Electrolyte for lithium secondary battery, secondary battery and electrical apparatus

By using specific additives and carboxylic acid ester solvents in the lithium secondary battery electrolyte, the problem of insufficient fast charging and cycling performance of lithium secondary battery is solved, and the overall performance and service life of the battery are significantly improved.

WO2024229998A1PCT designated stage expired Publication Date: 2024-11-14CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 16 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/111989
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2023-08-09
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Existing lithium secondary batteries have shortcomings in fast charging and circulation performance, especially carboxylate solvents are prone to cause negative electrode interface contact, produce gas, and affect the storage performance and service life of the battery.

Method used

Introduce specific contents and types of monofluorophosphate, fluorosulfonate and carbonate solvents into the electrolyte of lithium secondary batteries to form an organic/inorganic composite SEI film to prevent the contact between the carboxylic acid ester solvent and the negative electrode interface , reduce gas production.

Benefits of technology

It significantly improves the fast charging performance, circulation performance and storage performance of lithium secondary batteries, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023111989_14112024_PF_FP_ABST
    Figure CN2023111989_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to an electrolyte for a lithium secondary battery, a secondary battery and an electrical apparatus. The electrolyte for a lithium secondary battery comprises an organic solvent and, dissolved in the organic solvent, a first additive, a second additive and an electrolyte salt. The organic solvent comprises a carboxylic ester solvent, the mass percentage W1 of the carboxylic ester solvent in the organic solvent being 20% -80%; the first additive comprises one or more of monofluorophosphate, difluorophosphate, tetrafluoroborate, fluorosulfonate, oxalic acid borate, malonic acid borate, oxalic acid phosphate and malonic acid phosphate; the second additive comprises one or more of vinylene carbonate and a derivative thereof, and ethylene carbonate and a derivative thereof, the mass percentages of the first additive and the second additive in the electrolyte being W2 and W3 respectively, and 0.035≤(W2+W3) / W1≤0.15. The electrolyte of the present application enables secondary batteries to have relatively good fast-charging performance, cycle performance and storage performance.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte for lithium secondary battery, secondary battery and electrical device

[0001] Cross-references

[0002] This application claims priority to the Chinese patent application filed with the China Patent Office on May 8, 2023, with application number 2023105059142 and invention name “Electrolyte, Secondary Battery and Electrical Device for Lithium Secondary Batteries”, the entire contents of which are incorporated by reference into this application. Technical Field

[0003] The present application relates to the technical field of secondary batteries, and in particular to an electrolyte for a lithium secondary battery, a secondary battery, and an electrical device. Background Art

[0004] The statements herein merely provide background information related to the present application and do not necessarily constitute prior art.

[0005] In recent years, with the development of secondary battery technology, secondary batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power supplies for electronic equipment, power tools, electric bicycles, electric motorcycles, electric vehicles and other fields.

[0006] With the advancement of science and technology and society, the performance of various products has been further improved, thus placing higher demands on the fast charging performance, cycle performance, and storage performance of secondary batteries. How to provide a secondary battery with better fast charging performance, cycle performance, and storage performance is one of the key areas of focus for those skilled in the art.

[0007] Summary of the Invention

[0008] The present application is made in view of the above-mentioned problems, and one of its purposes is to provide an electrolyte for lithium secondary batteries, so that the secondary batteries using the electrolyte of the present application have better fast charging performance, cycle performance and storage performance.

[0009] In order to achieve the above-mentioned object, the first aspect of the present application provides an electrolyte for a lithium secondary battery, comprising an organic solvent and a first additive, a second additive and an electrolyte salt dissolved in the organic solvent;

[0010] The organic solvent includes a carboxylate solvent, and based on the total mass of the organic solvent, the mass percentage W1 of the carboxylate solvent is 20% to 80%;

[0011] The first additive comprises one or more of monofluorophosphate, difluorophosphate, tetrafluoroborate, fluorosulfonate, oxalatoborate, malonic acid borate, oxalatophosphate and malonic acid phosphate;

[0012] The second additive includes one or more compounds represented by the following formula I and formula II;

[0013] In formula I, R1 and R2 are each independently selected from a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 alkoxy group, a C2-C6 alkenyl group or a C2-C6 alkynyl group;

[0014] In formula II, R3, R4, R5 and R6 are each independently selected from a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 alkoxy group, a C2-C6 alkenyl group or a C2-C6 alkynyl group, and R3, R4, R5 and R6 do not represent a hydrogen atom at the same time;

[0015] The mass fractions of the first additive and the second additive in the electrolyte are W2 and W3 respectively, and 0.035≤(W2+W3) / W1≤0.15.

[0016] The present application adopts a specific content of carboxylic acid ester solvent in the organic solvent of the electrolyte, and introduces a first additive and a second additive of specific content and type. By combining the above components at specific contents, the secondary battery can have better fast charging performance, cycle performance and storage performance, and significantly improve the overall performance of the secondary battery.

[0017] In any embodiment, in Formula I, R1 and R2 are each independently selected from a hydrogen atom, a halogen atom, a C1-C4 alkyl group, a C1-C4 haloalkyl group, a C1-C4 alkoxy group, a C2-C4 alkenyl group or a C2-C4 alkynyl group.

[0018] In any embodiment, in Formula II, R3, R4, R5 and R6 are each independently selected from a hydrogen atom, a halogen atom, a C1-C4 alkyl group, a C1-C4 haloalkyl group, a C1-C4 alkoxy group, a C2-C4 alkenyl group or a C2-C4 alkynyl group.

[0019] In any embodiment, based on the total mass of the organic solvent, the mass percentage W1 of the carboxylate solvent is 30% to 70%. In this way, the fast charging performance of the secondary battery can be further improved while the secondary battery still has good cycle performance and storage performance.

[0020] In any embodiment, based on the total mass of the organic solvent, the mass percentage W1 of the carboxylate solvent is 40% to 60%, thereby further improving the overall performance of the secondary battery.

[0021] In any embodiment, 0.04≤(W2+W3) / W1≤0.10. In this way, the fast charging performance of the secondary battery can be further improved while still ensuring that the secondary battery has good cycle performance and storage performance.

[0022] In any embodiment, 0.05≤(W2+W3) / W1≤0.075. In this way, the overall performance of the secondary battery can be further improved.

[0023] In any embodiment, based on the total mass of the electrolyte, the mass percentage W2 of the first additive is 0.01% to 10%. In this way, the cycle performance and storage performance of the secondary battery can be further improved, and the secondary battery can have good fast charging performance.

[0024] In any embodiment, based on the total mass of the electrolyte, the mass percentage W2 of the first additive is 0.05% to 5%, thereby further improving the overall performance of the secondary battery.

[0025] In any embodiment, based on the total mass of the electrolyte, the mass percentage W3 of the second additive is 0.05% to 10%. In this way, the secondary battery has better cycle performance and storage performance while maintaining good fast charging performance, and the overall performance is better.

[0026] In any embodiment, based on the total mass of the electrolyte, the mass percentage W3 of the second additive is 0.1% to 5%, thereby further improving the overall performance of the secondary battery.

[0027] In any embodiment, the carboxylate solvent includes a compound represented by formula III;

[0028] Wherein, R7 and R8 are independently selected from any one of a C1-C3 alkyl group and a C1-C3 halogenated alkyl group. In this way, the viscosity of the electrolyte can be maintained within an appropriate range, the electrolyte has a higher conductivity, and the secondary battery has better fast charging performance.

[0029] In any embodiment, the carboxylate solvent includes one or more of the following compounds:

[0030] In any embodiment, the second additive includes one or more of vinylene carbonate, 4,5-diethylvinylene carbonate, fluoroethylene carbonate, and vinylethylene carbonate.

[0031] In any embodiment, the monofluorophosphate comprises lithium monofluorophosphate; the difluorophosphate comprises lithium difluorophosphate; and the tetrafluoroborate comprises lithium tetrafluoroborate.

[0032] In any embodiment, the oxalate borate comprises a compound represented by Formula IV;

[0033] Wherein, M1 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X1 is a halogen; m1 is an integer from 1 to 3; n1 is an integer from 0 to 4; and a1, b1, and c1 are all positive integers. Thus, during the secondary battery charging process, the oxalate borate can effectively form an organic / inorganic composite SEI film on the surface of the negative electrode together with the second additive, effectively preventing the carboxylate solvent from contacting the negative electrode interface, thereby reducing gas generation and improving the battery's cycling and storage performance.

[0034] In any embodiment, the malonate borate comprises a compound represented by formula V;

[0035] Wherein, M2 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X2 is a halogen; m2 is an integer from 1 to 3; n2 is an integer from 0 to 4; and a2, b2, and c2 are all positive integers. Thus, during the secondary battery charging process, the malonate borate can, together with the second additive, form an organic / inorganic composite SEI film on the surface of the negative electrode, alleviating gassing caused by contact between the carboxylate solvent and the negative electrode, thereby improving the battery's cycling and storage performance.

