Method for producing resin composition and resin composition
The twin-screw kneading extruder configuration with specific screw designs and zones ensures efficient dispersion and maintains long residual fiber length, addressing the challenges of fiber breakage and productivity in producing fiber-reinforced thermoplastic resin compositions for precision molded products.
Patent Information
- Application Number
- PCT/JP2024/017158
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-14
AI Technical Summary
Existing methods for producing fiber-reinforced thermoplastic resin compositions fail to balance the residual fiber length, fiber breakage, and productivity, particularly in precision molded products where the presence of undefibrated fibers leads to defects and reduced mechanical strength.
A twin-screw kneading extruder configuration is used where the thermoplastic resin and fibrous filler are supplied through separate ports, with a mixing and dispersing section and a resistance section, featuring screw segments with circular arcs and a conveyance zone, to ensure efficient dispersion and maintain long residual fiber length.
This method effectively disperses fibrous fillers while minimizing fiber breakage, resulting in a resin composition with improved mechanical strength and suitable for precision molding applications.
Smart Images

Figure JP2024017158_14112024_PF_FP_ABST
Abstract
Description
Resin composition manufacturing method and resin composition
[0001] The present invention relates to a method for producing a resin composition and a resin composition.
[0002] Thermoplastic resin compositions containing a thermoplastic resin and a fibrous filler have superior physical properties such as mechanical strength compared to thermoplastic resins that do not contain a fibrous filler. For this reason, thermoplastic resin compositions containing a fibrous filler are used as raw materials for automobile parts, parts for electric and electronic products, etc.
[0003] Examples of methods for producing fiber-filler-reinforced thermoplastic resin composition pellets by mixing and kneading a fiber-based filler with a thermoplastic resin include the following: First, a thermoplastic resin is fed into an extruder and melted. Next, a fiber-based filler is fed into the molten thermoplastic resin, and the thermoplastic resin and the fiber-based filler are mixed and kneaded in the extruder. Finally, the mixture is cooled and granulated. For example, a single-screw extruder or a twin-screw extruder (such as a co-rotating intermeshing twin-screw extruder) is used as the extruder. Compared to a single-screw extruder, a twin-screw extruder tends to have higher productivity and operating flexibility. Therefore, a twin-screw extruder is more preferably used for producing fiber-filler-reinforced thermoplastic resin composition pellets.
[0004] The fiber filler used in the production of the fiber-based filler reinforced thermoplastic resin composition pellets is, for example, a roving wound with about 300 to 3,000 monofilaments having a diameter of 6 to 20 μm, or chopped strands obtained by cutting the roving to a length of 1 to 6 mm, etc. Chopped strands are used. Because chopped strands are easier to use, when industrially producing fiber-based filler reinforced thermoplastic resin composition pellets, the most common method is to supply a thermoplastic resin to a twin-screw extruder, melt the thermoplastic resin, and then supply chopped strands from the middle of the twin-screw extruder. The molten thermoplastic resin and the fiber-based filler are mixed and kneaded, the mixture is extruded, and then cooled and solidified.
[0005] The productivity of fiber-filler-reinforced thermoplastic resin composition pellets produced using the twin-screw extruder is determined by the extruder's plasticizing and mixing capabilities. The plasticizing capability of a twin-screw extruder depends on the screw design, the torque generated by the screw, the screw groove depth (the difference between the outer diameter and the root diameter of the screw), the screw rotation speed, etc. Patent Document 1 defines the torque density as the value obtained by dividing the center distance between the two screws by the cube, and discloses a twin-screw extruder with high plasticizing capability and excellent productivity.
[0006] The mixing and kneading capacity of a twin-screw extruder also depends on the screw design. As the plasticizing capacity of twin-screw extruders has improved, the residence time has decreased. This has led to a demand for the development of screw designs that can efficiently mix and knead in a short time. As such, research is being conducted into technologies to improve the plasticizing and kneading capacity of twin-screw extruders.
[0007] Generally, as described above, bundles of monofilaments are used as fibrous fillers. This is because, when fibrous fillers are fed into a twin-screw extruder without bundling the monofilaments, the monofilaments tend to become cotton-like, impairing transportability and making handling difficult. The chopped strands are, for example, mixed and kneaded in the twin-screw extruder until they are defibrated into monofilaments, and at the same time, the chopped strands are broken by a screw or the like until the monofilaments have an average length of 200 to 500 μm.
[0008] If mixing and kneading in the twin-screw extruder is insufficient, some or all of the chopped strands, which are not defibrated into monofilaments but are in the form of an aggregate of monofilaments (undefibrated fiber filler bundles), will remain in the resin composition pellets. If some or all of the chopped strands remain in the fiber-filler-reinforced thermoplastic resin composition pellets, some or all of the chopped strands will clog the gate during injection molding, making injection molding impossible, or even if injection molding is possible, some or all of the chopped strands will be present in the molded product, which is likely to cause poor appearance or reduced functionality.
[0009] In particular, with the advancement of electronics-related technologies in recent years, fiber-filler reinforced thermoplastic resin compositions used in parts are required to be molded into thin, complex shapes. The gate nozzles of molding machines used in such precision molding are often less than 1 mm. The presence of unresolved fiber filler bundles is a serious defect in precision molded products. For this reason, a common measure is to increase the mixing strength of the fiber filler to eliminate unresolved fiber filler bundles. While increasing the mixing strength reduces unresolved fiber filler bundles, it also results in fibers breaking in the mixer, shortening the remaining fiber length, and thus defeating the purpose of dispersing long fibers in the thermoplastic resin to improve strength.
[0010] The kneading process using a twin-screw kneader to disperse the fibrous filler after its addition typically involves blocking the flow of resin downstream using a reverse flight, a seal ring, an L-shaped disk with disks offset against the flow direction, or an N-shaped disk with disks arranged perpendicular to the flow direction to create a confined region, followed by kneading using an R-shaped disk with disks offset toward the flow direction. Increasing the blocking force lengthens the confined region (kneading region) upstream, thereby increasing the kneading intensity. While the twin-screw extruder described in Patent Document 1 is said to improve productivity, particularly in precision molded products such as those described above, the residence time tends to be shorter under high throughput conditions, making it even more difficult to completely defibrate chopped strands into monofilaments and shorten the fiber length.
[0011] By combining a large number of kneading segments such as kneading disks, it is possible to some extent to increase the kneading intensity and defibrate fiber bundles into monofilaments. On the other hand, increasing the kneading intensity tends to significantly shorten the fiber length and reduce strength. Therefore, Patent Document 2 discloses a method of promoting the reaction between a glass-based inorganic filler and a thermoplastic resin in a molding machine by using a kneading segment having an arc with a predetermined radius of curvature at the location observed in an axial cross-section of the top of the flight section, thereby improving the adhesion between the glass-based inorganic filler and the thermoplastic resin. Patent Document 3 discloses that using a single progressive screw segment having a flight section formed with an arc-shaped notch significantly reduces the probability of remaining undefibrated glass fiber bundles.
