Steel manufacturing method and casting method

By combining blast furnace and electric furnace-produced steels at specific ratios and refining the resulting molten steel, the method addresses the challenge of producing high-quality steel with low impurities and reduced carbon emissions, achieving carbon neutrality in steel manufacturing.

WO2024232557A1PCT designated stage expired Publication Date: 2024-11-14POHANG IRON & STEEL CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2024/005066
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-04-16
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The steel industry faces challenges in producing high-quality steel with low impurity content and reduced carbon emissions, as electric furnace-produced molten steel has higher impurity levels and carbon content compared to blast furnace-produced molten iron, making it difficult to manufacture high-grade steel while minimizing carbon footprint.

Method used

A method involving the stepwise combination of blast furnace molten iron and electric furnace molten steel at specific ratios, followed by refining, to produce secondary molten steel with controlled impurity and carbon levels, reducing carbon emissions and improving steel quality.

Benefits of technology

This approach enables the efficient production of high-grade steel with reduced impurity and carbon content, achieving carbon neutrality by minimizing carbon dioxide emissions and enhancing the refining quality of the final steel product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2024005066_14112024_PF_FP_ABST
    Figure KR2024005066_14112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a steel manufacturing method and a casting method using same, the steel manufacturing method comprising the steps of: providing first molten iron; providing first molten steel having a lower carbon (C) content than the first molten iron; mixing the first molten iron and the first molten steel in a ratio ranging from 20.3:79.7 to 98.6:1.4; charging second molten iron prepared by the mixing step into a refining vessel; and refining the second molten iron to prepare second molten steel. Accordingly, high-grade steel can be efficiently manufactured and carbon emissions can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Steel manufacturing method and casting method

[0001] The present invention relates to a method for manufacturing steel and a casting method, and more particularly, to a method for manufacturing steel and a casting method capable of efficiently manufacturing high-grade steel and reducing carbon emissions.

[0002] To address the climate change crisis, carbon-neutral technologies are being actively developed to minimize carbon emissions. Accordingly, the steel industry is focusing its research and development on electric furnace technology, which can melt raw materials using electricity instead of blast furnaces, which generate large amounts of carbon, thereby minimizing carbon emissions.

[0003] Electric furnaces (EFFs) supply power to electrodes, utilizing the heat and arc generated by the electrodes to melt raw materials. However, molten steel produced in EFs has a higher content of impurities than molten iron produced in blast furnaces, making it difficult to produce high-quality steel products, such as automobile exterior panels, using EF-made molten steel.

[0004] The technology underlying the present invention is disclosed in the following patent documents.

[0005] (Patent Document 1) KR10-2020-0035705 A

[0006] (Patent Document 2) KR10-1883382 B1

[0007] The present invention provides a steel manufacturing method and a casting method capable of efficiently manufacturing high-grade steel.

[0008] The present invention provides a method for manufacturing steel and a casting method capable of reducing carbon generation.

[0009] A method for manufacturing steel according to an embodiment of the present invention comprises the steps of: preparing first molten iron; preparing first molten steel having a lower carbon (C) content than the first molten iron; combining the first molten iron and the first molten steel in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4; charging second molten iron produced by the combining process into a refining vessel; and refining the second molten iron to produce second molten steel.

[0010] The above-mentioned melting process is performed stepwise in multiple rounds, and the melt produced in the preceding round is used for the melting of the subsequent round. The first molten steel is melted only in the first round, and the first molten iron can be melted in all rounds.

[0011] The above-mentioned process of combining may include a process of combining the first molten iron and the first molten steel in a first ratio ranging from 20:80 to 80:20 to produce a combined molten iron; and a process of combining the first molten iron and the combined molten iron in a second ratio ranging from 7:93 to 93:7 to produce a second molten iron.

[0012] A steel manufacturing method according to an embodiment of the present invention includes: a process for preparing first molten iron; a process for preparing first molten steel having a lower carbon (C) content than the first molten iron; a process for producing a molten mixture by mixing the first molten iron and the first molten steel; a process for producing second molten iron by mixing the first molten iron and the molten mixture; a process for charging the second molten iron into a refining vessel; and a process for refining the second molten iron to produce second molten steel.

[0013] The first molten iron may include blast furnace molten iron manufactured in a blast furnace, and the first molten steel may include electric furnace molten steel manufactured in an electric furnace.

[0014] The process of preparing the first molten iron may include a process of manufacturing the first molten iron in a blast furnace so that the carbon (C) content is 4.0 to 4.5 wt%.

[0015] During the manufacturing of the first molten iron, the temperature of the first molten iron can be adjusted to 1,350 to 1,500°C.

[0016] The process for preparing the first molten steel may include a process for manufacturing the first molten steel in an electric furnace so that the carbon (C) content is 0.04 to 1.0 wt% and the oxygen (O) concentration is 5 to 400 ppm; and a process for adjusting the oxygen (O) concentration to 0 to 10 ppm by adding a deoxidizer to the first molten steel.

[0017] During the manufacturing of the first molten steel, the temperature of the first molten steel can be adjusted to 1,580 to 1,700°C.

[0018] The process for producing the above-mentioned molten steel may include: a process of receiving the first molten steel in a plurality of first transport containers having openable openings at the top; a process of receiving the first molten steel in second transport containers having open tops; a process of arranging the second transport containers above a portion of the first transport containers; a process of tilting the second transport containers to inject the first molten steel from the second transport containers into the portion of the first transport containers; and a process of forming the above-mentioned molten steel inside the portion of the first transport containers.

[0019] The process for producing the above-mentioned molten steel may include: a process of receiving the first molten steel in a plurality of first transport containers having openable openings at the top; a process of receiving the first molten steel in a plurality of second transport containers having a plurality of openable openings at the bottom; a process of arranging the second transport containers above a portion of the first transport containers; a process of opening the lower openings of the second transport containers and introducing the first molten steel from the second transport containers into the portion of the first transport containers; and a process of forming the above-mentioned molten steel inside the portion of the first transport containers.

[0020] In the process of manufacturing the above mixture, the temperature of the mixture can be adjusted to 1,430 to 1,650°C.

[0021] The process for manufacturing the second molten iron may include: preparing a loading container having an open top; placing a first transport container containing the molten iron among a plurality of first transport containers having an openable opening at the top thereof on the upper side of the loading container; placing a first transport container containing the first molten iron among a plurality of first transport containers on the upper side of the loading container; tilting the first transport container containing the first molten iron and the first transport container containing the molten iron to inject the molten iron and the remainder of the first molten iron into the loading container; and forming the second molten iron inside the loading container.

[0022] The process for manufacturing the second molten iron may include a process of adjusting the carbon (C) content of the second molten iron to 2 wt% or more and less than 4 wt%; and a process of adjusting the temperature of the second molten iron to 1,350 to 1,500°C.

[0023] The process of charging the second molten iron into the refining vessel may include a process of charging the second molten iron into the refining vessel so that the hot metal ratio (HMR) of the second molten iron is 35 to 100%.

[0024] The process for manufacturing the second molten steel may include a process of injecting a low-smelting gas into the refining vessel; and a process of adjusting the components of the second molten steel so that the nitrogen (N) content is in the range of 22 to 30 ppm, the copper (Cu) content is in the range of 0.02 to 0.04 wt%, and the nickel (Ni) content is in the range of 0.01 to 0.04 wt%.

