Method for manufacturing mg / tial composite with three-dimensional interconnected structure by using liquid metal dealloying, and mg / tial composite manufactured thereby
The method of using a Ti-X precursor alloy in a Mg molten metal, followed by Ti porous structure creation and immersion in Mg-Al alloy, addresses the inefficiencies in adding aluminum to the molten metal decomposition method, resulting in Mg/TiAl composite materials with enhanced hardness and properties.
Patent Information
- Application Number
- PCT/KR2024/005463
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
The existing molten metal decomposition method faces challenges in efficiently manufacturing Mg/TiAl composite materials due to the rapid reduction in reaction speed when aluminum is added as an alloy element, which is miscible with both the precursor alloy and the molten metal, leading to incomplete decomponentization and reduced physical properties.
A method involving a precursor alloy of Ti-X, where X is a metal miscible with Ti, immersed in a molten metal containing Mg, followed by removal of the Mg base material to create a Ti porous structure, and subsequent immersion in a Mg-Al alloy molten metal to achieve a three-dimensional continuous Mg/TiAl composite structure with enhanced properties.
This method allows for the efficient production of Mg/TiAl composite materials with improved hardness, up to twice that of traditional methods, and complete decomponentization without residual copper, resulting in a bi-continuous structure with excellent physical properties.
Smart Images

Figure KR2024005463_31102024_PF_FP_ABST
Abstract
Description
Method for manufacturing Mg / TiAl composite material having a three-dimensional continuous structure using a metal melt decomposition method and Mg / TiAl composite material manufactured thereby
[0001] The present invention relates to a method for manufacturing a Mg / TiAl composite material, and more specifically, to a method for manufacturing a Mg / TiAl composite material having a three-dimensional continuous structure using liquid metal dealloying (LMD).
[0002] Liquid metal dealloying (LMD) is a new dealloying method that was first reported to the academic world in 2011. It is known as the only dealloying method for producing three-dimensional continuous structures of non-precious metals because the process is simple and fast and oxidation can be suppressed during manufacturing.
[0003] The principle of molten metal decomposition is based on the selective reaction between a precursor alloy and the molten metal. When a precursor alloy is added to the molten metal, only the elements that are highly miscible with the precursor alloy diffuse into the molten metal, resulting in selective dissolution. The remaining insoluble elements self-organize into a three-dimensional, continuously connected structure through interfacial diffusion. Simultaneously, the molten metal fills the void left by the loss of the highly miscible elements, forming a composite material with a three-dimensional, continuously connected structure in which the two phases are infinitely connected. Furthermore, when the manufactured composite material is placed in an etching solution that selectively corrodes only one phase, a porous structure is formed consisting of the non-corroded phase. Composites manufactured by molten metal decomposition have a matrix-matrix structure in which the two metals are intertwined in a three-dimensional, continuously connected structure, and possess a nanoscale microstructure, resulting in excellent chemical and physical properties. However, to further improve the properties of the material, a process of adding alloying elements is required.
[0004] For example, to increase the strength of magnesium (Mg) / titanium (Ti) composites manufactured using the molten metal decomposition method, the addition of additional alloying elements is necessary. Aluminum (Al) is highly reactive with Ti, so adding it as an alloying element to Mg / Ti composites results in the formation of TiAl, which has high strength. Furthermore, Al has a low density and is less expensive than Mg and Ti, making it an ideal additive for the production of lightweight, high-strength composites.
[0005] To manufacture high-strength Mg / TiAl composites using the molten metal decomposition process, one option is to add Al alloying elements to a TiCu precursor alloy or to the molten Mg. However, if the added alloying elements are miscible with both the precursor alloy and the molten metal, the decomposition process speed will drastically decrease.
[0006] The technical problem to be solved by the present invention is to provide a method for manufacturing a Mg / TiAl composite material that is difficult to manufacture by a common metal melt decomposition method of alloying a precursor or a molten metal with aluminum (Al), and to provide a Mg / TiAl composite material that exhibits improved properties according to the addition of aluminum, and a Mg / TiAl composite material manufactured thereby.
[0007] In order to achieve the technical problem as described above, the present invention provides a method for producing a Mg / TiAl composite material, including the steps of (a) immersing a precursor alloy (Ti-X) including a metal (X) that is miscible with titanium (Ti) and is dissolved into a molten metal containing magnesium (Mg) to produce a Mg / Ti composite material, (b) producing a titanium (Ti) porous structure from the Mg / Ti composite material, and (c) producing a Mg / TiAl composite material by immersing the titanium (Ti) porous structure in a Mg-Al alloy molten metal (Fig. 1).