[0012] JP-T-11-512666A JP-A-2012-140526 JP-A-2012-213996
[0013] However, none of the above manufacturing methods are sufficient in terms of the balance between the remaining rate of unfibrillated fiber bundles, the remaining fiber length, and the improvement in productivity.
[0014] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing a resin composition that can maintain a long residual fiber length.
[0015] The present inventors have conducted extensive research and have completed the present invention.
[0016] That is, the present invention relates to the following: [1] A method for producing a resin composition by melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw kneading extruder, the twin-screw kneading extruder comprising, in order from upstream as viewed in a flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, and 50% by mass or more of the thermoplastic resin supplied from the first supply port is melted in the first kneading zone, and the second kneading zone comprises screw segments composed of flights or disks, and at least a portion of the top end faces of the flights and the end faces of the disks are composed of one or more arcs with a curvature radius R of 0.4 mm or more as viewed in a direction perpendicular to the axial direction of the flights or the disks. [2] The second kneading zone has, from upstream in the direction of material flow, a mixing and dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, the resistance section having a screw segment composed of a flight or a disk, and the flight or disk of the resistance section has a top end face of the flight or the upstream side of the end face of the disk composed of one or more arcs with a curvature radius R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or the disk. [3] The second kneading zone has, from upstream in the direction of material flow, a mixing and dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, the resistance section having a screw segment composed of a flight or a disk, and the flight or disk of the resistance section has a top end face of the flight or the upstream and downstream sides of the end face of the disk composed of one or more arcs with a curvature radius R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or the disk. [1] A method for producing a resin composition according to [2].[4] The second kneading zone has, from upstream in the direction of material flow, a mixing / dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, and the mixing / dispersion section has a screw segment composed of a flight or a disk, and the flight or the disk of the mixing / dispersion section has a top end face of the flight or the downstream side of the end face of the disk, when viewed from a direction perpendicular to the axial direction of the flight or the disk, A method for producing a resin composition according to any one of [1] to [3]. [5] The method for producing a resin composition according to any one of claims [1] to [4], wherein the second kneading zone has, from upstream to downstream in the material flow direction, a mixing / dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the material flow, the mixing / dispersion section having screw segments formed of flights or disks, and the flights or disks of the mixing / dispersion section are configured with one or more arcs having a radius of curvature R of 0.4 mm or more on the upstream and downstream sides of the top end face of the flight or the end face of the disk, as viewed from a direction perpendicular to the axial direction of the flight or the disk. [6] The method for producing a resin composition according to claim [4] or [5], wherein the flights of the mixing / dispersion section are single- or double-row flights having a length of 3D or more, and the clearance between the flight and the cylinder is 1.3% or more of the cylinder diameter. [7] The method for producing a resin composition according to any one of [1] to [6], further comprising a conveying zone composed of flights downstream of the second kneading zone, wherein the downstream side of the top end face of the flight in the conveying zone is composed of one or more arcs with a radius of curvature R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight. [8] The method for producing a resin composition according to any one of [1] to [7], wherein the fibrous filler is glass fiber or carbon fiber. [9] The method for producing a resin composition according to any one of [1] to [8], wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
[10] A resin composition obtained by the method for producing a resin composition according to any one of [1] to [9], wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
[0017] According to the present invention, there is provided a method for producing a resin composition capable of maintaining a long residual fiber length.
[0018] FIG. 1 is a schematic diagram showing an example of a twin-screw kneading extruder according to the present embodiment. FIG. 2 is a diagram explaining an example of a single-screw reverse lead flight used in the second kneading zone. FIG. 3 is a diagram explaining another example of a single-screw reverse lead flight used in the second kneading zone. FIG. 4 is a diagram explaining an example of a single-screw forward lead flight used in the second kneading zone. FIG. 5 is a diagram explaining an example of a reverse kneading disc used in the second kneading zone. FIG. 6 is a perspective view showing an example of a cutout segment. FIG. 7 is a diagram explaining an example of a flight used in the conveying zone. FIG. 8 is a diagram showing a single-screw reverse lead flight according to a comparative example. FIG. 9 is a diagram showing a single-screw forward lead flight according to a comparative example. FIG. 10 is a diagram explaining an example of a reverse kneading disc according to a comparative example. FIG. 11 is a diagram showing the resin pressure in Example 1. FIG. 12 is a schematic diagram showing the twin-screw kneading extruder used in Examples 7 to 9. FIG. 13 is a diagram explaining a single-screw reverse lead flight used in the second kneading zone of Examples 7 to 9. FIG. 14 is a diagram explaining a single-screw forward lead flight used in the second kneading zone of Examples 7 to 9.
[0019] Hereinafter, several embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments.
[0020] The method for producing a resin composition according to the present embodiment involves melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw extruder. The twin-screw extruder includes, in order from upstream to downstream in the direction of flow of the melt-kneaded materials, a first feed port, a first kneading zone, a second feed port, and a second kneading zone. The thermoplastic resin and the fibrous filler are fed into the twin-screw extruder through the first feed port and the second feed port, respectively. In the first kneading zone, 50% by mass or more of the thermoplastic resin fed through the first feed port is melted. The second kneading zone includes screw segments formed of flights or disks, and at least a portion of the top end faces of the flights and the end faces of the disks are formed by one or more arcs with a curvature radius R of 0.4 mm or more as viewed perpendicular to the axial direction of the flights or disks. This method allows for stable, high productivity dispersion of the fibrous filler in the thermoplastic resin while maintaining a long residual fiber length. In this method, the second kneading zone is equipped with a screw segment consisting of a flight or a disk, and at least a portion of the top end face of the flight and the end face of the disk are composed of one or more arcs with a radius of curvature R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or disk. Therefore, it is thought that the stress locally applied to the fibers when the material overcomes the clearance between the screw segment and the cylinder in the second kneading zone is reduced, and the fibers are less likely to be cut even when operated at a kneading intensity that results in a sufficiently dispersed state.
[0021] A specific example of the method according to this embodiment will be described below.
[0022] Fig. 1 is a schematic diagram showing an example of a twin-screw kneading extruder according to this embodiment. This twin-screw kneading extruder includes a cylinder (not shown), a screw 2 disposed in the cylinder, and a die (not shown) provided at the downstream end of the cylinder. The twin-screw kneading extruder may be configured to include screws that rotate and mesh with each other. Examples of twin-screw kneading extruders include co-rotating twin-screw kneading extruders.
