Water-repellent structure
A non-fluorine-based water-repellent structure on glass surfaces, utilizing a dialkyl silicone layer and a siloxane-based base layer, effectively addresses the deterioration of water repellency on tin-containing float glass surfaces, ensuring long-term weather resistance and environmental sustainability.
Patent Information
- Application Number
- PCT/JP2024/016197
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-01
- Filing Date
- 2024-04-25
- Publication Date
- 2024-11-07
AI Technical Summary
Existing water-repellent structures on glass surfaces, particularly those with fluorine-based compounds, face environmental concerns and deteriorate in weather resistance when applied to tin-containing surfaces of float glass, leading to reduced water repellency over time.
A non-fluorine-based water-repellent structure is developed, featuring a glass plate with a water-repellent layer containing dialkyl silicone and a siloxane-based base layer, where the base layer thickness is optimized between 50 to 600 nm to enhance weather resistance and maintain water repellency.
The structure maintains excellent water repellency and weather resistance, with a water contact angle of 92° or more after accelerated weathering tests, and a haze value of 0.5% or less, even after prolonged use, without the environmental concerns associated with fluorine-based compounds.
Smart Images

Figure JP2024016197_07112024_PF_FP_ABST
Abstract
Description
Water-repellent structure
[0001] The present disclosure relates to a water-repellent structure.
[0002] For use as window glass in automobiles and other transportation vehicles, glass laminates are known in which a water-repellent film is formed on the outer surface of a glass sheet to prevent the adhesion of rain, frost, ice, snow, etc. and maintain clear visibility. In this specification, a structure having a glass sheet and a water-repellent film formed on one surface thereof is referred to as a "water-repellent structure." The water-repellent film includes a water-repellent layer and may optionally include one or more other layers. The water-repellent film may have, for example, a base layer below the water-repellent layer. The surface of the water-repellent layer is exposed, and this surface is the outermost surface of the water-repellent film and is the water-repellent surface.
[0003] Conventionally, fluorine-based compounds have generally been used as materials for water-repellent layers. However, in recent years, concerns have arisen about the environmental impact of some fluorine-based compounds, such as C6 fluorine-based compounds, and development of non-fluorine-based compositions that do not contain fluorine-based compounds has been progressing as compositions for forming water-repellent layers.
[0004] In Patent Document 1, the applicant discloses a water-repellent structure having a water-repellent film including a water-repellent layer formed using a non-fluorine-based composition for forming a water-repellent layer containing one or more hydrolyzable silicon compounds (claim 1, etc.). This water-repellent layer contains a dialkyl silicone in which the alkyl group has 1 to 3 carbon atoms, and has excellent water repellency and abrasion resistance. The water-repellent film can further have an underlayer formed under the water-repellent layer using a non-fluorine-based composition for forming an underlayer containing one or more hydrolyzable silicon compounds (claim 2).
[0005] JP 2015-145463 A JP 2000-86293 A JP 2000-203884 A WO 2007 / 081025
[0006] The water-repellent layer preferably has good water repellency in the initial state and durability that allows it to maintain good water repellency even after long-term use. One example of durability is weather resistance. Glass plates manufactured by the float process (also called float glass) are widely used as glass plates. Generally, float glass tends to have a higher tin atom content on one surface than on the other. In float glass, the surface with a low tin atom content is also called the tin-free surface, top surface, or T surface, and the surface with a high tin atom content is also called the tin-containing surface, bottom surface, or B surface. The inventors have found that when a water-repellent layer containing dialkyl silicone is formed on a tin-containing surface (bottom surface), the water repellency tends to decrease after an accelerated weathering test compared to when the layer is formed on a tin-free surface (top surface). For example, this tendency was observed when the tin content of the tin-containing surface (bottom surface) was 0.1 atm% or more.
[0007] Patent Document 1 describes that when float glass is used, it is preferable to provide a water-repellent film on the top surface, which has a low tin content (paragraph 0020). Patent Document 1 also describes that the thickness of the primer layer is preferably 50 nm or less (paragraph 0109). In the "Examples" section of Patent Document 1, the primer layer is formed using 0.5 g of a primer layer-forming composition (paragraph 0141). Although the thickness is not specified, it is clearly 20 nm or less in consideration of the amount. Patent Document 1 does not disclose the problem of reduced weather resistance when a non-fluorine-based water-repellent layer is formed on the tin-containing surface (bottom surface) of float glass, nor does it disclose a means for solving this problem.
[0008] Other related technologies of the present disclosure include Patent Documents 2 to 4. Patent Documents 2 and 3 disclose water-repellent glass having an underlayer and a water-repellent layer formed using a fluoroalkyl group-containing silane compound (Claim 1 of Patent Document 2, Claim 1 of Patent Document 3). These documents state that the water-repellent layer can be formed on either the top or bottom surface of the float glass. In Patent Document 2, the thickness of the underlayer is 20 to 45 nm (Claim 1). In the "Examples" section of Patent Document 3, the thickness of the underlayer is 100 to 200 nm (Table 2). In Patent Documents 2 and 3, the water-repellent layer is fluorine-based.
[0009] Patent Document 4 discloses a vehicle glass plate having an underlayer and a water-repellent layer containing a fluoroalkyl group and / or an alkyl group (claims 1 and 4, paragraph 0021). In the "Examples" section, the underlayer and the water-repellent layer are formed on the tin-containing bottom surface of a soda-lime silica glass plate (paragraph 0050). Patent Document 4 also discloses that the thickness of the underlayer is preferably 5 to 300 nm (paragraph 0023). However, in the "Examples" section, the underlayer is formed using 0.01 g of chlorosilane (paragraph 0049). Although the thickness is not specified, the amount is clearly 20 nm or less. Patent Document 4 also describes a non-fluorine-based water-repellent layer, but the water-repellent layer formed in the "Examples" section is solely fluorine-based, and it cannot be said that a non-fluorine-based water-repellent layer is substantially disclosed.
[0010] Patent Documents 2 to 4 do not disclose a non-fluorine-based water-repellent layer containing dialkyl silicone, and do not disclose the problem of reduced weather resistance when a non-fluorine-based water-repellent layer containing dialkyl silicone is formed on the tin-containing surface (bottom surface) of float glass, nor do they disclose a means for solving the problem.
[0011] The present disclosure aims to provide a water-repellent structure that has a non-fluorine-based water-repellent layer formed on the tin-containing surface of a glass plate, and that has good water repellency in the initial state and good weather resistance.
[0012] The present disclosure provides the following water-repellent structure.
[0013] [1] A water-repellent structure comprising: a glass plate; and a water-repellent layer formed on one surface of the glass plate, the water-repellent layer containing one or more dialkylsilicones in which the alkyl group has 1 to 3 carbon atoms and containing no fluorine atoms; wherein the surface of the glass plate contains tin atoms; and wherein a base layer containing a siloxane compound and containing no fluorine atoms is provided between the glass plate and the water-repellent layer, the base layer having a thickness of 50 to 600 nm.
[0014] [2] The water-repellent structure of [1], wherein the thickness of the underlayer is 55 to 600 nm. [3] The water-repellent structure of [2], wherein the thickness of the underlayer is 55 to 500 nm. [4] The water-repellent structure of [3], wherein the thickness of the underlayer is 70 to 500 nm.
[0015] [5] The water-repellent structure according to any one of [1] to [4], wherein the one or more dialkyl silicones contain one or more hydrolyzable dialkyl silicones having a hydrolyzable group. [6] The water-repellent structure according to [5], wherein the hydrolyzable dialkyl silicone is a compound represented by the following formula (1): R 13 -(SiR 12 2 O) k1 -SiR 12 2 -Y 1 -Si(R 11 ) 3-n1 (X 1 ) n1 ...(1) (In the above formula, R 13 is an alkyl group having 1 to 30 carbon atoms. 12 are each independently an alkyl group having 1 to 3 carbon atoms. 1 is an alkylene group having 2 to 4 carbon atoms or an oxygen atom. 11 are each independently a monovalent hydrocarbon group. 1 are each independently a hydrolyzable group. 1 may be hydrolyzed to a hydroxyl group. k1 is an integer of 10 to 300. n1 is an integer of 1 to 3.
[0016] [7] The water-repellent structure according to any one of [1] to [4], wherein the water-repellent layer is a dried and cured product of a composition for forming a water-repellent layer, which contains one or more hydrolyzable dialkyl silicones having a hydrolyzable group and one or more hydrolyzable silicon compounds which may be partially hydrolyzed and condensed between the same or different species. [8] The water-repellent structure according to [7], wherein the hydrolyzable dialkyl silicone is a compound represented by the following formula (1): R 13 -(SiR 12 2 O) k1 -SiR 12 2 -Y 1 -Si(R 11 ) 3-n1 (X 1 ) n1 ...(1) (In the above formula, R 13 is an alkyl group having 1 to 30 carbon atoms. 12 are each independently an alkyl group having 1 to 3 carbon atoms. 1 is an alkylene group having 2 to 4 carbon atoms or an oxygen atom. 11 are each independently a monovalent hydrocarbon group. 1 are each independently a hydrolyzable group. 1 may be hydrolyzed to a hydroxyl group. k1 is an integer of 10 to 300. n1 is an integer of 1 to 3.
