Multi-component copolyester and preparation method therefor
By using initial depolymerization, repolymerization, esterification and polycondensation steps in regenerated PBAT, the heavy metal ions are removed by chelating agents, and a multi-copolyester with low heavy metal content is produced, which solves the high heavy metal and poor printing performance in the prior art. The problem has improved the biodegradable performance and application range.
Patent Information
- Application Number
- PCT/CN2024/091562
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-14
AI Technical Summary
The existing recycled PBAT has high heavy metal content and poor printing performance, which limits its application range, and is high in production costs and slow in biodegradation performance.
Using a preparation method of multi-polymerized copolyester, through the initial depolymerization, re-depolymerization, esterification and polycondensation steps, waste polyester is used as raw material, and chelating agent is added to remove heavy metal ions, so as to produce zinc content ≤100ppm and titanium content ≤ 120ppm multi-copolyester has good crystallinity and printing properties.
It achieves extremely low heavy metal content and good printing performance in multi-copolyesters, improves biodegradable properties, and is suitable for disposable packaging films and agricultural film fields.
Smart Images

Figure CN2024091562_14112024_PF_FP_ABST
Abstract
Description
A kind of multi-component copolyester and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of recycled polyester, in particular to a multi-component copolyester and a preparation method thereof. Background Art
[0002] Currently, biodegradable plastics account for approximately 58% of global plastic production, while non-degradable plastics account for 42%. The disposal of waste plastics is an urgent issue. In the future, my country will gradually address the environmental hazards posed by traditional waste plastic disposal through methods such as source reduction, reuse, the use of bio-based or biodegradable plastics instead of fossil-based materials, and plastic recycling through physical or chemical recovery. Chemical recycling primarily produces monomers and oligomers such as DMT, TPA, EG, BHET, and BHETA, while secondary products primarily include synthetic PET, UPR, ERD, VER, AR, PU, UPP, NPS, PIF, OP, AD, and PBAT.
[0003] Polybutylene terephthalate-adipate (PBAT) is a fully biodegradable polyester. Due to its excellent toughness, film-forming properties, and easy blowability, it has been widely used in the fields of disposable packaging films and agricultural films. In the prior art, some reports have been published on the preparation of recycled PBAT. For example, Chinese patent application CN112724388A discloses a production device for recycling polyester into the biodegradable material PBAT. The dried recycled PET is subjected to alcoholysis in an alcoholysis reaction system to obtain crude BHET. This is then subjected to a dealcoholization system to obtain BHET monomer. This is reacted with BDO in a first esterification reaction system to obtain BHBT monomer. This is then reacted with AA ester in a second esterification reaction system to obtain a copolyester. This is then polycondensed in a pre-polycondensation reaction system and a final polycondensation reaction system to increase the weight-average molecular weight to obtain the PBAT product. However, PBAT has poor strength, especially low tensile strength. PBAT usually requires the addition of calcium powder or blending with PLA to achieve better physical properties. During use, PBAT suffers from problems such as mechanical properties that fail to meet user requirements, limiting its application range.
[0004] There are prior art reports on modifying PBAT to produce multi-component copolyesters to improve the mechanical properties of the material. For example, CN 112080000 A discloses a method for synthesizing poly(terephthalic acid-adipate-meta-epoxypentadecylphenol) butanediol (PBATE material). The PBATE material is synthesized from PBAT and meta-epoxypentadecylphenol, and the mechanical properties of the material are superior to those of PBAT. CN 113861399 A discloses a biodegradable polyester poly(adipate-terephthalate-isosorbide-butylene glycol) (PBIAT) and its preparation method. The preparation method comprises uniformly mixing 27-23% adipic acid, 31-26% terephthalic acid, 6-48% isosorbide, and 36-3% butanediol in a reactor, reacting the mixture, and then adding a catalyst and raising the temperature to carry out a polycondensation reaction to obtain PBIAT polyester. However, the multi-component copolyesters reported in the prior art are not made from waste polyester.