[0023] The twin-screw kneading extruder includes, in order from upstream as viewed in the flow direction of the materials to be melt-kneaded, a supply zone 20, a first kneading zone 21, a conveying zone 22, a second kneading zone 23, and a conveying zone 24. A first supply port 1a and a second supply port 1b are provided in the supply zone 20 and the conveying zone 22, respectively, and a vent port 5 is provided in the conveying zone 24. That is, the twin-screw kneading extruder includes, in order from upstream as viewed in the flow direction of the materials to be melt-kneaded, a first supply port 1a, a first kneading zone 21, a second supply port 1b, and a second kneading zone 23. For example, hoppers (not shown) are connected to the first supply port 1a and the second supply port 1b.
[0024] The second kneading zone 23 is provided with screw segments composed of flights or discs, and at least a portion of the top end faces of the flights and end faces of the discs constituting the screw segments are composed of one or more arcs with a radius of curvature R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or disc. For example, one of the upstream and downstream sides of the flight top end face or the end face of the disc may be composed of one or more arcs with a radius of curvature R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or disc, or both the upstream and downstream sides may be composed of one or more arcs with a radius of curvature R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or disc.
[0025] FIG. 2 is a diagram illustrating an example of a screw segment used in the second kneading zone. This screw segment has a single reverse lead flight. This screw segment is composed of flights. FIG. 2(a) is a cross-sectional view of the screw segment viewed from a direction parallel to the axial direction of the flight, and FIG. 2(b) is a cross-sectional view of the screw segment viewed from a direction perpendicular to the axial direction of the flight. In FIG. 2, a indicates the clearance between the flight and the cylinder, b indicates the cylinder, dx indicates the cylinder diameter, e indicates the lead length, c indicates the upstream side of the top end face of the flight, and d indicates the downstream side of the top end face of the flight. The upstream side c of the top end face of the flight is composed of an arc with a curvature radius R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight.
[0026] FIG. 3 is a diagram illustrating another example of a screw segment used in the second kneading zone. This screw segment has a single reverse lead flight. This screw segment is composed of flights. (a) of FIG. 3 is a cross-sectional view of the screw segment viewed from a direction parallel to the axial direction of the flight, and (b) of FIG. 3 is a cross-sectional view of the screw segment viewed from a direction perpendicular to the axial direction of the flight. In FIG. 3, (a) indicates the clearance between the flight and the cylinder, (b) indicates the cylinder, (dx) indicates the cylinder diameter, (e) indicates the lead length, (c) indicates the upstream side of the top end face of the flight, and (d) indicates the downstream side of the top end face of the flight. The upstream side (c) of the top end face of the flight is composed of an arc with a curvature radius R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight.
[0027] FIG. 4 is a diagram illustrating another example of a screw segment used in the second kneading zone. This screw segment is a single-start forward lead flight. This screw segment is composed of flights. FIG. 4(a) is a cross-sectional view of the screw segment viewed from a direction parallel to the axial direction of the flight, and FIG. 4(b) is a cross-sectional view of the screw segment viewed from a direction perpendicular to the axial direction of the flight. In FIG. 4, a indicates the clearance between the flight and the cylinder, b indicates the cylinder, dx indicates the cylinder diameter, f indicates the flight width, e indicates the lead length, c indicates the upstream side of the top end face of the flight, and d indicates the downstream side of the top end face of the flight. The upstream side c and downstream side d of the top end face of the flight are composed of arcs with a curvature radius R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight.
[0028] Fig. 5 is a diagram illustrating another example of a screw segment used in the second kneading zone. This screw segment is a reverse kneading disc. This screw segment is composed of a disc. In Fig. 5, a indicates the clearance between the disc and the cylinder, b indicates the cylinder, dx indicates the cylinder diameter, e indicates the lead length, c indicates the upstream side of the end face of the disc, and d indicates the downstream side of the end face of the disc. The upstream side c of the end face of the disc is composed of an arc with a curvature radius R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the disc.
[0029] In the twin-screw kneading extruder shown in Figure 1, the second kneading zone 23 has, from upstream to downstream in the material flow direction, a mixing / dispersion section 23a that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section 23b that blocks the flow of the materials. The provision of the resistance section 23b in the second kneading zone 23 is thought to facilitate the mixture of the molten thermoplastic resin and the fibrous filler filling the voids in the mixing / dispersion section 23a, improving the mixing effect. The resistance section is a region configured with screw segments in which the pressure is highest at the upstream end of the resistance section 23b and decreases downstream. The mixing / dispersion section 23a is a region in which the pressure decreases from the downstream end (upstream end of the resistance section 23b) toward the upstream side.
[0030] The resistance portion 23b has, for example, a screw segment composed of a flight or a disk, and the flight or disk of the resistance portion 23b is composed of one or more arcs with a radius of curvature R of 0.4 mm or more on the upstream side of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
[0031] The mixing and dispersion section 23a is provided with, for example, a screw segment composed of a flight or a disk, and the flight or disk of the mixing and dispersion section 23a is composed of one or more arcs with a curvature radius R of 0.4 mm or more on the downstream side of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
[0032] The flights or disks used in the mixing / dispersing section 23a or the resistance section 23b may, for example, be configured such that the upstream and downstream sides of the top end face of the flight or the end face of the disk are configured with one or more arcs having a curvature radius R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or disk.
[0033] The mixing and dispersing section 23a can be configured by combining screw segments that are generally used as kneading segments, such as a forward kneading disk, a neutral kneading disk, a forward rotor, and the like, which are generally used for kneading.
[0034] The mixing / dispersing section 23a may be configured with one or two flights. The clearance between the flight and the cylinder may be, for example, 1.3% or more of the cylinder diameter. The length of the flight may be, for example, 2D or more, or 3D or more.
[0035] D usually refers to the approximate value of the diameter of the cylinder. That is, "length of 2D or more" means a length "about twice D", and "length of 3D or more" means a length "about three times D". Furthermore, the expression "1D upstream" described below means a length about "1 x D" upstream. The same applies to other similar expressions such as "0.5D".
[0036] In this specification, 1D is defined as a range of -8.0% to -5.0% of the cylinder diameter. In other words, if the cylinder diameter is defined as D', 1D means "0.92 x D' to 0.95 x D'". Similarly, "2D" means "0.92 x 2 x D' to 0.95 x 2 x D'", and "3D" means "0.92 x 3 x D' to 0.95 x 3 x D'".
[0037] The mixing / dispersing section 23a is preferably configured with a single flight or a double flight with a clearance between the flight and the cylinder of 1.3% or more of the cylinder diameter.
[0038] When a single flight is used, the flight width is preferably 20% or more of the lead length of the flight, and more preferably about 30%. By widening the flight width, dispersion and mixing effects in the gap between the screw and the flight tend to be more easily achieved.
[0039] When using double flights, it is usually difficult to increase the flight width, but it is preferable to increase the clearance between the flights and the cylinder. This increases the passage rate through the gap between the flights and the cylinder, which tends to make it easier to achieve dispersion and mixing effects. The clearance between the flights and the cylinder may be, for example, 1.3% or more, or 2% or more of the cylinder diameter.