[0017] [9] The water-repellent structure of [7] or [8], wherein the one or more hydrolyzable silicon compounds further comprise one or more compounds selected from one or more hydrolyzable alkylsilanes having a hydrolyzable group and an alkyl group, and one or more hydrolyzable bissilanes having hydrolyzable groups at both ends with a divalent organic group sandwiched between them, and which may be partially hydrolyzed and condensed between the same or different species.
[10] The water-repellent structure of [9], wherein the hydrolyzable alkylsilane is a compound represented by the following formula (2), and the hydrolyzable bissilane is a compound represented by the following formula (4): 22 -Si(R 21 ) 3-n2 (X 2 ) n2 ...(2) (In the above formula, R 22is an alkyl group having 1 to 30 carbon atoms. 21 are each independently a monovalent hydrocarbon group. 2 are each independently a hydrolyzable group. 2 may be hydrolyzed to a hydroxyl group. n2 is an integer of 1 to 3.) X 4 3 Si-R 4 -SiX 4 3 ...(4) (In the above formula, R 4 is a divalent organic group. 4 are each independently a hydrolyzable group. 4 may be hydrolyzed to a hydroxyl group.)
[0018]
[11] The water-repellent structure according to any one of [1] to
[10] , wherein the underlayer is a dried and cured product of a composition for forming an underlayer, which contains one or more hydrolyzable silicon compounds, which may be partially hydrolyzed and condensed between the same or different species, selected from the group consisting of compounds represented by the following formula (3) and compounds represented by the following formula (4): Si(R 31 ) 4-n3 (X 3 ) n3 ...(3) (In the above formula, R 31 are each independently a monovalent hydrocarbon group. 3 are each independently a hydrolyzable group. 3 may be hydrolyzed to a hydroxyl group. n3 is an integer of 1 to 4.) X 4 3 Si-R 4 -SiX 4 3 ...(4) (In the above formula, R 4 is a divalent organic group. 4 are each independently a hydrolyzable group. 4 may be hydrolyzed to a hydroxyl group.)
[0019]
[12] The water-repellent structure of any one of [1] to
[11] , wherein the initial haze value is 0.5% or less and the haze value after a heat resistance test in which the structure is maintained at 80°C for 500 hours is 1.0% or less.
[13] The water-repellent structure of any one of [1] to
[12] , wherein the surface of the water-repellent layer has an initial water contact angle of 92° or more and a water contact angle of 92° or more after an accelerated weather resistance test in accordance with JIS D 0205 5.4 at a black panel temperature of 63°C for 1000 hours.
[14] The water-repellent structure of
[13] , wherein the surface of the water-repellent layer has a water contact angle of 85° or more after an accelerated weather resistance test in accordance with JIS D 0205 5.4 at a black panel temperature of 63°C for 1500 hours.
[15] The water-repellent structure according to any one of [1] to
[14] , wherein the other surface of the glass plate has a coating containing one or more functional components selected from the group consisting of an ultraviolet ray shielding agent and an infrared ray shielding agent.
[0020] The base layer included in the water-repellent structure of the present disclosure has a thickness of 50 to 600 nm. According to the present disclosure, it is possible to provide a water-repellent structure that has a non-fluorine-based water-repellent layer formed on the tin-containing surface of a glass plate, and that has good water repellency in an initial state and good weather resistance.
[0021] 1 is a schematic cross-sectional view of a water-repellent structure according to an embodiment of the present invention.
[0022] In this specification, unless otherwise specified, the "surface" of a planar body such as a plate, sheet, or film refers to the main surface having a large area. In this specification, a compound represented by any formula (x) is also referred to as compound (x). In the chemical formula, Me represents a methyl group, nBu represents an n-butyl group. In a composition containing one or more hydrolyzable silicon compounds, the one or more hydrolyzable silicon compounds may be partially hydrolyzed and condensed between the same or different species. In this specification, the hydrolyzed condensate of one or more hydrolyzable silicon compounds refers to an oligomer (multimer) produced by hydrolyzing at least a portion of the hydrolyzable groups contained in one or more hydrolyzable silicon compounds, followed by dehydration condensation. In this specification, unless otherwise specified, the symbol "to" indicating a numerical range is used to mean that the numerical values before and after it are included as the lower and upper limits. Hereinafter, embodiments of the present invention will be described.
[0023] [Water-Repellent Structure] The water-repellent structure of the present disclosure includes a glass plate and a water-repellent film formed on one surface of the glass plate. The surface of the glass plate facing the water-repellent film contains tin atoms. The glass plate is, for example, a glass plate (also called float glass) manufactured by the float process. Generally, float glass tends to contain more tin atoms on one surface than on the other surface. In float glass, the side with a low tin atom content is also called the tin-free side, top surface, or T-surface, and the side with a high tin atom content is also called the tin-containing side, bottom surface, or B-surface. The tin content on the surface of the glass plate can be measured by known analyses such as secondary ion mass spectrometry (SIMS), laser ablation inductively coupled plasma mass spectrometry (LA-ICP-MS), and X-ray photoelectron spectroscopy (XPS) analysis. For example, when measuring the tin content on the surface of a glass plate by XPS analysis, a peak in the range of 480 to 490 ev is identified as a peak derived from tin atoms, and the tin content on the surface can be measured from the area intensity of that peak. In this measurement method, the tin content of the tin-containing surface (bottom surface) is higher than that of the tin-free surface (top surface or T-surface), and the specific range is not particularly limited. The lower limit of the tin content of the tin-containing surface (bottom surface) can be, for example, 0.1 atm%, 0.2 atm%, 0.3 atm%, 0.4 atm%, or 0.5 atm%. The upper limit of the tin content of the tin-containing surface (bottom surface) is not particularly limited, and can be, for example, 3.0 atm%, 2.5 atm%, 2.0 atm%, 1.5 atm%, or 1.0 atm%. The thickness of the glass plate is not particularly limited and can be designed according to the application. For use as vehicle window glass (windshield, side glass, rear glass, etc.), the thickness is preferably 2 to 6 mm.
[0024] The water-repellent film is formed on at least a partial region of the surface of the glass plate. The water-repellent film includes a water-repellent layer and an underlayer formed thereunder, and may have one or more intermediate layers between the water-repellent layer and the underlayer. The water-repellent layer is a layer containing one or more dialkylsilicones in which the alkyl group has 1 to 3 carbon atoms and does not contain fluorine atoms. The underlayer is a layer containing a siloxane compound and does not contain fluorine atoms. The surface of the water-repellent layer is exposed, and the surface of the water-repellent layer is the outermost surface of the water-repellent film and is the water-repellent surface.
[0025] 1 is a schematic cross-sectional view of a water-repellent structure according to one embodiment of the present invention. In the figure, reference numeral 1 denotes a water-repellent structure, reference numeral 10 denotes a glass plate, reference numeral 10S denotes the surface of the glass plate on the water-repellent film side, reference numeral 20 denotes a water-repellent film, reference numeral 20S denotes the outermost surface of the water-repellent film, reference numeral 21 denotes a water-repellent layer, reference numeral 21S denotes the surface of the water-repellent layer, and reference numeral 22 denotes an underlayer.
[0026] "Water repellency" can be classified into static water repellency, which is the property of water droplets not adhering easily, and dynamic water repellency (also called water sliding), which is the property of water droplets rolling off easily. Static water repellency can be evaluated by the water contact angle, and dynamic water repellency (water sliding) can be evaluated by the water sliding angle. It is preferable that the water-repellent layer has good water repellency in the initial state and durability that allows it to maintain good water repellency even after long-term use. One example of durability is weather resistance. In this specification, "water-repellent layer in the initial state" refers to the water-repellent layer at the time when film formation on a glass plate is completed, or a water-repellent layer that has been stored without undergoing any particular treatment or operation after film formation and without significant changes in properties. The form during storage is not particularly limited, and the water-repellent structure may be stored alone, or the water-repellent structure may be stored in the form of a final product mounted on a vehicle or the like. The storage environment temperature is, for example, -20 to 50°C, and the storage period is, for example, within one year. The "time when the formation of the water-repellent film is completed" refers to the time when the curing of the coating film made of the composition for forming a water-repellent layer is completed.
[0027] In the water-repellent structure of the present disclosure, the thickness of the underlayer is 50 to 600 nm. The lower limit is preferably 55 nm, more preferably 60 nm, and particularly preferably 70 nm. The upper limit is more preferably 500 nm, even more preferably 500 nm, particularly preferably 300 nm, and most preferably 200 nm.