[0005] In addition, for recycled PBAT copolyesters, existing technology (Zhang Hongming, Zhao Junyu, Gao Fengxiang, et al. Research on the "One-Pot" Synthesis of Biodegradable Polymers by Depolymerization-Cocondensation of PET [J]. Acta Polymerica Sinica, 2022(009):053) uses diols of different structures to hydrolyze PET into low-molecular-weight prepolymers, and then adds dibasic acids for further esterification and polycondensation, completing the PET depolymerization and copolymerization reactions in a "one-pot" process. However, since recycled materials often contain varying levels of heavy metals, and heavy metal catalysts are also used in the depolymerization process, catalyst residues can seriously affect the physical properties and aging resistance of the product. Current petroleum-based biodegradable plastics such as PBAT have high production costs and relatively slow biodegradability. Moreover, since PBAT is primarily used in packaging bags, which generally require printing with patterns, designs, or text, poor printing performance can lead to easy discoloration of the ink, thus affecting the appearance and safety of the packaging bags.
[0006] Therefore, it is necessary to provide a multi-component copolyester, which has low residual heavy metal content, better degradation performance, better toughness and tensile strength, low carbon emission value, and better printing performance.
[0007] Summary of the Invention
[0008] The purpose of the present invention is to overcome the defects of the prior art such as high heavy metal content and poor printing performance, and to provide a multi-component copolyester.
[0009] Another object of the present invention is to provide a method for preparing the above-mentioned multi-component copolyester.
[0010] To achieve the above object, the present invention adopts the following technical solutions:
[0011] A multi-component copolyester, comprising:
[0012] Component A, the dicarboxylic acid compound, based on the total molar amount of component A, comprises:
[0013] a1, 35 to 65 mol% of at least one aliphatic dicarboxylic acid;
[0014] a2, 35 to 65 mol% of at least one aromatic dicarboxylic acid or a derivative thereof;
[0015] Component B, 1,4-butanediol;
[0016] Component C, a third monomer, based on the total molar amount of component B and component C, the component C accounts for 5 to 30 mol%; the third monomer is at least one of ethylene glycol, 1,4-cyclohexanedimethanol, and isosorbide;
[0017] The crystallinity of the multi-component copolyester is 5-22%, including but not limited to 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, and 22%; the zinc content in the multi-component copolyester is ≤100ppm, and the titanium content is ≤120ppm.
[0018] The monomers of the multi-component copolyester of the present invention include an aliphatic-aromatic dicarboxylic acid compound, 1,4-butanediol, and a small amount of a third monomer. The copolyester has an extremely low metal ion content, with a zinc content of ≤100 ppm and a titanium content of ≤120 ppm, and a crystallinity of 5 to 22%. The copolyester exhibits good biodegradability, tensile strength, and printability.
[0019] The zinc and titanium residues in the multi-component copolyester of the present invention are introduced by the catalyst used in the depolymerization and polycondensation processes, and are also introduced by impurities in the waste polyester raw materials.
[0020] Preferably, the zinc content in the multi-component copolyester is 45-70 ppm, and the titanium content is 50-105 ppm.
[0021] Preferably, the calcium content in the multi-component copolyester is ≤71 ppm.
[0022] More preferably, the calcium content in the multi-component copolyester is 35 to 60 ppm.
[0023] Preferably, the silicon content in the multi-component copolyester is ≤85ppm.
[0024] More preferably, the silicon content in the multi-component copolyester is 35 to 50 ppm.
[0025] The residual calcium and silicon in the multi-component copolyesters are mainly due to the introduction of impurities in the polyester raw materials.
[0026] In the present invention, the crystallinity of the multi-component copolyester is analyzed using an X-ray diffractometer (XRD) according to the standard JY / T0587-2020. Specifically, a D8 ADVANCE X-ray diffractometer from BRUKER, Germany, is used at room temperature, with Cu Ka radiation (λ = 0.154 nm) collected every 0.05°, and a scanning angle range of 6° to 60°.
[0027] In the present invention, the zinc content and titanium content are tested according to the following method:
[0028] Inductively coupled plasma optical emission spectrometry (ICP-OES) was used according to the standard inductively coupled plasma atomic emission spectrometry method US EPA 6010C:2014.
[0029] Preferably, the melting point of the multi-component copolyester is 105-140°C, including but not limited to 105°C, 107°C, 109°C, 111°C, 113°C, 115°C, 117°C, 119°C, 121°C, 123°C, 125°C, 127°C, 129°C, 131°C, 133°C, 135°C, 137°C, 139°C, and 140°C.
