Extrusion molded catalyst for ortho-alkylation reaction and preparation method thereof

The ortho-alkylation reaction extrusion catalyst with a bimodal pore structure and specific surface area addresses the challenges of material diffusion and activity loss, achieving high selectivity and conversion rates in ortho-alkylation reactions, and reducing costs by maintaining uniform catalytic activity and eliminating the need for additional cocatalysts.

WO2024225671A1PCT designated stage expired Publication Date: 2024-10-31HANWHA SOLUTIONS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/004910
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing ortho-alkylation catalysts face challenges in achieving high selectivity and conversion rates due to material diffusion resistance and decreased activity during the extrusion molding process, which affects the production yield and economic efficiency.

Method used

An ortho-alkylation reaction extrusion catalyst is developed with a bimodal pore structure and specific BET surface area, comprising magnesium oxide, macropores, and mesopores, which minimizes material diffusion resistance and maintains uniform catalytic activity, eliminating the need for additional cocatalysts or adjusting reaction conditions.

Benefits of technology

The catalyst achieves high catalytic activity and selectivity, ensuring excellent conversion rates and yield in ortho-alkylation reactions, while reducing manufacturing costs and maintaining activity uniformity within the molded catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024004910_31102024_PF_FP_ABST
    Figure KR2024004910_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to an extrusion molded catalyst for an ortho-alkylation reaction and a preparation method thereof and, more specifically, to an extrusion molded catalyst for an ortho-alkylation reaction and a method for producing an ortho-alkylation reaction product by using same, wherein in the ortho-alkylation reaction of a phenolic compound, the ortho-alkylation reaction product can be obtained with high selectivity and conversion by minimizing the material diffusion resistance of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Ortho-alkylation reaction extrusion molding catalyst and method for producing the same

[0001] Cross-citation with related application(s)

[0002] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0055405, filed April 27, 2023, the entire contents of which are incorporated herein by reference.

[0003] The present invention relates to a technology for an ortho-alkylation reaction extrusion molding catalyst and a method for producing the same, and more specifically, to an ortho-alkylation reaction extrusion molding catalyst capable of obtaining an ortho-alkylation reaction product with high selectivity and conversion by minimizing the material diffusion resistance of the catalyst in the ortho-alkylation reaction of a phenolic compound, and a method for producing the same.

[0004]

[0005] Alkylated hydroxyaromatic compounds have a wide range of applications and are typically prepared by the gas-phase reaction of phenol and methanol. Further alkylation reactions can produce compounds with diverse structures, making them ideal for applications in high-performance thermoplastics.

[0006] These additional alkylation reactions have typically been performed in the presence of magnesium compounds, and various studies have been conducted to optimize the performance of magnesium catalysts.

[0007] In alkylation reactions, magnesium-based catalysts are required to possess high activity, long activity lifetimes, and high selectivity for the desired reaction product. Most alkylation catalysts used in the past produced large quantities of para-alkylated products, but extensive research has been conducted to obtain higher yields of the more useful ortho-alkylated products.

[0008] However, conventional technologies have had the problem of making it difficult to obtain ortho-alkylation products with the desired degree of selectivity and yield using conventional technologies that combine a cocatalyst compound with a magnesium catalyst, change the composition of the catalyst, or change the reaction conditions.

[0009] Accordingly, there is a need to develop an improved catalyst in the ortho-alkylation reaction in terms of catalyst selectivity, catalyst activity, production yield, cost reduction, and overall productivity.

[0010] Meanwhile, for alkylation reactions, it is possible to use a catalyst in powder form in small quantities at the laboratory level, but in order to produce the catalyst in large quantities and apply it to a commercial fixed bed reactor, the catalyst must be appropriately shaped to fit the reactor, taking into account the pressure drop during the reaction.

[0011] Extrusion and tablet molding are commonly used methods for catalyst molding. While tablet molding can produce precise molded products, its high equipment and manufacturing cost significantly reduce its economic feasibility. On the other hand, extrusion molding is a widely used molding method due to its simple equipment and relatively low manufacturing cost. However, molding a catalyst can affect the internal and external material diffusion resistance, which can lead to a decrease in activity in the manufactured molded catalyst. Therefore, various studies are needed to minimize this activity decrease.

[0012]

[0013] The present invention provides an ortho-alkylation reaction extrusion molding catalyst capable of achieving excellent conversion and yield in the production of a selective ortho-alkylation reaction product. In addition, the present invention provides an ortho-alkylation reaction extrusion molding catalyst capable of achieving uniform catalytic activity both inside and outside the molded catalyst without loss of activity.

[0014] In addition, the present invention provides a method for producing the catalyst.

[0015]

[0016] In order to solve the above problem, the present invention,

[0017] Contains magnesium oxide,

[0018] Containing macropores having a diameter of 50 nm to 10,000 nm and mesopores having a diameter of 2 nm to 50 nm,

[0019] BET surface area is 45 m 2 / g to 180 m 2 / g person,

[0020] An ortho-alkylation reaction extrusion molding catalyst is provided.

[0021]

[0022] In addition, the present invention provides a method for producing the ortho-alkylation reaction extrusion molding catalyst.

[0023] Specifically, it has a bimodal pore structure and a BET surface area of ​​100 m 2 / g to 180 m 2 A first step of preparing a mixture of magnesium oxide, an organic binder and a solvent; and

[0024] A second step comprising extruding the mixture,

[0025] A method for producing an ortho-alkylation reaction extrusion molding catalyst is provided.

[0026]

[0027] The ortho-alkylation reaction extrusion molding catalyst according to the present invention exhibits high catalytic activity, and when using it to produce an ortho-alkylation reaction product, it exhibits remarkably high selectivity and conversion.

[0028] In addition, the present invention provides an ortho-alkylation reaction extrusion molding catalyst that can minimize the material diffusion resistance of the catalyst by appropriately forming macropores and mesopores and having an appropriate BET specific surface area, thereby realizing excellent catalytic activity uniformly inside and outside the molded catalyst without a decrease in activity.