[0036] In any embodiment, the oxalophosphate comprises a compound represented by Formula VI;

[0037] Wherein, M3 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X3 is a halogen; m3 is an integer from 1 to 3; n3 is an integer from 0 to 4; and a3, b3, and c3 are all positive integers. Thus, the oxalophosphate and the second additive can form an organic / inorganic composite SEI film on the negative electrode surface, preventing the carboxylate solvent from contacting the negative electrode and improving the battery's cycling and storage performance.

[0038] In any embodiment, the malonate phosphate comprises a compound represented by Formula VII;

[0039] Wherein, M4 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X4 is a halogen; m4 is an integer from 1 to 3; n4 is an integer from 0 to 4; and a4, b4, and c4 are all positive integers. Thus, the malonic acid phosphate can form an organic / inorganic composite SEI film with the second additive on the negative electrode surface, preventing carboxylate solvents from contacting the negative electrode interface and improving the battery's cycling and storage performance.

[0040] In any embodiment, the fluorosulfonate comprises a compound represented by formula VIII; (FSO3) y M y+ Formula VIII

[0041] Where y is a positive integer; M y+ is a metal ion or an organic cation; metal ions include Li + 、Na + , K + , Rb + 、Cs + Mg 2+ , Ca 2+ 、Ba 2+ 、Al 3+ 、Fe 2+ 、Cu 2+ 、Fe 3+ 、Ni 2+ and Ni 3+ Thus, the fluorosulfonate can form an organic / inorganic composite SEI film with the second additive on the negative electrode surface, preventing the carboxylate solvent from contacting the negative electrode interface, thereby improving the cycle performance and storage performance of the battery.

[0042] In any embodiment, the organic solvent further comprises one or more of a linear carbonate and a cyclic carbonate.

[0043] In any embodiment, the linear carbonate includes one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate and ethyl propyl carbonate.

[0044] In any embodiment, the cyclic carbonate includes one or more of ethylene carbonate, propylene carbonate, and butylene carbonate.

[0045] In any embodiment, the electrolyte salt includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorobisoxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0046] The second aspect of the present application provides a secondary battery comprising the electrolyte for a lithium secondary battery according to the first aspect of the present application. Thus, the secondary battery has not only good fast charging performance, but also good cycle performance and storage performance, and has good overall performance.

[0047] In any embodiment, the secondary battery further comprises a negative electrode plate, wherein the negative electrode plate contains a negative electrode active material, and the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material is 10 -13 cm 2 / S~10 -10 cm 2 / S. In this way, the fast charging capability of the secondary battery can be further improved.

[0048] In any embodiment, the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material is 10 -12 cm 2 / S~10 -11 cm 2 / S. In this way, the fast charging capability of the secondary battery can be further improved.

[0049] In any embodiment, the volume average particle size Dv50 of the negative electrode active material is ≥6 μm, thereby further improving the cycle performance and storage performance of the secondary battery.

[0050] In any embodiment, the volume average particle size Dv50 of the negative electrode active material is 15 μm to 20 μm. In this way, the battery can have not only good cycle performance but also good kinetic performance.

[0051] In any embodiment, the BET specific surface area of ​​the negative electrode active material is 0.5 m 2 / g~2.0m 2 In this way, the cycle performance of the secondary battery can be further improved.

[0052] In any embodiment, the BET specific surface area of ​​the negative electrode active material is 0.8 m 2 / g~1.5m 2 In this way, the secondary battery can not only have good cycle performance, but also have better kinetic performance.

[0053] In any embodiment, the negative electrode active material includes one or more of graphite and silicon-based materials.

[0054] A third aspect of the present application provides an electrical device comprising the secondary battery of the second aspect of the present application.

[0055] The electrolyte for lithium secondary batteries of the present application adopts a specific content of carboxylic acid ester solvent in an organic solvent and introduces a first additive and a second additive of specific content and type. By combining the above components at specific contents, the secondary battery can have better fast charging performance, cycle performance and storage performance, thereby improving the overall performance of the secondary battery.

[0056] The details of one or more embodiments of the present application are set forth in the following drawings and description. Other features, objects, and advantages of the present application will become apparent from the description, drawings, and claims. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] In order to better describe and illustrate the embodiments or examples provided in this application, reference may be made to one or more of the accompanying drawings. The additional details or examples used to describe the accompanying drawings should not be considered as limiting the scope of the disclosed application, the embodiments or examples currently described, and any of the best modes currently understood for these applications. Moreover, the same reference numerals are used throughout the drawings to represent the same components. In the accompanying drawings:

[0058] FIG1 is a schematic diagram of a battery cell according to an embodiment of the present application;

[0059] FIG2 is an exploded view of a battery cell according to an embodiment of the present application shown in FIG1 ;

[0060] FIG3 is a schematic diagram of an electric device using a secondary battery as a power source according to an embodiment of the present application.

[0061] Explanation of reference numerals: 5, battery cell; 51, housing; 52, electrode assembly; 53, cover plate; 6, electrical device. DETAILED DESCRIPTION

[0062] Below, the embodiments of the lithium secondary battery electrolyte, secondary battery and electrical device of the present application are described in detail with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.

[0063] The "ranges" disclosed in this application can be defined in the form of lower limits and upper limits. A given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. Ranges defined in this way can be inclusive or exclusive of the end values, any end value can be included or excluded independently, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60 to 120 and 80 to 110 are listed for a particular parameter, it is understood that ranges of 60 to 110 and 80 to 120 are also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4, and 5 are also listed, the following ranges are all expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4, and 2 to 5. In this application, unless otherwise specified, the numerical range "a to b" is an abbreviation for any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to listing the parameter as, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, and so on. For example, when a parameter is expressed as an integer selected from "2-10," this is equivalent to listing the integers 2, 3, 4, 5, 6, 7, 8, 9, and 10.

[0064] In this application, "a plurality of" or "a plurality of" refers to a number greater than or equal to 2 unless otherwise specified. For example, "one or more" means one or more than or equal to two.

[0065] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0066] References to "embodiments" herein mean that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment or implementation of the present application. The appearance of such phrases in various locations in the specification does not necessarily refer to the same embodiment, nor does it necessarily refer to independent or alternative embodiments that are mutually exclusive with other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments. References to "implementations" herein have a similar understanding.

[0067] It will be appreciated by those skilled in the art that, in the methods of various embodiments or examples, the order in which the steps are written does not imply a strict order of execution and does not constitute any limitation on the implementation process, and the detailed order of execution of each step should be determined by its function and possible inherent logic. Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or steps (a), (c) and (b), or steps (c), (a) and (b), etc.

[0068] In this application, in the open technical features or technical solutions described with words such as "contain", "include", and "include", unless otherwise specified, additional members other than the listed members are not excluded, and it can be regarded as providing both closed features or solutions consisting of the listed members and open features or solutions that also include additional members in addition to the listed members. For example, A includes a1, a2, and a3. Unless otherwise specified, it may also include other members or may not include additional members. It can be regarded as providing both the feature or solution of "A consists of a1, a2, and a3" and the feature or solution of "A includes not only a1, a2, and a3, but also other members". In this application, unless otherwise specified, A (such as B) means that B is a non-limiting example of A, and it can be understood that A is not limited to B.

[0069] In this application, the terms "optionally," "optional," and "optional" are optional and refer to either option being present or absent. If a technical solution contains multiple "options," each option is considered independent unless otherwise specified and there are no conflicts or constraints.

[0070] The weights described in the examples of this application may be weight units known in the chemical industry, such as μg, mg, g, and kg.

[0071] At present, with the great development of secondary batteries, higher requirements are also put forward for the comprehensive performance of secondary batteries, such as fast charging performance, cycle performance and storage performance. As an important component of secondary batteries, electrolyte plays an irreplaceable role in improving the fast charging performance, cycle performance and storage performance of secondary batteries. Therefore, how to provide an electrolyte that can make secondary batteries have better fast charging performance, cycle performance and storage performance is one of the focuses of those skilled in the art. In this regard, the present application provides an electrolyte comprising a specific content of a carboxylic acid ester solvent, a first additive and a second additive, which can enable the secondary battery to have better fast charging performance, cycle performance and storage performance, and improve the comprehensive performance of the secondary battery.

