Electrochemical deintercalation and intercalation-based lithium enrichment apparatus, and lithium extraction method thereof

By setting up a hetero ion adsorption layer between the cathode chamber and the anion exchange membrane during the lithium extraction process of the salt lake, the diffusion of impurities is prevented by the principle of liquid gravity layering, the problem of impurities ion diffusion in the prior art is solved, and the anode chamber is improved Purity and productivity.

WO2024234303A1PCT designated stage expired Publication Date: 2024-11-21GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/094544
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-16
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In the existing method of lithium extraction in salt lakes, sodium ions, magnesium ions and other impurity ions in the cathode chamber diffuse to the anode chamber through osmotic action, increasing the content of impurity ions in the anode chamber, resulting in the need to increase the subsequent removal steps and increasing the production cost. .

Method used

A heteroion adsorption layer is provided between the cathode brine and the anion exchange membrane. The principle of liquid gravity layering is used to prevent impurity cations from penetrating the anion exchange membrane, improve the purity of the anode chamber and reduce the removal steps.

Benefits of technology

Effectively avoid impurity cations diffuse into the anode chamber, improve the purity of the anode chamber, reduce the difficulty and production cost of subsequent impurity removal steps, the Li+ concentration in the anode chamber reaches 0.253mol/L, and the concentration of Na+, Mg2+, and K+ is reduced to 0.508mol/L or less.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023094544_21112024_PF_FP_ABST
    Figure CN2023094544_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides an electrochemical deintercalation and intercalation-based lithium enrichment apparatus, and a lithium extraction method thereof. The apparatus comprises a power supply, a cathode chamber, an anode chamber, and an anion exchange membrane arranged between the cathode chamber and the anode chamber, wherein an impurity ion adsorption layer is arranged on the surface of the side of the anion exchange membrane close to the cathode chamber; a lithium-deficient lithium ion sieve electrode is arranged in the cathode chamber; a lithium-rich lithium ion sieve electrode is arranged in the anode chamber; the lithium-deficient lithium ion sieve cathode is connected to a negative electrode of the power supply; the lithium-rich lithium ion sieve electrode is connected to a positive electrode of the power supply. The apparatus of the present disclosure can avoid penetration of impurity cations through the anion exchange membrane due to osmosis in an electrochemical lithium extraction process, thereby reducing impurity removal steps and lowering the cost of a subsequent production process.
Need to check novelty before this filing date? Find Prior Art

Description

A device for electrochemical deintercalation and enrichment of lithium and a method for extracting lithium Technical Field

[0001] The present disclosure belongs to the technical field of lithium extraction from salt lakes, for example, a device for electrochemical deintercalation and enrichment of lithium and a method for extracting lithium therefrom. Background Art

[0002] With the rapid development of new energy vehicles in recent years, the demand for lithium-ion batteries has surged, and with it, the demand for lithium resources. Salt lake brine, lithium ore, and spent lithium-ion batteries are the primary sources of lithium in lithium-ion battery production. Salt lake brine, among other things, contains approximately 70% of global lithium resources and is a crucial raw material for lithium resource development. The main processes for extracting lithium from salt lakes include solarization, adsorption, solvent extraction, electrodialysis, and electrochemical deintercalation. The electrochemical deintercalation method, which utilizes electrochemical reactions to adsorb and desorb lithium ions from solid materials, can reduce the use of chemicals and has been extensively studied for its environmental friendliness, strong lithium ion selectivity, and good adaptability to brine.

[0003] CN115818801A discloses a method for extracting lithium from salt lake brine. The lithium extraction process is divided into two steps: lithium insertion and lithium removal. During lithium insertion, lead is used as the anode, a conductive substrate coated with an ion screen is used as the cathode, and an anion exchange membrane separates the anode and cathode. A sulfate solution is added to the anode, and salt lake brine is added to the cathode. During lithium removal, the electrode polarity of the cathode and cathode in the lithium extraction process is reversed. At the same time, the solution on the lead electrode side of the previous cycle remains unchanged. The brine is replaced with a fresh sulfate solution as the supporting electrolyte, and power is applied again to release the lithium sulfate.

