Electrode and electrochemical measurement system
The electrode with a tailored carbon film structure addresses the limitations of existing systems by reducing background current and enhancing sensitivity in stripping voltammetry, achieving improved metal detection through optimized sp² and sp³ bonding ratios and FWHM characteristics.
Patent Information
- Application Number
- PCT/JP2024/014423
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-11
- Filing Date
- 2024-04-09
- Publication Date
- 2024-11-14
AI Technical Summary
Existing electrochemical measurement systems face challenges in achieving low background current and high metal detection sensitivity in stripping voltammetry, particularly due to limitations in the background current and negative potential window, which affect the detection range and sensitivity of metal ions.
The development of an electrode with a carbon film having a specific sp² and sp³ bonding ratio of 0.3 to 0.45 and a full width at half maximum (FWHM) of the G band between 135 cm⁻¹ and 220 cm⁻¹, which reduces background current and enhances metal detection sensitivity by optimizing the carbon film's structure and conductivity.
The optimized electrode achieves low background current and high signal current in stripping voltammetry, improving metal detection sensitivity and expanding the range of detectable metals, while maintaining suitable conductivity for effective electrochemical measurements.
Smart Images

Figure JP2024014423_14112024_PF_FP_ABST
Abstract
Description
Electrodes and Electrochemical Measurement Systems
[0001] The present invention relates to an electrode and an electrochemical measurement system.
[0002] Stripping voltammetry is a known electrochemical measurement method in which metal ions present at low concentrations in an aqueous solution are reduced and concentrated (deposited) on the surface of an electrode, and then the reduced and concentrated metal is oxidized and eluted. The metal ions in the aqueous solution are measured with high sensitivity based on the current value obtained during this process.
[0003] Patent Document 1 discloses a substrate and a sp 2 Bonds and sp 3 and a conductive carbon layer having a bond therein, wherein the concentration ratio of oxygen to carbon on one surface in the thickness direction of the conductive carbon layer is 0.07 or less.
[0004] The electrode described in Patent Document 1 is said to be able to sufficiently reduce and concentrate the metal to be measured and reliably oxidize and dissolve it in stripping voltammetry, thereby increasing the signal current.Furthermore, it is said to be able to sufficiently reduce the hydrogen peroxide to be measured at a lower potential in cyclic voltammetry, thereby increasing sensitivity.
[0005] Japanese Patent Application Laid-Open No. 2021-56205
[0006] The metal detection characteristics of electrochemical measurements are affected by the background current or signal current and the negative potential window of stripping voltammetry. Specifically, the lower the background current and the higher the signal current of stripping voltammetry, the better the metal detection sensitivity, and the wider the negative potential window, the wider the range of detectable metals.
[0007] However, Patent Document 1 does not mention the background current or signal current of stripping voltammetry or the negative potential window, so there is room for improvement in terms of obtaining desired metal detection characteristics.
[0008] The present invention has been made to solve the above problems, and aims to provide an electrode that has a low background current in stripping voltammetry and excellent metal detection sensitivity. Another aim of the present invention is to provide an electrochemical measurement system including the electrode.
[0009] The electrode of the present invention is sp 2 Bonds and sp 3 a carbon film having sp bonds, 3 The bond ratio is 0.3 or more and 0.45 or less, and the full width at half maximum of the G band is 135 cm -1 220cm or more -1 The following is the result.
[0010] The electrochemical measurement system of the present invention comprises the electrode of the present invention.
[0011] According to the present invention, an electrode having a low background current in stripping voltammetry and excellent metal detection sensitivity can be provided. Furthermore, according to the present invention, an electrochemical measurement system including the electrode can be provided.
[0012] FIG. 1 is a cross-sectional view schematically showing one embodiment of an electrode of the present invention. FIG. 2 is a schematic diagram showing an example of an electrochemical measurement system of the present invention. FIG. 3 is an XPS C1s spectrum in Example 1. FIG. 4 is a Raman spectrum in Example 1. FIG. 5 is an SV waveform of lead in Example 1. FIG. 6 is a graph showing the concentration dependence of the oxidation current of lead in Example 1. FIG. 7 is an SV waveform of zinc in Example 8.