[0029] The ortho-alkylation reaction extrusion molding catalyst according to the present invention is manufactured by combining magnesium oxide with specific properties, an organic binder, and a solvent, thereby exhibiting high catalytic activity on its own without the use of a separate cocatalyst or additional additive, and when an ortho-alkylation reaction product is manufactured using the same, it exhibits remarkably high selectivity and conversion.

[0030]

[0031] Figure 1 is a graph showing the conversion rate versus selectivity according to the type of catalyst in the ortho-alkylation reaction forming catalyst of the examples and comparative examples of the present invention.

[0032] Figure 2 is a graph showing the conversion rate versus selectivity according to the type / content of the binder in the ortho-alkylation reaction forming catalyst of an embodiment of the present invention.

[0033] Figure 3 is a graph showing pore size versus pore volume according to the type of molded catalyst of examples and comparative examples of the present invention.

[0034]

[0035] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and technical scope of the present invention.

[0036] Furthermore, the terminology used herein is merely for the purpose of describing exemplary embodiments and is not intended to limit the present invention. Singular expressions include plural expressions unless the context clearly dictates otherwise. In this specification, it should be understood that terms such as "comprise," "include," or "have" indicate the presence of implemented features, steps, components, or combinations thereof, but do not preclude the possibility of the presence or addition of one or more other features, steps, components, or combinations thereof.

[0037] Additionally, in the present invention, when each component is referred to as being formed “on” or “over” each component, it means that each component is formed directly on each component, or that other components may be additionally formed between each layer, on the object, or on the substrate.

[0038]

[0039] Magnesium-based catalysts typically used in alkylation reactions require high activity, long lifespan, and high selectivity for the desired reaction product. Most alkylation catalysts used in the past produced large quantities of para-alkylated products, but extensive research has been conducted to obtain the more useful ortho-alkylated products with high selectivity.

[0040] Specifically, various technologies have been developed recently that combine magnesium-based catalysts with cocatalyst compounds, alter the catalyst composition, or modify reaction conditions. However, these technologies have struggled to produce ortho-alkylated products with the desired high selectivity and conversion.

[0041] To address these issues, the inventors of the present invention have confirmed that, for an extruded catalyst containing a specific magnesium oxide, when the catalyst satisfies an appropriate pore distribution and BET specific surface area, it can exhibit remarkably high catalytic activity in an alkylation reaction. Accordingly, the ortho-alkylation reaction catalyst according to the present invention exhibits excellent catalytic activity even as a single catalyst without additionally using a cocatalyst or adjusting reaction conditions, and when using it to produce an ortho-alkylation reaction product, it can exhibit remarkably high selectivity and conversion, thereby completing the present invention.

[0042] Meanwhile, for alkylation reactions, small amounts of powdered catalysts can be used in the laboratory, but to mass-produce catalysts and apply them to commercial fixed-bed reactors, the catalyst must be appropriately molded to fit the reactor, taking into account the pressure drop during the reaction. Commonly used catalyst molding methods include extrusion and tablet molding. Tablet molding can produce precise molded bodies, but the expensive equipment and high manufacturing cost significantly reduce economic feasibility. On the other hand, extrusion molding is a widely used molding method because the equipment is simple and the manufacturing cost is relatively low. However, there was a problem that the extrusion molding of the catalyst affected the internal / external material diffusion resistance, resulting in a decrease in activity in the manufactured extrusion-molded catalyst.

[0043] Accordingly, the inventors of the present invention have identified key factors affecting the catalytic activity of molded catalysts manufactured by extrusion molding to address these issues. Specifically, by using magnesium oxide having a specific pore structure as described above and simultaneously forming appropriate macro- and meso-sized pores in the final catalyst to achieve an appropriate BET specific surface area, the inventors have confirmed that uniform catalytic activity can be achieved in the manufactured extrusion molded catalyst by minimizing the influence of internal / external material diffusion resistance, thereby completing the present invention.

[0044]

[0045] I. Ortho-alkylation reaction extrusion molding catalyst

[0046] An ortho-alkylation reaction extrusion molding catalyst according to one embodiment of the invention comprises magnesium oxide, comprises macropores having a diameter of 50 nm to 10,000 nm and mesopores having a diameter of 2 nm to 50 nm, and has a BET specific surface area of ​​45 m 2 / g to 180 m 2 / g is satisfied.

[0047]

[0048] In general, the catalytic activity of a catalyst is determined by the reaction conditions or the acid-base properties of the catalyst. In the alkylation reaction of a meta-alkyl substituted phenolic monomer, if the catalyst has basic properties, it perpendicularly adsorbs the reactant and favors ortho-C-alkylation (see Figure (a) below). Accordingly, the ortho-alkylation reaction catalyst according to the present invention includes a magnesium oxide (MgO) component.

[0049]

[0050]

[0051] The above catalyst is manufactured using magnesium oxide having a bi-modal pore structure. Specifically, the magnesium oxide used in the manufacturing step has a bi-modal form of mesopores (mesopores), thereby facilitating the diffusion of reactants and enabling the reaction to be carried out effectively. Accordingly, it exhibits excellent catalytic activity in the ortho-alkylation reaction and can exhibit high selectivity, conversion, and yield.

[0052]

[0053] The above ortho-alkylation reaction extrusion molding catalyst comprises macro pores having a diameter of 50 nm to 10,000 nm and meso pores having a diameter of 2 nm to 50 nm.

[0054] In this way, macropores and mesopores are appropriately formed to minimize the material diffusion resistance of the catalyst, thereby enabling uniform and excellent catalytic activity to be achieved inside and outside the formed catalyst without a decrease in activity.