[0030] The melting point of the multi-component copolyester was tested using a differential scanning calorimeter in accordance with the standard ISO 11357-3:2018.
[0031] Preferably, the relative viscosity of the multi-component copolyester is 1.2 to 1.8, including but not limited to 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, and 1.8.
[0032] The relative viscosity of the multi-component copolyester is tested as follows:
[0033] According to the standard method of GB / T 17931-1999, the sample concentration was 5 mg / ml in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05°C.
[0034] Preferably, the terminal carboxyl content of the multi-component copolyester is 13 to 30 mmol / t, including but not limited to 13 mmol / t, 14 mmol / t, 15 mmol / t, 16 mmol / t, 17 mmol / t, 18 mmol / t, 19 mmol / t, 20 mmol / t, 21 mmol / t, 22 mmol / t, 23 mmol / t, 24 mmol / t, 25 mmol / t, 26 mmol / t, 27 mmol / t, 28 mmol / t, 29 mmol / t, and 30 mmol / t.
[0035] The terminal carboxyl content is tested as follows:
[0036] The terminal carboxyl content was tested according to standard FZ / T 50012-2006 using automatic potentiometric titration analysis.
[0037] Preferably, the weight average molecular weight of the multi-component copolyester is 40,000 to 100,000, including but not limited to 40,000, 45,000, 50,000, 55,000, 60,000, 65,000, 70,000, 75,000, 80,000, 85,000, 90,000, 95,000, and 100,000.
[0038] The weight average molecular weight is tested as follows:
[0039] According to the standard GB / T 21863-2008 gel permeation chromatography (GPC), an ultra-high performance polymer chromatograph (APC) was used, tetrahydrofuran was used as the eluent, a differential detector was used as the detector, the column temperature was 40°C, and the flow rate was 0.5 mL / min.
[0040] Preferably, the aliphatic dicarboxylic acid is selected from at least one of malonic acid, succinic acid, adipic acid, sebacic acid, pimelic acid, suberic acid, and azelaic acid, and the aromatic dicarboxylic acid or its derivative is selected from at least one of terephthalic acid or its derivative, and isophthalic acid or its derivative.
[0041] The present invention also provides a method for preparing the above-mentioned multi-component copolyester, comprising the following steps:
[0042] S1. Initial depolymerization:
[0043] Dissolving waste terephthalic acid polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product;
[0044] The temperature of the initial depolymerization reaction is 180-230°C and the time is 15-120 minutes;
[0045] S2. Re-disaggregation:
[0046] Extracting a portion of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions. After filtering the reactants, the obtained filtrate is the re-depolymerization product;
[0047] The temperature of the re-depolymerization reaction is 160-190° C. and the time is 10-20 minutes;
[0048] S3. Esterification reaction:
[0049] According to the monomer content of the multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer, and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender, and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield reaches 90% to obtain an esterified product;
[0050] S4. Polycondensation:
[0051] After removing excess alcohol solvent from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum conditions to obtain the multi-component copolyester.
[0052] The preparation method of the multi-component copolyester of the present invention uses waste polyester as raw material and prepares the multi-component copolyester with low heavy metal content and suitable crystallinity through the steps of two alcoholysis, esterification reaction and polycondensation.
[0053] In the primary depolymerization step, the waste polyester undergoes initial depolymerization in the presence of a depolymerization catalyst under normal pressure, an inert gas atmosphere, and microwave conditions. The temperature of the initial depolymerization reaction is relatively high, allowing the majority of the waste polyester to be depolymerized into monomers or oligomers. Ethylene glycol is then removed from the initial depolymerization product, and a chelating agent is added before a second depolymerization, or secondary depolymerization, is performed. The secondary depolymerization occurs at a lower temperature and for a shorter period of time than the initial depolymerization. The chelating agent simultaneously removes most of the heavy metal ions from the waste polyester during the secondary depolymerization process, and the addition of the chelating agent does not negatively impact the polyester's printing properties or crystallinity.