[0028] As explained in the section [Problem to be Solved by the Invention], the inventors have found that when a water-repellent layer containing dialkyl silicone is formed on a tin-containing surface of float glass, the water-repellent property tends to decrease after an accelerated weathering test compared to when the layer is formed on a tin-free surface of float glass. The inventors have found that when the thickness of the base layer is 50 nm or more, preferably 55 nm or more, the weathering resistance of the water-repellent layer can be improved and the decrease in water-repellent property after an accelerated weathering test can be suppressed.
[0029] Although it is not entirely clear, it is presumed as follows: When sunlight is irradiated onto the tin-containing surface of a glass plate such as float glass, SnO 2 It is presumed that active species such as superoxide anions and hydroxyl radicals are generated by the photocatalytic action of the above-mentioned compounds. Such active species diffuse within the underlayer, and some of them penetrate the underlayer to reach the water-repellent layer, promoting photodegradation of organic components such as the alkyl group of the dialkyl silicone contained in the water-repellent layer and reducing the weather resistance of the water-repellent layer. It is presumed that if the thickness of the underlayer is 50 nm or more, preferably 55 nm or more, the underlayer can function well as a barrier layer that prevents active species generated on the tin-containing surface of the glass plate from reaching the water-repellent layer in an accelerated weathering test. As a result, it is presumed that deterioration of the water-repellent layer is suppressed and the weather resistance of the water-repellent layer can be improved.
[0030] In the water-repellent structure of the present disclosure, the initial water contact angle on the surface of the water-repellent layer is preferably 92° or more, more preferably 95° or more. The upper limit of the initial water contact angle is not particularly limited, and may be, for example, 110°. In the water-repellent structure of the present disclosure, the surface of the water-repellent layer may have the following water contact angle after an accelerated weathering test in accordance with JIS D 0205 5.4 at a black panel temperature of 63°C. The water contact angle after a 1000-hour accelerated weathering test may be 92° or more, preferably 95° or more. The water contact angle after a 1500-hour accelerated weathering test may be 85° or more, preferably 90° or more, more preferably 95° or more. The water contact angle after a 2000-hour accelerated weathering test may be 70° or more, preferably 75° or more, more preferably 80° or more, even more preferably 85° or more, and particularly preferably 90° or more. The water contact angle can be measured by the method described in the Examples section below.
[0031] If the thickness of the underlayer is too large, cracks may occur in the underlayer when the formation of the water-repellent film is completed, resulting in an increase in the haze value of the water-repellent structure and a decrease in transparency. If the thickness of the underlayer is 600 nm or less, preferably 500 nm or less, cracks are prevented from occurring in the underlayer, resulting in a water-repellent structure with a small initial haze value and good transparency. The water-repellent structure of the present disclosure may have the following initial haze value and haze value after a heat resistance test at 80°C: The initial haze value may be 0.5% or less, preferably 0.3% or less. The haze value after a heat resistance test at 80°C for 500 hours may be 1.0% or less, preferably 0.7% or less, more preferably 0.5% or less, and particularly preferably 0.3% or less. The haze value after a heat resistance test at 80°C for 1000 hours may be 5.0% or less, more preferably 1.0% or less, particularly preferably 0.5% or less, and most preferably 0.3% or less. The haze value can be measured by the method described in the section [Examples] below.
[0032] The thickness of the water-repellent layer is not particularly limited as long as it can impart good water repellency and good weather resistance to the water-repellent film, and from the viewpoint of economy, it is preferably 50 nm or less. The lower limit is the thickness of a monolayer.
[0033] (Water-Repellent Layer) The water-repellent film includes a water-repellent layer containing one or more dialkyl silicones in which the alkyl group has 1 to 3 carbon atoms and does not contain fluorine atoms. The one or more dialkyl silicones may include one or more hydrolyzable dialkyl silicones (SC) having a hydrolyzable group. The water-repellent layer may be a dried and cured product of a water-repellent layer-forming composition containing one or more hydrolyzable dialkyl silicones (SC) having a hydrolyzable group and one or more hydrolyzable silicon compounds (ST) that may be partially hydrolyzed and condensed with the same or different species. It is preferable that at least a portion of the hydrolyzable dialkyl silicones (SC) contained in the water-repellent layer-forming composition maintain their chemical structure even after the composition is dried and cured.
[0034] The one or more hydrolyzable dialkyl silicones (SC) contained in the water-repellent layer-forming composition and the water-repellent layer may be a compound represented by the following formula (1) (also referred to as compound (1)): 13 -(SiR 12 2 O) k1 -SiR 12 2 -Y 1 -Si(R 11 ) 3-n1 (X 1 ) n1 ...(1) (In the above formula, R 13 is an alkyl group having 1 to 30 carbon atoms. 12 are each independently an alkyl group having 1 to 3 carbon atoms. 1 is an alkylene group having 2 to 4 carbon atoms or an oxygen atom. 11 are each independently a monovalent hydrocarbon group. 1 are each independently a hydrolyzable group. 1 may be hydrolyzed to a hydroxyl group. k1 is an integer of 10 to 300. n1 is an integer of 1 to 3.
[0035] Compound (1) has an alkyl group (R 13 ) at the other end, and a hydrolyzable group (X 1 The water-repellent layer obtained by using the compound (1) is a linear polyorganosiloxane having X in the compound (1). 1 or X 1 The water-repellent layer obtained by using the compound (1) can be excellent in both static and dynamic water repellency. This water-repellent layer can also be excellent in weather resistance.
[0036] From the viewpoint of improving the solubility of the compound (1) in the composition for forming a water-repellent layer, the coatability of the composition for forming a water-repellent layer, and the weather resistance of the water-repellent layer, 13 is an alkyl group having 1 to 30 carbon atoms. Examples of the alkyl group include a linear alkyl group, a branched alkyl group, and an alkyl group having a cyclic structure, with a linear alkyl group being preferred. The lower limit of the number of carbon atoms in the alkyl group is preferably 2, more preferably 3, and particularly preferably 4. The upper limit of the number of carbon atoms in the alkyl group is preferably 20, more preferably 10. R 13 A plurality of compounds (1) having different numbers of carbon atoms may be used in combination. For example, R 13 Compound (1) having 4 or more carbon atoms, and R 13 The compound (1) having 1 to 3 carbon atoms may be used in combination.
[0037] R 12 are each independently an alkyl group having 1 to 3 carbon atoms, preferably a linear alkyl group having 1 to 3 carbon atoms, more preferably a methyl group. 12 may be the same or different, and are preferably the same.
[0038] Y 1 is an alkylene group having 2 to 4 carbon atoms or an oxygen atom. 1 When Y is an alkylene group, it preferably has 2 to 3 carbon atoms. 1 is an alkylene group, compound (1) can be 1 is a linear alkylene group; and 1may be a mixture with a compound (1) in which Y is a branched alkylene group. 1 is an alkylene group having 2 carbon atoms, the group is -C 2 H 4 -, but compound (1) is represented by Y 1 Ga-CH 2 CH 2 Compound (1) where Y 1 -CH(CH 3 )-, provided that Y 1 In the compound (1), Y is an alkylene group. 1 It is preferable that the proportion of the compound (1) in which is a linear alkylene group is high.
[0039] R 11 are each independently a monovalent hydrocarbon group. Examples of the monovalent hydrocarbon group include an alkyl group, a cycloalkyl group, an alkenyl group, and an aryl group. 11 is preferably a monovalent saturated hydrocarbon group. 11 The number of carbon atoms in R is preferably 1 to 6, more preferably 1 to 3, and particularly preferably 1 to 2. From the viewpoint of the availability of raw materials and the ease of synthesis of compound (1), 11 is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and particularly preferably an alkyl group having 1 to 2 carbon atoms. 11 If there are multiple R 11 may be the same or different, and it is preferable that they are the same in terms of easy availability of raw materials.
[0040] X 1 is a hydrolyzable group, and Si—X 1 is hydrolyzed to produce Si—OH. Therefore, in the composition, X 1may be hydrolyzed to a hydroxyl group. Examples of hydrolyzable groups include an alkoxy group, an acyloxy group, a ketoxime group, an alkenyloxy group, an aminoxy group, an amide group, an isocyanate group, and a halogen atom. From the viewpoint of the balance between the chemical stability and ease of hydrolysis of compound (1), an alkoxy group, an isocyanate group, and a halogen atom are preferred. As the alkoxy group, an alkoxy group having 1 to 4 carbon atoms is preferred, and a methoxy group, an ethoxy group, and the like are more preferred. As the halogen atom, a chlorine atom and the like are preferred. X 1 As the X, a methoxy group, an ethoxy group, a chlorine atom, etc. are particularly preferred. 1 If there are multiple X 1 may be the same or different, and it is preferable that they are the same in terms of easy availability of raw materials.
