Separator for electrochemical device and electrochemical device comprising same
The separator for lithium secondary batteries with a silicon-based negative electrode uses a dual-coating layer structure of polymers with varying solubility indices to maintain pore integrity under high pressure and temperature, addressing deformation and short circuit issues, and enhancing battery performance and energy density.
Patent Information
- Application Number
- PCT/KR2024/095021
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-03
- Filing Date
- 2024-01-10
- Publication Date
- 2024-11-07
AI Technical Summary
The challenge is to develop a separator for electrochemical devices, particularly for lithium secondary batteries with silicon-based negative electrodes, that maintains pore structure integrity under high pressure and temperature during the lamination process, ensuring compression resistance and heat resistance while preventing deformation and electrical short circuits.
A separator with a porous polymer substrate coated with a first polymer resin and a second polymer resin having different solubilities in the electrolyte solution, where the first polymer resin has a higher solubility index than the second, is used. The first coating layer contains a first polymer resin such as poly styrene or poly acrylic acid, and the second coating layer contains a second polymer resin like PVDF-HFP copolymer with inorganic particles, enhancing compression resistance and heat resistance.
This configuration prevents pore deformation and ensures improved compression resistance and heat resistance, maintaining battery performance and preventing electrical short circuits, even with silicon-based anode active materials, thereby enhancing the energy density and cycle stability of lithium secondary batteries.
Smart Images

Figure KR2024095021_07112024_PF_FP_ABST
Abstract
Description
Separator for electrochemical devices and electrochemical devices containing the same
[0001] This application is based upon and claims priority to Korean Patent Application No. 10-2023-0058002, filed with the Korean Intellectual Property Office on May 3, 2023, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a separator for an electrochemical device and an electrochemical device including the same.
[0003] Secondary batteries, whose applications are expanding to include electric vehicles and other applications, such as lithium secondary batteries, typically generate electricity through a chemical reaction of lithium ions moving between the positive and negative electrodes. While the positive electrode determines the overall capacity and voltage of the battery, the negative electrode stores and then releases the lithium ions released from the positive electrode.
[0004] Meanwhile, while the anode and cathode represent the performance of a battery, the separator is the key material related to battery safety. Simply put, the separator is a thin insulating film that separates the anode and cathode within the battery, preventing them from contact. Furthermore, the separator contains microscopic pores, invisible to the naked eye, through which lithium ions move between the anode and cathode. Furthermore, when the internal temperature of the battery rises above a certain level, the pores on the separator's surface become clogged (shutdown), blocking the movement of lithium ions and preventing an internal short circuit (electrical shortage).
[0005] For these reasons, film substrates with numerous pores and polymer resin as a base are widely used as separators in electrochemical devices. Typically, electrode assemblies are manufactured through a lamination process that bonds the separator and electrode using heat and pressure. The higher the heat and pressure applied during this process, the stronger the bond between the electrode and separator.
[0006] The technical problem to be achieved by the present invention is to provide an electrochemical device separator equipped on a negative electrode including a silicon (Si)-based active material, in which the problem of pores in a porous polymer substrate being closed is improved by controlling the electrolyte solubility of a first polymer resin of a first coating layer and a second polymer resin of a second coating layer included in the coating layer, and an electrochemical device including the same.
[0007] One embodiment of the present invention provides a separator for an electrochemical device provided on a negative electrode including a silicon (Si)-based active material, the separator including: a porous polymer substrate; a first coating layer provided on at least one surface of the porous polymer substrate and including a first polymer resin; and a second coating layer provided on the first coating layer and including a second polymer resin and inorganic particles; wherein the solubility of the first polymer resin in an electrolyte is greater than the solubility of the second polymer resin in an electrolyte.
[0008] According to one embodiment of the present invention, the solubility index of the first polymer resin is about 17 MPa 1 / 2 More than 27 MPa 1 / 2 It could be as follows:
[0009] According to one embodiment of the present invention, the solubility index of the second polymer resin is about 17 MPa. 1 / 2 Less than or equal to 27 MPa 1 / 2 It may be excessive.
[0010] According to one embodiment of the present invention, the first polymer resin may include one selected from the group consisting of polystyrene, polyethyl acrylate, polymethyl acrylate, polystyrene sulfide, polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyvinyl acetate (PVAc), polyacrylonitrile (PAN), polylactic acid (PLA), polyacrylic acid (PAA), and combinations thereof.
[0011] According to one embodiment of the present invention, the second polymer resin may include one selected from the group consisting of PVDF-HFP copolymer, PVDF-CTFE copolymer, PVDF-HFP-CTFE terpolymer, cyanoethyl polyvinyl alcohol, and combinations thereof.
[0012] According to one embodiment of the present invention, the separation membrane may have a plurality of pores, the polydispersity index (PDI) of the porous polymer substrate may be about 2.5 or more and 10 or less, and the average pore diameter of the porous polymer substrate may be about 20 nm or more and 80 nm or less.
[0013] According to one embodiment of the present invention, the content of the silicon (Si)-based active material in the negative electrode may be about 50 wt% or more.
[0014] According to one embodiment of the present invention, the hardness of the cathode may be about 50 MPa or more and 350 MPa or less.
[0015] One embodiment of the present invention provides an electrochemical device including a positive electrode, a negative electrode, and an electrolyte, and a separator interposed between the positive electrode and the negative electrode.
[0016] According to one embodiment of the present invention, the solubility index of the electrolyte is about 17 MPa 1 / 2 More than 27 MPa 1 / 2 It could be as follows:
[0017] According to one embodiment of the present invention, the electrolyte may include one selected from the group consisting of propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC), and combinations thereof.
[0018] According to one embodiment of the present invention, the electrolyte may be a mixture of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC).
[0019] According to one embodiment of the present invention, the electrolyte may have a content ratio of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC) of about 10:90 to 99:1.
[0020] According to another embodiment of the present invention, a method for manufacturing a separator for an electrochemical device equipped with a negative electrode including a silicon (Si)-based active material is provided by coating a first polymer resin and a second polymer resin having different solubilities in an electrolyte on a porous polymer substrate.
[0021] The solubility of the first polymer resin in the electrolyte may be greater than the solubility of the second polymer resin in the electrolyte.
[0022] The above separation membrane may include a porous polymer substrate; a first coating layer provided on at least one surface of the porous polymer substrate and including a first polymer resin; and a second coating layer provided on the first coating layer and including a second polymer resin and inorganic particles.
[0023] The solubility index of the above first polymer resin is about 17 MPa 1 / 2 More than 27 MPa 1 / 2 It may be selected from the following materials.
[0024] The first polymer resin may be selected from the group consisting of polystyrene, polyethyl acrylate, polymethyl acrylate, polystyrene sulfide, polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyvinyl acetate (PVAc), polyacrylonitrile (PAN), polylactic acid (PLA), polyacrylic acid (PAA), and combinations thereof.
[0025] The second polymer resin may be selected from the group consisting of PVDF-HFP copolymer, PVDF-CTFE copolymer, PVDF-HFP-CTFE terpolymer, cyanoethyl polyvinyl alcohol, and combinations thereof.
[0026] According to one embodiment of the present invention, a separator for an electrochemical device can prevent deformation of pores in a porous polymer substrate even when a negative electrode including a silicon (Si)-based active material is applied by controlling the electrolyte solubility of a first polymer resin of a first coating layer and a second polymer resin of a second coating layer included in the coating layer.
[0027] An electrochemical device according to one embodiment of the present invention comprises a second coating layer comprising a second polymer resin and inorganic particles on a first coating layer comprising a first polymer resin, thereby preventing deformation of pores within a porous polymer substrate even when a negative electrode comprising a silicon (Si)-based active material is applied, thereby simultaneously improving compression resistance and heat resistance.