[0054] In the preparation method of the present invention, a portion of the diol is extracted in step S2, which is a depolymerization byproduct, and an aliphatic dicarboxylic acid and a third monomer are added in step S3, both to obtain a multi-component copolyester with an appropriate monomer content. The monomer content of the resulting multi-component copolyester satisfies the following range: Component A, a dicarboxylic acid compound, comprising: a1, 35-65 mol% of at least one aliphatic dicarboxylic acid, based on the total molar weight of component A; a2, 35-65 mol% of at least one aromatic dicarboxylic acid or its derivative; component B, 1,4-butanediol; and component C, a third monomer, comprising 5-30 mol% of component C, based on the total molar weight of components B and C.
[0055] The method for extracting part of the ethylene glycol in step S2 may be vacuum distillation.
[0056] Preferably, the waste polyester includes one or more of recycled polyethylene terephthalate (PET), polybutylene terephthalate (PBT), PET / PBT alloy, and PBAT.
[0057] Optionally, sources of the waste polyester include but are not limited to post-consumer recycled plastics (PCR), post-industry recycled plastics (PIR), ocean-bound plastics (OBP), and in-the-ocean plastics (IOP).
[0058] Preferably, the waste polyester further includes the steps of impurity removal, cleaning and crushing before the initial depolymerization.
[0059] Preferably, in step S2, the chelating agent is a biomass chelating agent.
[0060] Preferably, the chelating agent includes at least one of stearyl citrate, calcium citrate, tea polyphenols, and phytic acid.
[0061] More preferably, the chelating agent is tea polyphenols.
[0062] Tea polyphenols as a chelating agent can not only efficiently complex residual metal ions in waste polyester, but also help stabilize the reaction system and reduce yellowing of the product for multi-component copolyesters.
[0063] Preferably, in step S2, the amount of the chelating agent added is 0.01 to 0.1 wt.% of the waste polyester.
[0064] The chelating agent can be added in a relatively low amount to effectively remove metal ions from waste polyester.
[0065] Preferably, in step S1, the depolymerization catalyst includes at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate.
[0066] Preferably, in step S1, the amount of the depolymerization catalyst added is 0.05 to 0.5 wt.% of the waste polyester.
[0067] Preferably, the alcohol solvent includes at least one of 1,4-butanediol and ethylene glycol.
[0068] Preferably, the mass ratio of the waste polyester to the alcohol solvent is 1:0.8 to 1:2.
[0069] Preferably, the polymerization catalyst and the polycondensation catalyst are each independently selected from at least one of butyl titanate, tetraisopropyl titanate, titanium phosphorus compounds, titanium silicon compounds, titanium magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide.
[0070] Preferably, in step S3, the aliphatic dicarboxylic acid is adipic acid and / or sebacic acid.
[0071] Since the waste polyester is depolymerized in steps S1 and S2, some aliphatic alcohol already exists in the depolymerization product. In step S3, a certain amount of aliphatic alcohol is added to make the alcohol in the entire reaction system excessive.
[0072] The stabilizer is one or more of organic phosphites, trimethyl phosphates, and hindered phenols.
[0073] Optionally, the organic phosphite stabilizer may be one or more of trimethyl phosphite, triethyl phosphite or triphenyl phosphite.
[0074] Optionally, the phosphate stabilizer may be one or more of triphenyl phosphate, trimethyl phosphate or triethyl phosphate.
[0075] Optionally, the hindered phenol stabilizer may be 3,5-di-tert-butyl-4-hydroxybenzyl diethylphosphonate (antioxidant 1222) and / or antioxidant 1010.
[0076] The chain extender is at least one of pentaerythritol, trimethylolethane, trimethylolpropane (TMP), xylitol, sorbitol, HDI, MDI, TDI, isophorone diisocyanate, ethylene-methyl methacrylate copolymer (EMA), and multifunctional epoxy compound ADR.
[0077] Preferably, the added amount of the chain extender is 0 to 0.1 wt.% of the waste polyester.
[0078] Preferably, in step S3, the esterification reaction is carried out at a temperature of 170 to 210° C. and for a time of 1 to 2 hours.
[0079] Preferably, in step S3, the amount of the polymerization catalyst added is 0.01-0.1 wt.% of the waste polyester.
[0080] Preferably, in step S4, the amount of the polycondensation catalyst added is 0.03 to 0.1 wt.% of the waste polyester.
[0081] Preferably, in step S4, the temperature of the polycondensation reaction is 240-250° C., the time is 2-5 hours, and the pressure is 20-100 Pa.
