Method for recovering negative electrode graphite of waste lithium-ion battery
By mixing the negative graphite of waste lithium-ion battery with composite starch binder and asphalt, and processing it in a vertical continuous graphitization furnace, the problems of waste of graphite resources and environmental pollution in lithium-ion battery recycling are solved. , realizes high-efficiency and low-energy-consuming finished graphite product preparation.
Patent Information
- Application Number
- PCT/CN2023/094562
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2024-11-21
AI Technical Summary
In the existing lithium-ion battery recycling technology, negative electrode graphite materials are reused less, and conventional high-temperature graphitization processes consume high energy and are not conducive to continuous production, resulting in waste of graphite resources and environmental pollution.
The negative electrode graphite of waste lithium-ion battery is mixed with composite starch binder and asphalt. After wet mixing and drying, it is processed in a vertical continuous graphitization furnace. Gravity and arc heat exothermic technology are used to realize graphite. Removal of finished products and structural repairs to reduce energy consumption.
The preparation of high-purity and high crystallinity graphite is realized, which reduces the electrical power of the graphitization furnace, reduces the consumption of graphite crucibles, improves the strength and resource utilization of the finished graphite products, saves energy consumption, and is safer.
Smart Images

Figure CN2023094562_21112024_PF_FP_ABST
Abstract
Description
Method for recycling negative electrode graphite of waste lithium-ion batteries Technical Field
[0001] The present invention relates to the technical field of lithium-ion battery recycling, and in particular to a method for recycling negative electrode graphite of waste lithium-ion batteries. Background Art
[0002] With the rise of new energy electric vehicles, the consumption of lithium-ion batteries, which serve as their power source, has also increased significantly. The service life of lithium-ion batteries is generally 3 to 5 years, depending on the materials and usage conditions. The large number of scrapped lithium-ion batteries will not only cause resource shortages but also seriously pollute the environment. At present, the focus of lithium battery recycling is still on the reuse of precious metals (nickel, cobalt, manganese, etc.) in the positive electrode materials, and less attention is paid to the graphite materials commonly used in the negative electrode. Waste graphite has always been treated as hazardous waste because it contains various metal impurities and organic matter, resulting in a large amount of graphite waste. In addition, the current graphite resources on the market cannot meet the demand for lithium battery production, so the recycling of graphite from waste lithium batteries is particularly important.
[0003] In the field of recycling and regenerating negative electrode graphite from waste lithium-ion batteries, conventional high-temperature graphitization furnaces are generally used to graphitize the negative electrode graphite. The high temperature of the graphitization furnace is used to cause impurities in the negative electrode graphite to reach their melting and boiling points and escape, thereby achieving the purpose of removing impurities from the waste graphite. In addition, during the high-temperature graphitization process, the carbon atoms in the waste graphite undergo directional rearrangement during the graphitization process, repairing the graphite structure. However, the graphitization furnaces used in conventional graphitization processes are all Acheson furnaces or internal series furnaces. Regardless of whether they are Acheson furnaces or internal series furnaces, graphite powder must be loaded into a graphite crucible for graphitization, which consumes too many graphite crucibles and is not conducive to continuous production. In addition, graphitization consumes a lot of energy. The high consumption of graphite crucibles and the high energy cost of graphitization have both limited the application of high-temperature graphitization purification processes.
[0004] Summary of the Invention
[0005] The present disclosure aims to at least solve the technical problems existing in the above-mentioned prior art. To this end, the present disclosure proposes a method for recycling negative electrode graphite of waste lithium-ion batteries.