[0028] Figure 1 is a schematic diagram of a separator and a cathode for an electrochemical device according to one embodiment of the invention.
[0029] In some of the accompanying drawings, corresponding components are designated by the same reference numerals. Those skilled in the art will appreciate that the drawings illustrate elements simply and clearly and are not necessarily drawn to scale. For example, to facilitate understanding of various embodiments, the dimensions of some elements depicted in the drawings may be exaggerated relative to other elements. Furthermore, elements of known technology that are useful or essential in commercially feasible embodiments may often not be depicted so as not to obscure the spirit of various embodiments of the present invention.
[0030] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0031] In this specification, “A and / or B” means “A and B, or A or B.”
[0032] In this specification, when it is said that a component is “on”, this does not exclude other components being placed therebetween, unless otherwise specifically stated, but rather means that other components may be placed thereon.
[0033] In this specification, the characteristic of “having pores” means that the object includes a plurality of pores and that the pores are interconnected with each other, thereby allowing gaseous and / or liquid fluids to pass from one side of the object to the other side.
[0034] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values provided to aid understanding of the present invention.
[0035] While graphite is widely used as an anode material in lithium secondary batteries, the use of silicon (Si)-based anodes is expanding to improve their energy density. For example, silicon anodes offer approximately 10 times the energy density of graphite anodes. Therefore, their use can significantly improve battery performance, including increasing battery capacity and reducing charging speeds.
[0036] Meanwhile, in the secondary battery manufacturing process, the separator and electrode may go through a lamination process that applies relatively high temperature and pressure. When a silicon anode material is applied, its hardness is higher than that of a typical graphite anode material. Therefore, when the silicon anode material and the separator come into contact during the lamination process, there is a possibility that the pores of the separator may be deformed. Therefore, when a silicon anode material with high hardness is applied to the electrode assembly, the separator must secure compression resistance, insulation, and heat resistance so that the pores are not deformed even when it comes into contact with the silicon anode material due to the high pressure and heat of the lamination process.
[0037] For example, with recent efforts to improve productivity, process speeds have accelerated, shortening the time it takes for the separator to be heated. This has led to increased pressure to secure adhesion. However, this process raises concerns about separator deformation due to high pressure. Furthermore, the thickness of the polymer film substrate decreases significantly during the lamination process, which can significantly damage the pores of the separator. This, in turn, can lead to problems such as reduced battery performance and breakdown voltage of the separator.
[0038] In particular, when a silicon-based negative electrode active material such as Si, SiO, or Si alloy is applied as the negative electrode active material of a lithium secondary battery, the volume expansion of the negative electrode is large, so the compressive deformation of the separator due to the increase in internal pressure of the cell during charge / discharge is further aggravated. In addition, the silicon-based negative electrode active material has a larger particle size, roughness, and hardness than the graphite negative electrode active material, and thus may cause local damage to the separator during lamination with the separator. Accordingly, the present invention provides a separator having improved compression resistance, insulation, and heat resistance without deformation of pores when applying a silicon-based negative electrode active material.
[0039] In this specification, the separator has a porous characteristic including a plurality of pores, and acts as a porous ion-conducting barrier that allows ions to pass while blocking electrical contact between the cathode and the anode in an electrochemical device.
[0040] Hereinafter, the present invention will be described in more detail with reference to FIG. 1.
[0041] One embodiment of the present invention comprises a separator (100) for an electrochemical device provided on a negative electrode (200) including a silicon (Si)-based active material, wherein the separator (100) comprises: a porous polymer substrate (110); a first coating layer (131) provided on at least one surface of the porous polymer substrate (110) and including a first polymer resin; and a second coating layer (133) provided on the first coating layer (131) and including a second polymer resin and inorganic particles; wherein the solubility of the first polymer resin included in the first coating layer (131) in an electrolyte is greater than the solubility of the second polymer resin included in the second coating layer (133) in an electrolyte.
[0042] According to one embodiment of the present invention, a separator for an electrochemical device can prevent deformation of pores in a porous polymer substrate even when a negative electrode including a silicon (Si)-based active material is applied by controlling the electrolyte solubility of a first polymer resin of a first coating layer and a second polymer resin of a second coating layer included in the coating layer.
[0043] Figure 1 is a schematic diagram of a separator and a cathode for an electrochemical device according to one embodiment of the present invention. Referring to Figure 1, the separator and cathode for an electrochemical device according to one embodiment of the present invention will be described.
[0044] According to one embodiment of the present invention, the silicon (Si)-based negative electrode active material essentially includes a Si-based compound, and the Si-based compound reversibly absorbs and releases lithium through a compound formation reaction with lithium, and has a theoretical maximum capacity of about 4200 mAh / g (9366 mAh / cc, specific gravity 2.23), which is much larger than that of carbon-based materials, and is therefore used as a high-capacity negative electrode material.
[0045] According to one embodiment of the present invention, the Si-based compound is a Si / C composite, SiO2, SiO x (0 <x<2), 금속이 도핑된 SiO x (0 <x<2), 순수 Si(pure Si), 실리콘(Si) 나노 구조체, 및 Si합금(Si-alloy)로 이루어진 군으로부터 선택되는 어느 하나 또는 2종 이상의 혼합물일 수 있고, 상세하게는, SiO x (0 <x<2)의 실리콘계 산화물일 수 있다. 예를 들면 0.1≤x≤1.2일 수 있으며, 또는 x=1일 수 있다.
[0046] The above Si / C composite may be, for example, a composition in which carbon is coated on the surface of a particle by heat treatment (firing) while carbon is combined with silicon or silicon oxide particles, or a composition in which carbon is dispersed in an atomic state inside a silicon particle. Any composition in which carbon and silicon materials form a composite is possible without limitation.
[0047] In addition, SiO doped with the metal x (0 <x<2)는, Li, Mg, Al, Ca, 및 Ti로 이루어진 군에서 선택된 1종 이상의 금속이 도핑된 구성일 수 있다.
[0048] As above, SiO x When doped, SiO x Reducing the irreversible SiO2 phase of the material or converting it into an electrochemically inactive metal-silicate phase, SiOx It is more desirable to be able to increase the initial efficiency of the material.
[0049] The above Si alloy (Si-alloy) is an alloy of Si with one or more metals selected from the group consisting of Zn, Al, Mn, Ti, Fe, and Sn, and includes, but is not limited to, solid solutions, intermetallic compounds, and eutectic alloys with these.
[0050] The above negative electrode may further include other negative electrode active materials, such as graphite, in addition to the silicon (Si)-based negative electrode active material.
[0051] The silicon (Si)-based negative electrode active material described above is an anode active material that is being continuously researched and developed considering capacity, etc., but when applied as an anode active material in a lithium secondary battery, there is a problem that the compression deformation of the separator is further aggravated due to the increase in internal pressure of the cell during charge / discharge because the volume expansion of the anode is large. In addition, the Si-based negative electrode active material has a larger particle size, roughness, and hardness than the graphite negative electrode active material, which may cause local damage to the separator during lamination with the separator. Accordingly, a separator that can simultaneously secure compression resistance and heat resistance without deforming the pores of the separator is to be applied.
[0052] According to one embodiment of the present invention, the porous polymer substrate (110) of the separator may be manufactured from a known polymer that is known to be usable as a porous polymer substrate of a lithium secondary battery, such as polyolefin, polyethylene terephthalate, polybutylene terephthalate, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene oxide, polyphenylene sulfide, polyethylene naphthalene, etc., and in particular, may be manufactured using polyolefin as a base polymer. Examples of the polyolefin include polyethylene, polypropylene, polypentene, etc., and may include one or more of these.
