Method for manufacturing metal composite through liquid metal dealloying using molten mg-ca alloy and ti-based precursor alloy, and metal composite manufactured thereby

The use of a Mg-Ca alloy in the molten metal decomposition method accelerates the decomponentization of metal composite materials like Mg/Ti, improving their physical properties by enhancing the miscibility and distribution of elements, thus addressing the inefficiencies of conventional methods and achieving faster production with improved material quality.

WO2024225723A1PCT designated stage expired Publication Date: 2024-10-31KYUNGPOOK NAT UNIV IND ACADEMIC COOP FOUND +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005465
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-23
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The conventional molten metal decomposition method for manufacturing metal composite materials, such as Mg/Ti, is inefficient due to slow decomponentization, leading to increased process time and deterioration of physical properties as the precursor alloy thickness increases, resulting in coarsening of the Ti phase and reduced productivity.

Method used

The method involves using a Mg-Ca alloy molten metal with a precursor alloy like Ti-X, where calcium promotes the decomponentization of highly miscible elements like Cu, reducing the process time and improving the physical properties by increasing the volume fraction of the Mg matrix and refining the Ti phase through solid solution strengthening.

Benefits of technology

This approach significantly shortens the manufacturing time of metal composite materials like Mg/Ti while maintaining or improving their physical properties, achieving a faster production rate and enhanced mechanical and chemical properties by optimizing the miscibility and distribution of elements within the composite structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005465_31102024_PF_FP_ABST
    Figure KR2024005465_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a method for manufacturing a Mg / Ti composite, and a metal composite manufactured thereby, the method immersing, in a molten metal that contains (Mg) and calcium (Ca), a precursor alloy (Ti-X) that contains titanium (Ti) and a metal (X), which is miscible with the molten metal so as to be dissolved into the molten metal, wherein the Ca alloy element, which is included in a molten Mg-Ca alloy, is highly miscible with Cu so as to promote dealloying behavior by which Cu is dissolved into the molten metal, thereby greatly reducing process time, is dissolved in Mg matrix so as to increase the volume fraction of the Mg matrix in the composite, and reduces the coarsening rate of Ti and, simultaneously, improves the strength of the composite through solid-solution strengthening of the Mg matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Method for manufacturing a metal composite material through a metal melt decomposition method using a Mg-Ca alloy melt and a Ti-based precursor alloy, and a metal composite material manufactured thereby

[0001] The present invention relates to a method for manufacturing a metal composite material including magnesium and titanium, and more particularly, to a method for manufacturing a metal composite material including magnesium and titanium having a three-dimensional continuous structure using liquid metal dealloying (LMD).

[0002] Liquid metal dealloying (LMD) is a new dealloying method that was first reported to the academic world in 2011. It is known as the only dealloying method for producing three-dimensional continuous structures of non-precious metals because the process is simple and fast and oxidation can be suppressed during manufacturing.

[0003] The principle of the metal melt decomposition method is to utilize the selective reaction between the precursor alloy and the molten metal. When the precursor alloy is added to the molten metal, only the elements that make up the precursor alloy that are highly miscible with the molten metal diffuse into the molten metal and escape, which is called selective dissolution. The remaining insoluble elements of the precursor alloy self-organize into a three-dimensional continuous structure through interfacial diffusion. At the same time, the empty space left by the escaped highly miscible elements is filled with the molten metal, forming a composite material with a three-dimensional continuous structure in which the two phases are infinitely connected.

[0004] Furthermore, when the manufactured composite material is placed in an etching solution that selectively corrodes only one phase, a porous structure composed of the non-corroded phase is formed. Composites manufactured by the metal melt decomposition method have a matrix-matrix structure in which two metal materials are intertwined in a three-dimensional continuous structure, and possess a fine structure at the nano- or micro-scale, resulting in excellent chemical and physical properties.

[0005] Meanwhile, when manufacturing composite materials using molten metal decomposition, the thicker the precursor alloy sample used, the more rapidly the decomposition reaction reaches the center of the sample. This slow decomposition process not only increases the required process time and reduces productivity, but also causes the coarsening of the insoluble element phase in the precursor alloy, degrading the properties of the resulting composite.