[0013] The electrode and electrochemical measurement system of the present invention will be described below. However, the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention. A combination of two or more of the individual desirable configurations of the present invention described in the following embodiments also constitutes the present invention.
[0014] The drawings shown below are schematic diagrams, and the dimensions, aspect ratio, scale, etc. may differ from those of the actual product.
[0015] FIG. 1 is a cross-sectional view schematically showing one embodiment of the electrode of the present invention.
[0016] The electrode 10 shown in Fig. 1 includes a carbon film 20. As shown in Fig. 1, the electrode 10 preferably further includes a base substrate 30. In this case, the carbon film 20 is disposed on one main surface of the base substrate 30.
[0017] The carbon film 20 is sp 2 Bonds and sp 3 The carbon film 20 is made of carbon having bonds. That is, the carbon film 20 is a film having a graphite structure and a diamond structure. This gives the carbon film 20 good electrical conductivity.
[0018] In the electrode 10, the sp 3 The bond ratio is 0.3 or more and 0.45 or less, and the full width at half maximum of the G band is 135 cm -1 220cm or more -1 The present invention is characterized by the following:
[0019] sp in the carbon film 20 3 The bond ratio is sp 2 Number of bonded atoms and sp 3 sp relative to the sum of the number of bonded atoms 3 The ratio of the number of bonded atoms (sp 3 / sp 2 +sp 3 ) in the carbon film 20. 3 The bond ratio can be determined by performing X-ray photoelectron spectroscopy (XPS) on the carbon film 20 and analyzing the C1s spectrum. 2 Bonds and sp 3 The peak area of the binding can be determined and calculated.
[0020] The full width at half maximum (FWHM) of the G band in the carbon film 20 is used as an index of the degree of crystallinity. The higher the FWHM of the G band, the lower the degree of crystallinity, and the lower the FWHM of the G band, the higher the degree of crystallinity. The FWHM of the G band in the carbon film 20 can be calculated by performing Raman spectroscopy on the carbon film 20 to obtain a Raman spectrum, and separating the peaks into the G band and the D band.
[0021] sp 3 The bond ratio is 0.3 or more and 0.45 or less, and the full width at half maximum of the G band is 135 cm -1 220cm or more -1 The carbon film 20 having the following characteristics has a low background current in stripping voltammetry and is excellent in metal detection sensitivity.
[0022] The background current in stripping voltammetry arises from the desorption of water molecules, etc. 2 The π electrons of the bonded carbon function as adsorption sites, so sp 3 It is believed that a film structure with a high bonding ratio and a low number of π electrons can reduce the background current.
[0023] On the other hand, the sp 3 If the bonding ratio is too high, the conductivity of the carbon film 20 will be low, making it difficult to use as an electrode. 3 If the bonding ratio is too high, the internal stress of the carbon film 20 increases, making it more likely to peel off from the base substrate 30 .
[0024] Moreover, if the full width at half maximum of the G band in the carbon film 20 is too high, the conductivity of the carbon film 20 will be low, making it difficult to use as an electrode. Furthermore, if the full width at half maximum of the G band in the carbon film 20 is too high, the crystallite size (La) will be three times or less the carbon-carbon bond distance (0.14 nm) of the six-membered carbon ring, and the carbon film cannot be defined as having nano-sized crystals.
[0025] In the electrode 10, the sp 3 The bond ratio is 0.3 or more and 0.42 or less, and the full width at half maximum of the G band is 135 cm -1 210cm or more -1 It is preferable that:
[0026] sp 3 The bond ratio is 0.3 or more and 0.42 or less, and the full width at half maximum of the G band is 135 cm -1 210cm or more -1 The carbon film 20 having the following characteristics has a high signal current in stripping voltammetry and is excellent in metal detection sensitivity.
[0027] The oxidation current is proportional to the area of the electrode where reduction and concentration are active in stripping voltammetry. 2 Since the surface exposed area of the bonded carbon corresponds to the area of reduction and concentration, sp 2 It is believed that a film structure with a high bonding ratio can increase the signal current.