[0072] A first aspect of the present application provides an electrolyte for a lithium secondary battery, comprising an organic solvent and a first additive, a second additive, and an electrolyte salt dissolved in the organic solvent;

[0073] The organic solvent includes a carboxylate solvent, and the mass percentage W1 of the carboxylate solvent is 20% to 80% based on the total mass of the organic solvent;

[0074] The first additive includes one or more of monofluorophosphate, difluorophosphate, tetrafluoroborate, fluorosulfonate, oxalatoborate, malonic acid borate, oxalatophosphate, and malonic acid phosphate;

[0075] The second additive includes one or more compounds represented by the following formula I and formula II;

[0076] In formula I, R1 and R2 are each independently selected from a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 alkoxy group, a C2-C6 alkenyl group or a C2-C6 alkynyl group;

[0077] In formula II, R3, R4, R5 and R6 are each independently selected from a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 alkoxy group, a C2-C6 alkenyl group or a C2-C6 alkynyl group, and R3, R4, R5 and R6 do not represent a hydrogen atom at the same time;

[0078] The mass percentages of the first additive and the second additive in the electrolyte are W2 and W3 respectively, and 0.035≤(W2+W3) / W1≤0.15.

[0079] The present application adopts a specific content of carboxylic acid ester solvent in the organic solvent of the electrolyte for lithium secondary batteries, and introduces a first additive and a second additive of specific content and type. By combining the above components at specific contents, the secondary battery can have better fast charging performance, cycle performance and storage performance, and significantly improve the overall performance of the secondary battery.

[0080] Compared to carbonate solvents, carboxylate solvents have a lower freezing point and lower viscosity, significantly enhancing electrolyte conductivity and improving the fast-charging performance of secondary batteries. However, carboxylate solvents tend to absorb electrons at the battery's negative electrode, generating reducing gases such as CH4 and H2, which can increase internal pressure in the battery cell. After prolonged cycling, carboxylate solvents can cause severe cell expansion, particularly at high temperatures. This can squeeze out the electrolyte between the electrode layers, reduce the battery's internal ion conductivity, and worsen the battery's cycling and storage performance, ultimately impacting its lifespan.

[0081] To this end, the present application introduces specific types and amounts of first and second additives into the electrolyte for lithium secondary batteries. During the secondary battery charging process, these first and second additives preferentially form an organic / inorganic composite SEI film on the surface of the negative electrode, thereby preventing the carboxylate solvent from contacting the negative electrode interface and reducing gas generation. Furthermore, when the mass percentage W1 of the carboxylate solvent in the organic solvent, the mass percentage W2 of the first additive, and the mass percentage W3 of the second additive are within the aforementioned ranges, the secondary battery can achieve improved fast-charging performance, cycling performance, and storage performance.

[0082] It is understood that the mass percentage W1 of the carboxylate solvent in the organic solvent may be, but is not limited to, 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, 62%, 65%, 68%, 70%, 72%, 75%, 78%, or 80%. The value of (W2+W3) / W1 may be, but is not limited to, 0.035, 0.04, 0.045, 0.05, 0.055, 0.06, 0.065, 0.07, 0.075, 0.08, 0.085, 0.09, 0.095, 0.10, 0.11, 0.12, 0.13, 0.14, or 0.15.

[0083] In some embodiments, in Formula I, R1 and R2 are each independently selected from a hydrogen atom, a halogen atom, a C1-C4 alkyl group, a C1-C4 haloalkyl group, a C1-C4 alkoxy group, a C2-C4 alkenyl group, or a C2-C4 alkynyl group.

[0084] In some embodiments, in Formula II, R3, R4, R5 and R6 are each independently selected from a hydrogen atom, a halogen atom, a C1-C4 alkyl group, a C1-C4 haloalkyl group, a C1-C4 alkoxy group, a C2-C4 alkenyl group or a C2-C4 alkynyl group.

[0085] In some embodiments, the mass percentage W1 of the carboxylate solvent is 30% to 70% based on the total mass of the organic solvent. Controlling the mass percentage W1 of the carboxylate solvent in the organic solvent within the above range can further improve the fast charging performance of the secondary battery while still maintaining good cycle performance and storage performance.

[0086] In some embodiments, based on the total mass of the organic solvent, the mass percentage W1 of the carboxylate solvent is 40% to 60%, thereby further improving the overall performance of the secondary battery.

[0087] In some embodiments, the mass percentage of the carboxylate solvent in the organic solvent is W1, the mass percentage of the first additive in the electrolyte is W2, and the mass percentage of the second additive is W3, satisfying the following relationship: 0.04 ≤ (W2 + W3) / W1 ≤ 0.10. This can further improve the fast charging performance of the secondary battery while maintaining good cycling performance and storage performance.

[0088] In some embodiments, the mass percentage of the carboxylate solvent in the organic solvent is W1, the mass percentage of the first additive in the electrolyte is W2, and the mass percentage of the second additive in the electrolyte is W3, satisfying the following relationship: 0.05≤(W2+W3) / W1≤0.075. This can further improve the overall performance of the secondary battery.

[0089] In some embodiments, the carboxylate solvent includes a compound represented by Formula III;

[0090] wherein R7 and R8 are independently selected from any one of a C1-C3 alkyl group and a C1-C3 halogenated alkyl group. Selecting the aforementioned carboxylate solvent as the organic solvent for the electrolyte can maintain the viscosity of the electrolyte within a suitable range, resulting in a higher conductivity of the electrolyte and, in turn, better fast charging performance of the secondary battery.

[0091] In some embodiments, R7 and R8 in Formula III are independently selected from any one of methyl, ethyl, propyl, fluoromethyl, fluoroethyl, and fluoropropyl.

[0092] In some embodiments, the carboxylate solvent includes one or more of the following compounds:

[0093] In some embodiments, the carboxylate solvent includes one or more of the following compounds:

[0094] In some embodiments, the organic solvent further comprises one or more of linear carbonates and cyclic carbonates. In the present application, there is no particular limitation on the types of linear carbonates and cyclic carbonates used as other solvents, and they can be selected according to actual needs.

[0095] In some embodiments, the linear carbonate may be selected from at least one of the following: dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methylpropyl carbonate, and ethylpropyl carbonate.

[0096] In some embodiments, the cyclic carbonate may be selected from at least one of ethylene carbonate (or ethylene carbonate), propylene carbonate (or propylene carbonate), and butylene carbonate (or butylene carbonate).

[0097] In some embodiments, the mass percentage W2 of the first additive is 0.01% to 10% based on the total mass of the electrolyte, thereby further improving the cycle performance and storage performance of the secondary battery and enabling the secondary battery to have good fast charging performance.

[0098] It will be understood that the mass percentage W2 of the first additive in the electrolyte can be but is not limited to 0.01%, 0.05%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%.

[0099] In some embodiments, the mass percentage W2 of the first additive is 0.05% to 5% based on the total mass of the electrolyte. This can further improve the cycle performance and storage performance of the secondary battery while still maintaining good fast charging performance, thereby achieving better overall performance.

[0100] In some embodiments, the monofluorophosphate comprises lithium monofluorophosphate; the difluorophosphate comprises lithium difluorophosphate; and the tetrafluoroborate comprises lithium tetrafluoroborate.

[0101] In some embodiments, the oxalate borate comprises a compound represented by Formula IV;

[0102] Wherein, M1 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X1 is a halogen; m1 is an integer from 1 to 3; n1 is an integer from 0 to 4; and a1, b1, and c1 are all positive integers. During the secondary battery charging process, the oxalate borate can effectively form an organic / inorganic composite SEI film on the surface of the negative electrode together with the second additive, effectively preventing carboxylate solvents from contacting the negative electrode interface, thereby reducing gas generation.

[0103] In some embodiments, the malonate borate comprises a compound represented by Formula V;

[0104] Wherein, M2 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X2 is a halogen; m2 is an integer from 1 to 3; n2 is an integer from 0 to 4; and a2, b2, and c2 are all positive integers. The aforementioned malonic acid borate can also form an organic / inorganic composite SEI film on the surface of the negative electrode during secondary battery charging, along with the second additive, to alleviate gassing caused by contact between carboxylic acid ester solvents and the negative electrode.

[0105] In some embodiments, the oxalophosphate comprises a compound represented by Formula VI;

[0106] Wherein, M3 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X3 is a halogen; m3 is an integer from 1 to 3; n3 is an integer from 0 to 4; and a3, b3, and c3 are all positive integers. The aforementioned oxalophosphate can also form an organic / inorganic composite SEI film with the second additive on the negative electrode surface, alleviating gassing caused by contact between carboxylic acid ester solvents and the negative electrode.

[0107] In some embodiments, the malonate phosphate comprises a compound represented by Formula VII;

[0108] Wherein, M4 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu, and Ni; X4 is a halogen; m4 is an integer from 1 to 3; n4 is an integer from 0 to 4; and a4, b4, and c4 are all positive integers. The aforementioned malonic acid phosphate can also form an organic / inorganic composite SEI film with the second additive on the negative electrode surface, preventing carboxylate solvents from contacting the negative electrode interface and alleviating the gassing problem caused by contact between the carboxylate solvent and the negative electrode.

