Composite solid electrolyte and preparation method therefor, solid-state battery and electric device
By dispersing the phase change toughener in the solid electrolyte, it undergoes phase change under the action of external force, the problem of prone to cracking of traditional solid electrolytes is solved, the toughness and stability of the battery are improved, and short circuits caused by dendrites are prevented.
Patent Information
- Application Number
- PCT/CN2023/112632
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2023-08-11
- Publication Date
- 2024-11-07
AI Technical Summary
Traditional solid electrolytes are prone to cracking during use, especially when they are combined with lithium metal negative electrodes, the formation of lithium dendrites will lead to fragmentation and short-circuiting of solid electrolytes, which is difficult to meet the practical application needs.
The composite solid electrolyte is used to disperse the phase change toughener in the solid electrolyte substrate, so that it undergoes phase change under the action of external forces, improve mechanical strength and toughness, and prevent internal defects from occurring.
It improves the toughness of solid electrolytes and the service life of the battery, prevents cracking and short circuit caused by dendrites, and enhances the stability of the battery.
Smart Images

Figure CN2023112632_07112024_PF_FP_ABST
Abstract
Description
Composite solid electrolyte and preparation method thereof, solid-state battery and electrical device
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims priority and benefits of the following patent application, all of which are incorporated by reference into this application: Chinese patent application number 202310484808.0, filed with the State Intellectual Property Office of China on May 4, 2023, entitled “Composite solid electrolyte and preparation method thereof, solid-state battery and electrical device”. Technical Field
[0003] The present application relates to the field of battery technology, and in particular to a composite solid electrolyte and a preparation method thereof, a solid-state battery and an electrical device. Background Art
[0004] In recent years, advances in battery research have led to the emergence of solid-state batteries. These batteries replace liquid electrolytes with solid-state electrolytes and can use metals as negative electrode materials, reducing the likelihood of side reactions at high temperatures. Furthermore, solid-state electrolytes give solid-state batteries compact structures, scalability, and design flexibility, making them suitable for driving microelectronic devices, as well as for applications in power and energy storage.
[0005] However, traditional solid-state electrolytes have the problem of poor mechanical strength and easy cracking. Cracks are prone to occur during use, especially when combined with lithium metal negative electrodes. Lithium metal will form dendrites at the solid-state electrolyte interface. The formation of dendrites will cause the solid-state electrolyte to break and even penetrate the solid-state electrolyte, causing short circuits and failures of solid-state batteries, making it difficult to meet the needs of practical applications.
[0006] Summary of the Invention
[0007] Based on this, it is necessary to provide a composite solid electrolyte and its preparation method, a solid-state battery and an electrical device, aiming to improve the toughness of the solid-state electrolyte and thereby improve the efficiency of the solid-state battery.
[0008] This application is achieved through the following technical solutions.
[0009] In a first aspect of the present application, a composite solid electrolyte is provided, wherein the components of the composite solid electrolyte include a solid electrolyte substrate and a phase change toughening agent dispersed in the solid electrolyte substrate, wherein the phase change toughening agent can undergo phase change under the action of an external force.
[0010] The above-mentioned composite solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent dispersed in the solid electrolyte substrate. When subjected to external force, for example, when used in a battery, when affected by lithium dendrites, stress will be generated inside the phase change toughening agent accordingly. Under the stimulation of stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by this phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate, further prevent the generation of internal defects in the solid electrolyte, and thus improve toughness.
[0011] In some embodiments, the phase change toughening agent is uniformly distributed in the grains and grain boundaries of the solid electrolyte substrate.
[0012] As can be understood, a solid electrolyte matrix contains multiple grains. Grain boundaries are interfaces between grains of identical structure but different orientations. At these interfaces, the atomic arrangement transitions from one orientation to another, resulting in a transitional state at the grain boundaries. When observed under a brightfield scanning electron microscope (SEM), these grain boundaries appear dark and black. The aforementioned phase change toughening agent is uniformly distributed within the grains and at the grain boundaries of the solid electrolyte matrix.
[0013] In some embodiments, the dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate is determined by any one of a grid counting method, an intercept method, an area method, an area method, and an exclusive circle method;
[0014] Wherein, H satisfies: H>20%.
[0015] In some embodiments, H satisfies: 20%<H<100%.
[0016] In the above composite solid electrolyte, the dispersion uniformity of the phase change toughening agent in the solid electrolyte matrix is regulated to further make the phase change toughening agent more evenly dispersed in the solid electrolyte matrix, thereby improving the overall toughness of the composite solid electrolyte.
[0017] It can be understood that the physical and chemical states inside the solid electrolyte substrate are called metallographic phases, and the dispersion uniformity of the phase change toughening agent therein can refer to the quantitative test methods of particle distribution uniformity in traditional metallographic analysis methods, including any one of the grid counting method, intercept method, area method, area method and exclusive circle method. These methods are based on different statistical methods for calculation, and there are definite test procedures in this field. For specific definitions and statistical methods, please refer to: [Chang Hongying, Xie Chongjin, Xu Weixin. Quantitative metallographic analysis method for particle distribution uniformity [C] / / 2007 China Iron and Steel Annual Conference Proceedings. 2007].
[0018] In some embodiments, the intercept method is used to test the dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate, comprising the following steps:
[0019] Pressing the composite solid electrolyte into a sample to be tested, and cutting the sample to be tested along a direction parallel to the thickness of the wafer, wherein a cut section formed by cutting the sample to be tested is a cut section to be tested;
[0020] placing the cross section to be measured under a scanning electron microscope to form a scanning electron microscope image;
[0021] In the backscattered electron imaging mode, the solid electrolyte substrate and the phase change toughening agent in the scanning electron microscope image are distinguished according to the contrast, and the distance between any two phase change toughening agent particles in the scanning electron microscope image is measured by the grid line analysis method, which is recorded as di, i ranges from 1 to N, is the average distance between any two phase change toughening agent particles in the scanning electron microscope image, then:
[0022] N is an integer ≥2.
[0023] In some embodiments, the volume distribution particle size Dv50 of the phase change toughening agent satisfies: 50 nm ≤ Dv50 ≤ 100 nm.
[0024] By adjusting the particle size of the phase change toughening agent, the distribution density of the phase change toughening agent and the magnitude of the compressive stress generated during the phase change are further adjusted, thereby further improving the mechanical properties of the composite solid electrolyte.
[0025] In some embodiments, the phase change toughening agent comprises zirconium oxide and a stabilizer.
[0026] While the specific toughening mechanism of phase change toughening agents remains to be studied, researchers speculate that the phase change toughening agent possesses a metastable state, meaning it exists in a high-temperature stable crystal structure at room temperature. This allows the phase change toughening material to undergo a phase transition and volume change when stimulated by external forces, thereby inhibiting the fracture of the solid electrolyte and achieving phase change toughening. For example, pure ZrO2 generally undergoes the following phase transitions during cooling from high temperature to room temperature: cubic phase (c), tetragonal phase (t), and monoclinic phase (m). A t-to-m phase transition occurs at around 1150°C, accompanied by a volume change. If the t and m phase transition points of ZrO2 are stabilized at room temperature, allowing it to undergo a tm phase transition when subjected to external stress at room temperature, the volume effect generated by the phase transition absorbs a large amount of fracture energy, resulting in the material exhibiting exceptionally high fracture toughness and achieving a phase change toughening effect.
[0027] In some embodiments, the phase change toughening agent satisfies at least one of the following conditions (1) to (2):
[0028] (1) In the phase change toughening agent, the mass proportion of the stabilizer is 0.01% to 50%;
[0029] (2) The stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide.
[0030] In some embodiments, the composite solid electrolyte includes at least two phase change toughening agents having different activation energies.