[0041] k1 is 10 to 300, preferably 20 to 240, and more preferably 30 to 120. When k1 is within this range, the water-repellent layer can achieve both static and dynamic water repellency. Compound (1) may be a mixture of multiple types of compound (1) with different k1. In this case, k1 is expressed as an average value. n1 is an integer of 1 to 3, and from the viewpoint of improving adhesion between the water-repellent layer and the base, it is preferably 2 to 3, and particularly preferably 3.
[0042] Compound (1) can be produced by a known method, for example, by the method described in Patent Document 1. As compound (1), a commercially available product may also be used.
[0043] The one or more hydrolyzable silicon compounds (ST) can further include one or more compounds selected from one or more hydrolyzable alkylsilanes (SR) having a hydrolyzable group and an alkyl group, and one or more hydrolyzable bissilanes (SB) having hydrolyzable groups at both ends with a divalent organic group in between, and which may be partially hydrolyzed and condensed between the same or different species.
[0044] The hydrolyzable alkylsilane (SR) can be a compound represented by the following formula (2) (also referred to as compound (2)): 22 -Si(R 21 )3-n2 (X 2 ) n2 ...(2) (In the above formula, R 22 is an alkyl group having 1 to 30 carbon atoms. 21 are each independently a monovalent hydrocarbon group. 2 are each independently a hydrolyzable group. 2 may be hydrolyzed to a hydroxyl group, and n2 is an integer of 1 to 3.
[0045] Compound (2) has an alkyl group (R 22 ) at the other end, and a hydrolyzable group (X 2 The water-repellent layer obtained by using the compound (2) is an alkylsilane having X in the compound (2). 2 or X 2 The water-repellent layer obtained by using one or more hydrolyzable dialkylsilicones (SC) (preferably one or more compounds (1)) and one or more hydrolyzable alkylsilanes (SR) (preferably one or more compounds (2)) is excellent in both static and dynamic water repellency, and also in weather resistance.
[0046] When a hydrolyzable dialkylsilicone (SC) having a relatively large molecular weight is used in combination with a hydrolyzable alkylsilane (SR) having a relatively small molecular weight, it is thought that the gaps in the layer are filled with the hydrolyzable alkylsilane (SR) having a relatively small molecular weight or its reaction product, resulting in a dense water-repellent layer that is highly weather-resistant.
[0047] From the viewpoint of improving the solubility of the compound (2) in the composition for forming a water-repellent layer, the coatability of the composition for forming a water-repellent layer, and the weather resistance of the water-repellent layer, 22 is an alkyl group having 1 to 30 carbon atoms. Examples of the alkyl group include a linear alkyl group, a branched alkyl group, and an alkyl group having a cyclic structure, with a linear alkyl group being preferred.
[0048] The lower limit of the number of carbon atoms in the alkyl group is preferably 2, more preferably 5, and particularly preferably 8. The upper limit of the number of carbon atoms in the alkyl group is preferably 25, and more preferably 20. R 22A plurality of compounds (2) having different numbers of carbon atoms may be used in combination. For example, R 22 Compound (2) having 8 or more carbon atoms, and R 22 The compound (2) may be used in combination with the compound (2) having 7 or less carbon atoms.
[0049] R 21 are each independently a monovalent hydrocarbon group. Examples of the monovalent hydrocarbon group include an alkyl group, a cycloalkyl group, an alkenyl group, and an aryl group. 21 is preferably a monovalent saturated hydrocarbon group. 21 The number of carbon atoms in R is preferably 1 to 6, more preferably 1 to 3, and particularly preferably 1 to 2. From the viewpoint of the availability of raw materials and the ease of synthesis of compound (2), 21 is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and particularly preferably an alkyl group having 1 to 2 carbon atoms. 21 If there are multiple R 21 may be the same or different, and it is preferable that they are the same in terms of easy availability of raw materials.
[0050] X 2 is a hydrolyzable group, and Si—X 2 is hydrolyzed to produce Si—OH. Therefore, in the composition, X 2 may be hydrolyzed to a hydroxyl group. Examples of hydrolyzable groups include an alkoxy group, an acyloxy group, a ketoxime group, an alkenyloxy group, an amino group, an aminoxy group, an amide group, an isocyanate group, and a halogen atom. From the viewpoint of the balance between the chemical stability and ease of hydrolysis of compound (2), an alkoxy group, an isocyanate group, and a halogen atom are preferred. As the alkoxy group, an alkoxy group having 1 to 4 carbon atoms is preferred, and a methoxy group, an ethoxy group, and the like are more preferred. As the halogen atom, a chlorine atom and the like are preferred. X 2 As the X, a methoxy group, an ethoxy group, a chlorine atom, etc. are particularly preferred. 2 If there are multiple X 2may be the same or different, and it is preferable that they are the same in terms of easy availability of raw materials.
[0051] n2 is an integer of 1 to 3, preferably 2 to 3, and particularly preferably 3, from the viewpoint of improving the adhesion between the water-repellent layer and the substrate.
[0052] Preferred compounds (2) include R 22 is a linear alkyl group having 8 to 20 carbon atoms, and X 2 is a methoxy group, an ethoxy group, or a chlorine atom, and n2 is 3. Specific examples include octyltrimethoxysilane, octyltrichlorosilane, octadecyltrimethoxysilane, and octadecyltrichlorosilane. Compound (2) can be produced by a known method, and commercially available products may also be used as compound (2).
[0053] Examples of the hydrolyzable bissilane (SB) include the compound (4) described below. When the hydrolyzable bissilane (SB) is used, the same effects as when the hydrolyzable alkylsilane (SR) is used can be obtained.
[0054] <Other hydrolyzable silicon compounds (ST)> The one or more hydrolyzable dialkyl silicones (SC) can contain one or more other hydrolyzable silicon compounds other than the hydrolyzable dialkyl silicones (SC), the hydrolyzable alkyl silanes (SR), and the hydrolyzable bissilanes (SB). Examples of the other hydrolyzable silicon compounds include tetrafunctional hydrolyzable silicon compounds in which n3 is 4 among the compounds (3) described below.
[0055] <Blending ratio> In the composition for forming a water-repellent layer, relative to 100 parts by mass of the total amount of one or more hydrolyzable dialkyl silicones (SC), one or more hydrolyzable alkyl silanes (SR), and one or more hydrolyzable bisalkyl silanes (SB), the amount of the one or more hydrolyzable dialkyl silicones (SC) is preferably 99 to 50 parts by mass, more preferably 97 to 75 parts by mass, and the total amount of the one or more hydrolyzable alkyl silanes (SR) and one or more hydrolyzable bisalkyl silanes (SB) is preferably 1 to 50 parts by mass, more preferably 3 to 25 parts by mass. By designing the blending ratio as described above, it is easy to form a water-repellent layer that has good water repellency in the initial state and good weather resistance.
[0056] <Organic Solvent (VT)> The water-repellent layer-forming composition may contain one or more organic solvents (VT) as needed. Examples of organic solvents (VT) include alcohols, ethers, ketones, aromatic hydrocarbons, paraffinic hydrocarbons, and acetate esters. When an organic solvent is contained in the raw materials constituting the water-repellent layer-forming composition, the one or more organic solvents (VT) include the organic solvents in the raw materials. The content of organic solvents (VT) in the water-repellent layer-forming composition (the total amount when multiple types are used) is not particularly limited. From the viewpoints of thickness control of the water-repellent layer, uniformity of the water-repellent layer, economy, and workability, the content is preferably 80 to 98% by mass, more preferably 85 to 95% by mass.
[0057] <Water> The water-repellent layer-forming composition may contain water as needed. When water is contained in the raw materials constituting the water-repellent layer-forming composition, the water includes the water in the raw materials. In the water-repellent layer-forming step, the hydrolysis and condensation reaction of one or more hydrolyzable silicon compounds (ST) can be carried out using moisture in the atmosphere, so the water-repellent layer-forming composition does not need to contain water. The content of water in the water-repellent layer-forming composition is not particularly limited, and is, for example, 0 to 2 mass %.
[0058] <Catalyst> The water-repellent layer-forming composition may contain one or more catalysts as needed. When a catalyst is contained in the raw materials constituting the water-repellent layer-forming composition, the one or more catalysts include the catalyst contained in the raw materials. Examples of catalysts include acid catalysts and alkali catalysts. Examples of acid catalysts include hydrochloric acid, nitric acid, acetic acid, sulfuric acid, phosphoric acid, sulfonic acid, methanesulfonic acid, and p-toluenesulfonic acid. Examples of alkali catalysts include sodium hydroxide, potassium hydroxide, and ammonia. Acid catalysts are preferred. The catalyst can be used in the form of an aqueous solution. The content of the catalyst in the water-repellent layer-forming composition is not particularly limited. The content of the one or more catalysts (the total amount, if multiple types are used) is preferably 0.0001 to 10 mass% relative to the content of the one or more hydrolyzable silicon compounds (ST) (the total amount, if multiple types are used).