[0082] Preferably, in step S1, the microwave reaction conditions are as follows: frequency 2450 Hz, temperature 180-230° C., and time 15-120 min.
[0083] Preferably, in step S2, the microwave reaction conditions are as follows: frequency 2450 Hz, temperature 160-190° C., and time 10-20 min.
[0084] Compared with the prior art, the present invention has the following beneficial effects:
[0085] The present invention develops a multi-component copolyester and a preparation method thereof. The multi-component copolyester of the present invention uses waste polyester as raw material and is prepared through the steps of primary alcoholysis, secondary alcoholysis, esterification reaction and polycondensation to obtain a multi-component copolyester with low heavy metal content and suitable crystallinity.
[0086] The primary depolymerization and re-depolymerization are carried out under microwave conditions, wherein the re-depolymerization includes the addition of a chelating agent. The addition of the chelating agent and the re-depolymerization reaction synergistically remove most of the metal ion residues in the waste polyester. The obtained multi-component copolyester has an extremely low heavy metal content, wherein the zinc content is ≤100ppm and the titanium content is ≤120ppm.
[0087] Since the multi-component copolyester of the present invention has an extremely low heavy metal content and a good crystallinity range, the obtained multi-component copolyester has excellent printing performance and good biodegradability, and can be widely used in the fields of disposable packaging films and agricultural films. BRIEF DESCRIPTION OF THE DRAWINGS
[0088] FIG1 is an infrared spectrum of the multi-component copolyester of Example 1;
[0089] FIG2 is a hydrogen nuclear magnetic spectrum of the multi-component copolyester of Example 1;
[0090] FIG3 is an XRD pattern of the multi-component copolyester of Example 1;
[0091] FIG4 is a GPC chart of the multi-component copolyester of Example 1. DETAILED DESCRIPTION
[0092] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any form.
[0093] The raw materials in the examples and comparative examples of the present invention can be obtained commercially;
[0094] in:
[0095] Waste polyester-1, PET, recycled from electronic pallet materials;
[0096] Waste polyester-2, rPET-pellet, recycled from Indonesian ocean plastic;
[0097] Waste polyester-3, PET / PBT, recycled PET / PBT alloy;
[0098] Waste polyester-4, PBAT, recycled PBAT waste;
[0099] Condensation catalyst and polymerization catalyst: butyl titanate, purchased from Aladdin;
[0100] Depolymerization catalyst: zinc acetate, purchased from Aladdin;
[0101] Chain extender: trimethylolpropane;
[0102] Chelating agents: tea polyphenols, stearyl citrate, and phytic acid, all purchased from Maclean;
[0103] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.
[0104] Examples 1 to 4
[0105] Examples 1 to 4 provide a method for preparing a multi-component copolyester, respectively, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 1:
[0106] S1. Initial depolymerization:
[0107] Waste polyester with an average particle size of ≤2 mm was dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction in a nitrogen atmosphere under microwave conditions to obtain a primary depolymerization product; the microwave conditions were: a frequency of 2450 Hz.
[0108] S2. Re-disaggregation:
[0109] A portion of the diol is extracted from the primary depolymerization product obtained in step S1 by vacuum distillation, and a chelating agent is added. The product is placed in a microwave reactor and subjected to a re-depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions. The reactant is filtered to obtain a filtrate as the re-depolymerization product. The microwave conditions are: a frequency of 2450 Hz.
[0110] S3. Esterification reaction:
[0111] According to the monomer content of the target multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer, and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender, and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield reaches 90% to obtain an esterified product;
[0112] S4. Polycondensation:
[0113] After removing excess alcohol from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum conditions to obtain the multi-component copolyester.
[0114] Table 1 Raw materials and reaction conditions of Examples 1 to 4
[0115] Examples 5 to 10
[0116] Examples 5 to 10 provide a method for preparing a multi-component copolyester. Except for step S2, the other steps are the same as those in Example 1. Specifically, the preparation methods of Examples 5 to 10 differ from those of Example 1 in that:
[0117] In Example 5, the type of chelating agent is tea polyphenols;
[0118] In Example 6, the type of chelating agent is stearyl citrate;
[0119] In Example 7, the proportion of the chelating agent to the waste polyester is 0.01 wt.%;
[0120] In Example 8, the proportion of the chelating agent to the waste polyester is 0.1 wt.%;
[0121] The conditions for the re-depolymerization reaction in Example 9 were 190° C., 10 min;
[0122] The conditions for the re-depolymerization reaction in Example 10 were 160° C. for 20 min.