[0006] According to one aspect of the present disclosure, a method for recycling negative electrode graphite of waste lithium-ion batteries is proposed, comprising the following steps:
[0007] S1: mixing waste lithium-ion battery negative electrode graphite, composite starch binder and asphalt, adding water to the mixed powder for wet mixing to obtain a coated wet material;
[0008] S2: forming the coated wet material into a shaped part with a transverse dimension of 15-50 mm, drying it and then carbonizing it to obtain a graphite molded part;
[0009] S3: placing the graphite molded part into a vertical continuous graphitization furnace, and sequentially processing it through a low-temperature section and a high-temperature section of the vertical continuous graphitization furnace to obtain graphitized graphite, and crushing the graphitized graphite to obtain a finished graphite product; the temperature of the low-temperature section is 800-1700°C, and the temperature of the high-temperature section is 2400-2700°C.
[0010] The graphite molded parts are put into the vertical continuous graphitization furnace, and the materials move downward by gravity. The furnace temperature is distributed from top to bottom as a low-temperature section, a high-temperature section and a cooling section. When passing through the low-temperature section in the early stage, the graphite molded parts can remain as they are without breakage due to the network structure formed by the binder. When passing through the high-temperature section, the asphalt therein is carbonized to form a new aromatic ring structure, which is connected with the six-membered ring in the graphite to re-form a network structure at high temperature, so that the graphite parts maintain their original shape without being destroyed. The point contact and pores between the molded parts in the high-temperature zone form arc heat release, and the latent resistance of the material itself generates high temperature (the upper and lower ends of the vertical graphitization furnace are respectively There is a graphite electrode, which is the positive electrode and the negative electrode. When the current passes through the positive electrode, the material and the negative electrode, the pressures are different. The different pressure atmospheres produce arc discharge, and the generated heat energy electrically heats the material, reducing the power consumption of the graphitization furnace. The graphite slag is sintered at 2400-2700 ° C. The metal impurities (Ni, Co, Mn, Fe, Cu, etc.) and non-metallic impurities (Si, P, etc.) in the graphite slag are gasified at high temperature and concentratedly removed through the pores between the molded parts with the assistance of negative pressure pumping. The graphite structure defects caused by gas overflow are also repaired due to structural rearrangement caused by high temperature, and finally high-purity and high-crystallinity graphite parts are obtained.
[0011] There are two reasons for making 15-50mm shaped parts: 1. Safety considerations. Since the material is directly put into the vertical graphitization furnace without a container, if the material is powder, there is a risk of furnace explosion due to excessive dust at high temperature. Preparing shaped parts with larger sizes can avoid this risk. 2. Compared with ordinary granulation, the accumulation of larger shaped parts will form larger and more accumulation gap channels, which is conducive to the gasification and escape of impurities during the high-temperature graphitization process, achieving the effect of impurity removal. Although direct granulation is also a shaped part, the particles are still not large enough, and ordinary particles are prone to dust. During the generation process, the dust and flammable volatiles are under pressure, which can easily cause unsafe events such as furnace spraying. If the size of the shaped part is too small, the porosity formed by the accumulation is too small, and the pores are too small, which is not conducive to the gasification and escape of impurities. However, the size of the shaped part cannot be too large. Due to the power size of the molding equipment and the limitations of the molding mold, the size is too large, which is not conducive to the molding of strong shaped parts. The insufficient strength of the shaped part is easy to break during movement.
[0012] In some embodiments of the present disclosure, in step S1, the negative electrode graphite of the waste lithium ion battery is obtained by the following process: the waste lithium ion battery is discharged, crushed, calcined and sieved to obtain battery black powder, the battery black powder is acid-leached and then solid-liquid separated to obtain graphite wet slag, and the graphite wet slag is dried and heat-treated to obtain the negative electrode graphite of the waste lithium ion battery.
[0013] In some embodiments of the present disclosure, in step S1, the heat treatment is either oxygen sintering or oxygen-free sintering; the oxygen sintering temperature is 350-550°C for 2-4 hours, while the oxygen-free sintering temperature is 400-750°C for 2-4 hours. The heat treatment is used to remove the acid and organic binder remaining in the graphite slag.
[0014] In some embodiments of the present disclosure, in step S1, the calcination temperature is 300-600° C., and the calcination time is 3-10 h.