[0059] When one or more hydrolyzable silicon compounds (ST) contain a chlorine atom as a hydrolyzable group, the compound is highly reactive, and therefore, from the viewpoint of the storage stability of the composition for forming a water-repellent layer, the composition for forming a water-repellent layer preferably contains substantially no water and no catalyst. "Substantially no" means that the content in the composition for forming a water-repellent layer is 0.3 mass % or less.
[0060] <Other Optional Components> The water-repellent layer-forming composition may contain one or more other optional components in addition to those described above, as necessary. Examples of the other optional components include metal oxide particles, coloring materials such as dyes and pigments, antifouling materials, and additives such as various resins.
[0061] (Underlayer) The water-repellent film has an underlayer containing a siloxane compound but not containing fluorine atoms below the water-repellent layer. The siloxane compound is a compound having a siloxane bond (Si—O bond). The underlayer can improve the moisture resistance and adhesion of the water-repellent film. The underlayer can also function as a barrier layer that blocks components such as active species that migrate from the glass plate to the water-repellent film.
[0062] The underlayer can be formed using a composition for forming an underlayer containing one or more hydrolyzable silicon compounds (SU) selected from the group consisting of a compound represented by the following formula (3) (also referred to as compound (3)) and a compound represented by the following formula (4) (also referred to as compound (4)), which may be partially hydrolyzed and condensed between the same or different species. Si(R 31 ) 4-n3 (X 3 ) n3 ...(3) (In the above formula, R 31 are each independently a monovalent hydrocarbon group. 3 are each independently a hydrolyzable group. 3 may be hydrolyzed to a hydroxyl group. n3 is an integer of 1 to 4.) X 4 3 Si-R 4 -SiX 4 3 ...(4) (In the above formula, R 4 is a divalent organic group. 4 are each independently a hydrolyzable group. 4 may be hydrolyzed to a hydroxyl group.) The undercoat layer may be a dried and cured product of the composition for forming the undercoat layer.
[0063] X in formula (3) 3 is a hydrolyzable group, and Si—X 3 is hydrolyzed to produce Si—OH. Therefore, in the composition, X 3 may be hydrolyzed to a hydroxyl group. Examples of hydrolyzable groups include an alkoxy group, an acyloxy group, a ketoxime group, an alkenyloxy group, an amino group, an aminoxy group, an amide group, an isocyanate group, and a halogen atom. From the viewpoint of the balance between the chemical stability and ease of hydrolysis of compound (3), an alkoxy group, an isocyanate group, and a halogen atom are preferred. As the alkoxy group, an alkoxy group having 1 to 4 carbon atoms is preferred, and a methoxy group, an ethoxy group, and the like are more preferred. As the halogen atom, a chlorine atom and the like are preferred. X 3 As the X, a methoxy group, an ethoxy group, a chlorine atom, etc. are particularly preferred. 3may be the same or different, and it is preferable that they are the same in terms of easy availability of raw materials. 4 The same applies to.
[0064] Compound (3) is dimethyldimethoxysilane ((CH 3 ) 2 Si(OCH 3 ) 2 ) and other bifunctional hydrolyzable silicon compounds; methyltrimethoxysilane (MTMS) (CH 3 Si(OCH 3 ) 3 trifunctional hydrolyzable silicon compounds such as Si(NCO) 4 , tetraethoxysilane (TEOS) (Si(OCH 3 ) 4 ), and Si(OC 2 H 5 ) 4 and tetrafunctional hydrolyzable silicon compounds such as the above.
[0065] In formula (4), R 4 is any divalent organic group. 4 For example, an alkylene group is preferred. The number of carbon atoms in the alkylene group is preferably 1 to 8, more preferably 1 to 3. When the number of carbon atoms in the alkylene group is within this range, the underlayer has appropriate hydrophobicity, the moisture resistance of the water-repellent film can be improved, and the dynamic water repellency of the resulting water-repellent film is good. 4 Specific examples of the compound (4) in which is an alkylene group include (1,2-bistrimethoxysilylethane) (BTE) ((CH 3 O) 3 SiC 2 H 4 Si(OCH 3 ) 3 ), 1,6-bistrimethoxysilylhexane ((CH 3 O) 3 SiC 6 H 12 Si(OCH 3 ) 3 ), 1,8-bistrimethoxysilyl octane (BTO) ((CH 3 O) 3 SiCH 8CH 16 Si(OCH 3 ) 3 ); (C 2 H 5 O) 3 SiC 2 H 4 Si(OC 2 H 5 ) 3 ; (OCN) 3 SiC 2 H 4 Si(NCO) 3 ; Cl 3 SiC 2 H 4 SiCl 3 etc. 4 Specific examples of the compound (4) in which is a divalent organic group other than an alkylene group include bis[3-(trimethoxysilyl)propyl]amine, bis(3-(triethoxysilyl)propyl)tetrasulfide, and 4,4'-bis(triethoxysilyl)-1,1'-biphenyl.
[0066] <Organic Solvent> The underlayer-forming composition may contain one or more organic solvents (VU). Examples of organic solvents (VU) are the same as those of the water-repellent layer-forming composition. When an organic solvent is contained in the raw materials constituting the underlayer-forming composition, the one or more organic solvents (VU) include the organic solvent in the raw materials. The content of the organic solvent (VU) in the underlayer-forming composition is not particularly limited. From the viewpoints of thickness control of the underlayer, uniformity of the underlayer, economy, and workability, it is preferably 80 to 99% by mass, more preferably 90 to 98% by mass.
[0067] <Water> The underlayer-forming composition may contain water as needed. When water is contained in the raw materials constituting the underlayer-forming composition, the water includes the water in the raw materials. In the underlayer-forming step, the hydrolysis and condensation reaction of one or more hydrolyzable silicon compounds (SU) can be carried out using moisture in the atmosphere, so the underlayer-forming composition does not need to contain water. The content of water in the underlayer-forming composition is not particularly limited and is, for example, 0 to 10% by mass.
[0068] <Catalyst> The underlayer-forming composition may contain one or more catalysts as needed. Examples of catalysts are the same as those for the water-repellent layer-forming composition. When a catalyst is contained in the raw materials constituting the underlayer-forming composition, the one or more catalysts include the catalyst in the raw materials. The content of the catalyst in the underlayer-forming composition is not particularly limited. The content of the one or more catalysts (the total amount, if multiple types) is preferably 0.0001 to 10 mass% relative to the content of the one or more hydrolyzable silicon compounds (SU) (the total amount, if multiple types).
[0069] When one or more hydrolyzable silicon compounds (SU) contain a chlorine atom as a hydrolyzable group, the compound has high reactivity, and therefore, from the viewpoint of the storage stability of the composition for forming an underlayer, the composition for forming an underlayer preferably contains substantially no water and no catalyst. "Substantially no" means that the content in the composition for forming an underlayer is 0.3 mass% or less.
[0070] <Other Optional Components> The undercoat layer-forming composition may contain one or more other optional components in addition to those described above, as necessary. Examples of the other optional components include metal oxide particles, coloring materials such as dyes and pigments, antifouling materials, and additives such as various resins.
[0071] (Method for Forming Water-Repellent Layer) <Step of Forming Base Layer> The step of forming the base layer can include, for example, the steps of: preparing a base layer-forming composition containing one or more hydrolyzable silicon compounds (SU) that may be partially hydrolyzed and condensed homogeneously or heterogeneously, preferably selected from the group consisting of compound (3) and compound (4); applying the base layer-forming composition to at least a portion of the tin-containing surface of the glass plate and drying (partially or completely) as necessary to form an uncured base layer; and curing the uncured base layer. The uncured base layer may be cured before the application of the water-repellent layer-forming composition or simultaneously with the curing of the uncured water-repellent layer.
[0072] <Water-repellent layer forming process> The water-repellent layer forming process can include, for example, the steps of: preparing a water-repellent layer forming composition containing one or more hydrolyzable dialkyl silicones (SC) and one or more hydrolyzable silicon compounds (ST) which may be partially hydrolyzed and condensed between the same or different species; applying the water-repellent layer forming composition onto the uncured base layer or at least a partial region of the base layer, and drying (partially drying or completely drying) as necessary to form an uncured water-repellent layer; and curing the uncured water-repellent layer.
[0073] Examples of methods for applying the base layer-forming composition and the water-repellent layer-forming composition include hand coating, brush coating, flow coating, spin coating, dip coating, squeegee coating, and spray coating. Examples of methods for drying a coating layer made of the base layer-forming composition or the water-repellent layer-forming composition include a method in which the glass plate on which the coating layer has been formed is left to stand at room temperature and normal pressure in any atmosphere such as air or nitrogen. The relative humidity of the atmosphere in the drying step is preferably not high, preferably less than 50%, more preferably 40% or less.