[0109] In some embodiments, the fluorosulfonate salt comprises a compound of formula VIII; (FSO3) y My+ Formula VIII

[0110] Where y is a positive integer; M y+ is a metal ion or an organic cation; metal ions include Li + 、Na + , K + , Rb + 、Cs + Mg 2+ , Ca 2+ 、Ba 2+ 、Al 3+ 、Fe 2+ 、Cu 2+ 、Fe 3+ 、Ni 2+ and Ni 3+ The fluorosulfonate with the above structure can form an organic / inorganic composite SEI film on the negative electrode surface with the second additive, preventing the carboxylic acid ester solvent from contacting the negative electrode interface, thereby reducing gas generation.

[0111] In some embodiments, the mass percentage W3 of the second additive is 0.05% to 10% based on the total mass of the electrolyte. In this way, the secondary battery has better cycle performance and storage performance while maintaining good fast charging performance, and the overall performance is better.

[0112] It can be understood that the mass percentage W3 of the second additive in the electrolyte can be but is not limited to 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, 0.55%, 0.6%, 0.65%, 0.7%, 0.75%, 0.8%, 0.85%, 0.9%, 0.95%, and 10%.

[0113] In some embodiments, the mass percentage W3 of the second additive is 0.1% to 5% based on the total mass of the electrolyte. This can further improve the cycle performance and storage performance of the secondary battery while maintaining good fast charging performance, further improving the overall performance of the secondary battery.

[0114] In some embodiments, the electrolyte salt includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0115] In some embodiments, the concentration of the electrolyte salt in the electrolyte solution is 0.3 mol / L (mole / liter) or more, optionally 0.7 mol / L or more, optionally 1.7 mol / L or less, and further optionally 1.2 mol / L or less.

[0116] The second aspect of the present application provides a secondary battery, comprising the lithium secondary battery electrolyte of the first aspect of the present application. The secondary battery of the present application, by employing the lithium secondary battery electrolyte of the first aspect of the present application, not only has good fast-charging performance; but also, through the first additive and the second additive, forms an organic / inorganic composite SEI film on the negative electrode surface during battery charging, thereby preventing carboxylic acid ester solvents from contacting the negative electrode interface. The secondary battery has good cycling performance and storage performance.

[0117] In some embodiments, the secondary battery further comprises a negative electrode plate, wherein the negative electrode plate contains a negative electrode active material, and the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material is 10 -11 cm 2 / S~10 -12 cm 2 / S. That is, the negative electrode active material has a large lithium ion solid phase diffusion coefficient Ds. When the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material in the negative electrode plate is too small, it is not conducive to the migration of lithium ions in the negative electrode material, the kinetic performance of the material is insufficient, and the fast charging capability of the battery is insufficient. In addition, due to the insufficient kinetic performance of the material, there will be a risk of lithium precipitation when charging at a high rate, the battery performance will deteriorate sharply, and there will be a risk of battery gas production. Controlling the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material within the above range can make the lithium ion migration rate of the negative electrode material faster, the kinetic performance of the negative electrode material is excellent, and the fast charging capability of the secondary battery is further improved.

[0118] In some embodiments, the negative electrode active material has a volume average particle size Dv50 ≥ 6 μm. During battery charging, the first additive and the second additive form a SEI film of a certain thickness on the negative electrode surface. Controlling the volume average particle size Dv50 of the negative electrode active material to ≥ 6 μm can reduce the contact area between the negative electrode material and the electrolyte, further preventing the carboxylate solvent from undergoing side reactions on the negative electrode surface, thereby reducing gas generation and inhibiting the deterioration of cycle performance.

[0119] It can be understood that the volume average particle size Dv50 of the negative electrode active material can be but is not limited to 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm, 20μm, 21μm, 22μm, 23μm, 24μm, 25μm.

[0120] In some embodiments, the volume average particle size Dv50 of the negative electrode active material is 15 μm to 20 μm. This not only allows the battery to have good cycle performance, but also allows the battery to have better kinetic performance.

[0121] In some embodiments, the BET specific surface area of ​​the negative electrode active material is 0.5 m 2 / g~2.0m 2 During the battery charging process, the first additive and the second additive will form a SEI film of a certain thickness on the negative electrode surface, controlling the BET specific surface area of ​​the negative electrode active material to 0.5m 2 / g~2.0m 2 / g range, the contact area between the negative electrode material and the electrolyte can be reduced, and the side reaction of the carboxylic acid ester solvent on the negative electrode surface can be reduced, thereby reducing the generation of gas and improving the cycle performance of the battery.

[0122] It is understood that the BET specific surface area of ​​the negative electrode active material can be, but is not limited to, 0.5 m 2 / g, 0.6m 2 / g, 0.7m 2 / g, 0.8m 2 / g, 0.9m 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.2m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.6m 2 / g, 1.7m 2 / g, 1.8m 2 / g, 1.9m 2 / g, 2.0m 2 / g.

[0123] In some embodiments, the BET specific surface area of ​​the negative electrode active material is 0.8 m 2 / g~1.5m 2 In this way, the secondary battery can not only have good cycle performance, but also have better kinetic performance.

[0124] A third aspect of the present application provides an electrical device, which includes the secondary battery according to the second aspect of the present application.

[0125] The secondary battery and the electric device of the present application will be described below with reference to the accompanying drawings as appropriate.

[0126] Unless otherwise specified, the components, material types, or contents of the batteries mentioned are applicable to both lithium-ion secondary batteries and sodium-ion secondary batteries.

[0127] In one embodiment of the present application, a secondary battery is provided.

[0128] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The electrolyte conducts ions between the positive and negative electrodes. The separator, located between the positive and negative electrodes, primarily prevents short circuits between the positive and negative electrodes while allowing ions to pass through.

[0129] Positive electrode

[0130] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector.

[0131] As a non-limiting example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive electrode current collector.

[0132] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be obtained by forming a metal material on a polymer material substrate. In the positive electrode current collector, non-limiting examples of the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the positive electrode current collector, non-limiting examples of the polymer material substrate may include one or more of substrates such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE).

[0133] In some embodiments, the positive electrode active material may include a positive electrode active material for a battery known in the art.

[0134] As a non-limiting example, the positive electrode active material of the lithium-ion secondary battery may include one or more of the following materials: lithium-containing phosphates with an olivine structure, lithium transition metal oxides and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as battery positive electrode active materials may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide and their modified compounds. Non-limiting examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, and a composite material of lithium manganese iron phosphate and carbon. Non-limiting examples of lithium cobalt oxide may include LiCoO2; non-limiting examples of lithium nickel oxide may include LiNiO2; non-limiting examples of lithium manganese oxide may include LiMnO2, LiMn2O4, etc.; non-limiting examples of lithium nickel cobalt manganese oxide may include LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 ), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 ), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 ), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 ), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM 811 ) etc.; Non-limiting examples of lithium nickel cobalt aluminum oxide may include LiNi 0.85 Co 0.15 Al 0.05 O2.

[0135] It is understandable that the battery will be accompanied by lithium (Li) deintercalation and consumption during the charge and discharge process, and the content of Li in the positive electrode plate is different when the battery is discharged to different states. In the list of positive electrode materials in this application, unless otherwise specified, the Li content is the initial state of the material. The positive electrode material is applied to the positive electrode plate in the battery system, and after the charge and discharge cycle, the Li content in the positive electrode material contained in the plate will usually change. Among them, the Li content can be measured by molar content, but is not limited to this. Regarding "the Li content is the initial state of the material", the initial state of the material refers to the state before the material is added to the positive electrode slurry. It is understandable that new materials obtained by appropriate modification on the basis of the listed positive electrode materials are also within the scope of positive electrode materials. The aforementioned appropriate modification refers to acceptable modification methods for positive electrode materials, and non-limiting examples include coating modification.

[0136] In the examples of positive electrode materials in this application, the oxygen (O) content is only a theoretical value. Lattice oxygen release will cause the molar content of oxygen to change, and the actual O content will fluctuate. The O content can be measured by molar content, but is not limited to this.

[0137] As non-limiting examples, the positive electrode active material of a sodium ion secondary battery may include one or more of the following materials: sodium transition metal oxides, polyanionic compounds, and Prussian blue compounds. However, the present application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for sodium ion batteries may also be used.

[0138] As an optional technical solution of the present application, in the sodium transition metal oxide, the transition metal can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Sodium transition metal oxide is, for example, Na x MO2, wherein M is one or more of Ti, V, Mn, Co, Ni, Fe, Cr and Cu, and 0<x≤1.

[0139] As an optional technical solution of the present application, the polyanionic compound can be a compound having sodium ions, transition metal ions and tetrahedral (YO4) n- A class of compounds with anionic units. The transition metal can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; Y can be one or more of P, S and Si; n represents (YO4) n- valence.

[0140] Polyanionic compounds can also be sodium ions, transition metal ions, tetrahedral (YO4) n-A class of compounds containing anion units and halogen anions. The transition metal can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr, and Ce; Y can be one or more of P, S, and Si, and n represents (YO4) n- valence state; the halogen can be one or more of F, Cl and Br.