[0008]
[0009] In the above step (a), when a molten metal containing magnesium (Mg) is prepared and the precursor alloy (Ti-X) is immersed in the molten metal, selective dissolution occurs in which only metals (X) having high miscibility with the molten metal among the elements forming the precursor alloy diffuse into the molten metal and escape, while titanium (Ti), which is another component forming the precursor alloy and is insoluble in the molten metal, self-organizes a three-dimensional continuous connection structure through interfacial diffusion.
[0010] As a result of the dissolution of metal X into the molten metal and the self-organization of titanium (Ti) as described above, a void is formed at the interface where the precursor alloy and the molten metal come into contact, and the magnesium molten metal from which metal X is dissolved is filled into the void, so that the dissolution of metal X and the filling of the molten metal gradually progress from the surface of the precursor alloy to the inside, and ultimately, an Mg / Ti composite material including a matrix made of magnesium or a magnesium alloy and a matrix made of titanium or a titanium alloy is obtained.
[0011] Meanwhile, the metal X included in the precursor alloy is not particularly limited in type as long as it is a metal that has a negative enthalpy of mixing with magnesium and is miscible with magnesium. For example, the metal X may be copper (Cu), nickel (Ni), zinc (Zn), gallium (Ga), germanium (Ge), arsenic (As), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), indium (In), tin (Sn), antimony (Sb), platinum (Pt), gold (Au), mercury (Hg), lead (Pb), or bismuth (Bi). That is, the precursor alloy may be a Ti-Cu alloy, a Ti-Ni alloy, a Ti-Zn alloy, a Ti-Ga alloy, a Ti-Ge alloy, a Ti-As alloy, a Ti-Rh alloy, a Ti-Pd alloy, a Ti-Ag alloy, a Ti-Cd alloy, a Ti-In alloy, a Ti-Sn alloy, a Ti-Sb alloy, a Ti-Pt alloy, a Ti-Au alloy, a Ti-Hg alloy, a Ti-Pb alloy, or a Ti-Bi alloy.
[0012]
[0013] Next, in the step (b), a titanium (Ti) porous structure is manufactured by removing a matrix made of magnesium or a magnesium alloy from the previously manufactured Mg / Ti composite material.
[0014] The method for removing the matrix made of magnesium or a magnesium alloy from the Mg / Ti composite is not particularly limited, and for example, a titanium (Ti) porous structure can be manufactured by immersing the Mg / Ti composite in a solution containing an acid such as nitric acid that is highly corrosive to magnesium or a magnesium alloy and then maintaining the solution for a predetermined period of time to remove the matrix made of magnesium or a magnesium alloy.
[0015]
[0016] Next, when the titanium (Ti) porous structure manufactured in the step (c) is immersed in the Mg-Al alloy molten metal, the liquid Mg-Al alloy molten metal fills the gap between the solid Ti skeleton structures, and aluminum (Al) atoms, which have a much higher miscibility with titanium (Ti) than with magnesium (Mg), rapidly diffuse and move from the liquid Mg-Al alloy molten metal to the surface of the solid Ti skeleton structures. Accordingly, the titanium (Ti) matrix gradually changes from pure Ti or Ti alloy → Ti with Al element dissolved → TiAl → TiAl, and the matrix made of magnesium or a magnesium alloy and titanium or a titanium alloy with Al dissolved or Ti x Al y A three-dimensional continuously connected Mg / TiAl composite material is obtained, in which the matrix composed of a second phase is infinitely connected to form a bi-continuous structure.
[0017]
[0018] Furthermore, in another aspect of the present invention, there is provided a Mg / TiAl composite material manufactured according to the above manufacturing method, wherein the Mg / TiAl composite material has a hardness that is at most two times higher than that of a Mg / Ti composite material manufactured through a conventional metal melt decomposition method.
[0019] According to the method for manufacturing a Mg / TiAl composite material according to the present invention, by removing a magnesium matrix from a Mg / Ti composite material manufactured through a molten metal decomposition (LMD) method and then performing aluminum alloying using a Mg-Al alloy molten metal, a Mg / TiAl composite material having a three-dimensional continuous structure with excellent physical properties can be manufactured in a short period of time without any residual elements such as copper (Cu) contained in the precursor alloy.
[0020] Figure 1 is a process flow diagram illustrating each step of a method for manufacturing a Mg / TiAl composite material having a three-dimensional continuous connection structure using a metal melt decomposition method according to the present invention.
[0021] Figure 2 is a schematic diagram showing a process for manufacturing a composite material using a metal melt decomposition method in Examples 1 and 2 of the present invention and Comparative Examples 1 to 3.
