Method of manufacturing a varnish transfer foil
The method enhances the handling and flexibility of varnish transfer films by using radiation-curable resins and controlled curing, addressing the challenges of rigid and shrinking lacquers in existing technologies, and ensuring consistent anti-fingerprint effects on substrates.
Patent Information
- Application Number
- PCT/ES2023/070278
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-03
- Publication Date
- 2024-11-07
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
[0001] DESCRIPTION
[0002] METHOD OF MANUFACTURING A FOIL FOR TRANSFERRING A VARNISH
[0003] TECHNICAL FIELD
[0004] The present invention relates to a method of manufacturing a film for transferring a layer of varnish onto a substrate containing melamine resin.
[0005] STATE OF THE ART
[0006] The prior art variously describes treated PET (polyethylene terephthalate) sheets, for example, with respect to adhesive tapes as taught in DE 10 2004 058281 A1. Furthermore, treated PET sheets are known from EP 2 920 232 B1 and are used to bond a multi-layer coating to wooden substrates to form, for example, laminated floor panels. While the PET sheet forms part of the multi-layer structure of the laminate in these situations, the PET sheet can also be used to transfer a coating to the substrate by means of a press, whereby the backing sheet is subsequently removed. To achieve an anti-fingerprint effect, the PET sheet is designed with a rough surface facing the substrate, so that the produced laminate displays a rough, matte, and non-reflective surface. The surface of a PET backing sheet facing the press is left untreated, i.e., smooth and uniform.
[0007] For example, document W02022 / 058033A1 describes a carrier sheet for transferring a coating to a melamine resin film on a substrate. The carrier sheet comprises a foil, which may comprise any suitable plastic, e.g., PET. The sheet comprises a lower surface with a roughness Rz of 0.1 pm to 100 pm according to ISO 4287 and preferably a surface roughness RSm of 0.1-1000 pm, more preferably 0.5-500 pm, even more preferably 5-100 pm according to ISO 4287 and also an upper sheet surface with a roughness Rz of 0.1 pm to 100 pm according to ISO 4287 and preferably a surface roughness RSm of 0.1-1000 pm, more preferably 0.5-500 pm, even more preferably 5-100 pm according to ISO 4287. The two surfaces do not need to have the same roughness.Top and bottom refer to the position of the surfaces when imagined in a press, with the bottom surface facing the substrate and the top facing the press. Compared to the prior art, in which only one of the sheet surfaces has a roughness as described above, the roughness of the sheet's top surface allows air between the press and the carrier sheet to be expelled from the press. Thus, bubbles cannot form that cause dents in the produced laminate. Furthermore, no press profile, which would be rougher than the sheet surface roughness, is necessary to achieve this result. The carrier sheet described thus allows the production of laminates with the desired roughness, leading to an anti-fingerprint effect, regardless of a possibly inhomogeneous substrate density.
[0008] However, to provide the technical performance required for the transfer described in this document, relatively high lacquer thicknesses are often applied, which creates a significant handling problem because the lacquers become rigid and shrink during the curing process. These properties make them difficult to keep flat when handled, and can even cause lacquer peeling, which can, in turn, cause defects if not properly removed and pressed. This technical problem is solved by the method described in the claims accompanying this specification.
[0009] EXPLANATION OF THE INVENTION
[0010] The present invention relates to a method for manufacturing a foil configured to transfer a varnish (transfer foil). The method according to the present invention advantageously improves the flatness of the transfer foil, while increasing its flexibility, improving its handling and preventing it from peeling off during handling or cutting processes. This facilitates its use in industrial processes and reduces waste. These objectives are achieved by the method according to claim 1. Particular and / or preferred embodiments of the method according to the present invention are described in the dependent claims.
[0011] The method of manufacturing a foil for transferring a varnish, according to the invention, comprises: a first step of providing a foil that provides a surface finish on which a layer of transferable varnish is applied, a second step of applying one or more layers of a resin or resins on one side with the desired surface finish of the by-product obtained in the previous step, where at least one resin contains functional groups curable by radiation and a thermal polymerization initiator, a third step of partial radiation curing of the foil resulting from the previous step, and a fourth step of calendering or pressing the foil resulting from the previous step by applying pressure and temperature, to generate a determined surface finish, at the same time as the resin is cured by means of the thermal polymerization initiator provided in the second step together with the resin.