[0040] The mixed dispersion section 23a may have a length of, for example, 2D or more, or a length of 3D or more, from the viewpoint of providing a sufficient area filled with the mixture of the fibrous filler and the thermoplastic resin.
[0041] The resistance portion 23b may be, for example, a screw segment such as a reverse flight, a seal ring, a neutral kneading disk, a reverse kneading disk, or a notched segment (a flight or ring with a notch), or a combination thereof. From the viewpoint of facilitating filling with the mixture of the molten thermoplastic resin and the fibrous filler, the resistance portion 23b may be formed, for example, by adjusting the combination and length of the screw segments so that the conveying force to the downstream side is lower than the discharge rate under the operating conditions of the twin-screw kneading extruder.
[0042] A cutout segment is a segment having a cutout portion. An example of a cutout segment is shown in Fig. 6. The cutout segment 10 shown in Fig. 6 is a cutout segment having a plurality of cutout portions.
[0043] Although there are no particular limitations on the configuration of the conveying zones 22 and 24, it is preferable that the conveying zone 24 downstream of the second kneading zone 23 be configured with a flight. The downstream side of the top end face of the flight constituting the conveying zone may be configured with, for example, one or more arcs having a curvature radius R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight.
[0044] Figure 7 is a diagram illustrating an example of a flight used in a transfer zone. Figure 7(a) is a cross-sectional view of the transfer zone viewed from a direction parallel to the axial direction of the flight, and Figure 7(b) is a cross-sectional view of the transfer zone viewed from a direction perpendicular to the axial direction of the flight. In Figure 7, a indicates the clearance between the flight and the cylinder, b indicates the cylinder, dx indicates the cylinder diameter, e indicates the lead length, c indicates the upstream side of the top end face of the flight, and d indicates the downstream side of the top end face of the flight. The downstream side d of the top end face of the flight is configured as an arc with a curvature radius R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight.
[0045] The radius of curvature R of the arc of the flight or disc in the second kneading zone and the conveying zone is preferably 1.0 mm or more, more preferably 4.0 mm or more, from the viewpoint of further reducing fiber breakage. The upper limit of the radius of curvature R is, for example, ½D.
[0046] A method for producing a resin composition using the twin-screw kneading extruder is described below. In this method, a thermoplastic resin and a fibrous filler are melt-kneaded using the twin-screw kneading extruder to produce a resin composition. The resulting resin composition is, for example, a fibrous filler-reinforced thermoplastic resin composition pellet.
[0047] First, a thermoplastic resin is supplied from a first supply port 1a to a supply zone 20. The thermoplastic resin supplied from the first supply port 1a to the supply zone 20 is transported to a first kneading zone 21. In the first kneading zone 21, 50 mass% or more of the thermoplastic resin supplied from the first supply port 1a is melted. The thermoplastic resin leaving the first kneading zone 21 is transported to a conveying zone 22, where it joins with a fibrous filler.
[0048] The fibrous filler is fed from the feed port 1b to the conveying zone 22, where it meets with the thermoplastic resin.
[0049] The thermoplastic resin and fibrous filler that have left the conveying zone 22 are kneaded in the second kneading zone 23. This disperses the fibrous filler in the thermoplastic resin. The second kneading zone 23 may be provided with the resistance portion described above, if necessary.
[0050] The thermoplastic resin and fibrous filler that have left the second kneading zone 23 pass through the conveying zone 24 and are discharged from the die to the outside of the twin-screw kneading extruder. This allows a fiber-filler-reinforced thermoplastic resin composition to be obtained. The obtained fiber-filler-reinforced thermoplastic resin composition may be pelletized as necessary.
[0051] The manufacturing method of this embodiment may include, for example, a plasticization step in which a thermoplastic resin is supplied to the extruder and plasticized by heating and kneading; a kneading / dispersion step in which, after the plasticization step, one or more bundles of fibrous filler are supplied to the extruder and the defibrated fibrous filler and the plasticized thermoplastic resin are kneaded with a screw while defibrating the fibrous filler bundles; a devolatilization step in which volatile components are removed as necessary; an extrusion step in which the mixture obtained in the mixing / dispersion step is extruded from a die to the outside of the twin-screw kneading extruder; and a pelletization step in which the mixture extruded from the die is pelletized.
[0052] [Plasticization Step] The plasticization step is carried out, for example, in the feeding zone 20 and the first kneading zone 21 .
[0053] In the plasticizing step, the thermoplastic resin (for example, resin pellets) supplied from the supply port 1a is transported and melted.
[0054] Examples of the screw segments used in the supply zone 20 include conveying segments made of flights. Examples of the screw segments used in the first kneading zone 21 include screw segments such as reverse flights, seal rings, forward kneading discs, reverse kneading discs, and combinations thereof.
[0055] For example, resin pellets are transported in the supply zone 20. The supply zone 20 functions to transport the resin pellets from the supply port 1a side toward the die.
[0056] Preheating with an external heater may be carried out as a preparation step for plasticization.
[0057] Because the thermoplastic resin is sandwiched between the rotating screw 2 and the cylinder, frictional force is applied to the thermoplastic resin, generating frictional heat. The preheating and frictional heat may cause the thermoplastic resin to begin to melt. In some cases, the groove depth of the screw 2 and the preheating temperature may be adjusted by a conventionally known method in the supply zone 20 so that the thermoplastic resin is transported smoothly.
[0058] In the first kneading zone 21, pressure is applied to the thermoplastic resin transferred from the supply zone 20 to melt the thermoplastic resin. In the first kneading zone 21, shear stress is applied to the thermoplastic resin, and as a result, the thermoplastic resin is transferred further forward (towards the conveying zone 22) while being melted.
[0059] As described above, 50% by mass or more of the thermoplastic resin is melted in the first kneading zone 21. This tends to reduce breakage of the fibrous filler. It is believed that the reduction in the resin viscosity in the first kneading zone 21 reduces breakage of the fibrous filler.
[0060] The first kneading zone 21 may be provided with an open vent or a vacuum vent for removing excess volatile components after plasticizing and melting the thermoplastic resin.
[0061] The thermoplastic resin (melt) melted in the plasticizing step joins with the fibrous filler in the conveying zone 22 and is then subjected to a kneading and dispersing step in the second kneading zone 23. The fibrous filler is supplied to the extruder from the second supply port 1b. The number of fibrous fillers supplied to the extruder is, for example, one or more bundles.
[0062] [Kneading and Dispersing Step] In the kneading and dispersing step, the fibrous filler and the molten thermoplastic resin are kneaded together, whereby the fiber bundles of the fibrous filler are defibrated and dispersed in the thermoplastic resin.
[0063] The kneading and dispersing step is carried out in the second kneading zone 23 .