[0053] Polymer substrates manufactured using these polyolefins, which are porous, for example, with numerous pores, are advantageous in terms of imparting shutdown capabilities at appropriate temperatures. In particular, the inclusion of both polyethylene and polypropylene as polyolefins can simultaneously improve shutdown characteristics and physical properties, such as mechanical strength.
[0054] According to one embodiment of the present invention, the thickness of the porous polymer substrate may be about 1 ㎛ to 100 ㎛. For example, the thickness of the porous polymer substrate may be about 10 ㎛ to 95 ㎛, 15 ㎛ to 90 ㎛, 20 ㎛ to 85 ㎛, 25 ㎛ to 80 ㎛, 30 ㎛ to 75 ㎛, 35 ㎛ to 70 ㎛, 40 ㎛ to 65 ㎛, 45 ㎛ to 60 ㎛, 50 ㎛ to 65 ㎛, or 55 ㎛ to 60 ㎛. For example, the thickness may be about 1 ㎛ to 30 ㎛, or about 5 ㎛ to 30 ㎛. By controlling the thickness of the porous polymer substrate within the above-described range, the volume of the electrochemical device can be minimized, and the positive and negative electrodes can be electrically insulated.
[0055] According to one embodiment of the present invention, the porous polyolefin polymer substrate most commonly used as the porous polymer substrate can be manufactured as follows, but is not limited thereto.
[0056] The porous polyolefin polymer substrate may be manufactured by a method (dry method) in which a polyolefin polymer is melt-extruded into a sheet shape, then stretched to induce microcracks between lamellae, which are crystal portions of the polymer, thereby forming micropores. In addition, the separator may be manufactured by a method (wet method) in which a polyolefin polymer is mixed with a plasticizer (diluent) at a high temperature to form a single phase, the polymer material and the plasticizer are phase-separated during the cooling process, the plasticizer is extracted to form pores, and then stretched and heat-set.
[0057] According to one embodiment of the present invention, the separator for an electrochemical device includes a coating layer (130) provided on at least one surface of the porous polymer substrate. For example, the separator for an electrochemical device includes a coating layer provided on one or both surfaces of the porous polymer substrate. As described above, by the separator for an electrochemical device including a coating layer provided on at least one surface of the porous polymer substrate, the heat resistance of the separator can be improved, mechanical properties can be improved, and the shrinkage of the separator at high temperatures can be prevented, thereby preventing an electrical short circuit of the electrode.
[0058] According to one embodiment of the present invention, the separator includes a first coating layer (131) including a first polymer resin. For example, the first coating layer may be positioned on the porous polymer substrate. Accordingly, when the first coating layer is coated on the porous polymer substrate, the first polymer resin may be positioned inside the pores in the porous polymer substrate to close the pores. Accordingly, even when a lamination process is performed by applying an anode including a Si-based anode active material having relatively high hardness, the deformation phenomenon in which the pores become smaller or are blocked due to the first polymer resin positioned inside the pores can be improved. As described above, the separator includes a first coating layer including a first polymer resin, so that even when a Si-based anode active material is applied, an electrochemical device separator with improved compression resistance and heat resistance can be implemented.
[0059] According to one embodiment of the present invention, the separator is provided on the first coating layer and includes a second coating layer (133) including a second polymer resin and inorganic particles. For example, the second coating layer may be located on the first coating layer located on the porous polymer substrate. When the first polymer resin included in the first coating layer is located in the pores within the porous polymer substrate and the first coating layer does not remain entirely or partially, the second coating layer may be located in contact with the porous polymer substrate. As described above, the separator is provided on the first coating layer and includes a second coating layer including a second polymer resin and inorganic particles, thereby improving the heat resistance of the separator, improving the mechanical properties, preventing the separator from shrinking at high temperatures and causing an electrical short circuit of the electrode, and forming pores within the coating layer.
[0060] According to one embodiment of the present invention, each of the first polymer resin and the second polymer resin may be in particle form. As described above, by utilizing each of the first polymer resin and the second polymer resin in particle form, pores can be formed in the coating layer.
[0061] According to one embodiment of the present invention, each of the first polymer resin and the second polymer resin may be soluble. The soluble polymer means one that is dissolved by a solvent and does not exhibit a particle form.
[0062] According to one embodiment of the present invention, the first coating layer may not contain inorganic particles.
[0063] According to one embodiment of the present invention, the second coating layer may include a plurality of pores. Here, the pores refer to pores within the coating layer, and the locations of occurrence are different from the pores within the porous polymer substrate. For example, the coating layer may be a porous coating layer. For example, the coating layer may be a porous coating layer including a plurality of pores within it. As described above, by including a plurality of pores, the coating layer can physically block the negative electrode and the positive electrode while allowing lithium ions to pass through and current to flow.
[0064] According to one embodiment of the present invention, the second coating layer may be formed by bonding inorganic particles to second polymer resin particles. The pores within the second coating layer may be derived from interstitial volume, which is an empty space between the inorganic particles.
[0065] According to one embodiment of the present invention, the inorganic particles included in the second coating layer are not particularly limited as long as they are electrochemically stable. That is, the inorganic particles that can be used in the present invention can be used within the operating voltage range of the applied electrochemical device (e.g., Li / Li).+ There is no particular limitation as long as no oxidation and / or reduction reaction occurs at 0 to 5 V as a standard. For example, when inorganic particles having ion transfer capability are used, the ion conductivity within the electrochemical device can be increased to improve performance. In addition, when inorganic particles having a high dielectric constant (hereinafter referred to as “high-k inorganic particles”) are used as inorganic particles, the ion conductivity of the electrolyte can be improved by contributing to an increase in the degree of dissociation of an electrolyte salt, such as a lithium salt, in a liquid electrolyte. The inorganic particles may include high-k inorganic particles having a dielectric constant of about 5 or more or 10 or more, inorganic particles having a lithium ion transfer capability, or a mixture thereof. For example, the inorganic particles may include BaSO4, BaTiO3, Pb(Zr, Ti)O3(PZT), Pb 1-x La x Zr 1-y TiyO3(PLZT, 0 <x<1, 0<y<1), Pb(Mg 1 / 3 Nb 2 / 3 )O3-PbTiO3(PMN-PT), hafnia (HfO2), SrTiO3, SnO2, CeO2, MgO, Mg(OH)2, NiO, CaO, ZnO, ZrO2, SiO2, Y2O3, Al2O3, SiC, Al(OH)3, TiO2, aluminum peroxide, zinc tin hydroxide (ZnSn(OH)6), tin-zinc oxide (Zn2SnO4, ZnSnO3), antimony trioxide (Sb2O3), antimony tetroxide (Sb2O4), antimony pentoxide (Sb2O5), boehmite (AlO(OH)) and combinations thereof, but this is only an example and is not limited thereto.
[0066] According to one embodiment of the present invention, the size of the inorganic particles is not limited, but may be about 40 nm to 3 ㎛ in order to form a coating layer of uniform thickness and an appropriate porosity. For example, it may be about 40 nm to 2.5 ㎛ in length, 40 nm to 2 ㎛ in length, 40 nm to 1.5 ㎛ in length, or 40 nm to 1.0 ㎛ in length. When the size of the inorganic particles satisfies the above range, dispersibility is maintained, making it easy to control the properties of the separator, and the phenomenon of the thickness of the coating layer increasing can be avoided, so that the mechanical properties can be improved, and in addition, the probability of an internal short circuit occurring during battery charging and discharging due to an excessively large pore size is low.
[0067] According to one embodiment of the present invention, the thickness of the coating layer may be formed to a thickness of about 1 ㎛ to 10 ㎛ on one side of the porous polymer substrate, for example, about 1 ㎛ to 9 ㎛, 2 ㎛ to 8 ㎛, 3 ㎛ to 7 ㎛, 3 ㎛ to 6 ㎛, or 3 ㎛ to 5 ㎛. According to one embodiment, the coating may be performed on both sides with a thickness of 4 ㎛ on one side of the porous polymer substrate.
