Oxidation-controlled high-pressure acid leaching process for nickel laterite ore, leachate and use of biomass
By using biomass as a reducing agent in the high pressure acid leaching method of laterite nickel ore, the high processing cost and resource consumption of hexavalent chromium ions in the high pressure acid leaching method are solved, and low-cost and environmentally friendly hexavalent chromium ions are achieved. Improve product quality and environmental safety.
Patent Information
- Application Number
- PCT/CN2023/115888
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-05
- Filing Date
- 2023-08-30
- Publication Date
- 2024-11-14
AI Technical Summary
The existing high-pressure acid leaching method of laterite nickel ore has problems such as high cost of reducing agents and resource consumption, especially the high cost of hexavalent chromium ions, which affects product quality and environment.
In the process of high-pressure acid leaching, biomass is used as a reducing agent, and the hexavalent chromium ions are reduced by reacting with hexavalent chromium ions and strong oxidizing metal ions to achieve low-cost and environmentally friendly hexavalent chromium ions removal.
It effectively reduces the content of hexavalent chromium ions in the leaching liquid, improves product quality, reduces resource consumption, and avoids environmental pollution, is cheap and requires no additional treatment.
Smart Images

Figure CN2023115888_14112024_PF_FP_ABST
Abstract
Description
Laterite nickel ore controlled oxidation high-pressure acid leaching process, leachate, and biomass application
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 5, 2023, with application number 202310513197.8 and invention name “Laterite Nickel Ore Controlled Oxidation High-Pressure Acid Leaching Process, Leachate, and Biomass Application”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present application belongs to the field of hydrometallurgy technology, and in particular relates to a controlled oxidation high-pressure acid leaching process method for laterite nickel ore, leachate, and biomass application. Background Art
[0003] Industrial processing methods for laterite nickel ore include reduction smelting, ammonia leaching, atmospheric pressure acid leaching, and high-pressure acid leaching. High-pressure acid leaching, a hydrometallurgical technique, is currently the most widely used method for controlled oxidation high-pressure acid leaching of laterite nickel ore due to its low energy consumption and high output. The most critical step in high-pressure acid leaching is the high-pressure acid leaching treatment, which primarily involves the reaction of sulfuric acid with the ore to produce a leachate containing various metal ions, which is then processed. However, due to the varying origins of laterite nickel ore, the composition and properties of the ore vary. Some oxidizing laterite nickel ores contain hexavalent chromium ions in the leachate after high-pressure acid leaching. These hexavalent chromium ions are often oxidized by highly oxidizing metal ions in the ore pulp. Hexavalent chromium ions are oxidizing and toxic. If left untreated, they can enter subsequent products, such as nickel and cobalt hydroxide, through subsequent processing steps, affecting product quality, increasing treatment costs for downstream manufacturers, and affecting the hexavalent chromium content in discharged wastewater.
[0004] Currently, the high-pressure acid leaching method for treating hexavalent chromium from laterite nickel ore primarily involves adding reducing agents such as ferrous sulfate, sodium sulfite, sodium metabisulfite, sulfur, pyrite, and coal to reduce and precipitate the hexavalent chromium. However, these reducing agents are often expensive and costly, and a significant portion is a non-renewable mineral resource. Furthermore, excessive addition of reducing agents such as sodium sulfite and metabisulfite can slowly release small amounts of toxic sulfur dioxide during the subsequent reaction, polluting the environment and impacting human health. Reducing agents such as pyrite and coal can also introduce harmful metallic impurities, impacting product quality. Technical issues
[0005] The purpose of this application is to provide a method for controlling oxidation of laterite nickel ore by high-pressure acid leaching, aiming to solve the technical problems existing in the prior art of high-pressure acid leaching for laterite nickel ore treatment, including high reducing agent cost and resource consumption. Technical Solutions
[0006] Another object of the present application is to provide a leachate, aiming to solve the problems of the presence of hexavalent chromium ions in the leachate of high-pressure acid leaching treatment of laterite nickel ore in the prior art, as well as the high cost and resource consumption of reducing the hexavalent chromium ions.