[0025] The above second molten steel may include Hyper NO steel, HNO steel, MNO steel, LNO steel, EDDQ steel, S-EDDQ steel, DQ steel, DDQ steel, API steel, AHSS steel, and general steel.

[0026] When the standard emission amount of carbon dioxide is 1, the emission amount of carbon dioxide can be reduced to 0.25 in the process of preparing the first molten iron, the process of preparing the first molten steel, and the process of manufacturing the second molten steel.

[0027] A casting method according to an embodiment of the present invention may include a process of preparing steel manufactured by the steel manufacturing method; and a process of casting the prepared steel.

[0028] According to an embodiment of the present invention, first molten iron, which generates a large amount of carbon during manufacturing compared to first molten steel, and first molten steel, which has a higher content of impurity elements than the first molten iron, are mixed in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4 to manufacture second molten iron, and by refining the second molten iron, a sufficient amount of high-quality second molten steel can be manufactured in which the content of impurity elements and the content of carbon are each controlled to a desired level. From this, in gradually achieving carbon neutrality by gradually reducing the production amount of first molten iron and gradually increasing the production amount of first molten steel, the production amount of high-grade steel with a low content of impurity elements, such as ultra-low carbon steel, can be effectively increased, while the amount of carbon generated in the entire manufacturing process can be significantly reduced.

[0029] In addition, according to an embodiment of the present invention, by combining the first molten iron and the first molten steel to produce a mixture, and then combining the first molten iron and the mixture to produce a second molten iron, the mixing ratio of the first molten iron and the first molten steel can be adjusted to a final desired ratio through an intermediate step, thereby enabling a large amount of the first molten iron and a large amount of the first molten steel to be mixed at an accurate mixing ratio, while achieving homogenization of the second molten iron. As a result, the refining quality of the second molten steel can be improved. Accordingly, the casting quality of a semi-finished product cast therefrom can be improved.

[0030] Figure 1 is a flowchart showing a steel manufacturing method according to a first embodiment of the present invention.

[0031] Figure 2 is a process diagram schematically showing the entire process according to the first embodiment of the present invention.

[0032] Figure 3 is a process diagram showing in detail the mixing process according to the first embodiment of the present invention.

[0033] Figure 4 is a flowchart showing a steel manufacturing method according to a second embodiment of the present invention.

[0034] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. However, the present invention is not limited to the embodiments disclosed below and may be implemented in various different forms. These embodiments of the present invention are provided solely to ensure that the disclosure of the present invention is complete and to fully convey the scope of the invention to those skilled in the art. To illustrate the embodiments of the present invention, the drawings may be exaggerated, and like reference numerals in the drawings represent like elements.

[0035] The present invention relates to a method for manufacturing steel and a casting method. Hereinafter, embodiments of the present invention will be described in detail by exemplifying cases in which the method for manufacturing steel and the casting method are applied to manufacturing high-grade steel, such as ultra-low carbon steel used for casting high-grade products such as automobile exterior panels in iron and steel manufacturing operations, and casting semi-finished products therefrom.

[0036] Of course, the steel manufacturing method according to embodiments of the present invention can also be applied to various manufacturing processes for producing various types of molten metals. That is, the steel manufacturing method according to embodiments of the present invention can be applied to manufacturing processes for producing general steel, alloy steel, etc. Similarly, the casting method according to embodiments of the present invention can be applied to various casting processes for casting various types of semi-finished products.

[0037] Figure 1 is a flow chart illustrating a steel manufacturing method according to a first embodiment of the present invention. In addition, Figure 2 is a process diagram schematically illustrating the entire process according to the first embodiment of the present invention, and Figure 3 is a process diagram specifically illustrating the melting process according to the first embodiment of the present invention.

[0038] Referring to FIGS. 1 to 3, a steel manufacturing method according to a first embodiment of the present invention includes a process of preparing first molten iron (S110), a process of preparing first molten steel having a lower carbon (C) content than the first molten iron (S120), a process of combining the first molten iron and the first molten steel in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4 (S130), a process of charging second molten iron manufactured by combining the molten iron into a refining vessel (S140), and a process of refining the second molten iron to manufacture second molten steel (S150).

[0039] The first molten iron may include blast furnace molten iron manufactured in a blast furnace. In addition, the first molten iron may have a high carbon (C) content of 4.0 to 4.5 wt% based on the total weight. More specifically, the first molten iron may include carbon (C) of 4.0 to 4.5 wt% based on the total weight. In this case, the first molten iron may further include silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), titanium (Ti), chromium (Cr), vanadium (V), nickel (Ni), copper (Cu), and nitrogen (N) in predetermined content ranges, and may include iron (Fe) as the remainder.

[0040] Referring to (a) of FIG. 1 and FIG. 2, in the process of preparing the first molten iron (S110), blast furnace molten iron can be prepared. To this end, the process of preparing the first molten iron (S110) may include a process of manufacturing the first molten iron having a carbon (C) content of 4.0 to 4.5 wt% with respect to the total weight in the blast furnace. More specifically, the process of preparing the first molten iron (S110) may include a process of manufacturing the first molten iron including 4.0 to 4.5 wt% of carbon (C) with respect to the total weight in the blast furnace, further including silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), titanium (Ti), chromium (Cr), vanadium (V), nickel (Ni), copper (Cu), and nitrogen (N) in predetermined content ranges, and including iron (Fe) as the remainder.

[0041] Here, if the carbon (C) content of the first molten iron is outside the range of 4.0 to 4.5 wt% with respect to the total weight, the operating efficiency may be reduced when manufacturing the first molten iron in a blast furnace, and it may be difficult to control the carbon (C) content of the second molten iron to the target content.

[0042] Meanwhile, the process of preparing the first molten iron (S110) may include a process of providing the first molten iron manufactured in a blast furnace so as to have a carbon (C) content of 4.0 to 4.5 wt% with respect to the total weight.

[0043] In addition, the process of preparing the first molten iron (S110) may include a process of adjusting the temperature of the first molten iron to 1,350 to 1,500°C. To this end, the blast furnace operating conditions, such as the amount of hot air and the amount of coke input, may be adjusted to manufacture the first molten iron at a temperature of 1,350 to 1,500°C in the blast furnace. Of course, there may be various methods for adjusting the temperature of the first molten iron to a temperature of 1,350 to 1,500°C. On the other hand, if the temperature of the first molten iron is lower than 1,350°C, the temperature range of the second molten iron manufactured therefrom may be lowered, and an additional temperature increasing process may be required. In addition, if the temperature of the first molten iron is higher than 1,500°C, there is a problem that carbon emissions from the blast furnace increase.

[0044] The first molten steel may include electric furnace molten steel manufactured in an electric furnace. In addition, the first molten steel may have a lower carbon (C) content than the first molten iron. That is, the first molten steel may have a low carbon (C) content of 0.04 to 1.0 wt% based on the total weight. More specifically, the first molten steel may include carbon (C) in an amount of 0.04 to 1.0 wt% based on the total weight, and may further include silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), titanium (Ti), chromium (Cr), vanadium (V), nickel (Ni), copper (Cu), and nitrogen (N), and may include iron (Fe) as the remainder.