[0028] In the electrode 10, the sp 3 The bond ratio is 0.34 or more and 0.37 or less, and the full width at half maximum of the G band is 185 cm -1 210cm or more -1 More preferably, it is:
[0029] sp 3 The bond ratio is 0.34 or more and 0.37 or less, and the full width at half maximum of the G band is 185 cm -1 210cm or more -1 The carbon film 20 shown below has a wide potential window on the negative side and can detect many metal species.
[0030] The negative potential window indicates the potential at which the reduction reaction of water occurs, and is related to the ease of electron donation from the electrode to water molecules. 2 Since it is derived from a cluster formed by bonding, if the cluster size is small and there are few electron carriers, electron donation is difficult to occur, and the potential window on the negative side becomes wider.
[0031] Furthermore, when the negative potential window is wide, even when metals with high reduction potentials such as zinc are reduced and concentrated, they do not compete with the reduction reaction of water, which is thought to enable detection with good reproducibility.
[0032] Although the thickness of the carbon film 20 is not particularly limited, from the viewpoint of film formability, the thickness of the carbon film 20 is preferably 5 nm or more, and more preferably 10 nm or more. On the other hand, from the viewpoints of thinning and ease of handling, the thickness of the carbon film 20 is preferably 500 nm or less, more preferably 300 nm or less, and even more preferably 200 nm or less.
[0033] The thickness of the carbon film 20 can be calculated by measuring the X-ray reflectivity of the carbon film 20. For example, a multipurpose X-ray diffractometer SmartLab (manufactured by Rigaku Corporation) can be used to measure the X-ray reflectivity.
[0034] The carbon film 20 may contain other additives (including other elements) in addition to carbon. The carbon film 20 may be composed of multiple layers with different structures, compositions, additive concentrations, etc. Alternatively, the carbon film 20 may have a structure in which the structure, composition, additive concentration, etc. change stepwise.
[0035] When the electrode 10 includes the base substrate 30, the base substrate 30 has a sheet or film shape. The base substrate 30 supports the carbon film 20.
[0036] Examples of the base substrate 30 include an inorganic base material and an organic base material.
[0037] Examples of inorganic substrates include silicon substrates and glass substrates.
[0038] Examples of organic substrates include polymer films, etc. Examples of materials for polymer films include polyester resins (e.g., polyethylene terephthalate, polyethylene naphthalate), acetate resins, polyethersulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins (e.g., polycycloolefin polymers), (meth)acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, and polyphenylene sulfide resins.
[0039] The base substrate 30 is preferably conductive. Examples of the conductive base substrate 30 include conductive inorganic substrates such as conductive silicon substrates.
[0040] Although the carbon film 20 having a film structure suitable for metal detection may have low conductivity, by using a conductive substrate as the base substrate 30, it becomes possible to extract a current generated by an electrochemical reaction on the surface of the carbon film 20 through the base substrate 30, and therefore the carbon film 20 can be used as an electrode. Note that, when the resistance value of the carbon film and the resistance value of the base substrate are large and an IR drop has an effect, the potential of the electrode surface may fall below the applied potential, causing the apparent oxidation potential to shift to a higher potential. Therefore, it is preferable that the oxidation potential in cyclic voltammetry of the reactant does not shift to a higher potential due to the IR drop when current is extracted.
[0041] The term "conductive" as used herein means, for example, that the volume resistivity is less than 0.02 Ωcm.
[0042] The thickness of the base substrate 30 is not particularly limited, but is, for example, 2 μm or more, preferably 20 μm or more, and is, for example, 1000 μm or less, preferably 500 μm or less.
[0043] 1 is composed of a carbon film 20 and a base substrate 30, and may further include one or more functional layers, for example, between the carbon film 20 and the base substrate 30 or on the other main surface of the base substrate 30. Examples of functional layers include a gas barrier layer, a conductive layer, an adhesion layer, and a surface smoothing layer.
