Tire cord and manufacturing method thereof

The tire cord manufacturing method addresses the challenge of achieving high strength, modulus, and elongation by controlling the spinning process, resulting in a tire cord with improved mechanical properties for lightweight and durable tires.

WO2024225681A1PCT designated stage expired Publication Date: 2024-10-31KOLON INDUSTRIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005110
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-24
Filing Date
2024-04-17
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Current tire cords fail to simultaneously achieve high strength, high modulus, low shrinkage, and high elongation, making it difficult to produce lightweight tires with improved durability and fuel efficiency.

Method used

A tire cord manufacturing method using high-strength polyester yarn with a specific spinning process that controls the shear rate, polymer discharge rate, and spinning pack pressure to produce multifilaments with a denier range of 2.5 to 3.5, ensuring high tensile strength, modulus, and low shrinkage, while maintaining toughness and elongation.

Benefits of technology

The method results in a tire cord with enhanced mechanical properties, achieving high strength, high modulus, low shrinkage, and high elongation, thereby enabling weight reduction and improved tire performance, including reduced rolling resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005110_31102024_PF_FP_ABST
    Figure KR2024005110_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed in the present specification is a high-strength tire cord and a manufacturing method thereof, the tire cord, according to the ASTM D 885 standard test method, having a tenacity of 8.0 g / d or greater, LASE@2% of 1.1 g / d or greater, LASE@5% of 2.5 g / d or less and a toughness of 183 g / d.mm or greater, and satisfying a side wall indentation (SWI) of 3.6% or less.
Need to check novelty before this filing date? Find Prior Art

Description

Tire cord and its manufacturing method

[0001] The present invention relates to a tire cord using high-strength polyester yarn and a method for manufacturing the same.

[0002] As automobile performance continues to improve and road conditions improve, tires are required to maintain stability and durability during high-speed driving. Furthermore, considering environmental, energy, and fuel efficiency concerns, lightweight yet durable tires are in high demand. As one way to meet these demands, active research is being conducted on tire cords, which are used as rubber reinforcing materials in tires.

[0003] The tire cord is manufactured using industrial yarns, such as polyester yarn. Furthermore, ongoing research is being conducted to improve the mechanical properties of the polyester yarn, such as tensile strength and elongation, to enhance the physical properties of the tire cord.

[0004] Polyester yarn, a type of industrial yarn, can generally be manufactured by melting polyester chips, extruding the molten polyester using a spinneret to form filaments, cooling the semi-solidified filaments extruded from the spinneret, and then focusing, stretching, and winding the cooled filaments.

[0005] Currently, research is ongoing into methods for reducing the fineness of polyester tire cord (e.g., PET tire cord) to reduce the weight of tires. To achieve this weight reduction, three physical properties must be satisfied: modulus, toughness, and shrinkage. However, a method that satisfies all of the required physical properties of tire cord has not yet been developed. In other words, reducing the fineness of the tire cord reduces the pressure in the spinneret and spinneret, which reduces the toughness of the tire cord, making it impossible to achieve all the desired physical properties.

[0006]

[0007] In this specification, a tire cord using polyester having a wide range of finenesses can be provided that satisfies all of the characteristics of high strength, high modulus, low shrinkage and high elongation, and can realize a lightweight tire.

[0008] Additionally, in the present specification, a method for manufacturing the tire code may be provided.

[0009] In this specification, a polyester yarn comprising 90 mol% or more of polyethylene terephthalate is provided,

[0010] A tire cord can be provided that has a strength of 8.0 g / d or more, a LASE@2% of 1.1 g / d or more, a LASE@5% of 2.5 g / d or less, and a toughness of 183 g / d.mm or more, and satisfies a side wall indentation (SWI) value of 3.6% or less, according to the standard test method of ASTM D 885.

[0011] In the properties of the above tire code, the sidewall kerf may be measured by the following equation 1:

[0012] [Formula 1]

[0013] SWI (%) = [(D)-(C)] + [(A) - (B)]

[0014] In the above equation 1,

[0015] (A) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 20 to 45 g at 180°C for 2 minutes, with a specimen length of 250 mm), and then cooled for 1 minute.

[0016] (B) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 250 mm in length, 180°C, 2 minutes, and an initial tensile force (40 to 90 g)) and then cooled for 1 minute.

[0017] (C) is the elongation value of the above (A) specimen according to the standard test method of ASTM D 885 measured under a load of 1.5 to 3.0 kg,

[0018] (D) is the elongation value of the above (B) specimen according to the standard test method of ASTM D 885 measured under a load of 3.0 to 6.0 kg.

[0019] The above (A) may be 1.0 to 3.2%, the above (B) may be 0.7 to 2.8%, the above (C) may be 1.3 to 1.7%, and the above (D) may be 4.2 to 4.6%.

[0020] Additionally, the above tire code can have a strong utilization rate of 88% or more according to the following equation 2.

[0021] [Formula 2]

[0022] Tensile strength (%) = [Tensile strength of tire cord (g / d) / Tensile strength of polyester yarn (g / d)] Х100

[0023] The above tire code may include a high-tenacity polyester yarn made from a polyester multifilament including 200 to 2,000 polyester monofilaments having a fineness of 2.5 to 3.5 denier; and an adhesive layer impregnated into the high-tenacity polyester yarn.

[0024] The above polyester yarn can be manufactured from a molten polyester resin containing 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more.

[0025] Such polyester yarns may have a tensile strength of 7.5 to 11.0 g / d and an elongation of 10 to 20%.

[0026] The above tire cord may include a raw cord having a total fineness of 1000 to 6000 denier.

[0027]

[0028] In addition, the present specification provides a method for manufacturing a tire cord, comprising: a step of manufacturing a polyester yarn by spinning a molten polyester resin containing 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more using a spinning pack including a nozzle portion; a step of manufacturing a plied yarn using the polyester yarn; and a step of immersing the plied yarn in an adhesive solution and heat-treating the plied yarn.

[0029] More specifically, the step of manufacturing the polyester yarn may include a step of forming a polyester multifilament including a polyester monofilament having a fineness of 2.5 to 3.5 denier by ejecting the molten polyester resin through a nozzle including a nozzle having a shear rate of 220 to 260 1 / sec and a polymer ejection rate of 2.0 m / min or less under a spinneret pressure condition of 1800 to 2500 psi.

[0030] The tire cord provided according to the above tire cord manufacturing method has a strength of 8.0 g / d or more, a LASE@2% of 1.1 g / d or more, a LASE@5% of 2.5 g / d or less, and a toughness of 183 g / d.mm or more according to the standard test method of ASTM D 885, and can satisfy a side wall indentation (SWI) value of 3.6% or less.

[0031] The above polyester multifilament may comprise 200 to 2,000 polyester monofilaments having a fineness of 2.5 to 3.5 denier.