[0068] According to one embodiment of the present invention, the thickness of the polymer substrate and / or the coating layer, etc., can be measured using a contact thickness measuring device. The contact thickness measuring device can be, for example, VL-50S-B from Mitutoyo.
[0069] According to one embodiment of the present invention, the solubility of the first polymer resin in the electrolyte is greater than the solubility of the second polymer resin in the electrolyte.
[0070] For example, the first polymer resin refers to a polymer resin that is dissolved by an electrolyte that is injected into a battery case having an electrode assembly and impregnates the electrode assembly, and is ultimately eluted by the electrolyte in a lithium secondary battery product. The polymer solution that is coated on the porous polymer substrate is prepared by dissolving the first polymer resin that has solubility in the electrolyte in a solvent. Any liquid that can dissolve the first polymer resin can be used as the solvent, but using a solvent that has affinity with the polymer component of the porous polymer substrate makes it easy to penetrate the pores of the porous polymer substrate.
[0071] In addition, the second polymer resin refers to a polymer resin that is not dissolved or is dissolved in a very small amount by the electrolyte that is injected into the battery case having the electrode assembly and impregnates the electrode assembly, and is ultimately not dissolved in large quantities by the electrolyte in a lithium secondary battery product. In other words, since the second polymer resin does not need to be dissolved in the electrolyte, it should be interpreted to mean a polymer resin that is swollen by the electrolyte but not dissolved.
[0072] As described above, by controlling the solubility of the first polymer resin in the electrolyte to be greater than the solubility of the second polymer resin in the electrolyte, even when applying a negative electrode including a silicon (Si)-based active material, deformation of pores in the porous polymer substrate can be prevented, thereby improving compression resistance and heat resistance.
[0073] According to one embodiment of the present invention, the solubility index of the first polymer resin is about 17 MPa 1 / 2 More than 27 MPa 1 / 2 It may be less than, for example, about 18 MPa 1 / 2 More than 26 MPa 1 / 2 Below, 19 MPa 1 / 2 More than 25 MPa 1 / 2 Below 20 MPa 1 / 2More than 24 MPa 1 / 2 or less than 21 MPa 1 / 2 More than 23 MPa 1 / 2 It may be as follows. By controlling the solubility index of the first polymer resin, the solubility of the electrolyte can be increased, thereby implementing a separator for an electrochemical device with improved compression resistance.
[0074] According to one embodiment of the present invention, the solubility index of the second polymer resin is 17 MPa 1 / 2 Less than or equal to 27 MPa 1 / 2 It may be excessive. By controlling the solubility index of the second polymer resin, since the difference in solubility index with the electrolyte is relatively large, the particle state can be maintained even under the electrolyte, and the heat resistance of the separator according to the second polymer resin and inorganic particles can be improved by preventing it from being dissolved in the electrolyte, the mechanical properties can be improved, the separator can be prevented from shrinking at relatively high temperatures and causing an electrical short circuit of the electrode, and pores can be formed inside the coating layer.
[0075] According to one embodiment of the present invention, the difference between the solubility index of the first polymer resin and the solubility index of the second polymer resin may be about 3 or more and 100 or less. For example, it may be about 5 or more and 100 or less, or about 7 or more and 100 or less.
[0076] According to one embodiment of the present invention, the electrolyte solubility index can be expressed as a Hansen solubility parameter (HSP). That is, each substance has a unique solubility parameter value, and substances with similar solubility parameter values dissolve or mix well with each other.
[0077] The above Hansen Solubility Parameter was proposed by Dr. C. Hansen, and considers the degree of bonding within a substance by dividing it into the following three factors.
[0078] (1) Solubility factor (δD) resulting from nonpolar dispersion bonding
[0079] (2) Solubility factor (δP) caused by polar bonding due to permanent dipoles
[0080] (3) Solubility factor (δH) caused by hydrogen bonding
[0081] In this way, HSP can accurately and systematically evaluate the solubility or miscibility of a substance.
[0082] HSP=(δD, δP, δH), (J / cm3) ½ (1)
[0083] δTot =(δD 2 +δP 2 +δH 2 ) ½ , (J / ㎤) ½ (2)
[0084] HSP is a vector with magnitude and direction in a space composed of three elements, and δTot represents the magnitude of the HSP vector. The basic unit representing HSP is (J / ㎤). ½ is. These HSP values can be calculated using a program called HSPiP (Hansen Solubility Parameters in Practice) developed by Dr. Hansen's group, who proposed HSP. As mentioned earlier, if the HSP values of two substances are similar, they dissolve well in each other. However, since HSP is a vector, in order to determine that they are similar, all three HSP components and the sizes of the HSPs of each substance must be similar. All substances have HSPs, and by using this, we can compare and analyze the differences in similarity to predict whether the substances of interest will dissolve in each other.
[0085] According to one embodiment of the present invention, the first polymer resin may include one selected from the group consisting of polystyrene, polyethyl acrylate, polymethyl acrylate, polystyrene sulfide, polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyvinyl acetate (PVAc), polyacrylonitrile (PAN), polylactic acid (PLA), polyacrylic acid (PAA), and combinations thereof. It may be polyacrylic acid (PAA). As described above, by selecting a first polymer resin from the group listed above, a first coating layer dissolved in an electrolyte is formed, and even when a negative electrode including a silicon (Si)-based active material is applied, pore deformation within a porous polymer substrate can be prevented, thereby improving compression resistance.
[0086] According to one embodiment of the present invention, the second polymer resin may include one selected from the group consisting of a PVDF-HFP copolymer (polyvinylidenefluoridehexafluoropropylene copolymer), a PVDF-CTFE copolymer (vinylidenefluoride-chlorotrifluoroethylene copolymer), a PVDF-HFPCTFE terpolymer (vinylidenefluoride-hexafluoropropylene-chlorotrifluoroethylene terpolymer), cyanoethyl polyvinyl alcohol, and combinations thereof. For example, it may be a PVDF-HFP copolymer and / or a PVDF-CTFE copolymer. By selecting the second polymer resin from the group listed above as described above, a second coating layer including the second polymer resin that is not dissolved in an electrolyte is formed, so that even when an anode including a silicon (Si)-based active material is applied, pore deformation in a porous polymer substrate can be prevented, thereby simultaneously improving compression resistance and heat resistance.
[0087] According to one embodiment of the present invention, since the commonly used acrylic polymer has a high relative affinity for the electrolyte, it swells a lot under the electrolyte even if it is crosslinked, so when the acrylic polymer is used alone, it can swell and dissolve under the electrolyte. On the other hand, in the case of the PVDF polymer, which has a large difference in solubility index from the electrolyte, it is advantageous to maintain a particle form even under the electrolyte, so even if it swells under the electrolyte, it does not dissolve, thereby improving the compression resistance and heat resistance according to the present invention.
[0088] According to one embodiment of the present invention, the separation membrane may have a plurality of pores, the polydispersity index (PDI) of the porous polymer substrate may be about 2.5 or more and 10 or less, and the average particle size of the pores of the porous polymer substrate may be 20 nm or more and 80 nm or less. The polydispersity index of the porous polymer substrate is low, and the average particle size of the pores of the porous polymer substrate is small. When these ranges are simultaneously satisfied, the compression resistance may be improved. For example, the polydispersity index (PDI) of the porous polymer substrate may be about 3.0 or more and 9.5 or less, 3.5 or more and 9.0 or less, 4.0 or more and 8.5 or less, 4.5 or more and 8.0 or less, 5.0 or more and 7.5 or less, 5.5 or more and 7.0 or less, or 6.0 or more and 6.5 or less. If the above polydispersity index is less than 2.5, there is a problem of reduced processability and lower uniformity of the film, and if it exceeds 10, there is a problem of reduced compressibility.