[0074] Curing conditions can be appropriately designed depending on the composition, concentration, etc. Curing of the uncured underlayer can be carried out under normal pressure in any atmosphere, such as air or nitrogen. The temperature of the atmosphere is not particularly limited, but is preferably 20 to 50°C. The relative humidity of the atmosphere is not particularly limited, but is preferably 50 to 90%. When the relative humidity of the atmosphere is 50% or higher, curing can be carried out effectively by utilizing the moisture in the atmosphere. The time required for curing depends on the composition, concentration, and curing conditions of the underlayer-forming composition. Approximately 1 to 72 hours is preferred. Curing of the uncured water-repellent layer can be carried out under normal pressure in any atmosphere, such as air or nitrogen. The temperature of the atmosphere is not particularly limited, but is preferably 20 to 100°C, more preferably 20 to 80°C. The relative humidity of the atmosphere is not particularly limited, but is preferably 0 to 90%, more preferably 50 to 90%. When the relative humidity of the atmosphere is 50% or higher, curing can be carried out effectively by utilizing the moisture in the atmosphere. The time required for curing depends on the composition, concentration, and curing conditions of the water-repellent layer-forming composition, but is preferably about 10 minutes to 72 hours.
[0075] (Other Coatings) The water-repellent structure of the present disclosure can have one or more other coatings other than the water-repellent film, if necessary. The other coatings can contain one or more functional components (FU). Functions of the functional component (FU) include selective transmission, selective absorption, or selective reflection of light or radio waves in a specific wavelength range; reflection or absorption of heat rays; anti-reflection; low reflection; low radiation; electrical conduction; heating; scratch resistance; anti-fouling; antibacterial; decoration such as coloring; combinations thereof, and the like. The water-repellent structure of the present disclosure can have, for example, a coating containing one or more functional components selected from the group consisting of an ultraviolet ray shielding agent and an infrared ray shielding agent on the other surface of the glass plate (the tin-free surface, top surface, T surface, which is substantially free of tin atoms).
[0076] As the ultraviolet screening agent, known agents can be used, and they may be of either an ultraviolet absorbing type or an ultraviolet reflecting type. Preferred is one or more ultraviolet absorbers selected from the group consisting of benzophenone-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, benzodithiol-based ultraviolet absorbers, azomethine-based ultraviolet absorbers, indole-based ultraviolet absorbers, and triazine-based ultraviolet absorbers.
[0077] As the infrared shielding agent, known agents can be used, and they may be of an infrared absorbing type or an infrared reflecting type. As the infrared shielding agent, infrared shielding particles are preferred. As the infrared shielding particles, metal compound particles containing one or more metal compounds are preferred. For example, indium tin oxide (ITO), antimony-doped tin oxide (ATO), cesium-doped tungsten oxide (CWO (registered trademark)), fluorine-doped tin oxide (FTO), lanthanum hexaboride (LaB 6 ), and vanadium pentoxide (V 2 O 5 Metal compound particles containing one or more metal compounds selected from the group consisting of:
[0078] The infrared shielding particles include cesium-doped tungsten oxide (CWO®) and / or lanthanum hexaboride (LaB 6When using such metal compound particles, the absorbance of the coating for light with a wavelength of 800 to 1500 nm is preferably 2 The value obtained by dividing the mass of the infrared-shielding particles contained per unit area by the mass of the infrared-shielding particles contained per unit area can be made relatively large, for example, 1.5 or more. In this case, the content of the infrared-shielding particles in the coating can be reduced. This reduces the absolute number of particles present in the vicinity of the interface between the coating and the glass substrate, improving the adhesion between the glass substrate and the coating and improving the abrasion resistance.
[0079] The coating can be formed by a known method, and can be, for example, a dried and cured product of a liquid composition (LC) containing one or more hydrolyzable silicon compounds (S) having a hydrolyzable group and one or more functional components (FU). The coating formation process can include, for example, the steps of: preparing a liquid composition (LC) containing one or more hydrolyzable silicon compounds (S) having a hydrolyzable group and one or more functional components (FU); applying the liquid composition (LC) to the other surface of the glass plate and optionally drying (partially or completely) to form a coating film; and curing the coating film. The hydrolyzable silicon compound (S) is preferably one or more hydrolyzable silicon compounds selected from compounds (1) to (5), which may be partially hydrolyzed and condensed with each other, either homogeneously or heterogeneously.
[0080] The water-repellent layer included in the water-repellent structure of the present disclosure has good water repellency in the initial state and can have durability that allows good water repellency to be maintained even after long-term use. One example of durability is weather resistance. The water-repellent layer included in the water-repellent structure of the present disclosure can have weather resistance with little decrease in water repellency in an accelerated weathering test. The water-repellent layer included in the water-repellent structure of the present disclosure does not contain fluorine atoms, so there is no concern about environmental impact. As described above, according to the present disclosure, a water-repellent structure can be provided that has a non-fluorine-based water-repellent layer formed on the tin-containing surface of a glass plate, has good water repellency in the initial state, and has good weather resistance.
[0081] [Applications] The water-repellent structure of the present disclosure is suitable for window glass for transportation equipment. Examples of transportation equipment include trains, automobiles, ships, and aircraft. When the water-repellent structure of the present disclosure is used in window glass for transportation equipment, adhesion of rain, frost, ice, snow, and the like can be effectively suppressed. The water-repellent structure of the present disclosure is suitable for window glass (windshield, side glass, rear glass, etc.) for vehicles such as automobiles.
[0082] The present invention will be described below based on examples, but is not limited to these. Examples 11 to 19, 21, 31, 41, 51, 61, and 71 are examples, and Examples 111 to 114 and 171 are comparative examples. Unless otherwise specified, room temperature is 20 to 25°C.
[0083] [Materials] The following materials were prepared. <Compound (1)> (Hydrolyzable silicone (1-1)) Compound (1-m) (10.0 g) represented by the following formula, vinyltrimethoxysilane (1.47 g), and Pt catalyst (2 mass % xylene solution of Pt 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex) (0.015 g) were placed in a reactor (internal volume 50 mL) equipped with a stirrer and a Dimroth reactor, and the mixture was stirred at room temperature for 24 hours.
[0084] ...(1-m)
[0085] Volatile components were removed from the resulting crude reaction liquid at a temperature of 50°C and a pressure of 1.3 kPa to obtain 10.4 g of hydrolyzable silicone (1-1) represented by the following formula in a yield of 98%. ...(1-1) In the above formula, Y 1 is an ethylene group.
[0086] (Hydrolyzable Silicone (1-2)) A reactor (internal volume: 50 mL) equipped with a stirrer and a Dimroth reactor was charged with 10.0 g of the compound (1-n) represented by the following formula, 0.801 g of vinyltrimethoxysilane, and 0.008 g of a Pt catalyst (a 2% by mass xylene solution of a 1,3-divinyl-1,1,3,3-tetramethyldisiloxane complex of Pt), and the mixture was stirred at room temperature for 24 hours.
[0087] ...(1-n)
[0088] Volatile components were removed from the resulting crude reaction liquid at a temperature of 50°C and a pressure of 1.3 kPa to obtain 10.1 g of hydrolyzable silicone (1-2) represented by the following formula in a yield of 98%. ...(1-2) In the above formula, Y 1 is an ethylene group.
[0089] <Compound (2) or Compound (3)> C18(OMe): n-octadecyltrimethoxysilane (CH 3 (CH 2 ) 17 Si(OCH 3 ) 3 ), C8(OMe): n-octyltrimethoxysilane (CH 3 (CH 2 ) 7 Si(OCH 3 ) 3 ), C3Si(OMe):methyltrimethoxysilane (MTMS) (CH 3 Si(OCH 3 ) 3 ), TEOS: tetraethoxysilane, SI400: tetraisocyanate silane (Si(NCO 4 )).
[0090] <Compound (4)> BTE: 1,2-bistrimethoxysilylethane ((CH 3 O) 3 SiC 2 H 4 Si(OCH 3 ) 3 ), BTO: 1,8-bistrimethoxysilyl octane ((CH 3 O) 3 SiCH 8 CH 16 Si(OCH 3 ) 3 ).
[0091] <Mixed Solvent> AP-11: "Solmix AP-11" manufactured by Japan Alcohol Sales Co., Ltd.
[0092] [Evaluation Items and Evaluation Methods] The surface of the water-repellent layer of the water-repellent structure obtained in each example was evaluated as follows: Before each measurement, dirt on the surface of the water-repellent layer was removed with a paper cloth soaked in ethanol or butyl acetate.