[0032] In addition, the step of manufacturing the polyester yarn may include a step of manufacturing a plurality of filaments by ejecting a molten polyester resin having an inherent viscosity of 1.0 dl / g or more through a nozzle unit having a shear rate of 220 to 260 1 / sec and a polymer ejection rate of 2.0 m / min or less under a spinneret pressure condition of 1800 to 2500 psi; a step of heating the ejected plurality of filaments through a heating unit; a step of cooling the heated plurality of filaments through a cooling unit; a step of converging the plurality of filaments to form a polyester multifilament; a step of drawing the polyester multifilament; and a step of winding the drawn multifilament.

[0033] The step of drawing the polyester multifilament may include a step of drawing the polyester multifilament at a total draw ratio of 1.0 to 3.0 times.

[0034]

[0035] According to the present invention, when manufacturing polyester yarn, a low DPF (Denier per filament) is applied, and a polymer discharge speed from a nozzle is controlled to impart high spinning tension and spinning draft, and at the same time, the discharge pressure from the spinning pack is set high to maintain a high shear rate from the nozzle, thereby maintaining excellent mechanical properties of polyester yarn in tire cord and satisfying all properties required for lightweighting.

[0036] Therefore, the present invention can provide a lightweight tire cord that satisfies high strength, high modulus, low shrinkage, and high elongation.

[0037]

[0038] Figure 1 is a schematic diagram of a yarn manufacturing device according to an embodiment of the present invention.

[0039] Hereinafter, tire cords and their manufacturing methods according to implementation examples of the present invention will be described in more detail.

[0040] Unless otherwise defined herein, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein is for the purpose of describing specific embodiments only and is not intended to be limiting.

[0041] As used herein, the singular forms also include the plural forms unless the context clearly dictates otherwise.

[0042] As used herein, the term "including" means specifying a particular characteristic, region, integer, step, operation, element and / or component, but does not exclude the presence or addition of other particular characteristics, regions, integers, steps, operations, elements, components and / or groups.

[0043] The present invention is susceptible to various modifications and takes various forms. Specific embodiments are illustrated and described in detail below. However, this is not intended to limit the present invention to specific disclosed forms, but rather to encompass all modifications, equivalents, and alternatives falling within the spirit and scope of the invention.

[0044] In this specification, when the positional relationship between two parts is described as, for example, ‘on top of’, ‘upper part of’, ‘lower part of’, ‘next to’, etc., one or more other parts may be located between the two parts unless the expression ‘right’ or ‘directly’ is used.

[0045] In this specification, when a temporal relationship is described as, for example, ‘after’, ‘following’, ‘next to’, or ‘before’, it may also include cases where it is not continuous, unless the expression ‘immediately’ or ‘directly’ is used.

[0046] In this specification, the term 'primarily twisted yarn' refers to a single yarn made by twisting one filament in one direction.

[0047] In this specification, the term 'plied yarn' means a yarn made by twisting two or more strands of plied yarn together in one direction, and is also referred to as 'raw-cord'.

[0048] In this specification, the term 'tire cord' means a plied yarn containing an adhesive so that it can be directly applied to a rubber product for tires, and is also referred to as a 'dip-cord'.

[0049]

[0050] According to one embodiment of the invention, a tire cord can be provided, which comprises a polyester yarn containing 90 mol% or more of polyethylene terephthalate, has a tenacity of 8.0 g / d or more, a LASE@2% of 1.1 g / d or more, a LASE@5% of 2.5 g / d or less, and a toughness of 183 g / d.mm or more according to the standard test method of ASTM D 885, and satisfies a side wall indentation (SWI) value of 3.6% or less.

[0051] The present inventors have devised a method for maintaining excellent mechanical properties of polyester yarn, such as tensile strength and elongation, by applying a high multifilament spinning method that satisfies spinning conditions of low denier per filament, low spindle discharge speed and low shear speed, and including polyester yarn manufactured by controlling the pressure of a spinning pack, and have experimentally confirmed that a high-strength tire cord capable of exhibiting high modulus, high toughness and stable shrinkage properties can be provided by including the polyester yarn according to this method, and have completed the invention.

[0052] Here, in this specification, DPF (Denier per filaments) means the denier value per polyester monofilament contained in the polyester yarn.

[0053]

[0054] Tire cord is manufactured through a three-step process of yarn manufacturing, yarn twisting, and heat treatment. To obtain a product with superior performance, the tire cord must maintain the yarn properties mentioned above.

[0055] That is, yarn undergoes post-processing, such as rolling and heat treatment, which can result in deterioration and changes in yarn properties. For example, strength and toughness may be reduced, and shrinkage and intermediate elongation may also change. Therefore, it is necessary to ensure that yarn properties are maintained even after undergoing these post-processing steps.

[0056] In addition, the required properties of tire cord for weight reduction of tires must satisfy all three properties of high modulus, high toughness, and low and stable shrinkage as tire cord to replace the existing fineness range.

[0057] At this time, the factor representing the modulus is LASE (Load At Specific Elongation), and the factor representing the shrinkage rate is Side Wall Indentation (SWI). In addition, for high toughness, the modulus needs to be controlled low above a certain range. In other words, even if the modulus is increased, it is necessary to prevent the deterioration of other physical properties such as toughness. For example, in the extension-load curve obtained by the ASTM D885 measurement method, control of LASE@5%, which is the size of the modulus determined by the load (g / d) at the elongation corresponding to 5%, is required.

[0058] However, while a tire cord satisfying all three of the above-mentioned material properties has not been developed in the past, the tire cord according to the above-mentioned embodiment exhibits high strength even after post-processing of the yarn, and satisfies excellent modulus, toughness, and shrinkage characteristics.

[0059] These tire cords can be provided including polyester yarns manufactured by controlling the pressure of the spinning pack together with a high multifilament spinning method.

[0060] Specifically, the above yarn manufacturing conditions use the above high multifilament spinning method, which means applying a low DPF (Denier per filament), a low nozzle discharge speed, and a low nozzle shear rate.

[0061] However, these manufacturing conditions may result in reduced pressure in the radiant pack / detention, which is associated with a reduction in the toughness of the tire cord.

[0062] That is, the high multifilament spinning method can exhibit high strength, high modulus, and stable shrinkage properties of tire cord, but it is associated with a decrease in toughness (elongation at break). This is because each property has a conflicting relationship, and therefore, conventional spinning methods cannot implement tire cord properties that satisfy all the desired properties.

[0063] Accordingly, in this specification, an invention is devised to maintain high toughness by applying a high multifilament spinning method with specific spinning conditions while simultaneously controlling the pressure of the spinning pack.

[0064] Additionally, the above toughness limits the modulus range at LASE@5% to a specific range.

[0065] The tire cord manufactured in the above manner can be used in a tire that achieves weight reduction and improves rolling resistance by satisfying all of the above-described high strength, high modulus, low shrinkage and high elongation while maintaining the inherent properties of the yarn.

[0066] That is, by implementing a Gauge down of the code fineness of the tire (changing from 2000De to 1500De, 3000De→2000De), rolling resistance can be improved.