[0012] In a preferred embodiment of the invention, the method is executed sequentially, in the order indicated. However, in a non-limiting manner, there may be additional intermediate steps or the duplication and / or repetition of steps.
[0013] Furthermore, the present invention distinguishes between the "drying" and "curing" of the resin, which cannot be considered technically equivalent in any case. In a drying process, a solvent is extracted by evaporation, while in curing, a polymerization reaction takes place. Thus, according to the present invention, the radiation curing process, in a non-limiting manner, encompasses both ultraviolet (UV) radiation processes and media, as well as electron beam radiation processes and media, since both techniques, well known to those skilled in the art, are sources of radiant energy. Ultimately, in the present invention, radiation-curable resins are understood to mean all those resins that polymerize when exposed to a radiation source, such as, for example, a UV radiation source or an electron beam radiation source.
[0014] Throughout the description and claims, the word "comprises" and its variations are not intended to exclude other technical features, additives, components, or steps. For those skilled in the art, other objects, advantages, and features of the invention will be derived in part from the invention and in part from the practice of the invention. The following examples and drawings are provided by way of illustration and are not intended to restrict the present invention. Furthermore, the invention covers all possible combinations of particular and preferred embodiments indicated herein. PREFERRED EMBODIMENT OF THE INVENTION AND EXAMPLES
[0015] As previously indicated, the present invention consists of a method for manufacturing a foil for transferring a varnish, which comprises, in turn: a first step of providing a foil that provides a surface finish on which to apply a layer of transferable varnish, a second step of applying one or more layers of a resin or resins on one side with the desired surface finish of the by-product obtained in the previous step, where at least one resin contains radiation-curable functional groups and a thermal polymerization initiator, a third step of partial radiation curing of the foil resulting from the previous step, and a fourth step of calendering or pressing the foil resulting from the previous step by applying pressure and temperature, to generate a certain surface finish, at the same time as the resin is cured by means of the thermal polymerization initiator provided in the second step together with the resin.
[0016] Some examples are described below that illustrate non-limiting practical embodiments of the invention. Specifically, it indicates how each of the stages of the manufacturing method can be implemented in practice. As indicated, these embodiments are practical examples that can be combined with each other. At the same time, all percentages and weights of the resins in the following examples refer to their dry content.
[0017] A first stage of providing a folio that gives a surface finish on which to apply a layer of transferable varnish
[0018] The surface finish is not limited to a uniform gloss or matte finish, and may also have any other effect such as relief, any texture, geometric figures, combinations of the above, or any other finish or pattern that we wish to reproduce. In a first non-limiting practical embodiment, a polyethylene terephthalate (PET) sheet is provided, between 10 pm and 300 pm thick, more preferably between 30 pm and 150 pm, in particular between 30 pm and 100 pm, to which a layer of matte varnish cured by excimer (an excited dimer) has previously been applied on one of its faces, having an anti-fingerprint matte structure that will subsequently be reproduced in the final product.
[0019] In a second non-limiting practical embodiment of the first stage of the process, a sheet of bioriented paraffinic thermoplastic resin is provided, in particular BOPP, between 10 pm and 300 pm thick, preferably between 30 pm and 200 pm, in particular between 50 pm and 125 pm, to which the side where the varnish is applied has previously been embossed, so that it has a wood imitation structure that will subsequently be reproduced in the final product.
[0020] In a third non-limiting practical embodiment, a polyethylene terephthalate (PET) sheet is provided, between 10 pm and 300 pm thick, more preferably between 30 pm and 150 pm, in particular between 30 pm and 100 pm. Said sheet has the side on which the second stage will be applied in a gloss finish. a second step of applying one or more layers of a resin or resins to the side with the desired surface finish of the by-product obtained in the previous step, where at least one resin contains radiation-curable functional groups and a thermal polymerization initiator
[0021] In this second stage, one or more layers of a resin or resins are applied (Le. it can be a single type of resin or several types of stratified resins) where at least one contains functional groups curable by radiation and a thermal polymerization initiator, being able to additionally cure -in a non-limiting manner- by exposure to humidity, oxidation, thermal mechanisms, polymerization of two-component resin, polymerization of blocked isocyanate or another type of radiation different from ultraviolet or by electron beam, with a thickness between 10 pm and 300 pm.
