, and accumulates again on the bottom wall 42 side. For example, when only direct cooling is used, such as in a water-cooling system, water (refrigerant) is typically circulated using a liquid pump or the like. In this case, a liquid pump must be installed inside the device. On the other hand, in the boiling cooling system, as described above, the evaporated refrigerant is returned to its liquid phase by the heat exchanger 47, which is cooled by an external drive, as described above. Therefore, since there is no need to install a liquid pump or the like inside the oriented body manufacturing apparatus 1, vibrations and the like are less likely to occur in the oriented body manufacturing apparatus 1. Because vibrations are suppressed in this way, the oriented body manufacturing apparatus 1 can produce oriented bodies with excellent orientation characteristics, as described above.
[0074] In the boiling cooling method, the surface temperature of the coils 121 to 123 can be controlled by the boiling point of the refrigerant used, which makes it easy to prevent dielectric breakdown caused by an excessive rise in the surface temperature of the coils 121 to 123.
[0075] When an insulating boiling refrigerant (for example, a low boiling point insulating liquid) is used as the boiling refrigerant 46, the coils 121 to 123 can be easily insulated.
[0076] As described above, by adopting the boiling cooling method, it is possible to efficiently cool the coils 121 to 123 and also to simplify the insulation process for the coils 121 to 123. As a result, it is also possible to reduce the size of the oriented body manufacturing apparatus 1.
[0077] In the boiling cooling method, the surface temperature of the coils 121 to 123 can be controlled by the boiling point of the refrigerant, so in order to properly operate the oriented body manufacturing apparatus 1, it is necessary to mainly monitor the temperature of the coils 121 to 123 and the pressure of the refrigerant vaporized within the oriented body manufacturing apparatus 1. Furthermore, the boiling cooling method does not use a liquefied gas such as liquid nitrogen as a refrigerant. Therefore, the oriented body manufacturing apparatus 1 can be operated unmanned for a long period of time (for example, one month or more).
[0078] 4, in a configuration in which the coils 121 to 123 are wound via the spacers 12b, the spacers 12b create gaps inside the coils 121 to 123. As a result, the coils 121 to 123 can be cooled efficiently.
[0079] Next, an experimental example will be described.
[0080] FIG. 9 is a diagram showing an example of a prototype magnetic field generator. In the magnetic field generator 10 shown in FIG. 9, the shape of the magnetic body 111 (the shape of the first connecting portion 111g) was a regular hexagon with sides of 200 mm. The shape of the second connecting portion 111h was also a regular hexagon. The maximum length of the diagonal line of the second connecting portion 111h was 20 mm. Although hidden by the coils 121-123 in FIG. 9, the magnetic cores 111a-111f connected the center of each side of the first connecting portion 111g to the corresponding side of the second connecting portion 111h. The coils 121-123 were conical with the bottom side facing outward. The number of turns of the coils 121-123 was 700.
[0081] FIG. 10 is a diagram showing the relationship between the current flowing through the coils 121-123 and the magnetic flux density at the center of the magnetic field generating unit 10 (center O shown in FIG. 1 ) in FIG. 10 . The horizontal axis of FIG. 10 represents the maximum current (A), and the vertical axis represents the magnetic flux density (T: Tesla). The magnetic flux density was measured using a Tesla meter TM-701 (manufactured by Kanetec Corporation). As shown in FIG. 10 , it can be seen that a rotating magnetic field M having a magnetic flux density of 0.5 T or more (more specifically, 0.6 T or more) can be stably generated at the center O of the material placement region 2 of the magnetic field generating unit 10 shown in FIG. 9 . Therefore, for example, if the magnetic field generating unit 10 is scaled up by a factor of five, a rotating magnetic field M of 1.4 T can be generated in the material placement region 2 where the maximum length of the diagonal line in the second connecting portion 111h is 100 mm.
[0082] FIG. 11 is a view of an oriented body manufactured using the oriented body manufacturing apparatus 1 shown in FIG. 8, as viewed from the central axis direction, and FIG. 12 is a side view of the oriented body shown in FIG.
