Positive electrode active material and method for preparing same, and positive electrode sheet, battery and electric device comprising same
By introducing K elements into the positive electrode active material and using alkaline washing and sintering technology, the problem of limited performance of the positive electrode active material in sodium ion batteries is solved, and good cycle and rate performance and battery life are achieved.
Patent Information
- Application Number
- PCT/CN2023/094848
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium-ion batteries are facing the shortage of lithium resources. There are high content of free alkaline substances in the preparation of the positive electrode active materials of sodium-ion batteries that affect performance. It is difficult for existing surface modification technologies to effectively improve circulation and rate performance.
The layered transition metal oxide positive electrode active material containing K elements is adopted. Through alkaline washing liquid treatment and sintering technology, K elements are ensured to decrease distribution from the surface to the inside, stabilize the crystal structure, reduce stress and microcracks, and improve interface stability.
It significantly improves the circulation performance and rate performance of the positive electrode active material, extends the cycle life of the battery, reduces the probability of the crystal structure collapse after charging, and increases the energy density of the battery.
Smart Images

Figure CN2023094848_21112024_PF_FP_ABST
Abstract
Description
Positive electrode active material, preparation method thereof, positive electrode sheet, battery and electric device containing the same Technical Field
[0001] The present application relates to a positive electrode active material, a preparation method thereof, and a positive electrode plate, a battery, and an electrical device containing the same. Background Art
[0002] In recent years, batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. At present, lithium-ion batteries still occupy the core position of batteries. At the same time, lithium-ion batteries also face great challenges, such as the increasing shortage of lithium resources. Sodium resources are far more abundant than lithium resources, are more widely distributed, and have a much lower cost than lithium. Therefore, sodium-ion batteries have become a new generation of electrochemical systems with great potential to replace lithium-ion batteries. The positive electrode active material is a key factor affecting the performance of sodium-ion batteries. Due to the constraints of the preparation process, there is often a high content of free alkaline substances on the surface of the positive electrode active material, which will affect the performance of the sodium-ion battery. Therefore, effective technical means are needed to improve the performance of the positive electrode active material. The above statements are only used to provide background technical information related to this application and do not necessarily constitute prior art.
[0003] Summary of the Invention
[0004] The present application provides a positive electrode active material, a preparation method thereof, and a positive electrode plate, a battery, and an electrical device containing the same, which can stabilize the crystal structure of the positive electrode active material and enable the positive electrode active material to have good cycle performance and rate performance.
[0005] The first aspect of the present application provides a positive electrode active material, comprising a layered transition metal oxide represented by formula (I), Na x K y M a A b B c O m Q n Formula (I)
[0006] x>0.5, 0<y<0.5, 0<a≤1, 0≤b≤1 / 3, 0≤c≤1 / 3, 1.9≤m≤2, 0≤n≤0.1, M includes one or more of Mn, Fe, Co, Ni, and Cu, A includes one or more metal elements from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, and Group VIB, B includes one or more non-metallic elements from Group IIIA, Group IVA, Group VA, and Group VIA, Q includes one or more non-metallic elements from Group VA and Group VIIA, and the positive electrode active material includes K element, and the content of K element decreases from the particle surface of the positive electrode active material to the particle interior.
[0007] By introducing K element into the positive electrode active material with a decreasing content from the particle surface to the particle interior, the crystal structure of the positive electrode active material can be stabilized and the positive electrode active material can have good cycle performance and rate performance.
[0008] In any embodiment, the area formed by a distance of 0.05L extending from the surface of the positive electrode active material particle to the interior of the particle is recorded as the surface area of the positive electrode active material, L refers to the length of the major axis of the positive electrode active material particle, and the mass of the K element in the surface area of the positive electrode active material is 50% to 95% of the total mass of the K element in the positive electrode active material, and can be optionally 70% to 90%.
[0009] The content of K element in the positive electrode active material shows a decreasing characteristic from the particle surface to the particle interior, and the K element is mainly distributed in the surface area of the positive electrode active material, which can effectively reduce the stress during the battery cycle and thus reduce the generation of microcracks; it can also better play the role of K + It plays a supporting role, thereby stabilizing the crystal structure of the positive electrode active material, improving the interface stability, improving the stability of the crystal structure, and reducing the probability of crystal structure collapse or irreversible transformation after a large amount of sodium is removed from the positive electrode active material in the late stage of charging, thereby improving the cycle performance and / or rate performance of the battery.
[0010] In any embodiment, the positive electrode active material includes one or more of an O3 phase, a P2 phase, and a P3 phase.
[0011] In any embodiment, the positive electrode active material includes an O3 phase, and in the peak separation pattern of the X-ray diffraction pattern of the positive electrode active material, two diffraction peaks exist within the range of 2θ of 16.0° to 16.7°, the diffraction peak with 2θ between 16.0° and 16.3° is recorded as the first peak, and the diffraction peak with 2θ between 16.3° and 16.7° is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is less than or equal to 0.1:1, and can optionally be less than or equal to 0.076:1. This indicates that the main structure of the O3 phase of the positive electrode active material is well maintained, and the positive electrode active material contains only a small amount of lattice-distorted O3 phase.
[0012] In any embodiment, the positive electrode active material includes an O3 phase, and the X-ray diffraction pattern of the positive electrode active material includes a (104) crystal plane diffraction peak with 2θ located between 41.5° and 42.5° and a (015) crystal plane diffraction peak with 2θ located between 44.5° and 45.5°, and the ratio of the peak intensity of the (104) crystal plane diffraction peak to the peak intensity of the (015) crystal plane diffraction peak is greater than 10:1. This indicates that the layered structure of the positive electrode active material is relatively stable, and is not prone to crystal plane slip or transition metal element aggregation.
[0013] In any embodiment, A includes one or more elements selected from the group consisting of Li, Ti, Zr, Sb, Nb, Mg, Ca, Mo, Zn, Cr, W, Bi, Sn, Ge, Al, Ba, Sr, and V.
[0014] In any embodiment, B includes one or more elements selected from Si, P, B, S, and Se.
[0015] In any embodiment, Q includes one or more elements selected from the group consisting of F, Cl, and N.
[0016] In any embodiment, x ≥ 2 / 3.
[0017] In any embodiment, 0.012≤y≤0.05. When the content of the K element in the positive electrode active material is within the above range, the surface structure of the positive electrode active material can be better stabilized, reducing the probability of crystal structure collapse or irreversible transformation after a large amount of sodium removal in the positive electrode active material in the late stage of charging; and at the same time, the positive electrode active material can have a higher specific capacity and good cycle performance and rate performance.
[0018] In any embodiment, 0≤b≤1 / 3, 0≤c≤1 / 3, and 0<b+c≤1 / 3.
[0019] In any embodiment, the positive electrode active material includes a layered transition metal oxide represented by formula (I-1), Na x K y Mnp Fe q M′ a-p-q A b B c O m Q n Formula (I-1)
[0020] 0<p<1, 0<q<1, apq≥0, and M includes one or more elements selected from Co, Ni, and Cu.
[0021] In any embodiment, 0<p≤2 / 3.
[0022] In any embodiment, 0<q≤1 / 3.
[0023] In any embodiment, 0<apq≤1 / 3.
[0024] In any embodiment, the content of free alkaline substances on the surface of the positive electrode active material is 0.2-20 wt %, and optionally 0.5-1.4 wt %. The low content of free alkaline substances on the surface of the positive electrode active material can provide the positive electrode active material with high interfacial stability, thereby improving the cycle performance and / or rate performance of the battery, and also improving the processing performance of the positive electrode slurry and the battery.
[0025] In any embodiment, the pH of the positive electrode active material is 11.5-13.5, optionally 11.8-12.6. The lower pH of the positive electrode active material can provide the positive electrode active material with higher interfacial stability, thereby improving the cycle performance and / or rate performance of the battery, and also improving the processing performance of the positive electrode slurry and the battery.
[0026] In any embodiment, the morphology of the positive electrode active material includes one or more of spherical single crystals, flaky single crystals, and spherical polycrystals.
[0027] In any embodiment, the volume distribution particle size Dv50 of the positive electrode active material is 3-15 μm, optionally 4-9 μm. When the volume distribution particle size Dv50 of the positive electrode active material is within the above range, it can have a higher gram capacity and a higher compaction density, and can also have good ion transport capability and rate performance.