[0045] In the process (S120) of preparing the first molten steel having a lower carbon (C) content than the first molten steel, the molten steel may be prepared using an electric furnace. For example, the process (S120) of preparing the first molten steel may include a process of manufacturing the first molten steel in an electric furnace so that the carbon (C) content is 0.04 to 1.0 wt% and the oxygen (O) concentration is 5 to 400 ppm. To be more specific, the process of preparing the first molten steel (S120) may include a process of manufacturing the first molten steel in an electric furnace, which contains carbon (C) in an amount of 0.04 to 1.0 wt% based on the total weight, and further contains silicon (Si), manganese (Mn), phosphorus (P), sulfur (S), titanium (Ti), chromium (Cr), vanadium (V), nickel (Ni), copper (Cu), and nitrogen (N), and contains iron (Fe) as the remainder, and has an oxygen (O) concentration of 5 to 400 ppm. At this time, the component contents of the first molten steel manufactured in the electric furnace can be adjusted as described above by controlling the types and amounts of input materials such as direct reduced iron, scrap, and carbonaceous material input to the electric furnace.

[0046] Here, if the first molten steel contains less than 0.04 wt% of carbon (C) with respect to the total weight, the operating efficiency may be reduced when manufacturing the first molten steel in an electric furnace. In addition, if the first molten steel contains more than 1.0 wt% of carbon (C) with respect to the total weight, there is a problem in that the amount of the first molten steel increases to match the carbon content of the second molten steel, and thus the content of impurity components originating from the first molten steel increases. Meanwhile, the concentration of oxygen (O) may be set to be 5 to 400 ppm depending on the aforementioned carbon (C) content when manufacturing the first molten steel in an electric furnace.

[0047] Of course, the process of preparing the first molten steel (S120) may include a process of providing the first molten steel, which is manufactured in an electric furnace and has carbon (C) of 0.04 to 1.0 wt% with respect to the total weight and an oxygen (O) concentration of 5 to 400 ppm.

[0048] In addition, the process of preparing the first molten steel (S120) may include a process of adjusting the temperature of the first molten steel to a temperature of 1,580 to 1,700°C. This process may be performed while manufacturing the first molten steel in an electric furnace. For example, while melting direct reduced iron, scrap, etc. in an electric furnace, the temperature of the first molten steel may be adjusted to a temperature of 1,580 to 1,700°C by controlling operating conditions such as the lowering speed of the electrode and the amount of power supplied to the electrode. If the temperature of the first molten steel is lower than 1,580°C, the temperature range of the second molten iron manufactured therefrom may be lowered, and an additional temperature raising process may be required. In addition, if the temperature of the first molten iron is higher than 1,700°C, there is a problem that the consumption of the electrode in the electric furnace increases. Meanwhile, there may be various methods for adjusting the temperature of the first molten steel to 1,580 to 1,700°C.

[0049] In addition, the process of preparing the first molten steel (S120) may include, after the process of manufacturing the first molten steel in an electric furnace, a process of adding a deoxidizer to the first molten steel drawn from the electric furnace to adjust the concentration of oxygen (O) to 0 to 10 ppm. At this time, the deoxidizer may include an Al or Si-based deoxidizer. Here, the Al-based deoxidizer may contain an aluminum (Al) component, and the Si-based deoxidizer may contain a silicon (Si) component. Deoxidation of the first molten steel may be performed in a ladle, for example. Meanwhile, the first molten steel may be stirred during deoxidation using a stirrer such as an impeller or a low-smelling plug.

[0050] By adjusting the concentration of oxygen (O) in the first molten steel to 0 to 10 ppm in the process of preparing the first molten steel (S120), the boiling phenomenon due to the oxidation reaction of oxygen (O) and carbon (C) in the subsequent process (e.g., the process of combining) can be suppressed or prevented, and the overflow of the combined molten steel due to the boiling phenomenon can be suppressed or prevented.

[0051] Meanwhile, the order of the process of preparing the first vessel (S110) and the process of preparing the first steel (S120) is not particularly limited. These processes may be performed simultaneously or together, or sequentially in a prescribed order.

[0052] Once the first molten iron and the first molten steel are prepared, a process (S130) is performed in which the first molten iron and the first molten steel are combined in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4. This process allows the production of the second molten iron. If the mixing ratio of the first molten iron and the first molten steel exceeds the aforementioned ratio range, it may be difficult to reduce carbon emissions and secure a heat source from the converter.

[0053] The step of combining (S130) can be performed in stages in multiple rounds. Being performed in stages means that after performing the combining of the preceding round, the combining of the subsequent round is performed using the combined material. In other words, when the step-by-step ...

[0054] Meanwhile, when the combining process (S130) is performed stepwise in multiple passes, the first molten steel can be combined only in the first pass, and the first molten iron can be combined in all passes. This method allows for a more precise matching of the combining ratios of the first molten iron and the first molten iron. The combining process (S130) will be described below using an example where the number of passes in the multiple passes is two. However, the contents described below can be applied similarly or identically even when the number of passes in the multiple passes is different.

[0055] Referring to (a) and (b) of FIG. 2, the combining process (S130) may include a first combining process and a second combining process. Here, the first combining process may include a process of combining the first molten iron and the first molten steel at a first ratio ranging from 20:80 to 80:20 to produce a combined product. In addition, the second combining process may include a process of combining the first molten iron and the combined product at a second ratio ranging from 7:93 to 93:7 to produce a second molten iron. Of course, the number of turns of the combining process may vary, and accordingly, the combining ratio in each turn may also vary.

[0056] Hereinafter, with reference to (a) and (b) of FIG. 2 and (a) to (f) of FIG. 3, the process of combining (S130) according to an embodiment of the present invention will be described in more detail.

[0057] As described above, the process of combining the first molten iron and the first molten steel (S130) may include a process of combining the first molten iron and the first molten steel at a first ratio ranging from 20:80 to 80:20 to produce a mixture, and a process of combining the first molten iron and the mixture at a second ratio ranging from 7:93 to 93:7 to produce a second molten iron.

[0058] At this time, the process of manufacturing the molten steel may include a process of receiving the first molten steel in a plurality of first transport containers having openable openings at the top, a process of receiving the first molten steel in a second transport container having an open top, a process of arranging the second transport containers on the upper side of some of the first transport containers among the plurality of first transport containers, a process of pouring the first molten steel from the second transport containers into some of the first transport containers, and a process of forming the molten steel inside some of the first transport containers.

[0059] Referring to (a) of Fig. 2, the first molten iron produced from the blast furnace can be accommodated in a plurality of first transport containers. At this time, the first transport containers may have an openable opening at the top. For example, the first transport containers may include a torpedo ladle car (TLC). Of course, the types of the first transport containers may vary. Meanwhile, some of the plurality of first transport containers may be transported to a mixing area where the first mixing can be performed ((d) of Fig. 3), and the rest may be transported to a repair area where the second mixing can be performed ((f) of Fig. 3). For example, the number of first transport containers may be four, and two of them may be transported to the mixing area, and the remaining two may be transported to the repair area. Of course, the number of first transport containers, the number of first transport containers transported to the bundling yard, and the number of first transport containers transported to the repair yard may vary.