[0123] The monomer ratios prepared in Examples 5-10 are shown in Table 2
[0124] Table 2 Monomer ratios in the multi-component copolyesters prepared in Examples 5-10
[0125] Comparative Examples 1 to 5
[0126] Comparative Examples 1 to 5 provide a method for preparing a multi-component copolyester, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 3:
[0127] S1. Initial depolymerization:
[0128] Waste polyester with an average particle size of ≤2 mm was dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction under a nitrogen atmosphere and microwave conditions to obtain a primary depolymerization product;
[0129] S2. Re-disaggregation:
[0130] Extracting a portion of ethylene glycol from the primary depolymerization product obtained in step S1 by vacuum distillation, adding a chelating agent (or not adding a chelating agent), placing the product in a microwave reactor, and performing a re-depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions. After filtering the reactants, the obtained filtrate is the re-depolymerization product;
[0131] S3. Esterification reaction:
[0132] According to the monomer content of the target multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer, and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender, and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield reaches 90% to obtain an esterified product;
[0133] S4. Polycondensation:
[0134] After removing excess alcohol from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum conditions to obtain the multi-component copolyester.
[0135] Table 3 Raw materials and reaction conditions of Comparative Examples 1 to 5
[0136] Performance Testing
[0137] The performance of the multi-component copolyesters prepared in the above examples and comparative examples was tested as follows:
[0138] Melting point: ISO 11357-3:2018;
[0139] Relative viscosity: measured according to GB / T 17931-1999 standard method in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05°C, with a sample concentration of 5 mg / ml;
[0140] Terminal carboxyl content: FZ / T 50012-2006;
[0141] Metal ion residue: US EPA 6010C:2014;
[0142] Crystallinity: JY / T 0587-2020;
[0143] Weight average molecular weight: detected by gel permeation chromatography (GPC);
[0144] 50-day biodegradation rate: According to GB / T 19277-2003 "Determination of the ultimate aerobic biodegradability and disintegration of materials under controlled composting conditions using the method of measuring the released carbon dioxide", the biodegradation performance is determined by the composting method.
[0145] Print retention rate: in accordance with GB / T 38082-2019, Section 5.3.4 Printing quality test for biodegradable plastic shopping bags.
[0146] The multi-component copolyester prepared in Example 1 was subjected to infrared spectroscopy, nuclear magnetic hydrogen spectroscopy, and XRD. The specific methods were:
[0147] Infrared spectroscopy: The sample preparation method adopts hot pressing film forming, the wave number range is 4000~400cm-1, the number of scans is 16 times, the resolution is 4, and the sampling method is transmission;
[0148] H NMR spectrum: Deuterated trifluoroacetic acid was used as solvent and tetramethylsilane (TMS) was used as internal standard.
[0149] XRD: X-ray diffractometer (XRD) was used according to the standard JY / T 0587-2020.
[0150] Using XRD testing, the crystallization peak (sharp peak) and the non-crystallization peak area (diffuse peak) are obtained, and the crystallinity is calculated according to the following formula:
[0151] Where:
[0152] Wc-crystallinity
[0153] I C -Integrated area of diffraction peak in crystalline state
[0154] I a -Integrated area of diffraction peak of amorphous state
[0155] The infrared spectrum of the multi-component copolyester of Example 1 is shown in FIG1 , the H-NMR spectrum is shown in FIG2 , the XRD pattern is shown in FIG3 , and the GPC spectrum is shown in FIG4 .
[0156] The test results of the embodiments are shown in Table 4, and the test results of the comparative examples are shown in Table 4.