[0022] The resin or resins used in this second stage may contain - but are not limited to - a mixture of oligomers, monomers, additives with functionalities suitable for obtaining covalent interfacial crosslinking with the adjacent layer, as well as fillers to improve mechanical resistance to scratching and abrasion, nanoparticles, short fibers, pigments, rheological behavior modifiers, wetting agents, surface tension modifiers, solar radiation protection additives, antioxidants, anti-vandal additives (e.g., anti-graffiti), anti-fouling additives, antimicrobial additives, flame retardant additives, infrared radiation reflective additives, antistatic additives, anti-fingerprint additives, or any possible combination of the foregoing.
[0023] In a particular embodiment, the radiation-curable components have been selected from the group of unsaturated acrylates and methacrylates. In another particular preferred embodiment, said radiation-curable components are composed of an epoxy acrylate oligomer, preferably a polyester acrylate oligomer, and in particular a urethane acrylate oligomer or the corresponding methacrylate oligomers as prepolymers capable of radiation polymerization, and if appropriate diluted with mono- and / or polyfunctional acrylate monomers and / or their corresponding methacrylates. In another particular embodiment, to increase color stability when exposed to ultraviolet radiation, the prepolymer is an aliphatic urethane acrylate oligomer, which has been conveniently diluted with a 1-6 hexanediol diacrylate (HDDA) monomer.
[0024] In another particular embodiment, the thermal polymerization initiator is from the group of organic peroxides. In another particular embodiment, to have a suitable initiation temperature range, the thermal polymerization initiator is tert-butyl-peroxybenzoate. In another particular embodiment, the thermal polymerization initiator has been selected from the AZO group. A third stage of partial radiation curing of the film resulting from the previous stage
[0025] The process of the invention then proposes to partially cure the by-product obtained from the execution of the first and second stages, with the aim of obtaining a curing such that it even allows the foil to be wound if necessary and, in turn, ensure chemical anchoring points and reactivity to connect the adjacent coating layers.
[0026] The curing method is selected - but not limited to - from: electron beam curing, ultraviolet radiation curing, curing by thermal polymerization initiators, curing by exposure to moisture, oxidation curing, thermal curing, or a combination of any of the above processes.
[0027] Preferably, the film resulting from the previous stages is cured by electron beam and / or ultraviolet radiation, and more preferably it is cured by electron beam (EB) and in both cases it can be additionally cured - in a non-limiting manner - by exposure to humidity, oxidation, thermal mechanisms, polymerization of two-component resin, polymerization of free and / or blocked isocyanate, in order to obtain interconnection by crosslinking of all the layers, guaranteeing interfacial adhesion.
[0028] The problem of shrinkage (curling) is one of the biggest problems in this type of product. It occurs when one layer of the film shrinks differently than another, generating tension that causes the film to become unbalanced. This shrinkage occurs during drying and / or curing, and the degree to which it occurs depends mainly on the resins used and the degree of polymerization achieved.
[0029] In a particular embodiment, curing is performed using an electron beam. In this embodiment, although high-density crosslinking resins are used, which could present the disadvantage of high shrinkage, this is minimized thanks to the process of the invention. By performing this partial curing, the resin shrinks less and, in turn, being less crosslinked, it behaves more flexibly, adapting better to the shape of the surfaces to which it is to be adhered. This flexibility also prevents the resin from "creaking" and detaching from the film.
[0030] The resulting varnish layer is cured enough to be coiled, but it is not as stiff or contracted as it would have been if it had been fully cured.
[0031] There are many combinations, since several layers could be applied, and partial curing could be carried out in one or several times, on one or several of these layers, but the concept would be the same, to be able to produce a sheet containing a transferable varnish, in which one or several layers of lacquer are not completely cured, in order to improve flatness and prevent it from coming off during handling. a fourth stage of calendering or pressing the sheet resulting from the previous stage by applying pressure and temperature, to generate a specific surface finish, at the same time as the resin is cured by means of the thermal polymerization initiator supplied in the second stage together with the resin.In a particular embodiment, the finished product is successively placed with the side to which the second stage has been applied facing inwards, on a sheet of paper impregnated with melamine resin which in turn is on top of a stack of sheets of Kraft paper impregnated with phenol-formaldehyde resin and is pressed at a temperature of 160°C and a pressure of 80 kg / cm2, for 20 minutes.
