Thermoplastic resin composition for laser direct structuring process, and article comprising same
The thermoplastic resin composition, combining polyphenylene sulfide, polyphenylene ether, glass fiber, and specific metal oxides, addresses the limitations of existing compositions by achieving superior dielectric, plating, and mechanical properties, suitable for forming high-quality metal layers and electronic circuits.
Patent Information
- Application Number
- PCT/KR2024/003105
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-03-11
- Publication Date
- 2024-10-31
AI Technical Summary
Current thermoplastic resin compositions for laser direct structuring processes face limitations in achieving excellent dielectric properties, plating properties, rigidity, and appearance characteristics, particularly when used with heterogeneous polymers like polyphenylene sulfide resin and polyphenylene ether, which often result in deteriorated mechanical properties and appearance.
A thermoplastic resin composition comprising 40-70% polyphenylene sulfide resin, 1-10% polyphenylene ether resin, 20-50% glass fiber, 0.1-5 parts by weight of styrene-based resin, and 1-10 parts by weight of additives including specific metal oxides, such as antimony tin oxide and copper chromium oxide, optimized to achieve a dielectric constant of 4.05-4.25 and dielectric loss factor of 0.0044-0.0049, with improved plating and mechanical properties.
The composition provides a molded article with excellent dielectric properties, plating properties, rigidity, and appearance characteristics, enabling efficient formation of metal layers and electrical/electronic circuits on three-dimensional shapes, while maintaining mechanical integrity and aesthetic quality.
Smart Images

Figure KR2024003105_31102024_PF_FP_ABST
Abstract
Description
Thermoplastic resin composition for laser direct structuring process and molded article comprising the same
[0001] The present invention relates to a thermoplastic resin composition for a laser direct structuring process and a molded article comprising the same. More specifically, the present invention relates to a thermoplastic resin composition for a laser direct structuring process having excellent dielectric properties, plating properties, rigidity, appearance properties, and the like, and a molded article comprising the same.
[0002]
[0003] A laser direct structuring process (LDS process) can be used to plate a metal layer on at least a portion of the surface of a molded article formed from a thermoplastic resin composition. The LDS process is a process performed prior to the plating step, in which a laser is irradiated on the target area of the molded article surface to modify the target area of the molded article surface to provide properties suitable for plating. To this end, the thermoplastic resin composition for manufacturing the molded article must contain a laser direct structuring additive (LDS additive) capable of forming metal nuclei by the laser. The additive decomposes upon exposure to the laser to generate metal nuclei. In addition, the area irradiated with the laser has a roughened surface. Due to these metal nuclei and surface roughness, the area modified by the laser becomes suitable for plating.
[0004] The laser direct structuring process allows for the rapid and economical formation of electrical and electronic circuits on the three-dimensional shape of a molded product. For example, the laser direct structuring process can be used to manufacture antennas for portable electronic devices, radio frequency identification (RFID) antennas, and repeater antennas.
[0005] However, when applying additives for laser direct structuring, the application fields are limited due to changes in dielectric properties, and when applied together with heterogeneous polymers such as polyphenylene sulfide resin and polyphenylene ether to implement rigidity and dielectric properties, there is a problem that mechanical properties such as rigidity and appearance properties deteriorate.
[0006] Therefore, there is a need to develop a thermoplastic resin composition for a laser direct structuring process and a molded product including the same, which has excellent dielectric properties such as dielectric constant and dielectric loss factor within an appropriate range, and excellent plating properties, rigidity, and appearance properties.
[0007] The background technology of the present invention is disclosed in Korean Patent Publication No. 10-2011-0018319, etc.
[0008]
[0009] The purpose of the present invention is to provide a thermoplastic resin composition for a laser direct structuring process having excellent dielectric properties, plating properties, rigidity, appearance properties, etc.
[0010] Another object of the present invention is to provide a molded article formed from the thermoplastic resin composition for the laser direct structuring process.
[0011] The above and other objects of the present invention can all be achieved by the present invention described below.
[0012]
[0013] 1. One aspect of the present invention relates to a thermoplastic resin composition for a laser direct structuring process. The thermoplastic resin composition for a laser direct structuring process comprises: about 100 parts by weight of a base material including about 40 to about 70 wt% of a polyphenylene sulfide resin, about 1 to about 10 wt% of a polyphenylene ether resin, and about 20 to about 50 wt% of glass fiber; about 0.1 to about 5 parts by weight of a styrene-based resin including at least one of a styrene homopolymer and a styrene and olefin copolymer; And about 1 to about 10 parts by weight of an additive for laser direct structuring comprising a first metal oxide and a second metal oxide; wherein the first metal oxide comprises at least one of antimony tin oxide, indium tin oxide, titanium oxide, and bismuth oxide, and the second metal oxide comprises at least one of copper chromium oxide, zinc-containing metal oxide, magnesium-containing metal oxide, aluminum-containing metal oxide, gold oxide, and silver oxide, and the weight ratio of the first metal oxide and the second metal oxide is about 1:0.005 to about 1:0.15.