[0006] For example, when manufacturing an Mg / Ti composite by charging a Ti-Cu precursor alloy into a pure Mg melt according to a conventionally known metal melt decomposition method, as the thickness of the charged Ti-Cu precursor increases, it takes a long time to completely decompose even the Cu in the center of the precursor to manufacture an Mg / Ti composite, and in the process, coarsening occurs, which increases the size of the Ti phase, and the properties of the manufactured Mg / Ti composite deteriorate.

[0007] Accordingly, in order to improve the process efficiency of the molten metal decomposition method and to enhance the properties of the resulting composite material, a method is required that can manufacture a composite material in a short period of time by promoting the decomposition of elements that are highly miscible with the molten metal in the precursor.

[0008] The technical problem to be solved by the present invention is to provide a method for manufacturing a metal composite material at a significantly faster rate than a conventional metal melt decomposition method without causing a deterioration in the physical properties of the metal composite material ultimately obtained, and a metal composite material manufactured thereby.

[0009] In order to achieve the technical task as described above, the present invention provides a method for producing a metal composite material, which comprises the step of producing a Mg / Ti composite material by immersing a precursor alloy (Ti-X) containing a metal (X) that is miscible with titanium (Ti) and is dissolved into the molten metal, into a molten metal containing magnesium (Mg) and calcium (Ca).

[0010]

[0011] In order to manufacture a Mg / Ti composite material, a molten Mg-Ca alloy containing magnesium (Mg) and calcium (Ca) is prepared, and when the precursor alloy (Ti-X) is immersed in the molten metal, only the metal (X) having a high miscibility with the molten metal among the elements forming the precursor alloy diffuses into the molten metal and escapes, thereby causing selective dissolution, while titanium (Ti), which is another component forming the precursor alloy and is insoluble in the molten metal, self-organizes into a three-dimensional continuous structure through interfacial diffusion.

[0012] As a result of the dissolution of metal X into the molten metal and the self-organization of titanium (Ti) as described above, a void is formed at the interface where the precursor alloy and the molten metal come into contact, and the Mg-Ca alloy molten metal from which metal X is dissolved is filled into the void, so that the dissolution of metal X and the filling of the molten metal gradually progress from the surface to the inside of the precursor alloy, and ultimately, an Mg / Ti composite material including a matrix made of Mg matrix in which Ca is dissolved and a matrix made of titanium or a titanium alloy is obtained.

[0013] At this time, Ca added to the molten metal has a high miscibility with the metal X, and thus promotes the decomposition behavior in which the metal element X escapes into the molten metal, thereby significantly shortening the process time for manufacturing Mg / Ti composite materials. In addition, Ca added to the molten metal is dissolved in the Mg matrix, thereby increasing the volume fraction of the Mg matrix in the composite material and reducing the coarsening rate of Ti, and at the same time exhibits the effect of improving the strength of the composite material through solid solution strengthening of the Mg matrix.

[0014] Meanwhile, the metal X included in the precursor alloy is not particularly limited in type as long as it is a metal that has a negative enthalpy of mixing with titanium, magnesium, and calcium and is miscible with titanium, magnesium, and calcium, and for example, the metal X may be copper (Cu), nickel (Ni), zinc (Zn), gallium (Ga), germanium (Ge), arsenic (As), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), indium (In), tin (Sn), antimony (Sb), iridium (Ir), platinum (Pt), gold (Au), mercury (Hg), lead (Pb), or bismuth (Bi). That is, the precursor alloy may be a Ti-Cu alloy, a Ti-Ni alloy, a Ti-Zn alloy, a Ti-Ga alloy, a Ti-Ge alloy, a Ti-As alloy, a Ti-Rh alloy, a Ti-Pd alloy, a Ti-Ag alloy, a Ti-Cd alloy, a Ti-In alloy, a Ti-Sn alloy, a Ti-Sb alloy, a Ti-Ir alloy, a Ti-Pt alloy, a Ti-Au alloy, a Ti-Hg alloy, a Ti-Pb alloy, or a Ti-Bi alloy.

[0015] In addition, the calcium (Ca) content in the molten metal containing the magnesium (Mg) and calcium (Ca) is not particularly limited, and may include, for example, 10 wt% or less of calcium (Ca).