[0067] In addition, according to the above implementation example, the tire properties that are reduced as the fineness of the tire cord is reduced can be improved.

[0068]

[0069] More specifically, the tire cord of the above embodiment may have a strength of 8.0 g / d or more, or 8.5 g / d or more, according to the standard test method of ASTM D 885, and may also have a strength of 11 g / d or less, or 10 g / d or less.

[0070] Additionally, the tire cord of the above embodiment may have a LASE@2% value according to the standard test method of ASTM D 885 indicating modulus of 1.1 g / d or more, or 1.15 g / d or more, or 1.20 g / d or more. Additionally, the LASE@2% value may be 1.5 g / d or less, or 1.45 g / d or less, or 1.4 g / d or less.

[0071] The above tire code may have a LASE@5% value of 2.5 g / d or less, or 2.45 g / d or less, or 2.4 g / d or less according to the standard test method of ASTM D 885. Additionally, the LASE@5% value may be 2.0 g / d or more, or 2.05 g / d or more, or 2.1 g / d or more.

[0072] The above tire cord may have a toughness of 183 g / d.mm or more, or 200 g / d.mm or more, or 210 g / d.mm or more according to the standard test method of ASTM D 885. In addition, the above tire cord may have a toughness of 300 g / d.mm or less, or 280 g / d.mm or less, or 250 g / d.mm or less according to the standard test method of ASTM D 885.

[0073] The above tire code may have a sidewall erosion (SWI) value of 3.6% or less, or 3.55% or less, or 3.4% or less, and may have a sidewall erosion (SWI) value of 3.0% or more, or 3.1% or more, or 3.2% or more, or 3.3% or more.

[0074] Additionally, the tire cord may have a toughness of 300 g / d.mm or less, or 280 g / d.mm or less, or 250 g / d.mm or less according to the standard test method of ASTM D 885.

[0075] Accordingly, the tire cord according to one embodiment may have a strength of 8.0 to 11 g / d, a LASE@2% of 1.1 to 1.5 g / d, a LASE@5% of 2.0 to 2.5 g / d, a toughness of 183 to 300 g / d.mm, and a sidewall etching (SWI) value of 3.0 to 3.6% according to the standard test method of ASTM D 885.

[0076]

[0077] At this time, in the properties of the tire code, the sidewall kerf may be measured by the following equation 1:

[0078] [Formula 1]

[0079] SWI (%) = [(D)-(C)] + [(A) - (B)]

[0080] In the above equation 1,

[0081] (A) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 20 to 45 g at 180°C for 2 minutes, with a specimen length of 250 mm), and then cooled for 1 minute.

[0082] (B) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 250 mm in length, 180°C, 2 minutes, and an initial tensile force (40 to 90 g)) and then cooled for 1 minute.

[0083] (C) is the elongation value of the above (A) specimen according to the standard test method of ASTM D 885 measured under a load of 1.5 to 3.0 kg,

[0084] (D) is the elongation value of the above (B) specimen according to the standard test method of ASTM D 885 measured under a load of 3.0 to 6.0 kg.

[0085] Additionally, the above (A) may be 1.0 to 3.2%, the above (B) may be 0.7 to 2.8%, the above (C) may be 1.3 to 1.7%, and the above (D) may be 4.2 to 4.6%.

[0086] In the present specification, the dry heat shrinkage rate before cooling of the above (A) and (B) may be measured using a shrinkage tester, which is the ratio of the length (L0) measured under an initial tension load selected from the above range after leaving a tire cord having a length of 250 mm as a specimen at 25°C and 65% RH for 24 hours, and the length (L1) after processing under the initial tension load at 180°C for 2 minutes. That is, the length change rate of the specimen {=[(L0-L1) / L0]X100} may be the dry heat shrinkage rate (L2). Each of the above L0 and L1 may be measured 5 times.

[0087] In addition, the dry heat shrinkage rate after the cooling can mean the length (L3) of the specimen cooled for 1 minute after the L2 measurement, and the length change rate of L2 and L3 ({=[(L2-L3) / L2]X100}). The cooling can be performed at room temperature.

[0088] In addition, the super-tensile loads of (A) and (B) and the loads of (C) and (D) can be measured by appropriately setting the load range within the above range according to the fineness of the tire cord without distinction of fineness.

[0089] That is, the above SWI is not limited to the range of fineness of the tire cord, and can be measured as an average value by appropriately adjusting the load range according to various fineness range conditions. Specifically, it can be defined and set as each load according to the fineness of the tire cord.

[0090] According to one embodiment of the invention, the fineness of the tire cord may include raw cord having a total fineness of 1000 to 6000 denier. Furthermore, the superload range may be set according to the total fineness of the raw cord included in the tire cord set according to the yarn manufacturing conditions.

[0091] Accordingly, according to an embodiment of the present specification, when the total fineness of the tire cord is set to a range of 3000 denier and 4000 denier, the super tensile load of (A) may be 35 to 45 g, the super tensile load of (B) may be 70 to 90 g, the load of (C) may be 2.3 to 3.0 kg, and the load of (D) may be 4.6 to 6.0 kg.

[0092]

[0093] More specifically, when the fineness of the tire cord is set to 2000 denier, 2600 denier, 3000 denier, and 4000 denier, the super tensile load for measuring the dry heat shrinkage rate of (A) above may be 20 g, 30 g, 35 g, and 45 g, respectively.

[0094] The super tensile load for measuring the dry heat shrinkage of (B) under each of the above denier conditions may be 40 g, 60 g, 70 g, and 90 g, respectively.

[0095] Additionally, the load of (C) under each of the above denier conditions can be 1.5 kg, 2.0 kg, 2.3 kg, and 3.0 kg.

[0096] Additionally, the load of (D) under each of the above denier conditions can be 3.0 kg, 4.0 kg, 4.6 kg, and 6.0 kg.

[0097] Additionally, the above dry heat shrinkage rate may be an average value of values ​​measured at least 3 times, 4 times, or 5 times or more under the above load range.

[0098]

[0099] The above tire code may have a strip strength of 0.94 kg / dm / denier or more.

[0100] Specifically, the reinforcing capacity of a tire within a given area is crucial to its performance. Furthermore, strip strength based on fineness is crucial for weight reduction. Higher strip strength results in superior reinforcing capacity.

[0101] Therefore, high-strength cords must be used to ensure excellent tire reinforcing capabilities, and the distance between cords must be optimized to increase density.

[0102] Accordingly, the tire cord of the present invention can improve tire performance by exhibiting a high strip strength value of 0.94 kg / dm / denier or more.

[0103] More specifically, the strip strength can be defined as strength in a certain area, and in the present invention, it can mean performance in fabric within a tire.

[0104] The above strip strength can be obtained by measuring the strength (kg / dm) per decimeter (10 cm). In addition, the above strip strength can be expressed as strength when the above strength is converted to a value per denier (kg / dm / denier).