[0060] Referring to (a) of Fig. 3, the first molten steel tapped from the electric furnace can be accommodated in a second transport container. At this time, the second transport container can have multiple openings that can be opened and closed at the bottom. The opening and closing of each of the multiple openings can be controlled by a slide gate. In addition, the second transport container can have an open top. For example, the second transport container can include a ladle. Of course, the type of the second transport container can be various. Meanwhile, after the second transport container accommodates the first molten steel, it can be transported to a mixing yard. At this time, the second transport container can be transported to the mixing yard using a tapping cart, a crane, etc. (Fig. 3 (b), (c)).

[0061] Hereafter, referring to (d) of FIG. 3, the second transport container (ladle) can be placed on the upper side of the first transport container (TLC). For example, the second transport container (ladle) transported to the mixing tank can be placed on the upper side of the settling platform installed in the mixing tank, and the first transport container (TLC) can be introduced and stopped under the settling platform. In addition, by opening the lower opening of the second transport container (ladle) and pouring the first molten steel from the second transport container (ladle) into the first transport container (TLC), the first molten iron and the first molten steel can be combined. In addition, the second transport container (ladle) can be tilted and the first molten steel can be poured from the second transport container (ladle) into the first transport container (TLC), thereby combining the first molten iron and the first molten steel.

[0062] Here, in combining the first molten iron and the first molten steel, the first molten iron and the first molten steel can be divided into equal amounts within the margin of error, and combined at the same ratio within the margin of error. That is, the first molten iron to be combined during the first combining can be divided into equal amounts within the margin of error and accommodated in two first transport containers (TLC). In addition, the two first transport containers (TLC) are sequentially introduced into the lower portion of the settling platform so that the same amount of the first molten steel can be charged into each of the two first transport containers (TLC) from the second transport container (ladle) within the margin of error, and the opening and closing of the lower opening of the second transport container (ladle) is controlled so that the first molten steel can be divided and charged into each of the first transport containers (TLC). Similarly, the tilting method can control the tilting of the second transport vessel (ladle) so that the same amount of first molten steel can be injected into each first transport vessel (TLC) within a margin of error. At this time, the first molten iron and the first molten steel can be combined in each transport vessel (TLC) at a first ratio ranging from 20:80 to 80:20.

[0063] In addition, a mixture can be formed inside each of the plurality of first transport containers (TLC). That is, by mixing the first molten iron and the first molten steel inside the first transport container (TLC) using the kinetic energy of the first molten steel generated when the first molten steel is injected, a mixture can be formed inside the first transport container (TLC).

[0064] Meanwhile, during the process of manufacturing the molten metal, the temperature of the molten metal can be adjusted to a temperature of 1,430 to 1,650°C. For example, by controlling the time for transporting each transport container and the speed at which the first molten metal is injected, the range of temperature drop of the first molten metal and the first molten steel during the molten metal mixing process can be adjusted, and thereby the temperature of the molten metal can be adjusted to a temperature of 1,430 to 1,650°C.

[0065] Meanwhile, in the process of manufacturing a mixture, the mixture can be manufactured within the charging vessel by charging the first molten iron and the first molten steel into the charging vessel and mixing them.

[0066] When the process for manufacturing the mixed solution is completed, a process for manufacturing the second molten iron can be performed. The process for manufacturing the second molten iron can include a process for preparing a loading container having an open top, a process for arranging a first transport container containing the mixed solution among a plurality of first transport containers having an openable opening at the top thereof, on the upper side of the loading container, a process for arranging the first transport container containing the first molten iron among the plurality of first transport containers so as to face the first transport container containing the mixed solution on the upper side of the loading container, a process for tilting the first transport container containing the first molten iron and the first transport container containing the mixed solution to inject the mixed solution and the first molten iron into the loading container, and a process for forming the second molten iron inside the loading container.

[0067] Referring to (e) and (f) of FIG. 3, first, an open-top loading container can be prepared. At this time, the loading container can be placed in a repair area. In addition, the loading container can include, for example, loading ladle. Then, the first transport container containing the molten mixture (molten mixture TLC) and the first transport container containing the first molten iron (molten iron TLC) can be moved to the upper side of the loading container (loading ladle) and then placed to face each other. At this time, the loading container (loading ladle) can be positioned between these first transport containers. Thereafter, the first transport container containing the molten mixture (molten mixture TLC) and the first transport container containing the first molten iron (molten iron TLC) can be tilted toward the loading container (loading ladle) so that the molten mixture and the first molten iron can be placed into the charging container (loading ladle). At this time, the first vessel and the combined water can be combined in a second ratio ranging from 7:93 to 93:7.

[0068] In addition, a second molten iron can be formed inside a plurality of charging containers (charging ladle). That is, by mixing the molten iron and the first molten iron inside the charging container (charging ladle) using the kinetic energy generated when the molten iron and the first molten iron are charged, the second molten iron can be formed inside the charging container (charging ladle).

[0069] Meanwhile, in the process of manufacturing the second molten iron, if the molten iron has been manufactured in a charging container in advance, the first molten iron may be charged into the charging container containing the molten iron, and the second molten iron may be manufactured within the charging container.

[0070] Meanwhile, in the process of manufacturing the second molten iron, the carbon (C) content of the second molten iron can be adjusted to 2 wt% or more and less than 4 wt%, and the temperature of the second molten iron can be adjusted to 1,350 to 1,500°C. For example, by adjusting the amount of the combined molten iron and the first molten iron to be mixed so as to satisfy the third ratio, the carbon (C) content of the second molten iron manufactured from the combined molten iron and the first molten iron can be adjusted to 2 wt% or more and less than 4 wt%. In addition, by adjusting the time for transporting each transport container and the speed at which each transport container is tilted, the range of the temperature drop of the combined molten iron and the first molten iron until mixing can be adjusted, and from this, the temperature of the second molten iron can be adjusted to 1,350 to 1,500°C.

[0071] At this time, if the carbon (C) content of the second molten iron is less than 2 wt%, it may be difficult to control the nitrogen (N) content of the second molten iron produced therefrom to 30 ppm or less. In addition, if the carbon (C) content of the second molten iron is 4 wt% or more, there is a problem that the amount of the first molten iron combined increases, resulting in an increase in carbon emissions. In addition, if the temperature of the second molten iron is outside the temperature range of 1,350 to 1,500℃, normal operation during furnace operation may be difficult.

[0072] Referring to FIGS. 1 and 2 (b), when the process of manufacturing the second molten iron is completed, a process (S140) of loading the second molten iron into a refining vessel is performed. At this time, the refining vessel may include, for example, a converter. For example, when the manufacture of the second molten iron is completed in a repair shop, the charging vessel containing the second molten iron is transferred to the converter side after KR treatment, and then raised to the upper side of the converter, and the charging vessel is tilted to receive the second molten iron into the converter through the furnace opening of the converter. In addition, scrap may be loaded into the converter. At this time, the second molten iron and scrap may be loaded into the converter so that the hot metal ratio (HMR: Hot Metal Ratio) of the second molten iron becomes 35 to 100%. Here, the molten iron charge refers to the ratio of the amount of molten iron charged into the furnace to the total amount of molten iron charged into the furnace plus the amount of scrap charged into the furnace.