[0141] Polyanionic compounds can also be sodium ions, tetrahedral (YO4) n- Anion unit, polyhedron unit (ZO y ) m+ and an optional halogen anion. Y can be one or more of P, S and Si, and n represents (YO4) n- valence state; Z represents a transition metal, which can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce; m represents (ZO y ) m+ valence state; the halogen can be one or more of F, Cl and Br.

[0142] Polyanionic compounds include NaFePO4, Na3V2(PO4)3 (sodium vanadium phosphate, abbreviated as NVP), Na4Fe3(PO4)2(P2O7), NaM'PO4F (M' is one or more of V, Fe, Mn and Ni) and Na3(VO y )2(PO4)2F 3-2y One or more of (0≤y≤1).

[0143] Prussian blue compounds can be sodium ions, transition metal ions and cyanide ions (CN - ) compounds. The transition metal can be one or more of Mn, Fe, Ni, Co, Cr, Cu, Ti, Zn, V, Zr and Ce. Prussian blue compounds are, for example, Na a Me b Me' c (CN)6, wherein Me and Me' are each independently one or more of Ni, Cu, Fe, Mn, Co and Zn, 0<a≤2, 0<b<1, 0<c<1.

[0144] The weight ratio of the positive electrode active material in the positive electrode film layer is 80 to 100 weight percent based on the total weight of the positive electrode film layer.

[0145] In some embodiments, the positive electrode film layer further includes a binder. As a non-limiting example, the binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin. The weight ratio of the binder in the positive electrode film layer is 0 to 20 weight%, based on the total weight of the positive electrode film layer.

[0146] In some embodiments, the positive electrode film layer further includes a conductive agent. As non-limiting examples, the conductive agent may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. The weight ratio of the conductive agent in the positive electrode film layer is 0 to 20% by weight, based on the total weight of the positive electrode film layer.

[0147] In some embodiments, the positive electrode sheet can be prepared by the following method: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder and any other components, are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry, wherein the positive electrode slurry has a solid content of 40wt% to 80wt%, and the viscosity at room temperature is adjusted to 5000mPa·s to 25000mPa·s, the positive electrode slurry is coated on the surface of the positive electrode collector, and after drying, the positive electrode sheet is formed by cold rolling; the positive electrode powder coating unit area density is 150mg / m 2 ~350 mg / m 2 The compaction density of the positive electrode is 3.0g / cm 3 ~3.6g / cm 3 , optional 3.3g / cm 3 ~3.5g / cm 3 .

[0148] The calculation formula of the compacted density is:

[0149] Compaction density = coating surface density / (thickness of the electrode after extrusion - thickness of the current collector).

[0150] The mass M of the positive electrode active material per unit area of ​​the positive electrode membrane can be obtained by weighing using a standard balance.

[0151] The thickness T of the positive electrode film can be measured using a micrometer, for example, a Mitutoyo 293-100 with an accuracy of 0.1 μm. It should be noted that the thickness of the positive electrode film described in this application refers to the thickness of the positive electrode film in the positive electrode sheet after cold pressing and used in battery assembly.

[0152] Negative electrode

[0153] The negative electrode sheet includes a negative electrode current collector and a negative electrode film layer provided on at least one surface of the negative electrode current collector, wherein the negative electrode film layer includes a negative electrode active material.

[0154] As a non-limiting example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.

[0155] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be obtained by forming a metal material on a polymer material substrate. Among them, in the negative electrode current collector, non-limiting examples of the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy. In the negative electrode current collector, non-limiting examples of the polymer material substrate may include one or more of substrates such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.

[0156] In some embodiments, the negative electrode active material may be a negative electrode active material for batteries known in the art.

[0157] As a non-limiting example, the negative electrode active material of the lithium-ion secondary battery may include one or more of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials and lithium titanate. Silicon-based materials may include one or more of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites and silicon alloys. Tin-based materials may include one or more of elemental tin, tin oxides and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.

[0158] As a non-limiting example, the negative active material of the sodium ion secondary battery is generally a hard carbon material, a two-dimensional metal carbide or a nitride. Preferably, the negative active material of the sodium ion secondary battery is generally a hard carbon material.

[0159] In some embodiments, the negative electrode film layer further includes a binder. The binder may include one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0160] In some embodiments, the negative electrode film layer further includes a conductive agent, which may include one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0161] In some embodiments, the negative electrode film layer further includes other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).

[0162] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet, such as the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (a non-limiting example of the solvent is deionized water) to form a negative electrode slurry; the negative electrode slurry is coated on at least one side of the negative electrode current collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained. The surface of the negative electrode current collector coated with the negative electrode slurry can be a single surface of the negative electrode current collector or on both surfaces of the negative electrode current collector. The solid content of the negative electrode slurry can be 40wt% to 60wt%. The viscosity of the negative electrode slurry at room temperature can be adjusted to 2000mPa·s to 10000mPa·s. When coating the negative electrode slurry, the coating unit surface density on a dry weight basis (excluding the solvent) can be 75g / m 2 ~220g / m 2 The compaction density of the negative electrode can be 1.0g / cm 3 ~1.8g / cm 3 .

[0163] electrolyte

[0164] The electrolyte plays a role in conducting ions between the positive electrode and the negative electrode. In the secondary battery of the present application, the electrolyte of the first aspect of the present application is used.

[0165] In some embodiments, the electrolyte includes an electrolyte salt and an organic solvent.

[0166] In some embodiments, the electrolyte salt of the lithium ion secondary battery can be selected from one or more of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.

[0167] In some embodiments, the organic solvent includes a carboxylate solvent accounting for 20% to 80% by mass of the organic solvent.

[0168] The electrolyte salt of the sodium ion secondary battery can be selected from one or more of sodium hexafluorophosphate, sodium bis(fluorosulfonyl)imide, sodium bis(trifluoromethanesulfonyl)imide, sodium trifluoromethanesulfonate, sodium tetrafluoroborate, sodium difluorophosphate, sodium perchlorate, and sodium chloride.

[0169] The concentration of the electrolyte salt is generally 0.5 mol / L to 5 mol / L.

[0170] Isolation film

[0171] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical and mechanical stability can be selected.

[0172] In some embodiments, the material of the separator can include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0173] In some embodiments, the isolation film has a thickness of 6 μm to 40 μm, and may optionally be 12 μm to 20 μm.

[0174] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0175] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0176] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft shell, such as a pouch-type soft shell. The material of the soft shell can be plastic. Further, non-limiting examples of plastic can include one or more of polypropylene, polybutylene terephthalate, and polybutylene succinate.

[0177] A secondary battery includes at least one battery cell. A secondary battery may include one or more battery cells.

[0178] In this application, unless otherwise specified, a "battery cell" refers to a basic unit that can achieve the mutual conversion of chemical energy and electrical energy. Further, generally speaking, it includes at least a positive electrode plate, a negative electrode plate, and an electrolyte. During the battery's charge and discharge process, active ions are embedded in and out of the positive and negative electrode plates. The electrolyte plays the role of conducting active ions between the positive and negative electrode plates.

[0179] The present application has no particular limitation on the shape of the battery cell, which can be cylindrical, square, or any other shape. For example, FIG1 shows a battery cell 5 with a square structure as an example.

[0180] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0181] In some embodiments, the battery cells 5 can be assembled into a battery module. The number of battery cells 5 contained in the battery module can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module.

[0182] In the battery module, the plurality of battery cells 5 can be arranged in sequence along the length of the battery module. Of course, they can also be arranged in any other manner. Furthermore, the plurality of battery cells 5 can be fixed by fasteners.

[0183] In some embodiments, the battery module may further include a housing having a receiving space, and the plurality of battery cells 5 may be received in the receiving space.

[0184] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art based on the application and capacity of the battery pack.

[0185] A battery pack may include a battery box and multiple battery modules disposed within the box. The battery box comprises an upper case and a lower case. The upper case can be placed over the lower case to form an enclosed space for accommodating the battery modules. The multiple battery modules can be arranged in any manner within the battery box.

[0186] In addition, the present application also provides an electric device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electric device, and can also be used as an energy storage unit for the electric device. The electric device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but is not limited thereto.

[0187] As the electrical device, a secondary battery, a battery module or a battery pack can be selected according to its usage requirements.

[0188] FIG3 shows an example of an electric device 6. The electric device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the electric device's requirements for high power and high energy density of secondary batteries, a battery pack or battery module may be used.

[0189] Another example device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is generally required to be lightweight and thin, and may use a secondary battery as a power source.

[0190] The following are some examples.

[0191] In order to make the technical problems, technical solutions and beneficial effects solved by this application clearer, the application will be further described in detail below with reference to the embodiments and drawings. Obviously, the described embodiments are only a part of the embodiments of this application, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is in no way intended to limit the present application and its applications. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0192] If no specific techniques or conditions are specified in the examples, the experiments were carried out according to the techniques or conditions described in the literature in the field or according to the product instructions. All reagents or instruments used without specifying the manufacturer are commercially available conventional products.