[0015] In some embodiments of the present disclosure, in step S1, the acid leaching uses sulfuric acid with a concentration of 0.5-3 g / L; the temperature of the acid leaching is 60-90° C., and the time of the acid leaching is 20-40 h.
[0016] In some embodiments of the present disclosure, in step S1, the drying temperature is 80-200° C., and the drying time is 10-30 hours.
[0017] In some embodiments of the present disclosure, in step S1, the mass ratio of the negative electrode graphite, the composite starch binder and the asphalt is 1: (0.03-0.06): (0.05-0.08).
[0018] In some embodiments of the present disclosure, in step S1, the negative electrode graphite, composite starch binder and asphalt are mixed for 10-30 minutes.
[0019] In some embodiments of the present disclosure, in step S1, the amount of water added is 20%-50% of the mass of the negative electrode graphite.
[0020] In some embodiments of the present disclosure, in step S1, the wet mixing time is 20-40 minutes.
[0021] In some embodiments of the present disclosure, in step S1, the composite starch binder is a mixture of starch and SiO2; the starch is selected from at least one of corn starch, rice starch, potato starch, sweet potato starch, or wheat starch. The composite starch binder is a low-ash, low-volatile substance. Compared with ordinary starch, the addition of SiO2 powder to the composite starch binder has two functions: 1. SiO2 acts as a thickener and can be highly dispersed in water to form a network structure to promote bonding; 2. SiO2 can act as a catalyst for graphitization, promoting the occurrence of graphitization, so that the graphitization reaction can occur at a lower temperature.
[0022] In some embodiments of the present disclosure, in step S1, the mass ratio of starch to SiO2 in the composite starch binder is (3-10): 1. Alternatively, the mass ratio of starch to SiO2 in the composite starch binder is (3-6): 1.
[0023] In some embodiments of the present disclosure, in step S2, the shaped piece is at least one of a sphere, a rod, a tube, or a cube.
[0024] In some embodiments of the present disclosure, in step S2, the method for preparing the shaped part is to put the coated wet material into a molding machine and press it into a target shape.
[0025] In some embodiments of the present disclosure, in step S2, the drying temperature is 80-180° C., and the drying time is 3-30 hours.
[0026] In some embodiments of the present disclosure, in step S2, the carbonization process is as follows: heating to 200-350°C and maintaining the temperature for 0.5-2h under a protective atmosphere, and then heating to 500-1000°C and maintaining the temperature for 1-4h. Furthermore, the heating rate to 200-350°C is 5-20°C / min, and the heating rate to 500-1000°C is 3-10°C / min. The carbonization treatment decomposes part of the binder to form a network structure, thereby enhancing the strength and activity of the graphite molded parts. The effects of segmented carbonization: 1. Maintaining the temperature at 200-350°C for 0.5-2h allows the volatiles in the graphite to slowly escape through low-temperature cracking, preventing the risk of excessive volatiles in the high-temperature section from causing furnace spraying; 2. The effect of heating to 500-1000°C and maintaining the temperature for 1-4h is to remove the hydrogen atoms and oxygen atoms in the binder to form a carbon network structure.
[0027] In some embodiments of the present disclosure, in step S3, the low temperature treatment time is 1-1.5 hours.
[0028] In some embodiments of the present disclosure, in step S3, the high-temperature treatment time is 2-4 hours. There is a valve at the bottom of the vertical graphitization furnace. When the valve adjustment diameter is large, the material descends quickly; when the valve adjustment diameter is small, the material descends slowly. The residence time in different furnace temperature sections is controlled by the speed of the material discharge.
[0029] According to the embodiments of the present disclosure, there are at least the following beneficial effects:
[0030] 1. The present invention adopts a continuous graphitization technology for molded parts. Compared with the intermittent graphitization of graphite powder on the market, it has lower energy consumption. Conventional intermittent graphitization consumes about 14,000-16,000 kw·h of electricity per ton of material, while the continuous graphitization of the present invention consumes about 4,000-5,000 kw·h of electricity per ton of material. It has a shorter processing time and a higher production capacity. It does not require containers such as graphite crucibles for loading, nor does it require insulation materials and resistor materials.