[0028] The second aspect of the present application provides a method for preparing a positive electrode active material, comprising the following steps: providing an initial positive electrode active material, wherein the initial positive electrode active material comprises a sodium-containing layered transition metal oxide; washing the initial positive electrode active material with an alkaline washing solution, wherein the alkaline washing solution comprises K +After washing, the positive electrode active material is obtained by drying, wherein the positive electrode active material comprises a layered transition metal oxide represented by formula (I), Na x K y M a A b B c O m Q n Formula (I)
[0029] x>0.5, 0<y<0.5, 0<a≤1, 0≤b≤1 / 3, 0≤c≤1 / 3, 1.9≤m≤2, 0≤n≤0.1, M includes one or more of Mn, Fe, Co, Ni, and Cu, A includes one or more metal elements from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, and Group VIB, B includes one or more non-metallic elements from Group IIIA, Group IVA, Group VA, and Group VIA, Q includes one or more non-metallic elements from Group VA and Group VIIA, and the positive electrode active material includes K element, and the content of K element decreases from the particle surface of the positive electrode active material to the particle interior.
[0030] The positive electrode active material obtained by the preparation method of the present application has a lower pH, a lower content of free alkaline substances on the surface, and also has a K element whose content decreases from the particle surface to the interior of the particle. This can not only stabilize the crystal structure of the positive electrode active material, but also enable the positive electrode active material to have good cycle performance and rate performance.
[0031] In any embodiment, in the step of washing the initial positive electrode active material with an alkaline washing solution, the washing temperature is less than or equal to 35°C, and can be optionally 20°C-30°C. When the washing temperature is within the above range, the Na + / H + exchange rate and reduce interlayer sodium dissolution.
[0032] In any embodiment, in the step of washing the initial positive electrode active material with an alkaline washing solution, the washing time is less than or equal to 60 minutes, and can be 5-20 minutes. When the washing time is within the above range, the Na + / H + Exchange and reduce interlayer sodium dissolution.
[0033] In any embodiment, the pH of the alkaline washing solution is greater than or equal to 12, and can be optionally 13-14. When the pH of the alkaline washing solution is within the above range, the Na + / H + Exchange and reduce interlayer sodium dissolution.
[0034] In any embodiment, the solute in the alkaline washing solution includes one or more of potassium hydroxide, potassium carbonate, and potassium bicarbonate.
[0035] In any embodiment, the solvent in the alkaline washing solution includes one or more of water, alcohol solvents, and ester solvents, and may optionally include water.
[0036] In any embodiment, the alkaline washing solution further comprises Na + By making the alkaline washing solution include Na + , can supplement Na + , improve the capacity, and further reduce Na + / H + Exchange reduces the dissolution of sodium between layers and enables the positive electrode active material to better maintain its original layered structure.
[0037] In any embodiment, Na + With K + The molar ratio is 1:(0.1-10), and can be optionally 1:(0.2-2).
[0038] In any embodiment, the preparation method further comprises the step of: sintering the initial positive electrode active material after washing, to obtain the positive electrode active material.
[0039] Sintering can stabilize the surface of the material and make the surface unstable due to washing become stable again, thereby repairing surface defects and reducing vacancies. Sintering can also make the surface K + Stable in Na + Position, in order to better play the role of support, improve the rate performance, and also reduce the probability of crystal structure collapse or irreversible transformation after a large amount of sodium removal in the positive electrode active material in the late charging period. Through sintering treatment, the K + Further diffusion into the interior of the particle makes the content of K element show a better decreasing characteristic from the particle surface to the interior of the particle.
[0040] In any embodiment, the sintering temperature is 300°C-600°C, optionally 450°C-550°C.
[0041] In any embodiment, the sintering time is less than or equal to 10 hours, and can be optionally 3 hours to 8 hours.
[0042] In any embodiment, the sintering atmosphere is an oxygen-containing atmosphere. More preferably, the volume fraction of oxygen in the sintering atmosphere is 15%-40%. Sintering in an oxygen-containing atmosphere can stabilize the surface structure of the material, allowing surface sodium that has become unstable due to washing to react with oxygen and become stable again, thereby repairing surface defects and reducing vacancies, thereby improving the cycle performance and / or rate performance of the battery.
[0043] By adjusting one or more parameters such as the sintering temperature, sintering time, alkaline washing solution concentration, washing temperature, and washing time within the above range, the content of the K element can be gradually reduced from the surface of the positive electrode active material particles to the interior of the particles, and the K element can be prevented from exhibiting a uniform distribution characteristic in the positive electrode active material; the distribution area of the K element can also be adjusted.
[0044] The third aspect of the present application provides a positive electrode plate, comprising a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, wherein the positive electrode film layer comprises the positive electrode active material of the first aspect of the present application or the positive electrode active material prepared by the preparation method of the second aspect of the present application.
[0045] In any embodiment, the content of the positive electrode active material in the positive electrode film layer is 50 wt % to 99 wt %, and more preferably 85 wt % to 99 wt %, based on the total weight of the positive electrode film layer.
[0046] A fourth aspect of the present application provides a battery, comprising the positive electrode sheet of the third aspect of the present application.
[0047] A fifth aspect of the present application provides an electrical device comprising the battery of the fourth aspect of the present application.
[0048] The electric device of the present application includes the battery provided by the present application, and thus has at least the same advantages as the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0050] FIG1 is a schematic diagram of a battery cell according to an embodiment of the present application.
[0051] FIG. 2 is an exploded schematic diagram of an embodiment of the battery cell of FIG. 1 .
[0052] FIG3 is a schematic diagram of an embodiment of a battery module of the present application.
[0053] FIG4 is a schematic diagram of an embodiment of a battery pack of the present application.
[0054] FIG. 5 is an exploded schematic diagram of the embodiment of the battery pack shown in FIG. 4 .
[0055] FIG6 is a schematic diagram of an embodiment of an electric device including the battery of the present application as a power source.
[0056] FIG7 is an X-ray diffraction pattern of the positive electrode active materials prepared in Example 1, Comparative Example 1 and Comparative Example 3.
[0057] FIG8 is a cycle curve diagram of button batteries prepared in Example 1, Comparative Example 1 and Comparative Example 3.
[0058] In the accompanying drawings, which are not necessarily drawn to scale, reference numerals are as follows: 1 battery pack, 2 upper housing, 3 lower housing, 4 battery module, 5 battery cell, 51 housing, 52 electrode assembly, 53 cover plate. DETAILED DESCRIPTION
[0059] Below, with appropriate reference to the accompanying drawings, the embodiments of the positive electrode active material, its preparation method, and the positive electrode sheet, battery, and electrical device containing the same are specifically disclosed. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0060] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0061] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0062] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0063] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0064] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0065] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0066] In this application, the terms "plurality" and "multiple" refer to two or more.
[0067] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.
[0068] Unless otherwise stated, the numerical values of the various parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods given in the examples of this application. Unless otherwise stated, the test temperature of each parameter is 25°C.
[0069] The battery mentioned in the embodiments of the present application may be a single physical module including one or more battery cells to provide higher voltage and capacity. For example, the battery mentioned in the present application may include a battery cell, a battery module, or a battery pack.
[0070] A battery cell is the smallest unit of a battery, independently capable of charging and discharging. A battery cell can be cylindrical, flat, rectangular, or in other shapes, though this is not a limitation in the present invention. Figure 1 shows a battery cell 5 with a rectangular structure as an example.
[0071] When there are multiple battery cells, the multiple battery cells are connected in series, in parallel, or in mixed series via a busbar. In some embodiments, the battery may be a battery module; when there are multiple battery cells, the multiple battery cells are arranged and fixed to form a battery module. In some embodiments, the battery may be a battery pack, which includes a housing and battery cells, with the battery cells or battery modules housed in the housing. In some embodiments, the housing may serve as part of the vehicle's chassis structure. For example, a portion of the housing may form at least a portion of the vehicle's floor, or a portion of the housing may form at least a portion of the vehicle's crossbeam or longitudinal beam.
[0072] In some embodiments, the battery may be an energy storage device, including an energy storage container, an energy storage cabinet, and the like.
[0073] The battery cells provided in the embodiments of the present application include sodium ion battery cells, sodium metal battery cells, negative electrode-free sodium metal battery cells, etc., which are not limited in the embodiments of the present application.
[0074] A battery cell generally includes an electrode assembly. The electrode assembly generally includes a positive electrode sheet, a negative electrode sheet, and a separator located between the positive and negative electrode sheets. The electrode assembly can be a wound structure or a laminated structure, which is not limited in the present embodiment.