[0089] In addition, for example, the average particle size of the pores of the porous polymer substrate may be about 25 nm to 75 nm, 30 nm to 70 nm, 35 nm to 65 nm, 40 nm to 60 nm, or 45 nm to 55 nm. If the average particle size of the pores is less than 20 nm, the air permeability is reduced, and there is a problem that byproducts block the small pores during battery charging and discharging, and if it exceeds about 80 nm, the thickness of the separator is not uniform, thickness deformation occurs, and there is a problem that the compression resistance is reduced due to local thickness deformation.
[0090] According to one embodiment of the present invention, the average particle diameter of the pores of the porous polymer substrate can be calculated from the pore size distribution measured using the Capillary Flow Porometer method. For example, first, the membrane to be measured is wetted with a wetting agent such as a Galwick solution, and then the air pressure on one side of the substrate is gradually increased. When the applied air pressure becomes greater than the capillary attraction of the wetting agent present in the pores, the wetting agent blocking the pores is pushed out, and the pore size and distribution are measured through the pressure and flow rate at the moment of being pushed out, from which the average pore particle diameter can be confirmed.
[0091] According to one embodiment of the present invention, the content of the silicon (Si)-based active material in the negative electrode may be about 50 wt% or more. For example, it may be about 50 wt% or more and less than 100 wt%, 55 wt% or more and 95 wt% or less, 60 wt% or more and 90 wt% or less, 65 wt% or more and 85 wt% or less, 60 wt% or more and 80 wt% or less, or 65 wt% or more and 75 wt% or less. By controlling the content of the silicon (Si)-based active material in the negative electrode as described above, the energy density of the battery can be improved compared to when a graphite-based negative electrode active material is applied alone.
[0092] According to one embodiment of the present invention, the hardness of the negative electrode may be about 50 MPa or more and 350 MPa or less. For example, it may be about 75 MPa or more and 325 MPa or less, 100 MPa or more and 300 MPa or less, 125 MPa or more and 275 MPa or less, 150 MPa or more and 250 MPa or less, or 175 MPa or more and 225 MPa or less. If it is out of the above range, the pores of the separator are more likely to be deformed than when a graphite-based negative electrode active material is applied, which may reduce the energy density of the battery.
[0093] According to one embodiment of the present invention, the hardness is the indentation hardness (H) measured by a nanoindenter. IT ) may be.
[0094] The above indentation is an analysis technique for the mechanical properties of a material. It is an experimental method that compares and analyzes the indentation marks and the load during indentation after indenting a material with a diamond indenter of various shapes. This indentation test is not only a technique for measuring the fracture toughness or hardness of a material, but has also been studied in many different directions recently, and is also used as a research technique for elastic-plastic behavior of materials, analysis of residual stress states, adhesion tests of thin films, fracture characteristics, and phase transformation analysis. In particular, when performing indentation on a micro material such as an electrode as in the present invention, nanoindentation can be applied, which applies a load of units of N or less using an indenter.
[0095] The above hardness is obtained by continuously measuring the load and indentation depth from the indenter when the indenter is indented into the surface of the electrode active material layer during loading and unloading, and from the obtained load-indentation depth curve. For example, the above hardness is calculated by the formula (Pmax) / A from the maximum load (Pmax) and the contact projected area A of the indenter when the indenter is indented while applying the maximum load (Pmax).
[0096] The above hardness is an indicator that can represent the physical characteristics of the electrode active material layer. Higher hardness means that the degree of deformation of the electrode active material layer in response to external force is small. In other words, the higher the hardness, the more strongly the particles constituting the electrode active material layer are bonded to each other, indicating greater resistance to pressurization. Conversely, the lower the hardness, the weaker the particles constituting the electrode active material layer are bonded to each other, indicating less resistance to pressurization.
[0097] According to one embodiment of the present invention, the Si-based negative electrode active material has a higher hardness than the graphite negative electrode active material, and thus there is a problem that the pores of the separator are likely to be deformed during the electrode assembly process.
[0098] According to one embodiment of the present invention, the method for forming the coating layer is as follows, for example. First, a polymer solution is prepared by dissolving a binder resin in an appropriate organic solvent. For example, the solvent has a solubility index similar to that of the binder polymer to be used and a low boiling point. This is to facilitate uniform mixing and subsequent solvent removal. Non-limiting examples of usable solvents include acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), cyclohexane, water, or a mixture thereof. Next, inorganic particles are added and dispersed in the prepared polymer solution to prepare a porous polymer substrate (110). In the present invention, the content ratio of the inorganic particles and the binder is appropriately adjusted in consideration of the thickness, pore size, and porosity of the final coating layer of the present invention. Next, the first polymer material and the second polymer material for preparing the slurry for the first coating layer and the second coating layer are respectively selected. Thereafter, the solubility of the selected first polymer material in the electrolyte and the solubility of the second polymer material in the electrolyte are compared.
[0099] As a result of the comparison, if it is determined that the solubility of the first polymer material in the electrolyte is greater than the solubility of the second polymer material in the electrolyte, a slurry for a first coating layer is prepared by applying the selected first polymer material. Thereafter, the slurry for a first coating layer including the first polymer material is applied to at least one side of the prepared porous polymer substrate (110) and dried to form a first coating layer (131) on the porous polymer substrate (110). If, in step S140, it is determined that the solubility of the first polymer material in the electrolyte is less than the solubility of the second polymer material in the electrolyte, the process returns to the previous step and repeats the selection of the first polymer material and the second polymer material. Next, a slurry for a second coating layer is prepared by applying the selected second polymer material, and the prepared slurry for a second coating is applied on the first coating layer and dried to form a second coating layer.
[0100] The first coating layer and the second coating layer can be manufactured to be separated from each other in the same manner as described above. However, the first coating layer and the second coating layer may not be separated from each other, but may be coated simultaneously to form coating layers, for example. In addition, the order of the above-described manufacturing processes may be appropriately modified without being restricted by the described order. For example, the process of selecting the first polymer material and the second polymer material and comparing their solubility in the electrolyte may be performed even before the manufacture of the porous polymer solution, and the manufacture of the slurry for the first coating layer and the second coating layer using the first and second polymer materials may also be performed before the manufacture of the porous polymer solution. In addition, the slurry for the first coating layer and the slurry for the second coating layer may be manufactured independently at the same time or at different times without being restricted by the process order.
[0101] According to one embodiment of the present invention, the method for applying the slurry to the surface of the membrane substrate is not particularly limited to any of the methods described above. For example, various methods such as dip coating, die coating, roll coating, comma coating, or a combination thereof may be used.
[0102] According to one embodiment of the present invention, the drying process appropriately sets temperature and time conditions to minimize the occurrence of surface defects in the organic / inorganic composite coating layer. The drying may be performed using a drying auxiliary device such as a drying oven or a hot air blower within an appropriate range.
[0103] According to one embodiment of the present invention, the manufactured separator is interposed between a negative electrode and a positive electrode including a Si-based negative electrode active material and is manufactured into an electrode assembly through a lamination process in which heat and / or pressure are applied to bond them together. The lamination process can be performed by a roll press device including a pair of pressure rollers. That is, the negative electrode, the separator, and the positive electrode are sequentially laminated and placed between the pressure rollers to achieve interlayer bonding. At this time, the lamination process can be performed by a hot press method.
[0104] One embodiment of the present invention includes an electrochemical device including an anode, a cathode, and an electrolyte, and a separator interposed between the anode and the cathode.
[0105] An electrochemical device according to one embodiment of the present invention comprises a second coating layer comprising a second polymer resin and inorganic particles on a first coating layer comprising a first polymer resin, thereby preventing deformation of pores within a porous polymer substrate even when a negative electrode comprising a silicon (Si)-based active material is applied, thereby simultaneously improving compression resistance and heat resistance.