[0014] 2. In the above 1 specific example, the polyphenylene sulfide resin may include a repeating unit represented by the following chemical formula 1:
[0015] [Chemical Formula 1]
[0016]
[0017] In the above chemical formula 1, R1, R2, R3 and R4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms.
[0018] 3. In the above 1 or 2 specific examples, the polyphenylene ether resin may include a repeating unit represented by the following chemical formula 2:
[0019] [Chemical Formula 2]
[0020]
[0021] In the above chemical formula 2, R1, R2, R3 and R4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms.
[0022] 4. In the above 1 to 3 specific examples, the styrene and olefin copolymer may include at least one of a styrene-ethylene-butylene-styrene block copolymer, a styrene-butadiene copolymer, a styrene-butadiene block copolymer, a styrene-isoprene block copolymer, a styrene-butadiene-styrene block copolymer, a styrene-isoprene-styrene block copolymer, a styrene-ethylene-propylene block copolymer, a styrene-ethylene-propylene-styrene block copolymer, and a styrene-ethylene-ethylene-propylene-styrene block copolymer.
[0023] 5. In the above 1 to 4 specific examples, the thermoplastic resin composition for the laser direct structuring process may have a dielectric constant (Dk) of about 4.05 to about 4.25 of a 2.5 mm × 50 mm × 90 mm sized specimen measured at 3.1 GHz using the SPDR (split post dielectric resonator) method.
[0024] 6. In the above 1 to 5 specific examples, the thermoplastic resin composition for the laser direct structuring process may have a dielectric loss factor (Df) of about 0.0044 to about 0.0049 of a 2.5 mm × 50 mm × 90 mm sized specimen measured at 3.1 GHz using the SPDR (split post dielectric resonator) method.
[0025] 7. In the above 1 to 6 specific examples, the thermoplastic resin composition for the laser direct structuring process may be such that when the surface of a 2.5 mm × 50 mm × 90 mm injection-molded specimen is activated in a stripe shape through a laser direct structuring process, a copper layer is formed on the activated surface through a plating process (copper electroless plating), and then a plating layer is formed on the surface of the specimen through a copper and nickel electroplating method, a plating layer may be formed on the entire surface of the specimen.
[0026] 8. In the above 1 to 7 specific examples, the thermoplastic resin composition for the laser direct structuring process has a flexural modulus of about 120,000 to about 150,000 kgf / cm for a 6.4 mm thick specimen measured according to ASTM D790. 2 It could be.
[0027] 9. In the above 1 to 8 specific examples, the thermoplastic resin composition for the laser direct structuring process may be such that, when a 2 mm thick specimen is injection-molded in a pin point gate mold, no discoloration occurs in the gate area and surface of the specimen.
[0028] 10. Another aspect of the present invention relates to a molded article. The molded article is characterized in that it is formed from a thermoplastic resin composition according to any one of 1 to 9.
[0029] 11. In the above 10 specific examples, the molded product may include a metal layer formed by a laser direct structuring process and a plating process on at least a portion of the surface.
[0030]
[0031] The present invention has the effect of providing a thermoplastic resin composition for a laser direct structuring process having excellent dielectric properties, plating properties, rigidity, appearance properties, etc., and a molded article formed therefrom.
[0032]
[0033] Figure 1 schematically illustrates a molded product according to one specific example of the present invention.
[0034]
[0035] Hereinafter, the present invention will be described in detail as follows.
[0036] A thermoplastic resin composition according to the present invention is usable in a laser direct structuring process (LDS process), and comprises (A) a polyphenylene sulfide resin; (B) a polyphenylene ether resin; (C) glass fiber; (D) a styrene-based resin; and (E) an additive for laser direct structuring.
[0037] In this specification, “a to b” indicating a numerical range is defined as “≥a and ≤b”.
[0038]
[0039] (A) Polyphenylene sulfide resin
[0040] According to one specific example of the present invention, a polyphenylene sulfide resin can be applied together with a polyphenylene ether resin, glass fiber, a styrene resin, and a specific additive for laser direct structuring to improve the dielectric properties, plating properties, rigidity, appearance properties, etc. of a thermoplastic resin composition. A polyphenylene sulfide resin used in a typical thermoplastic resin composition can be used. For example, a polyphenylene ether resin including a repeating unit represented by the following chemical formula 1 can be used.
[0041] [Chemical Formula 1]
[0042]
[0043] In the above chemical formula 1, R1, R2, R3 and R4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms.