[0016]

[0017] Furthermore, the present invention provides a method for manufacturing an Mg / TiAl composite material to which aluminum (Al) is added as an alloying element in order to further improve the properties of the Mg / Ti composite material manufactured as described above, the method comprising the steps of (a) manufacturing an Mg / Ti composite material by immersing a precursor alloy (Ti-X) including a metal (X) that is miscible with titanium (Ti) and is eluted into the Mg-Ca alloy molten metal, into an Mg-Ca alloy molten metal including magnesium (Mg) and calcium (Ca), (b) manufacturing a titanium (Ti) porous structure from the Mg / Ti composite material, and (c) manufacturing an Mg / TiAl composite material by immersing the titanium (Ti) porous structure into an Mg-Al alloy molten metal.

[0018]

[0019] Since the above step (a) is the same as the method for manufacturing the Mg / Ti composite material described above, its description is omitted.

[0020]

[0021] In the above step (b), a titanium (Ti) porous structure is manufactured by removing a matrix made of magnesium or a magnesium alloy from the Mg / Ti composite material manufactured in the previous step.

[0022] The method for removing a matrix made of magnesium alloy from a Mg / Ti composite material is not particularly limited, and for example, a titanium (Ti) porous structure can be manufactured by immersing the Mg / Ti composite material in a solution containing an acid such as nitric acid that is highly corrosive to magnesium alloy and then maintaining the solution for a predetermined period of time to remove the matrix made of magnesium alloy.

[0023]

[0024] Next, when the titanium (Ti) porous structure manufactured in the step (c) is immersed in the Mg-Al alloy molten metal, the liquid Mg-Al alloy molten metal fills the gap between the solid Ti skeleton structures, and aluminum (Al) atoms, which have a much higher miscibility with titanium (Ti) than with magnesium (Mg), rapidly diffuse and move from the liquid Mg-Al alloy molten metal to the surface of the solid Ti skeleton structures. Accordingly, the titanium (Ti) matrix gradually changes from pure Ti or Ti alloy → Ti with Al element dissolved in solution → TiAl → TiAl, and the matrix made of magnesium or a magnesium alloy and the titanium or titanium alloy with Al dissolved in solution or Ti x Al y A three-dimensional continuously connected Mg / TiAl composite material is obtained, in which the matrix composed of a second phase is infinitely connected to form a bi-continuous structure.

[0025]

[0026] And, in another aspect of the present invention, the present invention provides a metal composite material such as a Mg / Ti composite material or a Mg / TiAl composite material manufactured according to the above manufacturing method.

[0027] According to the method for manufacturing a metal composite material through a metal melt decomposition method according to the present invention, the Ca alloy element contained in the Mg-Ca alloy melt has high miscibility with Cu, thereby promoting the decomposition behavior in which Cu escapes into the melt, thereby significantly shortening the process time required for manufacturing a composite material compared to the conventional technology using pure magnesium melt.

[0028] In addition, the Ca alloy element contained in the Mg-Ca alloy melt is dissolved in the Mg matrix, thereby increasing the volume fraction of the Mg matrix in the composite material, reducing the coarsening rate of Ti, and at the same time improving the strength of the composite material through the solid solution strengthening of the Mg matrix.

[0029] Figure 1 is a schematic diagram showing a process for manufacturing a Mg / Ti composite material using a metal melt decomposition method using Mg-1Ca (wt%) melt or pure Mg melt in Examples 1 and 2 of the present invention and Comparative Examples 1 and 2.

[0030] Figure 2 shows the results of measuring the time required for decomposition of Cu using Mg-1Ca (wt%) molten metal or pure Mg molten metal in the present invention and comparative examples.

[0031] Figure 3 shows scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) results of Mg / Ti composite materials according to the process time of the metal melt decomposition method using Mg-1Ca (wt%) melt or pure Mg melt in the present invention and comparative examples.

[0032] Figure 4 is a scanning electron microscope (SEM) photograph of a Mg / Ti composite material manufactured according to each of Example 1 and Comparative Example 1 of the present invention.