[0083] The magnetic field generator 10 shown in FIG. 9 was used for the magnetic field generator 10 of the oriented body manufacturing apparatus 1 for manufacturing the oriented body shown in FIGS. 11 and 12 . In the oriented body manufacturing apparatus 1, the inner diameter of the first portion 441 was 32 mm. The inner diameter of the second portion 442 was 15 mm. The distances L1, L2, and L3 shown in FIG. 8 were 70 mm, 95 mm, and 115 mm, respectively. The boiling refrigerant 46 was Fluorinert. The amount of the boiling refrigerant 46 was approximately 25 liters. The distance L4 shown in FIG. 8 was 130 mm. The heat exchanger 47 used a fin tube cooled by external cooling water. When manufacturing the oriented body, the holding unit 30 was supported at a predetermined position by a sample holder 50 having an outer tube 52 and an inner tube 53. During manufacturing of the oriented body, the sample holder 50 was connected to a vacuum device to evacuate the sample holder 50, and cooling air was circulated through the sample holder 50.
[0084] The raw material powder contained in the material 3 as a slurry was FAP powder to which 10 at % Yb was added as a rare earth element. The material 3 was held in the holding unit 30 shown in FIG. 2 and placed in the material placement tube 44. The cylindrical unit 31 of the holding unit 30 was a glass cylinder with a diameter of 12 mm and a length of 25 cm in the central axis direction. The opening of the cylindrical unit 31 (the opening on the bottom wall 42 side) was closed by the filter unit 32.
[0085] In manufacturing the oriented body, a three-phase AC voltage was applied to the magnetic field generating unit 10, and a rotating magnetic field M with a magnetic flux density of 0.58 T (tesla) and a rotation speed of 180 rpm (3 Hz) was applied to the material 3.
[0086] As shown in Figures 10 and 11, the oriented body manufactured under the above conditions was substantially cylindrical. Because material 3 (slurry) did not rotate, no deformation (e.g., distortion) due to the rotation of material 3 occurred. As shown in Figure 10, the oriented body had a slightly hexagonal prism shape. This is because the magnitude of the generated magnetic flux density varies by several percent depending on the direction of the magnetic field generated by each of the electromagnet pairs 101, 102, and 103, and is thought to be due to errors in the winding density, the arrangement positions of the electromagnet pairs 101, 102, and 103, etc.
[0087] Figure 13 is a graph showing the results of analyzing the sintered oriented body shown in Figures 10 and 11 using X-ray diffraction. The oriented body was sintered at a temperature of 1375°C for one hour. The vertical axis of Figure 13 represents intensity, and the horizontal axis represents 2θ (°), which is the angle between the incident X-ray direction and the diffracted X-ray direction. A powder X-ray diffractometer (RINT Ultima-III, manufactured by Rigaku Corporation) was used to measure the X-ray diffraction.
[0088] As shown in Figure 13, the intensity of the c-plane diffraction peak (intensity at the (002) and (004) planes) was very large. Furthermore, the Rod-Gehring factor was 0.537. The Rod-Gehring factor is the ratio of the intensity of the peak originating from the orientation control symmetric axis in the XRD spectrum, normalized to 1 for completely controlled orientation, with 0 for completely random orientation. From the results shown in Figure 13, it can be seen that the degree of orientation was improved in the sintered oriented body.
[0089] Various embodiments of the present invention have been described above. The present invention is not limited to the illustrated various embodiments, but includes the scope indicated by the claims, and is intended to include all modifications within the meaning and scope equivalent to the claims.
[0090] The oriented body manufacturing apparatus described in the above embodiment can be applied not only to the manufacture of an oriented body including a biaxial crystal but also to the manufacture of an oriented body including a uniaxial crystal.