[0105] In addition, in the present invention, the fabric may be a double-twisted yarn (i.e., a low-cord) made by immersing a polyester yarn in an adhesive solution and heat-treating the double-twisted yarn (i.e., a deep-cord).

[0106] According to one preferred embodiment of the invention, the strip strength of the tire cord may be calculated by taking into account the strength and the density of the denier of the fabric contained in the cord and may be 0.94 kg / dm / denier or more.

[0107]

[0108] The above tire cord may have a tensile strength of 7.5 to 9.5 g / d and an elongation of 14 to 22% according to the standard test method of ASTM D 885.

[0109] Additionally, the tire code may have a strength utilization rate of 88% or more according to the following equation 2.

[0110] [Formula 2]

[0111] Tensile strength (%) = [Tensile strength of tire cord (g / d) / Tensile strength of polyester yarn (g / d)] Х100

[0112] Specifically, the tire cord may exhibit a strength utilization ratio of 88.5% or more, or 88.6% or more, or 88.7% or more, or 88.8% or more, or 88.9% or more; and 91.0% or less, or 90.8% or less, or 90.6% or less, or 90.4% or less. Accordingly, the tire cord according to the present specification may have excellent strength.

[0113] Preferably, the tire cord can exhibit a strength utilization ratio of 88.5% to 91.0%, or 88.5% to 90.8%, or 88.6% to 90.8%, or 88.6% to 90.6%, or 88.7% to 90.6%, or 88.7% to 90.4%, or 88.8% to 90.4%, or 88.9% to 90.4%.

[0114] More specifically, the strength utilization rate of the tire cord may be at least 90% of the strength of the yarn.

[0115]

[0116] The above tire code may include a high-tenacity polyester yarn made from a polyester multifilament comprising 200 to 2,000 polyester monofilaments having a fineness of 2.5 to 3.5 denier; and an adhesive layer impregnated into the high-tenacity polyester yarn.

[0117] Specifically, the polyester yarn including the polyester multifilament may have a single yarn fineness of 2.5 to 3.5 denier and a total fineness of 500 to 3000 denier, or 1000 to 2000 denier.

[0118] The adhesive layer may be included in an amount of 0.5 to 10 parts by weight, or 1 to 8 parts by weight, or 1.5 to 6 parts by weight relative to 100 parts by weight of the high-strength polyester yarn.

[0119] Additionally, the polyester yarn can be manufactured from a molten polyester resin containing 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more.

[0120] According to one embodiment of the invention, the polyester yarn can be manufactured into a polyethylene terephthalate drawn yarn through a spinning process using chips composed of 90 mol% or more of polyethylene terephthalate (hereinafter, PET).

[0121] Specifically, the PET drawn yarn is manufactured by melt spinning the PET to produce undrawn yarn, and then drawing the undrawn yarn. In addition, the PET drawn yarn can be double-twisted and dipped in an adhesive to produce a tire cord in the form of a dip cord.

[0122] In addition, the PET drawn yarn according to one embodiment of the invention contains at least 90 mol% of PET to exhibit properties suitable for tire cord. If the PET drawn yarn contains less than 90 mol% of PET, it is difficult for the PET drawn yarn and the tire cord produced therefrom to exhibit desirable properties. Therefore, the term "PET" in the present invention refers to a case where PET is at least 90 mol% without any special explanation.

[0123] Such polyester yarns may have a tensile strength of 7.5 to 11.0 g / d and an elongation of 10 to 20%.

[0124]

[0125] The above tire code includes a raw cord made by twisting two or more strands of the above polyester elongated yarn together in one direction, and an adhesive attached to the raw cord.

[0126] The above polyester elongated yarn may have a single yarn fineness of 2.5 to 3.5 denier and a total fineness of 500 to 3000 denier.

[0127] The above tire cord may include a raw cord having a total fineness of 1000 to 6000 denier.

[0128] Preferably, the tire cord may comprise the low-cord having a total fineness of 1000 denier to 6000 denier, or 1000 denier to 5000 denier.

[0129] Additionally, the tire cord may be a 2-ply yarn comprising the polyester elongated yarn. As a non-limiting example, the low-cord may have a total fineness of 1000 denier to 6000 denier by 2-plying the polyester elongated yarn having a single yarn fineness of 2.5 to 3.5 denier and a total fineness of 500 to 3000 denier.

[0130] Specifically, in one example, a low-cord can be manufactured by feeding the polyester filament into a cable cord yarn and twisting and over-twisting it at a twist count of 200 to 500 TPM. A tire cord (dip-cord) can be manufactured by dipping the low-cord in an adhesive coating solution, followed by drying and heat treatment.

[0131] Meanwhile, according to another embodiment of the invention, a method for manufacturing a tire cord may be provided, comprising the steps of: manufacturing a polyester yarn by spinning a molten polyester resin containing 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more using a spinneret having a nozzle portion; manufacturing a plied yarn using the polyester yarn; and immersing the plied yarn in an adhesive solution and heat-treating it; wherein the step of manufacturing the polyester yarn comprises the step of forming a polyester multifilament including a polyester monofilament having a fineness of 2.5 to 3.5 denier by ejecting the molten polyester resin through a spinneret including a nozzle portion having a shear rate of 220 to 260 1 / sec and a polymer ejection rate of 2.0 m / min or less under a pressure condition of the spinneret of 1800 to 2500 psi.

[0132] Specifically, in order to manufacture tire cords that satisfy all of the above requirements of high strength, high modulus, low shrinkage, and high elongation, it is desirable to apply a low DPF to the polyester yarn. However, in the present specification, in addition to the low DPF for the polyester, high spinning tension and spinning draft can be imparted by controlling the polymer discharge speed from the nozzle.

[0133] In addition, since the toughness of the yarn and tire cord may decrease due to low nozzle discharge pressure under the above yarn manufacturing conditions, the present specification has the feature of setting the discharge pressure in the spinning pack high to maintain a high shear rate at the nozzle.

[0134] Therefore, in this specification, by controlling the spinning conditions and maintaining the spinning pack pressure within a certain range, the properties of the polyester yarn are excellently maintained in the tire cord even after the yarn undergoes post-processing processes of twisting and heat treatment, thereby satisfying all the properties of the tire cord required for lightweighting. In this case, the tire cord can be manufactured by a conventional method, except for controlling the spinning method and the pressure conditions of the spinning pack during the production of the polyester yarn.

[0135]

[0136] More specifically, as described above, high-tenacity polyester yarn for tire cord can be manufactured by spinning a molten polyester resin having an inherent viscosity of 1.0 dl / g or more using a spinneret including a nozzle portion.

[0137] In one example, the molten polyester resin may include a molten polyethylene terephthalate resin comprising 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more, or 1.1 dl / g to 1.9 dl / g. Preferably, the molten polyethylene terephthalate resin may have an inherent viscosity of 1.0 dl / g or more, or 1.1 dl / g or more. In addition, the molten polyethylene terephthalate resin may have an inherent viscosity of 1.7 dl / g or less, or 1.6 dl / g or less, or 1.5 dl / g or less, or 1.4 dl / g or less.