[0044] In a specific example, the polyphenylene sulfide resin includes poly(1,4-phenylene)sulfide, poly(2,6-dimethyl-1,4-phenylene)sulfide, poly(2,6-diethyl-1,4-phenylene)sulfide, poly(2,6-dipropyl-1,4-phenylene)sulfide, poly(2-methyl-6-ethyl-1,4-phenylene)sulfide, poly(2-methyl-6-propyl-1,4-phenylene)sulfide, poly(2-ethyl-6-propyl-1,4-phenylene)sulfide, poly(2,6-diphenyl-1,4-phenylene)sulfide, a copolymer of poly(2,6-dimethyl-1,4-phenylene)sulfide and poly(2,3,6-trimethyl-1,4-phenylene)sulfide, and poly(2,6-dimethyl-1,4-phenylene)sulfide. Examples include copolymers of poly(2,3,5-triethyl-1,4-phenylene)sulfide, and combinations thereof.
[0045] In a specific example, the polyphenylene sulfide resin may have a melt flow index of about 200 to about 1,000 g / 10 min, for example, about 300 to about 900 g / 10 min, measured under conditions of 316°C and a 5 kg load according to ASTM D1238. Within this range, the thermoplastic resin composition may have excellent rigidity, appearance properties, etc.
[0046] In a specific example, the polyphenylene sulfide resin may be included in an amount of about 40 to about 70 wt%, for example, about 50 to about 60 wt%, of 100 wt% of the base material including the polyphenylene sulfide resin, the polyphenylene ether resin, and the glass fiber. When the content of the polyphenylene sulfide resin is less than about 40 wt%, of 100 wt% of the base material, there is a concern that the dielectric properties, rigidity, appearance properties, etc. of the thermoplastic resin composition may be deteriorated, and when it exceeds about 70 wt%, there is a concern that the dielectric properties, rigidity, etc. of the thermoplastic resin composition may be deteriorated.
[0047]
[0048] (B) Polyphenylene ether resin
[0049] A polyphenylene ether resin according to one specific example of the present invention can be applied together with a polyphenylene sulfide resin, glass fiber, a styrene resin, and a specific additive for laser direct structuring to improve the dielectric properties, plating properties, appearance properties, etc. of a thermoplastic resin composition. A polyphenylene ether resin used in a typical thermoplastic resin composition can be used. For example, a polyphenylene ether resin including a repeating unit represented by the following chemical formula 2 can be used.
[0050] [Chemical Formula 2]
[0051]
[0052] In the above chemical formula 2, R1, R2, R3 and R4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms.
[0053] In a specific example, the polyphenylene ether resin is a copolymer of poly(1,4-phenylene) ether, poly(2,6-dimethyl-1,4-phenylene) ether, poly(2,6-diethyl-1,4-phenylene) ether, poly(2,6-dipropyl-1,4-phenylene) ether, poly(2-methyl-6-ethyl-1,4-phenylene) ether, poly(2-methyl-6-propyl-1,4-phenylene) ether, poly(2-ethyl-6-propyl-1,4-phenylene) ether, poly(2,6-diphenyl-1,4-phenylene) ether, poly(2,6-dimethyl-1,4-phenylene) ether and poly(2,3,6-trimethyl-1,4-phenylene) ether, poly(2,6-dimethyl-1,4-phenylene) ether and Examples include copolymers of poly(2,3,5-triethyl-1,4-phenylene) ether, and combinations thereof.
[0054] In a specific example, the polyphenylene ether resin may have a weight average molecular weight measured by GPC (gel permeation chromatography) of about 1,000 to about 40,000 g / mol, for example, about 2,000 to about 30,000 g / mol. Within this range, the dielectric properties, appearance properties, etc. of the thermoplastic resin composition may be excellent.
[0055] In a specific example, the polyphenylene ether resin may be included in an amount of about 1 to about 10 wt%, for example, about 3 to about 8 wt%, based on 100 wt% of the base material including the polyphenylene sulfide resin, the polyphenylene ether resin, and the glass fiber. When the content of the polyphenylene ether resin is less than about 1 wt%, based on 100 wt% of the base material, there is a concern that the dielectric properties of the thermoplastic resin composition may deteriorate, and when it exceeds about 10 wt%, there is a concern that the dielectric properties, rigidity, appearance properties, etc. of the thermoplastic resin composition may deteriorate.
[0056]
[0057] (C) Glass fiber
[0058] According to one specific example of the present invention, glass fibers can be applied together with polyphenylene sulfide resin, polyphenylene ether resin, styrene resin and a specific additive for laser direct structuring to improve dielectric properties, plating properties, rigidity, appearance properties, etc. of a thermoplastic resin composition, and glass fibers used in conventional thermoplastic resin compositions can be used.
[0059] In specific embodiments, the glass fibers may be in the form of fibers and may have various cross-sections such as circular, oval, rectangular, etc. For example, it may be preferable in terms of mechanical properties to use fibrous glass fibers having circular and / or rectangular cross-sections.