[0075] The battery cell may also include an outer packaging, which can be used to encapsulate the electrode assembly and electrolyte. The outer packaging can be a hard shell, such as a hard plastic shell, aluminum shell, steel shell, etc. The outer packaging can also be a soft package, such as a bag-type soft package. The soft package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0076] In some embodiments, as shown in Figure 2, the outer packaging may include a housing 51 and a cover plate 53. The housing 51 may include a bottom plate and side plates connected to the bottom plate, which together form a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover plate 53 is used to cover the opening, thereby sealing the receiving cavity. The electrode assembly 52 is enclosed in the receiving cavity. The number of electrode assemblies 52 contained in the battery cell 5 can be one or more, and can be adjusted according to needs.
[0077] In some embodiments, battery cells can be assembled into a battery module. The number of battery cells contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 3 is a schematic diagram of a battery module 4 as an example. As shown in Figure 3, in the battery module 4, multiple battery cells 5 can be arranged in sequence along the length of the battery module 4. Of course, they can also be arranged in any other manner. The multiple battery cells 5 can further be fixed by fasteners.
[0078] Optionally, the battery module 4 may further include a housing having an accommodation space, and the plurality of battery cells 5 are accommodated in the accommodation space.
[0079] In some embodiments, the battery modules described above may also be assembled into a battery pack, and the number of battery modules contained in the battery pack may be adjusted according to the application and capacity of the battery pack.
[0080] Figures 4 and 5 are schematic diagrams of an exemplary battery pack 1. As shown in Figures 4 and 5, the battery pack 1 may include a housing and multiple battery modules 4 disposed within the housing. The housing comprises an upper housing 2 and a lower housing 3. The upper housing 2 covers the lower housing 3 and forms an enclosed space for accommodating the battery modules 4. The multiple battery modules 4 may be arranged in any manner within the housing.
[0081] Sodium batteries typically use sodium-containing layered transition metal oxides as positive electrode active materials, which have poor interfacial stability. At the same time, a high-temperature sintering process is usually necessary when preparing the positive electrode active materials. In order to improve the yield and compensate for the volatilization of Na during high-temperature sintering during the preparation process, an excess of sodium source is usually added. As a result, after the high-temperature sintering process, some of the sodium source will remain on the surface of the positive electrode active material and react with moisture and CO2 in the air to form free alkaline substances such as NaOH and Na2CO3. Free alkaline substances cause the positive electrode slurry to easily gel or solidify, affecting the coating performance of the positive electrode slurry and the performance of the battery; alkaline substances such as Na2CO3 have poor thermal stability and are easily decomposed and gasified under high pressure; alkaline substances are not electrochemically active, and excessive content will hinder the transmission of sodium ions. In addition, after the high-temperature sintering process is completed, free alkaline substances such as NaOH and Na2CO3 are inevitably formed on the surface of the positive electrode active material. If this part of the free alkaline substances is not removed, it will continue to react with moisture and CO2 in the air and the electrolyte, thereby further hindering the transmission of sodium ions and even causing part of the sodium in the crystal structure of the positive electrode active material to be released, the stability of the crystal structure becomes worse, and the crystal structure is prone to irreversible transformation, thereby affecting the capacity of the positive electrode active material, the preparation of the battery and the performance of the battery.
[0082] The surface modification technologies currently used mainly include coating modification and washing modification.
[0083] Coating modification usually involves coating the surface of the positive electrode active material with an inactive material, which often leads to a decrease in the specific capacity of the positive electrode active material and a deterioration in the ion transport capability, thereby causing the cycle performance and rate performance of the positive electrode active material to deteriorate.
[0084] There are two main types of washing processes: one is washing with water or acidic solution, and the other is washing with organic solvent. Washing with water or acidic solution has a good application effect in lithium batteries, and can effectively reduce the content of free alkaline substances (mainly including LiOH, Li2CO3, etc.) on the surface of lithium-containing positive electrode active materials, especially ternary materials (such as NCM). However, the positive electrode active materials of sodium batteries, especially sodium-containing layered transition metal oxides, are very sensitive to water and acid, and Na is easily generated during washing with water or acidic solution. + / H + The exchange of sodium will lead to the reduction of lattice sodium, the deterioration of crystal structure stability, and the irreversible change of crystal structure. + / H + Exchange will also lead to a decrease in the lattice sodium of the positive electrode active material, a deterioration in the stability of the crystal structure, and an easy irreversible change in the crystal structure. In addition, the organic solvent washing process is complicated and the cost is high.
[0085] In view of the above problems, the inventors of the present application have provided a potassium ion-doped positive electrode active material after research, which has good crystal structure stability and also has good cycle performance and rate performance.
[0086] The positive electrode active material provided in the embodiment of the present application includes a layered transition metal oxide represented by formula (I), Na x K y M a A b B c O m Q n Formula (I)
[0087] x>0.5, 0<y<0.5, 0<a≤1, 0≤b≤1 / 3, 0≤c≤1 / 3, 1.9≤m≤2, 0≤n≤0.1, M includes one or more of Mn, Fe, Co, Ni, and Cu, A includes one or more metal elements from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, and Group VIB, B includes one or more non-metallic elements from Group IIIA, Group IVA, Group VA, and Group VIA, Q includes one or more non-metallic elements from Group VA and Group VIIA, and the positive electrode active material includes element K, and the content of element K decreases from the particle surface of the positive electrode active material to the particle interior.
[0088] K + The ionic radius is large (about 0.138nm), which occupies part of the surface of the positive electrode active material. + After the positive electrode active material is positioned, the interlayer spacing of the positive electrode active material can be increased, so that the positive electrode active material can have good rate performance.
[0089] After a large amount of sodium is removed from the positive electrode active material in the late stage of charging, the stability of the crystal structure becomes poor, and it is easy to undergo irreversible transformation from the layered structure to the rock salt phase structure. + After being introduced into the positive electrode active material, K + It can play a supporting role, stabilize the crystal structure of the positive electrode active material, improve the interface stability, and also improve the stability of the crystal structure, reducing the probability of crystal structure collapse or irreversible transformation after a large amount of sodium is removed from the positive electrode active material in the later stage of charging, thereby improving the cycle stability of the positive electrode active material.
[0090] The content of K element in the positive electrode active material shows a decreasing characteristic from the particle surface to the particle interior, which can effectively reduce the stress during the battery cycle and reduce the generation of microcracks, so that the battery using the positive electrode active material has a long cycle life.
[0091] Therefore, by introducing K element into the positive electrode active material with a decreasing content from the particle surface to the particle interior, the crystal structure of the positive electrode active material can be stabilized and the positive electrode active material can have good cycle performance and rate performance.
[0092] Unless otherwise specified, in the chemical formula of the positive electrode active material, when M is more than two elements, the above-mentioned limitation on the numerical range of a is not only a limitation on the stoichiometric number of each element as M, but also a limitation on the sum of the stoichiometric numbers of each element as M. For example, when M is more than two elements M1, M2...Mn, the stoichiometric numbers a1, a2...an of M1, M2...Mn must each fall within the numerical range of a defined in this application, and the sum of a1, a2...an must also fall within the numerical range. Similarly, in the embodiments of the present application, for the case where other elements are more than two elements, the limitation on the numerical range of their stoichiometric numbers also has the above meaning.
[0093] M includes one or more elements selected from the group consisting of Mn, Fe, Co, Ni, and Cu.
[0094] Layered transition metal oxides can be either monolithic or multi-component materials. A "monolithic material" refers to a material containing only one transition metal M, such as one of Mn, Fe, Co, Ni, and Cu. A "multi-component material" refers to a material containing at least two transition metals M, such as at least two of Mn, Fe, Co, Ni, and Cu, including a combination of Mn and Fe, a combination of Mn, Fe, and Ni, or a combination of Mn, Fe, and Cu.
[0095] In some embodiments, the positive electrode active material may include a layered transition metal oxide represented by formula (I-1), Na x K y Mn p Fe q M′ a-p-q A b B c O m Q n Formula (I-1)
[0096] 0<p<1, 0<q<1, apq≥0, and M includes one or more elements selected from Co, Ni, and Cu.
[0097] In some embodiments, 0<p≤2 / 3.
[0098] In some embodiments, 0<q≤1 / 3.
[0099] In some embodiments, 0≤apq≤1 / 3, optionally, 0<apq≤1 / 3.
[0100] In some embodiments, x may be ≥ 2 / 3, ≥ 0.7, ≥ 0.8, ≥ 0.9, ≥ 0.92, ≥ 0.94, ≥ 0.96.