[0007] Another object of the present application is to provide an application of biomass in a high-pressure acid leaching process for laterite nickel ore, aiming to solve the technical problems existing in the prior art of high-pressure acid leaching for laterite nickel ore treatment, including high reducing agent cost and resource consumption.
[0008] To achieve the above application objectives, the technical solutions adopted in this application are as follows:
[0009] In a first aspect, the present application provides a method for controlled oxidation high-pressure acid leaching of laterite nickel ore, comprising the following steps:
[0010] subjecting the slurry comprising the laterite nickel ore to high pressure acid leaching;
[0011] A reducing agent is added before and / or during the high-pressure acid leaching treatment, and the reducing agent includes biomass.
[0012] The present invention utilizes a biomass-based reducing agent in the controlled oxidation high-pressure acid leaching process for laterite nickel ore. This agent effectively reacts with hexavalent chromium ions in the laterite nickel ore slurry, or further reacts with strongly oxidizing metal ions, to reduce these ions during high-pressure acid leaching. Furthermore, the present invention offers excellent reduction efficiency, is clean and environmentally friendly, is low-cost, requires no additional steps, and utilizes a renewable reducing agent.
[0013] In a second aspect, the present application provides a leachate prepared by the laterite nickel ore controlled oxidation high-pressure acid leaching process method of the present application.
[0014] The leachate of the present application is prepared by the controlled oxidation high-pressure acid leaching process method of laterite nickel ore of the present application, so the hexavalent chromium ion content in the leachate is low and does not require additional treatment. It can be used to produce high-quality nickel cobalt hydroxide and other products, and the cost of reducing the hexavalent chromium ions is low, which also saves resources.
[0015] In a third aspect, the present application provides the use of biomass in a high-pressure acid leaching method for laterite nickel ore.
[0016] The application of the biomass in the present application can be to use the reducing agent including the biomass in the high-pressure acid leaching method of laterite nickel ore. The reducing agent including the biomass can not only reduce hexavalent chromium ions, but also has low cost and saves resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments or descriptions of the prior art. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0018] FIG1 is a flow chart of a controlled oxidation high-pressure acid leaching process for laterite nickel ore according to an embodiment of the present application. Modes for Carrying Out the Invention
[0019] In order to make the technical problems, technical solutions and beneficial effects to be solved by this application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit this application.
[0020] In this application, the term "and / or" describes the relationship between associated objects, indicating that three possible relationships exist. For example, A and / or B can represent: A exists alone, A and B exist simultaneously, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0021] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can each be single or plural.
[0022] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution. Some or all of the steps can be executed in parallel or sequentially. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0023] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms unless the context clearly indicates otherwise.
[0024] The weights of the relevant components mentioned in the examples of this application may not only refer to the specific content of each component, but also represent the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally increased or decreased according to the examples of this application, it is within the scope disclosed in the examples of this application. Specifically, the mass in the examples of this application may be a mass unit known in the chemical industry, such as μg, mg, g, kg, etc.
[0025] The terms "first" and "second" are used solely for descriptive purposes to distinguish objects, such as substances, from one another and should not be understood to indicate or imply relative importance or to implicitly specify the quantity of the technical features being referred to. For example, without departing from the scope of the embodiments of this application, a first XX may also be referred to as a second XX, and similarly, a second XX may also be referred to as a first XX. Thus, features defined as "first" or "second" may explicitly or implicitly include one or more of such features.
[0026] Some terms in this application can be understood as follows:
[0027] High Pressure Leaching: refers to a hydrometallurgical process that can include multiple steps, including a high pressure acid leaching step.
[0028] High-Pressure Acid Leaching: A treatment step in which the mineral is reacted with acid.
[0029] Slurry: refers to a liquid mixture formed by adding water and other auxiliary materials to solid raw materials such as dry ore. In the embodiment of the present application, it refers to the slurry formed by adding water and other auxiliary materials to laterite nickel ore raw materials.
[0030] Leachate: refers to the solution extracted from the slurry after the slurry is subjected to high-pressure acid leaching treatment.