[0138] Additionally, the molten polyethylene terephthalate resin may contain 90 mol% or more, 92 mol% or more, 95 mol% or more, 99 mol% or more, or 100 mol% of polyethylene terephthalate as a main component.

[0139] Additionally, various known additives can be added during the preparation of the PET polymer constituting the microfilament. Therefore, the types of additives are not limited.

[0140] Additionally, the radiation can be carried out in a radiation chamber having an odd number of holes of 300 to 550 at a temperature of 270 to 300°C, or 275 to 300°C, or 275 to 290°C.

[0141] In addition, the step of manufacturing the polyester yarn may include, after the step of manufacturing the plurality of filaments, a step of heating and cooling the plurality of discharged filaments, concentrating the cooled filaments and then stretching them to manufacture a polyester drawn yarn, and then winding them up.

[0142] Preferably, the method for manufacturing the polyester yarn may include the steps of: producing a plurality of filaments by ejecting a molten polyester resin having an inherent viscosity of 1.0 dl / g or more through a nozzle unit having a shear rate of 220 to 260 1 / sec and a polymer ejection speed of 2.0 m / min or less under a spinneret pressure condition of 1800 to 2500 psi; heating the ejected plurality of filaments through a heating unit; cooling the heated plurality of filaments through a cooling unit; converging the plurality of filaments to form a polyester multifilament; drawing the polyester multifilament; and winding the drawn multifilament.

[0143] For example, the high-tenacity polyester yarn can be manufactured through a manufacturing method including: a step of melting a polyethylene terephthalate resin (e.g., PET chip) containing 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more, or 1.1 dl / g or more, or 1.5 dl / g or more and ejecting it into a plurality of filaments through a nozzle unit by controlling spinning conditions and a spinning pack pressure under the above-described range conditions; a step of heating the plurality of ejected filaments through a heating unit positioned around the nozzle unit; a step of cooling the plurality of heated filaments through a cooling unit; a step of converging the plurality of filaments to form a polyester multifilament; a step of drawing the polyester multifilament; and a step of winding the drawn multifilament.

[0144] At this time, the above-mentioned radiation pack can adjust the discharge pressure range to 1800 to 2500 psi (approximately 126.55 to 175.8 kgf / cm2). If the discharge pressure of the above-mentioned radiation pack is less than 1800 psi, the polymer discharge speed from the nozzle may decrease, and the required performance may not be achieved. If it is more than 2500 psi, equipment problems such as pack leaks may occur due to excessive pressure.

[0145] In addition, when discharging the molten polyester resin through the nozzle section, the shear rate at the nozzle may be 220 to 260 1 / sec. If the shear rate is less than 220 1 / sec, the orientation of the polymer at the nozzle may decrease, which may lower the toughness of the yarn, and if the shear rate is more than 260 1 / sec, the dimensional stability value of the yarn may be affected due to a decrease in the spin draft.

[0146] In addition, the polymer discharge speed at the nozzle can be adjusted to be 2.0 m / min or less along with the shear rate control at the nozzle. More specifically, the polymer discharge speed at the nozzle can be 0.1 to 2.0 m / min, or 0.5 to 2.0 m / min, or 1 to 2.0 m / min, or 1 to 1.9 m / min, or 1.3 to 1.9 m / min, or 1.5 to 1.9 m / min. If the polymer discharge speed is 2 m / min or more, the polymer discharge speed at the nozzle may decrease, and the required performance may not be exhibited.

[0147] Through this process, a polyester multifilament including a polyester monofilament having a fineness of 2.5 to 3.5 denier can be formed. That is, according to the present specification, it means forming a polyester multifilament including a polyester monofilament having a DPF of 2.5 to 3.5 De / ea.

[0148] Additionally, the polyester multifilament may comprise 200 to 2,000, or 400 to 1,200, polyester monofilaments having a fineness of 2.5 to 3.5 denier. More specifically, the fineness of the polyester monofilament may be 2.6 to 3.5 denier, or 2.7 to 3.4 denier.

[0149] The polyester yarn including the above polyester multifilament may have a total fineness of 500 to 3000 denier, or 1000 to 2000 denier.

[0150]

[0151] Meanwhile, in the method for manufacturing the polyester yarn, the method of heating and cooling a plurality of ejected filaments, concentrating the cooled filaments and then drawing them to manufacture a polyester drawn yarn, and then winding them up can be performed by a conventional method.

[0152] In addition, as illustrated in FIG. 1, the manufacturing device (1) of the polyester yarn according to the embodiment of the present invention includes an extruder (10), a spinning pack (20), a cooling unit (30), a focusing unit (40), a stretching unit (50), and a winder (60).

[0153] A hopper (12) is formed on the upper surface of the extruder (10) to receive polymer chips, and a heating device and a conveying device are provided inside the extruder (10) to melt the polymer chips supplied through the hopper (12) and convey the molten resin to the spinneret (20). As the resin, a polyester resin may be used, but is not limited thereto. Hereinafter, for the convenience of explanation, a yarn manufacturing device (1) capable of manufacturing polyester yarn using a polyester resin will be described as an example. However, the yarn manufacturing device (1) according to an embodiment of the present invention is not only used for manufacturing polyester yarn, but may also be used for manufacturing other yarns known in the art.

[0154] In addition, the above-mentioned spin pack (20) forms a plurality of filaments (2) by ejecting molten polyester resin transferred from the extruder (10). The above-mentioned spin pack (20) may include a spin block, a pack body, a cap, and a heating unit, and its shape is not limited.

[0155] More specifically, the apparatus for manufacturing the polyester yarn may include a spinneret including a nozzle unit having a plurality of discharge holes formed therein for discharging a molten resin; a heating unit positioned around the nozzle unit for heating a plurality of filaments discharged through the plurality of discharge holes; a cooling unit for cooling the plurality of filaments heated by the heating unit; a focusing unit for converging the plurality of filaments cooled in the cooling unit to form a multifilament; and a drawing unit for drawing the multifilament. The plurality of discharge holes may be arranged in a circle in at least two rows. The distance between adjacent discharge holes in any one row, the distance between adjacent discharge holes in any other row, and the distance between discharge holes positioned close to each other in any one row and any other row adjacent to the any one row may be the same.

[0156] In this specification, the cooling unit (30) can use a general filament cooling method, and the method is not limited.

[0157]

[0158] For example, as illustrated in FIG. 1, in this specification, the refrigerant may be introduced into the cooling chamber (32) through the refrigerant inlet (34) and may be discharged from the cooling chamber (32) through the refrigerant outlet (36).

[0159] In addition, the high-tenacity polyester yarn for the tire cord can be manufactured through a manufacturing method including a step of drawing an undrawn multifilament (4) at least two or more times by including three or more godet rollers (52, 54, 56, 58). At this time, the at least three godet rollers include first, second, and third godet rollers sequentially arranged based on the moving direction of the multifilament, and the rotation speed of the first godet roller can be 2000 to 4000 m / min and the rotation speed of the third godet roller can be 5000 to 7000 m / min.