[0157] Table 4
[0158] Table 6
[0159] According to the test results in Table 4, the crystallinity range of the multi-component copolyester obtained by the technical solution of the present invention is appropriate, between 10-19.5%, and the heavy metal ion content is extremely low. The obtained product has excellent performance, among which the 50-day biodegradation rate is above 35%, and the printing peeling rate is below 7%. In addition, it can be seen from the infrared spectrum, nuclear magnetic hydrogen spectrum and other spectra of the multi-component copolyester obtained in Example 1 that the present invention has successfully prepared PBATE and can calculate the proportion of different chain segments. Infrared spectrum analysis: As shown in Figure 1, 1731cm -1 The carbonyl (-C=O) stretching vibration peak at 1104 cm -1 、1271cm -1 731cm is the ether bond (COC) stretching vibration peak. -1 The out-of-plane bending vibration peak of CH on the para-disubstituted benzene ring, the stretching vibration and out-of-plane bending vibration absorption peak of the (-CH) group at 3053 cm-1, is attributed to the (-CH) group on the benzene ring; -1 The new absorption peak at 1458 cm is the stretching vibration absorption peak of the benzene ring skeleton. -1 The absorption peak at 2957cm is the in-plane bending vibration absorption peak of -CH2-CH2- in PBATE copolyester; -1 and 1410cm -1 、1360cm -1 They are the stretching vibration absorption peak and in-plane bending vibration peak of methylene (-CH2-) on the PBATE copolyester chain; at 3630~3400cm -1 The stretching vibration peak of the hydroxyl group associated with the intermolecular bond is attributed to the terminal hydroxyl group in the PBATE copolyester. It can be confirmed that the obtained polyester is PBATE. T represents terephthalic acid Structural unit, A represents adipic acid Structural unit, B represents the butanediol-OCH2CH2CH2CH2O- structural unit, and E represents the ethylene glycol-OCH2CH2O- structural unit. Figure 2 shows that the peak a at a chemical shift of δ8.1 represents the hydrogen atom peak on the benzene ring of the T structural unit; the peaks j, k, and l at δ4.70-4.27 represent the two methylene hydrogen atom peaks of the E structural unit; the peaks b, c, d, and e at δ4.7-4.1 represent the two methylene hydrogen atom peaks attached to the oxygen atom of the B structural unit; the peak f at δ2.32 represents the two methylene hydrogen atom peaks attached to the carbonyl group of the A structural unit; the peaks g and h at δ1.80-1.97 represent the two middle methylene hydrogen atom peaks of the B structural unit; and the peak i at δ1.54-1.66 represents the two middle methylene hydrogen atom peaks of the A structural unit. By studying the split peaks at δ=4.70-4.27 and δ=4.43-4.09, the segment composition ratio and sequence distribution of the copolyester can be calculated. A randomness R=1 indicates a random copolymer, and the molar ratio of ethylene glycol segments in the polyester is calculated to be 5%.
[0160] According to Examples 1, 5, and 6, it can be seen that when tea polyphenols are used as a chelating agent, compared with phytic acid or stearyl citrate, the multi-component copolyester has a relatively lower metal ion content, higher tensile strength, better printing performance, and better biodegradability.
[0161] According to the test results of the comparative examples, in comparative examples 1 and 2, without adding a chelating agent, the metal ions of the obtained multi-component copolyester could not be effectively removed, the metal ion content was very high, and the tensile strength of the multi-component copolyester was poor.
[0162] According to the test results of Comparative Examples 3 and 4, it can be seen that in the re-depolymerization process of step S2, when the re-depolymerization temperature is too high or too low, the chelating agent cannot play a good role in removing metal ions, and the metal ion content of the obtained multi-component copolyester is still too high; and the crystallinity of the obtained multi-component copolyester is also not within the appropriate range, resulting in poor overall performance of the product.
[0163] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A multi-component copolyester, It is characterized in that The multi-component copolyester comprises: Component A, a dicarboxylic acid compound, based on the total molar amount of component A, comprises: a1, 35 to 65 mol% of at least one aliphatic dicarboxylic acid; a2, 35 to 65 mol% of at least one aromatic dicarboxylic acid or a derivative thereof; Component B, 1,4-butanediol; Component C, a third monomer, based on the total molar amount of component B and component C, the component C accounts for 5 to 30 mol%; the third monomer is at least one of ethylene glycol, 1,4-cyclohexanedimethanol, and isosorbide; The crystallinity of the multi-component copolyester is 5-22%, the zinc content in the multi-component copolyester is ≤100ppm, the titanium content is ≤120ppm, the calcium content is ≤71ppm, and the silicon content is ≤85ppm.