[0031] In a first aspect, the present invention provides a method for controlling oxidation of laterite nickel ore using high-pressure acid leaching. The method of the present invention is shown in FIG1 and includes the following steps:
[0032] S10: subjecting the slurry including the laterite nickel ore to high pressure acid leaching;
[0033] Wherein, a reducing agent is added before and / or during the high-pressure acid leaching treatment, and the reducing agent includes biomass.
[0034] In the controlled oxidation high-pressure acid leaching process method for laterite nickel ore in the embodiment of the present application, a reducing agent is added before and / or during the high-pressure acid leaching treatment, and the reducing agent includes biomass, that is, the reducing agent can be biomass, or the reducing agent can be a substance containing biomass. Biomass here is a term used in the field of natural resources and belongs to renewable resources. In a broad sense, it refers to various organisms, including all animals, plants, and microorganisms, and of course also includes their products such as fruits, waste, etc., as well as products obtained by artificial processing and the remaining organic components. In this way, during the high-pressure acid leaching treatment, as the pressure and temperature of the reaction increase, elements contained in the biomass, such as fixed carbon in high-molecular polysaccharides, can reduce the strongly oxidizing metal ions and hexavalent chromium ions in the ore pulp. The reducing organic matter in the biomass plays a reducing role. In contrast, the reducing substances in pyrite, sulfur, chromite, etc. are mainly low-valent inorganic substances of elements such as sulfur and iron, and the reducing substances in coal are mainly fixed carbon and volatile matter. The process method of the embodiment of the present application has the following beneficial effects: ① After high-pressure acid leaching, the reducing organic matter in these biomasses is converted into substances such as water and carbon dioxide, which do not require additional treatment and will not pollute the environment or affect human health. The reducing agents such as sodium sulfite in the prior art will release sulfur dioxide during use and require additional treatment; ② The biomass in the embodiment of the present application is used as a reducing agent without introducing impurities and will not affect the purity and quality of the product, while the reducing agents in the prior art, especially the reducing agents such as pyrite, are difficult to avoid; ③ The biomass in the embodiment of the present application is widely available, renewable, and low-cost, while the reducing agents used in the prior art are expensive, and a considerable portion of them are non-renewable mineral resources; ④ The use of a reducing agent containing biomass in the embodiment of the present application does not affect the original process steps of the high-pressure acid leaching method, and is therefore suitable for practical application. However, the reducing agents in the prior art are often in block form and need to be crushed and ground into powder before they can be used in high-pressure acid leaching treatment, which adds extra steps, energy consumption and costs.
[0035] It should be noted that, as shown in FIG1 , the reducing agent is added in the embodiments of the present application before the high-pressure acid leaching treatment, during the high-pressure acid leaching treatment, or both. The steps before the high-pressure acid leaching treatment include, but are not limited to, steps such as grinding, slurry preparation, pre-mixing, and preheating, as performed by various manufacturers.
[0036] In some embodiments, the reducing agent can be added during slurry preparation. Slurry preparation generally requires thorough and uniform mixing of the raw ore with water, auxiliary materials, and the like. Therefore, adding the reducing agent during slurry preparation facilitates thorough and uniform mixing of the reducing agent and slurry, thereby enhancing the reducing effect during high-pressure acid leaching.
[0037] In some embodiments, biomass is added at a ratio of biomass dry weight to laterite nickel ore dry weight greater than 0:1 and less than or equal to 0.01:1. Adding biomass at these ratios facilitates sufficient reduction of strongly oxidizing metal ions and hexavalent chromium ions by the reducing agent during high-pressure acid leaching, while also preventing excessive biomass addition and wasteful resource consumption. Examples of these ratios include, but are not limited to, 0.0001:1, 0.001:1, 0.005:1, and 0.01:1.