[0106] According to one embodiment of the present invention, the negative electrode comprises a negative electrode current collector and a negative electrode active material layer including a Si-based negative electrode active material on at least one surface of the current collector, a binder resin, and optionally a conductive material as needed. As the negative electrode active material, a silicon (Si)-based negative electrode active material may be used alone, or a carbon-based negative electrode active material such as graphite may be optionally used in combination. The silicon (Si)-based negative electrode active material may be the same as that described above.
[0107] According to one embodiment of the present invention, the content of the silicon (Si)-based negative electrode active material may be about 50 wt% or more. For example, it may be 50 wt% or more and less than 100 wt%, 55 wt% or more and 95 wt% or less, 60 wt% or more and 90 wt% or less, 65 wt% or more and 85 wt% or less, 60 wt% or more and 80 wt% or less, or 65 wt% or more and 75 wt% or less. By controlling the content of the silicon (Si)-based active material in the negative electrode as described above, the energy density of the battery can be improved compared to when a graphite-based negative electrode active material is applied alone.
[0108] According to one embodiment of the present invention, a positive electrode has a positive electrode current collector and a positive electrode active material layer including a positive electrode active material, a conductive material, and a binder resin on at least one surface of the positive electrode current collector. The positive electrode active material is a layered compound such as lithium manganese oxide (LiMn2O4, LiMnO2, etc.), lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, LiV3O4, V2O5, Cu2V2O7; chemical formula LiNi 1-x M xNi-site type lithium nickel oxide represented by O2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga and x = 0.01 to 0.3); chemical formula LiMn 1-x M x Lithium manganese composite oxide represented by O2 (wherein, M = Co, Ni, Fe, Cr, Zn or Ta, and x = 0.01 to 0.1) or Li2Mn3MO8 (wherein, M = Fe, Co, Ni, Cu or Zn); LiMn2O4 in which a part of the Li in the chemical formula is replaced by an alkaline earth metal ion; disulfide compound; Fe2(MoO4)3, or a mixture of two or more thereof. For example, LiNi 0.8 Mn 0.1 Co 0.1 It could be O2.
[0109] According to one embodiment of the present invention, the conductive material may be, for example, one selected from the group consisting of graphite, carbon black, carbon fibers or metal fibers, metal powders, conductive whiskers, conductive metal oxides, activated carbon, and polyphenylene derivatives, or a mixture of two or more conductive materials thereof. Further, for example, the conductive material may be one selected from the group consisting of natural graphite, artificial graphite, super-p, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, Denka black, aluminum powder, nickel powder, zinc oxide, potassium titanate, and titanium oxide, or a mixture of two or more conductive materials thereof.
[0110] According to one embodiment of the present invention, a polymer resin commonly used in electrodes in the art can be used as the binder resin.Non-limiting examples of such binder resins include polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polymethylmethacrylate, polyethylhexyl acrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, and cellulose acetate propionate. Examples thereof include, but are not limited to, cellulose acetatepropionate, cyanoethylpullulan, cyanoethylpolyvinylalcohol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxyl methyl cellulose (CMC), polyvinyl alcohol (PVA), polyacrylic acid (PAA), polyethylene glycol (PEG), polyacrylonitrile (PAN), and polyacryl amide (PAM).
[0111] The electrode assembly prepared as above can be placed in an appropriate case and an electrolyte can be injected to manufacture a battery.
[0112] According to one embodiment of the present invention, the solubility index of the electrolyte is about 17 MPa 1 / 2 More than 27 MPa 1 / 2 It may be less than, for example, about 18 MPa 1 / 2 More than 26 MPa 1 / 2 Below, 19 MPa 1 / 2 More than 25 MPa 1 / 2 Below 20 MPa 1 / 2 More than 24 MPa 1 / 2 or less than 21 MPa 1 / 2 More than 23 MPa 1 / 2 It may be as follows. When the range of the solubility index of the electrolyte is satisfied, even when a negative electrode including a silicon (Si)-based active material is applied by impregnating and then dissolving a first polymer resin having a solubility index similar to the solubility index, the compression resistance and heat resistance can be improved at the same time by preventing deformation of the pores in the porous polymer substrate. That is, the smaller the difference between the solubility index of the electrolyte and the solubility index of the first polymer resin, the better the solubility can be. Therefore, the solubility index of the electrolyte can be similar to or identical to the solubility index of the first polymer resin.
[0113] According to one embodiment of the present invention, the electrolyte is A + B - As a salt with the same structure, A + is Li + , Na + , K + Contains ions composed of alkali metal cations or combinations thereof, such as B - is PF6 - , BF4 - , Cl - , Br - , I - , ClO4 -, AsF6 - , CH3CO2 - , CF3SO3 - , NCF3SO2)2 - , CCF2SO2)3 - A salt containing an anion such as PC, ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma butyrolactone (γ-butyrolactone) or a mixture thereof is dissolved or dissociated in an organic solvent, but, for example, according to one embodiment of the present invention, the electrolyte may include one selected from the group consisting of propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC) and a combination thereof.
[0114] According to one embodiment of the present invention, the electrolyte may be a mixture of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC).
[0115] According to one embodiment of the present invention, the electrolyte may have a content ratio of propylene carbonate (PC) and dimethyl carbonate (DMC) of about 10:90 to 99:1. For example, the content ratio may be about 20:80 to 98:2, 30:70 to 97:3, 40:60 to 96:4, 50:50 to 95:5, 60:40 to 94:6, 70:30 to 93:7, 80:20 to 92:8, or about 90:10.
[0116] According to one embodiment of the present invention, a battery module including a battery including the electrode assembly as a unit cell, a battery pack including the battery module, and a device including the battery pack as a power source are provided. Specific examples of the device include, but are not limited to, a power tool that is powered by an electric motor; an electric vehicle including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), etc.; an electric two-wheeled vehicle including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; and a power storage system.
[0117] Hereinafter, the present invention will be described in detail using examples. However, the examples according to the present invention may be modified in various ways, and the scope of the present invention is not limited to the examples described below. The examples in this specification are provided to more fully explain the present invention to those of ordinary skill in the art.
[0118]
[0119] <Example>
[0120] As a porous polymer substrate, SV9 (thickness 9 μm, porosity 46%, basis weight 4.9 g / m) of Shanghai Energy Co., Ltd. 2 , Gurley value 70sec / 100cc) membrane fabric was used.
[0121] Meanwhile, poly acrylic acid (PAA, Dow, CK-702) was used as the first polymer resin having electrolyte solubility, and the first polymer resin was completely dissolved in water as a solvent at a concentration of 10 wt% to prepare a polymer solution. The solubility index of the first polymer resin in the electrolyte was 22.4 MPa. 1 / 2 am.
[0122] The prepared polymer solution was dip-coated on a porous polyethylene polymer substrate fabric and dried at 65°C to form a polymer coating layer.
[0123] Next, PVDF-HFP (Solvay, solef 21510, HFP 15 wt%) and PVDF-CTFE (Solvay, solef 32008) as the second polymer resin are dissolved in the solvent acetone. Then, a slurry containing Cyano resin (Miwon Commercial, CYR-301) as a dispersant dissolved in the solvent acetone is prepared. The solubility indices of the second polymer resins 21510 and 32008 are 13.5 MPa, respectively. 1 / 2 , 15.1 MPa 1 / 2 am.
[0124] Al2O3 with an average particle diameter of approximately 500 nm and Boehmite with an average particle diameter of 300 nm were prepared as inorganic particles. The weight ratio of the final slurry was Al2O3: Boehmite: 21510: 32008: CYR-301 = 66.3: 11.7: 15.5: 4.5: 2.0, and these components were added to the solvent acetone at a weight ratio of 15% and uniformly mixed to prepare a slurry.