[0073] In the process of charging the second molten iron into the refining vessel (S140), the charging order of the second molten iron and scrap can vary. For example, scrap can be charged first and then the second molten iron can be charged. Also, the second molten iron can be charged first and then scrap can be charged. Also, the second molten iron and scrap can be charged together. Meanwhile, in the case where the molten iron ratio of the second molten iron is to be 100%, only the second molten iron can be charged into the converter. By charging the second molten iron so that the molten iron ratio is 55 to 100% in the process of charging the second molten iron into the refining vessel (S140), the second molten steel produced thereby can be used as high-grade steel, such as Hyper NO steel, HNO steel, MNO steel, LNO steel, EDDQ steel, S-EDDQ steel, DQ steel, DDQ steel, API steel, and AHSS steel, which will be described later.

[0074] Meanwhile, before loading the second molten iron into the refining vessel, preliminary treatment of the second molten iron can be performed using a KR (kanvara reactor) device if necessary, and components such as silicon (Si), sulfur (S), and phosphorus (P) in the second molten iron can be controlled, for example, reduced.

[0075] Next, a process for manufacturing the second molten steel (S150) is performed. That is, a lance is inserted into the furnace opening of the furnace and placed at the top of the furnace, and then oxygen (O) can be supplied into the interior of the lance. Accordingly, oxygen (O) can be blown into the second molten iron inside the furnace from the lance, and refining, for example, oxygen blowing, can be performed. Accordingly, the second molten iron can be manufactured into the second molten steel. At this time, a low-blowing nozzle can be used to blow a low-blowing gas, for example, argon gas, into the furnace to agitate the second molten iron, and the composition of the second molten steel can be adjusted. At this time, ferrosilicon (Fe-Si), for example, can be injected into the furnace as a heat-generating agent.

[0076] In addition, in the process of manufacturing the second molten steel (S150), the components of the second molten steel can be adjusted so that the nitrogen (N) content is in the range of 22 to 30 ppm, the copper (Cu) content is in the range of 0.02 to 0.04 wt%, and the nickel (Ni) content is in the range of 0.01 to 0.04 wt%.

[0077] According to the process for manufacturing the second molten steel (S150), any one type of steel among Hyper NO steel (Hyper grade Non-grain Oriented electrical steel), HNO steel (High grade Non-grain Oriented electrical steel), MNO steel (Middle grade Non-grain Oriented electrical steel), LNO steel (Low grade Non-grain Oriented electrical steel), EDDQ (Extra Deep Drawing Quality) steel, S-EDDQ (Super Extra Deep Drawing Quality) steel, DQ (Drawing Quality) steel, DDQ (Deep Drawing Quality) steel, API (American Petroleum Institute) steel, AHSS steel (Advenced High Strength steel), and general steel can be manufactured. That is, the second molten steel manufactured according to the first embodiment of the present invention can include Hyper NO steel, HNO steel, MNO steel, LNO steel, EDDQ steel, S-EDDQ steel, DQ steel, DDQ steel, API steel, AHSS steel, and general steel. Among them, Hyper NO steel, HNO steel, MNO steel, and LNO steel can be used for electrical steel sheets. In addition, EDDQ steel and S-EDDQ steel can be used for automobile exterior panels. In addition, DQ steel and DDQ steel can be used for automobile interior panels. Meanwhile, since the component contents of the aforementioned steel types are already known, a detailed description of these steel types is omitted here.

[0078] Meanwhile, in the process of manufacturing the second molten steel (S150), a heat source may be added to the furnace. At this time, the heat source may include a Si-containing ferroalloy and carbon. The heat source may be added to the furnace before or during the second molten steel blowing.

[0079] Furthermore, once the production of the second molten steel is complete, the second molten steel can be drawn from the furnace. At this time, sampling of the second molten steel can be performed before and after drawing, and its temperature can be measured. Furthermore, the second molten steel, once drawn, can be transferred to the next process. This next process may include a casting process.

[0080] Meanwhile, in the first embodiment of the present invention, by manufacturing a mixture using the first molten steel, the amount of carbon dioxide emissions can be reduced below the standard amount of emissions in the process of preparing the first molten steel, the process of preparing the first molten steel, and the process of manufacturing the second molten steel.

[0081] More specifically, when the standard emission amount is 1, the carbon dioxide emissions can be reduced to 0.25 in the process of preparing the first molten iron, the process of preparing the first molten steel, and the process of manufacturing the second molten steel. In other words, the carbon dioxide emissions can be reduced to 25% of the standard emission amount. Here, the standard emission amount may refer to the carbon dioxide emissions in the process of preparing the first molten iron and the process of manufacturing the second molten steel when the process of preparing the first molten iron is omitted and, accordingly, the first molten iron is charged into the converter instead of the second molten iron and refining is performed. In this case, for example, the standard emission amount may be carbon dioxide (CO2) of 1.90 to 1.95 ton CO2 / ton in terms of carbon intensity unit.

[0082] In addition, the amount of carbon dioxide emissions reduced thereby can be, for example, 0.5 to 1.90 tons CO2 / ton of carbon dioxide (CO2) in terms of carbon source unit. At this time, the higher the mixing ratio of the first molten steel, that is, the more the production amount of the first molten steel increases and the less the production amount of the first molten iron accordingly, the more the amount of carbon dioxide emissions can be reduced in the processes of producing the first molten iron, producing the first molten steel, and producing the second molten iron.

[0083] That is, through the processes described above, in the first embodiment of the present invention, from the process of preparing the first molten steel (S110) to the process of manufacturing the second molten steel (S150), carbon dioxide (CO2) of 0.5 to 1.90 tons CO2 / ton can be emitted in terms of carbon intensity. That is, until manufacturing 1 ton of the second molten steel, carbon dioxide (CO2) of 0.5 to 1.90 tons can be emitted. More preferably, carbon dioxide (CO2) of 0.86 to 1.50 tons CO2 / ton can be emitted in terms of carbon intensity. That is, preferably, until manufacturing 1 ton of the second molten steel, carbon dioxide (CO2) of 0.86 to 1.50 tons can be emitted.

[0084] As described above, in the first embodiment of the present invention, the first molten iron and the first molten steel are combined in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4, the second molten iron produced by the combination is charged into a refining vessel, and the second molten iron is refined to produce the second molten steel, thereby lowering the content of impurity elements originating from the first molten steel to a target level, and producing a sufficient amount of high-quality second molten steel in which the contents of important elements such as carbon, copper, and nickel are each controlled to a desired level, while reducing carbon emissions to achieve carbon neutrality.

[0085] Hereinafter, a method for manufacturing steel according to a first embodiment of the present invention will be described with more specific examples.

[0086] First, prepare the first molten iron. That is, manufacture the first molten iron in the blast furnace. At this time, the first lead wire may contain carbon (C) in an amount of 0 to 4.5 wt% or less, silicon (Si) in an amount of 0 to 0.5 wt% or less, manganese (Mn) in an amount of 0 to 0.3 wt% or less, phosphorus (P) in an amount of 0 to 0.12 wt% or less, sulfur (S) in an amount of 0 to 0.015 wt% or less, titanium (Ti) in an amount of 0 to 0.06 wt% or less, chromium (Cr) in an amount of 0 to 0.01 wt% or less, vanadium (V) in an amount of 0 to 0.015 wt% or less, nickel (Ni) in an amount of 0 to 0.01 wt% or less, copper (Cu) in an amount of 0 to 0.001 wt% or less, nitrogen (N) in an amount of 0 to 0.007 wt% or less, and iron (Fe) as the remainder. Additionally, the temperature of the first line can be adjusted within a range of 1,350 to 1,500°C. The values ​​presented here are for the purpose of explaining the first embodiment and are not intended to limit the present invention.

