Hydrogen sulfide-based solid electrolyte for all-solid-state battery and method for manufacturing same
The development of a hydrosulfide-based solid electrolyte compound for all-solid-state batteries, created by mixing lithium sulfide and phosphorus pentasulfide and subsequent ball milling, addresses the stability and performance issues at the electrolyte/cathode interface, enhancing ionic conductivity and energy density for lithium metal anodes.
Patent Information
- Application Number
- PCT/KR2024/005677
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-25
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
All-solid-state batteries with lithium metal anodes face performance and stability issues due to chemical/electrochemical instability at the solid electrolyte/cathode interface, leading to increased interfacial resistance and reduced energy density.
A hydrosulfide-based solid electrolyte compound represented by the formula Li_x-y M_8-x Q_20-2x-y X_y, where M includes elements like P, As, Si, Ge, Al, Q includes S, Se, N, and X is a halogen or related species, is developed, with a method involving the mixing of lithium sulfide and phosphorus pentasulfide followed by ball milling to create a stable ionic conductor.
The hydrosulfide-based solid electrolyte enhances ionic conductivity and reduces activation energy, providing a stable interface for lithium metal anodes, thereby improving the performance and lifespan of all-solid-state batteries.
Smart Images

Figure KR2024005677_31102024_PF_FP_ABST
Abstract
Description
Hydrogen sulfide-based solid electrolyte for all-solid-state batteries and its manufacturing method
[0001] This application claims the benefit of priority to Korean Patent Application No. 10-2023-0054988, filed April 26, 2023, and Korean Patent Application No. 10-2024-0055408, filed April 25, 2024, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a hydrogen sulfide-based solid electrolyte for an all-solid-state battery and a method for manufacturing the same.
[0003] Among next-generation lithium secondary batteries, the all-solid-state battery industry is conducting research on applying lithium metal anodes to design high-energy-density batteries. However, direct contact between the solid electrolyte and the lithium metal anode in all-solid-state batteries increases the resistance at the solid electrolyte / cathode interface due to the chemical and electrochemical instability of the solid electrolyte, which reduces battery performance, lifespan, and stability.
[0004] Recently, research is being conducted to reduce the interfacial resistance between the electrode and the electrolyte by forming an interfacial phase between the solid electrolyte and lithium metal to solve the above problems.
[0005] However, the interfacial phases in the above study have a higher redox level than the existing lithium metal negative electrode, so there is a limitation that the operating voltage of the cell is lowered and the energy density is reduced.
[0006] Therefore, there is a need to develop a stable solid electrolyte for all-solid-state batteries with a lithium metal negative electrode that can overcome the above limitations.
[0007] [Prior Art Literature]
[0008] [Non-patent literature]
[0009] (Non-patent literature 1) Journal of Power Sources 244 (2013) 707-710
[0010] The purpose of the present invention is to provide a high ion conductivity sulfide-based solid electrolyte that simultaneously includes a sulfide-based solid electrolyte of the existing Li2S-P2S5 series and a hydride-based solid electrolyte that is reported to be stable to a lithium metal negative electrode.
[0011] To achieve the above purpose,
[0012] The present invention provides a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery represented by the following chemical formula 1.
[0013] [Chemical Formula 1]
[0014] Li x-y M 8-x Q 20-2x-y X y (6 <x≤7.6, 0<y<1)
[0015] In the above chemical formula 1,
[0016] wherein M is at least one element selected from the group consisting of P, As, Si, Ge, Al and B,
[0017] wherein Q is at least one element selected from the group consisting of S, Se and N,
[0018] The above X is a halogen element, BH4, BF4, NH2, or NO3.
[0019] In addition, the present invention may allow the y value to have a range of 0.1≤y≤0.9.
[0020] In addition, the present invention may have the x value in the range of 6.5≤x≤7.5.
[0021] In addition, the present invention may be such that M may be P.
[0022] In addition, the present invention may be such that Q may be S.
[0023] In addition, the present invention provides that X may be BH4.
[0024] In addition, in order to achieve the above purpose, the present invention
[0025] a) a step of mixing lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) by ball milling; and
[0026] b) A method for producing a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, comprising the step of adding LiBH4 to the mixture of step a) and then ball milling the mixture, can be provided.
[0027] In addition, in order to achieve the above purpose, the present invention
[0028] A solid electrolyte including the above-mentioned hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery can be provided.
[0029] In addition, in order to achieve the above purpose, the present invention
[0030] An all-solid-state battery including the above solid electrolyte can be provided.
[0031] In addition, the present invention may include the solid electrolyte in at least one of the positive electrode, negative electrode, or solid electrolyte membrane of the all-solid-state battery.