[0004] CN115612838A discloses a device for selective lithium extraction from salt lakes and its application. The device comprises: a power supply, an anion exchange membrane, a current collector grid, a water inlet, a water outlet and an adsorbent. The current collector grid is divided into a first current collector grid and a second current collector grid. The first current collector grid and the second current collector grid are respectively arranged in a first electrolysis chamber and a second electrolysis chamber. The first current collector grid and the second current collector grid are a three-dimensional structure with several layers of mesh arranged in parallel. The first current collector grid or the second current collector grid is electrically connected to the positive electrode or the negative electrode of the power supply.

[0005] In the above-mentioned method of extracting lithium from salt lakes, an anion exchange membrane is added between the cathode and the anode to intercept sodium and magnesium ions. However, in actual use, osmosis will cause some sodium ions, magnesium ions and other impurity ions in the cathode chamber to diffuse into the anode chamber, increasing the content of impurity ions in the anode chamber. Subsequently, an impurity removal step needs to be added, which lengthens the production process and increases costs.

[0006] Summary of the Invention

[0007] The following is a summary of the subject matter described in detail herein. This summary is not intended to limit the scope of the claims.

[0008] The purpose of the present disclosure is to provide a device for electrochemical deintercalation and enrichment of lithium and a method for lithium extraction thereof. The present disclosure utilizes the principle of liquid gravity stratification to set a miscellaneous ion adsorption layer between the cathode brine and the anion exchange membrane, thereby preventing impurity cations from penetrating the anion exchange membrane due to osmosis during the electrochemical lithium extraction process, and preventing some sodium ions, magnesium ions and other impurity ions in the cathode chamber from diffusing into the anode chamber, thereby reducing the impurity removal steps and lowering the cost of subsequent production processes.

[0009] To achieve this disclosure purpose, the present disclosure adopts the following technical solutions:

[0010] In the first aspect, an embodiment of the present disclosure provides a device for electrochemical deintercalation and enrichment of lithium, the device comprising a power supply, a cathode chamber, an anode chamber, and an anion exchange membrane arranged between the cathode chamber and the anode chamber, a miscellaneous ion adsorption layer being arranged on the surface of the anion exchange membrane close to the cathode chamber, a lithium-poor lithium ion sieve electrode being arranged in the cathode chamber, a lithium-rich lithium ion sieve electrode being arranged in the anode chamber, the lithium-poor lithium ion sieve cathode electrode being connected to the negative electrode of the power supply, and the lithium-rich lithium ion sieve electrode being connected to the positive electrode of the power supply.

[0011] In the embodiment of the present disclosure, a mixed ion adsorption layer is added to the cathode chamber side near the anion exchange membrane. Since the density of the mixed ion adsorption layer is quite different from that of the salt lake brine, according to the liquid gravity stratification principle, the liquid layer can be ensured to be located on the surface of the anion exchange membrane close to the salt lake brine side in the cathode chamber. This allows the cations that are about to pass through the anion exchange membrane due to osmosis to be complexed by the complexing agent in the mixed ion adsorption layer, thereby preventing impurity cations from penetrating the anion exchange membrane due to osmosis during the electrochemical lithium extraction process, improving the purity of the cations in the anode chamber, and reducing the difficulty of subsequent impurity removal steps.

[0012] In one embodiment, the lithium-poor lithium ion sieve electrode and the lithium-rich lithium ion sieve electrode are arranged in parallel laterally.

[0013] In one embodiment, the thickness of the mixed ion adsorption layer is 1 / 50 to 1 / 100 of the thickness of the brine in the cathode chamber, for example, 1 / 50, 1 / 60, 1 / 70, 1 / 80, 1 / 90 or 1 / 100.

[0014] In one embodiment, the density of the mixed ion adsorption layer is less than the density of the brine, the anode chamber is located at the top, and the cathode chamber is located at the bottom.

[0015] In one embodiment, the hetero ion adsorption layer includes an ethylenediamine solution and / or an ethylenediamine salt solution.