[0087] In addition, the first molten steel is prepared. That is, the first molten steel is manufactured in an electric furnace. At this time, the first molten steel may contain carbon (C) in an amount of 0 to 0.15 wt% or less, silicon (Si) in an amount of 0 to 0.04 wt% or less, manganese (Mn) in an amount of 0 to 0.045 wt% or less, phosphorus (P) in an amount of 0 to 0.009 wt% or less, sulfur (S) in an amount of 0 to 0.023 wt% or less, titanium (Ti) in an amount of 0 to 0.001 wt% or less, chromium (Cr) in an amount of 0 to 0.043 wt% or less, vanadium (V) in an amount of 0 to 0.039 wt% or less, copper (Cu) in an amount of 0 to 0.071 wt% or less, nitrogen (N) in an amount of 0 to 0.004 wt% or less, and may contain iron (Fe) as the remainder. In addition, the oxygen (O) concentration of the first molten steel can be adjusted to 5 to 400 ppm. In addition, the nitrogen (N) concentration of the first molten steel can be adjusted to 0.002 to 0.006 wt%. In addition, the temperature of the first molten steel can be adjusted to 1,580 to 1,700°C. In addition, after the first molten steel is manufactured, the first molten steel can be tapped from an electric furnace, and a deoxidizer can be added to the tapped first molten steel to adjust the oxygen (O) concentration to 0 to 10 ppm. At this time, as in the manufacture of the first molten iron, the values ​​presented for the first molten steel are for explaining the first embodiment and are not intended to limit the present invention.

[0088] Once the first molten iron and the first molten steel are prepared, they are combined. To this end, a predetermined amount of the first molten iron is placed in a torpedo ladle, and a predetermined amount of the first molten steel is placed in a ladle. Furthermore, the torpedo ladle containing the first molten iron and the ladle containing the first molten steel are transported to a combining facility. At this time, the temperature drop of the first molten iron may be in the range of 0°C to 76°C. Furthermore, the temperature drop of the first molten steel may be in the range of 140°C to 170°C.

[0089] The first mixing process is performed in the mixing tank. At this time, the first molten steel can be mixed with the first molten iron in the torpedo ladle by tilting the ladle or opening the lower opening of the ladle to drop the first molten steel from the ladle and feed it into the torpedo ladle car. Accordingly, a mixing product is produced in the torpedo ladle car. At this time, when producing the mixing product, the first molten iron and the first molten steel can be mixed at a first ratio ranging from 20:80 to 80:20. For example, a mixing product can be produced by mixing 200 tons of the first molten iron and 80 tons of the first molten steel, or a mixing product can be produced by mixing 80 tons of the first molten iron and 200 tons of the first molten steel. In addition, a mixing product can be produced by mixing 134 tons of the first molten iron and 146 tons of the first molten steel. Of course, 100 tons of first molten iron and 40 tons of first molten steel can be combined to produce a molten product, and 40 tons of first molten iron and 100 tons of first molten steel can be combined to produce a molten product. And, 67 tons of first molten iron and 73 tons of first molten steel can be combined to produce a molten product. Here, the molten product can be produced in multiple, for example, two torpedo ladle cars, and the amount of the molten product produced in each can be the same within the margin of error.

[0090] Afterwards, two torpedo ladle cars containing the molten metal are moved to the waterline. Here, the temperature drop range of the molten metal may be in the range of 45 to 73°C. In addition, two torpedo ladle cars containing the first molten metal are prepared and moved to the repair site. At this time, the temperature drop range of the first molten metal may be in the range of 0 to 76°C. Through this process, a total of four torpedo ladle cars are placed in the repair site.

[0091] And, a second mixing process is performed in the repair shop. At this time, the second mixing process can be performed so that the first molten iron and the mixed material are mixed in a second ratio ranging from 7:93 to 93:7. To this end, the torpedo ladle car containing the first molten iron and the torpedo ladle car containing the mixed material are arranged to face each other, and the charging ladle is placed between them. Thereafter, each torpedo ladle car is tilted to charge the first molten iron and the mixed material into the charging ladle, thereby producing the second molten iron within the charging ladle. In addition, when the second mixing process is completed, the ladle containing the second molten iron is transferred to the converter side. At this time, the temperature drop range of the second molten iron may be in the range of 71 to 85℃ or less.

[0092] At this time, by performing the first and second mixing as described above, the second molten iron manufactured therefrom can be mixed with the first molten iron and the first molten steel in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4.

[0093] When the second molten iron arrives at the location where the transformer is installed, the second molten iron is injected into the transformer. Additionally, scrap may be injected into the transformer depending on the cost of the molten iron. At this time, when the second molten iron is introduced into the furnace, the second molten iron may contain carbon (C) of 1.9 wt% or more and 4.5 wt% or less, silicon (Si) of 0 to 0.252 wt% or less, manganese (Mn) of 0 to 0.173 wt% or less, phosphorus (P) of 0 to 0.065 wt% or less, sulfur (S) of 0 to 0.019 wt% or less, titanium (Ti) of 0 to 0.031 wt% or less, chromium (Cr) of 0 to 0.027 wt% or less, vanadium (V) of 0 to 0.008 wt% or less, nickel (Ni) of 0 to 0.025 wt% or less, copper (Cu) of 0 to 0.036 wt% or less, and nitrogen (N) of 0.002 wt% to 0.01 wt%, based on the total weight. Iron (Fe) may be included as a residual content. Of course, the values ​​presented for the second lead are for the purpose of explaining the first embodiment and are not intended to limit the present invention.

[0094] And, the second molten iron is refined in the converter to manufacture the second molten steel. At this time, as a comparative example, under different conditions from the experimental examples below, for example, with a molten iron ratio of 47.9%, the second molten steel was fed into the converter together with scrap, and refining was performed by supplying a heat source. The second molten steel produced thereby can be used as, for example, MNO steel, LNO steel, DQ steel, DDQ steel, API steel, AHSS steel, and general steel, but it did not meet the conditions of Hyper NO steel, HNO steel, EDDQ steel, and S-EDDQ steel. This may be because, as the molten iron cost decreases compared to the experimental examples below when charging the furnace, the amount of scrap input increases, and the second molten iron produced from the second molten iron is adjusted so that the nitrogen (N) content is outside the range of 22 to 30 ppm, the copper (Cu) content is outside the range of 0.02 to 0.04 wt%, and the nickel (Ni) content is outside the range of 0.01 to 0.04 wt%.

[0095] In addition, as experimental examples, second molten steel was manufactured by varying the molten iron ratio, charging temperature, and input heat source of the second molten steel according to the conditions presented in Table 1 below, and second molten steel was manufactured in each case. At this time, the types of steel grades that can be used for the second molten steel manufactured are also exemplified in Table 1 below.