[0022] Figure 3 is a scanning electron microscope (SEM) photograph of the surface and the center of the Mg / TiAl composite material specimens manufactured in Examples 1 and 2 and Comparative Examples 2 and 3 of the present invention.
[0023] Figure 4 shows scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) results for the Mg / TiAl composite material manufactured in Examples 1 and 2 of the present invention and the Mg / Ti composite material manufactured in Comparative Example 1.
[0024] Figure 5 shows scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) results of a Mg / TiAl composite material according to the time of the Al alloying process (process 3) of the present invention.
[0025] Figure 6 shows the results of measuring the hardness of the Mg / Ti composite material manufactured in Comparative Example 1 of the present invention and the Mg / TiAl composite material according to the time of the Al alloying process (process 3) of the example.
[0026] In describing the present invention, if it is determined that a detailed description of a related known function or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.
[0027]
[0028] Embodiments according to the concept of the present invention may be modified in various ways and take various forms. Therefore, specific embodiments are illustrated in the drawings and described in detail in this specification or application. However, this is not intended to limit embodiments according to the concept of the present invention to specific disclosed forms, and it should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are included.
[0029]
[0030] The terminology used herein is for the purpose of describing specific embodiments only and is not intended to limit the present invention. The singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a described feature, number, step, operation, component, part, or combination thereof, but do not preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0031]
[0032] Hereinafter, the present invention will be described in more detail by way of examples.
[0033]
[0034] The embodiments described herein may be modified in various ways, and the scope of this specification is not to be construed as limited to the embodiments described below. The embodiments described herein are provided to more fully explain this specification to those of ordinary skill in the art.
[0035]
[0036] In this embodiment, as illustrated in FIG. 2, Mg / TiAl composite materials (Examples 1 and 2) manufactured by the method for manufacturing a three-dimensional continuous-connection structure Mg / TiAl composite material according to the present invention described above, an Mg / Ti composite material (Comparative Example 1) manufactured using a TiCu precursor and pure magnesium (Mg) melt according to a conventional metal melt decomposition method, an Mg / TiAl composite material (Comparative Example 2) manufactured using a precursor alloy (TiCuAl) to which aluminum (Al) was added and pure magnesium (Mg) melt, and an Mg / TiAl composite material (Comparative Example 3) manufactured using a TiCu precursor and magnesium (Mg) melt to which aluminum (Al) was added were manufactured, and the microstructure of each of the composite materials was observed and the mechanical properties were measured for comparison.
[0037]
[0038] <Example 1>
[0039] TiCu precursor alloy (Ti 30 Cu 70 ) was placed in a pure Mg molten metal at 800°C for 30 minutes to produce a Mg / Ti composite material (Process 1), which was placed in a nitric acid (HNO3) solution for 24 hours to produce a Ti porous structure (Process 2), which was then placed in a Mg-3Al (wt%) molten metal at 800°C for 10 seconds and then taken out to produce a Mg / TiAl composite material (Process 3).
[0040]
[0041] <Example 2>
[0042] TiCu precursor alloy (Ti 30 Cu 70 ) was charged into a pure Mg molten metal at 800°C for 30 minutes to produce a Mg / Ti composite material (process 1), which was then charged into a nitric acid (HNO3) solution for 24 hours to produce a Ti porous structure (process 2), which was then charged into a Mg-3Al (wt%) molten metal at 800°C for 1 hour and then taken out to produce a Mg / TiAl composite material (process 3).
[0043]
[0044] <Comparative Example 1>
[0045] According to the conventional general metal melt decomposition method, TiCu precursor alloy (Ti 30 Cu 70 ) was charged into pure Mg molten metal at 800°C for 30 minutes to produce a Mg / Ti composite material.
[0046]
[0047] <Comparative Example 2>
[0048] A method for manufacturing a Mg / TiAl composite material by alloying aluminum (Al) with a TiCu precursor, comprising: manufacturing a TiCuAl precursor alloy ((Ti) by adding Al to a TiCu alloy 30 Cu 70 ) 97 Al3) was charged into pure Mg molten metal at 800°C for 30 minutes to manufacture a Mg / TiAl composite material.
[0049]
[0050] <Comparative Example 3>
[0051] A method for manufacturing a Mg / TiAl composite material by alloying aluminum (Al) with molten magnesium (Mg), comprising: a TiCu precursor alloy (Ti 30 Cu 70 ) was charged into a Mg-3Al (wt%) molten metal at 800°C for 1 hour to produce a Mg / TiAl composite material.