[0031] By adjusting the types of phase change toughening agents in the composite solid electrolyte, using a mixture of phase change toughening agents with higher activation energy and those with lower activation energy, and differentiating the phase change activation conditions of the phase change toughening agents, a hierarchical toughening network is formed that can effectively inhibit defect and crack expansion, thereby further improving the toughness of the composite solid electrolyte.
[0032] In some embodiments, the composite solid electrolyte includes at least two phase change toughening agents with different activation energies.
[0033] In some embodiments, the composite solid electrolyte includes a first phase change toughening agent with an activation energy of T1 and a second phase change toughening agent with an activation energy of T2, and T1 and T2 satisfy 0<T2 / T1<0.8.
[0034] In some embodiments, in the composite solid electrolyte, the total mass of the phase change toughening agent accounts for 2% to 25%.
[0035] Optionally, the total mass proportion of the phase change toughening agent is 5% to 25%;
[0036] Optionally, the total mass proportion of the phase change toughening agent is 10% to 25%;
[0037] Optionally, the total mass proportion of the phase change toughening agent is 15% to 25%.
[0038] The mass proportion of the phase change toughening agent is regulated to further improve the toughness of the composite solid electrolyte while maintaining excellent ionic conductivity.
[0039] In some embodiments, the solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0040] A second aspect of the present application provides a method for preparing a composite solid electrolyte, comprising the following steps:
[0041] The solid electrolyte substrate and the phase change toughening agent are mixed to prepare a composite solid electrolyte.
[0042] The solid electrolyte substrate and the phase change toughening agent are mixed to disperse the phase change toughening agent in the solid electrolyte substrate.
[0043] In some embodiments, the mixing process adopts dry mixing, and the process of preparing the composite solid electrolyte further includes the following steps:
[0044] The mixture after the mixing process is subjected to a pressing process; the pressure used in the pressing process is 300MPa to 550MPa;
[0045] The mixing step adopts wet mixing, and the process of preparing the composite solid electrolyte also includes the following steps:
[0046] The mixture after the mixing treatment is applied to form a film and dried.
[0047] In a third aspect of the present application, a solid-state battery is provided, comprising the composite solid-state electrolyte of the first aspect or the composite solid-state electrolyte prepared by the preparation method of the composite solid-state electrolyte of the second aspect.
[0048] In a fourth aspect of the present application, an electrical device is provided, comprising the solid-state battery of the third aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:
[0050] FIG1 is a schematic diagram of a solid-state battery according to one embodiment;
[0051] FIG2 is a schematic diagram of an embodiment of a battery pack;
[0052] FIG3 is an exploded view of FIG2 ;
[0053] FIG4 is a schematic diagram of an embodiment of an electrical device using a solid-state battery as a power source;
[0054] FIG5 is an electron microscope image of a cross section of the composite solid electrolyte prepared in Example 1.
[0055] Explanation of the accompanying symbols: 1. battery pack; 2. upper box; 3. lower box; 4. battery; 5. electrical device. DETAILED DESCRIPTION
[0056] To make the above-mentioned objects, features, and advantages of the present application more clearly understood, the specific embodiments of the present application are described in detail below. The following description sets forth many specific details to facilitate a full understanding of the present application. However, the present application can be implemented in many other ways than those described herein, and those skilled in the art can make similar modifications without violating the scope of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0057] In this application, unless otherwise specified or limited, the terms "installed," "connected," "connect," "fixed," etc. should be understood in a broad sense. For example, they can refer to fixed connection, detachable connection, or integration; mechanical connection or electrical connection; direct connection or indirect connection through an intermediate medium; internal communication between two elements or interaction between two elements, unless otherwise specified. Those skilled in the art will understand the specific meanings of the above terms in this application based on specific circumstances.
[0058] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of such features. Throughout the description of this application, "plurality" means at least two, for example, two, three, etc., unless otherwise specifically defined.
[0059] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application pertains. The terms used herein in the specification of this application are for the purpose of describing specific embodiments only and are not intended to limit this application. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
[0060] As mentioned above, traditional solid-state electrolytes often share the fragile characteristics of ceramics. Traditionally, efforts have focused on developing new solid-state electrolytes or improving solid-state battery structures, but to date, no significant breakthroughs or progress have been achieved.
[0061] Based on this, after a lot of creative exploration, the composite solid electrolyte with excellent toughness in this application was obtained.
[0062] One embodiment of the present application provides a composite solid electrolyte, the components of which include a solid electrolyte substrate and a phase change toughening agent dispersed in the solid electrolyte substrate, wherein the phase change toughening agent can undergo phase change under the action of an external force.
[0063] The above-mentioned composite solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent dispersed in the solid electrolyte substrate. When subjected to external force, for example, when used in a battery, when affected by lithium dendrites, stress will be generated inside the phase change toughening agent accordingly. Under the stimulation of stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by this phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate, further prevent the generation of internal defects in the solid electrolyte, and thus improve toughness.
[0064] It can be understood that the external force in the above-mentioned "phase change toughening agent will undergo phase change under the action of external force" refers to the effect exerted on the phase change toughening agent by the external environment outside the phase change toughening agent itself. Furthermore, when the external force acts on the phase change toughening agent, it causes the phase change toughening agent to deform, and the various parts within the phase change toughening agent then generate interacting internal forces to resist the action of the external force and attempt to restore the phase change toughening agent from the deformed position to the position before deformation. This internal force is stress. Driven by the stress, a phase change will occur inside the phase change toughening agent, and a large amount of fracture energy will be absorbed due to the volume change caused by the phase change, thereby achieving the effect of phase change toughening.
[0065] In some embodiments, the phase change toughening agent is uniformly distributed in the grains and grain boundaries of the solid electrolyte substrate.
[0066] As can be understood, a solid electrolyte matrix contains multiple grains. Grain boundaries are interfaces between grains of identical structure but different orientations. At these interfaces, the atomic arrangement transitions from one orientation to another, resulting in a transitional state at the grain boundaries. When observed under a brightfield scanning electron microscope (SEM), these grain boundaries appear dark and black. The aforementioned phase change toughening agent is uniformly distributed within the grains and at the grain boundaries of the solid electrolyte matrix.
[0067] In some embodiments, the dispersion uniformity H of the phase change toughening agent in the solid electrolyte matrix is determined by any one of a grid counting method, an intercept method, an area method, an area method, and an exclusive circle method; wherein H satisfies: H>20%.
[0068] In the above composite solid electrolyte, the dispersion uniformity of the phase change toughening agent in the solid electrolyte matrix is regulated to further make the phase change toughening agent more evenly dispersed in the solid electrolyte matrix, thereby improving the overall toughness of the composite solid electrolyte.
[0069] It is understood that the physical and chemical state within the solid electrolyte substrate is referred to as the metallographic phase. The dispersion uniformity of the phase change toughening agent therein can be determined by referring to conventional metallographic analysis methods for quantitatively testing particle distribution uniformity, including any of the grid counting method, intercept method, planimetry, area method, and exclusive circle method. These methods are calculated based on different statistical methods, and there are established testing procedures in the art. For specific definitions and statistical methods, please refer to: [Chang Hongying, Xie Chongjin, Xu Weixin. Quantitative Metallographic Analysis Method for Particle Distribution Uniformity [C] / / 2007 China Iron and Steel Annual Conference Proceedings, 2007]. In some embodiments, H satisfies the following: 20% < H < 100%.