[0038] In some embodiments, biomass may include but is not limited to at least one of sawdust, humus, and sugarcane residue. These biomasses are widely available, renewable, low-priced, low-cost, and can save resources, turn waste into treasure, and will not introduce impurities. Moreover, after high-pressure acid leaching, the organic components therein are converted into substances such as carbon dioxide and water, which do not require additional treatment, and can efficiently and fully reduce strong oxidizing metal ions and hexavalent chromium ions. When these biomasses are used as reducing agents in the embodiments of the present application, they can be used alone or in combination of two or more. In addition, generally speaking, these biomasses have smaller particle sizes than the reducing agents used in the prior art, or the organic matter in the biomass is easily processed into additives suitable for high-pressure acid leaching treatment conditions, while the blocky inorganic reducing agents used in the prior art require additional processing steps such as crushing and grinding, which increases energy consumption and cost. The biomass in the embodiments of the present application may also include but is not limited to fruit residues such as apple pomace, coconut shell residue, as well as rice husks, straw, and the like.
[0039] When biomass contains sawdust, this generally refers to the residue left over from wood processing, including sawdust and wood shavings, primarily composed of cellulose. In some embodiments, the sawdust particle size can be ≤3 mm. Controlling the sawdust particle size within this range not only meets the particle size requirements of high-pressure acid leaching, but also increases the contact area between the sawdust and the strongly oxidizing metal ions and hexavalent chromium ions in the slurry, thereby more efficiently and fully exerting the reducing effect during high-pressure acid leaching and allowing for sufficient reaction with the strongly oxidizing metal ions and hexavalent chromium ions. In exemplary embodiments, the sawdust particle size may include, but is not limited to, 0.5 mm, 1 mm, 1.5 mm, 2 mm, and 3 mm.
[0040] When biomass contains humus, the humus is also called humus soil, which generally contains grass roots, tree bark, dead branches and leaves, or their long-term decay and fermentation substances. It is widely present in the topsoil layer of forests and grasslands, and may also contain organic waste (such as kitchen waste) or its fermented substances. Therefore, it is widely available and inexpensive. In addition, the surface soil layer of laterite nickel mining areas contains these humus soils, so they can be obtained locally.
[0041] When the biomass contains sugarcane bagasse, the residue left after sugarcane is extracted, in some embodiments, the particle size of the bagasse can be ≤3 mm. Controlling the bagasse particle size within this range not only meets the particle size requirements of high-pressure acid leaching, but also allows bagasse of this size to effectively and efficiently reduce strongly oxidizing metal ions and hexavalent chromium ions. In exemplary embodiments, the particle size of the sawdust can include, but is not limited to, 0.5 mm, 1 mm, 1.5 mm, 2 mm, and 3 mm.
[0042] In some embodiments, the acid-to-ore ratio for high-pressure acid leaching can be 180-450 kg / t. Acid-to-ore ratio is an industry term that refers to the ratio of the mass of acid required to react with the slurry to the mass of the dry weight components in the slurry under complete reaction conditions. Controlling the acid-to-ore ratio for high-pressure acid leaching within this range facilitates the full reaction of the slurry components into solutions of sulfates, such as nickel, cobalt, and manganese. This ensures that the acid fully penetrates the minerals in the slurry, converting the desired metal elements into ions and ensuring efficient utilization of the raw materials. Furthermore, the metal ions can better interact with the biomass, enhancing the reducing effect of the bioorganic matter and reducing strongly oxidizing metal ions and hexavalent chromium ions. In exemplary embodiments, the acid-to-ore ratio may include, but is not limited to, 180 kg / t, 250 kg / t, 300 kg / t, 350 kg / t, 400 kg / t, and 450 kg / t.
[0043] In some embodiments, the high-pressure acid leaching temperature can be ≥ 240°C. Controlling the high-pressure acid leaching temperature to no less than 240°C can, on the one hand, improve the efficiency and extent of the reaction between the acid and the pulp during the acid leaching process, and on the other hand, more effectively render elements such as fixed carbon in the biomass reducible, enabling them to act as reducing agents, effectively reducing strongly oxidizing metal ions and hexavalent chromium ions. The temperature can further be 240-280°C to avoid excessively high temperatures that increase energy consumption. In exemplary embodiments, the high-pressure acid leaching temperature may include, but is not limited to, 240°C, 250°C, 260°C, 280°C, etc.
