Negative electrode for all-solid-state rechargeable batteries and all-solid-state rechargeable batteries
The use of a carbon material coating layer with specific properties on the negative electrode current collector in all-solid-state secondary batteries addresses the challenges of lithium metal anode expansion and dendrite growth, enhancing charge/discharge efficiency and output characteristics by promoting uniform lithium metal deposition.
Patent Information
- Application Number
- PCT/KR2023/018509
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2023-11-17
- Publication Date
- 2024-10-31
AI Technical Summary
All-solid-state secondary batteries face challenges with lithium metal anodes due to volume expansion and the growth of irreversible lithium dendrites, leading to reduced reversible capacity and safety issues, particularly with existing precipitation-type cathodes exhibiting low initial charge/discharge efficiency and output characteristics.
A negative electrode for all-solid-state secondary batteries is designed with a carbon material coating layer on the current collector, optimized for lithium metal precipitation, characterized by specific X-ray diffraction values and physical properties such as interplanar spacing, particle size, and Raman spectroscopy ratios, facilitating uniform lithium metal deposition and improved electrochemical performance.
The solution enhances initial charge/discharge efficiency and output characteristics by ensuring uniform lithium metal precipitation, thereby improving the electrochemical properties and safety of all-solid-state secondary batteries.
Smart Images

Figure KR2023018509_31102024_PF_FP_ABST
Abstract
Description
Anode for all-solid-state secondary battery and all-solid-state secondary battery
[0001] It relates to a negative electrode for an all-solid-state secondary battery and an all-solid-state secondary battery.
[0002] Commercially available lithium secondary batteries use electrolytes containing flammable organic solvents, posing safety concerns that can lead to explosion or fire in the event of collisions, penetration, or other problems. Therefore, all-solid-state secondary batteries, which utilize solid electrolytes instead of the electrolyte, have been proposed. All-solid-state secondary batteries are composed entirely of solid materials, eliminating the risk of electrolyte leakage and explosion, making them safer. Furthermore, they facilitate the production of thin batteries, allowing for a reduced anode thickness, improving high-speed charge / discharge performance and enabling high-voltage operation and high-energy density.
[0003] Lithium metal anodes can be used as cathodes in all-solid-state secondary batteries. While this can increase energy density, it also suffers from the problem of lithium metal volume expansion. Furthermore, irreversible lithium dendrite growth on the cathode surface during charging and discharging can reduce reversible capacity and compromise safety due to battery short-circuiting.
[0004] Accordingly, research is being conducted on methods that utilize lithium metal as an anode active material by precipitating it onto the anode current collector during charging, rather than using lithium metal itself as the anode active material. However, existing precipitation-type anodes have limitations, such as low initial charge / discharge efficiency and output characteristics, and the potential for battery short-circuiting.
[0005] Provided is an anode for an all-solid-state secondary battery in which lithium metal can be uniformly and well deposited at a thickness during charging, and an all-solid-state secondary battery with improved initial charge / discharge efficiency and output characteristics.
[0006] In one embodiment, a negative electrode current collector is provided, and a negative electrode coating layer is positioned on the negative electrode current collector and includes a carbon material, wherein the carbon material has a d measured by X-ray diffraction.002 A negative electrode for an all-solid-state secondary battery having a value of 3.500 or more and 3.620 or less is provided.
[0007] In another embodiment, an all-solid-state secondary battery is provided, including the cathode and the anode, and a solid electrolyte membrane positioned between the cathode and the anode.
[0008] An anode for an all-solid-state secondary battery according to one embodiment can induce precipitation of a good lithium metal layer of uniform thickness during charging, thereby improving electrochemical characteristics such as initial charge / discharge efficiency and output characteristics of the all-solid-state secondary battery.
[0009] Figure 1 is a cross-sectional view schematically showing an all-solid-state secondary battery according to one embodiment.
[0010] Figure 2 is a schematic diagram of the carbon material of the cathode coating layer of Example 1.
[0011] Figure 3 is a field emission scanning electron microscope (FE-SEM) image of a cross-section of the cathode coating layer of Example 1.
[0012] Figure 4 is a schematic diagram of the carbon material of the cathode coating layer of Comparative Example 1.
[0013] Figure 5 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 1.
[0014] Figure 6 is a schematic diagram of the carbon material of the cathode coating layer of Comparative Example 2.
[0015] Figure 7 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 2.
[0016] Figure 8 is a schematic diagram of the carbon material of the cathode coating layer of Comparative Example 3.
[0017] Figure 9 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 3.
[0018] Figure 10 is a schematic diagram of the carbon material of the cathode coating layer of Comparative Examples 4 and 5.
[0019] Figure 11 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 4.
[0020] Figure 12 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 5.
[0021] Figure 13 is an image of a cross-section of a cathode taken by FE-SEM after initial charging of an all-solid-state secondary battery of Example 1.
[0022] Figure 14 is an image of the cross-section of the cathode of the all-solid-state secondary battery of Comparative Example 4 taken by FE-SEM after initial charging.
[0023] Figure 15 is an image of a cross-section of a cathode taken by FE-SEM after initial charging of an all-solid-state secondary battery of Comparative Example 5.
[0024] Below, specific implementation examples are described in detail to facilitate their implementation by those skilled in the art. However, the present invention may be implemented in various different forms and is not limited to the implementation examples described herein.
[0025] The terminology used herein is for the purpose of describing exemplary embodiments only and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise.
[0026] “Combination of these” means a mixture, laminate, composite, copolymer, alloy, blend, reaction product, etc. of the components.
[0027] It should be understood that terms such as "include," "comprise," or "have" are intended to specify the presence of a feature, number, step, component, or combination thereof, but do not preclude the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0028] To clearly illustrate various layers and regions in the drawings, their thicknesses are enlarged, and similar parts are designated by the same drawing reference numerals throughout the specification. When an element such as a layer, film, region, or plate is said to be "over" or "on" another element, this includes not only the case where it is "directly over" the other element, but also the case where there are other elements in between. Conversely, when an element is said to be "directly over" another element, it means that there are no other elements in between.
[0029] “Layer” includes not only shapes formed on the entire surface when observed in a plan view, but also shapes formed on some surfaces.
[0030] The average particle size can be measured by methods well known to those skilled in the art, for example, by measuring with a particle size analyzer, or by measuring with a transmission electron microscope image or a scanning electron microscope image. Alternatively, the average particle size can be obtained by measuring using dynamic light scattering, performing data analysis, counting the number of particles for each particle size range, and calculating from the counted number. Unless otherwise defined, the average particle size can mean the diameter (D50) of particles in a particle size distribution that have a cumulative volume of 50% by volume. In addition, unless otherwise defined, the average particle size can be obtained by randomly measuring the sizes (diameters or major axis lengths) of about 20 particles in a scanning electron microscope image to obtain a particle size distribution, and taking the diameter (D50) of particles in the particle size distribution that have a cumulative volume of 50% by volume as the average particle size.
[0031] “Or” is not interpreted as exclusive, for example, “A or B” is interpreted as including A, B, A+B, etc.
[0032] “Metal” is interpreted as a concept that includes common metals, transition metals, and metalloids (semi-metals).
[0033] cathode
[0034] In one embodiment, a negative electrode for an all-solid-state secondary battery is provided, which includes a negative electrode current collector and a negative electrode coating layer positioned on the negative electrode current collector and containing a carbon material. The carbon material in the negative electrode coating layer has a d measured by X-ray diffraction. 002 It is characterized by a value of 3.500 or more and 3.620 or less.
[0035] cathode coating layer
[0036] The cathode coating layer can be said to be a layer that helps lithium ions released from the cathode active material when charging an all-solid-state secondary battery to be used toward the cathode, thereby facilitating the deposition of lithium metal on the surface of the cathode current collector. During charging, lithium metal is deposited between the cathode current collector and the cathode coating layer, forming a lithium metal layer, which then functions as the cathode active material. Such a cathode can be expressed as a deposition-type cathode, and the cathode coating layer can be expressed as a lithium deposition-inducing layer or a cathode catalyst layer.
[0037] The carbon material of the anode coating layer plays a role in adsorbing lithium ions released from the cathode during charging, and in helping the lithium ions to smoothly move and pass with low energy and be uniformly deposited as lithium metal on the surface of the current collector. In one embodiment, a carbon material having properties optimized for this role is proposed. The carbon material of the anode coating layer is typically amorphous carbon, and examples of carbon black, activated carbon, acetylene black, Denka black, Ketjen black, or a combination thereof can be used. However, even the same type of carbon material can have various properties, and in one embodiment, a carbon material having properties optimized for inducing uniform deposition of lithium metal is proposed.