[0055]

[0056] The macropores of the above ortho-alkylation reaction extrusion molding catalyst may be included in an amount of 1 to 10 vol% based on the total mixed volume of the macropores and mesopores, and preferably, 1 to 9 vol%, 2 to 10 vol%, 2 to 9 vol%, or 2 to 5 vol%. When included in the above range, the material diffusion resistance of the molded catalyst can be minimized, which is preferable.

[0057] The mesopores of the above ortho-alkylation reaction extrusion molding catalyst may be included in an amount of 90 to 99 vol% based on the total mixed volume of the macropores and mesopores, and preferably, 90 to 98 vol%, 91 to 98 vol%, or 95 to 98 vol%. When included in the above range, the molded catalyst is suitable for realizing excellent catalytic activity without a decrease in activity.

[0058] The method for measuring the pore size and pore volume distribution of the above catalyst will be described in more detail in the experimental examples described below.

[0059]

[0060] The above ortho-alkylation reaction extrusion molding catalyst has a BET specific surface area of ​​45 m 2 / g to 180 m 2 / g is.

[0061] The above catalyst has the above-described macro pores and meso pores appropriately formed and at the same time exhibits a BET specific surface area value within a specific range, thereby minimizing the material diffusion resistance of the catalyst and enabling uniform, excellent catalytic activity to be realized on the inside and outside of the formed catalyst without a decrease in activity.

[0062] Preferably, the BET specific surface area is 45 m 2 / g to 150 m 2 / g, 45 m 2 / g to 130 m 2 / g, or 60 m 2 / g to 130 m 2 / g, and when the specific surface area of ​​the above range is implemented, it is preferable to minimize the material diffusion resistance of the formed catalyst. The method for measuring the BET specific surface area of ​​the catalyst will be described in more detail in the experimental examples described below.

[0063] Meanwhile, the pore distribution and BET specific surface area of ​​the catalyst can be preferably achieved by combining an organic binder and a solvent with magnesium oxide having specific physical properties. This will be described in more detail in the section on the manufacturing method.

[0064]

[0065] The above ortho-alkylation reaction extrusion molding catalyst can satisfy a size of 0.5 mm to 6.0 mm, and can realize uniform and excellent catalytic activity within the said range. More preferably, the size of the catalyst can be 1.0 mm to 3.0 mm or 1.2 to 2.0 mm. If the size of the catalyst is excessively small beyond the above-mentioned range, a large pressure drop may occur during the alkylation reaction, which may be problematic. In addition, if the size of the catalyst is excessively large beyond the above-mentioned range, there is a concern that a problem of reduced catalytic activity may occur.

[0066] The size of the above catalyst can be controlled depending on the diameter of the extrusion die used in the final extrusion step in the manufacturing process.

[0067] Typically, the shape of an extrusion-molded catalyst is implemented as a cylindrical shape by an extrusion die. The extrusion-molded catalyst according to the present invention may have a ratio of the diameter of the circular cross-section of the cylinder and the length of the cylinder of 1:1 (±0.1).

[0068] Accordingly, the size of the extruded catalyst may refer to the diameter of the circular cross-section of the cylinder and / or the length of the cylinder, and it is preferable that both the circular cross-section and the length of the cylinder simultaneously satisfy the above-mentioned range.

[0069] The specific method for measuring the size of the above catalyst will be described in more detail in the experimental examples described below.

[0070]

[0071] Ⅱ. Method for producing an ortho-alkylation reaction extrusion molding catalyst

[0072] According to another embodiment of the invention, a method for producing an ortho-alkylation reaction extrusion catalyst is provided, comprising the following steps:

[0073] Specifically, it has a bimodal pore structure and a BET surface area of ​​100 m 2 / g to 180 m 2 A method for producing a composite material, comprising: a first step of preparing a mixture of magnesium oxide, an organic binder, and a solvent; and a second step of extruding the mixture.

[0074] Below, each step will be explained in detail.

[0075]

[0076] Step 1: Preparation of the mixture

[0077] First, it has a bimodal pore structure and a BET surface area of ​​100 m 2 / g to 180 m 2 A mixture is prepared by mixing / g of magnesium oxide, an organic binder, and a solvent.

[0078] The above magnesium oxide can be applied in the same manner as described in the ortho-alkylation reaction extrusion molding catalyst.

[0079] Preferably, the magnesium oxide has a bimodal pore structure, specifically a bimodal form in the mesopore (mesopore) range, thereby facilitating diffusion of the reactants and enabling the reaction to be carried out effectively. Accordingly, it exhibits excellent catalytic activity in the ortho-alkylation reaction and can exhibit high selectivity, conversion, and yield.

[0080] Normally, the larger the BET surface area, the more active sites the catalyst has. However, in the case of a single-modal form, even if the BET surface area increases, the diffusion of the reactants is not smooth, making it difficult to carry out the reaction to the desired degree.

[0081] Preferably, in the bi-modal pore structure, the diameter of the first pore may be 2 nm to 10 nm, and the diameter of the second pore may be 10 nm to 50 nm, and more preferably, the diameter of the first pore may be 4 nm to 8 nm, and the diameter of the second pore may be 20 nm to 45 nm or 35 nm to 45 nm. The bi-modal pore structure having the diameter in the above range can exhibit the desired excellent catalytic activity, improved selectivity, conversion rate, and yield.

[0082] The above magnesium oxide has a BET surface area of ​​100 m 2 / g to 180 m 2 / g, and has excellent catalytic activity due to its relatively large surface area and many reactive sites. At the same time, as described above, it has a bimodal pore structure, which facilitates the diffusion of reactants, enabling the reaction to be carried out effectively. Accordingly, it has excellent catalytic activity in the ortho-alkylation reaction and can exhibit improved selectivity, conversion, and yield. The BET surface area is 100 m 2 If the BET surface area is less than 180 m , the reaction active sites are significantly reduced, which lowers the reaction conversion rate, making it difficult to achieve the desired activity. In addition, the BET surface area is less than 180 m . 2 When / g is exceeded, the reaction active point increases, but there is a problem that it is difficult to achieve high activity because the first pore is mainly formed and reactant / product diffusion is not smooth.