[0070] In the above “20%<H<100%”, the value of H includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 21%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 99%, 100%; or a range consisting of any two values, for example, 21% to 99%, 25% to 99%, 30% to 99%, 35%~99%, 40%~99%, 45%~99%, 50%~99%, 21%~99%, 21%~99%, 21%~99%, 21%~99%, 51%~99%, 55%~99%, 60%~99%, 65%~99%, 70%~99%, 75%~99%, 80%~99%, 51%~95%, 55%~95%, 60%~95%, 65%~95%, 70%~95%, 75%~95%, 80%~95%, 51%~90%, 55%~90%, 60%~90%, 65%~90%, 70%~90%, 75%~90%, 80%~90%, 51%~85%, 55%~85%, 60%~85%, 65%~85%, 70%~85%, 75%~85%, 80%~85%, 51%~80%, 55%~80%, 60%~80%, 65%~80%, 70%~80%, 75%~80%, 51%~75%, 55%~75%, 60%~75%, 65%~75%, 70%~75%, 51%~70%, 55%~70%, 60%~70%, 65%~70%.
[0071] In some embodiments, the intercept method is used to test the dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate, comprising the following steps:
[0072] The composite solid electrolyte is pressed into a sample to be tested, and the sample to be tested is cut along a thickness direction parallel to the sample to be tested, and the cut cross section formed when the sample to be tested is the cross section to be tested;
[0073] placing the cross section to be measured under a scanning electron microscope to form a scanning electron microscope image;
[0074] In the backscattered electron imaging mode, the solid electrolyte substrate and the phase change toughening agent in the scanning electron microscope image are distinguished based on the contrast, and the distance between any two phase change toughening agent particles in the scanning electron microscope image is measured by the grid line analysis method, which is recorded as di, i ranges from 1 to N, is the average distance between any two phase change toughening agent particles in the scanning electron microscope image, then:
[0075] N is an integer ≥2.
[0076] In some embodiments, the composite solid electrolyte is pressed into a disc-shaped sample to be tested.
[0077] Optionally, the wafer has a thickness of 100 μm to 2000 μm.
[0078] In some embodiments, in the step of pressing the composite solid electrolyte into a sample to be tested, the pressure used is 300 MPa to 550 MPa; further, the pressure used is 500 MPa.
[0079] Specifically, the grid line analysis method is to determine the distance between any two phase change toughening agent particles in the scanning electron microscope image by setting a grid for line analysis in the scanning electron microscope image, which is also called the intercept. Specifically, the grid is spread over the entire scanning electron microscope image so that the intercept can be confirmed by the grid.
[0080] Optionally, the minimum unit of the grid used is a square grid with a side length of 5 μm.
[0081] It should be noted that contrast refers to the difference in brightness between different areas on the image, that is, in the backscattered electron imaging mode, the difference in brightness between the solid electrolyte substrate and the phase change toughening agent in the scanning electron microscope image. The solid electrolyte substrate and the phase change toughening agent in the scanning electron microscope image can be distinguished based on the contrast.
[0082] In some embodiments, the sample to be tested is a wafer, and when the wafer is cut parallel to the thickness direction of the wafer, the cutting point is located at the diameter of the bottom surface of the wafer.
[0083] It should be noted that when cutting the sample to be tested, it can be parallel to the thickness direction of the sample to be tested, or it can be perpendicular to the thickness direction of the sample to be tested. Specifically, the cross section is the cross section formed by cutting perpendicular to the height or thickness direction, and the longitudinal section is the cross section formed by cutting parallel to the height or thickness direction. For example, for a cylinder, its cross section is the cross section formed by cutting perpendicular to the height direction, which is a circle, and its longitudinal section is the cross section formed by cutting parallel to the height direction, which is a rectangle. The height of the cylinder can also be called thickness. If the height of the cylinder is relatively low, for example, the height is less than the bottom diameter of the cylinder, then the cylinder is a disc, and the common height is called thickness.
[0084] In some embodiments, when the wafer is cut perpendicular to the thickness of the wafer, the cutting point is located at 1 / 2 of the thickness of the wafer.
[0085] In some embodiments, the volume distribution particle size Dv50 of the phase change toughening agent satisfies: 50 nm ≤ Dv50 ≤ 100 nm.
[0086] By adjusting the particle size of the phase change toughening agent, the distribution density of the phase change toughening agent and the magnitude of the compressive stress generated during the phase change are further adjusted, thereby further improving the mechanical properties of the composite solid electrolyte.
[0087] In the above “50nm≤Dv50≤100nm”, the value of Dv50 includes the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 50nm, 55nm, 60nm, 65nm, 70nm, 75nm, 80nm, 85nm, 90nm, 95nm, 100nm; or a range consisting of any two values, for example, 50nm~ 55nm, 50nm~60nm, 50nm~65nm, 50nm~70nm, 50nm~75nm, 50nm~80nm, 50nm~85nm, 50nm~90nm, 50nm~95 nm, 50nm~100nm, 55nm~60nm, 55nm~65nm, 55nm~70nm, 55nm~75nm, 55nm~80nm, 55nm~85nm, 55nm~90n m, 55nm~95nm, 55nm~100nm, 60nm~65nm, 60nm~70nm, 60nm~75nm, 60nm~80nm, 60nm~85nm, 60nm~90nm , 60nm~95nm, 60nm~100nm, 65nm~70nm, 65nm~75nm, 65nm~80nm, 65nm~85nm, 65nm~90nm, 65nm~95nm, 65nm~100nm, 70nm~75nm, 70nm~80nm, 70nm~85nm, 70nm~90nm, 70nm~95nm, 70nm~100nm, 75nm~80nm, 75nm~85nm, 75nm~90nm, 75nm~95nm, 75nm~100nm, 80nm~85nm, 80nm~90nm, 80nm~95nm, 80nm~100nm.
[0088] In this application, Dv50 refers to the particle size at which the cumulative volume distribution percentage of a material reaches 50%. It can be measured using instruments and methods known in the art. For example, it can be conveniently measured using a laser particle size analyzer, as described in GB / T 19077-2016: Particle Size Distribution - Laser Diffraction Method. The testing instrument can be a Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd., UK.
[0089] In some embodiments, the phase change toughening agent comprises zirconium oxide and a stabilizer.
[0090] Although the specific toughening mechanism of phase change toughening agents remains to be studied, technicians speculate as follows: phase change toughening agents have a metastable state, that is, phase change toughening agents exist in a high-temperature stable crystal structure at room temperature, which makes the phase change toughening material undergo phase change and volume change when stimulated by external force, thereby inhibiting the fracture of the solid electrolyte and playing a role in phase change toughening. For example: pure ZrO2 will generally undergo the following phase change in the process of cooling from high temperature to room temperature: cubic phase (c), tetragonal phase (t) to monoclinic phase (m), among which t to m phase change will occur at about 1150°C, accompanied by volume change. The tm phase transition point of ZrO2 is stabilized to room temperature by a stabilizer, so that it can produce tm phase change when induced by external force at room temperature. Due to the volume effect generated by the phase change, a large amount of fracture energy is absorbed, so that the material exhibits abnormally high fracture toughness, achieving the effect of phase change toughening.
[0091] In some embodiments, the stabilizer accounts for 0.01% to 50% by weight of the phase change toughening agent.
[0092] In some embodiments, the stabilizer contains at least one element selected from the group consisting of yttrium, scandium, magnesium, calcium, and cesium.
[0093] In some embodiments, the stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide.
[0094] When the stabilizers are yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide, the toughening agents are recorded as YSZ, SSZ, MSZ, CSZ, and CsSZ, respectively.
[0095] Optionally, the stabilizer comprises yttrium oxide.