[0060] In a specific example, the glass fibers having a circular cross-section may have a cross-sectional diameter of about 5 to about 20 μm and a length before processing of about 2 to about 20 mm, and the glass fibers having a rectangular cross-section may have a cross-sectional aspect ratio (cross-sectional major diameter / cross-sectional minor diameter) of about 1.5 to about 10, a minor diameter of about 2 to about 10 μm, and a length before processing of about 2 to about 20 mm. In the above ranges, the rigidity, processability, etc. of the thermoplastic resin composition may be improved.
[0061] In a specific example, the glass fiber may be treated with a conventional surface treatment agent. The surface treatment agent may include, but is not limited to, a silane compound, a urethane compound, an epoxy compound, or the like.
[0062] In a specific example, the glass fiber may be included in an amount of about 20 to about 50 wt%, for example, about 30 to about 45 wt%, of 100 wt% of the base material including the polyphenylene sulfide resin, the polyphenylene ether resin, and the glass fiber. If the content of the glass fiber is less than about 20 wt%, of 100 wt% of the base material, there is a concern that the dielectric properties, rigidity, etc. of the thermoplastic resin composition may be deteriorated, and if it exceeds about 50 wt%, there is a concern that the dielectric properties, appearance properties, etc. of the thermoplastic resin composition may be deteriorated.
[0063]
[0064] (D) Styrene resin
[0065] A styrenic resin according to one specific example of the present invention can be applied together with a polyphenylene sulfide resin, a polyphenylene ether resin, glass fiber, and a specific additive for laser direct structuring to improve the dielectric properties, plating properties, rigidity, appearance properties, etc. of a thermoplastic resin composition, and a styrene homopolymer and / or a styrene and olefin copolymer can be used.
[0066] In specific examples, the styrene and olefin copolymer may include a styrene-ethylene-butylene-styrene block copolymer, a styrene-butadiene copolymer, a styrene-butadiene block copolymer, a styrene-isoprene block copolymer, a styrene-butadiene-styrene block copolymer, a styrene-isoprene-styrene block copolymer, a styrene-ethylene-propylene block copolymer, a styrene-ethylene-propylene-styrene block copolymer, and a styrene-ethylene-ethylene-propylene-styrene block copolymer (SEEPS), combinations thereof, and the like. For example, a styrene-ethylene-butylene-styrene block copolymer (SEBS) may be used.
[0067] In a specific example, the styrene resin may have a melt flow index of about 1 to about 30 g / 10 min, for example, about 2 to about 20 g / 10 min, measured under conditions of 200° C. and a load of 5 kg according to ASTM D1238, and may have a styrene content of about 10 to about 100%, for example, about 15 to about 100%. Within this range, the appearance properties, dielectric properties, etc. of the thermoplastic resin composition may be excellent.
[0068] In a specific example, the styrene resin may be included in an amount of about 0.1 to about 5 parts by weight, for example, about 2 to about 4 parts by weight, based on about 100 parts by weight of the base material. If the content of the styrene resin is less than about 0.1 parts by weight based on about 100 parts by weight of the base material, there is a concern that the appearance properties of the thermoplastic resin composition may deteriorate, and if it exceeds about 5 parts by weight, there is a concern that the rigidity of the thermoplastic resin composition may deteriorate.
[0069]
[0070] (E) Additives for laser direct structuring
[0071] An additive for laser direct structuring (LDS) according to one specific example of the present invention is capable of forming a metal nucleus by a laser, and is applied together with a polyphenylene sulfide resin, a polyphenylene ether resin, glass fiber, and a styrene-based resin to improve dielectric properties, plating properties, rigidity, appearance properties, etc. of a thermoplastic resin composition, and includes a first metal oxide and a second metal oxide. Here, the laser refers to light amplified by stimulated emission (stimulated emission light), and the laser may be ultraviolet light having a wavelength of about 100 to about 400 nm, visible light having a wavelength of about 400 to about 800 nm, or infrared light having a wavelength of about 800 to about 25,000 nm, for example, infrared light having a wavelength of about 1,000 to about 2,000 nm.
[0072] In specific examples, the first metal oxide may include antimony tin oxide, indium tin oxide, titanium oxide, bismuth oxide, combinations thereof, and the like.
[0073] In specific examples, the second metal oxide may include copper chromium oxide, zinc-containing metal oxide, magnesium-containing metal oxide, aluminum-containing metal oxide, gold oxide, silver oxide, combinations thereof, and the like.
[0074] In a specific example, the additive for laser direct structuring may have an average particle diameter of about 0.01 to about 50 μm, for example, about 0.1 to about 30 μm, specifically about 0.5 to about 10 μm. Within this range, a uniform plating surface can be formed during plating via laser direct structuring. In the present invention, unless otherwise specified, the average particle diameter is a number average diameter, and means the diameter measured by D50 (the particle diameter at the point where the distribution ratio is 50%).