[0016] In one embodiment, the ethylenediamine salt solution includes any one of an ethylenediaminetetraacetic acid aqueous solution, an ethylenediaminetetraacetic acid disodium salt aqueous solution, or an ethylenediaminetetraacetic acid tetrasodium salt aqueous solution, or a combination of at least two thereof.

[0017] In one embodiment, the concentration of ethylenediamine and / or ethylenediamine salt in the heteroaryl ion adsorption layer is 0.1 to 10 mmol / L, for example, 0.1 mmol / L, 0.5 mmol / L, 1 mmol / L, 2 mmol / L, 5 mmol / L or 10 mmol / L.

[0018] In one embodiment, the density of the mixed ion adsorption layer is greater than the density of the brine, the anode chamber is located at the bottom, and the cathode chamber is located at the top.

[0019] In one embodiment, the hetero ion adsorption layer includes ethylenediamine solution and / or ethylenediamine salt solution and sodium salt and / or potassium salt.

[0020] In one embodiment, the sodium salt comprises sodium chloride and / or sodium sulfate.

[0021] In one embodiment, the potassium salt comprises potassium chloride and / or potassium sulfate.

[0022] In one embodiment, the concentration of ethylenediamine and / or ethylenediamine salt in the heteroaryl ion adsorption layer is 0.1 to 10 mmol / L, for example, 0.1 mmol / L, 0.5 mmol / L, 1 mmol / L, 2 mmol / L, 5 mmol / L or 10 mmol / L.

[0023] In one embodiment, the concentration of sodium salt and / or potassium salt in the heteroionic adsorption layer is 2-10 mol / L, for example, 2 mol / L, 4 mol / L, 6 mol / L, 8 mol / L or 10 mol / L.

[0024] In a second aspect, an embodiment of the present disclosure provides a method for extracting lithium from the device according to the first aspect, the method comprising the following steps:

[0025] (1) The positions of the cathode chamber, the anode chamber and the anion exchange membrane are set according to the concentration of the salt lake brine, a lithium-poor lithium ion sieve electrode is installed in the cathode chamber, a lithium-rich lithium ion sieve electrode is installed in the anode chamber, and an anion exchange membrane is installed between the cathode chamber and the anode chamber to obtain a lithium extraction tank in which the cathode and the anode are arranged in parallel transversely;

[0026] (2) Inject brine from the salt lake into the cathode chamber of the vertical lithium extraction tank, slowly inject the impurity ion adsorption layer into the side of the anion exchange membrane close to the cathode chamber, inject salt solution into the anode chamber, and apply voltage to the anode and cathode to extract lithium at a constant pressure.

[0027] In one embodiment, the lithium-rich lithium ion sieve electrode in step (1) is prepared by the following method:

[0028] The lithium ion sieve, a conductive agent, a pore-forming agent, PVDF and N-methylpyrrolidone are uniformly mixed in a mass ratio of 100:(10-15):(10-30):(5-15):(150-250), the mixed slurry is coated on a current collector, and dried at 50-80° C. for 3-10 hours to obtain the lithium-rich lithium ion sieve electrode.

[0029] In one embodiment, the lithium ion sieve includes any one of lithium manganese phosphate, lithium titanate, lithium manganate, lithium iron phosphate or lithium manganese iron phosphate, or a combination of at least two thereof.

[0030] In one embodiment, the pore former includes ammonium bicarbonate and / or ammonium carbonate.

[0031] In one embodiment, the conductive agent includes any one of conductive carbon black, conductive acetylene black, graphene, or carbon nanotubes, or a combination of at least two thereof.

[0032] In one embodiment, the current collector includes any one of titanium mesh, graphite plate, carbon cloth, carbon paper or aluminum foil, or a combination of at least two of them.

[0033] In one embodiment, the lithium-deficient lithium ion sieve anode is prepared by the following method:

[0034] A lithium-rich lithium ion sieve electrode is used as the positive electrode and an AgCl electrode is used as the negative electrode. The electrodes are placed in a salt solution and delithiation is performed at a constant voltage of 0.3 to 1.2 V. The reaction stops when the current drops to 0.2 mA, and a lithium-poor lithium ion sieve electrode is obtained.