[0096] Classification, specific carbon content, charging temperature, input heat source, steel grade, Hyper NOHNOMNOLNOEDDQS-EDDQDQDDQAPIAHSS, general steel, experimental example 156.13.11, 4001, 458, O, O, O, O, O, O, O, O, O, O, O, O, O, O, O, O, O, O, O, Experimental example 256.43.051, 4011, 485, O ...

[0097] The experimental examples presented in Table 1 correspond to the first embodiment of the present invention. As shown in this, the molten iron ratio was set to 56.1% and 56.4%, respectively, and the temperature was set to 1,350 to 1,500℃, and the second molten steel was charged into the converter together with scrap, and refining was performed with the temperature of the input heat source set to 1,458℃. The second molten steel produced thereby can be used in various ways as Hyper NO steel, HNO steel, MNO steel, LNO steel, EDDQ steel, S-EDDQ steel, DQ steel, DDQ steel, API steel, AHSS steel, and general steel. This may be because the second molten steel produced from the second molten iron has a nitrogen (N) content adjusted to a range of 22 to 30 ppm, a copper (Cu) content adjusted to a range of 0.02 to 0.04 wt%, and a nickel (Ni) content adjusted to a range of 0.01 to 0.04 wt%. From this, it can be seen that when the steel production process according to the first embodiment is performed, high-grade steel can be produced.

[0098] Thus, according to the first embodiment of the present invention, a first molten iron is prepared, a first molten steel having a lower carbon (C) content than the first molten iron is prepared, and the first molten iron and the first molten steel are mixed in a first ratio ranging from 160:80 to 220:20 to manufacture a second molten iron. In addition, by refining the second molten iron to manufacture the second molten steel, the nitrogen (N) content of the second molten steel can be adjusted to a range usable as high-grade steel, while the amount of the first molten iron used can be reduced, thereby reducing the amount of carbon generated in the entire process.

[0099] Although the first embodiment of the present invention has been described as above, the present invention can be configured in various ways, including the second to fourth embodiments below.

[0100] Figure 4 is a flowchart showing a steel manufacturing method according to a second embodiment of the present invention.

[0101] In the first embodiment of the present invention described above, the first molten iron and the first molten steel were mixed at the first ratio to produce the second molten iron. However, this is not limited thereto, and in the second embodiment of the present invention described below, the first molten iron and the first molten steel may be mixed to produce a mixture, and the first molten iron and the mixture may be mixed to produce the second molten iron. At this time, the mixing ratios thereof may vary.

[0102] Hereinafter, with reference to FIG. 4, a steel manufacturing method according to a second embodiment of the present invention will be described. At this time, the second embodiment will be described in detail, focusing on features that distinguish it from the aforementioned first embodiment of the present invention, and any content that overlaps with the description of the aforementioned first embodiment of the present invention will be omitted or briefly described.

[0103] Referring to FIG. 4, a steel manufacturing method according to a second embodiment of the present invention includes a process of preparing first molten iron (S210), a process of preparing first molten steel having a lower carbon (C) content than the first molten iron (S220), a process of mixing the first molten iron and the first molten steel to produce a mixture (S230), a process of mixing the first molten iron and the mixture to produce second molten iron (S240), a process of charging the second molten iron into a refining vessel (S250), and a process of refining the second molten iron to produce second molten steel (S260).

[0104] At this time, the process of preparing the first molten iron (S210), the process of preparing the first molten steel having a lower carbon (C) content than the first molten iron (S220), the process of charging the second molten iron into a refining vessel (S250), and the process of refining the second molten iron to manufacture the second molten steel (S260) may have the same or similar configurations and methods as the process of preparing the first molten iron (S110), the process of preparing the first molten steel having a lower carbon (C) content than the first molten iron (S120), the process of charging the second molten iron manufactured by smelting into a refining vessel (S140), and the process of refining the second molten iron to manufacture the second molten steel (S150) in the first embodiment of the present invention described above, and therefore, the description thereof is omitted.

[0105] In the process of manufacturing a mixture by combining the first molten iron and the first molten steel (S230), the first molten iron may be accommodated in a plurality of first transport containers, the first molten steel may be accommodated in a second transport container, and the second transport containers may be placed on the upper side of some of the first transport containers among the plurality of first transport containers. In addition, the first molten steel may be introduced from the second transport containers into some of the first transport containers, and the mixture may be formed inside some of the first transport containers.

[0106] At this time, while the first molten steel is being fed, the weight of the second transport container can be measured using a weight measuring device, such as a load cell. In addition, the control unit can receive the weight from the load cell, obtain the discharge amount of the first molten steel therefrom, and control the operation of a tilting actuator for tilting the second transport container according to the obtained discharge amount, thereby adjusting the inclination angle of the second transport container. For example, the operation of the tilting actuator can be controlled so that the inclination angle of the second transport container decreases as the discharge amount approaches the standard discharge amount. From this, the amount of the first molten steel fed can be accurately adjusted. Similarly, the control unit can control the operation of a slide gate that opens and closes the lower opening of the second transport container, thereby adjusting the opening degree of the slide gate according to the discharge amount of the first molten steel.

[0107] In the process of manufacturing the second molten iron by combining the first molten iron and the molten material (S240), a charging container is prepared, a first transport container containing the molten iron among a plurality of first transport containers is placed on the upper side of the charging container, a first transport container containing the first molten iron among a plurality of first transport containers is placed on the upper side of the charging container, and the first transport container containing the first molten iron and the first transport container containing the molten material are tilted to inject the molten iron and the first molten iron into the charging container, so that the second molten iron can be formed inside the charging container. At this time, the first molten iron and the molten material can be combined at a predetermined ratio. In addition, the mixing ratio of the first molten iron and the molten material when manufacturing the second molten iron can be determined according to the mixing ratio of the first molten iron and the first molten steel when manufacturing the mixing material. That is, the final mixing ratio of the first molten iron and the first molten steel for manufacturing the second molten iron can be determined at a predetermined ratio, and the mixing ratio of the first molten iron and the first molten steel at the time of manufacturing the mixing ratio can be obtained from the process (S230) of mixing the first molten iron and the first molten steel to manufacture the mixing product. Accordingly, the mixing ratio of the first molten iron and the mixing product at the time of manufacturing the second molten iron is determined according to the mixing ratio of the first molten iron and the first molten steel at the time of manufacturing the mixing product, so that the final mixing ratio can reach the predetermined ratio. Meanwhile, the configurations of the steel manufacturing methods of the first and second embodiments described above can be changed by combining each other.

[0108] Meanwhile, according to the third embodiment of the present invention, in the process of producing a mixture by the first mixing and the process of producing a second molten iron by the second mixing, the mixing can be performed in a refining vessel, such as a converter. That is, the first molten iron and the first molten steel can be charged into a converter and mixed to produce a mixture, and the first molten iron can be charged into the converter in which the mixture has been produced to produce the second molten iron. Accordingly, intermediate processes such as transportation are omitted until the charging into the converter, so that a temperature drop can be suppressed or prevented, and from this temperature perspective, the heating power can be lowered by lowering the electric furnace tapping temperature.

[0109] Hereinafter, a casting method according to a fourth embodiment of the present invention will be described. The casting method according to the fourth embodiment of the present invention may include a process of preparing steel manufactured using a steel manufacturing method according to the first to third embodiments of the present invention, and a process of casting the prepared steel.