[0075] In a specific example, the additive for laser direct structuring may be included in an amount of about 1 to about 10 parts by weight, for example, about 3 to about 7 parts by weight, relative to about 100 parts by weight of the base material. If the content of the additive for laser direct structuring is less than about 1 part by weight relative to about 100 parts by weight of the base material, there is a concern that the dielectric properties, plating properties, etc. of the thermoplastic resin composition may deteriorate, and if it exceeds about 10 parts by weight, there is a concern that the dielectric properties, etc. of the thermoplastic resin composition may deteriorate.
[0076] In a specific example, the weight ratio of the first metal oxide and the second metal oxide may be about 1:0.005 to about 1:0.15, for example, about 1:0.01 to about 1:0.1. When the weight ratio of the first metal oxide and the second metal oxide is less than about 1:0.005, there is a concern that the dielectric properties, plating properties, appearance properties, etc. of the thermoplastic resin composition may deteriorate, and when it exceeds about 1:0.15, there is a concern that the dielectric properties, etc. of the thermoplastic resin composition may deteriorate.
[0077]
[0078] A thermoplastic resin composition for a laser direct structuring process according to one embodiment of the present invention may further include additives included in conventional thermoplastic resin compositions. Examples of the additives include, but are not limited to, inorganic fillers, flame retardants, anti-drip agents, lubricants, nucleating agents, stabilizers, release agents, pigments, dyes, and mixtures thereof. When the additives are used, the content thereof may be about 0.001 to about 40 parts by weight, for example, about 0.1 to about 10 parts by weight, based on about 100 parts by weight of the base material.
[0079]
[0080] A thermoplastic resin composition for a laser direct structuring process according to one specific example of the present invention may be in the form of pellets obtained by mixing the above components and melt-extruding them at about 230 to about 370°C, for example, about 250 to about 350°C, using a conventional twin-screw extruder.
[0081] In a specific example, the thermoplastic resin composition for the laser direct structuring process may have a dielectric constant (Dk) of about 4.05 to about 4.25, for example, about 4.06 to about 4.20, of a 2.5 mm × 50 mm × 90 mm sized specimen measured at 3.1 GHz using a split post dielectric resonator (SPDR) method.
[0082] In a specific example, the thermoplastic resin composition for the laser direct structuring process may have a dielectric loss factor (Df) of about 0.0044 to about 0.0049, for example, about 0.0045 to about 0.0048, of a 2.5 mm × 50 mm × 90 mm sized specimen measured at 3.1 GHz using a split post dielectric resonator (SPDR) method.
[0083] In a specific example, the thermoplastic resin composition for the laser direct structuring process may be such that when the surface of a 2.5 mm × 50 mm × 90 mm injection molded specimen is activated in a stripe shape through a laser direct structuring process, a copper layer is formed on the activated surface through a plating process (copper electroless plating), and then a plating layer is formed on the surface of the specimen through a copper and nickel electroplating method, a plating layer may be formed on the entire surface of the specimen.
[0084] In a specific example, the thermoplastic resin composition for the laser direct structuring process has a flexural modulus of about 120,000 to about 150,000 kgf / cm for a 6.4 mm thick specimen measured according to ASTM D790. 2, for example, about 125,000 to about 140,000 kgf / cm 2 It could be.
[0085] In a specific example, the thermoplastic resin composition for the laser direct structuring process may be such that, when a 2 mm thick specimen is injection-molded in a pin point gate mold, no discoloration occurs at the gate area and surface of the specimen.
[0086]
[0087] The molded article according to the present invention is formed from the thermoplastic resin composition for the laser direct structuring process. For example, the molded article can be manufactured using the thermoplastic resin composition using a molding method such as injection molding, compression molding, blow molding, or extrusion molding. The molded article can be easily formed by a person skilled in the art to which the present invention pertains.
[0088] FIG. 1 schematically illustrates a molded article according to one embodiment of the present invention. The sizes of the components constituting the invention in the drawing are exaggerated for the sake of clarity of the specification and are not limited thereto. As illustrated in FIG. 1, a molded article (10) according to one embodiment of the present invention may include a metal layer (20) formed on at least a portion of the surface of the molded article (10) by a laser direct structuring process and a plating process. The molded article (10) according to one embodiment of the present invention may be a circuit carrier used for manufacturing an antenna, and the molded article (10) may be manufactured by, for example, manufacturing the molded article (10) by a method such as injection molding using the thermoplastic resin composition; irradiating a laser to a specific area (metal layer (20) portion) of the surface of the molded article (10); and metallizing (plating) the irradiated area to form the metal layer (20).