[0096] In the above “0.01% to 50%”, the values include the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include, but are not limited to, the point values in the embodiments and the following point values: 0.01%, 0.05%, 0.1%, 1%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%; or a range consisting of any two values, for example, 1% to 50%, 5% to 50%, 10% to 50%, 15% to 50%, 20% to 50%, 25% to 50%, 30% to 50%, 35% to 50%, 40% to 50%, 45% to 50%, 1% to 45%, 5% to 45%, 10% to 45%, 15% to 45%, 20% to 45%, 25% to 45%, 30%~45%, 35%~45%, 40%~45%, 1%~40%, 5%~40%, 10%~40%, 15%~40%, 20%~40%, 25%~40%, 30%~40%, 35%~40%, 1%~35%, 5%~35%, 10%~35%, 15%~35%, 20%~35%, 25%~35%, 30%~35%, 1%~30%, 5%~30%, 10%~30%, 15%~30%, 20%~30%, 1%~25%, 5%~25%, 10%~25%, 15%~25%, 20%~25%.
[0097] In some embodiments, the composite solid electrolyte includes at least two phase change toughening agents having different activation energies.
[0098] By adjusting the type of phase change toughening agent in the composite solid electrolyte, at least two phase change toughening agents with different activation energies are used, that is, phase change toughening agents with higher activation energy and phase change toughening agents with lower activation energy are mixed, and the phase change activation conditions of the phase change toughening agents are differentiated, a hierarchical toughening network is formed that can effectively inhibit the expansion of defects and cracks, thereby further improving the toughness of the composite solid electrolyte.
[0099] In some embodiments, the composite solid electrolyte includes a first phase change toughening agent with an activation energy of T1 and a second phase change toughening agent with an activation energy of T2, where T1 and T2 satisfy 0<T2 / T1<0.8.
[0100] By adjusting the activation energy ratio of two phase change toughening agents with different activation energies, the hierarchical toughening network is further improved.
[0101] It should be noted that: "activation energy" refers to the energy required for a molecule to change from a normal state to an active state that is prone to chemical reactions. Furthermore, the activation energy of a substance can be calculated by testing the Arrhenius formula. Specifically, the above-mentioned phase change toughening agent can be purchased through commercial channels, and the activation energy of the phase change toughening agent can be obtained by querying the product attribute parameter information or querying relevant literature records.
[0102] In some embodiments, the mass ratio of the first phase change toughening agent to the second phase change toughening agent is 1:(10-1).
[0103] In the above “1:(10-1)”, the values include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiment and the following point values: 1:10, 1:9, 1:8, 1:7, 1:6, 1:5, 1:4, 1:3, 1:2, 1:1; or a range consisting of any two values, for example, 1:(9-1), 1:(8-1), 1:(7-1), 1:(6-1), 1:(5-1), 1:(4-1), 1:(3-1), 1:(2-1), 1:(1 0~2), 1:(9~2), 1:(8~2), 1:(7~2), 1:(6~2), 1:(5~2), 1:(4~2), 1:(3~2), 1:(10~3), 1:(9~3), 1:(8~3), 1:(7~3), 1:(6~3), 1:(5~3), 1:(4~3), 1:(10~4), 1:(9~4), 1:(8~4), 1:(7~4), 1:(6~4), 1:(5~4), 1:(4~3), 1:(10~5), 1:(9~5), 1:(8~5), 1:(7~5), 1:(6~5).
[0104] In some embodiments, in the composite solid electrolyte, the total mass of the phase change toughening agent accounts for 2% to 25%.
[0105] In some embodiments, in the composite solid electrolyte, the total mass proportion of the phase change toughening agent is 5% to 25%.
[0106] In some embodiments, in the composite solid electrolyte, the total mass of the phase change toughening agent accounts for 10% to 25%.
[0107] In some embodiments, in the composite solid electrolyte, the total mass of the phase change toughening agent accounts for 15% to 25%.
[0108] The mass proportion of the phase change toughening agent is regulated to further improve the toughness of the composite solid electrolyte while maintaining excellent ionic conductivity.
[0109] In the above-mentioned "2% to 25%", the values include the minimum and maximum values of the range, and every value between the minimum and maximum values. Specific examples include but are not limited to the point values in the embodiments and the following point values: 2%, 5%, 10%, 15%, 20%, 25%; or a range consisting of any two numerical values, for example, it can be 2% to 5%, 2% to 10%, 2% to 15%, 2% to 20%, 2% to 25%, 5% to 10%, 5% to 15%, 5% to 20%, 5% to 25%, 10% to 15%, 10% to 20%, 10% to 25%, 15% to 20%, 15% to 25%, 20% to 25%.
[0110] In some embodiments, the solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte, and a potassium ion solid electrolyte.
[0111] The above-mentioned lithium ion solid electrolyte, sodium ion solid electrolyte and potassium ion solid electrolyte can be various lithium ion solid electrolytes, sodium ion solid electrolytes and potassium ion solid electrolytes commonly used in the art.
[0112] In some embodiments, the solid electrolyte substrate is a lithium-ion solid electrolyte.
[0113] Examples of lithium-ion solid electrolytes are provided here, including but not limited to:
[0114] LISICON type: such as γ-Li3PO4, etc.;
[0115] NASICON type; such as Li (1+x1) Q x M (2-x1) (PO4)3, 0≤x1<1, Q includes at least one of Al, Cr, Ba, Fe, Sc, In, Lu, Y, and La;
[0116] Garnet type; for example, Li (7-x2) La3Zr (2-x2) M x2 O12, etc., 0≤x2<1, M includes at least one of Sb, Nb, Ta, Te, and W;
[0117] LIPON type: such as Li x3 PO y1 N z1 ;0 <x3≤1,0<y1≤1,0<z1≤1;
[0118] Perovskite type: such as Li3 x 4Q (2 / 3-x4)MO3, etc., 0.04 < x4 < 0.17, Q includes at least one of La, Sr, Ba, Nd, M includes at least one of Al, Ti, Ge;
[0119] Anti-Perovskite type: such as Li3OCl, etc.; Thio-LiSICON type: such as Li (3+x5) My2A (1-y2) Q (4-z2) T z2 , where -1 < x5 < 2, 0 ≤ y2 ≤ 1, 0 ≤ z2 ≤ 2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, T includes at least one of F, Cl, Br, I;
[0120] Sulfide solid electrolyte, including: Thiophosphate type: Li3PS4, etc., Argyrodite type: Li6PS5Cl, Halide type: Li3InCl6, Hydride type: 0.7Li(CB9H 10 ) - 0.3Li(CB 11 H 12 ), etc.; such as Li (10+x6) M (1+y3) A (2-y3) Q (12-z3) H z3 type: where -2 < x6 < 2, 0 ≤ y3 ≤ 2, 0 ≤ z3 ≤ 2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo; A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, H includes at least one of F, Cl, Br, I: (100 - x7)Li2S·x7M·y4Q type: where 20 ≤ x7 ≤ 30, 0 ≤ y4 ≤ 50, M includes at least one of B2S3, Al2S3, In2S3, SiS2, GeS2, SnS2, P2S5, As2S3, Sb2S5, Bi2S3, WS2, MoS2, Q includes at least one of B2O3, Al2O3, In2O3, SiO2, GeO2, SnO2, P2O5, Sb2O5, Bi2O3, WO2, WO3, MoO2, MoO3, Fe2O3, ZnO, MgO, CuO, CaO, LiN, Li2O, LiF, LiCl, LiBr, LiI; Argyrodite type: Li (6+x8) M y5 A (1-y5) Q (5-z5) T (1+z5), where -1 ≤ x8 ≤ 1, 0 ≤ y5 ≤ 1, -1 < z5 ≤ 1, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, T includes at least one of F, Cl, Br, I; Halide type: Li3MJ or Li2Sc 2 / 3 J; M includes at least one of Y, Er, In, Sc, Ga, and J includes at least one of F, Cl, Br, I.
[0121] When the above sulfide solid electrolyte is a sulfide-based solid electrolyte, it includes but is not limited to: argyrodite electrolyte; binary sulfide-based solid systems such as Li2S-P2S5, Li2S-SiS2, Li2S-GeS, and Li2S-B2S3, and ternary systems of Li2S-Me-P2S5, where Me is selected from Si, Ge, Sn, or Al, etc.