[0093] (Thickness of Underlayer) The thickness of the center of the underlayer was measured using a stylus surface profiler ("DEKTAK 150" manufactured by ULVAC).
[0094] (Initial Water Contact Angle) A water droplet with a diameter of 1 mm was placed on the surface of the water-repellent layer of the water-repellent structure, and the water contact angle was measured using a fully automatic contact angle meter ("DM-701" manufactured by Kyowa Interface Science Co., Ltd.) Measurements were taken at six different points on the surface of the water-repellent layer, and the average value was used as data.
[0095] (Water contact angle after accelerated weathering test) Using a "Sunshine Weather Meter S80H" manufactured by Suga Test Instruments Co., Ltd. as an accelerated weathering tester, accelerated weathering tests were performed for 1000 hours, 1500 hours, or 2000 hours in accordance with JIS D 0205 5.4 under conditions of a black panel temperature of 63°C, ultraviolet irradiation, and rainfall. The water-repellent structure was placed so that light was irradiated from the water-repellent film side. The rainfall conditions were a repetition of one cycle consisting of 48 minutes of rainfall and 12 minutes of rest. The water contact angle of the surface of the water-repellent layer after the accelerated weathering test was determined using the same method as for (initial water contact angle).
[0096] (Initial Haze Value) Using "Haze Guard Plus" manufactured by BYK-Gardner, the initial haze value of the water-repellent structure was measured by irradiating measurement light from the water-repellent film side of the water-repellent structure.
[0097] (Haze Value After Heat Resistance Test) An "EYELA Constant Temperature Dryer NDO-401" manufactured by Toyorika Co., Ltd. was prepared as a test machine. The water-repellent structure was placed in the test machine set to 80°C, and a heat resistance test was carried out for 500 hours or 1000 hours. The haze value of the water-repellent structure after the heat resistance test was determined in the same manner as in (initial haze value).
[0098] [Production Example 11] (Preparation of undercoat layer-forming composition (U1)) 99.7 g of 2-propanol was placed in a glass container, and 0.051 g of tetraethoxysilane (TEOS) and 0.050 g of 1,2-bis(triethoxysilyl)ethane (BTE) were added thereto. Next, 0.187 g of a 0.463 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at room temperature for about 3 hours to prepare undercoat layer-forming composition (U1).
[0099] [Production Example 12] (Preparation of undercoat layer-forming composition (U2)) 99.7 g of 2-propanol was placed in a glass container, and 0.050 g of 1,2-bis(triethoxysilyl)ethane (BTE) was added thereto. 0.187 g of a 0.463 mass % aqueous nitric acid solution was then added dropwise, and the mixture was mixed and stirred at room temperature for approximately 3 hours. 0.051 g of tetraisocyanate silane (SI400) was added to the stirred solution, and the mixture was mixed and stirred to prepare undercoat layer-forming composition (U2).
[0100] [Production Example 13] (Preparation of undercoat layer-forming composition (U3)) 99.7 g of 2-propanol was placed in a glass container, and 0.051 g of tetraethoxysilane (TEOS) and 0.050 g of methyltrimethoxysilane (MTMS) (CSi(OMe)) were added thereto. Next, 0.187 g of a 0.463 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at room temperature for about 3 hours to prepare undercoat layer-forming composition (U3).
[0101] [Production Example 14] (Preparation of undercoat layer-forming composition (U4)) 99.7 g of 2-propanol was placed in a glass container, and 0.051 g of tetraethoxysilane (TEOS) and 0.050 g of 1,8-bistrimethoxysilyl octane (BTO) were added thereto. Next, 0.187 g of a 0.463 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at room temperature for about 3 hours to prepare undercoat layer-forming composition (U4).
[0102] [Production Example 21] (Preparation of Water-Repellent Layer-Forming Composition (T1)) 7.17 g of 2-butanol was placed in a glass container, and 1.67 g of 2-propanol and 0.96 g of hydrolyzable silicone (1-1) were added thereto, followed by mixing and stirring at room temperature for approximately 1 minute. Next, 0.17 g of a 10 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at 60°C for 2 hours using a water bath. Next, 0.039 g of n-octadecyltrimethoxysilane (C18OMe) was added, and the mixture was mixed and stirred at 60°C for 1 hour. The stirred solution was diluted with a mixed solvent (AP-11) to a solids content of 0.1 mass %, thereby preparing a water-repellent layer-forming composition (T1).
[0103] [Production Example 22] (Preparation of Water-Repellent Layer-Forming Composition (T2)) 7.17 g of 2-butanol was placed in a glass container, and 1.67 g of 2-propanol and 0.96 g of hydrolyzable silicone (1-1) were added, followed by mixing and stirring at room temperature for approximately 1 minute. Next, 0.17 g of a 10 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at 60°C using a water bath for 2 hours. Next, 0.039 g of n-octyltrimethoxysilane (COMe) was added, and the mixture was mixed and stirred at 60°C for 1 hour. The stirred solution was diluted with a mixed solvent (AP-11) to a solids content of 0.1 mass %, thereby preparing a water-repellent layer-forming composition (T2).
[0104] [Production Example 23] (Preparation of Water-Repellent Layer-Forming Composition (T3)) 7.17 g of 2-butanol was placed in a glass container, and 1.67 g of 2-propanol and 0.96 g of hydrolyzable silicone (1-1) were added thereto, followed by mixing and stirring at room temperature for approximately 1 minute. Next, 0.17 g of a 10 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at 60°C using a water bath for 2 hours. Next, 0.039 g of 1,2-bis(triethoxysilyl)ethane (BTE) was added, and the mixture was mixed and stirred at 60°C for 1 hour. The stirred solution was diluted with a mixed solvent (AP-11) to a solids content of 0.1 mass %, thereby preparing a water-repellent layer-forming composition (T3).
[0105] [Production Example 24] (Preparation of Water-Repellent Layer-Forming Composition (T4)) 7.17 g of 2-butanol was placed in a glass container, and 1.67 g of 2-propanol and 0.96 g of hydrolyzable silicone (1-2) were added thereto, followed by mixing and stirring at room temperature for approximately 1 minute. Next, 0.17 g of a 10 mass % aqueous nitric acid solution was added dropwise, and the mixture was mixed and stirred at 60°C using a water bath for 2 hours. Next, 0.039 g of n-octadecyltrimethoxysilane (C18OMe) was added, followed by mixing and stirring at 60°C for 1 hour. The stirred solution was diluted with a mixed solvent (AP-11) to a solids content of 0.1 mass %, thereby preparing a water-repellent layer-forming composition (T4).
[0106] [Example 11] (Production of water-repellent structure) Float glass (high heat ray absorbing glass "UVFL" manufactured by AGC, 300 mm x 300 mm, thickness 3.5 mm) was prepared as a glass plate. X-ray Photoelectron Spectroscopy (XPS) analysis was performed on both sides of the glass plate using a "Quantera SXM" manufactured by ULVAC-PHI, Inc. Peaks in the range of 480 to 490 ev were identified as peaks derived from tin atoms, and the tin content was calculated from the area intensity of the peaks. The tin content of the tin-free surface (top surface) was 0.01 atm%, and the tin content of the tin-containing surface (bottom surface) containing a large amount of tin atoms was 0.5 atm%. Onto the tin-containing surface (bottom surface) of this glass plate, 0.50 g of the primer layer-forming composition (U1) was applied by spray coating using an "r-coater" manufactured by Asahi Sunac Corporation, and dried at room temperature for about 1 minute to form an uncured primer layer. Next, 0.50 g of the water-repellent layer-forming composition (T1) was applied to the surface of the uncured primer layer by the same spray coating method as above.
[0107] The resulting laminate was then placed in a thermo-hygrostat chamber set at 50°C and 60% relative humidity for approximately 15 minutes. The laminate was removed from the chamber, and the surface of the laminate was wiped with a paper cloth (Kimberly-Clark Corporation's "Kimwipe") impregnated with 1.0 mL of butyl acetate to remove excess water-repellent layer-forming composition. The laminate was then placed in a thermo-hygrostat chamber set at 50°C and 60% relative humidity for 47 hours. In this manner, a water-repellent structure was obtained in which a water-repellent film consisting of a base layer and a water-repellent layer was formed on the tin-containing surface (bottom surface) of the glass plate. Table 1 shows the main manufacturing conditions and evaluation results. In the examples shown in Table 1, conditions not listed in the table were common conditions.
[0108] [Examples 12 to 19, 21, 31, 41, 51, 61, 71, 111 to 114, 171] Water-repellent structures were obtained in the same manner as in Example 11, except that one or more of the conditions of the type of composition for forming the base layer, the type of composition for forming the water-repellent layer, and the thickness of the base layer were changed. The main production conditions and evaluation results are shown in Table 1.