[0101] In some embodiments, 0.001≤y<0.5, optionally, 0.001≤y≤0.4, 0.001≤y≤0.3, 0.001≤y≤0.2, 0.001≤y≤0.1, 0.001≤y≤0.05, 0.005≤y≤0.05, 0.008≤y≤0.05, 0.012≤y≤0.05. When the content of K element in the positive electrode active material is within the above range, the surface structure of the positive electrode active material can be better stabilized, and the probability of crystal structure collapse or irreversible transformation after a large amount of sodium removal of the positive electrode active material in the late stage of charging can be reduced; at the same time, the positive electrode active material can also have a higher gram capacity and good cycle performance and rate performance. When the content of K element is too much, since K element does not provide capacity, the gram capacity of the positive electrode active material will be reduced, and excessive K + Occupy Na + Position, it will also hinder Na + migration, and affect the battery cycle performance and rate performance.
[0102] In some embodiments, b is 0.
[0103] In some embodiments, 0<b≤1 / 3.
[0104] In some embodiments, c is 0.
[0105] In some embodiments, 0<c≤1 / 3.
[0106] In some embodiments, b is 0 and c is 0.
[0107] In some embodiments, 0<b≤1 / 3 and 0<c≤1 / 3.
[0108] In some embodiments, 0≤b≤1 / 3, 0≤c≤1 / 3, and 0<b+c≤1 / 3. For example, b is 0, 0<c≤1 / 3; or, c is 0, 0<b≤1 / 3; or, 0<b<1 / 3, 0<c<1 / 3, and 0<b+c≤1 / 3.
[0109] When the total content of element A and element B is within an appropriate range, it helps to further improve the cycle performance and / or rate performance of the battery.
[0110] In some embodiments, A may include one or more elements of Li, Ti, Zr, Sb, Nb, Mg, Ca, Mo, Zn, Cr, W, Bi, Sn, Ge, Al, Ba, Sr, and V.
[0111] In some embodiments, B may include one or more elements of Si, P, B, S, and Se.
[0112] In some embodiments, n is 0.
[0113] In some embodiments, 0<n≤0.1. When the content of element Q is within a suitable range, it helps to further improve the cycle performance and / or rate performance of the battery.
[0114] In some embodiments, Q may include one or more elements of F, Cl, and N.
[0115] The content of each element in the positive electrode active material can be determined by inductively coupled plasma emission spectroscopy (ICP) in accordance with EPA 6010D-2014.
[0116] In some embodiments, the area formed by a distance of 0.05L extending from the surface of the positive electrode active material particles to the interior of the particles is recorded as the surface area of the positive electrode active material, L refers to the length of the major axis of the positive electrode active material particles, and the mass of the K element in the surface area of the positive electrode active material is 50% to 95% of the total mass of the K element in the positive electrode active material, which can be optionally 70% to 95%, 75% to 95%, 80% to 95%, 83% to 95%, 70% to 92%, 75% to 92%, 80% to 92%, 83% to 92%, 70% to 90%, 75% to 90%, 80% to 90%, 83% to 90%.
[0117] The content of K element in the positive electrode active material shows a decreasing characteristic from the particle surface to the particle interior, and the K element is mainly distributed in the surface area of the positive electrode active material, which can effectively reduce the stress during the battery cycle and thus reduce the generation of microcracks; it can also better play the role of K + It plays a supporting role, thereby stabilizing the crystal structure of the positive electrode active material, improving the interface stability, improving the stability of the crystal structure, and reducing the probability of crystal structure collapse or irreversible transformation after a large amount of sodium is removed from the positive electrode active material in the late stage of charging, thereby improving the cycle performance and / or rate performance of the battery.
[0118] The ratio of the mass of the K element in the surface region of the positive electrode active material to the total mass of the K element in the positive electrode active material can be obtained by measuring a cross-sectional image of the positive electrode active material.
[0119] The cross-sectional image of the positive electrode active material includes a cross-sectional image passing through the center of the positive electrode active material particle. The "center of the particle" refers to the range within a radius of 0.1 μm extending from the geometric center of the particle to the particle surface.
[0120] The major axis length of the positive electrode active material particle refers to the maximum value when the line connecting two points on the particle surface passes through the geometric center of the particle.
[0121] The cross section of the positive electrode active material can be prepared using a cross section polisher (e.g., an IB-09010CP argon ion cross section polisher from JEOL, Japan); then, referring to JY / T010-1996, a scanning electron microscope (e.g., a Sigma 300 scanning electron microscope from ZEISS, Germany) is used to scan the cross section of the positive electrode active material; and then, inductively coupled plasma emission spectroscopy (ICP) is used for detection.
[0122] The ratio of the mass of the K element in the surface area (the area extending 0.05L inward from the edge of the particle in the cross-sectional image, where L refers to the length of the major axis of the positive electrode active material particle) in the cross-sectional image of the obtained positive electrode active material to the mass of all K elements in the cross-sectional image of the obtained positive electrode active material is taken as the ratio of the mass of the K element in the surface area of the positive electrode active material to the total mass of the K element in the positive electrode active material.
[0123] In some embodiments, the volume distribution particle size Dv50 of the positive electrode active material may be 3-15 μm, optionally 4-9 μm. When the volume distribution particle size Dv50 of the positive electrode active material is within the above range, it may have a higher gram capacity and a higher compaction density, and may also have good ion transport capability and rate performance.
[0124] The volume distribution particle size Dv50 of the positive electrode active material is well known in the art and represents the particle size corresponding to the cumulative volume distribution percentage of the material reaching 50%. It can be measured using instruments and methods known in the art. For example, it can be conveniently measured using a laser particle size analyzer in accordance with GB / T 19077-2016. The testing instrument can be a Mastersizer 2000E laser particle size analyzer from Malvern Instruments Ltd. in the UK.
[0125] In some embodiments, the morphology of the positive electrode active material may include one or more of spherical single crystals, flaky single crystals, and spherical polycrystals.
[0126] The term "single crystal" also includes quasi-single crystals, which refer to particles composed of several or a dozen crystal grains aggregated together.
[0127] The term "spherical" also includes quasi-spherical, which means that the shape is basically spherical or the aspect ratio is close to 1, for example, the aspect ratio is not greater than 1.3, and optionally not greater than 1.2.
[0128] The morphology of the positive electrode active material can be tested using a scanning electron microscope, for example, according to JY / T010-1996. The testing instrument can be a Sigma 300 scanning electron microscope manufactured by the German ZEISS company.
[0129] In some embodiments, the positive electrode active material may include one or more of an O3 phase, a P2 phase, and a P3 phase.
[0130] In some embodiments, the positive electrode active material includes an O3 phase, and in the peak spectrum of the X-ray diffraction pattern of the positive electrode active material, there are two diffraction peaks in the range of 2θ of 16.0° to 16.7°, the diffraction peak with 2θ between 16.0° and 16.3° is recorded as the first peak, and the diffraction peak with 2θ between 16.3° and 16.7° is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is less than or equal to 0.1:1, and can be optionally less than or equal to 0.076:1.
[0131] The X-ray diffraction pattern of the positive electrode active material is obtained by using an X-ray diffractometer. The test can be carried out under the following conditions: CuK α The ray is the radiation source, and the wavelength of the ray is The scanning 2θ angle range is 10°-70°, and the scanning rate is 4° / min. The testing instrument can be a Brucker D8A_A25 X-ray powder diffractometer from Brucker AxS, Germany.
[0132] The peak spectrum of the X-ray diffraction pattern of the positive electrode active material is obtained by using Topas software and the Rietveld full spectrum fitting refinement method to refine the X-ray diffraction pattern of the positive electrode active material. The 2θ value of 16.0° to 16.7° corresponds to the peak position of the (003) crystal plane of the positive electrode active material.
[0133] The 2θ of the first peak is located between 16.0° and 16.3°, indicating the lattice-distorted O3 phase.
[0134] The 2θ of the second peak is located between 16.3° and 16.7°, indicating the bulk O3 phase.
[0135] The ratio of the peak intensity of the first peak to the peak intensity of the second peak represents the ratio of the content of the lattice-distorted O3 phase to the content of the bulk O3 phase.
[0136] The ratio of the peak intensity of the first peak to the peak intensity of the second peak is the ratio of the integrated area of the first peak to the integrated area of the second peak.
[0137] In the peak spectrum of the X-ray diffraction pattern of the positive electrode active material provided in the embodiment of the present application, the ratio of the peak intensity of the first peak to the peak intensity of the second peak is less than or equal to 0.1:1, indicating that the main structure of the O3 phase of the positive electrode active material provided in the embodiment of the present application is well maintained, and the positive electrode active material contains only a small amount of lattice-distorted O3 phase.