[0044] A method for manufacturing the electrode 10 shown in FIG. 1 includes, for example, a step of preparing a base substrate 30 and a step of forming a carbon film 20 on one main surface of the base substrate 30 .
[0045] In the step of preparing the base substrate 30, for example, a known or commercially available base material is prepared. If necessary, one main surface of the prepared base material may be subjected to a surface treatment, a cleaning treatment, or the like.
[0046] In the step of forming the carbon film 20 , the carbon film 20 is formed on one main surface of the base substrate 30 .
[0047] The film formation process is not particularly limited and is selected in order to control the structure of the carbon film 20. Examples include pulsed laser deposition (PLD), chemical vapor deposition (CVD), sputtering, paste printing of carbon materials, and carbonization of various organic materials (polyimide, liquid crystal polymer, epoxy, lignin, polyamide, phenolic resin, etc.).
[0048] The electrode of the present invention can be used as various electrodes, and is preferably used as an electrode for electrochemical measurements, specifically as a working electrode for stripping voltammetry.
[0049] An insulating layer patterned into a desired shape may be provided on one main surface of the electrode of the present invention from the viewpoint of adjusting the exposed surface (electrode surface) of the carbon film. Alternatively, the entire electrode or the carbon film may be patterned into a desired shape. Examples of the insulating layer include the polymer films described above for the base substrate.
[0050] An electrochemical measurement system including the electrode of the present invention will be described in detail below. Such an electrochemical measurement system also constitutes the present invention.
[0051] The electrochemical measurement system of the present invention includes, for example, a working electrode, a reference electrode, a potentiometer for measuring the electromotive force between these electrodes, and an aqueous solution (electrolyte). The electrode of the present invention is preferably used as the working electrode.
[0052] FIG. 2 is a schematic diagram showing an example of an electrochemical measurement system of the present invention.
[0053] The electrochemical measurement system 100 shown in FIG. 2 includes a working electrode 110, a reference electrode 120, a counter electrode (counter electrode) 130, a potentiostat 140 that controls the electrode potentials, an ammeter (not shown because it is incorporated into the potentiostat 140) that measures the current flowing between the working electrode 110 and the counter electrode 130, and an aqueous solution 150.
[0054] The working electrode 110 can be, for example, an electrode of the present invention, such as the electrode 10 shown in FIG.
[0055] Examples of the reference electrode 120 include a silver / silver chloride electrode, a saturated calomel electrode, and a standard hydrogen electrode.
[0056] Examples of the counter electrode 130 include a platinum electrode, a gold electrode, and a nickel electrode.
[0057] The aqueous solution 150 may be an aqueous solution containing the object to be measured.
[0058] In the electrochemical measurement system 100 shown in FIG. 2, for example, stripping voltammetry is carried out using the electrode of the present invention as the working electrode 110 .
[0059] The measurement target in stripping voltammetry is a metal ion, such as a heavy metal ion such as an iron ion, lead ion, gold ion, platinum ion, silver ion, copper ion, chromium ion, cadmium ion, mercury ion, zinc ion, arsenic ion, manganese ion, cobalt ion, nickel ion, molybdenum ion, tungsten ion, tin ion, bismuth ion, uranium ion, or plutonium ion.
[0060] As described above, in the electrode of the present invention, the sp 3 The bond ratio is 0.3 or more and 0.45 or less, and the full width at half maximum of the G band is 135 cm -1 220cm or more -1 Therefore, the background current in stripping voltammetry is low, and the metal detection sensitivity is excellent.
[0061] The present specification discloses the following:
[0062] <1> sp 2 Bonds and sp 3 a carbon film having sp bonds, 3 The bond ratio is 0.3 or more and 0.45 or less, and the full width at half maximum of the G band is 135 cm -1 220cm or more -1 Below are the electrodes.
[0063] <2> sp in the carbon film 3The bond ratio is 0.3 or more and 0.42 or less, and the full width at half maximum of the G band is 135 cm -1 210cm or more -1 The electrode according to <1>, which is as follows:
[0064] <3> sp in the carbon film 3 The bond ratio is 0.34 or more and 0.37 or less, and the full width at half maximum of the G band is 185 cm -1 210cm or more -1 The electrode according to <2>, which is as follows:
[0065] <4> The electrode according to any one of <1> to <3>, further comprising a base substrate, the carbon film being disposed on one main surface of the base substrate.