[0035] In one embodiment, the density of the salt lake brine in step (2) is 1.1-1.8 g / cm 3 , for example: 1.1g / cm 3 , 1.2g / cm 3 , 1.4g / cm 3 , 1.6g / cm 3 or 1.8g / cm 3 wait.

[0036] In one embodiment, the salt solution in step (2) includes a sulfate solution and / or a chloride salt solution.

[0037] In one embodiment, the concentration of metal ions in the salt solution is 0.05 to 2 mol / L, for example, 0.05 mol / L, 0.1 mol / L, 0.5 mol / L, 1 mol / L or 2 mol / L.

[0038] In one embodiment, the voltage in step (2) is 0.3-1.2V, for example, 0.3V, 0.5V, 0.8V, 1V or 1.2V.

[0039] In one embodiment, during the constant-voltage lithium extraction process in step (2), when the current is as low as 0.2 mA, the power is stopped and the anode and cathode are switched and then the power is continued, and this is repeated 2 to 5 times to obtain a lithium-rich solution.

[0040] The present disclosure has the following beneficial effects:

[0041] (1) The present invention utilizes the liquid gravity stratification principle to set a miscellaneous ion adsorption layer between the cathode brine and the anion exchange membrane, thereby preventing impurity cations from penetrating the anion exchange membrane due to osmosis during the electrochemical lithium extraction process, and preventing some sodium ions, magnesium ions and other impurity ions in the cathode chamber from diffusing into the anode chamber, thereby reducing the impurity removal steps and lowering the cost of subsequent production processes.

[0042] (2) The electrochemical deintercalation and enrichment method of lithium disclosed in the present invention, after lithium extraction, the Li + The concentration can reach above 0.253 mol / L, Na + The concentration can reach below 0.508mol / L (basically unchanged before and after), Mg 2+ The concentration can reach below 0.001mol / L, K + The concentration can reach below 0.012 mol / L, which improves the purity of the cations in the anode chamber and reduces the difficulty of subsequent impurity removal steps.

[0043] Still other aspects will become apparent upon reading and understanding the accompanying drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] The accompanying drawings are used to provide a further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of this application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.

[0045] Figure 1 is a schematic diagram of the device for the electrochemical deintercalation and lithium enrichment method described in Example 1 of the present disclosure, 1-lithium-rich lithium ion sieve, 2-lithium-poor lithium ion sieve, 3-anion exchange membrane, 4-miscellaneous ion adsorption layer.

[0046] Figure 2 is a schematic diagram of the device for the electrochemical deintercalation and lithium enrichment method described in Example 2 of the present disclosure, 1-lithium-rich lithium ion sieve, 2-lithium-poor lithium ion sieve, 3-anion exchange membrane, 4-miscellaneous ion adsorption layer.

[0047] Figure 3 is a schematic diagram of the device for the electrochemical deintercalation and lithium enrichment method described in Comparative Example 1, 1-lithium-rich lithium ion sieve, 2-lithium-poor lithium ion sieve, 3-anion exchange membrane. DETAILED DESCRIPTION

[0048] The technical solution of the present disclosure is further described below through specific implementation methods. Those skilled in the art should understand that the embodiments are only used to help understand the present disclosure and should not be regarded as specific limitations of the present disclosure.

[0049] The lithium-rich lithium ion sieve electrode described in the embodiments and comparative examples of the present disclosure is prepared by the following method: lithium iron phosphate lithium ion sieve and conductive carbon black, ammonium bicarbonate, PVDF and N-methylpyrrolidone are mixed uniformly in a mass ratio of 100:12:20:10:200, the mixed slurry is coated on a current collector, and dried at 60°C for 5 hours to obtain the lithium-rich lithium ion sieve electrode; the lithium-rich lithium ion sieve anode is prepared by the following method: taking the above-mentioned lithium-rich lithium ion sieve electrode as the positive electrode and the AgCl electrode as the negative electrode, placing them in a salt solution, delithiation at a constant voltage of 0.8V, and stopping the reaction when the current is as low as 0.2mA to obtain a lithium-poor lithium ion sieve electrode.