[0122] Specifically, the above sulfide electrolyte is selected from at least one of Li2S-P2S5, Li2S-SiS2, Li2S-GeS, Li2S-B2S3, and Li2S-Me-P2S5.
[0123] Sodium solid electrolytes include but are not limited to: NASICON type: Na(1 + x9 + 2y5)Zr (2-y5) M y5 P (3-x9) Si x9 O 12 , 0 ≤ x9 ≤ 3, 0 ≤ y5 ≤ 1, M includes at least one of Zn, Mg, Ca; Na-β-alumina type: Na2O·2Al2O3 or Na2O·3Al2O3, etc.; Na (3+x10) M y6 A (1-y6) Q (4-z6) T z6 type, where -1 < x10 < 2, 0 ≤ y6 ≤ 1, 0 ≤ z6 ≤ 2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes at least one of P, As, Sb, Bi, Q includes at least one of S, Se, T includes at least one of F, Cl, Br, I; Na (11+x11) M (2-y7) A (1+y7) Q (12-z7) T z7Type where -1 < x11 < 1, 0 ≤ y7 ≤ 2, 0 ≤ z7 ≤ 2, M includes at least one of B, Al, In, Si, Ge, Sn, Ti, W, Mo, A includes P, As, Sb, Bi; Q = at least one of S, Se, T includes at least one of F, Cl, Br, I; inverse perovskite type Na3OX, X includes at least one of Cl, Br, I, BH4.
[0124] Potassium ion solid electrolytes include, but are not limited to: β - Alumina type such as K2O·x13Al2O3, etc., x13 takes any number from 8 to 11, Anti - Perovskite type such as K3OI, at least one of K2Fe4O7 type, KSi2P3 type.
[0125] One embodiment of the present application further provides a preparation method of a composite solid electrolyte, including the following step S10.
[0126] Step S10: Mix the solid electrolyte substrate and the phase - change toughening agent to prepare a composite solid electrolyte. [[ID=1']]
[0127] In the above - mentioned preparation method, the solid electrolyte substrate and the phase - change toughening agent are mixed so that the phase - change toughening agent is dispersed in the solid electrolyte substrate.
[0128] The types and further mass ratios of the solid electrolyte substrate and the phase - change toughening agent are as described above and will not be elaborated here.
[0129] In some of these embodiments, the mixing time is 0.5 h to 24 h.
[0130] In some of these embodiments, in step S10, the mixing treatment is carried out by dry mixing. During the process of preparing the composite solid electrolyte, the following steps are further included:
[0131] Press the mixture after the mixing treatment; the pressure used for the pressing treatment is 300 MPa to 500 MPa.
[0132] It can be understood that dry mixing is to directly mix the solid electrolyte substrate and the phase - change toughening agent, which can be specifically carried out by a blender.
[0133] In some of these embodiments, in step S10, the mixing treatment step is carried out by wet mixing. During the process of preparing the composite solid electrolyte, the following steps are further included:
[0134] Coat the mixture after the mixing treatment into a film and dry it.
[0135] Optionally, the thickness of the film - like mixture is 10 μm to 500 μm.
[0136] In some embodiments, the wet mixing method is to mix the solid electrolyte matrix, the phase change toughening agent, and the solvent to form a mixture slurry.
[0137] Optionally, the solvent may be at least one of water, a small molecule alcohol, and an alcohol ether solvent. Further optionally, the small molecule alcohol includes ethanol, propanol, and the like.
[0138] The purpose of the drying step is to dry the solvent in the wet film formed by coating. There are no special requirements for the drying temperature or drying time. It is sufficient to evaporate the solvent in the wet film formed by coating and dry it. Specifically, the drying methods commonly used in the art can be used, including but not limited to: vacuum drying, heating drying, etc.
[0139] In some embodiments, the mixing time includes but is not limited to: 0.5 h to 24 h.
[0140] Furthermore, the mixing step is carried out under stirring conditions; for example, in a ball mill without adding grinding balls, because the force generated by the rotation of the ball mill causes the materials to be mixed.
[0141] In some embodiments, the rotation speed of the ball mill is 100 rpm to 300 rpm.
[0142] It can be understood that without adding grinding balls, the rotation of the ball mill has little effect on the particle size of the material, and the particle size change before and after the material mixing is small.
[0143] One embodiment of the present application provides a solid-state battery, which includes the above-mentioned composite solid-state electrolyte or a composite solid-state electrolyte prepared by the above-mentioned method for preparing the composite solid-state electrolyte.
[0144] The above-mentioned composite solid electrolyte includes a solid electrolyte substrate and a phase change toughening agent dispersed in the solid electrolyte substrate. When subjected to external force, for example, when applied to a battery, when affected by lithium dendrites, stress will be generated inside the phase change toughening agent accordingly. Under the stimulation of stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by this phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate, further prevent the generation of internal defects in the solid electrolyte, thereby improving toughness and thus improving the service life of the battery.
[0145] In some embodiments, in the above-mentioned solid-state battery, the composite solid-state electrolyte exists in the form of a membrane; further, the above-mentioned solid-state battery also includes a positive electrode sheet and a negative electrode sheet, and the composite solid-state electrolyte membrane is arranged between the electrode sheet and the negative electrode sheet.
[0146] The positive electrode sheet and the negative electrode sheet may be those commonly used in the art, and the positive electrode sheet and the negative electrode sheet are described herein by way of non-limiting examples.
[0147] [Negative electrode]
[0148] The negative electrode sheet includes a positive electrode current collector and a negative electrode active layer loaded on the surface of the positive electrode current collector.
[0149] The components of the negative electrode active layer include a negative electrode active material.
[0150] The above-mentioned negative electrode active material can adopt the commonly used negative electrode active materials in this application, including at least one of metallic lithium negative electrode materials, carbon family negative electrode materials, oxide negative electrode materials, and silicon-based negative electrode materials.
[0151] In any embodiment of the present application, the above-mentioned negative electrode active material includes metallic lithium, lithium-containing alloys, lithium-containing composites, mesophase carbon microspheres, graphite, glassy carbon, carbon nanotubes, carbon-carbon composites, carbon fibers, hard carbon, soft carbon, magnesium oxide, silicon-carbon composites, TiO2, MoO2, In2O3, Al2O3, Cu2O, VO2, SnO x 、SiO x , Ga2O3, Sb2O5, Bi2O.
[0152] In any embodiment of the present application, the mass proportion of the negative electrode active material in the negative electrode active layer is 70% to 99.9%.
[0153] In any embodiment of the present application, the components of the negative electrode active layer further include a negative electrode conductive agent and a negative electrode binder.
[0154] In any embodiment of the present application, the negative electrode conductive agent may be a conductive material commonly used in the art, including but not limited to at least one of graphite, carbon nanotubes, nanofibers, carbon black, and graphene. Specifically, the negative electrode conductive agent may be selected from at least one of SP, KS-6, acetylene black, branched Ketjen black ECP, SFG-6, vapor-grown carbon fiber VGCF, carbon nanotubes CNTs, graphene, and composite conductive agents thereof.
[0155] The weight ratio of the negative electrode conductive agent in the negative electrode active layer is 0 to 20 wt % based on the total weight of the negative electrode active layer.
[0156] The negative electrode binder can be a binder commonly used in the art, and can be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0157] The weight ratio of the negative electrode binder in the negative electrode active layer is 0 to 30 wt % based on the total weight of the negative electrode active layer.
[0158] In any embodiment of the present application, the negative electrode active layer may further optionally include other additives, such as a thickener, such as sodium carboxymethyl cellulose (CMC-Na), etc. Based on the total weight of the negative electrode active layer, the weight ratio of the other additives in the negative electrode active layer is 0 to 15 wt%.