[0032] In the prior art, thiophosphate (PS4 3- ) BH4 in the anion site (4b site) - Replacing anions had the problem of creating impurities because the anion radii were too different from each other to form a solid solution.
[0033] According to the present invention, S 2- BH4 in the anion site (4a or 4d site) - There is an advantage in that it is possible to provide a solid electrolyte without impurities by forming a solid solution by adding anions.
[0034] Figure 1 is a graph showing room temperature EIS data of a hydrogen sulfide-based solid electrolyte for an all-solid-state battery according to one embodiment of the present invention.
[0035] FIG. 2 is a graph showing an Arrhenius plot of a hydrogen sulfide-based solid electrolyte for an all-solid-state battery according to one embodiment of the present invention.
[0036] Figure 3 is a graph showing the ionic conductivity and activation energy at room temperature of a hydrogen sulfide-based solid electrolyte for an all-solid-state battery according to one embodiment of the present invention.
[0037] Figure 4 is a schematic diagram showing the composition ratio of a hydrogen sulfide-based solid electrolyte for an all-solid-state battery according to the prior art invention.
[0038] Figure 5 is a schematic diagram showing the composition ratio of a hydrogen sulfide-based solid electrolyte for an all-solid-state battery according to the present invention.
[0039] The inventors of the present invention used the Quasi-Ternary System (Li2S-P2S5-LiBH4) to determine whether the composition was synthesizable. x-y P 8-x S 20-2x-y (BH4) y , (6 <x≤7.6, 0≤y≤3.8) 조성에서 고상법으로 합성을 진행하한 결과, 신규한 전고체전지용 수소화황화물계 고체전해질 제조방법을 발견하기에 이르렀다.
[0040] For this purpose, as in previous studies, thiophosphate (PS4 3- ) BH4 in the anion site (4b site) - Rather than forming a solid solution by adding anions, S 2- BH4 in the anion site (4a or 4d site) - A solid electrolyte was synthesized by adding anions to form a solid solution.
[0041] Here, thiophosphate refers to a compound or anion having S or O surrounding a tetrahedral P.
[0042]
[0043] As a result, the present invention provides a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery represented by the following chemical formula 1.
[0044] [Chemical Formula 1]
[0045] Lix-y M 8-x Q 20-2x-y X y (6 <x≤7.6, 0<y<1)
[0046] In the above chemical formula 1,
[0047] wherein M is at least one element selected from the group consisting of P, As, Si, Ge, Al and B,
[0048] wherein Q is at least one element selected from the group consisting of S, Se and N,
[0049] The above X is a halogen element, BH4, BF4, NH2, or NO3.
[0050]
[0051] Figures 4 and 5 are schematic diagrams showing the ratios of Li2S, P2S5, and LiBH4 included in a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, thereby explaining the differences between each component.
[0052] FIG. 4 shows a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to a prior art, and FIG. 5 shows a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention.
[0053] In the case of a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the prior art, as shown in Fig. 1, Li 3-2x (PS4) (1-x) (BH4) x It can be expressed as PS4 3- Wow BH4 - You can see that they coexist,
[0054] In the case of the hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention, Li x-y P 8-x S 20-2x-y (BH4) y , (6 <x≤7.6, 0<y<1)의 식으로 나타냄에 따라서, 색칠된 면적 내부의 Tie-line은 S 2- Wow BH4- We can see that S coexists, and the tie-lines represent some of them. That is, if we fix the x value and change the y value, S 2- Wow BH4 - It can be confirmed that they coexist.
[0055] These differences are due to the fact that in conventional techniques thiophosphate (PS4 3- ) BH4 in the anion site (4b site) - Unlike the formation of a solid solution by substituting an anion, the present invention uses S 2- BH4 in the anion site (4a or 4d site) - It is thought that this is because a solid solution is formed by replacing anions.
[0056]
[0057] In one embodiment of the hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention, the y value may have a range of 0.1≤y≤0.9, preferably the y value may have a range of 0.2≤y≤0.8, more preferably the y value may have a range of 0.3≤y≤0.7, and most preferably the y value may have a range of 0.4≤y≤0.6.
[0058] A. When the above y value is less than 0.1, there is a problem that the ionic conductivity decreases and the activation energy increases, and when the above y value is greater than 0.9, there is a problem that the activation energy increases.
[0059] In one embodiment of the hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention, the x value may have a range of 6.5≤x≤7.5, and more preferably, the x value may be 7.
[0060]
[0061] In one embodiment of the hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention, M may preferably be P.
[0062] In one embodiment of the hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention, Q may preferably be S.