[0083] Preferably, the BET surface area of ​​the magnesium oxide is 130 m 2 / g to 180 m2 / g, more preferably 130 m 2 / g to 150 m 2 / g, and it is preferable that excellent catalytic activity can be achieved without the aforementioned problems within the above range.

[0084]

[0085] The above organic binder is a component that has a significant influence on implementing uniformity of catalytic activity by uniformly binding magnesium oxide during the production of a molded catalyst, facilitating catalyst production, and forming appropriate pores within the catalyst through sintering, particularly during the production of an extruded molded catalyst. If the magnesium oxide having the specific properties described above is used alone, the ease of catalyst production may be reduced, and the formation of the desired pores may be somewhat difficult. However, when used in combination, it is preferable because it can implement superior catalytic activity uniformly.

[0086] Specific examples of the organic binder include methylcellulose, carboxymethylcellulose, ethylene glycol, polyethylene glycol, polyphenylene oxide, glycerin, and propylene glycol, and these may be used alone or in combination of two or more. More preferably, methylcellulose, carboxymethylcellulose, and polyethylene glycol (PEG 20000 or PEG 400) may be used.

[0087] The organic binder may be included in an amount of 0.1 to 20 parts by weight, and preferably, 0.1 to 15 parts by weight, 0.1 to 10 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of magnesium oxide. It is suitable for implementing the aforementioned effects when used within the above range.

[0088]

[0089] The above solvent is used to enable the mixture to be kneaded uniformly, and to facilitate extrusion when manufacturing an extruded body.

[0090] Specific examples of the solvent include water, alcohol, etc., and these may be used alone or in combination of two or more. More preferably, water may be used. The water may be high-purity water such as distilled water, ion-exchanged water, or ultrapure water (DIW). If the water contains impurities, the impurities may adhere to the catalyst and reduce the activity of the catalyst, so it is preferable to use ultrapure water, etc. In the case of alcohol, a primary alcohol having a carbon content of C3 or higher may be preferably used.

[0091] The solvent may be included in an amount of 50 to 200 parts by weight, and preferably 80 to 150 parts by weight or 100 to 120 parts by weight, based on 100 parts by weight of magnesium oxide. The mixture mixed in the above ratio may preferably be in the form of a paste. In this case, the extrusion molding process can be easily performed, which is preferable.

[0092]

[0093] Meanwhile, according to one embodiment of the invention, the mixture may optionally include additional additives, for example, a lubricant or the like, so that the final molded catalyst can be manufactured uniformly or without fragmentation during the manufacturing process. Specific examples of the lubricant include, but are not limited to, magnesium stearate, aluminum stearate, graphite, and the like.

[0094] Additionally, other additives used in the field may be used without special restrictions as long as they do not impair the desired properties.

[0095]

[0096] Step 2: Extrusion Molding Stage

[0097] Next, a second step of extruding the mixture is included.

[0098] Tablet molding, which is commonly used in catalyst molding methods, can produce a precise molded body shape, but the expensive equipment and high manufacturing cost significantly reduce economic feasibility. On the other hand, extrusion molding is a molding method that is widely used because the equipment installation is simple and the manufacturing cost is relatively low. However, when a catalyst is molded, the internal / external material diffusion resistance is affected, so a decrease in activity may occur in the manufactured molded catalyst. In the case of the present invention, by using a combination of magnesium oxide with specific physical properties, an organic binder, and a solvent as described above, it is possible to produce an extrusion molded catalyst that has high activity and uniformity inside and outside the catalyst without these problems.

[0099] The above extrusion molding process can generally be used in screw form (Screw extruder) and piston form (Piston extruder), but

[0100] Preferably, the process can be performed using a single-piston extruder, which allows for the production of an extruded catalyst with a low moisture content and high compression ratio at high pressure. In this case, the extrusion process can be performed through a die of a specific diameter, but is not limited thereto.

[0101] The average diameter of the extrusion die used can be appropriately adjusted depending on the desired diameter range of the final molded catalyst.

[0102]

[0103] Additional steps: drying and firing

[0104] In one embodiment of the invention, the step of drying and firing after the extrusion molding may be further included.

[0105] The process conditions of the above drying and firing steps can be applied without any special restrictions as processes commonly applied in the field.

[0106]

[0107] Specifically, the temperature at which the drying step is performed is not particularly limited, but may be performed at, for example, 80°C to 120°C, and preferably 90°C to 110°C.

[0108] The time for performing the above drying step is not particularly limited, but may be performed for, for example, 1 to 13 hours, preferably 3 to 8 hours, or 4 to 6 hours.

[0109]

[0110] The temperature at which the above-mentioned firing step is performed is not particularly limited, but may be performed at, for example, 300°C to 600°C, and preferably 400°C to 550°C.

[0111] The time for performing the above calcination step is not particularly limited, but is performed for an appropriate time or longer to remove the organic binder and solvent in the mixture and form the desired pores in the catalyst, and is preferably performed for 1 to 9 hours, or 3 to 6 hours.

[0112]

[0113] The catalyst manufactured according to the above-described method for manufacturing an extrusion molding catalyst for ortho-alkylation reaction can realize excellent catalytic activity uniformly inside and outside the molded catalyst without a decrease in activity by using a combination of magnesium oxide having specific properties, an organic binder, and a solvent.

[0114]

[0115] Ⅲ. Ortho-alkylation reaction composition

[0116] According to one embodiment of the invention, the ortho-alkylation reaction composition comprises the above-described ortho-alkylation reaction extrusion molding catalyst and a monomer composition comprising a meta-alkyl substituted phenolic monomer.