[0038] According to an embodiment, the carbon material has an average plane spacing of (002) planes, d, measured by X-ray diffraction. 002 It is characterized by a value of 3.500 or more and 3.620 or less. d 002It refers to the interlayer spacing (d-spacing) of carbon and can be used as a measure of the degree of crystallinity of carbon materials, and its unit is Å. The d of the above carbon materials 002 For example, it can be 3.550 or more and 3.615 or less, or 3.555 or more and 3.610 or less. d in the above range 002 Carbon materials with a value can be said to have the most appropriate crystallinity for application to the negative electrode coating layer, and can lower the movement energy of lithium ions, thereby inducing the lithium ions to move smoothly and be deposited on the surface of the current collector. d of carbon materials 002 When the value exceeds 3.620, the crystallinity of the carbon material increases, increasing the mobility energy of lithium ions, and d 002 If the value is less than 3.500, the carbon structure is unstable, which hinders the movement of lithium ions, making it difficult to induce uniform precipitation of lithium metal and reducing the charge / discharge efficiency or output characteristics of the all-solid-state secondary battery.
[0039] d 002 can be calculated from the Bragg equation using the Bragg 2θ angle and half-width of the (002) plane peak in X-ray diffraction analysis of carbon materials, and the X-ray diffraction analysis can be performed under the condition of a wavelength of 1.541838 Å (CuKα).
[0040] According to one embodiment, the particle size of the primary particles of the carbon material may be 20 nm to 200 nm, for example, 20 nm to 150 nm, 20 nm to 100 nm, 20 nm to 70 nm, or 30 nm to 45 nm. When a carbon material satisfying the primary particle particle size range is used in the negative electrode coating layer, the resistance to the movement of lithium ions is minimized, which can induce the deposition of a uniform lithium metal layer and improve the charge / discharge efficiency and output characteristics of the all-solid-state secondary battery. For example, when the particle size of the primary particles of the carbon material exceeds 200 nm, the size of the pores between the particles may increase, which can increase the resistance to the movement of lithium ions, and when the particle size of the primary particles of the carbon material is less than 20 nm, the processability may deteriorate or it may be difficult to form a good negative electrode coating layer.
[0041] The particle size of the primary particles of carbon material can be measured, for example, through an electron microscope such as SEM, FE-SEM, or TEM for the cathode coating layer. Specifically, the particle size distribution is obtained by randomly measuring the size (diameter or length of major axis) of about 20 primary particles of carbon material in the electron microscope image for the cathode coating layer, and the size of the particle having a cumulative volume of 50% by volume in the particle size distribution, i.e., D 50 The value may be taken as the particle size of the primary particle.
[0042] According to one embodiment, the circularity of the primary particles of the carbon material may be 0.80 or more and 1.0 or less, for example, 0.81 or more and 1.0 or less, 0.82 or more and 1.0 or less, 0.83 or more and 1.0 or less, 0.84 or more and 1.0 or less, 0.80 or more and 0.99 or less, 0.80 or more and 0.95 or less, or 0.80 or more and 0.91 or less. When the circularity of the carbon material satisfies the above range, the movement distance of lithium ions within the negative electrode coating layer may be minimized, thereby helping lithium metal to be uniformly deposited on the surface of the current collector. For example, if the sphericity of the carbon material is less than 0.80, or if the carbon material is not close to a circle but has a plate-like, branch-like, or needle-like shape, the distance for lithium movement within the negative electrode coating layer becomes longer, making it difficult to expect effective lithium precipitation, and as a result, the output characteristics of the battery may deteriorate.
[0043] The sphericity of carbon materials means that the shape is closer to a sphere as it approaches 0 to 1, and can be measured using an electron microscope image such as FE-SEM of a cathode coating layer using the Image J program, for example. That is, the Image J program can recognize about 20 to 50 primary particles in the electron microscope image of the cathode coating layer and derive their sphericity.
[0044] According to an embodiment, the carbon material has a ratio of D band intensity to G band intensity measured by Raman spectroscopy (I D / I G ) may be 1.5 or more and 3.0 or less, for example 1.6 or more and 3.0 or less, 1.7 or more and 3.0 or less, 1.8 or more and 3.0 or less, 1.9 or more and 3.0 or less, 2.0 or more and 3.0 or less, 2.1 or more and 3.0 or less, 1.5 or more and 2.9 or less, or 1.5 or more and 2.8 or less.
[0045] I D / I GThe ratio can be said to be the ratio of the intensity of the D peak to the intensity of the G peak in Raman spectroscopy. The D peak is located at about 1200 cm -1 1400 cm inland -1 Peaks appearing at the wavelength of SP such as CH, C-OH, C-OOH, etc. 3 It can be said to be a peak indicating bonding. The G peak is about 1400 cm -1 1600 cm inland -1 The peak appears at the wavelength of the SP of CC 2 It can be said to be a peak indicating bonding. I of carbon material D / I G A higher ratio means that there is an increase in some kind of defects such as C-OOH, C-OH, etc. According to one implementation example, the I of the carbon material D / I G When the ratio satisfies 1.5 or more and 3.0 or less, the degree of defects in the carbon material is appropriately high, so that the affinity with lithium is increased, and the movement energy of lithium ions can be lowered, and accordingly, uniform precipitation of lithium metal is induced, and the charge / discharge efficiency and output characteristics of the battery can be improved. For example, I D / I G If the ratio is less than 1.5, the degree of lithiation of the carbon material is low, the mobility energy of lithium ions increases, it is difficult to induce uniform precipitation of lithium metal, and the initial charge / discharge efficiency and output characteristics of the battery may deteriorate.
[0046] I of carbon material D / I G can be obtained by Raman spectroscopy and measured, for example, by an analytical instrument Raman 2010 Spectra (NT-MDT Development Co.).
[0047] The BET surface area of the carbon material according to one embodiment is 10 m 2 / g to 200 m 2 / g can be, for example, 20 m 2 / g to 150 m 2 / g, 30 m2 / g to 120 m 2 / g, 40 m 2 / g to 100 m 2 / g, or 45 m 2 / g to 90 m 2 / g. If the BET surface area of the carbon material satisfies the above range, lithium ions can pass through the carbon material smoothly without being trapped inside the carbon material. For example, if the BET surface area is 200 m 2 / g exceeds, the pores inside the carbon material may become relatively large or enlarged, which may cause lithium ions to be trapped inside the carbon material, lengthening the movement path of lithium ions, which may ultimately hinder the precipitation of lithium metal, and thus deteriorate the electrochemical characteristics of the all-solid-state secondary battery. The BET specific surface area can be measured by the nitrogen gas adsorption method using a device such as HM model-1208 (MOUNTECH).
[0048] According to one embodiment, the carbon material may have a pore size between primary particles of 10 nm to 1000 nm, for example, 20 nm to 900 nm, 30 nm to 700 nm, or 40 nm to 500 nm. When the pore size between carbon particles satisfies the above range, the path of lithium ions can be minimized, thereby inducing uniform precipitation of lithium metal. When the pore size is too large, the migration path of lithium ions becomes longer or the energy required for migration increases, making uniform lithium metal precipitation difficult.
[0049] The size of the pores between the primary particles of the carbon material can be obtained by randomly measuring the sizes (diameter or length of the major axis) of about 20 pores in an electron microscope photograph of a cross-section of a cathode coating layer, for example, and taking the arithmetic average of these, and can also be expressed as the average pore size.
[0050] Meanwhile, in one example, the carbon material may include elemental sulfur, a sulfur-containing functional group, a sulfur-containing compound, or a combination thereof located on its surface. That is, elemental sulfur, a sulfur-containing functional group, or a sulfur-containing compound may be present on the surface of the carbon material according to one embodiment, and for example, elemental sulfur, a sulfur-containing functional group, or a sulfur-containing compound may be coated on the surface of carbon material particles in a continuous film form or an island form. In this case, the carbon material may have an increased affinity for lithium and an improved miscibility with a sulfide-based solid electrolyte, or the bonding with a lithium-philic metal that may be present in the negative electrode coating layer may be improved, or the dispersion degree of the lithium-philic metal may be improved.
[0051] The sulfur-containing functional group can be, for example, a thiol group, a sulfide group, a sulfonic acid group, a sulfone group, a sulfoxide group, or a combination thereof.
[0052] A sulfur-containing compound refers to an organic compound containing elemental sulfur, and may also be referred to as a compound having the aforementioned sulfur-containing functional group. For example, the sulfur-containing compound may be a thiol compound, a sulfide compound, a thiophene compound, a sulfonic acid, a sulfone, a sulfoxide, or a combination thereof.
[0053] The thiol compound may include, for example, mercapto acetic acid, 1-dodecanethiol, 6-mercapto-1-hexanol, 11-mercapto-1-undecanol, 2-naphthalenethiol, 1,4-benzenedimethanethiol, 4-mercaptobenzoic acid, 1,3-benzenedithiol, or combinations thereof.
[0054] The sulfide compound may include, for example, polyphenylene sulfide, carbon disulfide, a metal sulfide, or a combination thereof. In the metal sulfide, the metal may be, for example, Ag, Na, Zn, Fe, or a combination thereof.
[0055] The thiophene compound may include, for example, thiophene (C4H4S), 2-methylthiophene, thianaphthalene, 4,6-dimethylbenzothiophene, or a combination thereof.