[0063] In one embodiment of the hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery according to the present invention, X may preferably be BH4.
[0064]
[0065] In addition, in order to achieve the above purpose, the present invention
[0066] a) a step of mixing lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) by ball milling; and
[0067] b) A method for producing a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, comprising the step of adding LiBH4 to the mixture of step a) and then ball milling the mixture, can be provided.
[0068] According to the above manufacturing method, the hydrogen sulfide-based solid electrolyte compound for the all-solid-state battery of the present invention
[0069]
[0070] In addition, in order to achieve the above purpose, the present invention
[0071] A solid electrolyte including the above-mentioned hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery can be provided.
[0072] In one embodiment of the present invention, the solid electrolyte may additionally include another sulfide-based solid electrolyte in addition to the hydrogen sulfide-based solid electrolyte compound described above.
[0073] The sulfide-based solid electrolyte additionally included above contains sulfur (S) and has the ionic conductivity of a metal belonging to Group 1 or Group 2 of the periodic table, and may include Li-PS-based glass or Li-PS-based glass ceramic. Non-limiting examples of such sulfide-based solid electrolytes include Li2S-P2S5, Li2S-LiI-P2S5, Li2S-LiI-Li2O-P2S5, Li2S-LiBr-P2S5, Li2S-Li2O-P2S5, Li2S-Li3PO4-P2S5, Li2S-P2S5-P2S5, Li2S-P2S5-SiS2, Li2S-P2S5-SnS, Li2S-P2S5-Al2S3, Li2S-GeS2, Li2S-GeS2-ZnS, etc., and may include one or more of these. However, the present invention is not particularly limited thereto.
[0074]
[0075] In addition, the present invention can provide an all-solid-state battery including the solid electrolyte.
[0076] In addition, the present invention may include the all-solid-state battery, a positive electrode, a negative electrode or a solid electrolyte membrane, and may include the solid electrolyte in at least one of them.
[0077]
[0078] In the case of the positive electrode according to one embodiment of the present invention, the positive electrode current collector is for supporting the positive electrode active material, and is not particularly limited as long as it has excellent conductivity and is electrochemically stable in the voltage range of the lithium secondary battery. For example, the positive electrode current collector may be any one metal selected from the group consisting of copper, aluminum, stainless steel, titanium, silver, palladium, nickel, alloys thereof, and combinations thereof, and the stainless steel may be surface-treated with carbon, nickel, titanium, or silver, and as the alloy, an aluminum-cadmium alloy may be preferably used, and in addition, calcined carbon, a non-conductive polymer surface-treated with a conductive material, or a conductive polymer, etc. may be used.
[0079] The above positive electrode current collector can form fine irregularities on its surface to strengthen the bonding strength with the positive electrode active material, and can be used in various forms such as a film, sheet, foil, mesh, net, porous body, foam, and non-woven fabric.
[0080] The above positive electrode active material may optionally include a conductive material and a binder.
[0081] The above-described positive electrode active material may vary depending on the type of the all-solid-state battery. For example, the above-described positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; a lithium manganese oxide such as Li1+xMn2-xO4 (0≤x≤0.33), LiMnO3, LiMn2O3, LiMnO2; a lithium copper oxide (Li2CuO2); a vanadium oxide such as LiV3O8, V2O5, Cu2V2O7; a Ni-site type lithium nickel oxide represented by the chemical formula LiNi1-xMxO2 (M = Co, Mn, Al, Cu, Fe, Mg, B, or Ga; 0.01≤x≤0.3); Lithium manganese composite oxides represented by the chemical formula LiMn2-xMxO2 (M = Co, Ni, Fe, Cr, Zn or Ta; 0.01≤x≤0.1) or Li2Mn3MO8 (M = Fe, Co, Ni, Cu or Zn); lithium manganese composite oxides having a spinel structure represented by LiNixMn2-xO4; LiCoPO4; LiFePO4; elemental sulfur (S8); sulfur compounds such as Li2Sn (n=1), organosulfur compounds or carbon-sulfur polymers ((C2Sx)n: x=2.5 to 50, n=2), but are not limited thereto.
[0082] The above conductive material is a material that electrically connects the electrolyte and the positive electrode active material and serves as a path for electrons to move from the current collector to the positive electrode active material. Any material that does not cause chemical changes in a lithium secondary battery and has porosity and conductivity can be used without restriction.
[0083] For example, the conductive material may be a porous carbon-based material, such as carbon black, graphite, graphene, activated carbon, carbon fiber, etc.; metallic fibers such as metal mesh; metallic powders such as copper, silver, nickel, aluminum, etc.; or organic conductive materials such as polyphenylene derivatives. The conductive materials may be used alone or in combination.