[0066] <5> The electrode according to <4>, wherein the base substrate has electrical conductivity.
[0067] <6> An electrochemical measurement system comprising the electrode according to any one of <1> to <5>.
[0068] <7> The electrochemical measurement system according to <6>, wherein stripping voltammetry is performed using the electrode as a working electrode.
[0069] Examples that more specifically disclose the electrode of the present invention are given below, but the present invention is not limited to these examples.
[0070] Example 1: Carbon Film Formation A 200 nm thick carbon film was formed on a 350 μm thick conductive silicon substrate using pulsed laser deposition (PLD). In PLD, a graphite target placed in a chamber is irradiated with a pulsed laser, which instantaneously vaporizes the target and generates a plume. Active particles in the plume reach the substrate and re-condense to form a carbon film.
[0071] The film structure of the carbon film can be controlled by the PLD conditions. Specifically, by changing the film formation conditions, the way carbon atoms are ejected, the energy after reaching the substrate, etc., the film structure of the carbon film (degree of crystallization and sp 3 The bonding ratio can be controlled.
[0072] The conditions for this example are as follows: Target material: graphite Laser wavelength: Nd:YAG laser (266 nm) Laser density: 2.54 J / cm 2 Repetition frequency: 10 Hz Film formation atmosphere: vacuum (2.0 × 10 -7 Torr) Substrate temperature: 400°C
[0073] [Evaluation of Film Structure of Carbon Film] X-ray photoelectron spectroscopy (XPS) was performed on the carbon film.
[0074] FIG. 3 shows the XPS C1s spectrum in Example 1.
[0075] From the obtained C1s spectrum, sp 2 Bonds and sp 3 The peak area of the bond was calculated. 3 The bond ratio was calculated. 3 The binding ratio was 0.32.
[0076] Next, Raman spectroscopy was carried out.
[0077] FIG. 4 shows the Raman spectrum of the Raman spectroscopy in Example 1.
[0078] The obtained Raman spectrum was subjected to peak separation into G band and D band, and the full width at half maximum (FWHM) of the G band, which is an index of the degree of crystallinity, was calculated. In Example 1, the FWHM of the G band was 136 cm -1 It was. 2 The cluster size La due to bonding was estimated to be approximately 1.5 nm, and it was found to be amorphous carbon with nano-sized crystals.
[0079] The measurement and analysis conditions are as follows: [XPS] Measurement device: X-ray photoelectron spectrometer PHI XPS-1600R (manufactured by ULVAC) X-ray source: MgKα (1253.6 eV), 15 kV, 400 W Take-off angle: 45 degrees Measurement area: Φ800 μm Analysis conditions: baseline subtraction by the Shirley method and peak separation by Voigt function (Gauss 0.7, Lorentz 0.3) [Raman spectroscopy] Measurement device: fluorescence avoidance type laser Raman spectrophotometer RMP-510RS (manufactured by JASCO Corporation) Light source: Nd:YVO 4 Semiconductor laser (532 nm), 20 mW Grating: 900 gr / mm Measurement area: Magnification 20x, working distance 12 mm, numerical aperture 0.40 Analysis conditions: baseline subtraction using a linear function and peak separation using a Gaussian function
[0080] [Evaluation of lead detection properties of carbon film] The carbon film was used as a working electrode, a silver-silver chloride reference electrode, and a platinum wire as a counter electrode, and the electrodes were set in an electrochemical measurement cell (plate electrode evaluation cell kit, BAS). An acetate buffer solution (pH 5.6) containing lead chloride was poured so that each electrode was immersed, and the cells were connected to a potentiostat (Model 600E, BAS).