[0056] The sulfonic acid may include, for example, p-toluene sulfonic acid, sodium dodecylbenzenesulfonate, taurine, or a combination thereof, the sulfone may include dimethyl sulfone, 4,4'-dichlorodiphenyl sulfone, or a combination thereof, and the sulfoxide may include dimethyl sulfoxide, methyl phenyl sulfoxide, or a combination thereof.
[0057] By dry or wet mixing carbon materials and sulfur-containing raw materials and optionally heat treating them, elemental sulfur, sulfur-containing functional groups, or sulfur-containing compounds can be introduced to the surface of the carbon materials. The heat treatment can be performed at a temperature range of, for example, 70°C to 110°C. The sulfur-containing raw material can include the aforementioned thiol compounds, sulfide compounds, thiophene compounds, sulfonic acids, sulfones, sulfoxides, or combinations thereof.
[0058] When sulfur element, sulfur-containing functional group, or sulfur-containing compound is present on the surface of the carbon material, the weight ratio of carbon to sulfur may be, for example, 4:1 to 999:1, 4:1 to 900:1, 5:1 to 100:1, or 5:1 to 20:1.
[0059] Meanwhile, the negative electrode coating layer may further include a lithium-philic metal in addition to the carbon material. When the negative electrode coating layer further includes a lithium-philic metal, lithium metal can be effectively deposited on the surface of the negative electrode current collector during charging, a lithium metal layer of uniform thickness can be formed, the electrical conductivity of the negative electrode can be further improved, and the electrochemical characteristics of the all-solid-state secondary battery can be improved.
[0060] The lithiphilic metal may include, for example, Al, Ag, Au, Bi, Cu, Ge, In, Mg, Ni, Pd, Pt, Si, Sn, Zn, or a combination thereof, and may be composed of one of these or an alloy of two or more thereof. The average particle diameter (D) of the lithiphilic metal 50 ) may be about 900 nm or less, and may be, for example, 5 nm to 900 nm, 5 nm to 500 nm, 10 nm to 200 nm, 10 nm to 100 nm, or 20 nm to 80 nm. When the average particle diameter of the lithium-philic metal satisfies the above range, the uniformity of the particle size increases and it is appropriately dispersed in the negative electrode coating layer, thereby effectively inducing precipitation of the lithium metal.
[0061] The content of the lithium-philic metal may be 3 wt% to 40 wt% with respect to 100 wt% of the negative electrode coating layer, for example, 3 wt% to 30 wt%, 4 wt% to 25 wt%, 5 wt% to 20 wt%, or 5 wt% to 15 wt%. When the content of the lithium-philic metal satisfies the above range, a uniform lithium metal layer can be effectively formed during charging.
[0062] The cathode coating layer may include a mixture of carbon material and a lithium-philic metal, or may include a composite in which a lithium-philic metal is supported on a carbon material.
[0063] In one embodiment, the carbon material and the lithium-philic metal may be chemically bonded via sulfur. That is, the carbon material and the lithium-philic metal may not be simply physically mixed, but may be chemically bonded to each other. In this case, the bonding strength between the carbon material and the lithium-philic metal is excellent, and the problem of the carbon material and the lithium-philic metal separating from each other during the mixing process can be effectively prevented. In addition, the phenomenon of the lithium-philic metal agglomerating is prevented, so that it can be uniformly dispersed within the negative electrode coating layer, thereby uniformly distributing the current within the negative electrode and inducing uniform deposition of the lithium metal.
[0064] When carbon materials and a lithiophilic metal are chemically bonded via sulfur, peaks related to the bonding of the lithiophilic metal and sulfur can be identified in the X-ray photoelectron spectroscopy (XPS) spectrum. For example, when the lithiophilic metal contains Ag, a peak can be identified in the S2p spectrum obtained by XPS analysis in the range of 160 eV to 162 eV, which is the Ag-S bond energy.
[0065] A composite in which carbon material and a lithium-philic metal are chemically bonded via sulfur can be manufactured by mixing carbon material and sulfur-containing raw materials in a dry or wet manner, optionally heat-treating them, then supporting the lithium-philic metal and heat-treating the mixture.
[0066] A method for supporting a lithiophilic metal may be, for example, a method of mixing a mixture of a carbon material and a sulfur-containing raw material, a lithiophilic metal compound, and a reducing agent in a solvent. The solvent may include, for example, water, ethanol, glycerol, benzene, xylene, or a combination thereof, and the reducing agent may include NaBH4, ascorbic acid, trisodium citrate, ethylene glycol, or a combination thereof. The lithiophilic metal compound may be a nitrate, sulfate, perchlorate, or the like containing a lithiophilic metal, and may include, for example, AgNO3, Ag2SO4, AgClO4, or a combination thereof.
[0067] The heat treatment after supporting the lithium-philic metal can usually be carried out at a temperature at which the sulfur-containing raw material can be decomposed and removed, for example, at 100°C to 500°C, 150°C to 500°C, 200°C to 450°C, or 200°C to 400°C. Specifically, when a thiol compound is used as the sulfur-containing raw material, the heat treatment can be carried out at 100°C to 400°C. The heat treatment can be carried out in an atmosphere of nitrogen, argon, or a combination thereof for about 2 to 20 hours.
[0068] The thickness of the cathode coating layer may be, for example, 100 nm to 40 μm, or 500 nm to 30 μm, or 1 μm to 20 μm. When the cathode coating layer satisfies the above thickness range, a lithium metal layer of uniform thickness can be effectively formed during charging.
[0069] The cathode coating layer may further include a binder, for example, a conductive binder. The cathode coating layer may also further include additives such as fillers, dispersants, and ionic conductive agents.
[0070] The binder of the cathode coating layer may include a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof.
[0071] Non-aqueous binders include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0072] The aqueous binder may be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluoroelastomer, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenol resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0073] When using an aqueous binder as the cathode binder, a cellulose-based compound capable of imparting viscosity may be further included. The cellulose-based compound may be a mixture of one or more of carboxymethyl cellulose, hydroxypropylmethyl cellulose, methyl cellulose, or an alkali metal salt thereof. The alkali metal may be Na, K, or Li.
[0074] The dry binder is a polymeric material capable of being fiberized, such as polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.
[0075] The binder may be included in an amount of 0.1 to 5 wt%, 0.1 to 3 wt%, or 0.5 to 2 wt%, based on 100 wt% of the cathode coating layer.
[0076] negative current collector
[0077] The negative electrode current collector may include, for example, indium (In), copper (Cu), magnesium (Mg), stainless steel, titanium (Ti), iron (Fe), cobalt (Co), nickel (Ni), zinc (Zn), aluminum (Al), germanium (Ge), lithium (Li) or an alloy thereof, and may be in the form of a foil or a sheet. The thickness of the negative electrode current collector may be, for example, 1 μm to 20 μm, 5 μm to 15 μm, or 7 μm to 10 μm.
[0078] lithium metal layer
[0079] According to one embodiment, the negative electrode is a type of precipitation-type negative electrode, and an all-solid-state secondary battery including the same starts initial charging in a state in which no negative electrode active material is present, and during charging, a high-density lithium metal is precipitated or deposited between the negative electrode collector and the negative electrode coating layer, or on the negative electrode coating layer, to form a lithium metal layer, which can function as the negative electrode active material. Therefore, an all-solid-state secondary battery that has been charged at least once may include, for example, a negative electrode collector, a lithium metal layer positioned on the negative electrode collector, and a negative electrode coating layer positioned on the lithium metal layer. The lithium metal layer means a layer in which lithium ions are precipitated as lithium metal during the charging process of the battery, and may be expressed as a metal layer, a lithium layer, a lithium deposition layer, or a negative electrode active material layer.
[0080] The lithium metal layer may include lithium metal or a lithium alloy. The lithium alloy may be, for example, a Li-Al alloy, a Li-Sn alloy, a Li-In alloy, a Li-Ag alloy, a Li-Au alloy, a Li-Zn alloy, a Li-Ge alloy, or a Li-Si alloy.
[0081] The thickness of the lithium metal layer may be, for example, 1 μm to 500 μm, 5 μm to 500 μm, 5 μm to 400 μm, 5 μm to 300 μm, or 10 μm to 200 μm. If the thickness of the lithium metal layer is too thin, it may be difficult to perform the role of a lithium storage tank, and if it is too thick, the battery volume may increase and the performance may deteriorate.