[0110] First, steel manufactured using the steel manufacturing methods according to the first to third embodiments described above is prepared. For example, according to the steel manufacturing methods according to the first to third embodiments, steel manufactured in a converter is drawn from the converter into a ladle. The ladle is then transported to a casting facility, where the steel is cast to manufacture a semi-finished product. The semi-finished product may be in various forms, such as a slab, a thin plate slab, a coil, a billet, or a bloom. Furthermore, the configuration and method of the casting facility for casting these products may also vary.

[0111] The above embodiments of the present invention are intended to illustrate the present invention and are not intended to limit the present invention. It should be noted that the configurations and methods disclosed in the above embodiments of the present invention may be combined or intersected with each other and combined and modified in various forms, and that such modifications may also be considered within the scope of the present invention. In other words, the present invention may be implemented in various different forms within the scope of the claims and equivalent technical concepts thereof, and those skilled in the art will understand that various embodiments are possible within the scope of the technical concepts of the present invention.

Claims

1. The process of preparing the first charter; A process for preparing first molten steel having a lower carbon (C) content than the first molten steel; A process of combining the first molten iron and the first molten steel in a ratio (%) ranging from 20.3:79.7 to 98.6:1.4; The process of loading the second molten iron produced by the above-mentioned combination into a refining vessel; and A steel manufacturing method comprising a process of refining the second molten iron to manufacture second molten steel.

2. In claim 1, The above-mentioned mixing process is performed stepwise in multiple rounds, and the mixture produced in the previous round is used in the mixing of the subsequent round. The above first molten steel is mixed only in the first round, The above first method of manufacturing steel is combined in all rounds.

3. In claim 1, The above process of combining is, A process for producing a mixture by mixing the first molten iron and the first molten steel in a first ratio ranging from 20:80 to 80:20; and A steel manufacturing method comprising: a process of manufacturing a second molten steel by mixing the first molten steel and the mixture in a second ratio ranging from 7:93 to 93:

7.

4. Process of preparing the first charter; A process for preparing first molten steel having a lower carbon (C) content than the first molten steel; A process for producing a mixture by combining the first molten iron and the first molten steel; A process of manufacturing a second molten iron by combining the first molten iron and the molten iron; The process of loading the second line into the refining vessel; and A steel manufacturing method comprising a process of refining the second molten iron to manufacture second molten steel.

5. In any one of claims 1 to 4, The above first molten iron includes blast furnace molten iron manufactured in a blast furnace, The above first molten steel is a steel manufacturing method including electric furnace molten steel manufactured in an electric furnace.

6. In claim 5, The process of preparing the above first charter is as follows: A method for manufacturing steel, comprising: a process for manufacturing the first molten iron in a blast furnace so that the carbon (C) content is 4.0 to 4.5 wt%; 7. In claim 6, A steel manufacturing method in which the temperature of the first molten steel is adjusted to 1,350 to 1,500°C while manufacturing the first molten steel.

8. In claim 5, The process of preparing the above first molten steel is as follows: A process for manufacturing the first molten steel in an electric furnace so that the carbon (C) content is 0.04 to 1.0 wt% and the oxygen (O) concentration is 5 to 400 ppm; and A steel manufacturing method comprising a process of adjusting the concentration of oxygen (O) to 0 to 10 ppm by adding a deoxidizer to the first molten steel.

9. In claim 8, A steel manufacturing method in which the temperature of the first molten steel is adjusted to 1,580 to 1,700°C during the manufacturing of the first molten steel.

10. In claim 3 or claim 4, The process of making the above mixture is as follows: A process of accommodating the first vessel in a plurality of first transport containers having openable openings at the top; A process of receiving the first molten steel in a second transport container with an open top; A process of placing the second transport container on top of a number of the first transport containers; A process of tilting the second transport container and feeding the first molten steel from the second transport container into the first transport container of the number; and A method for manufacturing steel, comprising: a process of forming the mixture inside the first transport container of the above number; 11. In claim 3 or claim 4, The process of making the above mixture is as follows: A process of accommodating the first vessel in a plurality of first transport containers having openable openings at the top; A process of receiving the first molten steel in a second transport container having a plurality of openable openings at the bottom; A process of placing the second transport container on top of a number of the first transport containers; A process of opening the lower opening of the second transport container and injecting the first molten steel from the second transport container into the first transport container of the number of said first transport containers; and A method for manufacturing steel, comprising: a process of forming the mixture inside the first transport container of the above number; 12. In claim 3 or claim 4, A steel manufacturing method in which the temperature of the mixture is adjusted to 1,430 to 1,650°C during the process of manufacturing the mixture.

13. In claim 3 or claim 4, The process of manufacturing the above second line is as follows: The process of preparing a loading container with an open top; A process of placing the first transport container containing the mixture among a plurality of first transport containers having an openable opening at the top, on the upper side of the loading container; A process of placing the first transport container containing the first vessel among a plurality of first transport containers on the upper side of the loading container; A process of tilting the first transport container containing the first vessel and the first transport container containing the mixture to inject the mixture and the remainder of the first vessel into the loading container; and A steel manufacturing method comprising a process of forming the second molten metal inside the charging container.

14. In claim 3 or claim 4, The process of manufacturing the above second line is as follows: A process for adjusting the carbon (C) content of the second lead wire to 2 wt% or more and less than 4 wt%; A steel manufacturing method comprising a process of adjusting the temperature of the second molten steel to 1,350 to 1,500°C.

15. In claim 5, The process of loading the above second line into the refining vessel is as follows: A steel manufacturing method comprising: a process of charging the second molten iron into the refining vessel so that the hot metal ratio (HMR) of the second molten iron is 35 to 100%; 16. In claim 15, The process of manufacturing the above second molten steel is as follows: The process of injecting low-odor gas into the above-mentioned refining vessel; and A method for manufacturing steel, comprising: a process for adjusting the components of the second molten steel so that the nitrogen (N) content is in the range of 22 to 30 ppm, the copper (Cu) content is in the range of 0.02 to 0.04 wt%, and the nickel (Ni) content is in the range of 0.01 to 0.04 wt%.

17. In claim 15, The above second molten steel is a steel manufacturing method including Hyper NO steel, HNO steel, MNO steel, LNO steel, EDDQ steel, S-EDDQ steel, DQ steel, DDQ steel, API steel, AHSS steel and general steel.

18. In claim 5, A steel manufacturing method in which the standard carbon dioxide emission amount is 1, and the carbon dioxide emission amount is reduced to 0.25 in the process of preparing the first molten steel, the process of preparing the first molten steel, and the process of manufacturing the second molten steel.

19. A process for preparing steel manufactured by the steel manufacturing method described in any one of claims 1 to 4; and A casting method comprising the process of casting prepared steel.

Citation Information

Patent Citations

  • Raw steel production based on a pre-melt

    EP3822371A1

  • Method for producing molten steel

    JP2009102697A

  • Steel-making method using iron scrap

    JP2011111625A

  • Method for manufacturing iron-based powder

    KR101376140B1

  • A deposition mask of metal material for OLED pixel deposition and OLED display panel fabrication method

    KR1020210092448A