Low-melting-point brazing material and preparation method therefor

By introducing tin wire into the welding material and adjusting the flux composition, the problem of high melting temperature of the welding material is solved, low melting point and high-efficiency welding are achieved, the heating temperature and oxidation effects of the base material are reduced, and the active temperature range of the flux is enhanced , improves welding effect.

WO2024227314A1PCT designated stage expired Publication Date: 2024-11-07HANGZHOU HUAGUANG ADVANCED WELDING MATERIALS CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/104708
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2023-06-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

When brazing steel and steel, the existing welding materials need to be heated to high temperature due to the high melting temperature of the solder, which affects the production rhythm and surface oxidation, and cannot take into account the plasticity of the solder and the solid-liquid phase reduction.

Method used

Low melting point welding material is used, which consists of copper-zinc alloy outer skin, tin wire and flux. The tin wire is located in the middle of the material, reducing the thickness of the outer brazing material and increasing the active temperature range of the flux. By adjusting the flux composition and filling rate, ensure The welding temperature range is between 649.21 and 790.5°C. The flux consists of boric acid, potassium fluoroborate, fluoride, and borate, and the filling rate is controlled between 10% and 20%.

Benefits of technology

The melting point of welding materials is reduced, the welding production efficiency is improved, the heating temperature and oxidation effects of the base material are reduced, and the active temperature range of the flux is increased, ensuring the stability of the welding effect and deoxidation protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023104708_07112024_PF_FP_ABST
    Figure CN2023104708_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a low-melting-point brazing material and a preparation method therefor. The cross section of the low-melting-point brazing material is composed of a filler metal outer coat, a brazing flux, and a solder wire; the outermost filler metal outer coat is made of copper-zinc alloy; the mass ratio of the innermost solder wire to the filler metal outer coat is 0.005-0.01; and the mass of the brazing flux accounts for 6%-25% of the total mass of the low-melting-point brazing material. The thickness of the filler metal outer coat ranges from 0.1 to 0.5 millimeter. The diameter of the solder wire ranges from 0.1 millimeter to 3 millimeters. The activation temperature of the brazing flux ranges from 650°C to 1050°C; the brazing flux is formed by mixing boric acid, potassium fluoroborate, fluoride, and borate; the mass of the boric acid accounts for 30%-50% of the total mass of the brazing flux; the mass of the potassium fluoroborate accounts for 20%-40% of the total mass of the brazing flux; the mass of the fluoride accounts for 5%-20% of the total mass of the brazing flux; and the mass of the borate accounts for 15%-35% of the total mass of the brazing flux. The present application can achieve both the low melting point and the plasticity, and has a large activation temperature range of a brazing flux and a wide range of application.
Need to check novelty before this filing date? Find Prior Art

Description

Low melting point welding material and preparation method thereof Technical Field

[0001] The present application relates to a low melting point welding material and a preparation method thereof, which is mainly suitable for induction brazing or flame brazing between metal materials. Background Art

[0002] Welding materials can be used for brazing steel and copper to steel, and they offer excellent performance after welding. However, when brazing steel to steel using conventional welding materials, due to the high melting point of the brazing filler metal, which ranges from 750.42°C to 900.92°C, high-frequency welding requires heating the base metal to very high temperatures to completely melt, wet, and spread the packaged filler metal onto the base metal. This high-temperature heating of the base metal slows production and significantly increases the surface oxide layer, thus hindering practical application. Because welding materials must meet the plasticity requirements during preparation, existing welding materials cannot address both the filler metal plasticity requirements and the lowering of the solidus and liquidus phases.

[0003] Due to the decrease in the overall temperature of the welding material, the active temperature range of the flux is required to be larger, and the existing active temperature range of the flux is difficult to meet the requirements. Summary of the Invention

[0004] The first technical problem solved by the present application is to provide a low-melting-point welding material so that the low-melting-point welding material can take into account both low melting point and plasticity; the second technical problem solved by the present application is to enable the active temperature range of the flux matched with the low-melting-point welding material to meet the set brazing temperature range; the third technical problem solved by the present application is to provide a preparation method of the above-mentioned low-melting-point welding material.