[0159] In any embodiment of the present application, the current collector in the negative electrode sheet may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material on a polymer substrate.
[0160] Optionally, the metal material includes at least one of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy.
[0161] Optionally, the polymer substrate includes at least one of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0162] In any embodiment of the present application, the negative electrode sheet can be prepared by the following method: the above-mentioned components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0163] In some embodiments, the solvent is water, such as deionized water.
[0164] In some embodiments, the negative electrode slurry has a solid content of 30 wt% to 70 wt%, and the viscosity at room temperature is adjusted to 2000 mPa·s to 10000 mPa·s. The obtained negative electrode slurry is coated on the negative electrode current collector, dried, and cold pressed, such as by rollers, to obtain a negative electrode sheet. The negative electrode powder coating unit area density is 75 mg / m 2 ~220 mg / m 2 , the compaction density of the negative electrode is 1.2g / m 3 ~2.0g / m 3 .
[0165] [Positive electrode]
[0166] The positive electrode sheet includes a positive electrode current collector and a positive electrode active layer loaded on the surface of the positive electrode current collector.
[0167] The components of the positive electrode active layer include a positive electrode active material.
[0168] In some embodiments, the mass proportion of the positive electrode active material in the positive electrode active layer is 70% to 100%.
[0169] In some embodiments, the positive electrode active material may be a positive electrode active material for a secondary battery known in the art.
[0170] In any embodiment of the present application, the positive electrode active material includes any one of a sodium ion positive electrode active material and a lithium ion positive electrode active material.
[0171] As an example, the lithium ion active material may include at least one of the following materials: lithium phosphates containing olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of lithium transition metal oxides may include but are not limited to lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), lithium manganese phosphate (such as LiMnPO4), and lithium manganese iron phosphate.
[0172] In any embodiment of the present application, the molecular formula of the lithium ion active material is: LiFe x Mn (1-x) PO4, x is any number from 0 to 1.
[0173] It can be understood that when x is 0, LiFe x Mn (1-x) PO4 is LiMnPO4 lithium manganese phosphate, and when x is 1, LiFePO4 is LiFePO4 lithium iron phosphate.
[0174] As an example, the sodium ion positive electrode active material may include at least one of the following materials: a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound. However, the present application is not limited to these materials, and other conventionally known materials that can be used as sodium ion battery positive electrode active materials may also be used.
[0175] In any embodiment of the present application, the positive electrode active material includes at least one of a sodium transition metal oxide, a polyanionic compound, and a Prussian blue compound;
[0176] Optionally, the positive electrode active material includes at least one of a sodium transition metal oxide and a polyanionic compound.
[0177] Sodium transition metal oxides have a layered transition metal structure. Compared to the rhombohedral phase of Prussian blue compounds, theoretically, layered transition metal structures should have a greater thickness rebound rate. However, in practice, Prussian blue compounds easily absorb water, forming crystalline water and vacancy defects, which increase the thickness rebound rate and even cause structural collapse. Therefore, when sodium transition metal oxides are used as positive electrode active materials, the thickness rebound rate of the positive electrode sheet is actually smaller.
[0178] The anionic structural units in the polyanionic compound are connected into a three-dimensional structure through covalent bonds, and the structure has good stability. When it is used as a positive electrode active material, the thickness rebound rate of the positive electrode sheet is low.
[0179] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Sodium transition metal oxide is, for example, Na x MO2, wherein M includes at least one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.
[0180] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. Transition metals include at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y includes at least one of P, S, and Si; n represents (YO4) n- valence.
[0181] Polyanionic compounds can also be sodium ions, transition metal ions, tetrahedral (YO4) n- A class of compounds containing anion units and halogen anions. The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y includes at least one of P, S, and Si, and n represents (YO4) n- valence state; the halogen may be at least one of F, Cl and Br.
[0182] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y includes at least one of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, including at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce, m represents (ZO y ) m+ valence state; the halogen may be at least one of F, Cl and Br.
[0183] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y At least one of (0≤y≤1).
[0184] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ). The transition metal includes at least one of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' each independently include at least one of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.
[0185] In any embodiment of the present application, the components of the positive electrode active layer further include a positive electrode binder, and the mass proportion of the positive electrode binder in the positive electrode active layer is 0.05% to 10%.
[0186] Optionally, the mass proportion of the positive electrode binder in the positive electrode active layer is 0.1% to 8%.
[0187] The positive electrode binder can be any of various binders commonly used in the art. As an example, the positive electrode binder includes at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorine-containing acrylate resin, sodium carboxymethyl cellulose, hydroxypropyl cellulose, sodium hydroxymethyl cellulose, potassium hydroxymethyl cellulose, diacetyl cellulose, polyacrylic acid, sodium alginate, styrene-butadiene rubber, acrylic butadiene rubber, polypyrrole, polyaniline, epoxy resin, and guardo gum.
[0188] In any embodiment of the present application, the components of the positive electrode active layer further include a positive electrode conductive agent, and the mass proportion of the positive electrode conductive agent in the positive electrode active layer is 0.05% to 8%.
[0189] Optionally, the mass proportion of the positive electrode conductive agent in the positive electrode active layer is 0.1% to 6%.
[0190] As an example, the positive electrode conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0191] The positive electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base material. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer base material (such as a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0192] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the positive electrode conductor, the positive electrode binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0193] In some embodiments, the solid-state battery is an all-solid-state battery or a semi-solid-state battery.
[0194] In some embodiments, in a solid-state battery, the composite solid-state electrolyte exists in the form of a composite solid-state electrolyte membrane, which is located between the positive electrode sheet and the negative electrode sheet.
[0195] In some embodiments, the positive electrode sheet and the negative electrode sheet can be made into an electrode assembly through a winding process or a lamination process.
[0196] Furthermore, the solid-state battery further includes a shell for packaging the positive electrode sheet, the negative electrode sheet, and the composite solid-state electrolyte membrane.
[0197] In some embodiments, the housing may be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. Alternatively, the housing may be a soft package, such as a bag-type soft package. The soft package may be made of plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0198] The present application has no particular limitation on the shape of the battery, which can be cylindrical, square, or any other shape. For example, FIG1 shows a solid-state battery 4 with a square structure as an example.
[0199] The present application also provides an electrical device, which includes the above-mentioned solid-state battery.
[0200] Furthermore, in the above-mentioned electrical device, the solid-state battery may exist in the form of a battery cell, or may be further assembled into a battery pack.
[0201] Figures 2 and 3 illustrate an example battery pack 1. Battery pack 1 includes a battery case and one or more solid-state batteries 4 disposed within the case. The case comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for the batteries 4.
[0202] Multiple solid-state batteries 4 can be arranged in the battery box in any manner.
[0203] The above-mentioned solid-state battery or the battery pack assembled therefrom can be used as a power source for an electrical device or as an energy storage unit for an electrical device.
[0204] The above-mentioned electrical devices may be, but are not limited to, mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0205] Figure 4 shows an example of an electric device 5. The electric device 5 is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the electric device 5, a battery pack can be used.
[0206] As another example, the power-consuming device may be a mobile phone, a tablet computer, a laptop computer, etc. Such a device is usually required to be light and thin, and may use a battery as a power source.
[0207] The present application will be described below in conjunction with specific embodiments, but the present application is not limited to the following embodiments. It should be understood that the attached claims summarize the scope of the present application. Under the guidance of the concept of the present application, those skilled in the art should realize that certain changes made to the various embodiments of the present application will be covered by the spirit and scope of the claims of the present application.
[0208] The following are specific examples.