[0160] The step of drawing the polyester multifilament may include a step of drawing the polyester multifilament at a total draw ratio of 1.0 to 3.0 times, and a polyester drawn yarn may be manufactured through the method.

[0161] Preferably, the total draw ratio may be 1.5 to 3.0 times, or 1.5 to 2.5 times. That is, in order to increase the degree of orientation through drawing and thereby exhibit an appropriate level of strength, the total draw ratio of the polyester drawn yarn is preferably 1.0 times or more. However, in order to prevent breakage due to excessive drawing, the total draw ratio of the polyester drawn yarn is preferably 3.0 times or less.

[0162] In addition, the multi-stage elongation speed ratio can be defined as the ratio of the difference between the rotation speed of the first godet roller and the rotation speed of the second godet roller, and the difference between the rotation speed of the second godet roller and the rotation speed of the third godet roller, and at this time, the multi-stage elongation speed ratio can be 30:70 to 60:40.

[0163] At this time, the radiation draft may be 1500 to 2000.

[0164] In the winder (60), the multifilament drawn in the drawing section (50) is wound to produce polyester yarn (6).

[0165] The high-strength polyester yarn manufactured according to the above method can have a tensile strength of 7.5 to 11.0 g / d and an elongation of 10 to 20%.

[0166]

[0167] Meanwhile, the step of manufacturing a plied yarn using the polyester yarn may be a step of manufacturing a low-cord by twisting and top-twisting the polyester drawn yarn under certain twist conditions.

[0168] Specifically, in one example, the low-code can be manufactured by feeding the polyester elongated yarn into a cable cord twisting machine and twisting and over-twisting it at a twist count of 200 TPM to 500 TPM.

[0169] In addition, the step of immersing the above-mentioned compound in an adhesive solution and heat-treating it may be a step of manufacturing a tire cord (dip-cord) by immersing the low-code in an adhesive solution and then drying and heat-treating it.

[0170] Specifically, the adhesive layer can be formed by impregnating the above-mentioned compound with a commonly known adhesive solution, and the adhesive solution can be one used for the production of a conventional tire cord, for example, a Resorcinol Formaldehyde-Latex (RFL) adhesive solution.

[0171] After impregnating the adhesive solution, a heat treatment process may be performed. The heat treatment process may be performed at a temperature of 220 to 260°C for 90 to 360 seconds, preferably at a temperature of 230 to 250°C for 90 to 240 seconds, and more preferably at a temperature of 240 to 245°C for 90 to 120 seconds.

[0172] By immersing the above high-strength polyester yarn in an adhesive solution and heat-treating it under these conditions, the dimensional stability of the tire cord can be further improved, and changes in physical properties during tire curing can be further reduced.

[0173]

[0174] Hereinafter, the present invention will be described in more detail through examples and comparative examples. However, the following examples and comparative examples are provided solely to aid understanding of the present invention and are not intended to limit the scope of the present invention.

[0175] [Examples and Comparative Examples: Manufacturing of Polyester Yarn]

[0176] <Examples 1 to 3>

[0177] Using the yarn manufacturing device (1) illustrated in Fig. 1, a polyester yarn (6) made of polyethylene terephthalate (PET) having a single filament fineness of 2.7 to 3.4 denier (d) and a total fineness of 1500 denier (d) was manufactured.

[0178] Specifically, PET chips containing 90 mol% PET and having an intrinsic viscosity (IV) of 1.0 to 1.4 dl / g were melted in a single-screw extruder to produce a molten polyester resin. Thereafter, as described in Table 1 below, the molten polyester resin was spun at a spinning speed of 3200 m / min through a spindle (170) (L / D = 4.0 / 1.0, number of discharge holes: 500) to produce a plurality of filaments (2).

[0179] At this time, the conditions for manufacturing multiple filaments, including the passage speed of the detention, were adjusted as shown in Table 2 (DPF, polymer discharge speed at nozzle, shear rate at nozzle, spinning pack pressure).

[0180] Afterwards, the plurality of filaments (2) were heated through a heating unit, the plurality of filaments (2) were cooled in a cooling unit (30), and the cooled filaments (2) were concentrated to manufacture a multifilament (4) (undrawn yarn) in an undrawn state.

[0181] The above-mentioned melt for spinning was extruded through a spinneret to obtain a polyester drawn yarn having a total fineness of 1000 denier (single yarn fineness of approximately 4 denier). The process for obtaining the above-mentioned polyester drawn yarn was carried out under a spinning temperature of 290°C, a spinning speed of 3200 m / min, a total draw ratio of 1.5 times, and a relaxation rate of 1.5% (heat treatment at 180°C after drawing).

[0182] The above-mentioned stretched multifilament was wound to produce a polyester yarn (stretched yarn).

[0183]

[0184] <Comparative Examples 1 and 2, Reference Example 1>

[0185] Polyester yarn was manufactured in the same manner as in Example 1, except that the detention diameter, odd number, spinning conditions and spinneret pressure were changed as shown in Tables 1 and 2.

[0186] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Reference Example 1 Spinning Speed ​​(mpm) 3 200 3 200 3 200 3 200 2 500 3 100 Final Fineness (De') 1 500 1 500 1 500 1 500 1 500 Winding Speed ​​(mpm) 5 6 20 6 000 5 6 20 6 000 7 000 5 500 Dia. (mm) 1 1 1 1 1 Number of Holes 5 0 5 5 0 4 5 6 0 0 6 5 0 3 8 4 Spinning Draft 1 8 5 1 1 9 0 8 1 6 4 8 2 0 8 1 1 5 1 0 1 4 0 8 Total Max. Draft 3 9 6 3 4 0 8 3 3 5 2 7 4 5 5 4 1 3 6 3 1 1 0

[0187] Conditions DPF Nozzle Polymer Discharge Velocity Nozzle Shear Velocity Spinning Pack Discharge Pressure Unit De / eam / min1 / spsi Example 13.01.72302200 Example 22.71.72241800 Example 33.41.92592500 Comparative Example 12.51.52051600 Comparative Example 22.31.72211400 Reference Example 13.92.22942200

[0188] [Examples 4 to 6, Comparative Examples 3 to 4 and Reference Example 1: Production of tire cords] Using the polyester yarns produced in Examples 1 to 3, Comparative Examples 1 to 2 and Reference Example 1, tire cords of Examples 4 to 6, Comparative Examples 3 to 4 and Reference Example 2 were produced under the same conditions, respectively.

[0189] Specifically, polyester yarn was fed into a cable cord twisting machine, and two strands of a lower twist yarn (Z-direction) having a twist count of 460 TPM were prepared, and then these two strands of lower twist yarns were twisted together (S-direction) at a twist count of 460 TPM to produce a plied yarn (raw-cord). The plied yarn thus produced was immersed in an adhesive coating solution containing resorcinol-formaldehyde-latex (RFL), dried at 150°C for 100 seconds, and heat-treated at 240°C for 100 seconds to produce a tire cord (dip-cord). The tension applied to the raw-cord during the immersion, drying, and heat-treatment processes was 0.5 kg / cord.