2. The multi-component copolyester according to claim 1, It is characterized in that The melting point of the multi-component copolyester is 105-140°C.
3. The multi-component copolyester according to claim 1, It is characterized in that The relative viscosity of the multi-component copolyester is 1.2-1.
8.
4. The multi-component copolyester according to claim 1, It is characterized in that The terminal carboxyl content of the multi-component copolyester is 13-30 mmol / t.
5. The multi-component copolyester according to claim 1, It is characterized in that The zinc content in the multi-component copolyester is 45-70 ppm, and the titanium content is 50-105 ppm.
6. The multi-component copolyester according to claim 1, It is characterized in that The aliphatic dicarboxylic acid is selected from at least one of malonic acid, succinic acid, adipic acid, sebacic acid, pimelic acid, suberic acid, and azelaic acid, and the aromatic dicarboxylic acid or its derivative is selected from at least one of terephthalic acid or its derivative, and isophthalic acid or its derivative.
7. A method for preparing the multi-component copolyester according to any one of claims 1 to 6, It is characterized in that The steps include: S1. Initial depolymerization: Dissolving waste terephthalic acid polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product; The temperature of the initial depolymerization reaction is 180-230°C and the time is 15-120 minutes; S2. Re-depolymerization: Extracting part of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions, and filtering the reactant to obtain a filtrate as the re-depolymerization product; The temperature of the re-depolymerization reaction is 160-190°C and the time is 10-20 minutes; S3. Esterification reaction: According to the monomer content of the multi-component copolyester, at least one of an aliphatic dicarboxylic acid, a third monomer and 1,4-butanediol is added to the re-depolymerized product of step S2, and a polymerization catalyst, a chain extender and a stabilizer are added, and an esterification reaction is carried out under an inert gas atmosphere until the theoretical water yield is 85-95%, to obtain an esterified product; S4. Polycondensation: After removing excess alcohol solvent from the esterification product of step S3, the product is mixed with a polycondensation catalyst and subjected to a polycondensation reaction under vacuum until the relative viscosity of the system is 1.2 to 1.8, thereby obtaining the multi-component copolyester.
8. The preparation method according to claim 7, It is characterized in that The waste polyester includes one or more of recycled PET, PBT, PET / PBT alloy, and PBAT.
9. The preparation method according to claim 7, It is characterized in that At least one of the following (a)-(e): (a) In step S2, the chelating agent includes at least one of stearyl citrate, calcium citrate, tea polyphenols, and phytic acid; preferably tea polyphenols; (b) In step S1, the depolymerization catalyst includes at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate; (c) the polymerization catalyst and the polycondensation catalyst are each independently selected from at least one of butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds, titanium-magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide; (d) the stabilizer is one or more of organic phosphites, trimethyl phosphates, and hindered phenols; (e) The chain extender is at least one of pentaerythritol, trimethylolethane, trimethylolpropane, xylitol, sorbitol, HDI, MDI, TDI, isophorone diisocyanate, ethylene-methyl methacrylate copolymer, and multifunctional epoxy compound ADR.
10. The preparation method according to claim 7, It is characterized in that At least one of (f)-(j): (f) In step S2, the chelating agent is added in an amount of 0.01 to 0.1 wt.% of the waste polyester; (g) In step S1, the amount of the depolymerization catalyst added is 0.05 to 0.5 wt.% of the waste polyester; (h) the amount of the chain extender added is 0 to 0.1 wt.% of the waste polyester; (i) In step S4, the amount of the polycondensation catalyst added is 0.03 to 0.1 wt.% of the waste polyester; (j) In step S3, the amount of the polymerization catalyst added is 0.01-0.1 wt.% of the waste polyester.
Citation Information
Patent Citations
Reutilization material for silk screen board and reutilization method of reutilization material
CN106647193A
Method for continuously preparing spinnable colorless recycled polyester from colored waste polyester textiles
CN112646135A
Method for manufacturing modified engineering polyester by using byproducts generated after cyclic regeneration fiber production through chemical method
CN113773477A
Biodegradable polyester PBIAT and preparation method thereof
CN113861399A
Method for preparing regenerated polyester by closed-loop recovery of waste polyester with typical green and low-carbon characteristics
CN114031756A
Cited By
Flexible treating agent for silk-flax blended fabric
CN120905940A