[0064] [Post-Process] After the kneading and dispersion process, a conveying process may be performed in which the resin is conveyed to the tip of the kneader by a conveying screw flight. The conveying process is performed in a conveying zone 24. The conveying zone 24 may be provided with an open vent or a vacuum vent for removing volatile components contained in the raw resin, decomposition products of the surface treatment agent and sizing agent of the fibrous filler, and reaction residues. From the viewpoint of suppressing oxidation and deterioration of the resin, it is preferable to provide a vacuum vent.
[0065] There are no limitations on the fibrous filler and thermoplastic resin used in the method according to this embodiment, but specific examples are shown below.
[0066] [Fiber-based filler] The fiber-based filler is, for example, a fiber bundle formed by bundling a plurality of monofilaments with a sizing agent or the like. Fiber bundles bound with a sizing agent or the like are easy to handle during kneading. There are no particular restrictions on the number of monofilaments constituting the fiber bundle, but it may be, for example, 300 to 3,000, or 1,100 to 2,200. The fiber-based filler may be formed by continuously feeding a bundle of monofilaments as rovings to a twin-screw kneading extruder, or may be fed to a twin-screw kneading extruder in the form of chopped strands obtained by cutting the rovings. Chopped strands are preferred as the fiber-based filler from the viewpoints of transportation and handling.
[0067] Examples of the fibrous filler include glass fiber, carbon fiber, aramid fiber, and basalt fiber. One type of fibrous filler may be used alone, or two or more types may be used in combination.
[0068] (Glass Fiber) The fiber diameter of the monofilaments forming the glass fiber bundle is not particularly limited, but is preferably in the range of, for example, 6 to 20 μm, and those with diameters of 6 μm, 10 μm, and 13 μm are commonly available on the market.
[0069] The fiber diameter can be determined, for example, by cutting the fibers perpendicular to the fiber direction, measuring the diameters of the cross sections by observing them under a microscope, and calculating the number average of the diameters of 100 or more fibers.
[0070] (Carbon fiber) The type of carbon fiber is not particularly limited, but examples thereof include PAN (polyacrylonitrile)-based carbon fiber, which is mainly made of acrylonitrile, pitch-based carbon fiber, which is mainly made of tar pitch, and rayon-based carbon fiber. For example, PAN-based carbon fiber is preferred from the viewpoint of composition purity and uniformity. The method for producing the carbon fiber is not particularly limited.
[0071] The fiber diameter of the monofilaments forming the carbon fiber bundle may be, for example, more than 2 μm and not more than 15 μm, 3 to 12 μm, or 4 to 10 μm. If the fiber diameter is 2 μm or less, the rigidity of the fiber tends to decrease. If the fiber diameter exceeds 15 μm, the aspect ratio of the fiber (the ratio of length (L) to thickness (D): L / D) decreases, and the rigidity, heat resistance, etc. may decrease.
[0072] As the PAN-based carbon fiber, for example, "Pyrofil" manufactured by Mitsubishi Rayon Co., Ltd., "Torayca" manufactured by Toray Industries, Inc., or "Besfight" manufactured by Toho Tenax Co., Ltd. can be used.
[0073] As the pitch-based carbon fiber, for example, "Dialead" manufactured by Mitsubishi Plastics, Inc., "DonaCarbo" manufactured by Osaka Gas Chemicals, or "Kureka" manufactured by Kureha Chemical Industry Co., Ltd. can be used.
[0074] (Aramid Fiber) The aramid constituting the aramid fiber is preferably meta-aramid, para-aramid, or copolymerized para-aramid, more preferably para-aramid or copolymerized para-aramid, and even more preferably copolymerized para-aramid. Here, the para-aramid refers to an aramid having a structure in which each benzene ring is linearly linked via an amide group (CONH).
[0075] Specific examples of aramid fibers include meta-aramid fibers such as NOMEX, a trade name of DuPont, TEIJINCONEX, a trade name of Teijin Limited, Japan, METASTAR, a trade name of Yantai Co., Ltd., China, and X-FIPER, a trade name of SRO Group, China, as well as TWARON, a trade name of Teijin Limited, KEVLAR, a trade name of DuPont, KERMEL TECH, a trade name of Kermel, and HERACRON, a trade name of Kolon Industries.
[0076] The fiber diameter of the monofilaments forming the aramid fiber bundle may be, for example, 1 to 50 μm, 3 to 30 μm, or 5 to 15 μm, from the viewpoint of increasing the bending strength and impact resistance of the resulting resin composition.
[0077] (Basalt fiber) Basalt fiber is made by melting the mineral basalt in a melting furnace and spinning it into fibers, and is usually made of only basalt. Basalt fiber is usually made of silicon oxide (SiO 2 ) in an amount of 55 to 65 mass % and aluminum oxide (Al 2 O 3 ) 15 to 20 mass % and iron oxide (FeO, Fe 2 O 3 ) etc. Because recrystallization occurs during melt spinning, it tends to have a more homogeneous crystalline structure than other rock wools.
[0078] The fiber diameter of the monofilaments forming the basalt fiber bundle may be, for example, 2 to 15 μm, 6 to 13 μm, or 9 to 13 μm.
[0079] The fibrous filler is preferably glass fiber or carbon fiber.
[0080] In order to improve dispersibility, the fibrous filler may be surface-treated with a surface treatment agent such as an organic silane coupling agent, a titanate coupling agent, an aluminate coupling agent, a zirconate coupling agent, a silicone compound, a higher fatty acid, a fatty acid metal salt, or a fatty acid ester.
[0081] There are no limitations on the binder used to bind the fibrous filler, but for example, when the fibrous filler is an organic fiber, a polar resin or the like is preferably used.
[0082] Examples of polar resins include thermosetting resins such as unsaturated polyesters, vinyl ester resins, epoxy resins, phenolic (e.g., resol) resins, urea-melamine resins, polyimides, urethane resins, copolymers and modified products thereof; and thermoplastic resins such as saturated polyesters, polyamides, acrylic resins, copolymers and modified products thereof, and acid-modified polyolefins.
[0083] [Thermoplastic Resin] Examples of thermoplastic resins include polycarbonate, polybutylene terephthalate, polyethylene terephthalate, polyethylene naphthalate, various polyamides (PA6, PA66, PA46, PA12, semi-aromatic PA, etc.), acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene (AS) resin, methyl methacrylate-styrene (MS) resin, polyethylene, polypropylene, polyacetal, polyamideimide, polyethersulfone, polyimide, polyphenylene oxide, polyphenylene sulfide (PPS resin), polyphenylsulfone, polyetheretherketone, polystyrene, syndiotactic polystyrene, liquid crystalline polyester (liquid crystal polymer), thermoplastic polyurethane, polyvinyl chloride, fluororesin, and mixtures thereof. These may be used alone or in combination of two or more. The thermoplastic resin may be appropriately selected from the properties required for the intended use, such as heat resistance, chemical resistance, and moldability.
[0084] The thermoplastic resin preferably contains at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin, and liquid crystal polymer.