[0091] The oriented body manufacturing apparatus is used for oriented laser media and various laser application devices using the oriented laser media, such as laser processing devices (cutting devices, drilling devices, bending devices, manipulation devices, etc.), laser measurement devices (lidar, component analysis devices, etc.), laser display devices (displays, etc.), laser cosmetic devices (blemish removal devices, etc.), laser illumination devices (headlights, etc.), laser material manufacturing devices (ablation application devices, laser sintering devices, etc.), laser power supply devices, etc. The oriented body manufacturing apparatus can also be applied to the manufacture of ceramics other than ceramic laser media. For example, the oriented body manufacturing apparatus can be used for the manufacture of oriented rare earth high temperature superconductor REBa 2 Cu 4 O 8 It can be used to manufacture oriented ceramics that require a variable magnetic field, such as graphite ceramics (RE is a rare earth ion) and graphite ceramics, as well as to manufacture other materials besides oriented ceramics, such as fine powders produced by applying the magnetic properties of catalytic reactions.
[0092] The number of electromagnet pairs included in the magnetic field generation unit may be 2, or may be 4 or more. The configuration of the magnetic field generation unit is not limited as long as it is fixed relative to the material placement region and can generate a time-varying magnetic field in the material placement region.
[0093] The various embodiments and modifications described above may be combined as appropriate without departing from the spirit of the invention.
[0094] 1...aligned body manufacturing apparatus, 2...material placement area, 3...aligned body material, 10...magnetic field generating unit, 20...driving device, 40...housing, 46...boiling refrigerant (insulating liquid), 47...heat exchanger, 101, 102, 103...electromagnet pair (ith electromagnet), 101A, 101B...electromagnet, 102A, 102B...electromagnet, M...rotating magnetic field (magnetic field that changes over time).
Claims
1. An oriented body manufacturing apparatus comprising: a magnetic field generating unit that generates a magnetic field and is fixed in position relative to a material placement area in which an oriented body material whose orientation is controlled by a magnetic field is placed; and a driving device that drives the magnetic field generating unit to generate a time-varying magnetic field in the material placement area.
2. The oriented body manufacturing apparatus according to claim 1, wherein the magnetic field generating unit generates the magnetic field so that the magnetic flux density in the material placement region is greater than 0.5 T.
3. The apparatus for producing an oriented body according to claim 1, wherein the magnetic field generating unit generates a rotating magnetic field.
4. The oriented body manufacturing apparatus according to claim 3, wherein the magnetic field generating unit generates the magnetic field such that the magnetic flux density in the material placement region is greater than 0.5 T, and the rotation speed of the rotating magnetic field is greater than 60 rpm.
5. The oriented body manufacturing apparatus of claim 3 or 4, wherein the magnetic field generating section has N electromagnet pairs (N is an integer equal to or greater than 2), and when one of the N electromagnet pairs is referred to as the i-th electromagnet pair (i is any value from 1 to N), the directions of the magnetic fields generated by each of the two electromagnets in the i-th electromagnet pair are the same, and the two electromagnets in the i-th electromagnet pair are arranged on either side of the material placement area.
6. The apparatus for producing an oriented body according to claim 5, wherein the driving device applies voltages to the N electromagnet pairs with a phase shift so that the magnetic field generated by the N electromagnet pairs changes over time.
7. The apparatus for producing an oriented body according to claim 5, wherein the N electromagnet pairs are three electromagnet pairs, and the drive device applies voltages of each phase of a three-phase AC current to each of the three electromagnet pairs so as to generate the rotating magnetic field.
8. The apparatus for producing an oriented body according to claim 5, wherein the cooling method for cooling the magnetic field generating unit is a boiling cooling method.
9. The alignment body manufacturing apparatus according to claim 8, further comprising a housing having the material placement area and accommodating the magnetic field generating unit, wherein within the housing, the magnetic field generating unit is disposed in an insulating liquid having a boiling point lower than that of water.
10. The apparatus for manufacturing an oriented body according to claim 9, further comprising a heat exchanger disposed within the housing for returning the vaporized insulating liquid to a liquid phase, wherein a refrigerant is supplied to the heat exchanger from outside the housing.
Citation Information
Patent Citations
Ebullition cooling type electromagnet for linear motor
JP1983112457A
Resin molded body and method of manufacturing the same
JP2013241489A
Orientating element device and orientating element manufacturing method
JP2019192668A