[0031] 2. The present invention introduces an easily split composite starch binder to produce graphite molded parts with high molding strength and low ash content, and uses asphalt to reform a network structure with graphite under high temperature conditions, thereby ensuring the strength of the graphite molded parts throughout the entire graphitization process, making it difficult for them to break after being squeezed and collided in a vertical graphitization furnace; because the solid particle properties of the graphite molded parts are maintained throughout the entire graphitization process, the safety of the entire graphitization process is guaranteed (powders are prone to furnace explosion in high temperature environments).
[0032] 3. The graphite molded parts disclosed herein will accumulate to form pores in the vertical continuous graphitization furnace, which is conducive to the escape of ash through the "pores" during the graphitization process. Therefore, compared with direct graphitization of graphite powder, the ash removal effect of the disclosed method is better.
[0033] 4. The present invention directly fills the graphite molded parts into the vertical continuous graphitization furnace during the graphitization process. By utilizing the sealing structure and high-temperature oxygen-free characteristics of the furnace itself, high-temperature graphitization can be performed without the need for additional protective gas, further saving energy consumption.
[0034] 5. The present invention removes impurities from waste graphite through high-temperature purification and rearranges the structure, thereby preparing high-performance graphite materials and realizing resource utilization of waste graphite. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The present disclosure is further described below with reference to the accompanying drawings and embodiments, wherein:
[0036] FIG1 is a SEM image of graphite after graphitization according to Example 3 of the present disclosure. DETAILED DESCRIPTION
[0037] The following will clearly and completely describe the concept and technical effects of the present disclosure in conjunction with embodiments to fully understand the purpose, features and effects of the present disclosure.
[0038] Example 1
[0039] A method for recycling negative electrode graphite of waste lithium-ion batteries, the specific process is as follows:
[0040] (1) Waste lithium-ion batteries were discharged through a salt solution, dried, crushed, calcined at 400°C for 5 hours, and sieved to obtain battery black powder. The battery black powder was acid-leached with sulfuric acid at a concentration of 3g / L, stirred at 90°C for 35 hours, and filtered after acid leaching to obtain graphite wet slag;
[0041] (2) drying the wet graphite slag at 150°C for 20 h to obtain dry graphite slag, and sintering the dry slag at 450°C in an air atmosphere for 3 h to obtain pyrolytic graphite;
[0042] (3) Pyrolytic graphite is mixed with a composite starch binder (a mixture of corn starch and SiO2 with a mass ratio of 3:1) and asphalt at a high speed, with the mass ratio of pyrolytic graphite, binder and asphalt being 1:0.04:0.07, and the mixing time is 20 minutes. The mixed powder is wet-mixed with 30% water of the mass of the pyrolytic graphite for 30 minutes to obtain a coated wet material;
[0043] (4) The coated wet material is put into a molding machine to form a ball with a diameter of 3 cm, and then dried at 110°C for 24 hours to obtain a graphite ball; the graphite ball is then sent to a carbonization and activation integrated furnace for oxygen-free high-temperature heat treatment: nitrogen is introduced into the carbonization and activation integrated furnace, and the temperature is increased to 300°C at a rate of 10°C / min and kept constant at this temperature for 1.5 hours, and then increased to 1000°C at a rate of 5°C / min and kept constant at this temperature for 2 hours, so that part of the binder is decomposed to form a network structure, thereby enhancing the strength and activity of the graphite ball;
[0044] (5) After the heat treatment is completed, nitrogen is continued to flow until the temperature of the carbonization and activation integrated furnace drops below 70°C, and then the material is discharged to obtain a high-strength, low-ash graphite molded part;
[0045] (6) The graphite molded parts are placed in a vertical continuous graphitization furnace, and arcs and resistance are formed through point contact and pores between the balls to generate high temperature, thereby reducing the power consumption of the graphitization furnace. The graphite molded parts are first treated in the low temperature range of 800-1600°C for 1-1.5 hours, and then sintered at a high temperature range of 2400°C for 2 hours to remove metal impurities (Ni, Co, Mn, Fe, Cu, etc.) and non-metallic impurities (Si, P, etc.) in the graphite slag to obtain graphitized graphite;
[0046] (7) The graphitized graphite is crushed, demagnetized, and screened to obtain the final graphite product.