[0138] In some embodiments, the positive electrode active material includes an O3 phase, and the X-ray diffraction pattern of the positive electrode active material includes a (104) crystal plane diffraction peak with 2θ located between 41.5° and 42.5° and a (015) crystal plane diffraction peak with 2θ located between 44.5° and 45.5°, and the ratio of the peak intensity of the (104) crystal plane diffraction peak to the peak intensity of the (015) crystal plane diffraction peak is greater than 10:1.
[0139] The ratio of the peak intensity of the (104) crystal plane diffraction peak to the peak intensity of the (015) crystal plane diffraction peak is the ratio of the integrated area of the (104) crystal plane diffraction peak to the integrated area of the (015) crystal plane diffraction peak.
[0140] In the X-ray diffraction pattern of the positive electrode active material provided in the embodiment of the present application, the ratio of the peak intensity of the (104) crystal plane diffraction peak to the peak intensity of the (015) crystal plane diffraction peak is greater than 10:1, indicating that the layered structure of the positive electrode active material provided in the embodiment of the present application is relatively stable, and is not prone to crystal plane slip or transition metal element aggregation.
[0141] In some embodiments, the interlayer spacing d of the (003) crystal plane of the positive electrode active material is 003 for In this case, the positive electrode active material can have good rate performance and high stability.
[0142] The interlayer spacing d of the (003) crystal plane of the positive electrode active material 003 The interlayer spacing d of the (003) crystal plane can be obtained by measuring the X-ray diffraction pattern using an X-ray diffractometer according to JIS K0131-1996 X-ray diffraction analysis general rules. 003 The test can be carried out under the following conditions: CuK α The ray is the radiation source, and the wavelength of the ray is The scanning 2θ angle range is 10°-70°, and the scanning rate is 4° / min. The testing instrument can be a Brucker D8A_A25 X-ray powder diffractometer from Brucker AxS, Germany.
[0143] In some embodiments, the content of free alkaline substances on the surface of the positive electrode active material may be 0.2-20 wt %, optionally 0.2-15 wt %, 0.2-10 wt %, 0.2-5 wt %, 0.2-2.5 wt %, 0.2-2 wt %, 0.5-1.5 wt %, or 0.5-1.4 wt %. A low content of free alkaline substances on the surface of the positive electrode active material can provide the positive electrode active material with high interfacial stability, thereby improving the cycle performance and / or rate performance of the battery, and also improving the processing performance of the positive electrode slurry and the battery.
[0144] The free alkaline substances on the surface of the positive electrode active material mainly include NaOH and Na2CO3. The content of free alkaline substances can be detected by chemical titration or potentiometric titration. The content of free alkaline substances on the surface of different types of positive electrode active materials varies.
[0145] In some embodiments, the pH of the positive electrode active material may be 11.5-13.5, optionally 11.8-12.6. A lower pH of the positive electrode active material can provide the positive electrode active material with higher interfacial stability, thereby improving the battery's cycle performance and / or rate capability, and also improving the processing performance of the positive electrode slurry and battery.
[0146] The pH of the positive electrode active material is well known in the art and can be measured using instruments and methods known in the art. For example, the test can be performed with reference to GB / T 9724-2007. In some embodiments, the test can be performed as follows: at 25°C, a solution of the positive electrode active material sample and deionized water is prepared in a mass ratio of 1:9. The solution is sealed and stirred on a magnetic stirrer for 30 minutes, then allowed to stand for 90 minutes and filtered. The pH of the filtrate is measured using a pH meter (e.g., pHS-3C), which is the pH of the positive electrode active material.
[0147] [Preparation method]
[0148] The present invention also provides a method for preparing a positive electrode active material, comprising the following steps: providing an initial positive electrode active material, wherein the initial positive electrode active material comprises a sodium-containing layered transition metal oxide; washing the initial positive electrode active material with an alkaline washing solution, wherein the alkaline washing solution comprises K + After washing, the positive electrode active material is obtained by drying.
[0149] The positive electrode active material includes a layered transition metal oxide represented by formula (I), Na x K y M a A b B c O m Qn Formula (I)
[0150] x>0.5, 0<y<0.5, 0<a≤1, 0≤b≤1 / 3, 0≤c≤1 / 3, 1.9≤m≤2, 0≤n≤0.1, M includes one or more of Mn, Fe, Co, Ni, and Cu, A includes one or more metal elements from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, and Group VIB, B includes one or more non-metallic elements from Group IIIA, Group IVA, Group VA, and Group VIA, Q includes one or more non-metallic elements from Group VA and Group VIIA, and the positive electrode active material includes element K, and the content of element K decreases from the particle surface of the positive electrode active material to the particle interior.
[0151] The preparation method provided in the embodiment of the present application comprises K + The sodium-containing layered transition metal oxide is washed with an alkaline washing solution. During the washing process, the free alkaline substances (such as NaOH, Na2CO3, etc.) on the surface of the material will be washed away, so the content of free alkaline substances on the surface of the obtained positive electrode active material is low and the pH is also low. During the washing process, the high concentration of K + Will react with Na in the material + K + / Na + Ion exchange, thereby K + Doped into the material. At the same time, because the washing liquid is alkaline, it contains a lot of OH - , which can also inhibit Na + / H + exchange.
[0152] After a large amount of sodium is removed from the positive electrode active material in the late stage of charging, the stability of the crystal structure becomes poor, and it is easy to undergo irreversible transformation from the layered structure to the rock salt phase structure. + After being introduced into the positive electrode active material, K + It can play a supporting role, stabilize the crystal structure of the positive electrode active material, improve the interface stability, and also improve the stability of the crystal structure, reducing the probability of crystal structure collapse or irreversible transformation after a large amount of sodium is removed from the positive electrode active material in the later stage of charging.
[0153] K + The ionic radius is large (about 0.138nm), which occupies part of the surface of the positive electrode active material. + After the positive electrode active material is positioned, the interlayer spacing of the positive electrode active material can be increased, so that the positive electrode active material can have good rate performance.
[0154] The content of K element in the positive electrode active material shows a decreasing characteristic from the particle surface to the interior of the particle, which can effectively reduce the stress during the battery cycle, thereby reducing the generation of microcracks and enabling the battery using the positive electrode active material to have a long cycle life.
[0155] Therefore, the positive electrode active material obtained by the preparation method of the embodiment of the present application has a lower pH, a lower surface free alkaline substance content, and also has a K element whose content decreases from the particle surface to the interior of the particle. This can not only stabilize the crystal structure of the positive electrode active material, but also enable the positive electrode active material to have good cycle performance and rate performance.
[0156] Sodium-containing layered transition metal oxides are extremely sensitive to moisture, and Na is easily generated during washing with water or acidic solution. + / H + The desodium phenomenon is caused by the exchange of sodium ions and the entry of water into the crystal structure of the material. In addition, after a large amount of sodium ions are released, the sodium-containing layered transition metal oxide will also experience crystal plane slip, which causes significant changes in the material's X-ray diffraction pattern. Taking the O3 phase layered transition metal oxide as an example, after washing with water or acidic solution, the (003) crystal plane diffraction peak in the material's X-ray diffraction pattern tends to shift to lower angles, while the (015) crystal plane diffraction peak is enhanced and the (104) crystal plane diffraction peak is weakened.
[0157] The positive electrode active material obtained by the preparation method provided in the embodiment of the present application has almost no change in its crystal structure compared with the initial positive electrode active material before washing, and the intensity and position of each characteristic peak in the X-ray diffraction pattern of the material also almost do not change. Taking the O3 phase layered transition metal oxide as an example, the positive electrode active material obtained by the preparation method provided in the embodiment of the present application has a ratio of the peak intensity of the (104) crystal plane diffraction peak to the peak intensity of the (015) crystal plane diffraction peak greater than 10:1, and in the peak spectrum of the X-ray diffraction pattern of the positive electrode active material, there are two diffraction peaks in the range of 2θ from 16.0° to 16.7°, the diffraction peak with 2θ between 16.0° and 16.3° is recorded as the first peak, and the diffraction peak with 2θ between 16.3° and 16.7° is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is less than or equal to 0.1:1; at the same time, compared with the X-ray diffraction pattern of the material before washing, the amount of shift of the (003) crystal plane diffraction peak to a low angle is less than or equal to 0.2°.