[0085] Although an example of the method for producing the resin composition according to the present embodiment has been described above, the method is not limited to this.
[0086] For example, the transport zone and vent port may or may not be present.
[0087] The resin composition manufacturing method described above involves melt-kneading a thermoplastic resin and a fibrous filler using a twin-screw kneading extruder. The twin-screw kneading extruder is equipped with, in order from upstream as viewed from the flow direction of the melt-kneaded materials, a first feed port, a first kneading zone, a second feed port, and a second kneading zone. The thermoplastic resin and the fibrous filler are fed into the twin-screw kneading extruder from the first feed port and the second feed port, respectively. In the first kneading zone, 50% by mass or more of the thermoplastic resin fed from the first feed port is melted. The second kneading zone is equipped with screw segments composed of flights or disks, and at least a portion of the top end faces of the flights and the end faces of the disks are composed of one or more arcs with a curvature radius R of 0.4 mm or more as viewed perpendicular to the axial direction of the flights or disks. This method allows the remaining fiber length to be maintained long.
[0088] The top end faces of the flights and the end faces of the disks in the second kneading zone may be, for example, configured on the downstream and upstream sides with one or more arcs having a curvature radius R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flights or disks.
[0089] The above method may further include, for example, a conveying zone composed of flights downstream of the second kneading zone, and the downstream side of the top end face of the flight of the conveying zone may be composed of one or more arcs having a radius of curvature R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or disk.
[0090] The second kneading zone may have, for example, from upstream in the direction of material flow, a mixing and dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, and the resistance section is equipped with a screw segment composed of a flight or a disk, and the flight or disk of the resistance section may be composed of one or more arcs with a radius of curvature R = 0.4 mm or more on the upstream side or the upstream and downstream sides of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
[0091] The mixing and dispersion section may, for example, comprise a screw segment composed of a flight or a disk, and the flight or disk of the mixing and dispersion section may be configured with one or more arcs having a curvature radius R of 0.4 mm or more on the downstream side or the upstream and downstream sides of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
[0092] The flights of the mixing / dispersing section are preferably single or double flights with a length of 3D or more, and the clearance between the flights and the cylinder is preferably 1.3% or more of the cylinder diameter.
[0093] [Resin Composition] The resin composition (fiber-based filler reinforced thermoplastic resin composition) obtained by the resin composition manufacturing method according to this embodiment maintains the inherent performance of the thermoplastic resin composition while improving its mechanical strength due to the fiber-based filler. The resin composition has long fiber length and is considered to have excellent mechanical strength, such as flexural modulus. The resin composition can be subjected to various molding methods, such as injection molding, extrusion molding, compression molding, blow molding, and injection compression molding. In particular, it is suitable for use in injection molding. The resin composition is suitable for use in, for example, plastic parts that require mechanical strength. The resin composition is particularly suitable for use in automobile parts, building materials, electrical appliance parts, and the like.
[0094] The present invention will be described below using examples and comparative examples, but the present invention is not limited to these examples.
[0095] (Materials) The materials used in the examples and comparative examples are shown below.
[0096] [Thermoplastic resins] AS resin: Cevian N050SF (melt index (MI) 32 g / 10 min) manufactured by Daicel Miraize Co., Ltd. PA6 resin: A1020BRL (melt index (MI) 34 g / 10 min) manufactured by Unitika Ltd. PP resin: Noblen R101 (melt index (MI) 20 g / 10 min) manufactured by Sumitomo Chemical Co., Ltd. to which 1.5% maleic anhydride-modified PP has been added.
[0097] [Glass fiber bundle] GF (1): ECS03 T-351 manufactured by Nippon Electronic Glass Co., Ltd. (chopped strands of 3 mm length formed by bundling monofilaments of 13 μm diameter) GF (2): ECS03 T-249H manufactured by Nippon Electronic Glass Co., Ltd. (chopped strands of 3 mm length formed by bundling monofilaments of 10.5 μm diameter) GF (3): ECS03 T-480H manufactured by Nippon Electronic Glass Co., Ltd. (chopped strands of 3 mm length formed by bundling monofilaments of 10.5 μm diameter) GF (4): ER2310T-431N manufactured by Nippon Electronic Glass Co., Ltd. (roving formed by bundling monofilaments of 17 μm diameter)
[0098] The materials were used so that the resin composition would contain 70% by weight of thermoplastic resin and 30% by weight of glass fiber bundles.
[0099] (Configuration and Conditions of the Extruder) A twin-screw extruder was used, which was equipped with, from upstream to downstream in the direction of flow of the melt-mixed material, a first feed port, a first kneading zone, a second feed port, a second kneading zone, and a conveying zone, and the second kneading zone had, from upstream to upstream in the direction of flow of the material, a mixing / dispersion section and a resistance section. The thermoplastic resin and the fibrous filler were fed into the twin-screw extruder from the first feed port and the second feed port, respectively, and 50% by mass or more of the thermoplastic resin fed from the first feed port was melted in the first kneading zone. The configuration and conditions of the extruder used are shown below.
[0100] Extruder (1): Co-rotating intermeshing twin-screw extruder TEX25αIII (manufactured by The Japan Steel Works, Ltd.) (twin-screw kneading extruder in Figure 1) Cylinder bore (cylinder diameter): 26.5 mm Cylinder temperature: 250°C, discharge rate: 100 kg / hr Pressure sensors: Installed at the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section), and at positions 43.75 mm upstream (equivalent to 1.75D upstream) and 87.50 mm upstream (equivalent to 3.50D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section).
[0101] [Screw segments] (1) Screw segments used in resistance sections BF: a two-start reverse lead flight with a lead length of 1.0D and a clearance to the cylinder of 0.75% of the cylinder diameter BMS: a single-start reverse lead flight with a lead length of 0.25D and a clearance to the cylinder with a notch in the flight of 0.75% of the cylinder diameter (FIG. 6) BS1: a single-start reverse lead flight with a lead length of 0.25D and a clearance to the cylinder of 3.96% of the cylinder diameter (in FIG. 8, a single-start reverse lead flight with a lead length e of 0.25D and a clearance to the cylinder a of 3.96% of the cylinder diameter dx) BS2: A single reverse lead flight with a radius of curvature R of 0.3 to 0.5 mm only on the upstream side of the flight, a lead length of 0.50 D, and a clearance with the cylinder of 3.96% of the cylinder diameter (in Figure 2, this is a single reverse lead flight with an R of 0.3 to 0.5 mm on the upstream side c of the flight, a lead length e of 0.50 D, and a clearance with the cylinder a of 3.96% of the cylinder diameter dx). BS3: A single reverse lead flight with a radius of curvature R of 0.9 mm only on the upstream side of the flight, a lead length of 0.50 D, and a clearance with the cylinder a of 3.96% of the cylinder diameter (in Figure 2, this is a single reverse lead flight with an R of 0.9 mm on the upstream side c of the flight, a lead length e of 0.50 D, and a clearance with the cylinder a of 3.96% of the cylinder diameter dx). BS4: A single-streak reverse lead flight with a radius of curvature R of 1.8 mm only on the upstream side of the flight, a lead length of 0.50 D, and a clearance with the cylinder of 3.96% of the cylinder diameter (in Figure 2, this is a single-streak reverse lead flight with a radius of curvature R of 1.8 mm on the upstream side c of the flight, a lead length e of 0.50 D, and a clearance with the cylinder a of 3.96% of the cylinder diameter dx). BS5: A single-streak reverse lead flight with a radius of curvature R of 1.8 mm only on the upstream side of the flight, a lead length of 0.25 D, and a clearance with the cylinder of 3.96% of the cylinder diameter (in Figure 3, this is a single-streak reverse lead flight with a radius of curvature R of 1.8 mm on the upstream side c of the flight, a lead length e of 0.25 D, and a clearance with the cylinder a of 3.96% of the cylinder diameter dx).Orthogonal kneading discs: Five discs are arranged in 1D, shifted by 90° in the opposite direction to the screw rotation direction. Reverse kneading discs: Five discs are arranged in 1D, shifted by 45° in the opposite direction to the screw rotation direction (Figure 11).