[0082] In one embodiment, by applying the carbon material having the above-described properties to the negative electrode coating layer, a lithium metal layer having a uniform thickness and a flat surface can be formed. Therefore, according to one embodiment, the lithium metal layer formed during charging may have a very uniform thickness and a small thickness deviation. For example, the deviation in the thickness of the lithium metal layer may be 40% or less, 30% or less, 20% or less, 15% or less, 10% or less, or 5% or less. Here, the deviation in the thickness of the lithium metal layer may mean that the thickness of the lithium metal layer is measured at about 10 points in an electron microscope image of the negative electrode cross-section, the arithmetic mean is calculated, and then the absolute value of the difference between one data point and the arithmetic mean is divided by the arithmetic mean and multiplied by 100. Also, for example, the thickness of the lithium metal layer may be 5 ㎛ to 80 ㎛, and the standard deviation of the thickness may be 0.1 ㎛ to 20 ㎛, 0.1 ㎛ to 15 ㎛, 0.1 ㎛ to 10 ㎛, 0.1 ㎛ to 5 ㎛, and 0.1 ㎛ to 3 ㎛. Similarly, the standard deviation of the thickness of the lithium metal layer may be calculated by measuring the thickness at about 10 points in an electron microscope photograph. The fact that the deviation or standard deviation of the thickness of the lithium metal layer satisfies the above range means that the lithium metal is well deposited in the form of a film with a uniform thickness, and accordingly, the electrochemical characteristics of the all-solid-state secondary battery may be improved.
[0083] etc
[0084] Meanwhile, the negative electrode according to one embodiment may further include a thin film on the surface of the negative electrode current collector, that is, between the negative electrode current collector and the negative electrode coating layer, or between the negative electrode current collector and the lithium metal layer. The thin film may include an element capable of forming an alloy with lithium. The element capable of forming an alloy with lithium may include, for example, Al, Ag, Au, Bi, Cu, Ge, In, Mg, Ni, Pd, Pt, Si, Sn, Zn, or a combination thereof. The thin film may further flatten the deposition morphology of the lithium metal layer and assist in forming a lithium metal layer with a uniform thickness. The thin film may be formed by, for example, a vacuum deposition method, a sputtering method, a plating method, or the like. The thickness of the thin film may be, for example, 1 nm to 500 nm.
[0085] All-solid-state secondary battery
[0086] In one embodiment, an all-solid-state secondary battery is provided, including the aforementioned cathode and anode, and a solid electrolyte membrane positioned between the cathode and the anode.
[0087] Fig. 1 is a cross-sectional view of an all-solid-state secondary battery according to an embodiment. Referring to Fig. 1, an all-solid-state secondary battery (100) may have a structure in which an electrode assembly in which a negative electrode (400), a solid electrolyte layer (300), and a positive electrode (200) are laminated is housed in a battery case.
[0088] As described above, the negative electrode (400) includes a current collector (401) and a negative electrode coating layer (405) positioned on the current collector. The all-solid-state secondary battery (100) is initially charged in a state in which no negative electrode active material is present, and during charging, high-density lithium metal is precipitated or deposited between the current collector (401) and the negative electrode coating layer (405) or on the negative electrode coating layer (405) to form a lithium metal layer (404), which can serve as the negative electrode active material. In the all-solid-state secondary battery (100) that has been charged at least once, the negative electrode (400) includes, for example, a current collector (401), a lithium metal layer (404) positioned on the current collector, and a negative electrode coating layer (405) positioned on the metal layer.
[0089] The positive electrode (200) includes a positive electrode current collector (201) and a positive electrode active material layer (203).
[0090] The all-solid-state secondary battery (100) may further include an elastic layer (500) on the outer side of at least one of the positive electrode (200) and the negative electrode (400). FIG. 1 illustrates one electrode assembly including the negative electrode (400), the solid electrolyte layer (300), and the positive electrode (200), but an all-solid-state secondary battery may be manufactured by stacking two or more electrode assemblies.
[0091] anode
[0092] In one embodiment, the device comprises a current collector and a positive electrode active material layer positioned on the current collector, wherein the positive electrode active material layer comprises a positive electrode active material and optionally may comprise a solid electrolyte, a binder, and / or a conductive material.
[0093] positive electrode active material
[0094] A compound capable of reversible intercalation and deintercalation of lithium (a lithiated intercalation compound) can be used as a cathode active material. Specifically, one or more of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and combinations thereof can be used.
[0095] The above composite oxide may be a lithium transition metal composite oxide, and specific examples thereof include lithium nickel-based oxide, lithium cobalt-based oxide, lithium manganese-based oxide, lithium iron phosphate-based compound, cobalt-free nickel-manganese-based oxide, lithium-rich layered oxide, or a combination thereof.
[0096] For example, the cathode active material may be a high-nickel cathode active material in which the nickel content is 80 mol% or more based on 100 mol% of metals excluding lithium in a lithium transition metal composite oxide. The nickel content in the high-nickel cathode active material may be 85 mol% or more, 90 mol% or more, 91 mol% or more, or 94 mol% or more, and 99 mol% or less based on 100 mol% of metals excluding lithium. The high-nickel cathode active material can realize high capacity and thus can be applied to high-capacity, high-density lithium secondary batteries.
[0097] As a more specific example, a compound represented by any one of the following chemical formulas may be used: Li a A 1-b X b O 2-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Mn 2-b X b O 4-c D c (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.05); Li a Ni 1-b-c Co b X c O 2-α D α (0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤0.5, 0 < α < 2);Li a Ni 1-b-c Mn b X c O 2-α D α(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.5, 0 ≤ c ≤ 0.5, 0 < α < 2);Li a Ni b Co c L 1 d G e O2(0.90 ≤ a ≤ 1.8, 0 ≤ b ≤ 0.9, 0 ≤ c ≤ 0.5, 0 ≤ d ≤ 0.5, 0 ≤ e ≤ 0.1);; Li a NiG b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a CoG b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn 1-b G b O2(0.90 ≤ a ≤ 1.8, 0.001 ≤ b ≤ 0.1); Li a Mn2G b O4(0.90 ≤ a ≤1.8, 0.001 ≤ b ≤ 0.1); Li a Mn 1-g G g PO4(0.90 ≤ a ≤ 1.8, 0 ≤ g ≤ 0.5); Li (3-f) Fe2(PO4)3(0 ≤ f ≤ 2); Li a FePO4(0.90 ≤ a ≤ 1.8)
[0098] In the above chemical formula, A is Ni, Co, Mn, or a combination thereof; X is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element, or a combination thereof; D is O, F, S, P, or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V, or a combination thereof; Q is Ti, Mo, Mn, or a combination thereof; Z is Cr, V, Fe, Sc, Y, or a combination thereof; L 1 is Mn, Al or a combination thereof.
[0099] The cathode active material may include, for example, a lithium nickel-based oxide represented by the following chemical formula 11, a lithium cobalt-based oxide represented by the following chemical formula 12, a lithium iron phosphate-based compound represented by the following chemical formula 13, a cobalt-free lithium nickel-manganese-based oxide represented by the following chemical formula 14, or a combination thereof.
[0100] [Chemical Formula 11]
[0101] Li a1 Ni x1 M 1 y1 M 2 z1 O 2-b1 X b1
[0102] In the above chemical formula 11, 0.9≤a1≤1.8, 0.3≤x1≤1, 0≤y1≤0.7, 0≤z1≤0.7, 0.9≤x1+y1+z1≤1.1, and 0≤b1≤0.1, and M 1 and M 2 are each independently one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0103] In the above chemical formula 1, 0.6≤x1≤1, 0≤y1≤0.4, and 0≤z1≤0.4, or 0.8≤x1≤1, 0≤y1≤0.2, and 0≤z1≤0.2.
[0104] [Chemical Formula 12]
[0105] Li a2 Co x2 M 3 y2 O 2-b2 X b2
[0106] In the above chemical formula 12, 0.9≤a2≤1.8, 0.7≤x2≤1, 0≤y2≤0.3, 0.9≤x2+y2≤1.1, and 0≤b2≤0.1, and M 3is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn and Zr, and X is one or more elements selected from the group consisting of F, P and S.
[0107] [Chemical Formula 13]
[0108] Li a3 Fe x3 M 4 y3 PO 4-b3 X b3
[0109] In the above chemical formula 13, 0.9≤a3≤1.8, 0.6≤x3≤1, 0≤y3≤0.4, and 0≤b3≤0.1, and M 4 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Co, Cr, Cu, Mg, Mn, Mo, Ni, Se, Si, Sn, Sr, Ti, V, W, Y, Zn and Zr, and X is one or more elements selected from the group consisting of F, P and S.
[0110] [Chemical Formula 14]
[0111] Li a4 Ni x4 Mn y4 M 5 z4 O 2-b4 X b4
[0112] In the above chemical formula 14, 0.9≤a2≤1.8, 0.8≤x4<1, 0 <y4≤0.2, 0≤z4≤0.2, 0.9≤x4+y4+z4≤1.1, 및 0≤b4≤0.1이고 M 5 is one or more elements selected from the group consisting of Al, B, Ba, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, and Zr, and X is one or more elements selected from the group consisting of F, P, and S.