[0081] Lead ion concentration is 1 x 10 -7 M, 5 x 10 -7 M, 1 x 10 -6 M, 2 x 10 -6 The solutions were prepared so that the concentration of lead chloride in the solution was M, and stripping voltammetry (SV) was performed on each solution. Specifically, a voltage was first applied to the carbon film at a reduction potential of -1.4 V and a deposition time of 300 seconds. This reduced and concentrated lead ions in the low-concentration lead chloride aqueous solution on the surface of the carbon film. Next, linear sweep voltammetry was performed at a sweep rate of 200 mV / s, and the concentrated lead was oxidized and eluted.
[0082] Fig. 5 is an SV waveform of lead in Example 1. Fig. 6 is a graph showing the concentration dependency of the oxidation current of lead in Example 1.
[0083] In Example 1, the background current (BG current) of the SV was 25 μA / cm 2 , the slope of the lead calibration curve is 19 μA / μM cm2 The current value at 0 V of the SV waveform was defined as the SV BG current.
[0084] Example 2 A film was produced under the same conditions as in Example 1, except that the substrate temperature was changed to room temperature (RT). Evaluation of the film structure and lead detection characteristics were carried out in the same manner as in Example 1.
[0085] Example 3: The atmosphere was changed to nitrogen (1.0 × 10 -2 The film was fabricated under the same conditions as in Example 1, except that the pressure was changed to 100 Pa (Torr). The film structure and lead detection characteristics were evaluated in the same manner as in Example 1.
[0086] Comparative Example 1: The atmosphere was changed to argon (1.0 × 10 -2 The film was fabricated under the same conditions as in Example 1, except that the pressure was changed to 100 Pa (Torr). The film structure and lead detection characteristics were evaluated in the same manner as in Example 1.
[0087] Comparative Example 2 A carbon film having a thickness of 70 μm was formed on a polyimide film having a thickness of 125 μm by using a laser carbonization method. Laser carbonization is a phenomenon in which an organic material such as a resin is transformed into a graphite structure by laser energy.
[0088] The film structure of the carbon film can be controlled by the laser irradiation conditions. Specifically, by changing the degree of heat applied to the surface of a resin such as polyimide depending on the laser wavelength, the film structure of the carbon film (degree of crystallization and sp 3 By using the laser carbonization method, it is possible to produce carbon films with a high degree of crystallization, which is difficult to produce using the PLD method.
[0089] The conditions for Comparative Example 2 are as follows: After preparation, the film structure and lead detection characteristics were evaluated in the same manner as in Example 1. Irradiation material: Kapton R (manufactured by Toray DuPont) Laser device: 3Axis-CO 2 Laser marker / head: ML-Z9510 (Keyence Corporation) Laser wavelength: 10.6 μm Laser output: 6 W Atmosphere: air Sweep speed: 250 mm / s Sweep interval: 100 μm
[0090] Comparative Example 3 A carbon film having a thickness of 50 μm was formed on a polyimide film having a thickness of 125 μm by using a laser carbonization method. A laser wavelength different from that used in Comparative Example 2 was used to control the film structure.
[0091] The conditions for Comparative Example 3 are as follows. After preparation, the film structure and lead detection characteristics were evaluated in the same manner as in Example 1. Irradiation material: Kapton R (manufactured by Toray DuPont) Laser device: 3-Axis Hybrid Laser Marker MD-X1000 (manufactured by Keyence Corporation) Laser wavelength: 1064 nm Laser output: 5 W Atmosphere: air Sweep speed: 250 mm / s Sweep interval: 25 μm
[0092] The film formation conditions, film structure indexes, and lead detection characteristics of Examples 1 to 3 and Comparative Examples 1 to 3 are summarized in Table 1. In Table 1, carbon films for which no lead oxidation current was detected are marked with "-".
[0093]
[0094] The BG current of the SV in Examples 1 to 3 was one order of magnitude smaller than the BG current of the SV in Comparative Examples 1 to 3, and the oxidation current of lead was confirmed. 3 The bond ratio is 0.3 or more and 0.45 or less, and the FWHM of the G band is 135 cm -1 220cm or more -1 If the value is below this, the detection sensitivity is high and it can be said to be suitable for metal detection.