[0032] In a particular embodiment, a finishing plate with a relief is used in the press, such that said relief is added to that of the first stage sheet, so that the surface finish is a combination of that of the first stage sheet and that of the finishing plate of the press.
[0033] In addition to the essential features indicated above, it is possible to incorporate the following additional steps into the method of the invention: an optional step of applying one or more layers of adhesion-promoting resin(s) and / or adhesive
[0034] Optionally, the process of the invention comprises, after the second and / or after the third stage, applying one or more layers of adhesion-promoting resin or resins and / or adhesive to the face where the second stage is applied, subsequently subjecting the process, if necessary, to a drying and / or curing stage selected - in a non-limiting manner - from: curing by ultraviolet radiation, electron beam radiation, curing by thermal polymerization initiators, curing by exposure to moisture, curing by oxidation, physical drying of water, drying by solvent removal or a combination of any of the above processes.
[0035] In a particular embodiment, a water-based resin capable of physical drying and / or radiation curing is used to produce HPL. The content of this adhesive resin is between 1 and 50 g / m2, preferably between 2 g / m2 and 40 g / m2, more preferably between 10 g / m2 and 30 g / m2, considering the weight relative to the resin itself and its water content. An optional step is to apply one or more layers of resin or resins to the side opposite the one applied in the second step. Because the varnish layer is not fully cured, it may have a more gummy behavior. To prevent it from sticking during the rewinding process, it may be advisable to apply a layer of varnish to the outer side of the sheet to help reduce adhesion during winding (the outer side is the contact side during rewinding). This allows for a lower partial curing without the risk of sticking.This additional layer, in turn, may contain additives that increase electrical conductivity to prevent the buildup of static charges (antistatic effect), which helps prevent dust from being attracted to the foil, reducing contamination during the fourth-stage process.
[0036] In one particular embodiment, a layer of resin is applied that provides such roughness that it reduces the contact surface between layers, helping to reduce adhesion between layers during winding. In another particular embodiment, said resin contains release agents, which reduce this undesired effect.
[0037] Example 1
[0038] We take a 50um PET sheet that has been previously treated with excimer lamps to give one side a particular anti-fingerprint matte finish. On this treated side, we apply 50um of an acrylic varnish composed of urethane acrylate resin diluted with HDDA monomer until we achieve an application viscosity of 2000 mPa s at 25°C and measured at a shear rate of 1000 s-1, to which we have added 1% peroxide. We partially cure said sheet using an electron beam, applying a voltage of 200kV with a low dose of 3kGy.
[0039] We then apply an additional layer to promote adhesion to the substrate using a physically drying resin. The finished product is then dried and placed, with the side to which the second layer was applied facing inward, on a sheet of paper impregnated with melamine resin. This sheet is then placed on top of a stack of Kraft paper sheets impregnated with phenol-formaldehyde resin. It is then pressed at a temperature of 160°C and a pressure of 80 kg / cm2 for 20 minutes.
[0040] Example 2
[0041] We take a 50um PET film that has been previously treated to give one side a particular finish. On this treated side, we apply 50um of a highly scratch-resistant acrylic varnish, to which we have added 1% peroxide. Before curing, we apply a second 15um layer of adhesion promoter, also acrylic, to which we also add 1% peroxide and acrylated melamine. We cure the film using an electron beam, applying a low dose of 3kGy at a voltage of 200kV, and we wind the film with the varnish. Finally, we press it as in example 1.
[0042] Example 3
[0043] We take a 50um PET sheet that has been previously treated to give one side a particular finish. On this treated side, we apply 50um of an acrylic varnish, to which we have added 1% peroxide. Before curing, it is laminated onto another 50um PET sheet, to which a physically drying varnish containing acrylic groups yet to react and which also contains peroxide has been applied (and dried). We then electron beam cure this set of sheets, curing with a voltage of 250kV and a low dose of 4kGy. Before winding it, we remove the second PET sheet, ensuring that the varnish it contained remains adhered to the other.
[0044] The finished product is placed with the side to which the second stage has been applied facing inwards, on a sheet of paper impregnated with melamine resin, which in turn is placed on top of a chipboard, and is pressed at a temperature of 180°C and a pressure of 40 kg / cm2, for 40 seconds.