[0117] The above ortho-alkylation reaction extrusion molding catalyst comprises magnesium oxide, and comprises macropores having a diameter of 50 nm to 10,000 nm and mesopores having a diameter of 2 nm to 50 nm, and has a diameter of 45 m 2 / g to 180 m 2 / g has a BET surface area. All of the above can be applied equally to this.

[0118] Specifically, the aforementioned macro pores and meso pores are appropriately formed to minimize the material diffusion resistance of the catalyst, thereby enabling uniform and excellent catalytic activity to be realized inside and outside the formed catalyst without a decrease in activity.

[0119] In addition, the magnesium oxide included in the catalyst has a bimodal pore structure, specifically, a mesopore bimodal form, thereby facilitating the diffusion of reactants and enabling the reaction to be carried out effectively. In addition, by simultaneously satisfying the BET specific surface area within the above-mentioned specific range, it exhibits excellent catalytic activity in the ortho-alkylation reaction and can exhibit high selectivity and conversion.

[0120]

[0121] In the above monomer composition, the meta-alkyl substituted phenolic monomer may be meta-cresol (m-cresol).

[0122] The above monomer composition further comprises, in addition to the meta-alkyl substituted phenolic monomer, an alkanol and distilled water (DI water), and an alkyl group can be introduced through a reaction with the alkanol. By using the distilled water together, the decomposition reaction of the alkanol can be suppressed, which is preferable. The alkanol can preferably be methanol.

[0123] The monomer composition may preferably contain phenolic monomer: alkanol: distilled water in an amount of 1:3 to 10:1 to 5 parts by weight, and more preferably, 1:4 to 6:1 to 3 parts by weight. At this time, if the content of alkanol is included in a small amount outside the above range, the alkylation mediator (agent) is reduced, resulting in a lower conversion rate. If the content of distilled water is included in a small amount outside the above range, the effect of suppressing the decomposition reaction of the alkanol is reduced. If the alkanol or distilled water is included in an excessive amount outside the above range, the reactivity may be reduced due to competitive adsorption with the phenolic monomer at the catalyst active site.

[0124] When included in the above content range, it is preferable to produce an ortho-alkylation reaction product with the desired selectivity and conversion rate.

[0125]

[0126] Ⅳ. Method for producing ortho-alkylation reaction product

[0127] According to one embodiment of the invention, a method for producing an ortho-alkylation reaction product comprises an alkylation reaction of a monomer composition comprising a meta-alkyl substituted phenolic monomer in the presence of the above-described ortho-alkylation reaction extrusion molding catalyst. Specifically, the method for producing an ortho-alkylation reaction product can be performed using an ortho-alkylation reaction composition comprising the above-described ortho-alkylation reaction extrusion molding catalyst. The above-described contents can be equally applied to both the catalyst and the reaction composition.

[0128] The above ortho-alkylation reaction extrusion molding catalyst comprises magnesium oxide, has macropores with a diameter of 50 nm to 10,000 nm and mesopores with a diameter of 2 nm to 50 nm, and has a BET specific surface area of ​​45 m 2 / g to 180 m 2 / g is satisfied. All of the above can be applied equally to this.

[0129] Specifically, by including the above-described extruded catalyst, it is possible to realize uniform and excellent catalytic activity on the inside and outside of the molded catalyst without a decrease in activity.

[0130]

[0131] In the method for producing the above ortho-alkylation reaction product, the monomer composition may be applied in the same manner as described above, and specifically, the monomer composition may be a meta-alkyl substituted phenolic monomer, such as meta-cresol. The method for producing the above ortho-alkylation reaction product can exhibit high selectivity and conversion of the desired ortho-alkylation reaction product by using a reaction composition including the above-described extrusion molding catalyst.

[0132]

[0133] The above ortho-alkylation reaction product may be, for example, at least one selected from the group consisting of 2,5-dimethylphenol, 2,3-dimethylphenol, 2,3,6-trimethylphenol, 3-methylanisole, 3,4-dimethylphenol, and tetramethylphenol, and may be produced by selectively substituting an alkyl group at the ortho position in m-cresol through a multi-step reaction as follows.

[0134]

[0135]

[0136] The above alkylation reaction may preferably be carried out at a temperature of 350°C to 550°C, and more preferably at a temperature of 350°C to 550°C. At this time, if the temperature is lower than 350°C, the alkylation reaction may not be sufficiently activated, and if it exceeds 550°C, a large amount of by-products are generated due to overreaction.

[0137]

[0138] The above alkylation reaction can be carried out under inert conditions, for example, in the presence of an inert carrier gas. Nitrogen, helium, neon, argon, etc. can be used as the inert carrier gas, and nitrogen is preferably used.

[0139] The above nitrogen flow rate is not particularly limited, but preferably, it can be performed at 5 to 70 cc / min, 10 to 50 cc / min, or 15 to 40 cc / min, and by performing under the above conditions, it is preferable to produce an ortho-alkylation reaction product with the desired selectivity and conversion rate.

[0140]

[0141] Meanwhile, in the above alkylation reaction, a process of raising and maintaining the inside of the reactor to an activation temperature for catalyst activation prior to the introduction of the monomer composition may be performed, and the temperature range may be the same as the reaction temperature. The time for performing the catalyst activation is not particularly limited, but may be about 30 minutes to 1 hour.

[0142]

[0143] The above alkylation reaction can be preferably carried out using a continuous flow gas phase reactor, in which case the monomer composition is introduced into the continuous flow gas phase reactor at a rate of 0.5 hr. -1 2.0 hr -1 It can be performed by injecting at the LHSV (liquid hourly space velocity). At this time, if the space velocity range is exceeded, the reactants may not be sufficiently activated at the catalytic active site, making it difficult to obtain the product smoothly, and also the activity or selectivity of the catalyst may decrease, reducing the amount of the product.

[0144] By performing the process under the above conditions, it is preferable to produce an ortho-alkylation reaction product with the desired selectivity and conversion.