[0050] Example 1

[0051] This embodiment provides a method for electrochemical deintercalation and enrichment of lithium. A schematic diagram of a device for the electrochemical deintercalation and enrichment of lithium is shown in FIG1 . The method comprises the following steps:

[0052] (1) The density of the miscellaneous ion adsorption layer is less than the density of the brine. The lithium-poor lithium ion sieve is used as the cathode, the lithium-rich lithium ion sieve is used as the anode, and the anode and cathode chambers are separated by an anion exchange membrane. The anode chamber is located at the top and the cathode chamber is located at the bottom. The miscellaneous ion adsorption layer is located below the anion exchange membrane and at the top of the brine in the cathode chamber.

[0053] (2) Salt lake brine was injected into the cathode chamber of the vertical lithium extraction tank. The thickness of the impurity ion adsorption layer was 1 / 90 of the brine in the cathode chamber. Finally, a 0.5 mol / L sodium chloride solution was injected into the anode chamber above the anion exchange membrane. The impurity ion adsorption layer was an ethylenediamine aqueous solution with a concentration of 0.5 mmol / L and a brine density of 1.5 g / cm 3 Apply a 0.8V voltage to the anode and cathode for constant voltage lithium extraction. When the current drops to 0.2mA, stop the reaction and switch the anode and cathode. The lithium-intercalated lithium ion sieve is disengaged and the lithium-poor lithium ion sieve is restored. Lithium ions are enriched in the anode chamber. Repeat the above steps three times to obtain a lithium-rich solution.

[0054] Example 2

[0055] This embodiment provides a method for electrochemical deintercalation and enrichment of lithium. A schematic diagram of a device for the electrochemical deintercalation and enrichment of lithium is shown in FIG2 . The method comprises the following steps:

[0056] (1) The density of the miscellaneous ion adsorption layer is greater than the density of the brine. The lithium-poor lithium ion sieve is used as the cathode, the lithium-rich lithium ion sieve is used as the anode, and the anode and cathode chambers are separated by an anion exchange membrane. The anode chamber is located at the bottom and the cathode chamber is located at the top. The miscellaneous ion adsorption layer is located above the anion exchange membrane and the brine is at the bottom of the cathode chamber.

[0057] (2) Salt lake brine is injected into the cathode chamber of the vertical lithium extraction tank. The thickness of the mixed ion adsorption layer is 1 / 80 of the brine in the cathode chamber. Finally, a 0.5 mol / L sodium chloride solution is injected into the anode chamber above the anion exchange membrane. The mixed ion adsorption layer is a mixed aqueous solution of disodium ethylenediaminetetraacetic acid and sodium chloride. The concentration of disodium ethylenediaminetetraacetic acid is 3 mmol / L, the concentration of sodium chloride is 6 mol / L, and the density of the brine is 1.5 g / cm 3 Apply a 0.9V voltage to the anode and cathode for constant voltage lithium extraction. When the current drops to 0.2mA, stop the reaction and switch the anode and cathode. The lithium-intercalated lithium ion sieve is disengaged and the lithium-poor lithium ion sieve is restored. Lithium ions are enriched in the anode chamber. Repeat the above steps three times to obtain a lithium-rich solution.

[0058] Example 3

[0059] The only difference between this embodiment and embodiment 1 is that the thickness of the impurity ion adsorption layer is 1 / 30 of the brine in the cathode chamber, and other conditions and parameters are exactly the same as those in embodiment 1.

[0060] Example 4

[0061] The only difference between this embodiment and embodiment 1 is that the thickness of the impurity ion adsorption layer is 1 / 120 of the brine in the cathode chamber, and the other conditions and parameters are exactly the same as those in embodiment 1.

[0062] Comparative Example 1

[0063] The only difference between this comparative example and Example 1 is that the lithium extraction tank is placed horizontally, and the lithium-poor lithium ion sieve electrode and the lithium-rich lithium ion sieve electrode are arranged longitudinally and parallelly. The schematic diagram of the device is shown in Figure 3.

[0064] Comparative Example 2

[0065] The only difference between this comparative example and Example 1 is that no mixed ion adsorption layer is added, and other conditions and parameters are exactly the same as those in Example 1.