[0158] In some embodiments, the initial positive electrode active material refers to the positive electrode active material to be washed. The initial positive electrode active material includes a sodium-containing layered transition metal oxide, which can be a material known in the art, and the embodiments of the present application are not limited thereto. The initial positive electrode active material can be prepared by methods known in the art, for example, it can be obtained by solid phase sintering, or it can be commercially available. In some embodiments, the initial positive electrode active material can include Na x1 M a A b B c O m Q n , x1>0.5, other parameters are as defined above and will not be repeated here.
[0159] In some embodiments, the preparation method further comprises the step of: sintering the initial positive electrode active material after washing, to obtain the positive electrode active material.
[0160] Washing will make the surface properties of the material unstable. Sintering can stabilize the surface of the material and make the surface unstable due to washing become stable again, thereby repairing surface defects and reducing vacancies. Sintering can also make the surface K + Stable in Na + position to better play a supporting role, improve rate performance, and reduce the probability of crystal structure collapse or irreversible transformation after a large amount of sodium is removed from the positive electrode active material in the late stage of charging.
[0161] During the washing process, K + It will occupy a large amount of Na in the shallow surface layer through ion exchange + location, but there is still a part of K + The K residue on the surface of the material can be sintered to + Further diffusion into the interior of the particle results in a more gradual decrease in the K content from the particle surface to the interior. Compared to cathode active materials uniformly doped with K, cathode active materials with a decreasing K content can effectively alleviate stress during battery cycling, thereby reducing the generation of microcracks and improving the cycling performance of both the cathode active material and the battery.
[0162] In some embodiments, the sintering temperature may be 200°C-700°C, optionally 300°C-600°C, and more optionally 450°C-550°C.
[0163] In some embodiments, the sintering time may be less than or equal to 20 hours, optionally less than or equal to 10 hours, and more optionally 3 hours to 8 hours, or 3 hours to 5 hours.
[0164] In some embodiments, the sintering atmosphere may be an oxygen-containing atmosphere. Sintering in an oxygen-containing atmosphere can stabilize the surface structure of the material, allowing surface sodium that has become unstable due to washing to re-react with oxygen and become stable, thereby repairing surface defects and reducing vacancies, thereby improving the battery's cycle performance and / or rate performance.
[0165] In some embodiments, the volume fraction of oxygen in the sintering atmosphere may be 15%-40%, 17%-30%.
[0166] In some embodiments, the sintering atmosphere may further contain an inert gas, such as one or more of nitrogen, helium, and argon.
[0167] In some embodiments, the sintering atmosphere may be an air atmosphere, thereby reducing production costs.
[0168] In some embodiments, the morphology of the initial positive active material may include one or more of spherical single crystals, flaky single crystals, and spherical polycrystals.
[0169] K + It can be diffused to a suitable depth by ion exchange and sintering. For spherical single crystals or polycrystalline, its Na + Migration channels can be along all directions, so K + / Na + Ion exchange and K + Diffusion can also occur in all directions, K + Doping will also form in all directions. For a sheet single crystal, the larger plane is the ab plane, and the direction perpendicular to the plane is the c-axis direction. + Migration usually occurs along the ab plane, so K + Doping is usually performed in a direction perpendicular to the c-axis.
[0170] In some embodiments, in the step of washing the initial positive electrode active material with an alkaline washing solution, the washing temperature may be less than or equal to 35°C, and may be 20°C-30°C. When the washing temperature is within the above range, the Na + / H + exchange rate and reduce interlayer sodium dissolution.
[0171] In some embodiments, in the step of washing the initial positive electrode active material with an alkaline washing solution, the washing time may be less than or equal to 60 minutes, optionally less than or equal to 20 minutes, and more optionally 5-20 minutes. When the washing time is within the above range, the Na + / H + Exchange and reduce interlayer sodium dissolution.
[0172] In some embodiments, in the step of washing the initial positive electrode active material with an alkaline washing solution, the pH of the alkaline washing solution may be greater than or equal to 11, optionally greater than or equal to 12, and more optionally 12.5-14, 13-14. When the pH of the alkaline washing solution is within the above range, the Na + / H + Exchange and reduce interlayer sodium dissolution.
[0173] In some embodiments, the solute in the alkaline washing solution may include a soluble potassium salt, for example, including but not limited to one or more of potassium hydroxide, potassium carbonate, and potassium bicarbonate.
[0174] In some embodiments, the solvent in the alkaline washing solution may include one or more of water, alcohol solvents, and ester solvents, and may optionally include water.
[0175] In some embodiments, the solvent in the alkaline cleaning solution may include only water, such as deionized water.
[0176] In some embodiments, the alkaline cleaning solution may also include Na + For example, the solute in the alkaline washing solution may further include a soluble sodium salt, such as but not limited to one or more of sodium hydroxide, sodium carbonate, and sodium bicarbonate.
[0177] When washing with alkaline detergent, part of Na will be washed away, which will cause defects and vacancies on the surface of the material. + , can supplement Na + , improve the capacity; In addition, during the sintering process, the Na + It can also react with oxygen to repair surface defects and reduce vacancies.
[0178] By making the alkaline washing solution include Na + , and further reduce Na + / H + Exchange reduces the dissolution of sodium between layers and enables the positive electrode active material to better maintain its original layered structure.
[0179] In some embodiments, Na + With K + The molar ratio of can be 1:(0.1-1), optionally 1:(0.2-5), and more optionally 1:(0.2-2).
[0180] By adjusting one or more parameters such as sintering temperature, sintering time, alkaline washing solution concentration, washing temperature, washing time, etc. within the above range, the content of K element can be made to decrease from the surface of the positive electrode active material particles to the interior of the particles, and the K element can be prevented from being uniformly distributed in the positive electrode active material; the distribution area of the K element can also be adjusted so that the mass of the K element in the surface area of the positive electrode active material is 50% to 95% of the total mass of the K element in the positive electrode active material, which can be optionally 70% to 95%, 75% to 95%, 80% to 95%, 83% to 95%, 70% to 92%, 75% to 92%, 80% to 92%, 83% to 92%, 70% to 90%, 75% to 90%, 80% to 90%, 83% to 90%.
[0181] In some embodiments, 0.001≤y<0.5, optionally, 0.001≤y≤0.4, 0.001≤y≤0.3, 0.001≤y≤0.2, 0.001≤y≤0.1, 0.001≤y≤0.05, 0.005≤y≤0.05, 0.008≤y≤0.05, 0.012≤y≤0.05. When the content of K element in the positive electrode active material is within the above range, the surface structure of the positive electrode active material can be better stabilized, and the probability of crystal structure collapse or irreversible transformation after a large amount of sodium removal of the positive electrode active material in the late stage of charging can be reduced; at the same time, the positive electrode active material can also have a higher gram capacity and good cycle performance and rate performance. When the content of K element is too much, since K element does not provide capacity, the gram capacity of the positive electrode active material will be reduced, and excessive K + Occupy Na + Position, it will also hinder Na + migration, and affect the battery cycle performance and rate performance.
[0182] In some embodiments, the preparation method of the positive electrode active material comprises the following steps: providing an initial positive electrode active material, wherein the initial positive electrode active material comprises a sodium-containing layered transition metal oxide; washing the initial positive electrode active material with an alkaline washing solution, wherein the alkaline washing solution comprises K + , and the pH of the alkaline washing solution is greater than or equal to 12, and can be optionally 13-14; the initial positive electrode active material after washing is sintered to obtain the positive electrode active material.
[0183] This can further reduce Na + / H + exchange, reduce interlayer sodium dissolution, and stabilize the structure of the positive electrode active material.
[0184] In some embodiments, the preparation method of the positive electrode active material comprises the following steps: providing an initial positive electrode active material, wherein the initial positive electrode active material comprises a sodium-containing layered transition metal oxide; washing the initial positive electrode active material with an alkaline washing solution, wherein the alkaline washing solution comprises K + and Na + , Na + With K + The molar ratio can be 1:(0.1-1), optionally 1:(0.2-2), the pH of the alkaline washing solution is greater than or equal to 12, optionally 13-14, the washing temperature is less than or equal to 35°C, optionally 20°C-30°C, and the washing time is less than or equal to 60min, optionally 5-20min; the initial positive electrode active material after washing is sintered to obtain a positive electrode active material, wherein the sintering temperature is 300°C-600°C, optionally 450°C-550°C, the sintering time is less than or equal to 10h, optionally 3h-8h, the sintering atmosphere is an oxygen-containing atmosphere, and optionally, the volume fraction of oxygen is 15%-40%.