[0125] The prepared slurry was coated on both sides to a thickness of 8 μm on the aforementioned polymer coating layer and dried at 45°C to form an outer coating layer.
[0126]
[0127] Manufacturing of anodes
[0128] Cathode active material (LiNi) 0.8 Mn 0.1 Co 0.1 O2), a conductive agent (carbon black), a dispersant, and a binder resin (a mixture of PVDF-HFP and PVDF) were mixed with water in a weight ratio of 97.5:0.7:0.14:1.66 to prepare a slurry for a positive electrode active material layer with a concentration of 50 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of an aluminum thin film (thickness 10 μm) and dried to manufacture a positive electrode having a positive electrode active material layer (thickness 120 μm).
[0129]
[0130] Manufacturing of cathode
[0131] Silicon particles (Elkem, M702), PAM binder (Arakawa, BUH0452), conductive agent (Imerys, SFG-6L), conductive agent (SWCNT, Ocsial, Tuball dispersion), and CMC dispersant (SWCNT, Ocsial, Tuball dispersion) were mixed with water in a weight ratio of 80:9.4:9.6:0.4:0.6 to prepare a slurry for the negative active material layer with a concentration of 25 wt% of the remaining components excluding water. Next, the slurry was applied to the surface of a copper thin film (8 ㎛ thick) and dried to obtain a negative electrode loading of 8 mAh / cm. 2 A cathode having a hardness of 80 MPa was manufactured.
[0132]
[0133] lamination process
[0134] The separators of the examples and comparative examples were interposed between the manufactured cathodes and anodes, and a lamination process was performed to obtain an electrode assembly. The lamination process was performed using a hot press at 70°C and 5.2 MPa for 10 seconds.
[0135]
[0136] Electrolyte injection process
[0137] The electrode assembly obtained in the above lamination process was inserted into a pouch outer material, and an electrolyte containing 0.5 M LiPF and 1.0 M LiFSI dissolved in a solvent mixed with an electrolyte composition of DEC / FEC = 90 / 10 (vol.%) was injected to manufacture a lithium secondary battery.
[0138]
[0139] <Comparative Example 1>
[0140] It was manufactured in the same manner as in the example, except that the solution of the first polymer resin was not coated on the membrane fabric.
[0141]
[0142] <Comparative Example 2>
[0143] The membrane fabric is not coated with a solution of the first polymer resin. And the solubility in the electrolyte is 17 MPa with the second polymer resin. 1 / 2 A slurry of PVDF (Solvay, KF9700) dissolved in acetone is prepared. The solubility index of PVDF, the second polymer resin, is 19.2 MPa. 1 / 2 And prepare a slurry by dissolving Cyano resin (Miwon Corporation, CYR-301) as a dispersant in acetone as a solvent.
[0144] Al2O3 with an average particle diameter of approximately 500 nm and Boehmite with an average particle diameter of 300 nm were prepared as inorganic particles. The weight ratio of the final slurry was Al2O3: Boehmite: PVDF: CYR-301 = 66.3:11.7:20:2.0, and these components were added to the solvent acetone at a weight ratio of 15% and uniformly mixed to prepare a slurry.
[0145] The prepared slurry was coated on both sides to a thickness of 8 μm and dried at 45°C to form an outer coating layer.
[0146]
[0147] <Comparative Example 3>
[0148] As a porous polymer substrate, SV9 (thickness 9 μm, porosity 46%, basis weight 4.9 g / m) of Shanghai Energy Co., Ltd. 2 , Gurley value 70sec / 100cc) membrane fabric was used.
[0149] Meanwhile, poly acrylic acid (PAA, Dow, CK-702) was used as the first polymer resin having electrolyte solubility, and the first polymer resin was completely dissolved in water as a solvent at a concentration of 10 wt% to prepare a polymer solution. The solubility index of the first polymer resin in the electrolyte was 22.4 MPa. 1 / 2 am.
[0150] The second polymer resin has a solubility in the electrolyte of 17 MPa. 1 / 2 A slurry of PVDF (Solvay, KF9700) dissolved in acetone is prepared. The solubility index of PVDF, the second polymer resin, is 19.2 MPa. 1 / 2 And prepare a slurry by dissolving Cyano resin (Miwon Corporation, CYR-301) as a dispersant in acetone as a solvent.
[0151] Al2O3 with an average particle diameter of approximately 500 nm and Boehmite with an average particle diameter of 300 nm were prepared as inorganic particles. The weight ratio of the final slurry was Al2O3: Boehmite: PVDF: CYR-301 = 66.3:11.7:20:2.0, and these components were added to the solvent acetone at a weight ratio of 15% and uniformly mixed to prepare a slurry.
[0152] The prepared slurry was coated on both sides to a thickness of 8 μm on the aforementioned polymer coating layer and dried at 45°C to form an outer coating layer.
[0153]
[0154] <Comparative Example 4>
[0155] Polyacrylamide (PAM, Songgangsa, MP15) was used as the first polymer resin that does not have electrolyte solubility, and the first polymer resin was completely dissolved in water as a solvent at a concentration of 10 wt% to prepare a polymer solution. The solubility index of the first polymer resin in the electrolyte was 13.5 MPa. 1 / 2 And the first polymer resin is coated on the same porous polymer substrate as in the example.
[0156] Next, PVDF-HFP (Solvay, solef 21510, HFP 15 wt%) and PVDF-CTFE (Solvay, solef 32008) as the second polymer resin are dissolved in the solvent acetone. Then, a slurry containing Cyano resin (Miwon Commercial, CYR-301) as a dispersant dissolved in the solvent acetone is prepared. The solubility indices of the second polymer resins 21510 and 32008 are 13.5 MPa, respectively. 1 / 2 , 15.1 MPa 1 / 2 am.
[0157] Al2O3 with an average particle diameter of approximately 500 nm and Boehmite with an average particle diameter of 300 nm were prepared as inorganic particles. The weight ratio of the final slurry was Al2O3: Boehmite: 21510: 32008: CYR-301 = 66.3: 11.7: 15.5: 4.5: 2.0, and these components were added to the solvent acetone at a weight ratio of 15% and uniformly mixed to prepare a slurry.
[0158] The prepared slurry was coated on both sides to a thickness of 8 μm on the aforementioned polymer coating layer and dried at 45°C to form an outer coating layer.
[0159]
[0160] Comparative Example 5
[0161] Polyacrylamide (PAM, Songgangsa, MP15) was used as the first polymer resin that does not have electrolyte solubility, and the first polymer resin was completely dissolved in water as a solvent at a concentration of 10 wt% to prepare a polymer solution. The solubility index of the first polymer resin in the electrolyte was 13.5 MPa. 1 / 2 And the first polymer resin is coated on the same porous polymer substrate as in the example.
[0162] The second polymer resin has a solubility in the electrolyte of 17 MPa. 1 / 2 A slurry of PVDF (Solvay, KF9700) dissolved in acetone is prepared. The solubility index of PVDF, the second polymer resin, is 19.2 MPa. 1 / 2 And prepare a slurry by dissolving Cyano resin (Miwon Corporation, CYR-301) as a dispersant in acetone as a solvent.
[0163] Al2O3 with an average particle diameter of approximately 500 nm and Boehmite with an average particle diameter of 300 nm were prepared as inorganic particles. The weight ratio of the final slurry was Al2O3: Boehmite: PVDF: CYR-301 = 66.3:11.7:20:2.0, and these components were added to the solvent acetone at a weight ratio of 15% and uniformly mixed to prepare a slurry.
[0164] The prepared slurry was coated on both sides to a thickness of 8 μm on the aforementioned polymer coating layer and dried at 45°C to form an outer coating layer.