[0044] In some embodiments, the pressure of the high-pressure acid leaching process can be ≥3.0 MPa. Controlling the high-pressure acid leaching pressure to no less than 3.0 MPa can, on the one hand, improve the efficiency and extent of the reaction between the acid and the slurry during the acid leaching process, and on the other hand, more effectively enhance the reducibility of elements such as fixed carbon in the biomass, allowing it to act as a reducing agent, effectively reducing strongly oxidizing metal ions (such as high-valent manganese ions) and hexavalent chromium ions. The pressure can further be 3.0-6.0 MPa to avoid excessive pressure and increased energy consumption. In exemplary embodiments, the high-pressure acid leaching pressure may include, but is not limited to, 3.0 MPa, 4.0 MPa, 4.5 MPa, 5.0 MPa, and 6 MPa.
[0045] In some embodiments, the high-pressure acid leaching treatment time can be 0.5 to 2 hours. Controlling the high-pressure acid leaching treatment time to these values allows for sufficient reaction between the acid, slurry, and biomass, ensuring that the biomass effectively reduces strongly oxidizing metal ions and hexavalent chromium ions. In exemplary embodiments, the high-pressure acid leaching treatment time may include, but is not limited to, 0.5 hours, 1 hour, 1.5 hours, and 2 hours.
[0046] In some embodiments, the hexavalent chromium ion content in the leachate obtained after high-pressure acid leaching can be less than 0.1 g / L. In actual production, due to the complex factors affecting the redox properties of laterite nickel ore, the amount of reducing agent added is difficult to precisely control. Ideally, no hexavalent chromium ions are detectable in the leachate (typically using a colorimetric method with a detection limit of 0.1 mg / L). In reality, the leachate may contain a small amount of hexavalent chromium, or ferrous iron may be present due to overreduction. In actual production, hexavalent chromium and ferrous iron in the leachate are typically analyzed, and secondary precise redox control is performed in subsequent steps. Therefore, in the embodiments of the present application, the hexavalent chromium ion content in the leachate can be required to be less than 0.1 g / L (100 mg / L, 100 ppm). In exemplary embodiments, the hexavalent chromium ion content requirement can be less than 0.005 mg / L, 0.01 mg / L, 0.1 mg / L, 1 mg / L, 10 mg / L, or 100 mg / L. A preferred limit is less than 0.1 mg / L.
[0047] Furthermore, for the leachate obtained from high-pressure acid leaching, industry professionals can also set up corresponding subsequent processing steps based on the final product to be produced. For example, to produce nickel cobalt hydroxide, the leachate can be subjected to a series of steps, including cyclic leaching and neutralization, CCD countercurrent washing, iron and aluminum removal, and nickel cobalt hydroxide precipitation.
[0048] In a second aspect, an embodiment of the present application provides a leachate prepared by the controlled oxidation high-pressure acid leaching process method of laterite nickel ore according to an embodiment of the present application.
[0049] The leachate of the embodiment of the present application is produced by the controlled oxidation high-pressure acid leaching process method of laterite nickel ore of the embodiment of the present application, so the hexavalent chromium ion content in the leachate is low and does not require additional treatment. It can be used to produce high-quality nickel cobalt hydroxide and other products, and the cost of reducing the hexavalent chromium ions is low, which also saves resources.
[0050] In a third aspect, the embodiments of the present application provide the application of biomass in the high-pressure acid leaching method of laterite nickel ore.
[0051] The application of biomass in the embodiment of the present application can be to use a reducing agent including biomass in a high-pressure acid leaching process for laterite nickel ore. Specifically, the reducing agent can be added before and / or during the high-pressure acid leaching process. In this way, the reducing agent including biomass can not only reduce hexavalent chromium ions, but also has low cost and saves resources.
[0052] The following describes the details in conjunction with specific embodiments.