[0109]
[0110] [Summary of Results] In each example shown in Table 1, a water-repellent film was formed having a laminate structure of an underlayer containing a siloxane compound and not containing fluorine atoms, and a water-repellent layer containing dimethyl silicone and not containing fluorine atoms. In Examples 11 to 19, 21, 31, 41, 51, 61, and 71 in which the underlayer thickness was 50 to 600 nm, the water contact angle was 95° or greater initially and after 1000 hours of accelerated weathering testing, the water contact angle was 85° or greater after 1500 hours of accelerated weathering testing, and the water contact angle was 70° or greater after 2000 hours of accelerated weathering testing, demonstrating good weather resistance. Note that if the water contact angle after 1000 hours of accelerated weathering testing is 95° or greater, the initial water contact angle is considered to be 95° or greater.
[0111] In particular, in Examples 12 to 19, 21, 31, 41, 51, 61, and 71, in which the thickness of the underlayer was 55 to 600 nm, the water contact angle after 1,500 hours of accelerated weathering testing was 90° or greater. In Examples 14 to 19, in which the thickness of the underlayer was 70 to 600 nm, the water contact angle after 2,000 hours of accelerated weathering testing was 90° or greater. In these examples, water-repellent structures with better weather resistance were obtained. In Examples 11 to 19, 21, 31, 41, 51, 61, and 71, in which the thickness of the underlayer was 50 to 600 nm, the initial haze value was 0.5% or less, and a crack-free, highly transparent water-repellent film was stably formed. In particular, in Examples 11 to 18, 21, 31, 41, 51, 61, and 71 in which the thickness of the undercoat layer was 50 to 500 nm, the haze value after heat resistance tests of 500 hours and 1000 hours was 0.5% or less, and a water-repellent film with good heat resistance was formed.
[0112] In Examples 111, 112, and 171, in which the thickness of the underlayer was less than 50 nm, the water contact angle after 1000 hours of accelerated weathering test was 90° or less, the water contact angle after 1500 hours of accelerated weathering test was 80° or less, and the water contact angle after 2000 hours of accelerated weathering test was less than 70°, and the weather resistance was poor. In Examples 113 and 114, in which the thickness of the underlayer was more than 600 nm, the initial haze value was 5.0% or more, and a highly transparent water-repellent film could not be formed. It is believed that cracks occurred.
[0113] The present invention is not limited to the above-described embodiments and examples, and various modifications can be made to the design as appropriate without departing from the spirit of the present invention.
[0114] This application claims priority based on Japanese Patent Application No. 2023-075358, filed May 1, 2023, the disclosure of which is incorporated herein by reference in its entirety.
[0115] 1: Water-repellent structure, 10: Glass plate, 10S: Surface of glass plate, 20: Water-repellent film, 21: Water-repellent layer, 22: Underlayer.
Claims
1. A water-repellent structure comprising a glass plate and a water-repellent layer formed on one surface of the glass plate, the water-repellent layer containing one or more dialkyl silicones in which the alkyl group has 1 to 3 carbon atoms and containing no fluorine atoms, the surface of the glass plate containing tin atoms, and a base layer containing a siloxane compound and containing no fluorine atoms between the glass plate and the water-repellent layer, the base layer having a thickness of 50 to 600 nm.
2. The water-repellent structure according to claim 1, wherein the thickness of the underlayer is 55 to 600 nm.
3. The water-repellent structure according to claim 2, wherein the thickness of the underlayer is 55 to 500 nm.
4. The water-repellent structure according to claim 3, wherein the thickness of the underlayer is 70 to 500 nm.
5. The water-repellent structure according to claim 1 or 2, wherein the one or more dialkyl silicones include one or more hydrolyzable dialkyl silicones having a hydrolyzable group.
6. The water-repellent structure according to claim 5, wherein the hydrolyzable dialkyl silicone is a compound represented by the following formula (1): 13 -(SiR 12 2 O) k1 -SiR 12 2 -Y 1 -Si(R 11 ) 3-n1 (X 1 ) n1 ...(1) (In the above formula, R 13 is an alkyl group having 1 to 30 carbon atoms. 12 are each independently an alkyl group having 1 to 3 carbon atoms. 1 is an alkylene group having 2 to 4 carbon atoms or an oxygen atom. 11 Each of X is independently a monovalent hydrocarbon group. 1 Each of X is independently a hydrolyzable group. 1 may be hydrolyzed to a hydroxyl group. k1 is an integer of 10 to 300. n1 is an integer of 1 to 3.
7. The water-repellent structure according to claim 1 or 2, wherein the water-repellent layer is a dried and cured product of a composition for forming a water-repellent layer, which contains one or more hydrolyzable dialkyl silicones having hydrolyzable groups and contains one or more hydrolyzable silicon compounds which may be partially hydrolyzed and condensed between the same or different species.
8. The water-repellent structure according to claim 7, wherein the hydrolyzable dialkyl silicone is a compound represented by the following formula (1): 13 -(SiR 12 2 O) k1 -SiR 12 2 -Y 1 -Si(R 11 ) 3-n1 (X 1 ) n1 ...(1) (In the above formula, R 13 is an alkyl group having 1 to 30 carbon atoms. 12 are each independently an alkyl group having 1 to 3 carbon atoms. 1 is an alkylene group having 2 to 4 carbon atoms or an oxygen atom. 11 Each of X is independently a monovalent hydrocarbon group. 1 Each of X is independently a hydrolyzable group. 1 may be hydrolyzed to a hydroxyl group. k1 is an integer of 10 to 300. n1 is an integer of 1 to 3.
9. The water-repellent structure according to claim 7, wherein the one or more hydrolyzable silicon compounds further include one or more compounds selected from one or more hydrolyzable alkylsilanes having a hydrolyzable group and an alkyl group, and one or more hydrolyzable bissilanes having hydrolyzable groups at both ends with a divalent organic group between them, which may be partially hydrolyzed and condensed between the same or different species.
10. The water-repellent structure according to claim 9, wherein the hydrolyzable alkylsilane is a compound represented by the following formula (2), and the hydrolyzable bissilane is a compound represented by the following formula (4). 22 -Si(R 21 ) 3-n2 (X 2 ) n2 ...(2) (In the above formula, R 22 is an alkyl group having 1 to 30 carbon atoms. 21 Each of X is independently a monovalent hydrocarbon group. 2 Each of X is independently a hydrolyzable group. 2 may be hydrolyzed to a hydroxyl group. n2 is an integer of 1 to 3.) X 4 3 Si-R 4 -SiX 4 3 ...(4) (In the above formula, R 4 is a divalent organic group. 4 Each of X is independently a hydrolyzable group. 4 may be hydrolyzed to a hydroxyl group.) 11. The water-repellent structure according to claim 1 or 2, wherein the undercoat layer is a dried and cured product of a composition for forming an undercoat layer, the composition containing one or more hydrolyzable silicon compounds, which may be partially hydrolyzed and condensed between the same or different species, selected from the group consisting of compounds represented by the following formula (3) and compounds represented by the following formula (4): Si(R 31 ) 4-n3 (X 3 ) n3 ...(3) (In the above formula, R 31 Each of X is independently a monovalent hydrocarbon group. 3 Each of X is independently a hydrolyzable group. 3 may be hydrolyzed to a hydroxyl group. n3 is an integer of 1 to 4.) X 4 3 Si-R 4 -SiX 4 3 ...(4) (In the above formula, R 4 is a divalent organic group. 4 Each of X is independently a hydrolyzable group. 4 may be hydrolyzed to a hydroxyl group.) 12. The water-repellent structure according to claim 1 or 2, which has an initial haze value of 0.5% or less and a haze value of 1.0% or less after a heat resistance test in which the structure is held at 80° C. for 500 hours.
13. A water-repellent structure according to claim 1 or 2, wherein the surface of the water-repellent layer has an initial water contact angle of 92° or more, and a water contact angle of 92° or more after an accelerated weather resistance test of 1,000 hours at a black panel temperature of 63° C. in accordance with JIS D 0205 5.
4.
14. The water-repellent structure according to claim 13, wherein the surface of the water-repellent layer has a water contact angle of 85° or more after undergoing an accelerated weather resistance test for 1,500 hours at a black panel temperature of 63°C in accordance with JIS D 0205 5.
4.
15. The water-repellent structure according to claim 1 or 2, which has on the other surface of the glass plate a coating containing one or more functional components selected from the group consisting of an ultraviolet ray shielding agent and an infrared ray shielding agent.
Citation Information
Patent Citations
Surface treating material for forming film excellent in drip dropping property and method for forming surface-treated film
JP2001259509A
Translucent substrate, method of manufacturing for the same, building and vehicle
JP2002211956A
Water repellent oil repellent Anti-fouling glass panel, method of manufacturing the same and automobile and electromagnetic cooking device using the same
JP2005206447A
Hydrophobic coating including underlayer(s) deposited via flame pyrolysis
US20060110606A1