[0045] Example 4
[0046] We take a 50um PET film that has been previously treated to give one side a particular finish. On this treated side, we apply 50um of acrylic varnish, to which we have added 1% hydrogen peroxide, and we cure the film using an electron beam, applying a low dose of 5kGy at a voltage of 200kV.
[0047] We then applied an additional 15um layer to promote adhesion to the substrate using a radiation-curing resin, to which we also added adhesion-enhancing additives and a thermal polymerization initiator. Finally, we cured again with a low dose of 5kGy, but this time at a voltage of 150kV.
[0048] Example 5
[0049] We take a 50um PET film that has been previously treated to give one side a particular finish. On the other side, we apply a layer of varnish to provide a structure that helps reduce adhesion. On the first treated side, we apply 50um of an acrylic varnish, to which we have added 1% peroxide, and we cure the film using an electron beam, applying a voltage of 200kV and a low dose of 4kGy. We then apply an additional layer to promote adhesion to the substrate using a physical drying resin. Finally, we press the film as in example 1.
[0050] Example 6
[0051] We take a 50um PET film that has been previously treated to give one side a particular finish. On the other side, we apply a layer of varnish that provides a structure that helps reduce adhesion and contains antistatic additives. On the first treated side, we apply 50um of an acrylic varnish, to which we have added 1% peroxide, and we cure the film using an electron beam, applying a voltage of 200kV and a low dose of 4kGy. We then apply an additional layer to promote adhesion to the substrate using a physical drying resin. Finally, we press the film as in example 1.
[0052] Example 7
[0053] We take a 50um PET film with a gloss finish on one side. On this gloss side, we apply 50um of a highly scratch-resistant acrylic varnish, to which we have added 1% peroxide. Before curing, we apply a second 15um layer of acrylic adhesion promoter, to which we also add 1% peroxide and acrylated melamine. We cure the film using an electron beam, applying a low dose of 3kGy at a voltage of 200kV, and we wind the film with the varnish. Finally, we press it as in example 1, obtaining a high-gloss surface.
Claims
.CLAIMS 1. A method of manufacturing a foil for transferring a varnish comprising: a first step of providing a foil that provides a surface finish on which a layer of transferable varnish is applied, a second step of applying one or more layers of a resin or resins on one side with the desired surface finish of the by-product obtained in the previous step, where at least one resin contains radiation-curable functional groups and a thermal polymerization initiator, a third step of partial radiation curing of the foil resulting from the previous step, and a fourth step of calendering or pressing the foil resulting from the previous step by applying pressure and temperature, to generate a certain surface finish, at the same time as the resin is cured by means of the thermal polymerization initiator provided in the second step together with the resin.
2. The method according to claim 1, wherein the foil of the first stage is a PET foil, preferably between 10-150um, and more preferably between 50-1 OOum.
3. The method according to claim 1, wherein the first stage film is composed of bioriented paraffinic thermoplastic resin, in particular BOPP, preferably between 10 pm and 300 pm thick, more preferably between 30 pm and 200 pm.
4. The method according to any of the preceding claims, wherein the first stage foil has a matte finish, which has been produced by applying a microstructure by excimer curing.
5. The method according to any of the preceding claims, wherein the sheet of the first stage had previously been embossed on the side where we now apply the varnish.
6. The method according to any of the preceding claims, wherein a varnish has additionally been applied to the other side of the first stage foil, to reduce adhesion in case there is a winding process after the third stage, thus preventing the partially cured material from adhering to each other.
7. The method according to claim 6, wherein the additional varnish layer has antistatic properties.
8. The method according to any one of the preceding claims, comprising an additional step of applying one or more additional layers of adhesion-promoting resin(s) and / or adhesive, applicable between the second and third partial radiation curing steps or between the third and fourth calendering or pressing steps.
Citation Information
Patent Citations
double-sided pressure-sensitive adhesive tapes for manufacturing or bonding LC displays with light-absorbing properties
DE102004058281A1
Surface material for coating melamine resin laminates
EP2920232B1
Painable and painted material having structured surface
CN115836106A
Manufacturing process for a decorative sheet
EP3971344A1
Surfacing materials and method of manufacture
US10933608B2