[0193] Example 1:

[0194] 1) Preparation of positive electrode sheet

[0195] The lithium iron phosphate positive electrode material, the conductive agent acetylene black, and the binder polyvinylidene fluoride (PVDF) were added to the solvent N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5, and the mixture was thoroughly stirred and mixed to obtain a positive electrode slurry (solid content of 67%); the positive electrode slurry was then evenly coated on the positive electrode current collector to obtain a single-sided positive electrode sheet with a film weight of 350 mg / 1540.25 mm 2 The positive electrode sheet is then dried, cold pressed and cut to obtain the positive electrode sheet.

[0196] 2) Preparation of negative electrode sheet

[0197] The negative electrode active material artificial graphite, conductive agent carbon black, binder styrene-butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC-Na) are dissolved in deionized water at a weight ratio of 90:4:4:2 and mixed evenly to prepare a negative electrode slurry (solid content 48%). The negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and then dried, cold pressed, and cut to obtain a negative electrode sheet. The lithium ion solid phase diffusion coefficient Ds of the negative electrode active material is 5*10 -12 cm 2 / S, the volume average particle size Dv50 is 17 μm, and the BET specific surface area is 1 m 2 / g.

[0198] 3) Isolation film

[0199] A conventional commercially available polypropylene film was used as the isolation film.

[0200] 4) Electrolyte

[0201] In an argon atmosphere glove box (H2O <0.1ppm, O2 <0.1ppm), ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed evenly in a volume ratio of 3:7. Based on the total weight of the solvent, the total weight of ethylene carbonate and ethyl methyl carbonate accounted for 80%. Methyl acetate was added thereto at 20% of the total weight of the solvent. Subsequently, LiPF6 lithium salt, a first additive (lithium difluorophosphate), and a second additive (vinylene carbonate) were added and dissolved in an organic solvent to a concentration of LiPF6 of 12.5%, a mass percentage of the first additive of 1%, and a mass percentage of the second additive of 2%. The mixture was stirred evenly to obtain an electrolyte.

[0202] 5) Battery assembly

[0203] The positive electrode sheet (87 mm wide by 605 mm long), the separator (98 mm wide by 1896 mm long), and the negative electrode sheet (93 mm wide by 735 mm long) are stacked in order, with the separator placed between the positive and negative electrode sheets to serve as an isolation, and then wound to obtain an electrode assembly; the electrode assembly is placed in a battery case, dried, and then injected with 12.0 g of electrolyte (3 Ah, injection coefficient 4.0 g / Ah), and then subjected to processes such as formation and static standing to obtain a lithium-ion secondary battery.

[0204] Example 2:

[0205] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 1, except that the mass percentage W1 of the carboxylate solvent in the organic solvent of the electrolyte in this embodiment is 30%; accordingly, (W2+W3) / W1 is 0.1.

[0206] Example 3:

[0207] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 1, except that the mass percentage W1 of the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is 40%; accordingly, (W2+W3) / W1 is 0.075.

[0208] Example 4:

[0209] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 1, except that the mass percentage W1 of the carboxylate solvent in the organic solvent of the electrolyte in this embodiment is 50%; accordingly, (W2+W3) / W1 is 0.06.

[0210] Example 5:

[0211] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 1, except that the mass percentage W1 of the carboxylate solvent in the organic solvent of the electrolyte in this embodiment is 60%; accordingly, (W2+W3) / W1 is 0.05.

[0212] Example 6:

[0213] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 1, except that the mass percentage W1 of the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is 70%; accordingly, (W2+W3) / W1 is 0.04.

[0214] Example 7:

[0215] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 1, except that the mass percentage W1 of the carboxylate solvent in the organic solvent of the electrolyte in this embodiment is 80%; accordingly, (W2+W3) / W1 is 0.0375.

[0216] Example 8:

[0217] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, with the only difference being that the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is ethyl acetate.

[0218] Example 9:

[0219] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, with the only difference being that the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is ethyl difluoroacetate.

[0220] Example 10:

[0221] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 5, with the only difference being that the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is methyl difluoroacetate.

[0222] Example 11:

[0223] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the mass percentage W2 of the first additive lithium difluorophosphate in the electrolyte of this embodiment is 5%; accordingly, (W2+W3) / W1 is 0.117.

[0224] Example 12:

[0225] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the first additive in the electrolyte of this embodiment is lithium difluorobisoxalatoborate.

[0226] Example 13:

[0227] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the first additive in the electrolyte of this embodiment is lithium tetrafluoroborate.

[0228] Example 14:

[0229] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the first additive in the electrolyte of this embodiment is lithium fluorosulfonate.

[0230] Example 15:

[0231] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the mass percentage W3 of the second additive in the electrolyte of this embodiment is 5%; accordingly, (W2+W3) / W1 is 0.1.

[0232] Example 16:

[0233] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the type of the second additive in the electrolyte of this embodiment is

[0234] Example 17:

[0235] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the type of the second additive in the electrolyte of this embodiment is

[0236] Example 18:

[0237] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the type of the second additive in the electrolyte of this embodiment is

[0238] Example 19:

[0239] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, with the only difference being that the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is methyl formate.

[0240] Example 20:

[0241] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, with the only difference being that the carboxylic acid ester solvent in the organic solvent of the electrolyte in this embodiment is propyl propionate.

[0242] Example 21:

[0243] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material in the secondary battery of this embodiment is 10 -11 cm 2 / S.

[0244] Example 22:

[0245] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material in the secondary battery of this embodiment is 10 -12 cm 2 / S.

[0246] Example 23:

[0247] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material in the secondary battery of this embodiment is 10 -10 cm 2 / S.

[0248] Example 24:

[0249] The preparation method of the secondary battery of this embodiment is basically the same as that of embodiment 5, except that the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material in the secondary battery of this embodiment is 10 -13 cm 2 / S.

[0250] Example 25:

[0251] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the volume average particle size Dv50 of the negative electrode active material in the secondary battery of this embodiment is 15 μm.

[0252] Example 26:

[0253] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the volume average particle size Dv50 of the negative electrode active material in the secondary battery of this embodiment is 20 μm.

[0254] Example 27:

[0255] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the volume average particle size Dv50 of the negative electrode active material in the secondary battery of this embodiment is 10 μm.

[0256] Example 28:

[0257] The preparation method of the secondary battery of this embodiment is substantially the same as that of embodiment 5, with the only difference being that the volume average particle size Dv50 of the negative electrode active material in the secondary battery of this embodiment is 25 μm.

[0258] Example 29:

[0259] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 5, except that the BET specific surface area of ​​the negative electrode active material in the secondary battery of this embodiment is 0.5 m 2 / g.

[0260] Example 30:

[0261] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 5, except that the BET specific surface area of ​​the negative electrode active material in the secondary battery of this embodiment is 2 m 2 / g.

[0262] Example 31:

[0263] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 5, except that the BET specific surface area of ​​the negative electrode active material in the secondary battery of this embodiment is 0.1 m 2 / g.

[0264] Example 32:

[0265] The preparation method of the secondary battery of this embodiment is basically the same as that of Example 5, except that the BET specific surface area of ​​the negative electrode active material in the secondary battery of this embodiment is 3 m 2 / g.

[0266] Comparative Example 1:

[0267] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, except that the mass percentage W2 of the first additive potassium difluorophosphate in the electrolyte in this comparative example is 0.005%; accordingly, (W2+W3) / W1 is 0.0334.

[0268] Comparative Example 2:

[0269] The preparation method of the secondary battery of this comparative example is basically the same as that of Example 5, except that the mass percentage W2 of the first additive potassium difluorophosphate in the electrolyte in this comparative example is 0.01%; accordingly, (W2+W3) / W1 is 0.0335.

[0270] Comparative Example 3:

[0271] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, except that the mass percentage W2 of the first additive potassium difluorophosphate in the electrolyte in this comparative example is 0.05%; accordingly, (W2+W3) / W1 is 0.034.

[0272] Comparative Example 4:

[0273] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, except that in this comparative example, the mass percentage W2 of the first additive potassium difluorophosphate in the electrolyte is 10%; accordingly, (W2+W3) / W1 is 0.2.

[0274] Comparative Example 5:

[0275] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, except that the mass percentage W2 of the first additive potassium difluorophosphate in the electrolyte in this comparative example is 11%; accordingly, (W2+W3) / W1 is 0.217.

[0276] Comparative Example 6:

[0277] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that the mass percentage W3 of the second additive in the electrolyte in this comparative example is 0.04%; accordingly, (W2+W3) / W1 is 0.0173.

[0278] Comparative Example 7:

[0279] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that the mass percentage W3 of the second additive in the electrolyte in this comparative example is 0.05%; accordingly, (W2+W3) / W1 is 0.0175.