[0185] This can further stabilize the structure of the positive electrode active material, enable the positive electrode active material to better maintain its original layered structure, and also increase the capacity of the positive electrode active material, and enhance the cycle performance and rate performance of the positive electrode active material.
[0186] Unless otherwise specified, all raw materials used in the above preparation methods can be obtained commercially.
[0187] [Positive electrode]
[0188] The embodiment of the present application also provides a positive electrode plate.
[0189] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer arranged on at least one surface of the positive electrode current collector, and the positive electrode film layer includes the positive electrode active material as described above in this application or the positive electrode active material prepared by the preparation method as described above in this application.
[0190] In some embodiments, the content of the positive electrode active material in the positive electrode film layer is 50 wt % to 99 wt %, optionally 85 wt % to 99 wt %, based on the total weight of the positive electrode film layer.
[0191] The positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is arranged on any one or both of the two opposite surfaces of the positive electrode current collector.
[0192] The positive electrode film layer may also include other positive electrode active materials known in the art, such as, but not limited to, one or more of fluorides, sulfides, phosphates, pyrophosphates, metal organic frameworks / metal hexacyanides, and organic compounds. These other positive electrode active materials may be used alone or in combination of two or more. For example, other positive electrode active materials may include NaCoO2, Na 2 / 3 [Cu 1 / 3 Mn 2 / 3 ]O2、Na 2 / 3 [Fe 1 / 3 Mn 2 / 3 ]O2、Na 2 / 3 [Li 1 / 3 Ni 2 / 3 ]O2、Na[Ni 0.5 Co 0.5 ]O2、Na 7 / 9 [Cu 2 / 9 Fe 1 / 9 Mn 2 / 3 ]O2、Na 2 / 3 [Li 1 / 3 Mn 1 / 2 Ti 1 / 6 ]O2、Na[Ni 0.5 Fe 0.5 ]O2、Na[Co 0.5 Fe 0.5 ]O2、Na[Ni 1 / 3 Fe 1 / 3 Mn 1 / 3 ]O2、Na[Cu 1 / 9 Ni 2 / 9 Fe 1 / 3 Mn 1 / 3 ]One or more of O2.
[0193] In some embodiments, the positive electrode film layer may further include a positive electrode conductive agent. The present application does not particularly limit the type of the positive electrode conductive agent. As examples, the positive electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0194] In some embodiments, the positive electrode film layer may further optionally include a positive electrode binder. The present application does not particularly limit the type of positive electrode binder. As an example, the positive electrode binder may include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, fluorinated acrylic resin, styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), carboxymethyl chitosan (CMCS) One or more.
[0195] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. As an example of a metal foil, aluminum foil may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0196] The positive electrode film is typically formed by coating a positive electrode slurry onto a positive electrode current collector, drying it, and cold pressing it. The positive electrode slurry is typically formed by dispersing the positive electrode active material, an optional conductive agent, an optional binder, and any other components in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP).
[0197] [Negative electrode]
[0198] The battery cell includes a negative electrode plate. The structure and composition of the negative electrode plate can be selected according to the type of battery cell, and the embodiments of the present application are not limited thereto.
[0199] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector and comprising a negative electrode active material. For example, the negative electrode current collector may have two opposing surfaces in its thickness direction, and the negative electrode film layer may be disposed on either or both of the two opposing surfaces of the negative electrode current collector.
[0200] The negative electrode active material may be any material known in the art. For example, the negative electrode active material includes but is not limited to one or more of soft carbon, hard carbon, and mesophase microcarbon beads.
[0201] In some embodiments, the negative electrode film layer may further optionally include a negative electrode conductive agent. The present application does not particularly limit the type of the negative electrode conductive agent. As examples, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0202] In some embodiments, the negative electrode film layer may further optionally include a negative electrode binder. The present application does not particularly limit the type of the negative electrode binder. As examples, the negative electrode binder may include one or more of styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, water-based acrylic resin (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0203] In some embodiments, the negative electrode film layer may further include other additives. For example, the other additives may include a thickener, such as sodium carboxymethyl cellulose (CMC), a PTC thermistor material, and the like.
[0204] The negative electrode film layer is typically formed by coating the negative electrode slurry onto the negative electrode current collector, drying it, and cold pressing it. The negative electrode slurry is typically formed by dispersing the negative electrode active material, an optional conductive agent, an optional binder, and other optional additives in a solvent and stirring them uniformly. The solvent can be, but is not limited to, N-methylpyrrolidone (NMP) or deionized water.
[0205] The negative electrode plate does not exclude other additional functional layers in addition to the negative electrode film layer. For example, in some embodiments, the negative electrode plate may further include a conductive primer layer (e.g., composed of a conductive agent and a binder) disposed on the surface of the negative electrode current collector and sandwiched between the negative electrode current collector and the negative electrode film layer; in some embodiments, the negative electrode plate may further include a protective layer covering the surface of the negative electrode film layer.
[0206] In some embodiments, the negative electrode sheet may include a negative electrode current collector and a metal layer disposed on at least one surface of the negative electrode current collector. The metal material in the metal layer may include one or more of sodium element and sodium alloy.
[0207] The sodium alloy may be an alloy of metallic sodium and other metallic elements or non-metallic elements. For example, the other metallic elements in the sodium alloy may include one or more of tin, zinc, aluminum, magnesium, silver, gold, gallium, indium, and platinum, and the non-metallic elements in the sodium alloy may include one or more of boron, carbon, and silicon.
[0208] In some embodiments, the negative electrode sheet may be a sodium sheet (foil) or a sodium alloy sheet (foil).
[0209] In some embodiments, the negative electrode sheet may include a negative electrode current collector to assemble into a negative electrode-free sodium metal battery cell.
[0210] In some embodiments, the negative electrode current collector may include a metal foil, a three-dimensional porous current collector, or a composite current collector. As examples of metal foils, copper foil, copper alloy foil, nickel foil, nickel alloy foil, aluminum foil, and aluminum alloy foil may be used. As examples of three-dimensional porous current collectors, copper mesh, nickel mesh, foam copper, foam nickel, and foam aluminum may be used. The composite current collector may include a polymer material base layer and a metal material layer formed on at least one surface of the polymer material base layer. As an example, the metal material may include one or more of copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, aluminum, aluminum alloy, silver, and silver alloy. As an example, the polymer material base layer may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0211] [Electrolytes]
[0212] The battery cell includes an electrolyte. This application does not specifically limit the type of electrolyte, and the electrolyte can be selected according to needs. For example, the electrolyte can include one or more selected from solid electrolytes and liquid electrolytes (i.e., electrolytes).
[0213] In some embodiments, the electrolyte is an electrolyte solution including an electrolyte salt and a solvent.
[0214] The type of electrolyte salt is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the electrolyte salt can include one or more of NaPF6, NaClO4, NaBCl4, NaSO3CF3, and Na(CH3)C6H4SO3.
[0215] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, the solvent may include one or more of an ester solvent, a sulfone solvent, and an ether solvent. As an example, the solvent may include but is not limited to ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE). One or more.
[0216] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, or additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.
[0217] [Isolation film]
[0218] Battery cells using electrolytes, as well as some battery cells using solid electrolytes, also include a separator. The separator is placed between the positive and negative electrode sheets to prevent internal short circuits.
[0219] The present application has no particular limitation on the type of isolation membrane, and any known isolation membrane with a porous structure having good chemical stability and mechanical stability can be selected.
[0220] In some embodiments, the material of the isolation membrane may include one or more of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The isolation membrane may be a single-layer film or a multi-layer composite film. When the isolation membrane is a multi-layer composite film, the materials of each layer may be the same or different.
[0221] The preparation method of battery cells is well known. In some embodiments, the positive electrode sheet, separator, negative electrode sheet and electrolyte can be assembled to form a battery cell. As an example, the positive electrode sheet, separator, and negative electrode sheet can be formed into an electrode assembly through a winding process and / or a lamination process, and the electrode assembly is placed in an outer package, dried and injected with the above-mentioned electrolyte, and then subjected to packaging, standing, formation and other processes to obtain a battery cell. Multiple battery cells can also be further connected in series, in parallel or in a mixed connection to form a battery module. Multiple battery modules can also be connected in series, in parallel or in a mixed connection to form a battery pack. In some embodiments, multiple battery cells can also directly form a battery pack.
[0222] Electrical devices
[0223] The present application also provides an electrical device, which includes a battery provided in the present application. The battery can be used as a power source for the electrical device or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, a mobile device (such as a mobile phone, a tablet computer, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship, a satellite, an energy storage system, etc.