[0095] As mentioned above, the BG current of SV is generated by the desorption of water molecules. 2 The π electrons of the bonded carbon function as adsorption sites, so sp 3 It is believed that a film structure with fewer π electrons, which has a higher bonding ratio and a lower degree of crystallinity, can reduce the BG current.
[0096] Example 4: Laser density: 3.57 J / cm 2 Except for the above change, the film was produced under the same conditions as in Example 2. Evaluation of the film structure and lead detection characteristics were carried out in the same manner as in Example 1.
[0097] Example 5 After film formation under the same conditions as in Example 2, annealing was performed in the same chamber (substrate temperature: 400°C, atmosphere: vacuum (2.0 × 10 -7 Torr, and time: 1 hour. The film structure and lead detection characteristics were evaluated in the same manner as in Example 1.
[0098] Example 6 After film formation under the same conditions as in Example 3, except that the substrate temperature was changed to room temperature (RT), annealing treatment was performed in the same chamber (substrate temperature: 400°C, atmosphere: vacuum (2.0 × 10 -7 Torr, and time: 1 hour. The film structure and lead detection characteristics were evaluated in the same manner as in Example 1.
[0099] Example 7 After film formation under the same conditions as Comparative Example 1 except that the substrate temperature was changed to room temperature (RT), annealing treatment was performed in the same chamber (substrate temperature: 400°C, atmosphere: vacuum (2.0 × 10 -7 Torr, and time: 1 hour. The film structure and lead detection characteristics were evaluated in the same manner as in Example 1.
[0100] The film formation conditions, film structure indexes, and lead detection characteristics of Examples 1 to 7 are summarized in Table 2.
[0101]
[0102] The slopes of the calibration curves for lead in Examples 1, 3, 4, 6, and 7 were 1.5 times or more larger than the slopes of the calibration curves for lead in Examples 2 and 5. 3 The bond ratio is 0.3 or more and 0.42 or less, and the FWHM of the G band is 135 cm -1 210cm or more -1 If the value is less than this, the detection sensitivity is higher and it can be said to be suitable for metal detection.
[0103] As mentioned above, the oxidation current is proportional to the size of the electrode area where reduction and concentration of SV is active. 2 Since the surface exposed area of the bonded carbon corresponds to the area of reduction and concentration, sp 2 It is believed that the slope of the calibration curve can be increased in a film structure containing a large amount of bonded carbon.
[0104] Example 8: Laser density: 2.65 J / cm 2 Except for the above change, the film was produced under the same conditions as in Example 2. In addition to the evaluation of the film structure and the lead detection characteristics in the same manner as in Example 1, the zinc detection characteristics were evaluated as follows.
[0105] [Evaluation of Zinc Detection Properties of Carbon Film] The zinc detection properties were evaluated using the same setup as in Example 1 for evaluating the lead detection properties. Detection of metals with high reduction potentials, such as zinc, requires increasing the negative reduction potential of the SV, which can compete with the water reduction reaction and reduce reproducibility. Therefore, the width of the negative potential window and the reproducibility of the zinc oxidation current were evaluated. Note that a wide negative potential window reduces the effect of the water reduction reaction.
[0106] The potential window was evaluated by cyclic voltammetry in 0.05 M sulfuric acid at a sweep rate of 50 mV / s. -4 A / cm 2 The negative potential window was defined as the negative potential window. The reproducibility of the zinc oxidation current was evaluated when the zinc ion concentration was 1 × 10 -5 The procedure was the same as in Example 1, except that the reduction potential was changed to −2.0 V.
[0107] FIG. 7 shows the SV waveform of zinc in Example 8.
[0108] In Example 8, the negative potential window was −1.4 V, and the zinc oxidation current measured three times was 47 μA / cm 2 , 50 μA / cm 2 , 50 μA / cm 2 Highly reproducible measurements were possible.
[0109] Example 9: The deposition chamber was changed and the laser density was set to 0.91 J / cm 2 The film was fabricated under the same conditions as in Example 2, except for the above change. In addition to the evaluation of the film structure and the lead detection characteristics in the same manner as in Example 1, the zinc detection characteristics in the same manner as in Example 8 were also evaluated.