[0280] Comparative Example 8:

[0281] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that the mass percentage W3 of the second additive in the electrolyte in this comparative example is 0.1%; accordingly, (W2+W3) / W1 is 0.018.

[0282] Comparative Example 9:

[0283] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that the mass percentage W3 of the second additive in the electrolyte in this comparative example is 10%; accordingly, (W2+W3) / W1 is 0.183.

[0284] Comparative Example 10:

[0285] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that the mass percentage W3 of the second additive in the electrolyte in this comparative example is 11%; accordingly, (W2+W3) / W1 is 0.2.

[0286] Comparative Example 11:

[0287] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that in this comparative example, no second additive is added to the electrolyte, that is, W3 is 0; accordingly, (W2+W3) / W1 is 0.0167.

[0288] Comparative Example 12:

[0289] The preparation method of the secondary battery of this comparative example is substantially the same as that of Example 5, with the only difference being that in this comparative example, the first additive is not added to the electrolyte, that is, W2 is 0; accordingly, (W2+W3) / W1 is 0.033.

[0290] Comparative Example 13:

[0291] The preparation method of the secondary battery of this comparative example is basically the same as that of Example 5, except that the mass percentage W1 of methyl acetate in the organic solvent of the electrolyte in this comparative example is 10%; accordingly, (W2+W3) / W1 is 0.3.

[0292] Comparative Example 14:

[0293] The preparation method of the secondary battery of this comparative example is basically the same as that of Example 5, except that the mass percentage W1 of methyl acetate in the organic solvent of the electrolyte in this comparative example is 90%; accordingly, (W2+W3) / W1 is 0.033.

[0294] Performance Testing

[0295] 1) Fast charging performance test:

[0296] At 25°C, the divided batteries were subjected to a 2.5V to 3.65V charge and discharge test. The test steps were as follows: first, charging at a 3C constant current to 30% SOC, then charging at a 2C constant current to 60% SOC, then charging at a 1C constant current and constant voltage to 80% SOC with a cutoff current of 0.01C and a 5-minute rest period. Finally, discharging at a 1C constant current to 2.0V and a 5-minute rest period was performed. The time it took for the batteries to reach 80% SOC was measured.

[0297] 2) Cyclic performance test:

[0298] At 45°C, charge the secondary battery at a constant current of 0.5C to 3.65V, then charge it at a constant voltage of 3.65V until the current drops below 0.05C. Then discharge it at a constant current of 0.5C to 2.5V. This constitutes one charge and discharge cycle (i.e., one cycle). Repeat this cycle, and record the number of cycles required for the capacity retention rate to reach 80%.

[0299] 3) Storage performance test:

[0300] The lithium-ion secondary battery is charged to 3.65V at a constant current of 0.33C, and then charged to a current of 0.05C at a constant voltage of 3.65V to fully charge the secondary battery. The volume of the battery is tested using the water displacement method, and the volume at this time is recorded as the volume before storage. The secondary battery is then stored at 60°C for 30 days. After the storage period, the secondary battery is placed in an environment of 25°C and the volume of the battery is tested using the water displacement method, and the volume at this time is recorded as the volume after storage. The volume expansion rate of the battery is calculated according to the following formula:

[0301] Battery volume expansion rate = (volume after storage / volume before storage - 1) × 100%.

[0302] 4) Lithium ion solid phase diffusion coefficient test:

[0303] Taking the GITT method as an example, the steps for testing the lithium ion solid phase diffusion coefficient of the negative electrode active material are as follows:

[0304] The negative electrode active material was ground into a powder microelectrode. This powder microelectrode was connected to an electrochemical workstation and coulometric titration was performed. A GITT curve was obtained using a 20μA pulse current, a 1h titration time, and a 4h rest period (Note: To compare the effects of pulse current and time, a parallel experiment with 10μA and 10min was performed). The lithium ion diffusion coefficient was calculated using the following formula:

[0305] Where D is the lithium ion diffusion coefficient; I0 ​​is the applied current 20μA; V m is the molar volume of the active substance; F is the Faraday constant; A is the electrode surface area; dE / dx is the slope of the coulomb titration curve, that is, the slope of the open circuit potential at a certain concentration on the Li concentration curve of the electrode; dE / d(t 1 / 2 ) is the polarization voltage versus t 1 / 2The slope of the curve. For details, please refer to: Xie et al., Solid State Ionics, 2007, 178: 1218–1224; Yang et al., Electrochimica Acta, 2012, 66: 88–93.

[0306] 5) Volume average particle size test:

[0307] "Dv50" represents the particle size at which 50% of the volume of a material is accumulated, measured from the smallest particle size. Typically, Dv50 can be measured using methods and instruments known in the art, such as a laser diffraction particle size distribution analyzer (e.g., a Malvern Mastersizer 3000).

[0308] 6) BET specific surface area test:

[0309] The test method refers to the standard GB / T19587-2004, "Determination of Specific Surface Area of ​​Solid Substances by Gas Adsorption BET Method." 8-15g of the sample to be tested is placed in a sample tube, and the initial mass of the sample is recorded. The weighed sample is then loaded into the NOVA2000e instrument. Degassing is then initiated, and the sample is heated to 200°C and held for 2 hours. The mass of the degassed sample is then recorded. The degassed sample is then returned to the instrument and liquid nitrogen is added for the BET test.

[0310] The fast charging performance, cycle performance, and storage performance of the secondary batteries of the above embodiments and comparative examples were tested, and the specific test results are shown in Tables 1 to 9.

[0311] Table 1

[0312] Table 2

[0313] Table 3

[0314] Table 4

[0315] Table 5

[0316] Table 6

[0317] Table 7

[0318] Table 8

[0319] Table 9

[0320] It can be seen from the data of the above-mentioned preparation examples and comparative examples that in Examples 1 to 7, W1 is in the range of 20% to 80%, and (W2+W3) / W1 is in the range of 0.035 to 0.15. As the mass fraction of the carboxylic acid ester solvent methyl acetate in the organic solvent gradually increases, the fast charging performance of the battery gradually improves. Although the cycle performance and storage performance of the battery decline, they are both at a good level.

[0321] In Examples 2 to 6, W1 is in the range of 30% to 70%, and (W2+W3) / W1 is in the range of 0.04 to 0.1. Compared with Examples 1 and 7, the comprehensive performance of the secondary batteries of Examples 2 to 6 is better.

[0322] In Examples 3 to 5, W1 is in the range of 40% to 60%, and (W2+W3) / W1 is in the range of 0.05 to 0.075. Compared with Examples 1, 2, 6 and 7, the comprehensive performance of the secondary batteries of Examples 3 to 5 is further improved.

[0323] Compared with Example 5, the amount of the first additive, lithium difluorophosphate, was increased in Example 11, and the storage performance of the secondary battery was significantly improved. Compared with Example 5, the amount of the second additive, vinylene carbonate, was increased in Example 15, and the storage performance of the secondary battery was also significantly improved.

[0324] Compared with Example 5, Comparative Examples 1, 2, and 3 reduce the amount of the first additive, lithium difluorophosphate. Although their fast charging performance is improved, their cycle performance and storage performance are significantly reduced, and the overall performance is poor.

[0325] Compared with Example 5, the amount of the first additive lithium difluorophosphate in the electrolyte of Comparative Examples 4 and 5 is increased. Although the storage performance of the battery is improved, the fast charging performance and cycle performance of the battery are significantly reduced, and the overall performance is also poor.

[0326] Compared with Example 5, the amount of the second additive vinylene carbonate in the electrolyte of Comparative Examples 6, 7 and 8 is reduced. Although the fast charging performance of the batteries is slightly improved, the cycle performance and storage performance of the batteries are significantly reduced.

[0327] Compared with Example 5, the amount of the second additive vinylene carbonate in the electrolyte of Comparative Examples 9 and 10 is increased. Although the storage performance of the battery is improved, the fast charging performance and cycle performance of the battery are significantly reduced.

[0328] In Comparative Example 11, the second additive was not added to the electrolyte, and the battery's cycle performance and storage performance were significantly reduced. In Comparative Example 12, the first additive was not added to the electrolyte, and the battery's cycle performance and storage performance also showed a significant decline. In Comparative Example 13, the amount of carboxylic acid ester in the organic solvent was less than 20%, and the battery's fast charging performance was greatly reduced. In Comparative Example 14, the amount of carboxylic acid ester in the organic solvent exceeded 80%, and the battery's cycle performance and storage performance were greatly reduced.

[0329] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present application, embodiments having substantially the same structure as the technical concept and exerting the same effects are all included in the technical scope of the present application. In addition, within the scope of the subject matter of the present application, various modifications that can be conceived by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements in the embodiments are also included in the scope of the present application.