[0047] Example 2
[0048] A method for recycling negative electrode graphite of waste lithium-ion batteries, the specific process is as follows:
[0049] (1) Waste lithium-ion batteries were discharged through a salt solution, dried, crushed, calcined at 400°C for 5 hours, and sieved to obtain battery black powder. The battery black powder was acid-leached with sulfuric acid at a concentration of 3g / L, stirred at 90°C for 35 hours, and filtered after acid leaching to obtain graphite wet slag;
[0050] (2) drying the wet graphite slag at 150°C for 20 h to obtain dry graphite slag, and sintering the dry slag at 450°C in an air atmosphere for 3 h to obtain pyrolytic graphite;
[0051] (3) Pyrolytic graphite is mixed with a composite starch binder (a mixture of corn starch and SiO2 with a mass ratio of 4:1) and asphalt at a high speed, with the mass ratio of pyrolytic graphite, binder and asphalt being 1:0.04:0.07, and the mixing time is 20 minutes. The mixed powder is wet-mixed with 30% water of the mass of the pyrolytic graphite for 30 minutes to obtain a coated wet material;
[0052] (4) The coated wet material is put into a molding machine to form a ball with a diameter of 3 cm, and then dried at 110°C for 24 hours to obtain a graphite ball; the graphite ball is then sent to a carbonization and activation integrated furnace for oxygen-free high-temperature heat treatment: nitrogen is introduced into the carbonization and activation integrated furnace, and the temperature is increased to 250°C at a rate of 10°C / min and kept constant at this temperature for 1.5 hours, and then increased to 900°C at a rate of 5°C / min and kept constant at this temperature for 3 hours, so that part of the binder is decomposed to form a network structure, thereby enhancing the strength and activity of the graphite ball;
[0053] (5) After the heat treatment is completed, nitrogen is continued to flow until the temperature of the carbonization and activation integrated furnace drops below 70°C, and then the material is discharged to obtain a high-strength, low-ash graphite molded part;
[0054] (6) The graphite molded parts are placed in a vertical continuous graphitization furnace, and arcs and resistance are formed through point contact and pores between the balls to generate high temperature, thereby reducing the power consumption of the graphitization furnace. The graphite molded parts are first treated in the low temperature range of 800-1600°C for 1-1.5 hours, and then sintered at a high temperature range of 2500°C for 2 hours to remove metal impurities (Ni, Co, Mn, Fe, Cu, etc.) and non-metallic impurities (Si, P, etc.) in the graphite slag to obtain graphitized graphite;
[0055] (7) The graphitized graphite is crushed, demagnetized, and screened to obtain the final graphite product.