[0110] For Examples 1, 3, 4, 6 and 7, an evaluation of the zinc detection characteristics was added in the same manner as in Example 8, and the film formation conditions, film structure index, and lead detection characteristics are summarized in Table 3. The criteria for reproducible zinc detection were as follows: ◯: The variation from the average value of oxidation currents measured three times was within 5%; ×: The variation from the average value of oxidation currents measured three times was 5% or more, or no oxidation current was detected.
[0111]
[0112] In Examples 4, 8, and 9, the negative potential window was wider by 0.2 V or more than that in Examples 1, 3, 6, and 7, and zinc could be detected with good reproducibility. 3 The bond ratio is 0.34 or more and 0.37 or less, and the FWHM of the G band is 185 cm -1 210cm or more -1 If the value is less than this, a wider range of metal types can be detected, making it suitable for metal detection.
[0113] As mentioned above, the negative potential window refers to the potential at which the reduction reaction of water occurs, and is related to the ease of electron donation from the electrode to water molecules. 2 Because it is derived from clusters formed by bonding, electron donation is difficult when the cluster size is small and there are few electron carriers, resulting in a wide negative potential window. Furthermore, when the negative potential window is wide, even during the reduction and concentration of metals with high reduction potentials such as zinc, there is little competition with the reduction reaction of water, which is thought to ensure reproducibility.
[0114] Example 10: This example was produced under the same conditions as in Example 8, except that the base substrate was changed to a polyimide film (Kapton®, manufactured by DuPont-Toray Co., Ltd.). When the film structure was evaluated in the same manner as in Example 1, the results were similar to those of Example 8, in which the base substrate was a conductive silicon substrate. However, the electrode resistance was high, making electrochemical measurement difficult.
[0115] From the above, it can be said that a carbon film formed on a conductive base substrate, as in Examples 1 to 9, can be used as an electrode for electrochemical measurements even if the carbon film is thin. When the conductivity of the carbon film is low, a carbon film with a thickness of 200 nm alone has high electrode resistance, making it difficult to use as an electrode for electrochemical measurements by itself. Therefore, by using a conductive base substrate, it becomes possible to extract the current generated by the electrochemical reaction on the carbon film surface through the base substrate, and therefore the carbon film can be used as an electrode.
[0116] REFERENCE SIGNS LIST 10 Electrode 20 Carbon film 30 Underlying substrate 100 Electrochemical measurement system 110 Working electrode 120 Reference electrode 130 Counter electrode (counter electrode) 140 Potentiostat 150 Aqueous solution
Claims
1. sp 2 Bonds and sp 3 A carbon film having sp bonds, 3 The bond ratio is 0.3 to 0.45, and the full width at half maximum of the G band is 135 cm -1 220cm or more -1 Below are the electrodes.
2. sp in the carbon film 3 The bond ratio is 0.3 to 0.42, and the full width at half maximum of the G band is 135 cm -1 210cm or more -1 2. The electrode of claim 1 , wherein:
3. sp in the carbon film 3 The bond ratio is 0.34 to 0.37, and the full width at half maximum of the G band is 185 cm -1 210cm or more -1 3. The electrode of claim 2, wherein:
4. The electrode according to any one of claims 1 to 3, further comprising a base substrate, the carbon film being disposed on one main surface of the base substrate.
5. The electrode according to claim 4, wherein the underlying substrate is electrically conductive.
6. An electrochemical measurement system comprising the electrode according to any one of claims 1 to 5.
7. The electrochemical measurement system according to claim 6, wherein stripping voltammetry is carried out using the electrode as a working electrode.
Citation Information
Patent Citations
Electrochemical measuring carbon electrode and its manufacturing method
JP2006090875A
Carbon-coated metal member, and its production method
JP2008144245A
Electrode structure, manufacturing method of the same, and electrochemical sensor
JP2010230369A
Electrode and electrochemical measurement system
JP2020144116A
Electrode
WO2022210387A1