[0113] The average particle diameter (D50) of the positive electrode active material may be 1 μm to 25 μm, for example, 3 μm to 25 μm, 1 μm to 20 μm, 1 μm to 18 μm, 3 μm to 15 μm, or 5 μm to 15 μm. For example, the positive electrode active material may include small particles having an average particle diameter (D50) of 1 μm to 9 μm and large particles having an average particle diameter (D50) of 10 μm to 25 μm. A positive electrode active material having such a particle diameter range can be harmoniously mixed with other components within a positive electrode active material layer and can realize high capacity and high energy density. Here, the average particle diameter may be obtained by selecting 20 or so random particles from a scanning electron microscope image of the positive electrode active material, measuring their particle diameters (diameter, major axis, or major axis length), obtaining a particle size distribution, and then taking the diameter (D50) of particles having a cumulative volume of 50% by volume from the particle size distribution as the average particle diameter.
[0114] The above-mentioned positive electrode active material may be in the form of a secondary particle formed by agglomeration of a plurality of primary particles, or may be in the form of a single particle. In addition, the above-mentioned positive electrode active material may be spherical or nearly spherical in shape, or may be polyhedral or irregular in shape.
[0115] Meanwhile, the positive electrode active material may include a buffer layer on the particle surface. The buffer layer may be expressed as a coating layer, a protective layer, etc., and may play a role in lowering the interfacial resistance between the positive electrode active material and the sulfide-based solid electrolyte particles. For example, the buffer layer may include a lithium-metal-oxide, wherein the metal may be one or more elements selected from the group consisting of Al, B, Ca, Ce, Cr, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ta, V, W, and Zr. The lithium-metal-oxide is excellent in lowering the interfacial resistance between the positive electrode active material and the solid electrolyte particles while improving the performance of the positive electrode active material by facilitating the movement of lithium ions and electron conduction.
[0116] The positive electrode active material may be included in an amount of 55 wt% to 99.5 wt% based on 100 wt% of the positive electrode active material layer, for example, 65 wt% to 95 wt%, or 75 wt% to 91 wt%.
[0117] bookbinder
[0118] The binder helps the positive electrode active material particles adhere well to each other and also helps the positive electrode active material adhere well to the current collector. Representative examples of binders include, but are not limited to, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylic resin, polyester resin, nylon, etc.
[0119] Challenge
[0120] Conductive materials are used to impart conductivity to electrodes, and any material that does not cause chemical changes and is electronically conductive can be used in the battery. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials containing copper, nickel, aluminum, silver, etc. in the form of metal powder or metal fibers; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0121] The content of the binder and the conductive agent may be 0.5 wt% to 5 wt%, respectively, with respect to 100 wt% of the positive electrode active material layer.
[0122] The cathode active material layer may optionally further include a solid electrolyte. The solid electrolyte may include, for example, a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or a combination thereof, and specific descriptions thereof will be provided later in the section on solid electrolyte membranes.
[0123] For 100 wt% of the positive electrode active material layer, the solid electrolyte may be included in an amount of 0.1 wt% to 35 wt%, for example, 1 wt% to 35 wt%, 5 wt% to 30 wt%, 8 wt% to 25 wt%, or 10 wt% to 20 wt%.
[0124] In the positive electrode active material layer, the positive electrode active material may be comprised in an amount of 65 to 99 wt% and the solid electrolyte in an amount of 1 to 35 wt%, based on 100 wt% of the total of the positive electrode active material and the solid electrolyte, for example, the positive electrode active material may be comprised in an amount of 80 to 90 wt% and the solid electrolyte in an amount of 10 to 20 wt%. When the solid electrolyte is comprised in the positive electrode in such an amount, the efficiency and life characteristics of the all-solid-state secondary battery can be improved without reducing the capacity.
[0125] Al may be used as the above current collector, but is not limited thereto.
[0126] solid electrolyte membrane
[0127] The solid electrolyte membrane includes a solid electrolyte. The solid electrolyte may be a type of inorganic solid electrolyte, such as a sulfide-based solid electrolyte, an oxide-based solid electrolyte, a halide-based solid electrolyte, or a combination thereof.
[0128] Sulfide-based solid electrolyte
[0129] Sulfide-based solid electrolytes include, for example, Li2S-P2S5, Li2S-P2S5--LiX (where X is a halogen element, for example, I or Cl), Li2S-P2S5-Li2O, Li2S-P2S5-Li2O-LiI, Li2S-SiS2, Li2S-SiS2-LiI, Li2S-SiS2-LiBr, Li2S-SiS2-LiCl, Li2S-SiS2-B2S3-LiI, Li2S-SiS2-P2S5-LiI, Li2S-B2S3, Li2S-P2S5-Z. m S n (m, n are integers, Z is Ge, Zn or Ga), Li2S-GeS2, Li2S-SiS2-Li3PO4, Li2S-SiS2-Li p MO q (p, q are integers, and M is P, Si, Ge, B, Al, Ga or In), or a combination thereof.
[0130] A sulfide-based solid electrolyte can be obtained, for example, by mixing Li2S and P2S5 in a molar ratio of 50:50 to 90:10, or 50:50 to 80:20, and optionally heat-treating them. Within the above mixing ratio range, a sulfide-based solid electrolyte having excellent ionic conductivity can be produced. The ionic conductivity can be further improved by further including other components such as SiS2, GeS2, and B2S3.
[0131] Methods for mixing sulfur-containing raw materials for producing sulfide-based solid electrolytes include mechanical milling or the solution method. Mechanical milling involves placing raw materials in a ball mill reactor and vigorously stirring them to finely atomize and mix them. Using the solution method, the raw materials are mixed in a solvent to obtain a solid electrolyte as a precipitate. Furthermore, heat treatment after mixing can solidify the crystals of the solid electrolyte and improve ionic conductivity. For example, a sulfide-based solid electrolyte can be produced by mixing sulfur-containing raw materials and heat-treating them twice or more, resulting in a sulfide-based solid electrolyte with high ionic conductivity and robustness.
[0132] According to one embodiment, sulfide-based solid electrolyte particles can be manufactured through, for example, a first heat treatment in which sulfur-containing raw materials are mixed and calcined at 120°C to 350°C, and a second heat treatment in which the first heat treatment result is mixed and calcined at 350°C to 800°C. The first heat treatment and the second heat treatment can each be performed in an inert gas or nitrogen atmosphere. The first heat treatment can be performed for 1 to 10 hours, and the second heat treatment can be performed for 5 to 20 hours. The first heat treatment can have the effect of milling small raw materials, and the second heat treatment can synthesize the final solid electrolyte. Through two or more such heat treatments, a high-performance sulfide-based solid electrolyte with high ionic conductivity and robustness can be obtained, and such a solid electrolyte can be said to be suitable for mass production. The temperature of the first heat treatment may be, for example, 150°C to 330°C, or 200°C to 300°C, and the temperature of the second heat treatment may be, for example, 380°C to 700°C, or 400°C to 600°C.
[0133] For example, the sulfide-based solid electrolyte particles may include argyrodite-type sulfides. The argyrodite-type sulfide-based solid electrolyte particles may have an ionic conductivity of 10, which is the ionic conductivity of a typical liquid electrolyte at room temperature. -4 10 inland -2 It has a high ionic conductivity approaching the S / cm range, can form a close bond between a positive electrode active material and a solid electrolyte without causing a decrease in ionic conductivity, and can further form a close interface between an electrode layer and a solid electrolyte layer. An all-solid-state secondary battery including the same can have improved battery performance, such as rate characteristics, Coulombic efficiency, and cycle life characteristics.
[0134] The argyrodite-type sulfide-based solid electrolyte particles may include, for example, a compound represented by the chemical formula 21 below.
[0135] [Chemical Formula 21]
[0136] (Li a M 1 b M 2 c )(P d M 3 e )(S f M 4 g )X h
[0137] In the above chemical formula 21, 4≤a≤8, and M 1 is Mg, Cu, Ag, or a combination thereof, and 0≤b<0.5, and M 2 is Na, K, or a combination thereof, 0≤c<0.5, and M 3 is Sn, Zn, Si, Sb, Ge, or a combination thereof, and 0 <d<4, 0≤e<1 이고, M 4 is O, SO n , or a combination thereof, and 1.5≤n≤5, 3≤f≤12, 0≤g<2, and X is F, Cl, Br, I, or a combination thereof, and 0≤h≤2.
[0138] For example, in chemical formula 21, a halide element (X) may be included as an essential element, in which case 0 <h≤2로 표시될 수 있다. 일 예로 화학식 21에 M 1 Elements may be required, in which case 0 <b<0.5로 표시될 수 있다. 화학식 21에서 M 3 can be understood as an element substituted in place of P and 0 <e<1일 수 있다. 화학식 21에서 M 4 is substituted in the S position, for example, 0 <g<2일 수 있으며 S의 비율인 f는 예를 들어 3≤f≤7일 수 있다. M 4 Go SO n If SO n It can be, for example, S4O6, S3O6, S2O3, S2O4, S2O5, S2O6, S2O7, S2O8, SO4, or SO5, and can be, for example, SO4.
[0139] For example, in chemical formula 21, a+b+c+h=7, d+e=1, and f+g+h=6.