[0084] Current commercially available products include acetylene black series (such as those from Chevron Chemical Company or Gulf Oil Company), Ketjen Black EC series (from Armak Company), Vulcan XC-72 (from Cabot Company), and Super P (from MMM). Examples include acetylene black, carbon black, and graphite.
[0085] In addition, the positive electrode may additionally include a binder, and the binder increases the bonding strength between the components constituting the positive electrode and between them and the current collector, and any binder known in the art may be used.
[0086] For example, the binder may be a fluororesin binder including polyvinylidene fluoride (PVdF) or polytetrafluoroethylene (PTFE); a rubber binder including styrene butadiene rubber (SBR), acrylonitrile-butidiene rubber, and styrene-isoprene rubber; a cellulose binder including carboxyl methyl cellulose (CMC), starch, hydroxy propyl cellulose, and regenerated cellulose; a polyalcohol binder; a polyolefin binder including polyethylene and polypropylene; a polyimide binder; a polyester binder; and a silane binder. One, two or more mixtures or copolymers selected from the group consisting of may be used.
[0087]
[0088] In the case of the negative electrode according to one embodiment of the present invention, the negative electrode may, like the positive electrode, include a conductive material and a binder as needed. In this case, the negative electrode current collector, conductive material, and binder may be those typically used in negative electrodes, as described above.
[0089] According to one embodiment of the present invention, the negative active material may be in the form of lithium metal, lithium alloy, or negative electrode free.
[0090] The above negative electrode-free form may be a structure including only a negative electrode collector, or a structure in which a carbon layer including a binder is coated on the negative electrode collector.
[0091] The above examples are presented to help understand the present invention.
[0092] However, the following examples are only intended to aid understanding of the present invention, and the present invention is not limited to the following examples.
[0093]
[0094] Example: Preparation of a hydrogen sulfide-based solid electrolyte using a solid-state reaction (x=7,0≤y≤1)
[0095] All experiments were performed in a glove box protected from moisture and oxygen. Compositions of y = 0.1, 0.5, and 0.9, excluding compositions of y = 0 and y = 1, were synthesized twice using a solid-state reaction using mechanochemical ball milling. In the first round, lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) were synthesized at the following molar ratios, 400 RPM, 20 hours based on a 1.5 g batch of sample. In the second round, lithium borohydride (LiBH4) was added at the following molar ratio to the sample obtained in the first round, and synthesized at 400 RPM, 20 hours based on a 1.0 g batch of sample.
[0096] The compositions y=0 and y=1 were prepared by adding lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) in the molar ratios shown below and performing a solid-state synthesis method under the same conditions as the first step. Through the above process, a hydrogen sulfide-based solid electrolyte was obtained.
[0097] Specifically, 1) In the first ball milling, lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) were mixed at molar ratios of 87.5:12.5 (7:1), 85.7:14.3 (6:1), 83.3:16.7 (5:1), 80:20 (4:1), 75:25 (3:1), 66.7:33.3 (2:1), 50:50 (1:1), and 0:100 (0:1).
[0098] 2) After adding lithium borohydride (LiBH4) to the first ball-milled mixture, a second ball-milling is performed to obtain a compound with the chemical formula Li x-y P 8-x S 20-2x-y (BH4) y , (6 <x≤7.6, 0≤y≤1)에서 x=7, y=0~1.0를 제조하였다.
[0099]
[0100] Comparative example: Li7PS6 [(1) Hayashi Akitoshi et al., The Chemical Society of Japan, Chemistry Letters 2001, Vol.30, No.9]
[0101] Lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) were synthesized in a molar ratio of 87.5:12.5 (7:1) using a solid-state synthesis method at 370 RPM for 20 hours in one cycle. The results are summarized in the table below.
[0102] Comparative Example 1 Molar ratio of each component Ionic conductivity (mS / cm) Li7PS687.5:12.50.2
[0103] Experimental Example 1. Method for Measuring Physical Properties
[0104] In the examples and experimental examples according to the present invention, the method for measuring physical properties is as follows.
[0105] 1.1) XRD analysis method: After placing the sample in a quartz capillary to prevent exposure to the atmosphere and moisture, it is completely sealed with liquid paraffin and then measured.
[0106] 1.2) XRD analysis conditions: Using an X-ray wavelength of Cu ka (1.54 Å). [scan range: 10°-70°, step size: 0.02°, scan speed: 2° / min]
[0107]
[0108] 2.1) Method for manufacturing electrode cell for EIS analysis: Use electrode with diameter of 10 mm (area: 0.7854 cm2), put 100-120 mg of solid electrolyte into the electrode and press at a pressure of 441.8 MPa.