[0165]
[0166] <Experimental Example>
[0167] [PDI Measurement]
[0168] PDI = (weight average molecular weight) / (number average molecular weight)
[0169] At this time, the weight average molecular weight and number average molecular weight values were derived by cutting the membrane into a certain size and performing GPC (Gel Permeation Chromatography) analysis.
[0170]
[0171] [Measurement of average pore size]
[0172] The particle size was measured according to the pore size distribution using a capillary flow porometer (CFP method).
[0173]
[0174] [Thickness reduction ratio after hot-pressing]
[0175] The membranes of the examples and comparative examples manufactured above were pressurized using a hot press to change their thickness, and then the thickness was measured. The thickness reduction rate was calculated using the following formula. The pressurization was performed under the conditions of 70°C, 5.2 MPa, and 10 sec. The thickness was measured using a thickness gauge (Mitutoyo, VL-50S).
[0176] Thickness reduction ratio = {(Separator thickness before hot pressing - Separator thickness after hot pressing) / Separator thickness before hot pressing} * 100
[0177]
[0178] [Wet heat shrinkage measurement experiment]
[0179] The membrane was cut to 5 X 5 cm, prepared, and 1 g of PC solution was poured into a pouch and sealed to prepare a sample. After leaving the sample at a temperature of 135°C for 30 minutes, the shrinkage rate of the membrane was measured.
[0180] The above shrinkage rate is the result of marking two arbitrary points in the MD and TD directions of the membrane, respectively, and calculating the increase / decrease rate of the distance between them (the point distance) according to the following (Formula 1).
[0181] (Formula 1) Shrinkage rate (%) = {(BA) / A} X 100
[0182] In the above equation, A is the gauge distance in the initial state before being stored at high temperature, and B is the gauge distance in the final state after being stored at high temperature.
[0183]
[0184] [Capacity retention measured after 500 cycles at 25℃, 1C / 1C]
[0185] For the battery manufactured by the above-described method, charging and discharging were repeated in the range of 2.5 V to 4.25 V at a rate of 1 C each at 25°C, and the ratio of discharge capacity after 500 cycles was derived by calculation.
[0186]
[0187] Example Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 First polymer resin solubility index (MPa 1 / 2 )22.4--22.413.513.5Second polymer resin solubility index (MPa 1 / 2)13.5, 15.113.5, 15.119.219.213.5, 15.119.2Total thickness (before press, μm)17.016.917.116.816.917.0Thickness (after press, μm)14.213.513.813.913.614.0Thickness reduction ratio after hot press (%)162019172018Wet heat shrinkage (@130℃ 30min, MD / TD)6 / 414 / 1114 / 138 / 69 / 78 / 625℃1C / 1C, Capacity retention after 500 cycles (%)928284908688
[0188]
[0189] In the table above, it was confirmed that wet heat shrinkage was reduced in Comparative Examples 1 and 2 compared to the examples because the first polymer resin was not coated on the fabric.
[0190] In the case of Comparative Example 2 compared to Comparative Example 1, it was confirmed that there was a slight improvement in the cell capacity retention rate because the solubility index of the coating layer was relatively similar to that of the electrolyte.
[0191] Comparative Example 3 is a separator in which the difference in solubility between the first polymer resin and the second polymer resin is reduced compared to the example, and due to the characteristic of being excessively dissolved in the electrolyte compared to the example, the ionic conductivity of the electrolyte is inferior, and thus the long-term cell capacity retention rate tends to be inferior.
[0192] In the case of Comparative Example 4, both the first polymer resin and the second polymer resin are separators coated with polymers that do not dissolve in the electrolyte, and it was confirmed that the cell capacity retention rate was the worst compared to the example and Comparative Examples 3 and 5.
[0193] In Comparative Example 5, the first polymer resin coated on the substrate is a separator that does not dissolve in the electrolyte, while the second polymer resin applied to the coating layer is relatively soluble in the electrolyte. However, the reason the cell capacity retention rate is inferior compared to the example is that the solubility index of the second polymer resin applied to the coating layer is lower than the solubility index of the first polymer resin coated on the fabric of the example, resulting in inferior solubility in the electrolyte.
[0194] While the present invention has been described above with reference to preferred embodiments, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes can be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
[0195]
[0196] [Explanation of symbols]
[0197] 100: Membrane
[0198] 110: Porous polymer substrate
[0199] 130: Coating layer
[0200] 131: First coating layer
[0201] 133: Second coating layer
[0202] 200: Cathode
Claims
1. In a separator for an electrochemical device equipped on a cathode containing a silicon (Si)-based active material, The above separation membrane comprises a porous polymer substrate; a first coating layer provided on at least one surface of the porous polymer substrate and including a first polymer resin; and a second coating layer provided on the first coating layer and including a second polymer resin and inorganic particles. A separator for an electrochemical device, wherein the solubility of the first polymer resin in the electrolyte is greater than the solubility of the second polymer resin in the electrolyte.
2. In claim 1, The solubility index of the above first polymer resin is 17 MPa 1 / 2 More than 27 MPa 1 / 2 Lee Ha-in, separator for electrochemical devices.
3. In claim 1, The solubility index of the above second polymer resin is 17 MPa 1 / 2 Less than or equal to 27 MPa 1 / 2 Excessive, separator for electrochemical devices.
4. In claim 1, A separator for an electrochemical device, wherein the first polymer resin comprises one selected from the group consisting of polystyrene, polyethyl acrylate, polymethyl acrylate, polystyrene sulfide, polyethylene terephthalate, polyvinyl chloride (PVC), polyvinyl pyrrolidone (PVP), polyvinyl acetate (PVAc), polyacrylonitrile (PAN), polylactic acid (PLA), polyacrylic acid (PAA), and combinations thereof.
5. In claim 1, A separator for an electrochemical device, wherein the second polymer resin comprises one selected from the group consisting of PVDF-HFP copolymer, PVDF-CTFE copolymer, PVDF-HFP-CTFE terpolymer, cyanoethyl polyvinyl alcohol, and combinations thereof.
6. In claim 1, The above membrane has a number of pores, The polydispersity index (PDI) of the above porous polymer substrate is 2.5 or more and 10 or less, A separator for an electrochemical device, wherein the average pore diameter of the porous polymer substrate is 20 nm or more and 80 nm or less.
7. In claim 1, A separator for an electrochemical device, wherein the content of silicon (Si)-based active material in the above cathode is 50 wt% or more.
8. In claim 1, A separator for an electrochemical device, wherein the hardness of the cathode is 50 MPa or more and 350 MPa or less.
9. An electrochemical device comprising a positive electrode, a negative electrode, and an electrolyte, and a separator according to claim 1 interposed between the positive electrode and the negative electrode.
10. In claim 9, The solubility index of the above electrolyte is 17 MPa 1 / 2 More than 27 MPa 1 / 2 Lee Ha-in, electrochemical device.
11. In claim 9, An electrochemical device, wherein the electrolyte comprises one selected from the group consisting of propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), fluoroethylene carbonate (FEC), and combinations thereof.
12. In claim 11, An electrochemical device in which the above electrolyte is a mixture of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC).
13. In claim 12, An electrochemical device wherein the electrolyte has a content ratio of diethyl carbonate (DEC) and fluoroethylene carbonate (FEC) of 10:90 to 99:1.
Citation Information
Patent Citations
A sperator for an electrochemical device and an electrochemical device comprising the same
KR1020240160967A
Separator for secondary battery comprising dual porous coating layers of inorganic particles with different average particle diameter, secondary battery comprising the same, and method for preparing the separator
KR101745631B1
Method of steering a mobile device from a public mobile network to a private mobile network
KR1020220128312A
A separator for an electrochemical device and a method for preparing the same
KR102366306B1
UWB antenna
KR102431800B1