[0033] Figure 5 is a scanning electron microscope (SEM) photograph of a Mg / Ti composite material manufactured according to each of Example 2 and Comparative Example 2 of the present invention.

[0034] In describing the present invention, if it is determined that a detailed description of a related known function or configuration may unnecessarily obscure the gist of the present invention, the detailed description will be omitted.

[0035]

[0036] Embodiments according to the concept of the present invention may be modified in various ways and take various forms. Therefore, specific embodiments are illustrated in the drawings and described in detail in this specification or application. However, this is not intended to limit embodiments according to the concept of the present invention to specific disclosed forms, and it should be understood that all modifications, equivalents, and alternatives included within the spirit and technical scope of the present invention are included.

[0037]

[0038] The terminology used herein is for the purpose of describing specific embodiments only and is not intended to limit the present invention. The singular expressions include plural expressions unless the context clearly indicates otherwise. In this specification, it should be understood that the terms "comprises" or "has" indicate the presence of a described feature, number, step, operation, component, part, or combination thereof, but do not preclude the presence or addition of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0039]

[0040] Hereinafter, the present invention will be described in more detail by way of examples.

[0041]

[0042] The embodiments described herein may be modified in various ways, and the scope of this specification is not to be construed as limited to the embodiments described below. The embodiments described herein are provided to more fully explain this specification to those of ordinary skill in the art.

[0043]

[0044] In this example, a metal melt decomposition method is proposed in which Ca, which can promote the decomposition of Cu constituting a Ti-Cu precursor as illustrated in Fig. 1, is added to a Mg melt. Accordingly, the microstructures of Mg / Ti composite materials (Examples 1 and 2) manufactured by the metal melt decomposition method using a Ti-Cu precursor and an Mg-Ca melt and Mg / Ti composite materials (Comparative Examples 1 and 2) manufactured by the conventional metal melt decomposition method using a Ti-Cu precursor and a pure magnesium (Mg) melt were observed and the mechanical properties were measured for comparison.

[0045]

[0046] <Example 1>

[0047] Ti-Cu precursor alloy (Ti 30 Cu 70 ) was placed in a Mg-1Ca (wt%) alloy molten metal at 800°C for 10 minutes and then taken out to manufacture a Mg / Ti composite material.

[0048]

[0049] <Example 2>

[0050] Ti-Cu precursor alloy (Ti 30 Cu 70 ) was charged into a Mg-1Ca (wt%) alloy molten metal at 800°C for 60 minutes and then taken out to manufacture a Mg / Ti composite material.

[0051]

[0052] <Comparative Example 1>

[0053] According to the conventional general metal melt decomposition method, Ti-Cu precursor alloy (Ti 30 Cu 70 ) was placed in a pure Mg molten metal at 800℃ for 30 minutes and then taken out to manufacture a Mg / Ti composite material.

[0054]

[0055] Comparative Example 2

[0056] According to the conventional general metal melt decomposition method, Ti-Cu precursor alloy (Ti 30 Cu 70 ) was placed in a pure Mg molten metal at 800℃ for 60 minutes and then taken out to manufacture a Mg / Ti composite material.

[0057]

[0058] Figure 2 shows the results of measuring the time required for decomposition of Cu using Mg-1Ca (wt%) molten metal or pure Mg molten metal in the present invention and comparative examples.

[0059] Referring to FIG. 2, when using a Mg-1Ca (wt%) molten metal as in the present example, the decomposition of Cu was completed in 10 minutes after charging the precursor alloy into the molten metal (Cu content in the precursor ≤ 1 wt%), whereas in the comparative example using a pure Mg molten metal, the decomposition of Cu was completed only after 30 minutes after charging the precursor alloy into the molten metal.

[0060] As described above, the reason why Cu decomposition is completed more quickly in the examples than in the comparative examples is that Ca present in the Mg-1Ca (wt%) molten metal has high miscibility with Cu constituting the precursor, and the degree of miscibility is higher than the miscibility between Cu and Mg (Ca-Cu mixing enthalpy (ΔH mix ) : -13 kJ / mol, Mg-Cu mixing enthalpy (ΔH mix ) : -3 kJ / mol), because decomposition of Cu from the precursor alloy is promoted in the Mg-1Ca (wt%) melt compared to the pure Mg melt.