[0140] As a specific example, argyrodite-type sulfide-based solid electrolyte particles include Li3PS4 and Li7P3S. 11 , Li7PS6, Li6PS5Cl, Li6PS5Br, Li 5.8 PS 4.8 Cl 1.2 , Li 6.2 PS 5.2 Br 0.8 , Li 5.75 PS 4.75 Cl 1.25 , (Li 5.69 Cu 0.06 )PS 4.75 Cl 1.25 , (Li 5.72 Cu 0.03 )PS 4.75 Cl 1.25 , (Li 5.69 Cu 0.06 )P(S 4.70 (SO4) 0.05 )Cl 1.25 , (Li 5.69 Cu0.06 )P(S 4.60 (SO4) 0.15 )Cl 1.25 , (Li 5.72 Cu 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 , (Li 5.72 Na 0.03 )P(S 4.725 (SO4) 0.025 )Cl 1.25 , Li 5.75 P(S 4.725 (SO4) 0.025 )Cl 1.25 , or combinations thereof, but are not limited thereto.
[0141] An argyrodite-type sulfide-based solid electrolyte can be manufactured, for example, by mixing lithium sulfide and phosphorus sulfide, optionally a lithium halide. After mixing these, a heat treatment may be performed. The heat treatment may include, for example, two or more heat treatment steps. Here, manufacturing an argyrodite-type sulfide-based solid electrolyte may include, for example, a first heat treatment of mixing raw materials and calcining at 120°C to 350°C, and a second heat treatment of mixing the resultant of the first heat treatment again and calcining at 350°C to 800°C.
[0142] The average particle size (D50) of the sulfide-based solid electrolyte particles may be, for example, 0.1 ㎛ to 5.0 ㎛ or 0.1 ㎛ to 3.0 ㎛, and may be small particles of 0.1 ㎛ to 1.9 ㎛ or large particles of 2.0 ㎛ to 5.0 ㎛. The sulfide-based solid electrolyte particles may be a mixture of small particles having an average particle size of 0.1 ㎛ to 1.9 ㎛ and large particles having an average particle size of 2.0 ㎛ to 5.0 ㎛. The average particle size of the sulfide-based solid electrolyte particles may be measured from an electron microscope image, and for example, a particle size distribution may be obtained by measuring the size (diameter or major axis length) of about 20 particles in a scanning electron microscope image, and D50 may be calculated from this.
[0143] Oxide-based solid electrolyte
[0144] Oxide-based solid electrolytes include, for example, Li 1+x Ti 2-x Al(PO4)3(LTAP)(0≤x≤4), Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 (0 <x<2, 0≤y<3), BaTiO3, Pb(Zr,Ti)O3(PZT), Pb 1-x La x Zr 1-y Ti y O3(PLZT)(0≤x<1, 0≤y<1), PB(Mg3Nb 2 / 3 )O3-PbTiO3(PMN-PT), HfO2, SrTiO3, SnO2, CeO2, Na2O, MgO, NiO, CaO, BaO, ZnO, ZrO2, Y2O3, Al2O3, TiO2, SiO2, lithium phosphate (Li3PO4), lithium titanium phosphate (Li x Ti y (PO4)3, 0 <x<2, 0<y<3), Li 1+x+y (Al, Ga) x (Ti, Ge) 2-x Si y P 3-y O12 (0≤x≤1, 0≤y≤1), lithium lanthanum titanate (Li x La y TiO3, 0 <x<2, 0<y<3), Li2O, LiAlO2, Li2O-Al2O3-SiO2-P2O5-TiO2-GeO2계 세라믹스, 가넷(Garnet)계 세라믹스 Li 3+x La3M2O 12 (M= Te, Nb, or Zr; x is an integer from 1 to 10), or mixtures thereof.
[0145] Halide-based solid electrolyte
[0146] The solid electrolyte membrane may further include, for example, a halide-based solid electrolyte. The halide-based solid electrolyte contains a halogen element as a main component, and may mean that the ratio of the halide element to all elements constituting the solid electrolyte is 50 mol% or more, 70 mol% or more, 90 mol% or more, or 100 mol%. For example, the halide-based solid electrolyte may not contain a sulfur element.
[0147] The halide-based solid electrolyte may contain lithium element, a metal element other than lithium, and a halogen element. The metal element other than lithium may be Al, As, B, Bi, Ca, Cd, Co, Cr, Fe, Ga, Hf, In, Mg, Mn, Ni, Sb, Sc, Sn, Ta, Ti, Y, Zn, Zr, or a combination thereof. The halogen element may be F, Cl, Br, I, or a combination thereof, and may be Cl, Br, or a combination thereof. The halide-based solid electrolyte may contain, for example, Li aM1X6 (M is Al, As, B, Bi, Ca, Cd, Co, Cr, Fe, Ga, Hf, In, Mg, Mn, Ni, Sb, Sc, Sn, Ta, Ti, Y, Zn, Zr, or a combination thereof, X is F, Cl, Br, I, or a combination thereof, and 2≤a≤3) can be represented. The halide-based solid electrolyte is, for example, Li2ZrCl6, Li 2.7 Y 0.7 Zr 0.3 Cl6, Li 2.5 Y 0.5 Zr 0.5 Cl6, Li 2.5 In 0.5 Zr 0.5 Cl6, Li2In 0.5 Zr 0.5 Cl6, Li3YBr6, Li3YCl6, Li3YBr2Cl4, Li3YbCl6, Li 2.6 Hf 0.4 Yb 0.6 Cl6, or combinations thereof, but is not limited thereto.
[0148] bookbinder
[0149] The solid electrolyte membrane may further include a binder. Binders include, for example, nitrile-butadiene rubber, hydrogenated nitrile-butadiene rubber, styrene-butadiene rubber, acrylated styrene-butadiene rubber, acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluoroelastomer, natural rubber, polydimethylsiloxane, polyethylene oxide, polyvinylpyrrolidone, polyvinylpyridine, chlorosulfonated polyethylene, polyvinyl alcohol, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-propylene-diene copolymer, polyamideimide, polyimide, poly(meth)acrylate, polyacrylonitrile, polystyrene, polyurethane, and the like. copolymers, or combinations thereof.
[0150] The binder may be included in an amount of 0.1 wt% to 3 wt% based on 100 wt% of the solid electrolyte membrane, for example, 0.5 wt% to 2 wt%, or 0.5 wt% to 1.5 wt%. When the binder is included in the above range, the components within the solid electrolyte membrane can be well combined without lowering the ionic conductivity of the solid electrolyte, thereby improving the durability and reliability of the battery.
[0151] Other ingredients
[0152] The solid electrolyte membrane may optionally further comprise an alkali metal salt, and / or an ionic liquid, and / or a conductive polymer.
[0153] The above alkali metal salt may be, for example, a lithium salt. The content of the lithium salt in the solid electrolyte layer may be 1 M or more, for example, 1 M to 4 M. In this case, the lithium salt may improve ion conductivity by enhancing the lithium ion mobility of the solid electrolyte layer.
[0154] The lithium salt may be applied without limitation on type, and may include, for example, LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiSCN, LiN(CN)2, lithium bis(oxalato)borate (LiBOB), lithium difluoro(oxalato)borate (LiDFOB), lithium difluorobis(oxalato)phosphate (LiDFBP), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(pentafluoroethanesulfonyl)imide (LiBETI), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, or a combination thereof.
[0155] For example, the lithium salt may be an imide-based lithium salt such as LiTFSI, LiFSI, LiBETI, or a combination thereof. The imide-based lithium salt can maintain or improve ionic conductivity by appropriately maintaining chemical reactivity with the ionic liquid.
[0156] Ionic liquids are salts or molten salts that are composed only of ions and are liquid at room temperature, with a melting point below room temperature.
[0157] The ionic liquid comprises a) one or more cations selected from ammonium, pyrrolidinium, pyridinium, pyrimidinium, imidazolium, piperidinium, pyrazolium, oxazolium, pyridazinium, phosphonium, sulfonium, trizolium, and mixtures thereof, and b) BF4. - , PF6 - , AsF6 - , SbF6 - , AlCl4 - , HSO4 - , ClO4 - , CH3SO3 - , CF3CO2 - , Cl - , Br - , I - , BF4 - , SO4 - , CF3SO3 - , (FSO2)2N - , (C2F5SO2)2N - , (C2F5SO2)(CF3SO2)N - , and (CF3SO2)2N - It may be a compound containing one or more anions selected from among.
[0158] The ionic liquid may be at least one selected from the group consisting of, for example, N-methyl-N-propylpyrrolidinium bis(trifluoromethanesulfonyl)imide, N-butyl-N-methylpyrrolidinium bis(3-trifluoromethylsulfonyl)imide, 1-butyl-3-methylimidazolium bis(trifluoromethylsulfonyl)amide, and 1-ethyl-3-methylimidazolium bis(trifluoromethylsulfonyl)amide.