[0089] In a specific example, the laser direct structuring additive included in the molded product (10) is decomposed by the laser irradiation, thereby generating metal nuclei. In addition, the area irradiated with the laser has a surface roughness suitable for plating. The wavelength of the laser may be 248 nm, 308 nm, 355 nm, 532 nm, 1,064 nm, or 10,600 nm.
[0090] In a specific embodiment, the metallization process may be performed through a conventional plating process. For example, a metal layer (20) (electrically conductive path) may be formed on the laser-irradiated area of the surface of the molded product (10) by immersing the laser-irradiated molded product (10) in one or more electroless plating baths. Non-limiting examples of the plating process include copper plating, gold plating, nickel plating, silver plating, zinc plating, and tin plating.
[0091] In this way, a molded product having a metal layer formed on at least a portion of the surface by a laser direct structuring process can be easily formed by a person having ordinary skill in the art to which the present invention pertains.
[0092]
[0093] Hereinafter, the present invention will be described in more detail through examples; however, these examples are for the purpose of explanation only and should not be construed as limiting the present invention.
[0094]
[0095] Example
[0096] Below, the specifications of each component used in the examples and comparative examples are as follows.
[0097] (A) Polyphenylene sulfide resin
[0098] Poly(1,4-phenylene)sulfide (Manufacturer: HDC POLYALL, Product name: ECOTRAN J200) was used.
[0099] (B) Polyphenylene ether resin
[0100] Poly(1,4-phenylene) ether (Manufacturer: Bluestar, Product name: LXR-035C) was used.
[0101] (C) Glass fiber
[0102] Glass fiber (Manufacturer: Nittobo, Product name: CSG 3PA-832) was used.
[0103] (D) Styrene resin
[0104] (D1) Styrene homopolymer (polystyrene resin, manufacturer: Formosa, product name: TAIRIREX GP-5000) was used.
[0105] (D2) Styrene-ethylene-butylene-styrene block copolymer (SEBS, manufacturer: Shell, product name: KRATON G1651) was used.
[0106] (E) Additives for laser direct structuring
[0107] (E1) As the first metal oxide, a mixture of titanium dioxide and antimony tin oxide (manufacturer: Merck, product name: Iriotec 8850) was used.
[0108] (E2) Copper chromite (manufacturer: Shepherd, product name: Black 1G) was used as the second metal oxide.
[0109] (E3) Antimony tin oxide (manufacturer: K&W, product name: Stanostat CP05) was used as the first metal oxide.
[0110] (E4) Copper phosphate (manufacturer: OMEGA, product name: MEGA-CHP200) was used.
[0111]
[0112] Examples 1 to 5 and Comparative Examples 1 to 11
[0113] Each of the above components was added in the amounts shown in Tables 1, 2, and 3 below, and then extruded at 300°C to produce pellets. The extrusion was performed using a twin-screw extruder with an L / D of 36 and a diameter of 45 mm. The manufactured pellets were dried at about 100°C for about 4 hours or more, and then injected using a 10 Oz injection molding machine (molding temperature: about 32°C, mold temperature: about 12°C) to produce specimens. The physical properties of the manufactured specimens were evaluated using the following methods, and the results are shown in Tables 1, 2, and 3 below.
[0114]
[0115] Method of measuring physical properties
[0116] (1) Permittivity: Using the SPDR (split post dielectric resonator) method (using DAK3.5-TL-P (200 MHz - 20 GHz) equipment and DAK1.2E-PL probe), the permittivity (Dk) of a specimen measuring 2.5 mm × 50 mm × 90 mm was measured at 3.1 GHz.
[0117] (2) Dielectric loss factor: Using the SPDR (split post dielectric resonator) method (using DAK3.5-TL-P (200 MHz - 20 GHz) equipment and DAK1.2E-PL probe), the dielectric loss factor (Df) of a specimen measuring 2.5 mm × 50 mm × 90 mm was measured at 3.1 GHz.
[0118] (3) Plating property evaluation: The surface of an injection-molded specimen measuring 2.5 mm × 50 mm × 90 mm was activated in a stripe shape through a laser direct structuring process under various conditions, a copper layer was formed on the activated surface through a plating process (copper electroless plating), and then a plating layer (copper and nickel plating layer) was formed on the surface of the specimen through a known copper and nickel electroplating method, thereby manufacturing a specimen with a plating layer formed thereon. After completion of manufacturing, the plating property of the specimen with the plating layer formed thereon was evaluated using an optical microscope according to the following criteria.
[0119] (○: Plating layer formed on 100% of the specimen surface, △: Plating layer formed on 50% or more but less than 100% of the specimen surface, ×: Plating layer formed on less than 50% of the specimen surface)
[0120] (4) Stiffness evaluation: Flexural modulus of 6.4 mm thick specimen according to ASTM D790 (unit: kgf / cm 2 ) was measured.
[0121] (5) Appearance evaluation: After injection molding a 2 mm thick specimen in a pin point gate mold, the gate area of the specimen and the presence of discoloration on the specimen surface were visually checked.