[0102] (2) Screw segments used in the mixing / dispersing section Double-flighted: a double-flighted with a lead length of 1.5D and a cylinder clearance of 0.75% of the cylinder diameter (in FIG. 10, a double-flighted with a lead length e of 1.5D and a cylinder clearance a of 0.75% of the cylinder diameter dx) Single-flighted a: a single-flighted with a lead length of 1.5D and a cylinder clearance of 3.01% of the cylinder diameter (in FIG. 9, a single-flighted with a lead length e of 1.5D and a cylinder clearance a of 3.01% of the cylinder diameter dx) Single flight b: A single flight with a curvature radius R of 4.0 mm on both sides of the flight, a lead length of 1.5D, and a clearance with the cylinder of 3.01% of the cylinder diameter (in Figure 4, a single flight with R on the upstream side c and downstream side d of the flight of 4.0 mm, a lead length e of 1.5D, and a clearance with the cylinder a of 3.01% of the cylinder diameter dx) Forward kneading disc: A kneading disc with five discs arranged in 1D, shifted by 45° in the same direction as the screw rotation direction
[0103] (3) Screw segments used in the conveying zone Double-row flight a: A double-row flight with a lead length of 1.0D and a cylinder clearance of 0.75% of the cylinder diameter (in FIG. 10, a double-row flight with a lead length e of 1.0D and a cylinder clearance a of 0.75% of the cylinder diameter dx). Double-row flight b: A double-row flight with a lead length of 1.0D and a cylinder clearance of 0.75% of the cylinder diameter, with a radius of curvature R of 0.4 mm given to the downstream side of the flight (in FIG. 7, a double-row flight with a radius of curvature d of 0.4 mm on the downstream side of the flight, a lead length e of 1.0D and a cylinder clearance a of 0.75% of the cylinder diameter dx).
[0104] Extruder (2): Co-rotating intermeshing twin-screw kneading extruder TEM-26SX (manufactured by Shibaura Machine Co., Ltd.) (twin-screw kneading extruder in Figure 13) Cylinder diameter: 26.6 mm Extrusion conditions: cylinder temperature 250°C, discharge rate 50 kg / hour Pressure sensor: installed at the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section), and at a position 40.0 mm upstream (corresponding to 1.61 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section).
[0105] [Screw Segment] (1) Screw segment used in resistance section BS6: Single-start reverse lead flight with a radius of curvature R of 1.0 mm only on the upstream side of the flight, a lead length of 0.52D, and a clearance with the cylinder of 3.95% of the cylinder diameter (in FIG. 14, this is a single-start reverse lead flight with a radius of curvature c of 1.0 mm, a lead length e of 0.52D, and a clearance with the cylinder a of 3.95% of the cylinder diameter dx).
[0106] (2) Screw segment used in the mixing / dispersion section Single-row flight c: A single-row flight having a radius of curvature R of 9.0 mm only on the downstream side of the flight, a lead length of 1.09 D, and a clearance with the cylinder of 6.02% of the cylinder diameter (in FIG. 15, the radius of the downstream side d of the flight is 9.0 mm, the lead length e is 1.09 D, and the clearance with the cylinder a is 6.02% of the cylinder diameter dx).
[0107] (3) Screw segment used in the conveying zone: Double-start flight c: Double-start flight with a lead length of 1.09D and a clearance to the cylinder of 3.76% of the cylinder diameter (in FIG. 10, the lead length e is 1.09D and the clearance a to the cylinder is 3.76% of the cylinder diameter dx).
[0108] Examples 1 to 4 and Comparative Examples 1 to 3: 70% by weight of AS resin (Cevian N050SF) and 30% by weight of GF(1) (ECS03 T-351) were melt-kneaded using a co-rotating intermeshing twin-screw extruder, TEX25αIII, to obtain a resin composition. The screw configurations of the resistance section, mixing / dispersion section, and conveying zone of the twin-screw extruder, as well as the screw rotation speed, are shown in Table 1. Table 2 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section), as well as the resin pressures at positions 43.75 mm upstream (corresponding to 1.75 D upstream) and 87.50 mm upstream (corresponding to 3.50 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section).
[0109]
[0110] In the table, the notation "BS2 (2D)" indicates that BS2 has a length of 2D. Similarly, the notation "two-row flight a (2D)" indicates that "two-row flight a" has a length of 2D. The same applies to other similar notations in this specification.
[0111] (Evaluation of Resin Composition) The resulting resin composition was evaluated according to the following procedures. The evaluation results are shown in Table 2.
[0112] [Glass fiber length] The fiber length of the glass fibers in the obtained resin composition was evaluated according to the following procedures (1) to (5). (1) 5 g of the obtained resin composition was heated under specified conditions and incinerated. (2) The incinerated ash was dispersed in ethanol and uniformly placed in a petri dish. (3) An image was captured using a digital microscope (50x magnification). (4) The size of the glass fibers was measured from the captured image. (5) The average fiber length (weight average fiber length) of the measured values was taken as the glass fiber length.
[0113] [Number of White Spots and Flexural Modulus] The resulting resin composition was dried at 120°C for 4 hours and then molded into test specimens using an injection molding machine IS80EPN-2A manufactured by Shibaura Kikai at a cylinder temperature of 240°C and a mold temperature of 60°C.
[0114] The 30 test pieces were visually inspected to count white spots (unopened GF) of 0.5 mm or more, and the number of white spots was quantified.
[0115] The flexural modulus of the test piece was measured using a Tensilon universal testing machine RTC-1310A manufactured by A&D.