[0159] In the solid electrolyte layer, the weight ratio of the solid electrolyte to the ionic liquid may be 0.1:99.9 to 90:10, for example, 10:90 to 90:10, 20:80 to 90:10, 30:70 to 90:10, 40:60 to 90:10, or 50:50 to 90:10. A solid electrolyte layer satisfying the above range can maintain or improve ionic conductivity by improving the electrochemical contact area with the electrode. Accordingly, the energy density, discharge capacity, rate characteristics, etc. of the all-solid-state secondary battery can be improved.
[0160] The above-mentioned all-solid-state secondary battery may be a unit cell having a structure of positive electrode / solid electrolyte layer / negative electrode, a bi-cell having a structure of positive electrode / solid electrolyte layer / negative electrode / solid electrolyte layer / positive electrode, or a laminated battery in which the structure of the unit cell is repeated.
[0161] The shape of the above-mentioned all-solid-state secondary battery is not particularly limited, and may be, for example, coin-shaped, button-shaped, sheet-shaped, stacked, cylindrical, flat, etc. In addition, the above-mentioned all-solid-state secondary battery can be applied to large-scale batteries used in electric vehicles, etc. For example, the above-mentioned all-solid-state secondary battery can be used in hybrid vehicles such as plug-in hybrid electric vehicles (PHEVs). In addition, it can be used in fields requiring a large amount of power storage, and for example, it can be used in electric bicycles or power tools, etc. In addition, the above-mentioned all-solid-state secondary battery can be used in various fields such as portable electronic devices.
[0162] Hereinafter, examples and comparative examples of the present invention are described. The following examples are merely examples of the present invention, and the present invention is not limited to the following examples.
[0163] Examples 1 to 4 and Comparative Examples 1 to 6
[0164] 1. Manufacturing of the cathode
[0165] A mixed powder was prepared by mixing 95 wt% of carbon material having the properties shown in Table 1 below and 5 wt% of Ag having an average size of about 60 nm through dry mixing.
[0166] The manufactured Ag / C mixture, styrene butadiene rubber, and sodium carboxymethyl cellulose were mixed in a weight ratio of 100:6:3 in a water solvent to prepare a negative electrode coating layer composition. This was coated on a 10 μm thick stainless steel foil current collector and then vacuum-dried at 80°C to prepare a deposition-type negative electrode in which a negative electrode coating layer of approximately 10 μm thickness was formed on the current collector.
[0167] 2. Manufacturing of all-solid-state secondary batteries
[0168] LiNi coated with Li2O-ZrO2 0.8 Co 0.15 Mn 0.05 A positive electrode composition was prepared by mixing 85 wt% of O2 positive electrode active material, 13.5 wt% of solid electrolyte Li6PS5Cl, 1.0 wt% of polyvinylidene fluoride binder, and 0.5 wt% of carbon nanotube conductive material. The prepared positive electrode composition was coated on a positive electrode current collector using a bar coater, and dried and rolled to prepare a positive electrode.
[0169] A composition for a solid electrolyte membrane was prepared by adding 2 wt% of an acrylic copolymer binder (SX-A334, Zeon) and 98 wt% of a solid electrolyte (Li6PS5Cl, D50=3.5㎛) to an isobutyl isobutyrate (IBIB) solvent and mixing them. This was applied onto a release PET film using a blade coater, pre-dried at about 50°C, and then dried at about 70°C under vacuum conditions to prepare a solid electrolyte membrane having a thickness of about 400㎛.
[0170] A solid electrolyte film was laminated on a cathode, and an anode was laminated thereon to manufacture a unit cell. This was then placed in a laminate film and subjected to warm isostatic pressing (WIP) at 80°C and 500 MPa for 30 minutes to manufacture an all-solid-state secondary battery.
[0171] Carbon material property analysis method
[0172] In Table 1 below, the circularity of the primary particles of the carbon material was analyzed using the Image J program after photographing the carbon material with an FE-SEM. The particle size of the primary particles of the carbon material was obtained by measuring the diameters of about 20 particles randomly from the images of the carbon material taken with an FE-SEM to obtain a particle size distribution, and the diameter of the particle with a cumulative volume of 50% by volume (D) in the particle size distribution 50 ) was taken as the particle size of the primary particle.
[0173] I of carbon material D / I G It was analyzed by Raman spectroscopy, using an analytical instrument Raman 2010 Spectra (NT-MDT Development Co.) under the following conditions.
[0174] - Wavelength laser: 515 nm
[0175] - Minimum Raman shift: ~ 50 cm -1
[0176] - Spatial resolution: 500 nm
[0177] - Measurement range: 500 to 4000 cm -1
[0178] d of carbon material 002 It is analyzed by X-ray diffraction, and can be said to be a value calculated from the Bragg equation using the Bragg 2θ angle and half-width of the (002) plane peak. X-ray diffraction analysis was performed under the following conditions.
[0179] - X-ray wavelength: 1.541838 Å (CuKα)
[0180] - Slit conditions: Divergence Silt, Scattering Slit 0.5°, Receiving Slit 0.15mm
[0181] - Scan conditions: 0.02 step, 2° / min
[0182] The BET specific surface area of carbon materials was measured by the nitrogen gas adsorption method using a measuring device HM model-1208 (MOUNTECH). Approximately 0.3 g of a carbon material sample was heated in a preprocessor in a nitrogen atmosphere at 300°C for 1 hour, then preprocessed for an additional 15 minutes at 300°C in a surface area measuring device, cooled to the temperature of liquid nitrogen, and saturated with a gas containing 30% nitrogen and 70% helium. The sample was then heated to room temperature, and the amount of desorbed gas was measured. The specific surface area was calculated from the results obtained using the conventional BET method.
[0183] Evaluation Example 1: Initial Charge-Discharge Efficiency
[0184] For the batteries manufactured in Examples 1 to 4 and Comparative Examples 1 to 6, initial charge and discharge were performed by charging at a constant current of 0.1 C at 45°C to an upper limit voltage of 4.25 V, charging at a constant voltage of 0.05 C, and then discharging at 0.1 C to an end-of-discharge voltage of 2.5 V. The ratio of the initial discharge capacity to the initial charge capacity was calculated and presented as the initial charge and discharge efficiency in Table 1 below.
[0185] Evaluation Example 2: Output Characteristics
[0186] Following the initial charge / discharge of Evaluation Example 1, the second cycle involved charging at 0.1 C and discharging at 0.33 C, and the third cycle involved charging at 0.1 C and discharging at 1 C. The ratio of the discharge capacity of the third cycle to the initial discharge was calculated and shown as the output characteristics in Table 1 below.
[0187] Carbon material properties Electrochemical evaluation Circularity Primary particle size (nm) I D / I G d 002 (Å)BET(m 2 / g) Initial charge / discharge efficiency (%) Output characteristics (%) Example 10.87 352.5 3.60 559 87 56.5 Example 20.9 1 352.63.61 558 8.862 Example 30.86 452.43.58 54 585.860 Example 40.84 302.23.55 58 882.15 3.2 Comparative Example 10.9 48 1.13.55 439 8.91 0.6 (NG) Comparative Example 20.8 1 50000.33.36 72 36.4 (NG) Short (NG) Comparative Example 30.8 2 34 1.63.60 580085.74 0.6 (NG) Comparative Example 40.68 50000.13.40 7106 (NG)Short (NG)Comparative Example 50.58801.53.575786.82.5 (NG)Comparative Example 60.55251.13.4938085.140.7 (NG)
[0188] Referring to Table 1 above, it can be seen that Examples 1 to 4 have higher initial charge / discharge efficiency and superior output characteristics compared to Comparative Examples 1 to 6. The specific details will be described later.
[0189] Evaluation Example 3: Schematic diagram and cross-sectional analysis of the electrode plate according to carbon material properties
[0190] Figures 2, 4, 6, 8, and 10 are schematic diagrams of carbon materials for better understanding, where gray particles represent primary particles of carbon materials and arrows represent the migration paths of lithium ions. Figures 3, 5, 7, 9, 11, and 12 are images of cross-sections of negative electrode plates taken with an FE-SEM, and the scale bars are all 1.00 μm.
[0191] Fig. 2 is a schematic diagram of the carbon material of Example 1, and Fig. 3 is an FE-SEM image of a cross-section of the cathode coating layer of Example 1. Referring to Figs. 2 and 3 and Table 1, the carbon material in the cathode coating layer according to Example 1 has a d of 3.605. 002 It has a value of 1. The particle size of the primary particle is about 35 nm, the circularity is 0.87, and I D / I G The ratio is 2.5 and the BET surface area is 59 m 2 / g level, it can be said that it has a structure and crystallinity optimized for the movement of lithium ions.
[0192] Figure 4 is a schematic diagram of the carbon material of Comparative Example 1, and Figure 5 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 1. The carbon material of Comparative Example 1 is a type of Super P, which is commonly used as amorphous carbon. Referring to Figures 4, 5, and Table 1, the carbon material of Comparative Example 1 has an I of 1.1. D / I G It can be seen that by having a ratio, the degree of defects decreases and accordingly, the energy of lithium movement increases, which lowers the output characteristics of the battery.