Claims

1. An electrolyte for a lithium secondary battery, comprising an organic solvent and a first additive, a second additive and an electrolyte salt dissolved in the organic solvent; The organic solvent includes a carboxylate solvent, and based on the total mass of all organic solvents, the mass percentage W1 of the carboxylate solvent is 20% to 80%; The first additive comprises one or more of monofluorophosphate, difluorophosphate, tetrafluoroborate, fluorosulfonate, oxalate borate, malonic acid borate, oxalate phosphate and malonic acid phosphate; The second additive includes one or more compounds represented by the following formula I and formula II; In Formula I, R1 and R2 are each independently selected from a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 alkoxy group, a C2-C6 alkenyl group or a C2-C6 alkynyl group; In formula II, R3, R4, R5 and R6 are each independently selected from a hydrogen atom, a halogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, a C1-C6 alkoxy group, a C2-C6 alkenyl group or a C2-C6 alkynyl group, and R3, R4, R5 and R6 do not represent a hydrogen atom at the same time; in, The mass percentages of the first additive and the second additive in the electrolyte are W2 and W3 respectively, and 0.035≤(W2+W3) / W1≤0.

15.

2. The electrolyte for lithium secondary battery according to claim 1, characterized in that: The electrolyte satisfies at least one of the following (1) to (2): (1) In formula I, R1 and R2 are each independently selected from a hydrogen atom, a halogen atom, a C1-C4 alkyl group, a C1-C4 haloalkyl group, a C1-C4 alkoxy group, a C2-C4 alkenyl group or a C2-C4 alkynyl group; (2) In formula II, R3, R4, R5 and R6 are each independently selected from a hydrogen atom, a halogen atom, a C1-C4 alkyl group, a C1-C4 haloalkyl group, a C1-C4 alkoxy group, a C2-C4 alkenyl group or a C2-C4 alkynyl group.

3. The electrolyte for lithium secondary battery according to claim 1 or 2, characterized in that: Based on the total mass of the organic solvent, the mass percentage W1 of the carboxylate solvent is 30% to 70%.

4. The electrolyte for lithium secondary battery according to any one of claims 1 to 3, characterized in that Based on the total mass of the organic solvent, the mass percentage W1 of the carboxylate solvent is 40% to 60%.

5. The electrolyte for lithium secondary battery according to any one of claims 1 to 4, characterized in that 0.05≤(W2+W3) / W1≤0.

075.

6. The electrolyte for lithium secondary battery according to any one of claims 1 to 5, characterized in that Based on the total mass of the electrolyte, the mass percentage W2 of the first additive is 0.01% to 10%.

7. The electrolyte for lithium secondary battery according to any one of claims 1 to 6, characterized in that Based on the total mass of the electrolyte, the mass percentage W2 of the first additive is 0.05% to 5%.

8. The electrolyte for lithium secondary battery according to any one of claims 1 to 7, characterized in that Based on the total mass of the electrolyte, the mass percentage W3 of the second additive is 0.05% to 10%.

9. The electrolyte for lithium secondary battery according to any one of claims 1 to 8, characterized in that Based on the total mass of the electrolyte, the mass percentage W3 of the second additive is 0.1% to 5%.

10. The electrolyte for lithium secondary battery according to any one of claims 1 to 9, characterized in that: The carboxylate solvent includes a compound represented by formula III; Wherein, R7 and R8 are independently selected from any one of C1-C3 alkyl and C1-C3 halogenated alkyl.

11. The electrolyte for lithium secondary battery according to claim 10, characterized in that: The carboxylate solvent includes one or more of the following compounds:

12. The electrolyte for lithium secondary battery according to any one of claims 1 to 11, characterized in that: The second additive includes one or more of vinylene carbonate, 4,5-diethylvinylene carbonate, fluoroethylene carbonate, and vinylethylene carbonate.

13. The electrolyte for lithium secondary battery according to any one of claims 1 to 12, characterized in that: The electrolyte satisfies at least one of the following (3) to (5): (3) The monofluorophosphate comprises lithium monofluorophosphate; (4) The difluorophosphate comprises lithium difluorophosphate; (5) The tetrafluoroborate includes lithium tetrafluoroborate.

14. The electrolyte for lithium secondary battery according to any one of claims 1 to 13, characterized in that: The oxalate borate includes a compound represented by formula IV; Among them, M1 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni; X1 is a halogen; m1 is an integer of 1 to 3; n1 is an integer of 0 to 4; a1, b1 and c1 are all positive integers.

15. The electrolyte for lithium secondary battery according to any one of claims 1 to 14, characterized in that: The malonate borate includes a compound shown in formula V; Among them, M2 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni; X2 is a halogen; m2 is an integer of 1 to 3; n2 is an integer of 0 to 4; a2, b2 and c2 are all positive integers.

16. The electrolyte for lithium secondary battery according to any one of claims 1 to 15, characterized in that: The oxalophosphate includes a compound shown in formula VI; Among them, M3 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni; X3 is a halogen; m3 is an integer from 1 to 3; n3 is an integer from 0 to 4; a3, b3 and c3 are all positive integers.

17. The electrolyte for lithium secondary battery according to any one of claims 1 to 16, characterized in that: The malonate phosphate includes a compound shown in formula VII; Wherein, M4 is selected from one or more of Li, Na, K, Rb, Cs, Mg, Ca, Ba, Al, Fe, Cu and Ni; X4 is a halogen; m4 is an integer from 1 to 3; n4 is an integer from 0 to 4; a4, b4, and c4 are all positive integers.

18. The electrolyte for lithium secondary battery according to any one of claims 1 to 17, characterized in that: The fluorosulfonate salt includes a compound represented by formula VIII; (FSO3) y M y+ Formula VIII Where y is a positive integer; M y+ is a metal ion or an organic cation; the metal ion includes Li + 、Na + , K + , Rb + , Cs + Mg 2+ , Ca 2+ , Ba 2+ 、Al 3+ , Fe 2+ , Cu 2+ , Fe 3+ 、Ni 2+ and Ni 3+ One or more of .

19. The electrolyte for lithium secondary battery according to any one of claims 1 to 18, characterized in that: The organic solvent further comprises one or more of chain carbonates and cyclic carbonates.

20. The electrolyte for lithium secondary battery according to claim 19, characterized in that: The electrolyte satisfies at least one of the following (6) to (7): (6) The linear carbonate comprises one or more of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl propyl carbonate and ethyl propyl carbonate; (7) The cyclic carbonate includes one or more of ethylene carbonate, propylene carbonate and butylene carbonate.

21. The electrolyte for lithium secondary battery according to any one of claims 1 to 20, characterized in that: The electrolyte salt includes one or more of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium bisfluorosulfonyl imide, lithium bistrifluoromethanesulfonyl imide, lithium trifluoromethanesulfonate, lithium difluorooxalatoborate, lithium bisoxalatoborate, lithium difluorobisoxalatophosphate, and lithium tetrafluorooxalatophosphate. 22 . A secondary battery comprising the electrolyte for a lithium secondary battery according to claim 1 .

23. The secondary battery according to claim 22, characterized in that: The secondary battery further comprises a negative electrode plate, wherein the negative electrode plate contains a negative electrode active material, and the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material is 10 -13 cm 2 / S~10 -10 cm 2 / S; Optionally, the lithium ion solid phase diffusion coefficient Ds of the negative electrode active material is 10 -12 cm 2 / S~10 -11 cm 2 / S.

24. The secondary battery according to claim 22 or 23, characterized in that: The secondary battery further comprises a negative electrode plate, wherein the negative electrode plate contains a negative electrode active material, and the volume average particle size Dv50 of the negative electrode active material is ≥6 μm; Optionally, the volume average particle size Dv50 of the negative electrode active material is 15 μm to 20 μm.

25. The secondary battery according to any one of claims 22 to 24, characterized in that: The secondary battery further comprises a negative electrode plate, wherein the negative electrode plate contains a negative electrode active material, and the BET specific surface area of ​​the negative electrode active material is 0.5 m 2 / g~2.0m 2 / g; Optionally, the BET specific surface area of ​​the negative electrode active material is 0.8 m 2 / g~1.5m 2 / g.

26. The secondary battery according to any one of claims 22 to 25, characterized in that: The secondary battery further comprises a negative electrode plate, wherein the negative electrode plate contains a negative electrode active material, and the negative electrode active material comprises one or more of graphite and silicon-based materials.

27. An electrical device comprising the secondary battery according to any one of claims 22 to 26.

Citation Information

Patent Citations

  • High-voltage electrolyte and lithium ion battery using electrolyte

    CN104979589A

  • Electrolyte for high-capacity lithium ion battery, preparation method and lithium ion battery

    CN106299324A

  • Superlow-temperature lithium ion battery electrolyte and lithium ion battery using same

    CN108511800A

  • Electrolyte and battery containing electrolyte

    CN110148788A

  • Electrolyte and lithium ion battery comprising same

    CN112072180A