[0209] Example 1
[0210] 1. Preparation of composite solid electrolyte, the specific steps are as follows:
[0211] S1: The solid electrolyte substrate (Li6PS5Cl) and the phase change toughening agent were dry-mixed using a Fritsch Pulverisette planetary ball mill at 200 rpm for 6 h to obtain a mixture.
[0212] Among them, the phase change toughening agent includes zirconium oxide and stabilizer. The mass of the phase change toughening agent is used as the calculation basis, and the mass proportion of the stabilizer is recorded as Y1;
[0213] Referring to GB / T 19077-2016 particle size distribution laser diffraction method, a laser particle size analyzer is used to measure the Dv50 of the phase change toughening agent, which indicates the particle size corresponding to 50% of the cumulative volume distribution percentage of the material. The testing instrument can be the Mastersizer 2000E laser particle size analyzer produced by Malvern Instruments Ltd., UK.
[0214] Taking the total mass of the mixture as the calculation basis, the mass proportion of the phase change toughening agent is recorded as Y2;
[0215] The phase change toughening agents used above were purchased from commercial channels, and the activation energy of the phase change toughening agents was recorded as T n , n corresponds to the type of phase change toughening agent. If there are multiple types, the activation energy of each type is recorded as T1, T2…T n , please see Table 1 for specific parameters.
[0216] S2: The mixture was placed in a mold and pressed at a pressure of 500 MPa for 10 minutes to obtain a composite solid electrolyte in the form of a disc with a thickness of 1 mm.
[0217] S3: Performance testing of composite solid electrolyte.
[0218] (1) Test of the dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate:
[0219] 1. Cut the disc parallel to the thickness of the disc-shaped composite solid electrolyte, with the cutting line located at the diameter of the disc, and the cutting cross section formed when cutting the disc is the cross section to be measured;
[0220] 2. Place the cross section to be measured under a scanning electron microscope to form a scanning electron microscope image;
[0221] 3. In the backscattered electron imaging mode, the solid electrolyte substrate and the phase change toughening agent in the scanning electron microscope image are distinguished based on the contrast, and the distance between any two phase change toughening agent particles in the scanning electron microscope image is determined by the grid line analysis method: that is, a grid for line analysis is set in the scanning electron microscope image to determine the distance between any two phase change toughening agent particles in the scanning electron microscope image, which is denoted as di, and i is 1, 2, 3, ,, N, is the average distance between any two phase change toughening agent particles in the scanning electron microscope image. Specifically, the scanning electron microscope image is covered with a grid so that the intercept can be confirmed by the grid. The dispersion uniformity H is calculated as follows:
[0222] N is an integer.
[0223] The smallest unit of the grid used is a square grid unit with a side length of 5 μm. Please see Table 1 for specific results.
[0224] Among them, the scanning electron microscope image of the cross section of the composite solid electrolyte to be tested is shown in FIG5 , from which it can be clearly seen that the phase change toughening agent is dispersed throughout the electrolyte substrate.
[0225] (2) Fracture toughness test of composite solid electrolyte:
[0226] Fracture toughness is a parameter that describes the ability of a material to absorb strain energy before fracture. The fracture toughness value (K IC ) indicates a stronger resistance to crack propagation, which also reflects the composite solid electrolyte's ability to resist cracking and short circuiting caused by dendrites. Fracture toughness can be measured using a four-point bending test or a Vickers cone indentation test. The Vickers cone indentation test is used here. The specific process is as follows:
[0227] In an argon atmosphere, the surface of the composite solid electrolyte disc is polished with sandpaper, starting from 800 mesh, then to 2000 mesh, then to 4000 mesh, and finally to 8000 mesh, until the disc surface shows mirror properties without obvious defects. Then, the polished surface is subjected to an indentation test using a Vickers cone indentation tester. The indentation tester is driven with an appropriate load P until radial cracks appear at the four corners of the cone indentation. According to the indentation load P, radial crack extension length C, and microhardness H obtained during the test, the indentation load P and radial crack extension length C are calculated. V , the fracture toughness value K is further calculated by the following formula IC :
[0228] Where P is the indentation load when cracks appear, in N; C is the extension length of radial cracks, in mm; H V is the microhardness, unit is kgf / mm 2 ; E is Young's modulus, unit is GPa; K IC is the fracture toughness of the solid electrolyte, the unit is MPa·m 1 / 2 .
[0229] (3) Critical current density test of composite solid electrolyte
[0230] The critical current density refers to the minimum current density at which dendrites and short circuits occur when electrochemical deposition of a composite solid electrolyte material occurs in combination with the corresponding alkali metal electrode. In other words, dendrites and short circuits will not occur when electrochemical deposition of the composite solid electrolyte occurs below the critical current density.
[0231] The critical current density of the composite solid electrolyte is measured by the traditional symmetrical battery step-by-step current density cycle method. Taking lithium-ion solid electrolyte as an example, the process is as follows:
[0232] The above composite solid electrolyte disc is made into a lithium / solid electrolyte / lithium symmetrical solid-state battery. After the solid-state battery is assembled and packaged, the solid-state battery is made to 2 Starting with a current of 1 mAh / cm, 1 mAh / cm 2 After lithium, the current was increased to 0.5 mA / cm 2 , maintain 1mAh / cm 2 After the surface capacity deposition and stripping, the current is increased to 0.75mA / cm 2 , 1.0mA / cm 2 , 1.25mA / cm 2 ...to 10mA / cm 2 , and monitor the voltage change during the process. The current density when the voltage suddenly drops sharply is recorded as the critical current density (Jc). The specific results are shown in Table 1.
[0233] Among them, the preparation of the composite solid-state battery is as follows:
[0234] Preparation of solid electrolyte membrane: The solid electrolyte material and binder nitrile rubber (NBR) prepared above are dissolved in xylene at a mass ratio of 98:2, and the mixture is thoroughly stirred to prepare a solid electrolyte slurry; the solid electrolyte slurry is coated on polyethylene terephthalate (PET), and then dried, cold pressed, slit, and processed into a solid electrolyte membrane.
[0235] Preparation of positive electrode sheets: The positive electrode active material, the above-mentioned solid electrolyte, the binder nitrile rubber (NBR), and the conductive agent VGCF are dissolved in xylene in a mass ratio of 85:13:1:1, and the mixture is thoroughly stirred and mixed to prepare a positive electrode slurry; the positive electrode slurry is evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and cut to obtain positive electrode sheets;
[0236] Preparation of negative electrode sheets: Pure lithium metal foil is shaped and rolled to form a 50μm lithium metal foil, which is then rolled again to cover one side of the copper foil and cut to obtain negative electrode sheets.
[0237] The solid electrolyte membrane is placed between the negative electrode sheet and the positive electrode sheet, and they are bonded to ensure close contact at the interface to form a solid-state battery.
[0238] (4) Ionic conductivity test of composite solid electrolyte
[0239] Ionic conductivity is a core indicator for measuring the ability of composite solid electrolytes to conduct corresponding metal ions. Ionic conductivity is generally tested by electrochemical impedance spectroscopy, and the corresponding ionic conductivity is calculated. The specific process is as follows:
[0240] A 200nm-thick nickel layer was deposited on both sides of the composite solid-state electrolyte wafer using magnetron sputtering PVD. The current collector was then bonded to the nickel layer and connected to an electrochemical workstation via tabs. Electrochemical impedance spectroscopy (EIS) measurements were performed on the composite solid-state electrolyte wafer at a bias voltage of 10mV and a frequency of 106Hz to 0.1Hz. The Z' coordinate of the point closest to the Z' axis in the low-frequency band of the EIS curve, moving from right to left, was used as the resistance, R, and the ionic conductivity, σ, was calculated using the following formula.
[0241] Wherein, d is the thickness of the composite solid electrolyte sheet, and A is the contact area between the solid electrolyte sheet and the current collector.