[0193] Fig. 6 is a schematic diagram of the carbon material of Comparative Example 2, and Fig. 7 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 2. Referring to Figs. 6, 7, and Table 1, the carbon material of Comparative Example 2 is d 002 The crystallinity is low as the value is low at 3.367, the particle size of the primary particle is too high at 5000 nm, and I D / I G The ratio is low at 0.3, which reduces the defect rate and increases the energy of lithium movement. Accordingly, referring to Table 1, the all-solid-state secondary battery of Comparative Example 2 showed low initial charge / discharge efficiency and output characteristics.
[0194] Fig. 8 is a schematic diagram of the carbon material of Comparative Example 3, and Fig. 9 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 3. The carbon material of Comparative Example 3 is a type of Ketjen Black, which is commonly used as amorphous carbon. Referring to Figs. 8, 9, and Table 1, the carbon material of Comparative Example 3 has a BET specific surface area of 800 m 2 / g level is too high, so lithium ions cannot move smoothly, which reduces the output characteristics of the battery.
[0195] Fig. 10 is a schematic diagram of the carbon materials of Comparative Examples 4 and 5, Fig. 11 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 4, and Fig. 12 is an FE-SEM image of a cross-section of the cathode coating layer of Comparative Example 5. Referring to Figs. 10 to 12 and Table 1, the carbon material of Comparative Example 4 is a kind of plate-shaped carbon material, and the circularity is too low, and the size of the primary particles, i.e., the length of the major axis of the plate-shaped shape is high at the level of 5000 nm, and d 002 The value is low at 3.407, which means the crystallinity is low, and I D / I G The ratio is low at 0.1, which reduces the defect rate and increases the energy of lithium movement. Accordingly, the battery of Comparative Example 4 showed very low initial charge / discharge efficiency and output characteristics. The carbon material of Comparative Example 5 is a type of branched carbon material, and its circularity is very low at 0.58, which prevents smooth movement of lithium ions and reduces the output characteristics of the battery.
[0196] Although the carbon material of Comparative Example 6 is not shown in the drawing, it is a type of oval carbon material with a low circularity of 0.55, so the mobility of lithium decreases as shown in Fig. 10, and d 002 The value is low at 3.493, which means the crystallinity is low, and I D / I G Since the ratio is low at 1.1, the defect rate is low and the energy of lithium movement can be said to be high. Accordingly, Comparative Example 6 showed a decrease in the output characteristics of the battery.
[0197] Evaluation Example 4: Analysis of the battery cross-section in a charged state
[0198] After the initial charging of the all-solid-state secondary batteries of Example 1 and Comparative Examples 4 and 5, cross-sections of the batteries were photographed using FE-SEM and are shown in FIGS. 13, 14, and 15, respectively. Referring to FIG. 13, it can be confirmed that the battery of Example 1 had a lithium metal layer of about 16 μm deposited due to charging, and that a lithium metal layer with a uniform thickness and good shape was formed overall. On the other hand, it can be seen that in Comparative Example 4 of FIG. 14 and Comparative Example 5 of FIG. 15, an uneven lithium metal layer was deposited.
[0199] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts defined in the following claims also fall within the scope of the present invention.
[0200] [Explanation of symbols]
[0201] 100: All-solid-state battery 200: Cathode
[0202] 201: Cathode current collector 203: Cathode active material layer
[0203] 300: Solid electrolyte layer 400: Cathode
[0204] 401: Negative current collector 404: Lithium metal layer
[0205] 405: Cathode coating layer 500: Elastic layer
Claims
1. Negative current collector, and A negative electrode coating layer positioned on the negative electrode current collector and including a carbon material, The above carbon material was measured by X-ray diffraction method 002 A negative electrode for an all-solid-state secondary battery having a value of 3.500 or more and 3.620 or less.
2. In paragraph 1, The above carbon material was measured by X-ray spectroscopy. 002 A negative electrode for an all-solid-state secondary battery having a value of 3.555 or more and 3.610 or less.
3. In paragraph 1, An anode for an all-solid-state secondary battery, wherein the primary particle size of the above carbon material is 20 nm or more and 200 nm or less.
4. In paragraph 3, An anode for an all-solid-state secondary battery, wherein the primary particle size of the above carbon material is 20 nm or more and 70 nm or less.
5. In paragraph 1, A negative electrode for an all-solid-state secondary battery, wherein the circularity of the primary particles of the above carbon material is 0.80 or more and 1.0 or less.
6. In paragraph 5, An anode for an all-solid-state secondary battery, wherein the sphericity of the primary particles of the above carbon material is 0.84 or more and 1.0 or less.
7. In paragraph 1, The above carbon material has a ratio of D band intensity to G band intensity measured by Raman spectroscopy (I D / I G ) A negative electrode for an all-solid-state secondary battery having a value of 1.5 or more and 3.0 or less.
8. In paragraph 7, The above carbon material has a ratio of D band intensity to G band intensity measured by Raman spectroscopy (I D / I G ) A negative electrode for an all-solid-state secondary battery having a value of 2.0 or more and 3.0 or less.
9. In paragraph 1, The BET surface area of the above carbon material is 10 m 2 / g to 200 m 2 / g negative electrode for all-solid-state secondary batteries.
10. In paragraph 9, The BET surface area of the above carbon material is 40 m 2 / g to 100 m 2 / g negative electrode for all-solid-state secondary batteries.
11. In paragraph 1, The above carbon material is an all-solid-state secondary battery negative electrode having a pore size between primary particles of 10 nm or more and 1000 nm or less.
12. In paragraph 1, An anode for an all-solid-state secondary battery, wherein the carbon material comprises a sulfur element, a sulfur-containing functional group, a sulfur-containing compound, or a combination thereof located on its surface.
13. In paragraph 12, An anode for an all-solid-state secondary battery, wherein the carbon material comprises a sulfur element, a thiol group, or a combination thereof located on its surface.
14. In paragraph 1, An anode for an all-solid-state secondary battery, wherein the above cathode coating layer further comprises a lithium-philic metal.
15. In paragraph 14, The above lithium-philic metal is a negative electrode for an all-solid-state secondary battery comprising Al, Ag, Au, Bi, Cu, Ge, In, Mg, Ni, Pd, Pt, Si, Sn, Zn, or a combination thereof.
16. In paragraph 14, An anode for an all-solid-state secondary battery, wherein the content of the lithium-philic metal is 3% to 40% by weight based on 100% by weight of the total of the carbon material and the lithium-philic metal.
17. In paragraph 14, An anode for an all-solid-state secondary battery, wherein the carbon material and the lithium-philic metal are chemically bonded via sulfur.
18. In paragraph 17, An anode for an all-solid-state secondary battery, wherein the above cathode coating layer has a peak corresponding to the binding energy of a lithium-philic metal and sulfur in a spectrum measured by X-ray photoelectron spectroscopy.
19. In paragraph 17, The above lithium-philic metal includes Ag, An anode for an all-solid-state secondary battery, wherein the cathode coating layer has a peak at 160 eV to 162 eV corresponding to the Ag-S binding energy in the S2p spectrum measured by X-ray photoelectron spectroscopy.
20. In paragraph 1, A negative electrode for an all-solid-state secondary battery, wherein the thickness of the above negative electrode coating layer is 100 nm to 40 ㎛.
21. In paragraph 1, An anode for an all-solid-state secondary battery further comprising a lithium metal layer formed by charging between the anode current collector and the anode coating layer.
22. In paragraph 21, The thickness of the lithium metal layer is 5 ㎛ to 500 ㎛, A negative electrode for an all-solid-state secondary battery, wherein the deviation in the thickness of the lithium metal layer is 40% or less.
23. In paragraph 22, A negative electrode for an all-solid-state secondary battery, wherein the standard deviation of the thickness of the lithium metal layer is 0.1 ㎛ to 20 ㎛.
24. A cathode according to any one of paragraphs 1 to 23; Bipolar, and An all-solid-state secondary battery comprising a solid electrolyte membrane positioned between the cathode and the anode.
25. In paragraph 24, An all-solid-state secondary battery, wherein at least one of the positive electrode and the solid electrolyte membrane comprises a sulfide-based solid electrolyte.
26. In paragraph 25, The above sulfide-based solid electrolyte is an all-solid-state secondary battery containing an argyrodite-type sulfide.
27. In paragraph 24, The above positive electrode includes a positive electrode active material, An all-solid-state secondary battery wherein the positive electrode active material comprises lithium nickel-based oxide, lithium cobalt-based oxide, lithium iron phosphate-based compound, cobalt-free lithium nickel-manganese-based oxide, lithium-rich layered oxide, or a combination thereof.
Citation Information
Patent Citations
Negative electrode active material for lithium secondary battery and manufacture of the active material
JP2001006681A
lithium secondary battery
JP3178815B2
Lithium sulfur battery and method for manufacturaing the same
KR1020170001375A
Video Super Resolution Method
KR1020240092529A
KR20230023210A