[0061]

[0062] Figure 3 shows scanning electron microscope (SEM) images and energy dispersive X-ray spectroscopy (EDS) results of Mg / Ti composite materials according to the process time of the metal melt decomposition method using Mg-1Ca (wt%) melt or pure Mg melt in the present invention and comparative examples.

[0063] According to Fig. 3, in Comparative Example 1, it was confirmed that the decomposition of Cu in the pure Mg molten metal was completed in 30 minutes, and a Mg / Ti composite material having a three-dimensional continuous connection structure and composed of a pure Mg matrix and a pure Ti matrix was manufactured.

[0064] In contrast, in Example 1, the decomposition of Cu in the Mg-1Ca (wt%) molten metal was completed in 10 minutes, and it was found that an Mg / Ti composite material was manufactured, which included an Mg matrix composed of an α-Mg phase with a three-dimensional continuous structure and 0.6 wt% Ca dissolved therein. Ca is not miscible with Ti and is not dissolved in the Ti matrix, but is miscible with Mg (Ca-Ti mixing enthalpy (ΔH mix ) : 43 kJ / mol, Ca-Mg mixing enthalpy (ΔH mix ) : -6 kJ / mol), a Mg / Ti composite material including an α-Mg matrix formed by dissolving Ca in a Mg matrix was manufactured.

[0065]

[0066] Figure 4 is a scanning electron microscope (SEM) photograph of a Mg / Ti composite material manufactured according to Example 1 and Comparative Example 1, respectively.

[0067] Referring to Fig. 4, the Mg / Ti composite material manufactured in Comparative Example 1 had a volume fraction of Mg matrix and Ti matrix of 30:70, so the area of ​​the Ti matrix was much higher, and the hardness was measured to be 115.2 Hv.

[0068] The Mg / Ti composite material manufactured in Example 1 showed a significantly increased volume fraction of the Mg matrix compared to Comparative Example 1, and the volume fraction of the Mg matrix and the Ti matrix showed an ideal ratio of 51:49. In addition, even though the volume fraction of the Mg matrix, which has relatively low strength compared to the Ti matrix, was significantly increased compared to Comparative Example 1, the hardness of the Mg / Ti composite material was measured to be 107.4 Hv, which was not much different from that of Comparative Example 1. This is because Ca contained in the Mg-1Ca (wt%) molten metal used in the manufacture of the Mg / Ti composite material was dissolved in the Mg matrix, forming an α-Mg matrix having higher properties than the Mg matrix, and the size of the Ti matrix was refined.

[0069] Therefore, the Mg / Ti composite manufactured by immersing in Mg-1Ca (wt%) molten metal for 10 minutes has an ideal ratio of volume fractions of Ti matrix and Mg matrix close to 50:50, despite the fact that the molten metal immersion time is significantly reduced to 1 / 3 compared to the Mg / Ti composite manufactured by immersing in pure Mg molten metal for 30 minutes. The closer the volume fraction is to the ideal 50:50, the greater the interfacial area between the Ti matrix and Mg matrix, and thus superior mechanical and chemical properties can be expected.

[0070]

[0071] Figure 5 is a scanning electron microscope (SEM) photograph of a Mg / Ti composite material manufactured according to Example 2 and Comparative Example 2, respectively.

[0072] According to Fig. 5, in Comparative Example 2, the volume fraction of the Mg matrix and the Ti matrix was 30:70, similar to Comparative Example 1, and the volume fraction of the Ti matrix was much higher, and the size of the Ti matrix was 3.4 μm on average.

[0073] In Example 2, as in Example 1, the volume fraction of the Mg matrix and the Ti matrix had an ideal ratio of 48:52, and the size of the Ti matrix was confirmed to be finer than that of Comparative Example 2, with an average size of 2.9 μm.

[0074]

[0075] While the embodiments of the present invention have been described above with reference to the attached drawings, those skilled in the art will appreciate that the present invention can be implemented in other specific forms without altering the technical spirit or essential characteristics thereof. Therefore, the embodiments described above should be understood to be illustrative in all respects and not restrictive.