[0242] Please see Table 1 for specific results.
[0243] Examples 2 to 4
[0244] Examples 2 to 4 are basically the same as Example 1, except that the type of stabilizer in step S1 is different from that in Example 1. Please see Table 1 for specific conditions.
[0245] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0246] Examples 5 to 7
[0247] Examples 5 to 7 are basically the same as Example 1, except that in step S1, the mass proportion Y2 of the phase change toughening agent in the mixture is controlled to be different from that in Example 1. For specific conditions, see Table 1.
[0248] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0249] Examples 8 to 10
[0250] Examples 8 to 10 are basically the same as Example 1, except that the mixing time in step S1 is adjusted so that the dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate is different from that in Example 1. For specific conditions, see Table 1.
[0251] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0252] Examples 11 to 13
[0253] Examples 11 to 13 are basically the same as Example 1, except that the mass proportion Y1 of the stabilizer in the phase change toughening agent in step S1 is different from that in Example 1. Please see Table 1 for specific conditions.
[0254] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0255] Examples 14-15
[0256] Examples 13 to 14 are basically the same as Example 1, except that the Dv50 of the phase change toughening agent is different from that of Example 1. Please see Table 1 for specific conditions.
[0257] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0258] Example 15
[0259] Example 15 is basically the same as Example 1, except that the phase change toughening agent in the example is replaced by two different phase change toughening agents, and the mass ratio of the two phase change toughening agents is 1:1; in the mixture, the total mass proportion Y2 of the two phase change toughening agents is the same as the mass proportion Y2 of the phase change toughening agent in Example 1. For specific conditions, please see Table 1.
[0260] Other steps and conditions are the same as those in Example 1. The test results are shown in Table 1.
[0261] Comparative Example 1
[0262] Comparative Example 1 is substantially the same as Example 1, except that: in Comparative Example 1, a solid electrolyte substrate (Li6PS5Cl) is directly provided to perform step S4 and subsequent steps.
[0263] The parameters and performance test results of each embodiment and comparative example are shown in Table 1, where the mass of the phase change toughening agent is used as the calculation basis, the mass proportion of the stabilizer is recorded as Y1, the total mass of the composite solid electrolyte is used as the calculation basis, the mass proportion of the phase change toughening agent is recorded as Y2, and the dispersion uniformity of the phase change toughening agent in the solid electrolyte substrate is H.
[0264] Table 1 Note: “ / ” indicates that the step or substance does not exist.
[0265] From the experimental results in the above table, analysis and comparison of the data of Example 1 and Comparative Example 1 show that the composite solid electrolyte of the present application has high toughness. When subjected to external force, for example, when applied to a battery, when subjected to the action of lithium dendrites, stress will be generated inside the phase change toughening agent accordingly. Under the stimulation of stress, the phase change toughening agent will undergo a phase change. The stress transformation brought about by the phase change process can improve the mechanical strength and toughness of the solid electrolyte substrate, further prevent the generation of internal defects in the solid electrolyte, thereby improving toughness and improving battery performance.
[0266] The technical features of the above-mentioned embodiments can be combined arbitrarily. In order to make the description concise, not all possible combinations of the technical features in the above-mentioned embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0267] The above-described embodiments merely represent several implementation methods of the present application. While the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the patent. It should be noted that a person skilled in the art could make several modifications and improvements without departing from the spirit of the present application, all of which fall within the scope of protection of the present application. Therefore, the scope of protection of the patent in this application shall be based on the appended claims, and the specification and drawings may be used to interpret the claims.
Claims
1. A composite solid electrolyte, It is characterized in that The components of the composite solid electrolyte include a solid electrolyte substrate and a phase change toughening agent dispersed in the solid electrolyte substrate, and the phase change toughening agent can undergo phase change under the action of external force.
2. The composite solid electrolyte according to claim 1, Features ,, the phase change toughening agent is uniformly dispersed in the solid electrolyte substrate.
3. The composite solid electrolyte according to claim 1, Features ,, the phase change toughening agent is uniformly distributed in the grains and grain boundaries of the solid electrolyte substrate.
4. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate is obtained by any one of a grid counting method, an intercept method, an area method, an area method and an exclusive circle method; wherein H satisfies: H>20%.
5. The composite solid electrolyte according to claim 4, It is characterized in that H satisfies: 20%<H<100%.
6. The composite solid electrolyte according to claim 4, Features ,, using the intercept method to test the dispersion uniformity H of the phase change toughening agent in the solid electrolyte substrate, comprising the following steps: Pressing the composite solid electrolyte into a sample to be tested, and cutting the sample to be tested along a thickness direction parallel to the sample to be tested, wherein a cutting section formed by cutting the sample to be tested is a section to be tested; placing the cross section to be measured under a scanning electron microscope to form a scanning electron microscope image; In the backscattered electron imaging mode, the solid electrolyte substrate and the phase change toughening agent in the scanning electron microscope image are distinguished according to the contrast, and the distance between any two particles of the phase change toughening agent in the scanning electron microscope image is determined by the grid line analysis method, which are respectively recorded as d i , i ranges from 1 to N, is the average distance between any two particles of the phase change toughening agent in the scanning electron microscope image, then: N is an integer ≥2.
7. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The volume distribution particle size Dv50 of the phase change toughening agent satisfies: 50nm≤Dv50≤100nm.
8. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The phase change toughening agent comprises zirconium oxide and a stabilizer.
9. The composite solid electrolyte according to claim 8, It is characterized in that The phase change toughening agent satisfies at least one of the following conditions (1) to (2): (1) In the phase change toughening agent, the mass proportion of the stabilizer is 0.01% to 50%; (2) The stabilizer includes at least one of yttrium oxide, scandium oxide, magnesium oxide, calcium oxide, and cesium oxide.
10. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The composite solid electrolyte includes at least two phase change toughening agents having different activation energies.
11. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The composite solid electrolyte comprises a first phase change toughening agent with an activation energy of T1 and a second phase change toughening agent with an activation energy of T2, wherein T1 and T2 satisfy 0<T2 / T1<0.
8.
12. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that In the composite solid electrolyte, the total mass proportion of the phase change toughening agent is 2% to 25%.
13. The composite solid electrolyte according to any one of claims 1 to 3, It is characterized in that The solid electrolyte substrate includes any one of a lithium ion solid electrolyte, a sodium ion solid electrolyte and a potassium ion solid electrolyte.
14. A method for preparing a composite solid electrolyte, It is characterized in that The steps include: The solid electrolyte substrate and the phase change toughening agent are mixed to prepare a composite solid electrolyte.
15. The method for preparing the composite solid electrolyte according to claim 14, It is characterized in that The mixing treatment adopts dry mixing, and the process of preparing the composite solid electrolyte also includes the following steps: The mixture after the mixing process is subjected to a pressing process; the pressure used in the pressing process is 300MPa to 550MPa; The mixing step adopts wet mixing, and the process of preparing the composite solid electrolyte also includes the following steps: The mixture after the mixing treatment is applied into a film and dried.
16. A solid-state battery, It is characterized in that The solid-state battery comprises a composite solid electrolyte as claimed in any one of claims 1 to 13 or a composite solid electrolyte prepared by the method for preparing a composite solid electrolyte as claimed in any one of claims 14 to 15.
17. An electrical device, It is characterized in that The electrical device comprises the solid-state battery as claimed in claim 16.
Citation Information
Patent Citations
Composite solid electrolyte membrane, preparation method thereof and solid-state battery
CN114142082A
Composite solid electrolyte, preparation method thereof, solid-state battery and electric device
CN116231051A
Ceramic lamination body and its manufacture
JP2000292406A
High Voltage Electrolyte for 5V Solid State Lithium-ion Battery Cell
US20230013068A1