[0122] (○: No occurrence of color difference, ×: Occurrence of color difference)
[0123]
[0124] Example 12345(A) (% by weight)55.555.55755.555.5(B) (% by weight)4.54.534.54.5(C) (% by weight)4040404040(D1) (parts by weight)333-3(D2) (parts by weight)---3-(E1) (parts by weight)5355-(E2) (parts by weight)0.10.10.10.10.10.1(E3) (parts by weight)----5(E4) (parts by weight)-----Dielectric constant4.104.084.154.064.10Dielectric loss factor0.00450.00450.00460.00450.0045Plating property○○○○○Flexural modulus (kgf / cm) 2)130,000128,000132,000125,000130,000Appearance Evaluation○○○○○
[0125] * Weight parts: Weight parts per 100 weight parts of basic materials (A+B+C)
[0126]
[0127] Comparative Example 123456(A) (Wt%)3559.58040.555.555.5(B) (Wt%)250.554.54.54.5(C) (Wt%)404015554040(D1) (Wt%)33330.056(D2) (Wt%)------(E1) (Wt%)555555(E2) (Wt%)0.10.10.10.10.10.10.1(E3) (Wt)------(E4) (Wt)------Dielectric Constant4.004.303.524.504.134.06Dielectric Loss rate 0.00430.00490.00330.00520.00460.0044 Plating property ○○○○○○ Flexural modulus (kgf / cm) 2 )118,000141,00057,000156,000138,000119,000Appearance Evaluation×○○××○
[0128] * Weight parts: Weight parts per 100 weight parts of basic materials (A+B+C)
[0129]
[0130] Comparative Example 7891011(A) (Wt%)55.555.555.555.555.555.5(B) (Wt%)4.54.54.54.54.54.5(C) (Wt%)4040404040(D1) (Wt%)33333(D2) (Wt%)-----(E1) (Wt%)0.510-55(E2) (Wt%)0.120.10.0051(E3) (Wt)-----(E4) (Wt)--5--Dielectric Constant4.014.284.054.144.12Dielectric Loss Factor0.00430.00470.00430.00430.0050Plating Properties×○×△○Flexural Modulus (kgf / cm) 2 )126,000131,000125,000131,000134,000Appearance Evaluation○○○×○
[0131] * Weight parts: Weight parts per 100 weight parts of basic materials (A+B+C)
[0132]
[0133] From the above results, it can be seen that the thermoplastic resin composition for the laser direct structuring process of the present invention is excellent in dielectric properties (dielectric constant and dielectric loss factor), plating properties, rigidity (flexural modulus), appearance properties, etc.
[0134] On the other hand, in the case of Comparative Example 1 where a small amount of polyphenylene sulfide resin was applied and an excessive amount of polyphenylene ether resin was applied, it can be seen that dielectric properties, rigidity, and appearance properties were deteriorated. In the case of Comparative Example 2 where a small amount of polyphenylene ether resin was applied, it can be seen that dielectric properties were deteriorated. In the case of Comparative Example 3 where an excessive amount of polyphenylene sulfide resin was applied and a small amount of glass fiber was applied, it can be seen that dielectric properties, rigidity, and the like were deteriorated. In the case of Comparative Example 4 where an excessive amount of glass fiber was applied, it can be seen that dielectric properties, appearance properties, and the like were deteriorated. In the case of Comparative Example 5 where a small amount of styrene resin was applied, it can be seen that appearance properties were deteriorated. In the case of Comparative Example 6 where an excessive amount of styrene resin was applied, it can be seen that rigidity, and the like were deteriorated. In the case of Comparative Example 7, where a small amount of the additive for laser direct structuring was applied, it can be seen that the dielectric properties, plating properties, etc. were deteriorated. In the case of Comparative Example 8, where an excessive amount of the additive for laser direct structuring was applied, it can be seen that the dielectric properties, etc. were deteriorated. In the case of Comparative Example 9, where copper phosphate (E4) was applied instead of the first metal oxide of the present invention, it can be seen that the dielectric properties, plating properties, etc. were deteriorated. In addition, even if the contents of the first metal oxide and the second metal oxide are within the scope of the present invention, when their weight ratio is less than the scope of the present invention (1:0.001) (Comparative Example 10), it can be seen that the dielectric properties, plating properties, appearance properties, etc. were deteriorated. When the content exceeds the scope of the present invention (1:0.2) (Comparative Example 11), it can be seen that the dielectric properties, etc. were deteriorated.
[0135]
[0136] The present invention has been described with reference to exemplary embodiments. Those skilled in the art will appreciate that the present invention can be implemented in modified forms without departing from its essential characteristics. Therefore, the disclosed embodiments should be considered illustrative rather than limiting. The scope of the present invention is set forth in the claims, not the foregoing description, and all differences within the scope equivalent thereto should be construed as being encompassed by the present invention.