[0066] Performance testing:

[0067] The concentrations of various main elements in the anode chamber solution of the electrochemical deintercalation and lithium enrichment device described in the Examples and Comparative Examples before and after lithium extraction are shown in Table 1:

[0068] Table 1

[0069] As can be seen from Table 1, according to Examples 1-2, the electrochemical deintercalation and enrichment method of lithium disclosed in the present invention has a Li + The concentration can reach above 0.253 mol / L, Na + The concentration can reach below 0.508mol / L (basically unchanged before and after), Mg 2+ The concentration can reach below 0.001mol / L, K + The concentration can reach below 0.012 mol / L, which prevents impurity cations from penetrating the anion exchange membrane due to osmosis during the electrochemical lithium extraction process, improves the purity of the cations in the anode chamber, and reduces the difficulty of subsequent impurity removal steps.

[0070] By comparing Example 1 with Examples 3-4, it can be seen that the thickness of the heteroionic adsorption layer disclosed in the present invention will significantly affect the effect of lithium enrichment. When the thickness of the heteroionic adsorption layer is controlled to be 1 / 50 to 1 / 100 of the thickness of the brine in the cathode chamber, the effect of lithium enrichment is better. If the thickness of the heteroionic adsorption layer is too small, the purity of the cations in the cation chamber will be reduced.

[0071] By comparing Example 1 and Comparative Example 1, it can be seen that when a conventional electrolytic cell is used to add a miscellaneous ion adsorption layer, the miscellaneous ion adsorption layer cannot be located on the cathode side of the anion exchange membrane through the liquid gravity stratification principle, and therefore cannot filter out the impurity ions that penetrate the anion exchange membrane due to osmosis.

[0072] By comparing Example 1 and Comparative Example 2, it can be seen that the present invention adds an impurity ion adsorption layer near the anion exchange membrane on the cathode chamber side, thereby preventing impurity cations from penetrating the anion exchange membrane due to osmosis during the electrochemical lithium extraction process, improving the purity of the cations in the anode chamber, and reducing the difficulty of the subsequent impurity removal step.

Claims

1. A device for electrochemical deintercalation and enrichment of lithium, the device comprising a power supply, a cathode chamber, an anode chamber and an anion exchange membrane arranged between the cathode chamber and the anode chamber, wherein a mixed ion adsorption layer is arranged on the surface of the anion exchange membrane close to the cathode chamber, a lithium-poor lithium ion sieve electrode is arranged in the cathode chamber, a lithium-rich lithium ion sieve electrode is arranged in the anode chamber, the lithium-poor lithium ion sieve cathode electrode is connected to the negative electrode of the power supply, and the lithium-rich lithium ion sieve electrode is connected to the positive electrode of the power supply.

2. The device according to claim 1, wherein: The lithium-poor lithium ion sieve electrode and the lithium-rich lithium ion sieve electrode are arranged in parallel transversely; Optionally, the thickness of the impurity ion adsorption layer is 1 / 50 to 1 / 100 of the thickness of the brine in the cathode chamber.

3. The device according to claim 1 or 2, wherein: The density of the impurity ion adsorption layer is less than the density of the brine, the anode chamber is located at the top, and the cathode chamber is located at the bottom.

4. The device according to any one of claims 1 to 3, wherein: The hetero ion adsorption layer comprises ethylenediamine solution and / or ethylenediamine salt solution.

5. The device according to claim 4, wherein: The ethylenediamine salt solution includes any one of an ethylenediaminetetraacetic acid aqueous solution, an ethylenediaminetetraacetic acid disodium salt aqueous solution, or an ethylenediaminetetraacetic acid tetrasodium salt aqueous solution, or a combination of at least two thereof; Optionally, the concentration of ethylenediamine and / or ethylenediamine salt in the hetero-ion adsorption layer is 0.1-10 mmol / L.

6. The device according to any one of claims 1 to 5, wherein: The density of the impurity ion adsorption layer is greater than the density of the brine, the anode chamber is located at the bottom, and the cathode chamber is located at the top; Optionally, the hetero-ion adsorption layer comprises ethylenediamine solution and / or ethylenediamine salt solution and sodium salt and / or potassium salt; Optionally, the sodium salt comprises sodium chloride and / or sodium sulfate; Optionally, the potassium salt comprises potassium chloride and / or potassium sulfate.