[0190] Additionally, the total fineness of the above-mentioned lo-code showed a denier of 1000 to 6000.

[0191] However, the tire code of Comparative Example 6 using Comparative Example 3 could not be manufactured, so its properties could not be measured.

[0192]

[0193] [Experimental Example 1: Evaluation of the Physical Properties of Polyester Yarn and Tire Cord]

[0194] Tensile strength and elongation, etc. were measured for the polyester yarns manufactured in the above examples, comparative examples, and reference examples, and tire cords using the same.

[0195]

[0196] Tensile strength, elongation at break and intermediate elongation

[0197] According to the standard test method of ASTM D 885, the tensile strength (g / d), elongation, and strength utilization ratio according to Equation 2 of polyester oriented yarn and tire cord were measured using a universal testing machine from Instron, and the results are shown in Tables 3 and 4. The specimen length was 250 mm, the tensile speed was 300 mm / min, and the initial load was set to 0.05 g / d.

[0198] In the Stress-Strain curve obtained from the above test, the elongation at a load of 4.5 g / d was expressed as ‘intermediate elongation.’

[0199] [Formula 2]

[0200] Tensile strength (%) = [Tensile strength of tire cord (g / d) / Tensile strength of polyester yarn (g / d)] × 100

[0201] Tensile strength (g / d) Intermediate elongation @ 4.5 kgf (%) Elongation (%) Example 19.8 5.1 12.0 Example 29.9 5.0 11.8 Example 39.7 5.3 12.4 Comparative Example 110.1 4.7 10.6 Comparative Example 2---Reference Example 19.4 5.6 13.1

[0202] Tensile strength (g / d) Intermediate elongation @ 4.5 kgf (%) Elongation (%) High strength utilization (%) Example 4 8.8 2.8 18.0 90 Example 5 8.9 2.7 17.6 90 Example 6 8.7 2.9 18.4 90 Comparative example 3 9.1 2.7 16.2 90 Comparative example 4 --- 90 Reference example 28.5 3.5 17.1 90

[0203] Referring to Tables 3 and 4 above, the polyester yarns of Examples 1 to 4 and the tire cords of Examples 4 to 6 using the same all exhibited excellent physical properties at an equivalent level or higher compared to the comparative examples and reference examples.

[0204] [Experimental Example 2: Evaluation of Tire Cord Properties]

[0205] The strength, modulus, toughness, and SWI properties of the tire cords manufactured in the above examples, comparative examples, and reference examples were measured. The results are shown in Table 5.

[0206]

[0207] (1) Tenacity and toughness

[0208] According to the standard test method of ASTM D 885, the strength, tensile strength (g / d), elongation (%), and toughness of tire cords were measured using an Instron universal testing machine. The specimen length was 250 mm (cord length: 600 mm), the tensile speed was 300 mm / min, and the initial load was set to 0.05 g / d.

[0209]

[0210] (2) Modulus (Lase@2%, LASE@5%)

[0211] Stress-strain curves were obtained for each tire cord according to the standard test method of ASTM D 885. Using these stress-strain curves, the loads at 2% and 5% longitudinal strain were determined, and the elongation values, LASE@2% and LASE@5%, were measured.

[0212] Before measurement, the sample was left in an atmosphere of 20℃ and 65% RH for 24 hours and then measured.

[0213]

[0214] (3) Side Wall Indentation (SWI)

[0215] Using equipment from Testrite, UK, SWI was measured according to Equation 1 below.

[0216] [Formula 1]

[0217] SWI (%) = [(D)-(C)] + [(A) - (B)]

[0218] In the above equation 1,

[0219] (A) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 20 to 45 g at 180°C for 2 minutes, with a specimen length of 250 mm), and then cooled for 1 minute.

[0220] (B) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 250 mm in length, 180°C, 2 minutes, and an initial tensile force (40 to 90 g)) and then cooled for 1 minute.

[0221] (C) is the elongation value of the above (A) specimen according to the standard test method of ASTM D 885 measured under a load of 1.5 to 3.0 kg,

[0222] (D) is the elongation value of the above (B) specimen according to the standard test method of ASTM D 885 measured under a load of 3.0 to 6.0 kg.

[0223] In addition, the above (A) is 1.0 to 3.2%, the above (B) is 0.7 to 2.8%, the above (C) is 1.3 to 1.7%, and the above (D) is 4.2 to 4.6%.

[0224] Specifically, for 2500 mm of specimens having a total fineness of 1000 to 6000 denier, the length (L0) was measured under an initial tensile load of 0.01 g / d after leaving the specimen at 25°C and 65% RH for 24 hours. Thereafter, the specimen was treated under an initial tensile load of 0.01 g at 180°C for 2 minutes using the shrinkage rate measuring device, and the length (L1) of the specimen was measured. The L0 and L1 were each measured three times. The length change rate of the specimen {=[(L0-L1) / L0]X100} was defined as the dry heat shrinkage rate (L2) before cooling.

[0225] In addition, using the shrinkage rate measuring device, after measuring the dry heat shrinkage rate of the above specimen, the specimen was taken out of the device under the same load, left at room temperature (25°C) for about 1 minute, and the dry heat shrinkage rate was measured while the code was stable. That is, the dry heat shrinkage rate after cooling is measured by measuring the length (L3) of the specimen that was cooled for 1 minute after the L2 measurement, and represents the length change rate of L2 and L3 ({=[(L2-L3) / L2]X100}).

[0226]

[0227] PropertyTenacityLASE@2%LASE@5%ToughnessSWIUnitg / dg / dg / dg / d.mm%Example48.81.32.3194.03.4Example58.91.42.4196.73.3Example68.71.22.2191.73.5ComparativeExample39.11.42.7181.73.7ComparativeExample4-----ReferenceExample28.51.02.3175.03.5

[0228] Referring to Table 5, the tire cords of Examples 4 to 6 have a strength of 8.0 g / d or more, a LASE@2% of 1.1 g / d or more, a LASE@5% of 2.5 g / d or less, and a toughness of 183 g / d.mm or more, and all satisfy a SWI value of 3.6% or less. That is, the tire cords of Examples 4 to 6 maintain excellent strength even after the post-processing process of the yarn, while exhibiting high modulus, low shrinkage, and high elongation effects, thereby showing better results than Comparative Examples 3 to 4 and Reference Example 2.

[0229] In comparison, Comparative Example 3, although exhibiting a certain strength, showed lower modulus and toughness than the examples and SWI of 3.7%, showing poor results overall. In addition, Comparative Example 4 was unable to manufacture tire cord.

[0230] In addition, Reference Example 2 had a low toughness value of 175.0 g / d.mm because the radiation draft was lower than the original range and the DPF was high at 3.9. In addition, Reference Example 2 had a LASE@2% value of 1.0%, which was lower than that of the examples, limiting the improvement in modulus.