[0109] 2.2) EIS analysis conditions: AC: 0.1V, frequency 10 MHz ~ 1 Hz.
[0110] 2.3) EIS analysis method: The temperature was increased and decreased by 10 ℃ from 25 ℃ to 110 ℃, the resistance value at that time was measured, and the ionic conductivity was calculated based on the following equation 1).
[0111] Equation) Ionic conductivity (σ) = thickness (l) / (resistance (Ω) X area (a), [area: 0.7854 cm 2 , thickness: 0.7~1.0 mm]
[0112]
[0113] The above manufactured Li x-y P 8-x S 20-2x-y (BH4) y Among the compounds expressed as 6 <x≤7.6, 0≤y≤1.0 에서의 조성, x=7 일 때 y의 값에 따라 S 2- Anions and BH4 - It was confirmed that the ratio of coexistence of anions changed and the ionic conductivity changed.
[0114]
[0115] Specifically, for the hydrogen sulfide-based solid electrolytes for all-solid-state batteries manufactured in the above examples and comparative examples, room temperature EIS data for each composition are shown in Fig. 1. Through Fig. 1, the ionic conductivity could be confirmed by measuring the resistance for each composition of the synthesized electrolyte.
[0116]
[0117] *For the hydrogen sulfide-based solid electrolytes for all-solid-state batteries manufactured in the above examples and comparative examples, an Arrhenius plot of activation energy values for each composition was created and shown in Fig. 2.
[0118] In addition, the ionic conductivity and activation energy at room temperature for the hydrogen sulfide-based solid electrolytes for all-solid-state batteries manufactured in the above examples and comparative examples are shown in Table 2 and Figure 3 below according to each composition.
[0119] Ionic conductivity [S cm -1 ]Activation energy[kJ mol -1]Li7PS61.17 x 10 -4 34.9Li 6.9 PS 5.9 (BH4) 0.1 1.54 x 10 -4 34.4Li 6.5 PS 5.5 (BH4) 0.5 2.92 x 10 -4 30Li 6.1 PS 5.1 (BH4) 0.9 6.54 x 10 -4 34Li6PS5(BH4)5.65 x 10 -4 34.3
[0120] In the case of ionic conductivity, it was found that Comparative Example 1 was the lowest, increased from Example 1 to Example 3, and then decreased again in Comparative Example 2. In the case of activation energy, it was found that Comparative Example 1 was the highest, decreased from Example 1, became the lowest in Example 2, and then increased again. In other words, when considering ionic conductivity and activation energy comprehensively, it was found that Example 2 (y = 0.5) showed the optimal effect.
Claims
1. A hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery represented by the following chemical formula 1. [Chemical Formula 1] Li x-y M 8-x Q 20-2x-y X y (6 <x≤7.6, 0<y<1) In the above chemical formula 1, wherein M is at least one element selected from the group consisting of P, As, Si, Ge, Al and B, wherein Q is at least one element selected from the group consisting of S, Se and N, The above X is a halogen element, BH4, BF4, NH2, or NO3.
2. In paragraph 1, A hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, characterized in that the above y value has a range of 0.1≤y≤0.
9.
3. In paragraph 1, A hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, characterized in that the above x value has a range of 6.5≤x≤7.
5.
4. In paragraph 1, A solid electrolyte compound based on hydrogen sulfide for an all-solid-state battery, wherein the above M is P.
5. In paragraph 1, A hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, characterized in that the above Q is S.
6. In paragraph 1, A hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery, characterized in that the above X is BH4. 7.a) A step of mixing lithium sulfide (Li2S) and phosphorus pentasulfide (P2S5) by ball milling; and b) a step of adding LiBH4 to the mixture of step a) and then ball milling; A method for producing a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery of the first paragraph.
8. A solid electrolyte comprising a hydrogen sulfide-based solid electrolyte compound for an all-solid-state battery of the first paragraph.
9. An all-solid-state battery comprising the solid electrolyte of Article 8.
10. In paragraph 9, The above all-solid-state battery is an all-solid-state battery characterized in that it includes the solid electrolyte in at least one of the positive electrode, the negative electrode, or the solid electrolyte membrane.
Citation Information
Patent Citations
Hydrogen sulfide-based solid-state electrolytes for all-solid-state batteries and the method for preparing thereof
KR1020240158167A
Solid electrolyte
JP2016134316A
Mehtod and system for generating domain-transformed image
KR1020240076316A
Apparatus and method device for providing social network services using augmented reality
KR102419056B1
KR20200053099A