Claims
1. About 100 parts by weight of a base material comprising about 40 to about 70 wt% of polyphenylene sulfide resin, about 1 to about 10 wt% of polyphenylene ether resin, and about 20 to about 50 wt% of glass fiber; About 0.1 to about 5 parts by weight of a styrene-based resin comprising at least one of a styrene homopolymer and a styrene and olefin copolymer; and A laser direct structuring additive comprising about 1 to about 10 parts by weight of a first metal oxide and a second metal oxide; The above first metal oxide includes at least one of antimony tin oxide, indium tin oxide, titanium oxide, and bismuth oxide, The second metal oxide includes at least one of copper chromium oxide, zinc-containing metal oxide, magnesium-containing metal oxide, aluminum-containing metal oxide, gold oxide, and silver oxide. A thermoplastic resin composition for a laser direct structuring process, characterized in that the weight ratio of the first metal oxide and the second metal oxide is about 1:0.005 to about 1:0.
15.
2. A thermoplastic resin composition for a laser direct structuring process, characterized in that in the first paragraph, the polyphenylene sulfide resin comprises a repeating unit represented by the following chemical formula 1: [Chemical Formula 1] In the above chemical formula 1, R1, R2, R3 and R4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms.
3. A thermoplastic resin composition for a laser direct structuring process, characterized in that the polyphenylene ether resin according to claim 1 or 2 includes a repeating unit represented by the following chemical formula 2: [Chemical Formula 2] In the above chemical formula 2, R1, R2, R3 and R4 are each independently a hydrogen atom, a halogen atom, an alkyl group having 1 to 6 carbon atoms or an aryl group having 6 to 12 carbon atoms.
4. A thermoplastic resin composition for a laser direct structuring process according to any one of claims 1 to 3, wherein the styrene and olefin copolymer comprises at least one of a styrene-ethylene-butylene-styrene block copolymer, a styrene-butadiene copolymer, a styrene-butadiene block copolymer, a styrene-isoprene block copolymer, a styrene-butadiene-styrene block copolymer, a styrene-isoprene-styrene block copolymer, a styrene-ethylene-propylene block copolymer, a styrene-ethylene-propylene-styrene block copolymer, and a styrene-ethylene-ethylene-propylene-styrene block copolymer.
5. A thermoplastic resin composition for a laser direct structuring process according to any one of claims 1 to 4, characterized in that the thermoplastic resin composition for a laser direct structuring process has a dielectric constant (Dk) of about 4.05 to about 4.25 of a 2.5 mm × 50 mm × 90 mm sized specimen measured at 3.1 GHz using a split post dielectric resonator (SPDR) method.
6. A thermoplastic resin composition for a laser direct structuring process according to any one of claims 1 to 5, characterized in that the thermoplastic resin composition for a laser direct structuring process has a dielectric loss factor (Df) of about 0.0044 to about 0.0049 of a 2.5 mm × 50 mm × 90 mm sized specimen measured at 3.1 GHz using a split post dielectric resonator (SPDR) method.
7. A thermoplastic resin composition for a laser direct structuring process according to any one of claims 1 to 6, wherein the thermoplastic resin composition for a laser direct structuring process is characterized in that when a surface of a 2.5 mm × 50 mm × 90 mm injection-molded specimen is activated in a stripe shape through a laser direct structuring process, a copper layer is formed on the activated surface through a plating process (copper electroless plating), and then a plating layer is formed on the surface of the specimen through a copper and nickel electroplating method, a plating layer is formed on the entire surface of the specimen.
8. In any one of claims 1 to 7, the thermoplastic resin composition for the laser direct structuring process has a flexural modulus of about 120,000 to about 150,000 kgf / cm for a 6.4 mm thick specimen measured according to ASTM D790. 2 A thermoplastic resin composition for a laser direct structuring process, characterized by:
9. A thermoplastic resin composition for a laser direct structuring process according to any one of claims 1 to 8, characterized in that when a 2 mm thick specimen is injection-molded in a pin-point gate mold, no discoloration occurs in the gate area and surface of the specimen.
10. A molded product characterized by being formed from a thermoplastic resin composition for a laser direct structuring process according to any one of claims 1 to 9.
11. A molded product according to claim 10, characterized in that the molded product includes a metal layer formed by a laser direct structuring process and a plating process on at least a portion of the surface.
Citation Information
Patent Citations
Thermoplastic resin composition for LDS antenna
KR101919279B1
Resin composition, resin molded article, and method for producing resin molded article
KR1020150143870A
Laser direct structured materials and their methods of making
KR1020170106296A
Methdo of forming multi-layer curcuit using lds - lds painting repeat process
KR1020170129331A
Polyphenylene sulfide compositions for laser direct structuring processes and the shaped articles therefore
WO2022137163A1