[0145]

[0146] Hereinafter, the functions and effects of the invention will be described in more detail through specific examples. However, these examples are provided merely as examples of the invention and do not define the scope of the invention.

[0147]

[0148] [Example 1 and Comparative Example 1]

[0149] Example 1-1. Preparation of extrudate catalyst (preparation of extrusion molding catalyst)

[0150] Magnesium oxide (MgO powder, Crystallite size 9 nm, BET surface area 144.4 m 2 / g, Total pore volume 0.72 cm 3 / g, Pore size 6, 40 nm), 50 g of organic binder (methyl cellulose), 1 g of distilled water were added to a mixing bowl and mixed evenly to make a paste. Once the dough was made, it was extruded through a 2 mm diameter die using a single piston extruder catalyst molding equipment. The noodle shape extruded from the single piston extruder was evenly spread on a tray.

[0151] Next, after drying at 100°C for 4 hours using a convection oven, the dried extruded catalyst was cut into 2 mm intervals and calcined at 450°C for 6 hours using a muffle furnace to manufacture a magnesium-based extruded catalyst (A-1).

[0152]

[0153] Comparative Example 1-1. Tablet catalyst manufacturing

[0154] Magnesium oxide (MgO powder, Crystallite size 9 nm, BET surface area 144.4 m 2 / g, Total pore volume 0.72 cm 3 / g, pore size 6, 40 nm) was first pressed into a disc shape using a plate-type press equipment and an aluminum dish, and then crushed to produce granules with an appropriate particle size to provide flowability. 10 wt% of an organic binder (PPO, polyphenylene oxide) and 1 wt% of a lubricant (magnesium stearate) were mixed into the manufactured granules, and tablets with a diameter of 2.4 mm were manufactured using a single rotary tablet press catalyst molding equipment.

[0155] Next, after drying at 100°C for 4 hours using a convection oven, the dried tablet-forming catalyst was calcined at 450°C for 1 hour using a muffle furnace to complete a magnesium-based tablet-forming catalyst (B-1).

[0156]

[0157] Examples 1-2 to 1-8

[0158] The same method was followed except that the components and contents of the binder resin and solvent used in Example 1-1 were changed as shown in Table 1 below.

[0159] Classification FormBinder ResinSolventExample 1-1(A-1)ExtrudateMC 1gD.I.water 60gExample 1-2(A-2)ExtrudateMC 1gD.I.water 60gExample 1-3(A-3)ExtrudateMC 0.2gD.I.water 60gExample 1-4(A-4)ExtrudateMC 2gD.I.water 60gExample 1-5(A-5)ExtrudateMC 10gD.I.water 60gExample 1-6(A-6)ExtrudateMC 1gD.I.water 72gExample 1-7(A-7)ExtrudatePEG 20000 1gD.I.water 60gExample 1-8(A-8)ExtrudatePEG 400 1gD.I.water 60g Comparative Example 1-1 (B-1) Tablet PPO 10 wt%, Mg stearate 1 wt% - <Catalyst Form> Extrudate: Extrusion molding catalyst Tablet: Tablet molding catalyst <Binder Resin> MC: Methylcellulose PEG: Polyethylene glycol PPO: Polyphenylene oxide

[0160] [Experimental Example 1: Analysis of the ortho-alkylation reaction catalyst]

[0161] (1) BET surface area analysis

[0162] The catalysts of Example 1 and Comparative Example 1 were subjected to nitrogen-adsorption-desorption analysis experiments, and the BET specific surface area value was measured according to the BET (Brunauer Emmett Teller) calculation formula for the isothermal adsorption curve and the amount of adsorbed nitrogen at standard temperature and pressure, and the results are shown in Table 2.

[0163] The average diameter of the catalyst in the form of an extrudate refers to the diameter of the circular cross-section of a cylindrical catalyst manufactured by a die mounted on a single piston extruder, and the average diameter of the catalyst in the form of a tablet refers to the diameter of the circular cross-section of a cylindrical catalyst manufactured by a punch mounted on a rotary tablet press.

[0164] Classification Size (average diameter) / Shape BET specific surface area (m2 / g) Example 1-1 (A-1) 2 mm / Extrudate 7 7.86 Example 1-2 (A-2) 1.2 mm / Extrudate 6 0.32 Example 1-3 (A-3) 2 mm / Extrudate 1 2 9.82 Example 1-4 (A-4) 2 mm / Extrudate 1 2 9.42 Example 1-5 (A-5) 2 mm / Extrudate 7 1.87 Example 1-6 (A-6) 2 mm / Extrudate 1 3 1.17 Example 1-7 (A-7) 2 mm / Extrudate 4 5.09 Example 1-8 (A-8) 2 mm / Extrudate 8 3.71 Comparative Example 1-1 (B-1) 2.4 mm / Tablet 8 2.40

[0165] (2) Hg porosity analysis The pore structures of the macro and meso regions of the catalysts of Example 1 and Comparative Example 1 were confirmed through Hg porosity, and the results are shown in Table 3 and Figure 3.

[0166] Macropore size (mL / g) / (vol%) * Mesoporosity (mL / g) / (vol%) * Bulk density (mL / g) Apparent density (g / mL) Example 1-1 (A-1) 0.0153 / 2.63 0.56 62 / 97.37 1.008 2 3.07 64 Example 1-2 (A-2) 0.0153 / 2.76 0.53 89 / 97.24 0.89 4 82.66 45 Example 1-3 (A-3) 0.0187 / 3.04 0.59 74 / 96.96 0.915 92.71 16 Example 1-5 (A-5) 0.0558 / 8.84 0.57 53 / 91.16 0.96 7 13.60 60 Example 1-6(A-6)0.0575 / 7.170.7441 / 92.830.78072.8106Comparative example 1-1(B-1)0.0799 / 17.040.3889 / 82.961.12143.0060

[0167] * As can be seen in Tables 2 and 3 and Fig. 3, in order to minimize the decrease in activity due to internal / external material diffusion resistance, it is desirable to manufacture an extrusion-molded catalyst through extrudate using an appropriate organic binder and solvent limited herein, thereby forming appropriate pores from the meso to micro range, and at the same time, it was confirmed to have an appropriate range of BET specific surface area.