[0056] Example 3
[0057] A method for recycling negative electrode graphite of waste lithium-ion batteries, the specific process is as follows:
[0058] (1) Waste lithium-ion batteries were discharged through a salt solution, dried, crushed, calcined at 400°C for 5 hours, and sieved to obtain battery black powder. The battery black powder was acid-leached with sulfuric acid at a concentration of 3g / L, stirred at 90°C for 35 hours, and filtered after acid leaching to obtain graphite wet slag;
[0059] (2) drying the wet graphite slag at 150°C for 20 h to obtain dry graphite slag, and sintering the dry slag at 450°C in an air atmosphere for 3 h to obtain pyrolytic graphite;
[0060] (3) Pyrolytic graphite is mixed with a composite starch binder (a mixture of corn starch and SiO2 with a mass ratio of 6:1) and asphalt at a high speed, with the mass ratio of pyrolytic graphite, binder and asphalt being 1:0.04:0.07, and the mixing time is 20 minutes. The mixed powder is wet-mixed with 30% water of the mass of the pyrolytic graphite for 30 minutes to obtain a coated wet material;
[0061] (4) The coated wet material is put into a molding machine to form a ball with a diameter of 3 cm, and then dried at 110°C for 24 hours to obtain a graphite ball; the graphite ball is then sent to a carbonization and activation integrated furnace for oxygen-free high-temperature heat treatment: nitrogen is introduced into the carbonization and activation integrated furnace, and the temperature is increased to 200°C at a rate of 10°C / min and kept constant at this temperature for 2 hours, and then increased to 800°C at a rate of 5°C / min and kept constant at this temperature for 3.5 hours, so that part of the binder is decomposed to form a network structure, thereby enhancing the strength and activity of the graphite ball;
[0062] (5) After the heat treatment is completed, nitrogen is continued to flow until the temperature of the carbonization and activation integrated furnace drops below 70°C, and then the material is discharged to obtain a high-strength, low-ash graphite molded part;
[0063] (6) The graphite molded parts are placed in a vertical continuous graphitization furnace, and arcs and resistance are formed through point contact and pores between the balls to generate high temperature, thereby reducing the power consumption of the graphitization furnace. The graphite molded parts are first treated in the low temperature range of 800-1600°C for 1-1.5 hours, and then sintered at a high temperature range of 2600°C for 2 hours to remove metal impurities (Ni, Co, Mn, Fe, Cu, etc.) and non-metallic impurities (Si, P, etc.) in the graphite slag to obtain graphitized graphite;
[0064] (7) The graphitized graphite is crushed, demagnetized, and screened to obtain the final graphite product.
[0065] FIG1 is a SEM image of the sample after graphitization in this embodiment. It can be seen from the image that the graphite has an irregular flake structure.
[0066] Comparative Example 1
[0067] A method for recycling negative electrode graphite of waste lithium-ion batteries, which differs from Example 1 in that the recovered graphite powder is directly processed using an internal graphitization furnace. The specific process is as follows:
[0068] (1) Waste lithium-ion batteries were discharged through a salt solution, dried, crushed, calcined at 400°C for 5 hours, and sieved to obtain battery black powder. The battery black powder was acid-leached with sulfuric acid at a concentration of 3g / L, stirred at 90°C for 35 hours, and filtered after acid leaching to obtain graphite wet slag;
[0069] (2) drying the wet graphite slag at 150° C. for 20 h to obtain dry graphite slag;
[0070] (3) The obtained dry graphite slag is placed in a porous crucible, and then the crucibles are connected end to end in series and placed in an inner string graphitization furnace. After the two sides and the upper cover are filled with insulation materials, graphitization is completed by supplying power for 14 hours. The graphitization temperature is 2400°C, and the metal impurities (Ni, Co, Mn, Fe, Cu, etc.) and non-metallic impurities (Si, P, etc.) in the graphite slag are removed to obtain graphitized graphite.
[0071] Comparative Example 2
[0072] A method for recycling negative electrode graphite of waste lithium-ion batteries, which differs from Example 1 in that no composite starch binder is added. The specific process is as follows:
[0073] (1) Waste lithium-ion batteries were discharged through a salt solution, dried, crushed, calcined at 400°C for 5 hours, and sieved to obtain battery black powder. The battery black powder was acid-leached with sulfuric acid at a concentration of 3g / L, stirred at 90°C for 35 hours, and filtered after acid leaching to obtain graphite wet slag;
[0074] (2) drying the wet graphite slag at 150°C for 20 h to obtain dry graphite slag, and sintering the dry slag at 450°C for 3 h in an air atmosphere to obtain pyrolytic graphite;
[0075] (3) Pyrolytic graphite and asphalt are mixed at a high speed, with a mass ratio of pyrolytic graphite to asphalt of 1:0.07, and the mixing time is 20 min. The mixed powder is wet-mixed with water of 30% of the mass of the pyrolytic graphite for 30 min to obtain a coated wet material;
[0076] (4) The coated wet material was put into a molding machine to form balls with a diameter of 3 cm. The obtained graphite balls were dried at 110°C for 24 hours. After drying, the molded graphite balls broke and returned to powder; therefore, the subsequent carbonization and continuous graphitization treatments could not be continued.