[0005] The technical solution adopted by this application to solve the first technical problem mentioned above is: a low-melting-point welding material, characterized in that the cross-section of the low-melting-point welding material is composed of a solder sheath, a flux, and a tin wire. The outermost solder sheath is made of copper-zinc alloy, the mass ratio of the innermost tin wire to the solder sheath is between 0.005 and 0.01, and the flux mass accounts for 6% to 25% of the total mass of the low-melting-point welding material. This application adds a low-melting-point solid tin wire inside the low-melting-point welding material, places the tin required for the solder component in the middle of the low-melting-point welding material, and reduces the thickness of the outermost solder layer. On the one hand, this prevents the solder sheath from being too thick, resulting in difficulty in forming and melting. On the other hand, the low-melting-point tin wire melts first in the middle of the welding material during the welding process, thereby dissolving the solder sheath from the inside, accelerating the melting rate of the solder sheath, and thus achieving the purpose of lowering the melting point of the low-melting-point welding material.

[0006] The melting point range of the low-melting-point welding material of the present application is between 649.21 and 790.5° C., and the mass ratio of copper to zinc is 58:42.

[0007] The low-melting-point solder material of this application can be manufactured into various shapes based on actual needs. The most commonly used shapes are solder wire or solder rings composed of solder wire. The cross-section of the low-melting-point solder material is oblate, and the solder outer skin thickness is between 0.1 and 0.5 mm. The thickness is the distance between any point on the inner surface of the solder outer skin and the closest point to the outer surface of the solder outer skin. The diameter of the tin wire of this application is generally between 0.1 and 3 mm.

[0008] The technical solution employed by this application to address the second technical problem mentioned above is as follows: the flux described herein has an active temperature between 650 and 1050°C and is composed of a mixture of boric acid, potassium fluoroborate, fluoride, and borate, with boric acid accounting for 30-50% of the total flux mass, potassium fluoroborate for 20-40%, fluoride for 5-20%, and borate for 15-35%. The flux is stirred and dried to form a powder, which is then fed for coating. By controlling the feeding and stepping speeds, the flux filling rate (the percentage of the flux in the total mass of the low-melting-point welding material) is maintained between 10% and 20%. This application adjusts the flux composition by incorporating high- and low-temperature components to expand the flux's active temperature range, thereby meeting the practical application requirements of low-melting-point welding materials. The flux weight percentage in this application has been increased from 6% to 25% to 10% to 20%, enabling more precise control of the added amount and improving welding performance.

[0009] The technical solution adopted by the present application to solve the third technical problem is: a method for preparing a low melting point welding material, characterized by comprising the following steps:

[0010] S1 prepares the solder into a thin strip;

[0011] The S2 solder and tin wire are cleaned to remove surface dirt and oxides, and the solder is rolled and deformed by rollers to form a U-shaped belt that opens upwards;

[0012] S3 synchronously transports the tin wire to the middle of the U-shaped belt, and the flux is poured into the gap between the U-shaped belt and the tin wire through the conveyor belt.

[0013] S4 is rolled and deformed by rollers so that the open ends of the U-shaped strips are butted together to form welding wires;

[0014] S5 uses a brush to clean the surface of the welding wire.

[0015] Compared with the original welding wire, this application greatly reduces the overall melting temperature of the solder. In the actual welding process, it has good welding performance, improves welding production efficiency, and reduces other effects caused by excessively high temperature during the welding process.

[0016] The present application may further include step S6, wherein the welding wire is formed by a ring forming machine, and welding rings of various shapes and sizes can be formed according to actual needs. Since the brazing flux is evenly added during the welding wire forming process of the present application, the brazing flux ratio in the final welding ring is more accurate and the quality is more stable.

[0017] Compared with existing technologies, this application offers the following advantages and effects: The solder ring has a lower melting point, reducing the base metal heating temperature during the welding process, and minimizing the impact on the base metal material and oxidation. The increased flux activity temperature range allows the flux to effectively deoxidize and protect the solder at both high and low temperatures, further facilitating product use. Improvements in the preparation method allow for more precise control of the flux addition amount, avoiding excess flux residue while still meeting the requirements for use. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] FIG1 is a schematic cross-sectional view of a welding ring according to an embodiment of the present application. Implementation Method

[0019] The present application will be further described in detail below with reference to the accompanying drawings and examples. The following examples are intended to explain the present application but the present application is not limited to the following examples.