7. The device according to claim 6, wherein: The concentration of ethylenediamine and / or ethylenediamine salt in the hetero-ion adsorption layer is 0.1 to 10 mmol / L; Optionally, the concentration of the sodium salt and / or potassium salt in the hetero-ion adsorption layer is 2 to 10 mol / L.

8. A method for extracting lithium according to any one of claims 1 to 7, the method comprising the following steps: (1) according to the concentration of salt lake brine, the positions of the cathode chamber, the anode chamber and the anion exchange membrane are set, a lithium-poor lithium ion sieve electrode is installed in the cathode chamber, a lithium-rich lithium ion sieve electrode is installed in the anode chamber, and an anion exchange membrane is installed between the cathode chamber and the anode chamber to obtain a lithium extraction tank in which the cathode and the anode are arranged in parallel transversely; (2) Inject salt lake brine into the cathode chamber of the vertical lithium extraction cell, slowly inject the impurity ion adsorption layer into the side of the anion exchange membrane close to the cathode chamber, inject salt solution into the anode chamber, and apply voltage to the anode and cathode to extract lithium at a constant pressure.

9. The method of claim 8, wherein: The lithium-rich lithium ion sieve electrode in step (1) is prepared by the following method: The lithium ion sieve, conductive agent, pore-forming agent, PVDF and N-methylpyrrolidone are uniformly mixed in a mass ratio of 100:(10-15):(10-30):(5-15):(150-250), the mixed slurry is coated on the current collector, and dried at 50-80° C. for 3-10 hours to obtain the lithium-rich lithium ion sieve electrode.

10. The method of claim 9, wherein: The lithium ion sieve comprises any one of lithium manganese phosphate, lithium titanate, lithium manganate, lithium iron phosphate or lithium manganese iron phosphate, or a combination of at least two thereof; Optionally, the pore former comprises ammonium bicarbonate and / or ammonium carbonate; Optionally, the conductive agent includes any one of conductive carbon black, conductive acetylene black, graphene or carbon nanotubes, or a combination of at least two thereof; Optionally, the current collector includes any one of titanium mesh, graphite plate, carbon cloth, carbon paper or aluminum foil, or a combination of at least two of them.

11. The method according to any one of claims 8 to 10, wherein: The lithium-deficient lithium ion sieve electrode is prepared by the following method: Take a lithium-rich lithium ion sieve electrode as the positive electrode and an AgCl electrode as the negative electrode, place them in a salt solution, and delithiate at a constant voltage of 0.3 to 1.2 V. When the current is as low as 0.2 mA, the reaction stops, and a lithium-poor lithium ion sieve electrode is obtained.

12. The method according to any one of claims 8 to 11, wherein: The density of the salt lake brine in step (2) is 1.1-1.8 g / cm 3 .

13. The method according to any one of claims 8 to 12, wherein: The salt solution in step (2) includes a sulfate solution and / or a chloride salt solution; Optionally, the concentration of metal ions in the salt solution is 0.05-2 mol / L.

14. The method according to any one of claims 8 to 13, wherein: The voltage in step (2) is 0.3 to 1.2V.

15. The method according to any one of claims 8 to 14, wherein: During the constant-pressure lithium extraction process in step (2), when the current drops to 0.2 mA, the power is stopped and the anode and cathode are switched and then the power is continued. This is repeated 2 to 5 times to obtain a lithium-rich solution.

Citation Information

Patent Citations

  • Method and device for separating magnesium and lithium and enriching lithium from salt lake brine

    CN102382984A

  • Method for extracting lithium from lithium-contained solution based on LiMn2O4 electrode material

    CN107201452A

  • Device and method for separating magnesium / lithium and enriching lithium in salt lake brine

    CN109267086A

  • Device and method for using membrane electrochemical in-situ leaching of serpentine while Mg < 2 + > for capturing and storing CO2

    CN109355497A

  • Electrode structure capable of extracting lithium and manufacturing method and application of electrode structure

    CN109609977A