[0077] Physical and chemical properties
[0078] Table 1 is a comparison of the impurity element content of the samples prepared in Examples 1, 2, and 3 and Comparative Examples 1 and 2, and Table 2 is a comparison of the specific surface area, volatile matter, and ash content.
[0079] Table 1 Graphite impurity element content (ppm)
[0080] Table 2 Graphite volatile matter, ash content and specific surface area
[0081] As can be seen from the examples in Tables 1 and 2, the content of impurity elements decreases significantly with increasing graphitization temperature. Volatile matter, ash content, and specific surface area also decrease accordingly. The difference between Comparative Example 1 and the examples is that the examples use pre-carbonization before high-temperature graphitization in a continuous graphitization furnace, while Comparative Example 1 uses a conventional internal graphitization furnace instead of a continuous graphitization furnace to graphitize the dried graphite without preparing it into balls. In Table 1, the impurity element content of Comparative Example 1 is similar to that of the embodiment, while the volatile matter, ash content and surface area of the graphite of Comparative Example 1 in Table 2 are higher. This is because Comparative Example 1 and each embodiment are all graphitized, and at the same graphitization temperature, the removal effect of impurity elements by different graphitization treatment methods is not much different. However, the treatment methods in the embodiments are all to first pyrolyze the dried graphite in a furnace, and then pre-carbonize it in a carbonization and activation integrated furnace. During the pyrolysis and pre-carbonization process, organic impurities such as organic binders in the graphite slag can be removed, and volatiles are removed more thoroughly in this process. The lower ash content is because when the embodiment is subjected to a continuous graphitization furnace, the balls are stacked to form pores, which is conducive to the escape of ash through the "pores" during the graphitization process. Therefore, the embodiment has a better ash removal effect. The specific surface area is related to the volatile matter and ash content. The higher the volatile matter and ash content, the more impurities in the graphite and the higher the specific surface area.
[0082] Test example
[0083] The graphite materials were fabricated into batteries. Specifically, graphite, PVDF, and super P conductive agent were dissolved in NMP at a ratio of 91.6:6.6:1.8 to form a slurry. The slurry was then coated onto copper foil, and the electrodes were dried in a drying oven at 80°C for 8 hours. Finally, button cells were assembled in an argon-filled glove box. The electrolyte used was NaClO₄ dissolved in ethylene carbonate and propylene carbonate in a 1:1 volume ratio. Lithium metal foil served as the counter and reference electrodes. The button cells were then tested for electrical performance using a test voltage of 0–2 V, constant current charge and discharge, and a 0.1C rate.
[0084] Table 3 is a comparison of the first discharge specific capacity and coulombic efficiency of the samples prepared in Examples 1, 2, 3 and Comparative Examples 1 and 2.
[0085] Table 3 First discharge specific capacity and coulombic efficiency test data of graphite samples
[0086] As can be seen from the examples in Table 3, as the impurity element content decreases, the specific capacity and initial efficiency are improved. The graphite volatile matter, ash content, and specific surface area of Comparative Examples 1 and 2 are higher than those of the examples, making their electrochemical performance significantly inferior to that of the examples.