[0053] Example 1
[0054] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0055] The steps include:
[0056] S1. Premix
[0057] The raw laterite nickel ore contains the following components: Ni 1.46%, Fe 44.41%, Mn 1.03%, Cr 1.64%, and Mg 0.92%. The raw ore is made into a slurry, and wood chips with a particle size of 1 to 2 mm are added to the slurry as a biomass reducing agent. The added weight is based on a ratio of 1:500 of dry weight of wood chips to dry weight of the raw ore, that is, 0.2%;
[0058] S2. High-pressure acid leaching
[0059] The ore pulp obtained after the above steps was subjected to high-pressure acid leaching treatment at a reaction acid-ore ratio of 260 kg / t, a reaction temperature of 260° C., a reaction pressure of 4.5 MPa, and a reaction time of 1 hour to obtain a leachate.
[0060] Example 2
[0061] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0062] The steps include:
[0063] S1. Premix
[0064] The raw laterite nickel ore contains the following components: Ni 1.15%, Fe 42.03%, Mn 0.82%, Cr 2.11%, Mg 0.50%. The raw ore is made into slurry;
[0065] S2. High-pressure acid leaching
[0066] The slurry is subjected to high-pressure acid leaching treatment, and sawdust with a particle size of 1.5 to 2.5 mm is added as a biomass reducing agent during the treatment process. The added weight is based on a ratio of the dry weight of the sawdust to the dry weight of the original ore of 1:500, i.e. 0.2%. The reaction acid-ore ratio is 250 kg / t, the reaction temperature is 250°C, the reaction pressure is 4 MPa, and the reaction time is 2 hours to obtain a leachate.
[0067] Example 3
[0068] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0069] The steps include:
[0070] S1. Premix
[0071] The raw laterite nickel ore contains the following components: Ni 1.32%, Fe 40.03%, Mn 0.90%, Cr 1.91%, Mg 1.53%; the raw ore is made into slurry;
[0072] S2. High-pressure acid leaching
[0073] The slurry is subjected to high-pressure acid leaching treatment, and wood chips with a particle size of 0.5 to 2 mm are added as a biomass reducing agent before and during the treatment. The total added weight is 1:500, i.e. 0.2%, based on the ratio of the dry weight of the wood chips to the dry weight of the original ore. The reaction acid-ore ratio is 280 kg / t, the reaction temperature is 270°C, the reaction pressure is 5 MPa, and the reaction time is 1 hour to obtain a leachate.
[0074] Example 4
[0075] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0076] The only difference between the steps and Example 1 is that the sawdust in step S1 is replaced with cane sugar residue with a particle size of 1 to 2 mm as the reducing agent, and the added amount keeps the dry weight ratio consistent.
[0077] Example 5
[0078] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0079] The only difference between the steps and Example 1 is that the sawdust in step S1 is replaced by a mixture of sawdust with a particle size of 1 to 2 mm and sugarcane residue with a particle size of 1 to 2 mm as the reducing agent, and the total added amount keeps the dry weight ratio consistent.
[0080] Example 6
[0081] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0082] The only difference between the steps and Example 1 is that the weight of sawdust added in step S1 is changed to a ratio of 1:4999 of the dry weight of sawdust to the dry weight of the original ore, i.e. 0.02%.
[0083] Comparative Example 1
[0084] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0085] The only difference between the steps and Example 1 is that the sawdust is added into the leachate after step S2 instead of being added into step S1.
[0086] Comparative Example 2
[0087] Controlled oxidation high-pressure acid leaching process method for laterite nickel ore and leachate
[0088] The only difference between the steps and Example 1 is that no reducing agent is added in step S1.
[0089] Related tests and result analysis
[0090] The leaching solutions of Examples 1 to 6 and Comparative Examples 1 to 2 were taken and the Cr 6+ The detection limit of the colorimetric method is 0.1 mg / L.
[0091] The above results are summarized in the following Table 1.