[0020] Referring to Figure 1, the cross-section of the low-melting-point welding material in the embodiment of the present application is composed of a solder sheath (copper-zinc alloy) 1, a flux 2, and a tin wire 3. The thickness of the outermost solder sheath 1 is 0.1 to 0.5 mm, and the mass ratio of the innermost tin wire 3 to the solder sheath 1 is 0.5% to 1%. The thickness of the intermediate flux 2 is designed according to the filling amount of the flux 2, and the mass of the flux 2 accounts for 10 to 20% of the total mass of the low-melting-point welding material. Compared with the original products, this application adds a solid tin wire inside the welding wire or welding ring, and places the tin required for the solder component in the middle of the low-melting-point welding material, reducing the thickness of the outermost layer of solder 1. On the one hand, it prevents the solder skin from being too thick, which makes it difficult to form and melt. On the other hand, the tin wire melts first in the middle of the low-melting-point welding material during the welding process, thereby dissolving the inner surface of the solder outer skin 1 from the inside, accelerating the melting speed of the solder outer skin 1, and thus achieving the purpose of lowering the melting point of the welding material. At the same time, the mass proportion of the flux 2 is changed from the original 6-25% to 10-20%, and the addition amount is more accurately controlled, which is conducive to improving the welding effect. At the same time, the mass proportion of the flux 2 is changed from the original 6-25% to 10-20%, and the addition amount is more accurately controlled, which is conducive to improving the welding effect. The melting point range of the low-melting-point welding material in this application is 649.21-790.5℃.

[0021] The low-melting-point soldering material of this application can be made into various shapes according to actual needs. The most commonly used shapes are welding wire or welding rings composed of welding wire. The cross-section of the low-melting-point soldering material is usually oblate or circular. When the cross-section of the low-melting-point soldering material is oblate, the thickness of the solder sheath 1 refers to the distance between any point on the inner surface of the solder sheath 1 and the closest point on the outer surface of the solder sheath 1. When the cross-section of the low-melting-point soldering material is circular, the thickness of the solder sheath 1 refers to the difference between the outer diameter and the inner diameter of the solder sheath 1. In the embodiment of this application, the diameter of the tin wire 3 is usually between 0.1 and 3 mm.

[0022] The flux described in this application has an active temperature between 650 and 1050°C. It is composed of a mixture of boric acid, potassium fluoroborate, fluoride, and borate, with boric acid accounting for 30-50% of the total flux mass, potassium fluoroborate for 20-40%, fluoride for 5-20%, and borate for 15-35%. The flux is stirred and dried to form a powder, which is then fed for coating. By controlling the feeding and stepping speeds, the flux filling rate (the percentage of the flux in the total mass of the low-melting-point welding material) is maintained at 10-20%. Industrial Applicability

[0023] The preparation method of the low-melting-point welding material of the present application is as follows: the solder is prepared into a thin strip, the tin wire is prepared into a flat tin wire, the solder is cleaned to remove surface dirt and oxides, the solder is curled and deformed by a roller to form an upwardly open U-shaped strip composed of the deformed solder, and the tin flat wire is synchronously transmitted to the middle of the U-shaped strip, the flux is vibrated from the funnel to the conveyor belt, the powdered flux is transferred by the conveyor belt and poured into the gap between the U-shaped strip and the tin flat wire, and then the flux is deformed by rolling with a roller so that the open ends of the U-shaped strip are butted to form a flat structure as shown in Figure 1, the surface is cleaned with a brush, and finally the low-melting-point welding wire is made. The low-melting-point welding wire is formed into a ring by a ring-making machine of the existing technology, and low-melting-point welding rings of various shapes and sizes can be made according to actual needs.

[0024] Table 1. Data related to the examples and comparative examples of the flux of the present application (the data in the table refer to the percentage of the components to the flux mass)

[0025]

[0026] As shown in Table 1, by adjusting the ratio and type of flux components, a flux formula with higher activity at different filling rates was obtained.

[0027] Table 2. Ratio table of the embodiments and comparative examples of the low-melting-point welding materials of the present application. The data of tin wire in the table are its mass ratio to the outer skin, the data of copper and zinc are their proportions in the outer skin, and the corresponding data of boric acid, potassium fluoroborate, fluoride, and borate are their proportions in the flux.