[0231]

[0232] (4) Strip strength

[0233] For the tire code of Example 6 above, the strip strength was measured based on 1500 De (yarn density 118ea / decimeter, load 26.1kg) according to Table 6 below.

[0234] Specifically, the cord within the tire may have a warp density of 118 ea / decimeter when the cord has a strength of 8.0 g / d or more based on 1500 denier. Accordingly, the strip strength may be calculated using the density value of the tire cord under a given load.

[0235] At this time, the strip strength was measured even when the strength (i.e., strength) of the tire code was 8.0 g / d.

[0236] (Example 6) 1500De EPDMKg / dm / denier3079.8 / 3000=1.02662832 / 3000=0.944Strip Strength / Denier

[0237] As shown in Table 6 above, the strip strength of the tire cord of Example 6 (strength 8.7 g / d) and having a strength of 8.0 g / d satisfies 0.94 kg / dm / denier or more, so that the strength of the fabric within the tire cord is excellent, and thus a high-strength tire can be provided. Therefore, when manufacturing yarn to provide a tire cord, the pressure of the spinning pack must be controlled while applying a high multifilament spinning method with specific spinning conditions, so that all properties can be excellent and, in particular, the toughness can be maintained high.

[0238]

[0239] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above implementation examples, and includes all changes that can be easily modified and deemed equivalent by a person having ordinary skill in the art to which the invention pertains from the embodiments of the present invention.

[0240]

[0241] [Explanation of symbols]

[0242] 1: Yarn manufacturing device

[0243] 2: Multiple filaments

[0244] 4: Unstretched multifilament

[0245] 6: Polyester yarn

[0246] 10: Extruder

[0247] 12: Hopper

[0248] 20: Radiation Pack

[0249] 30: Cooling section

[0250] 32: Cooling chamber

[0251] 34: Refrigerant inlet

[0252] 36: Refrigerant outlet

[0253] 40: Focus

[0254] 50: Extension Department

[0255] 52, 54, 56, 58: Godet Roller

[0256] 60: Winder

Claims

Comprising a polyester yarn containing 1.90 mol% or more of polyethylene terephthalate, It has a strength of 8.0 g / d or more, a LASE@2% of 1.1 g / d or more, a LASE@5% of 2.5 g / d or less, and a toughness of 183 g / d.mm or more, according to the standard test method of ASTM D 885, and satisfies the Side Wall Indentation (SWI) value of 3.6% or less. Tire code.

2. In paragraph 1, The above sidewall kerf is measured by the following equation 1, tire code: [Formula 1] SWI (%) = [(D)-(C)] + [(A) - (B)] In the above equation 1, (A) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 20 to 45 g at 180°C for 2 minutes, with a specimen length of 250 mm), and then cooled for 1 minute. (B) is the dry heat shrinkage measured using a shrinkage tester (measured under a load of 250 mm in length, 180°C, 2 minutes, and an initial tensile force (40 to 90 g)) and then cooled for 1 minute. (C) is the elongation value of the above (A) specimen according to the standard test method of ASTM D 885 measured under a load of 1.5 to 3.0 kg, (D) is the elongation value of the above (B) specimen according to the standard test method of ASTM D 885 measured under a load of 3.0 to 6.0 kg.

3. In paragraph 2, The above (A) is 1.0 to 3.2%, The above (B) is 0.7 to 2.8%, The above (C) is 1.3 to 1.7%, The above (D) is a tire code of 4.2 to 4.6%.

4. In paragraph 1, The above tire code has a strip strength of 0.94 kg / dm / denier or more, Tire code.

5. In paragraph 1, The above tire code is a tire code having a strength utilization rate of 88% or more according to the following formula 2. [Formula 2] Tensile strength (%) = [Tensile strength of tire cord (g / d) / Tensile strength of polyester yarn (g / d)] Х100 6. In paragraph 1, The above tire code is a high-tenacity polyester yarn made from polyester multifilament comprising 200 to 2,000 polyester monofilaments having a fineness of 2.5 to 3.5 denier; and A tire cord comprising an adhesive layer impregnated into the high-strength polyester yarn.

7. In paragraph 6, A tire cord, wherein the polyester yarn comprises at least 90 mol% of polyethylene terephthalate and is manufactured from a molten polyester resin having an inherent viscosity of at least 1.0 dl / g.

8. In paragraph 6, The above polyester yarn is a tire cord having a tensile strength of 7.5 to 11.0 g / d and an elongation of 10 to 20%.

9. In paragraph 1, The tire cord comprises a raw cord having a total fineness of 1000 to 6000 denier.

10. A step of manufacturing polyester yarn by spinning a molten polyester resin containing 90 mol% or more of polyethylene terephthalate and having an inherent viscosity of 1.0 dl / g or more using a spinning pack including a nozzle portion; A step of manufacturing a plied yarn using the above polyester yarn; and A step of heat-treating the above-mentioned compound by immersing it in an adhesive solution; The step of manufacturing the above polyester yarn is: A step of forming a polyester multifilament including a polyester monofilament having a fineness of 2.5 to 3.5 denier by ejecting the molten polyester resin through a nozzle part having a shear rate of 220 to 260 1 / sec and a polymer ejection rate of 2.0 m / min or less under a spinneret pressure condition of 1800 to 2500 psi, A method for manufacturing the tire cord of Article 1.

11. In paragraph 10, A method for manufacturing a tire cord, wherein the polyester multifilament comprises 200 to 2,000 polyester monofilaments having a fineness of 2.5 to 3.5 denier.

12. In paragraph 10, The step of manufacturing the above polyester yarn is: A step of manufacturing a plurality of filaments by ejecting a molten polyester resin having an inherent viscosity of 1.0 dl / g or more through a nozzle section having a shear rate of 220 to 260 1 / sec and a polymer ejection rate of 2.0 m / min or less under a spinneret pressure condition of 1800 to 2500 psi; A step of heating the plurality of filaments discharged above through a heating unit; A step of cooling the above-described plurality of heated filaments through a cooling unit; A step of forming a polyester multifilament by focusing the plurality of filaments; A step of drawing the above polyester multifilament; and A step of winding the above-mentioned extended multifilament; A method for manufacturing a tire cord including:

13. In paragraph 10, The step of drawing the polyester multifilament includes a step of drawing the polyester multifilament at a total draw ratio of 1.0 to 3.0 times. Method for manufacturing tire cord.

Citation Information

Patent Citations

  • Pneumatic tire

    JP2021187211A

  • Poly(ethyleneterephthalate) drawn fiber, poly(ethyleneterephthalate) tire-cord and method for manufacturing thereof

    KR1020130079257A

  • Method for improving productivity of synthetic fibers using partial heating of spinneret

    KR1020170088148A

  • Polyester tire code with improved heat resistance and tire comprising the same

    KR102227153B1

  • Target holding apparatus for test of howitzer fuze

    KR102487888B1