[0052]
[0053] Figure 3 is a scanning electron microscope (SEM) photograph of the surface and the center of the Mg / TiAl composite material specimens manufactured in Examples 1 and 2 and Comparative Examples 2 and 3 of the present invention.
[0054]
[0055] Referring to Fig. 3, in Comparative Example 2, as Al was added to the precursor alloy, the LMD reaction rate of the precursor in the Mg molten metal rapidly decreased, and even after 1 hour of LMD treatment, the Cu element of the precursor was not completely dealloyed, and thus remained as an Mg2Cu phase on both the surface and the center of the manufactured composite material. Therefore, dedifferentiation did not occur completely, and the Mg / TiAl composite material could not be manufactured.
[0056]
[0057] In addition, in Comparative Example 3, as with Comparative Example 2, the LMD reaction rate decreased rapidly as Al was added to the Mg molten metal, and thus, despite 1 hour of LMD treatment, the dealloying of the Cu element did not proceed completely, and a large amount of 49.6 wt% of Cu remained in the center of the manufactured composite. On the other hand, the concentration of Al in the composite was very low, less than 0.5 wt%. Therefore, the dealloying decreased rapidly, and the Mg / TiAl composite could not be manufactured.
[0058]
[0059] On the other hand, in the composite material manufactured by charging the Ti porous structure manufactured by charging in the nitric acid solution in Example 1 into the Mg-3Al (wt%) molten metal for 10 seconds, no Cu exists in the center, indicating a complete decomposition state. The composite material is composed of a TiAl matrix in which an α-Ti phase and a Ti3Al phase coexist with a small amount of Al dissolved in Ti, and an α-Mg matrix in which a small amount of Al is dissolved, and the size of each matrix is also fine. In addition, the composite material has a uniform structure with almost no microstructural difference between the surface and the center. Therefore, it was confirmed that it is possible to manufacture an Mg / TiAl composite material having a three-dimensional continuous structure with complete decomposition of Cu and high strength.
[0060]
[0061] In addition, the composite material manufactured by immersing the Ti porous structure in the Mg-3Al (wt%) molten metal in Example 2 for 1 hour shows that Cu is completely decomposed. The manufactured composite material is composed of a TiAl matrix in which Ti3Al phase and TiAl phase coexist and an α-Mg matrix in which a small amount of Al is dissolved, and the Al concentration of the composite material is very high, at 20 wt% or more. In addition, as in Example 1, the composite material has a uniform structure with almost no microstructural difference between the surface and the center. Therefore, it was confirmed that it is possible to manufacture an Mg / TiAl composite material having a three-dimensional continuous structure with complete decomposition of Cu and high strength.
[0062]
[0063] Figure 4 shows scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) results for the Mg / TiAl composite material manufactured in Examples 1 and 2 of the present invention and the Mg / Ti composite material manufactured in Comparative Example 1.
[0064]
[0065] Referring to Fig. 4, it was confirmed that the Mg / Ti composite material manufactured in Comparative Example 1 achieved complete decomposition of Cu, was composed of an Mg matrix and a Ti matrix, and had an area fraction of the Ti matrix and the Mg matrix at a ratio of 7:3.
[0066]
[0067] In the case of the Mg / TiAl composite material manufactured in Example 1, it can be seen that complete decomposition of Cu was achieved, and that it was composed of a TiAl matrix and an α-Mg matrix in which α-Ti and Ti3Al phases coexist. In addition, the size of the Ti matrix was finer than that of the Mg / Ti composite material manufactured in Comparative Example 1, and the area fraction of the TiAl matrix and the α-Mg matrix was confirmed to have an ideal 5:5 ratio.
[0068] In the Mg / TiAl composite material manufactured in Example 2, complete decomposition of Cu was achieved, and it was confirmed that the composite material consisted of a TiAl matrix and an α-Mg matrix in which Ti3Al and TiAl phases coexisted. In addition, the size of the Ti matrix was coarser than that of the Mg / Ti composite material manufactured in Comparative Example 1, and the area fraction of the TiAl matrix and the α-Mg matrix was found to have a ratio of 7:3.
[0069]
[0070] Figure 5 shows scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) results of a Mg / TiAl composite material according to the time of the Al alloying process (process 3) of the present invention.
[0071] In the manufacturing of Mg / TiAl composites in Examples 1 and 2 of the present invention, as the time for charging the Ti porous structure into the Mg-3Al (wt%) molten metal in the Al alloying process of Process 3 increased, the concentration of Al in the composite increased, and a phase change such as α-Ti → Ti3Al → TiAl occurred in the Ti matrix. After 1 hour of performing the Al alloying process, most of the TiAl matrix changed to the TiAl phase, and the size of the TiAl matrix increased as the process time increased.