[0028]

[0029] Table 3. Comparison of relevant data of the low melting point welding material examples, comparative examples and existing products of this application

[0030] Product Name Solidus / ℃Liquidus / ℃ Specific gravity of outer skin Mass ratio of tin wire to outer skin Specific gravity of flux Penetration after welding / mm Welding strength / Mpa Surface finish Joint crack resistance Comparison 1750.42900.9285.00%0.00%15%4.5327.5 Excellent Comparison 2745.3890.885.00%0.00%15%4.43330.8 Excellent Comparison 3720.75880.7985.00%0.00%15%4.7340.1 Excellent Comparison 4740889.685.00%0.00%15%4.6 5337.7Excellent Example 1692.1841.989.78%0.25%10%4.8334.9Good Example 2670.6815.389.55%0.50%10%5.13330.4Excellent Example 3652.41791.5889.33%0.75%10%5.25328.9Excellent Example 4635.79773.2489.10%1.00%10%5.3325.6Excellent Example 5620.82764.188.88%1.25%10%5.5300.2Poor Example Example 6 689.24838.5184.79%0.25%15%5.05334.2 Good Example 7 670.65815.3784.58%0.50%15%5.21329.6 Excellent Example 8 649.21790.584.36%0.75%15%5.5327.5 Excellent Example 9 636.01772.4884.15%1.00%15%5.62325.3 Excellent Example 10 624.8763.1983.94%1.25%15%5.7295.1 Poor Flux Residue Example 11686.43835.3579.80%0.25%20%5.1332.3Good Example 12667.58811.7379.60%0.50%20%5.2328.2Excellent Example 13645.72787.8579.40%0.75%20%5.53325.4Excellent Example 14632.04769.9479.20%1.00%20%5.65322.5Excellent Example 15625.82765.2479.00%1.25%20%5.7290.9Poor flux residue

[0031] As can be seen from Table 3, the melting point of the embodiment of the present application is low, the heating temperature of the base material during the welding process is reduced, and the impact on the base material material and oxidation is smaller.

Claims

1. A low melting point welding material, characterized by: The cross section of the low melting point welding material consists of a solder sheath, a flux and a tin wire. The outermost solder sheath is made of copper-zinc alloy. The mass ratio of the innermost tin wire to the solder sheath is between 0.005 and 0.

01. The mass of the flux accounts for 6% to 25% of the total mass of the low melting point welding wire.

2. The low melting point welding material according to claim 1, characterized in that: The low melting point welding material is welding wire or welding ring formed by welding wire.

3. The low melting point welding material according to claim 1, characterized in that: The melting point range of the low-melting-point welding material is between 649.21 and 790.5° C., and the mass ratio of copper to zinc is 58:

42.

4. The low melting point welding material according to claim 1, characterized in that: The solder skin thickness is between 0.1 and 0.5 mm.

5. The low melting point welding material according to claim 1, characterized in that: The diameter of the tin wire is between 0.1 and 3 mm.

6. The low melting point welding material according to claim 1, characterized in that: The active temperature of the flux is between 650 and 1050° C. The flux is composed of a mixture of boric acid, potassium fluoroborate, fluoride and borate, wherein the mass of boric acid accounts for 30 to 50% of the total mass of the flux, the mass of potassium fluoroborate accounts for 20 to 40% of the total mass of the flux, the mass of fluoride accounts for 5 to 20% of the total mass of the flux, and the mass of borate accounts for 15 to 35% of the total mass of the flux.

7. The low melting point welding material according to claim 6, characterized in that: The flux accounts for 10% to 20% of the total mass of the low melting point welding material.

8. A method for preparing the low melting point welding material according to claim 1, characterized in that The following steps are involved: S1 prepares the solder into a thin strip; The S2 solder and tin wire are cleaned to remove surface dirt and oxides, and the solder is rolled and deformed by a roller to form a U-shaped belt that opens upward; S3 synchronously transmits the tin wire to the middle of the U-shaped belt, and the flux is transferred into the gap between the U-shaped belt and the tin wire through the conveyor belt. S4 is deformed by rolling with a roller, so that the open ends of the U-shaped strip are butted to form a welding wire; S5 uses a brush to clean the surface of the welding wire.

9. The method for preparing the low melting point welding material according to claim 8, characterized in that The following steps are also included: S6 shapes the welding wire into welding rings through a ring making machine.

Citation Information

Patent Citations

  • Brass strip core flux-cored welding ring and preparation method thereof

    CN104384758A

  • Brass flux-cored brazing filler metal with reducing agents and flow aids and preparation method thereof

    CN104907722A

  • Brazing ring and brazing system

    CN107617829A

  • Metal -cored compound silver solder

    CN204686295U

  • From brass medicine core brazing filler metal of taking reductant, flow aid

    CN204843292U