[0076] According to the present invention, the process time required for manufacturing a composite material can be significantly shortened compared to the conventional technology using pure magnesium melt through a metal melt decomposition method using Mg-Ca alloy melt, and a composite material having improved strength can be manufactured.

Claims

1. A method for producing a metal composite material, comprising the step of producing a Mg / Ti composite material by immersing a precursor alloy (Ti-X) containing a metal (X) that is miscible with titanium (Ti) and is dissolved into the molten metal, in a molten metal containing magnesium (Mg) and calcium (Ca).

2. In paragraph 1, A method for manufacturing a metal composite material, characterized in that the molten metal contains less than 10 wt% of calcium (Ca).

3. In paragraph 1, A method for producing a metal composite material, characterized in that the precursor alloy is selected from the group consisting of a Ti-Cu alloy, a Ti-Ni alloy, a Ti-Zn alloy, a Ti-Ga alloy, a Ti-Ge alloy, a Ti-As alloy, a Ti-Rh alloy, a Ti-Pd alloy, a Ti-Ag alloy, a Ti-Cd alloy, a Ti-In alloy, a Ti-Sn alloy, a Ti-Sb alloy, a Ti-Ir alloy, a Ti-Pt alloy, a Ti-Au alloy, a Ti-Hg alloy, a Ti-Pb alloy, and a Ti-Bi alloy.

4. In paragraph 1, A method for manufacturing a metal composite material, characterized in that a Ti-Cu alloy is immersed in a molten metal containing magnesium (Mg) and calcium (Ca), copper is eluted into the molten metal, and the molten metal fills the pores formed in the precursor alloy by the eluted copper, thereby forming a Mg / Ti composite material.

5. In paragraph 4, A precursor alloy (Ti) containing titanium (Ti) and copper (Cu) in an atomic ratio of 30:70 is added to a molten alloy (Mg-1wt%Ca) composed of 99 wt% magnesium (Mg) and 1 wt% calcium (Ca). 30 Cu 70 ) for less than 10 minutes to produce a Mg / Ti composite material.

6. In paragraph 1, (a) A step of manufacturing a Mg / Ti composite material by immersing a precursor alloy (Ti-X) containing a metal (X) that is miscible with titanium (Ti) and is also miscible with the molten metal and is dissolved into the molten metal, in a molten metal containing magnesium (Mg) and calcium (Ca); (b) a step of manufacturing a titanium (Ti) porous structure from the above Mg / Ti composite material; and (c) a step of manufacturing a Mg / TiAl composite material by immersing the titanium (Ti) porous structure in a Mg-Al alloy molten metal; A method for manufacturing a metal composite material, characterized in that it includes:

7. In paragraph 6, In the above step (b), A method for producing a metal composite material, characterized in that the above Mg / Ti composite material is immersed in an acid solution to remove magnesium or a magnesium alloy from the Mg / Ti composite material and produce a titanium (Ti) porous structure.

8. In paragraph 6, In the above step (c), A method for producing a metal composite material, characterized in that the above titanium (Ti) porous structure is immersed in a Mg-3 wt% Al alloy molten metal to produce a Mg / TiAl composite material.

9. In paragraph 6, (a) A precursor alloy (Ti) containing titanium (Ti) and copper (Cu) in an atomic ratio of 30:70 in a molten metal containing magnesium (Mg) and calcium (Ca) 30 Cu 70 ) to manufacture a Mg / Ti composite material; (b) a step of immersing the Mg / Ti composite material in a nitric acid (HNO3) aqueous solution to remove magnesium or magnesium alloy from the Mg / Ti composite material and produce a titanium (Ti) porous structure; and (c) a step of manufacturing a Mg / TiAl composite material by immersing the titanium (Ti) porous structure in a Mg-3 wt% Al alloy molten metal for 10 seconds to 2 hours; A method for manufacturing a metal composite material, characterized in that it includes:

10. A metal composite material manufactured by a manufacturing method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for manufacturing metal member

    JP2018178207A

  • Porous metal

    JP2020125523A

  • Magnesium-based composite material having ti particles dispersed therein, and method for production thereof

    KR1020100092969A

  • Metal member manufacturing method, and metal member

    WO2011092909A1

  • KR20230044630A