[0072]
[0073] Figure 6 shows the results of measuring the hardness of the Mg / Ti composite material manufactured in Comparative Example 1 of the present invention and the Mg / TiAl composite material according to the time of performing the Al alloying process (process 3) of the example.
[0074] Referring to Fig. 6, as the Al alloying process time increased, the hardness of the Mg / TiAl composite material increased. In addition, when compared with the Mg / Ti composite material of Comparative Example 1 manufactured by the existing metal melt decomposition method, the Mg / TiAl composite materials according to Examples 1 and 2 manufactured through the present invention showed a hardness increase of 1.2 times or more when the process 3 time was 10 seconds or longer, and a hardness increase of 2.0 times or more when the process time was 1 hour or longer.
[0075]
[0076] While the embodiments of the present invention have been described above with reference to the attached drawings, those skilled in the art will appreciate that the present invention can be implemented in other specific forms without altering the technical spirit or essential characteristics thereof. Therefore, the embodiments described above should be understood to be illustrative in all respects and not restrictive.
[0077] According to the present invention, a Mg / TiAl composite material having a three-dimensional continuous connection structure and excellent physical properties can be manufactured within a short period of time.
Claims
1. (a) A step of manufacturing a Mg / Ti composite material by immersing a precursor alloy (Ti-X) containing a metal (X) that is miscible with titanium (Ti) and is dissolved into the molten metal, into a molten metal containing magnesium (Mg); (b) a step of manufacturing a titanium (Ti) porous structure from the above Mg / Ti composite material; and (c) a step of manufacturing a Mg / TiAl composite material by immersing the titanium (Ti) porous structure in a Mg-Al alloy molten metal; A method for manufacturing a Mg / TiAl composite material including:
2. In paragraph 1, In the above step (a), A method for producing a Mg / TiAl composite material, characterized in that the precursor alloy is selected from the group consisting of a Ti-Cu alloy, a Ti-Ni alloy, a Ti-Zn alloy, a Ti-Ga alloy, a Ti-Ge alloy, a Ti-As alloy, a Ti-Rh alloy, a Ti-Pd alloy, a Ti-Ag alloy, a Ti-Cd alloy, a Ti-In alloy, a Ti-Sn alloy, a Ti-Sb alloy, a Ti-Pt alloy, a Ti-Au alloy, a Ti-Hg alloy, a Ti-Pb alloy, and a Ti-Bi alloy.
3. In paragraph 2, In the above step (a), A method for manufacturing an Mg / TiAl composite material, characterized in that a Ti-Cu alloy is immersed in a molten metal made of magnesium (Mg), copper is eluted into the molten metal, and the molten metal fills the pores formed in the precursor alloy by the eluted copper, thereby forming an Mg / Ti composite material.
4. In paragraph 1, In the above step (b), A method for producing a Mg / TiAl composite material, characterized in that the Mg / Ti composite material is immersed in an acid solution to remove magnesium or a magnesium alloy from the Mg / Ti composite material, thereby producing a titanium (Ti) porous structure.
5. In paragraph 1, In the above step (c), A method for producing a Mg / TiAl composite material, characterized in that the above titanium (Ti) porous structure is immersed in a Mg-3 wt% Al alloy molten metal to produce a Mg / TiAl composite material.
6. In paragraph 1, (a) A precursor alloy (Ti) containing titanium (Ti) and copper (Cu) in an atomic ratio of 30:70 in a molten metal composed of magnesium (Mg) 30 Cu 70 ) to manufacture a Mg / Ti composite material; (b) a step of immersing the Mg / Ti composite material in a nitric acid (HNO3) aqueous solution to remove magnesium or magnesium alloy from the Mg / Ti composite material and produce a titanium (Ti) porous structure; and (c) a step of manufacturing a Mg / TiAl composite material by immersing the titanium (Ti) porous structure in a Mg-3 wt% Al alloy molten metal for 10 seconds to 2 hours; A method for manufacturing a Mg / TiAl composite material, characterized in that it includes .
7. A Mg / TiAl composite material manufactured by a manufacturing method according to any one of claims 1 to 6.
Citation Information
Patent Citations
Method for manufacturing metal member
JP2018178207A
Porous metal
JP2020125523A
Magnesium-based composite material having ti particles dispersed therein, and method for production thereof
KR1020100092969A
Light emitting device, polycyclic compound for the same, and display device including the light emitting device
KR1020240150607A
Metal member manufacturing method, and metal member
WO2011092909A1