[0168] By implementing the corresponding pore distribution and BET specific surface area value, the material diffusion resistance can be minimized during the alkylation reaction, resulting in high conversion and selectivity. This will be explained in more detail in Experimental Example 2.

[0169]

[0170] [Example 2 and Comparative Example 2]

[0171] Example 2-1: Preparation of alkylation reaction product of m-cresol

[0172] The alkylation reaction of m-cresol was performed using a continuous flow gas phase reactor. First, 1 g of the molded catalyst of Example 1-1 having the properties shown in Table 1 was charged into a stainless steel tube-type reactor with a diameter of 1 / 2 inch x a length of 50 cm, and then installed in the main furnace.

[0173] After that, N2 as a carrier gas was flowed (37.5 cc / min) using a mass flow controller (MFC), and the inside of the reactor was raised to the activation temperature (450 ℃) for catalyst activation and maintained for 1 hour. After that, the monomer composition (12.5 mg / min, m-cresol: Methanol: DIwater = 1:5:1, LHSV 0.75 / h) was introduced after vaporization through a pre-heater (250 ℃). The reaction composition including the catalyst and monomer composition was introduced into the reactor, and thereafter, the alkylation reaction (450 ℃, maintained at normal pressure) was performed for 5 hours to obtain the reaction product.

[0174] During the reaction, the product was captured in liquid form (IPA (isopropyl alcohol) was used as a solvent) for analysis.

[0175]

[0176] Examples 2-2 to 2-8, Comparative Example 2-1

[0177] An alkylation reaction was carried out in the same manner as in Example 2-1, except that the catalyst was changed from the catalyst of Example 1-1 to the catalyst of Examples 1-2 to 1-8 and Comparative Example 1-1 in Table 1, and a reaction product was obtained.

[0178]

[0179] [Experimental Example 2: Analysis of ortho-alkylation reaction products]

[0180] (2-1) Analysis of reaction products according to catalyst type

[0181] The liquids in which the reaction products prepared in Example 2 and Comparative Example 2 were collected were analyzed using a gas chromatography device (GC) equipped with a flame ionization detector (FID), and the m-cresol conversion rate and the selectivity of the target product (2,3,6-TMP, 2,5-DMP, 2,3-DMP, Tetra-methyl phenol) were calculated from the GC results using the following mathematical equations 1 and 2, and the results are shown in Table 4, Fig. 1 (type (size / shape) of catalyst) and Fig. 2 (type / content of binder used in catalyst preparation).

[0182] The target product was defined as 2,3,6-TMP, the final product, and 2,5-DMP and 2,3-DMP, which can be obtained as the final product through further reaction as intermediate materials.

[0183] [Mathematical Formula 1]

[0184]

[0185] [Equation 2]

[0186]

[0187]

[0188] Category (catalyst type) Conversion rate Selectivity m-cresol Target product a DMP b TMP c TeMP dExample 2-1 (A-1) 96.1388.5121.1562.458.59 Example 2-2 (A-2) 93.5895.3937.9148.872.2 Example 2-3 (A-3) 97.9185.2515.7166.0211.57 Example 2-4 (A-4) 97.1487.1319.2163.659.77 Example 2-5 (A-5) 93.5089.9427.256.576.98 Example 2-6 (A-6) 99.4083.589.9871.5113.52 Example 2-7(A-7)93.7491.9629.1456.105.72Example 2-8(A-8)94.9593.9926.4761.764.69Comparative Example 2-1(B-1)85.0192.6829.1656.04.82 a Target product: DMP and TMP b DMP: 2,5-dimethylphenol and 2,3-dimethylphenolc TMP: 2,3,6-trimethylphenold TeMP: Tetra-methyl phenol

[0189] As can be seen from the experimental data in Table 4 above, when the extruded catalyst according to the present invention is used, high catalytic activity is exhibited even with a single catalyst, and when the ortho-alkylation reaction product is produced using the same, it was confirmed that significantly high selectivity and conversion can be exhibited. In the case of Comparative Example 2-1, it was confirmed that it was difficult to achieve the desired level of catalytic activity by using a tablet-shaped molded catalyst, and accordingly, the conversion rate, etc. were lowered compared to the examples.

[0190]

[0191] (2-2) Analysis of products according to reaction conditions

[0192] Example 3: Changing the reaction temperature

[0193] The alkylation reaction was performed in the same manner as in Example 2-1 except that the methylation reaction temperature was changed from 400°C to 450°C by increasing by 10°C every 3 hours, and the m-cresol conversion rate and the selectivity of the target product (2,3,6-TMP, 2,5-DMP, 2,3-DMP) were calculated according to the method of Experimental Example 2 described above, and the results are shown in Table 5 below.

[0194]

[0195] Example 4: Changing the carrier gas flow rate

[0196] The alkylation reaction was performed in the same manner as in Example 2-1 except that the carrier gas flow rate was set to 18.7 cc / min, and the m-cresol conversion rate and the selectivity of the target product (2,3,6-TMP, 2,5-DMP, 2,3-DMP) were calculated according to the method of Experimental Example 2 described above, and the results are shown in Table 5 below.

[0197]

[0198] Example 5: Changing the amount of methanol injected

[0199] The alkylation reaction was performed in the same manner as in Example 1 except that the liquid mixture including the reactants was injected as m-cresol: Methanol: DIwater = 1:4:1 (11.1 mg / min, LHSV 0.666 / h) and m-cresol: Methanol: DIwater = 1:3:1 (9.7 mg / min, LHSV 0.582 / h), and the m-cresol conversion and the selectivity of the target product (2,3,6-TMP, 2,5-DMP, 2,3-DMP) were calculated according to the method of Experimental Example 2 described above, and the results are shown in Table 5 below.