[0092] Case Reducing agent Reducing agent particle size / mm Addition steps Reducing agent dry weight to ore dry weight ratio High pressure acid leaching temperature / ℃ High pressure acid leaching pressure / MPa Reaction acid ore ratio / kg / t Leachate Cr 6+ Content / mg / L Example 1 Sawdust 1-2S10.2%2604.5260 Not detected Example 2 Sawdust 1.5-2.5S20.2%2504250 Not detected Example 3 Sawdust 0.5-2S1, S20.2%2805280 Not detected Example 4 Sugarcane residue 1-2S10.2%2604.5260 Not detected Example 5 Sawdust + Sugarcane residue 1-2S10.2%2604.5260 Not detected Example 6 Sawdust 1-2S10.02%2604.526060 Comparative Example 1 Sawdust 1-2S2 after 0.2%2604.5260290 Comparative Example 2 / / / / 2604.5260300
[0093] Table 1
[0094] As can be seen from Table 1, compared with Comparative Example 1 and Comparative Example 2, the amount of the biomass-containing reducing agent added in Examples 1 to 6 of the present application can be selected according to the dry weight ratio of the original ore, and the content of hexavalent chromium ions in the leachate after high-pressure acid leaching is significantly reduced. In addition, the selection of an appropriate amount of the biomass-containing reducing agent added in Examples 1 to 5 can further reduce the hexavalent chromium ion content in the leachate until it cannot be detected by colorimetry.
[0095] In combination with Examples 1 to 6 and Comparative Example 1, it can be seen that in the embodiments of the present application, the biomass-containing reducing agent needs to be added before and / or during the high-pressure acid leaching treatment in order to utilize the high temperature and high pressure conditions of the high-pressure acid leaching treatment to achieve a better reduction effect.
[0096] It can be seen from Examples 1 to 6 that various biomasses can be used alone or in combination, and can all play the role of reducing agents.
[0097] It can be seen from Examples 1 to 6 that, compared with Example 6, Examples 1 to 5 can further improve the reduction effect of hexavalent chromium ions and reduce the content of hexavalent chromium ions in the leachate by selecting a suitable addition amount.
[0098] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent replacements and improvements made within the spirit and principles of the present application should be included in the scope of protection of the present application.
Claims
1. Controlled oxidation high pressure acid leaching process for laterite nickel ore, It is characterized in that The steps include: subjecting the ore slurry including the laterite nickel ore to high pressure acid leaching; A reducing agent is added before and / or during the high pressure acid leaching treatment, and the reducing agent includes biomass.
2. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to claim 1, Features: The reducing agent is added when preparing the ore slurry.
3. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to claim 1 or 2, Features: The biomass is added in a ratio of the dry weight of the biomass to the dry weight of the laterite nickel ore that is greater than 0:1 and less than or equal to 0.01:
1.
4. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to claim 1 or 2, Features: The biomass includes at least one of wood chips, humus, sugarcane residue, apple residue, coconut shell residue, rice husk and straw.
5. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to claim 4, Features: The particle size of the wood chips is ≤3 mm.
6. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to claim 4, Features: The particle size of the sugarcane residue is ≤3 mm.
7. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to any one of claims 1, 2, 5 or 6, Features: The conditions of the high pressure acid leaching treatment include at least one of the following (1) to (4): (1) Acid-ore ratio is 180-450 kg / t; (2) The reaction temperature is 240-280°C; (3) The reaction pressure is 3.0-6.0 MPa; (4) The reaction time is 0.5 to 2 hours.
8. The method for controlled oxidation high pressure acid leaching of laterite nickel ore according to any one of claims 1, 2, 5 or 6, Features: In the leaching solution obtained after the high-pressure acid leaching treatment, the hexavalent chromium ion content is less than 0.1 g / L.
9. Leachate, Features: The product is prepared by the controlled oxidation high pressure acid leaching process of laterite nickel ore as described in any one of claims 1 to 8.
10. Application of biomass in high pressure acid leaching of laterite nickel ore.
Citation Information
Patent Citations
Method for leaching nickel-cobalt from low-grade laterite nickel ore
CN101255494A
Method for reducing hexavalent chromium in laterite-nickel ore high-pressure acid leaching process
CN113481365A
Nickel smelting process
JP2005281733A