Claims
1. A method for recycling negative electrode graphite of waste lithium-ion batteries, It is characterized in that The following steps are involved: S1: mixing the negative electrode graphite of waste lithium-ion batteries, composite starch binder and asphalt, adding water to the mixed powder for wet mixing to obtain coated wet material; S2: forming the coated wet material into a shaped piece with a transverse dimension of 15-50 mm, drying it and then carbonizing it to obtain a graphite molded piece; S3: putting the graphite molded part into a vertical continuous graphitization furnace, and sequentially processing it through a low temperature section and a high temperature section of the vertical continuous graphitization furnace to obtain graphitized graphite, and the graphitized graphite is crushed to obtain a finished graphite product; the temperature of the low temperature section is 800-1700°C, and the temperature of the high temperature section is 2400-2700°C.
2. The method according to claim 1, It is characterized in that In step S1, the negative electrode graphite of the waste lithium ion battery is obtained by the following process: the waste lithium ion battery is discharged, crushed, calcined and sieved to obtain battery black powder, the battery black powder is acid-leached and then solid-liquid separated to obtain graphite wet slag, and the graphite wet slag is dried and heat-treated to obtain the negative electrode graphite of the waste lithium ion battery.
3. The method according to claim 2, It is characterized in that In step S1, the heat treatment is oxygen sintering or oxygen-free sintering; the temperature of the oxygen sintering is 350-550°C, and the time is 2-4 hours; the temperature of the oxygen-free sintering is 400-750°C, and the time is 2-4 hours.
4. The method according to claim 2, It is characterized in that In step S1, the calcination temperature is 300-600°C, and the calcination time is 3-10h.
5. The method according to claim 2, It is characterized in that In step S1, the acid leaching uses sulfuric acid with a concentration of 0.5-3 g / L; the temperature of the acid leaching is 60-90° C., and the time of the acid leaching is 20-40 hours.
6. The method according to claim 2, It is characterized in that In step S1, the drying temperature is 80-200°C, and the drying time is 10-30 hours.
7. The method according to claim 1, It is characterized in that In step S1, the mass ratio of the negative electrode graphite, the composite starch binder and the asphalt is 1:(0.03-0.06):(0.05-0.08).
8. The method according to claim 1, It is characterized in that In step S1, the negative electrode graphite, composite starch binder and asphalt are mixed for 10-30 minutes.
9. The method according to claim 1, It is characterized in that In step S1, the amount of water added is 20%-50% of the mass of the negative electrode graphite.
10. The method according to claim 1, It is characterized in that In step S1, the wet mixing time is 20-40 minutes.
11. The method according to claim 1, It is characterized in that In step S1, the composite starch binder is starch and SiO 2 The starch is selected from at least one of corn starch, rice starch, potato starch, sweet potato starch or wheat starch.
12. The method according to claim 1, It is characterized in that In step S2, the shaped piece is at least one of a sphere, a rod, a tube or a cube.
13. The method according to claim 1, It is characterized in that In step S2, the method for preparing the shaped part is to put the coated wet material into a molding machine and press it into a target shape.
14. The method according to claim 1, It is characterized in that In step S2, the drying temperature is 80-180°C, and the drying time is 3-30 hours.
15. The method according to claim 1, It is characterized in that In step S2, the carbonization process is as follows: heating to 200-350°C and maintaining the temperature for 0.5-2h under a protective atmosphere, and then heating to 500-1000°C and maintaining the temperature for 1-4h.
16. The method according to claim 1, It is characterized in that In step S3, the low temperature treatment time is 1-1.5 hours.
17. The method according to claim 1, It is characterized in that In step S3, the high temperature treatment period is 2-4 hours.
Citation Information
Patent Citations
Lithium battery graphite anode material production process
CN108101042A
Method for recovering a lithium ion battery anode material
CN108879014A
Regeneration method of waste graphite negative electrode material of lithium ion battery
CN114843648A
Negative electrode raw material pelletizing preparation process and graphitization charging method
CN115676816A
Method for recovering graphite from black powder acid leaching residues of waste lithium batteries
CN115974069A
Cited By
Slag iron graphite separation and purification equipment and method
CN119910011A
Method for recovering graphite from waste lithium battery negative plate
CN120229716A
Repairing and regenerating method of graphite negative electrode material of waste lithium battery
CN120440891A