[0200] Classification (catalyst type) Reaction conditions Conversion rate Selectivity m-cresol Target product a DMP bTMP c TeMP d Example 3 (A-1) Reaction temperature control 400 ℃ 47.129 7.168 2.32 14.84 0410 ℃ 60.58 97.22 76.26 20.96 0.49 420 ℃ 70.09 96.97 67.52 9.47 0.98 430 ℃ 84.9 195.28 46.16 49.122 93 440 ℃ 90.38 94.12 36.22 57.94 06 450 ℃ 95.5 592.41 24.74 67.67 5.75 Example 4 (A-1) Nitrogen flow rate control 37.5 cc / min (same as Example 2-1) 96.138 8.5 121.156 2.45 8.5 9 18.7 cc / min98.7687.6712.6575.029.93Example 5 (A-1)Feed ratio adjustment1:3:159.9896.1475.4520.690.561:4:196.2989.6126.9562.667.541:5:1 (same as Example 2-1)96.1388.5126.0662.458.59 a Target product: DMP and TMP b DMP: 2,5-dimethylphenol and 2,3-dimethylphenolc TMP: 2,3,6-trimethylphenold TeMP: Tetra-methyl phenol

[0201] As can be confirmed from the experimental data in Table 5 above, in the case of Example 3, the methylation reaction temperature was changed from 400°C to 450°C by starting at 400°C and increasing by 10°C every 3 hours, and it was confirmed that the catalytic performance increased according to the reaction temperature. In the case of Example 4, the nitrogen flow rate was changed, and through this, the effect on the contact time between the catalyst and the reactants (GHSV, Gas hourly space velocity) could be confirmed.

[0202] In the case of Example 5, the ratio of the input feed was changed, and through this, it was confirmed that there was an effect of the ratio of meta-cresol, which is a reactant, and methanol, which is an alkylation medium.

Claims

1. Contains magnesium oxide, Containing macropores having a diameter of 50 nm to 10,000 nm and mesopores having a diameter of 2 nm to 50 nm, BET surface area is 45 m 2 / g to 180 m 2 / g person, Ortho-alkylation reaction extrusion molding catalyst.

2. In paragraph 1, Regarding the total mixed volume of the above macropores and mesopores The above macropores are included in an amount of 1 to 10 vol%, The above mesopores are included at 90 to 99 vol%, Ortho-alkylation reaction extrusion molding catalyst.

3. In paragraph 1, The size of the above extruded catalyst is 0.5 mm to 6.0 mm, Ortho-alkylation reaction extrusion molding catalyst.

4. A method for manufacturing a catalyst according to paragraph 1, It has a bimodal pore structure and a BET surface area of ​​100 m 2 / g to 180 m 2 A first step of preparing a mixture of magnesium oxide, an organic binder and a solvent; and A second step comprising extruding the mixture, Method for producing an ortho-alkylation reaction extrusion molding catalyst.

5. In paragraph 4, The bimodal pore structure of the above magnesium oxide is A first pore having a diameter of 2 nm to 10 nm, and comprising a second pore having a diameter of 10 nm to 50 nm, Method for producing an ortho-alkylation reaction extrusion molding catalyst.

6. In paragraph 4, For 100 parts by weight of the above magnesium oxide, 0.1 to 20 parts by weight of organic binder resin, and Containing 50 to 200 parts by weight of solvent, Method for producing an ortho-alkylation reaction extrusion molding catalyst.

7. In paragraph 4, The organic binder comprises at least one selected from the group consisting of methyl cellulose, carboxymethyl cellulose, ethylene glycol, polyethylene glycol, polyphenylene oxide, glycerin, and propylene glycol. Method for producing an ortho-alkylation reaction extrusion molding catalyst.

8. In paragraph 4, The solvent is alcohol, water or a mixture thereof. Method for producing an ortho-alkylation reaction extrusion molding catalyst.

9. In paragraph 4, The above solvent is water, Method for producing an ortho-alkylation reaction extrusion molding catalyst.

10. In paragraph 4, The extrusion molding in step 2 above is performed using a single piston extruder. Method for producing an ortho-alkylation reaction extrusion molding catalyst.

11. In paragraph 4, After the extrusion molding of step 2 above, further comprising a drying and firing step, Method for producing an ortho-alkylation reaction extrusion molding catalyst.

12. In paragraph 11, The above drying is performed at 80°C to 120°C. Method for producing an ortho-alkylation reaction extrusion molding catalyst.

13. In paragraph 11, The above firing is performed at 300°C to 600°C. Method for producing an ortho-alkylation reaction extrusion molding catalyst.

14. A monomer composition comprising an ortho-alkylation reaction extrusion molding catalyst according to paragraph 1 and a meta-alkyl substituted phenolic monomer, Ortho-alkylation reaction composition.

15. Comprising an alkylation reaction of a monomer composition comprising a meta-alkyl substituted phenolic monomer in the presence of an ortho-alkylation reaction extrusion molding catalyst according to paragraph 1. A method for producing an ortho-alkylation reaction product.

Citation Information

Patent Citations

  • Catalyst and method for the alkylation ofhydroxyaromatic compounds

    KR1020040045497A

  • Method to improve catalytic activities by employing network-typed pore structure in formed-catalyst

    KR1020130066916A

  • Method for preparation of magnesium oxide architectures with meso-macro pores

    KR1020130126437A

  • Method for preparing an alkylation catalyst, and for ortho-alkylating hydroxyaromatic compounds; and related compositions

    US6261987B1

  • Orthoalkylation catalyst for phenol and process for producing orthoalkylated phenol with use thereof

    US6951966B1