[0116]
[0117] For Example 1, the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section), and the resin pressure at positions 43.75 mm upstream (corresponding to 1.75D upstream) and 87.50 mm upstream (corresponding to 3.50D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing-dispersion section) are shown in Figure 12. As is clear from Figure 12, in Example 1, the pressure is highest at the upstream end of the resistance section and decreases toward the downstream side, and the mixing-dispersion section has a region configured with screw segments in which the pressure decreases from the downstream end (upstream end of the resistance section) toward the upstream side.
[0118] (Example 5 and Comparative Example 4) 70% by weight of PA6 resin (A1020BRL) and 30% by weight of GF(2) (ECS03 T-249H) were melt-kneaded using a co-rotating intermeshing twin-screw extruder TEX25αIII to obtain a resin composition. The screw configurations of the resistance section and mixing / dispersion section of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 3. The conveying zone had the same configuration as in Example 1. Table 4 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section), as well as the resin pressures at positions 43.75 mm upstream (corresponding to 1.75D upstream) and 87.50 mm upstream (corresponding to 3.50D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section).
[0119]
[0120] The glass fiber length of the resulting resin composition was evaluated in the same manner as in Example 1. The results are shown in Table 4.
[0121]
[0122] (Example 6 and Comparative Example 5) 70 wt% PP resin (Noblen R101 with maleic anhydride-modified PP added) and 30 wt% GF(3) (ECS03 T-480H) were melt-kneaded using a co-rotating intermeshing twin-screw extruder TEX25αIII to obtain a resin composition. The screw configurations of the resistance section and mixing / dispersion section of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 5. The conveying zone had the same configuration as in Example 1. Table 6 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section), as well as the resin pressures at positions 43.75 mm upstream (corresponding to 1.75 D upstream) and 87.50 mm upstream (corresponding to 3.50 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section).
[0123]
[0124] The glass fiber length of the resulting resin composition was evaluated in the same manner as in Example 1. The results are shown in Table 6.
[0125]
[0126] Examples 7 to 9: 70% by weight of AS resin (Cevian N050SF) and 30% by weight of GF(4) (ER2310T-431N) were melt-kneaded using a co-rotating intermeshing twin-screw extruder TEM-26SX to obtain a resin composition. The screw configurations of the resistance section, mixing / dispersion section, and conveying zone of the twin-screw kneading extruder, as well as the screw rotation speed, are shown in Table 7. Table 8 also shows the resin pressure at the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section) and the resin pressure at a position 40.0 mm upstream (corresponding to a distance of 1.61 D upstream) from the upstream end of the resistance section (i.e., the downstream end of the mixing / dispersion section).
[0127]
[0128] The glass fiber length of the resulting resin composition was evaluated in the same manner as in Example 1. The results are shown in Table 8.
[0129]
[0130] It can be seen that the method according to the example can maintain a long residual fiber length compared to the method according to the comparative example. In other words, it can be seen that the method according to the example can produce a resin composition with a long residual fiber length.
[0131] 1a, 1b...supply ports, 5...vent port, 10...notched segment, 20...supply zone, 21...first kneading zone, 22, 24...conveying zone, 23...second kneading zone, 23b...resistance section, 23a...mixing and dispersing section.
Claims
1. A method for producing a resin composition in which a thermoplastic resin and a fibrous filler are melt-kneaded using a twin-screw kneading extruder, the twin-screw kneading extruder having, in order from upstream as viewed in the flow direction of the materials to be melt-kneaded, a first supply port, a first kneading zone, a second supply port, and a second kneading zone, the thermoplastic resin and the fibrous filler are supplied to the twin-screw kneading extruder from the first supply port and the second supply port, respectively, and in the first kneading zone, 50% by mass or more of the thermoplastic resin supplied from the first supply port is melted, and the second kneading zone has a screw segment composed of a flight or a disk, and at least a portion of the top end face of the flight and the end face of the disk are composed of one or more arcs with a radius of curvature R = 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight or the disk.
2. A method for producing a resin composition as described in claim 1, wherein the second kneading zone has, from the upstream in the direction of material flow, a mixing and dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, the resistance section having a screw segment composed of a flight or a disk, and the flight or disk of the resistance section is composed of one or more arcs with a radius of curvature R = 0.4 mm or more on the upstream side of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
3. A method for producing a resin composition as described in claim 1, wherein the second kneading zone has, from the upstream in the direction of material flow, a mixing and dispersion section that mixes the materials and disperses the fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, the resistance section having a screw segment composed of a flight or a disk, and the flight or disk of the resistance section is composed of one or more arcs with a radius of curvature R = 0.4 mm or more on the upstream and downstream sides of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
4. A method for producing a resin composition according to any one of claims 1 to 3, wherein the second kneading zone has, from the upstream in the direction of material flow, a mixing / dispersing section that mixes the materials and disperses a fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, the mixing / dispersing section having a screw segment composed of a flight or a disk, and the flight or disk of the mixing / dispersing section is composed of one or more arcs with a radius of curvature R = 0.4 mm or more on the downstream side of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
5. A method for producing a resin composition according to any one of claims 1 to 3, wherein the second kneading zone has, from the upstream in the direction of material flow, a mixing / dispersing section that mixes the materials and disperses a fibrous filler in the thermoplastic resin, and a resistance section that blocks the flow of the materials, the mixing / dispersing section having a screw segment composed of a flight or a disk, and the flight or disk of the mixing / dispersing section is composed of one or more arcs with a radius of curvature R = 0.4 mm or more on the upstream and downstream sides of the top end face of the flight or the end face of the disk when viewed from a direction perpendicular to the axial direction of the flight or disk.
6. A method for producing a resin composition as described in claim 4, wherein the flight of the mixing and dispersion section is a single flight or double flight having a length of 3D or more, and the clearance between the flight and the cylinder is 1.3% or more of the cylinder diameter.
7. A method for producing a resin composition according to any one of claims 1 to 3, further comprising a transport zone composed of flights downstream of the second kneading zone, wherein the downstream side of the top end face of the flight in the transport zone is composed of one or more circular arcs having a radius of curvature R of 0.4 mm or more when viewed from a direction perpendicular to the axial direction of the flight.
8. A method for producing a resin composition according to any one of claims 1 to 3, wherein the fibrous filler is glass fiber or carbon fiber.
9. A method for producing a resin composition according to any one of claims 1 to 3, wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin and liquid crystal polymer.
10. A resin composition obtained by the method for producing a resin composition according to any one of claims 1 to 3, wherein the thermoplastic resin comprises at least one selected from the group consisting of polypropylene, polyester, polyamide, polycarbonate, polystyrene, polyphenylene ether, ABS resin, AS resin, PPS resin and liquid crystal polymer.
Citation Information
Patent Citations
Raw material for electromagnetic wave-shielding material and its production
JP1997235382A
Method and device for the production of a fibre-reinforced plasticate
US20210268717A1
Method for manufacturing resin composition and biaxial kneading and extruding machine
WO2017179584A1