[0224] The electrical device can select a specific type of battery, such as a battery cell, a battery module, or a battery pack, according to its usage requirements.
[0225] Figure 6 is a schematic diagram of an exemplary electric device. This device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of this device, a battery pack or battery module may be used.
[0226] As another example, an electric device may be a mobile phone, a tablet computer, a laptop computer, etc. Such an electric device is usually required to be lightweight and thin, and may use a battery cell as a power source.
[0227] Example
[0228] The following examples describe the present disclosure in more detail. These examples are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by mass, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing. The instruments used in the examples are commercially available.
[0229] Comparative Example 1
[0230] A total of 30 g of Na2CO3, Mn2O3, Fe2O3, and NiO were weighed according to the molar ratio of Na:Mn:Fe:Ni of 1:0.4:0.3:0.3. The obtained sample was pre-ground in an agate mortar and added to a planetary ball mill for 1 hour to obtain a precursor mixture. The obtained precursor mixture was evenly placed in an open crucible, and then heated from 25°C to 950°C in a muffle furnace at a heating rate of 5°C / min, and kept at a constant temperature of 950°C for 15 hours. The atmosphere used was dehumidified and decarbonized air. After completion, the temperature was naturally lowered to obtain unmodified NaNi 0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides.
[0231] Comparative Example 2
[0232] A total of 30 g of Na2CO3, Mn2O3, Fe2O3, and NiO were weighed according to a molar ratio of Na:Mn:Fe:Ni of 1:0.4:0.3:0.3, and then KNO3 (based on the mass of K element being 0.44 wt%) was added; the obtained sample was pre-ground in an agate mortar and then added to a planetary ball mill for 1 hour to obtain a precursor mixture; the obtained precursor mixture was evenly placed in an open crucible, and then heated from 25°C to 950°C in a muffle furnace at a heating rate of 5°C / min, and maintained at a constant temperature of 950°C for 15 hours in an atmosphere of dehumidified and carbon dioxide-free air; after completion, the temperature was naturally lowered to obtain K + Uniformly doped NaNi 0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides.
[0233] Comparative Example 3
[0234] 10g of layered transition metal oxide was added to 10ml of deionized water and stirred at 400 rpm in a magnetic stirrer at 25°C for 5 minutes. The mixture was then filtered. The resulting solid was dried in a vacuum oven at 120°C for 12 hours. The dried powder was placed in a muffle furnace and heated at a rate of 5°C / min to 500°C. The temperature was maintained at this temperature for 5 hours in an air atmosphere. After completion, the mixture was allowed to cool naturally to obtain the positive electrode active material.
[0235] Comparative Example 4
[0236] NaOH was prepared into an alkaline washing solution with a concentration of 1 mol / L, and the solvent was deionized water. The unmodified NaNi prepared in Comparative Example 1 was taken according to a solid-liquid ratio of 1:1. 0.3 Fe 0.3 Mn 0.410g of O2 layered transition metal oxide and 10ml of alkaline washing solution were added to 10ml of the alkaline washing solution and stirred at 400rpm in a magnetic stirrer at 25°C for 5 minutes. The mixture was then filtered. The solid obtained by filtration was dried in a vacuum oven at 120°C for 12 hours. The dried powder was placed in a muffle furnace and heated at a rate of 5°C / min to 500°C. The temperature was maintained at this temperature for 5 hours in an air atmosphere. After completion, the temperature was naturally cooled to obtain the positive electrode active material.
[0237] Example 1
[0238] (1) NaOH and KOH were mixed according to Na + / K + The alkaline washing solution is prepared with a molar ratio of 1:0.5 to a total concentration of 1 mol / L, and the solvent is deionized water.
[0239] (2) According to the solid-liquid ratio of 1:1, the unmodified NaNi prepared in Comparative Example 1 was taken. 0.3 Fe 0.3 Mn 0.4 10 g of O2 layered transition metal oxide and 10 ml of alkaline washing solution: add 10 g of layered transition metal oxide to 10 ml of alkaline washing solution, stir at 400 rpm at 25 ° C for 5 minutes in a magnetic stirrer, and then filter.
[0240] (3) The solid obtained by filtration was placed in a vacuum oven at 120°C and dried for 12 h.
[0241] (4) The dried powder was placed in a muffle furnace, heated to 500°C at a heating rate of 5°C / min, and maintained at a constant temperature for 5 h. The atmosphere used was air.
[0242] (5) After the end, the temperature is naturally cooled and the surface K + Doped positive electrode active material.
[0243] Example 2
[0244] A total of 30 g of Na2CO3, Mn2O3, Fe2O3, and NiO were weighed according to the molar ratio of Na:Mn:Fe:Ni of 1:0.4:0.3:0.3. The obtained sample was pre-ground in an agate mortar and added to a planetary ball mill for 1 hour to obtain a precursor mixture. The obtained precursor mixture was evenly placed in an open crucible, and then heated from 25°C to 900°C in a muffle furnace at a heating rate of 5°C / min, and maintained at a constant temperature of 900°C for 15 hours. The atmosphere used was dehumidified and decarbonized air. After completion, the temperature was naturally lowered to obtain unmodified NaNi 0.3 Fe 0.3 Mn0.4 O2 layered transition metal oxides.
[0245] Then, the unmodified NaNi 0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides are washed and the surface K + Doped positive electrode active material.
[0246] Example 3
[0247] A total of 30 g of Na2CO3, Mn2O3, Fe2O3, and NiO were weighed according to the molar ratio of Na:Mn:Fe:Ni of 1:0.4:0.3:0.3. The obtained sample was pre-ground in an agate mortar and added to a planetary ball mill for 1 hour to obtain a precursor mixture. The obtained precursor mixture was evenly placed in an open crucible, and then heated from 25°C to 970°C in a muffle furnace at a heating rate of 5°C / min, and maintained at a constant temperature of 970°C for 20 hours. The atmosphere used was dehumidified and carbon dioxide-free air. After completion, the temperature was naturally lowered to obtain unmodified NaNi 0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides.
[0248] Then, the unmodified NaNi 0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides are washed and the surface K + Doped positive electrode active material.
[0249] Example 4
[0250] Na2CO3 and spherical precursor Ni 0.3 Fe 0.3 Mn 0.4 (OH)2 was weighed in a total of 30 g of sample at a molar ratio of 0.5:1. The obtained sample was mixed by a high-speed mixer for 1 hour to obtain a precursor mixture. The obtained precursor mixture was evenly placed in an open crucible, and then heated from 25 ° C to 900 ° C in a muffle furnace at a heating rate of 5 ° C / min, and kept at a constant temperature of 900 ° C for 15 hours. The atmosphere used was dehumidified and decarbonized air. After the end, the temperature was naturally cooled to obtain unmodified NaNi 0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides.
[0251] Then, the unmodified NaNi0.3 Fe 0.3 Mn 0.4 O2 layered transition metal oxides are washed and the surface K + Doped positive electrode active material.
[0252] Example 5
[0253] The preparation process of the positive electrode active material is the same as that of Example 1, except that the alkaline washing solution in step (1) is a 1 mol / L KOH solution.
[0254] Examples 6 to 9
[0255] In addition to the Na in the alkaline washing solution in step (1), + / K + Except for the different molar ratios, the preparation process of the positive electrode active material is the same as that of Example 1. Specific parameters are shown in Table 1.
[0256] Examples 10 to 12
[0257] Except for the different concentration and pH of the alkaline washing solution in step (2), the preparation process of the positive electrode active material is the same as that of Example 1. Specific parameters are shown in Table 1.
[0258] Examples 13 to 14
[0259] Except for the washing temperature in step (2), the preparation process of the positive electrode active material is the same as that in Example 1. Specific parameters are shown in Table 1.
[0260] Examples 15 to 17
[0261] Except for the washing time in step (2), the preparation process of the positive electrode active material is the same as that in Example 1. Specific parameters are shown in Table 1.
[0262] Examples 18 to 21
[0263] Except for the different sintering temperature in step (2), the preparation process of the positive electrode active material is the same as that of Example 1. Specific parameters are shown in Table 1.
[0264] Examples 22 to 25
[0265] Except for the different sintering time in step (2), the preparation process of the positive electrode active material is the same as that in Example 1. Specific parameters are shown in Table 1.
[0266] Test section
[0267] (1) Test of the content of free alkaline substances on the surface of positive electrode active materials
[0268] Weigh 20.000 g of the positive electrode active material prepared above, add it to 100 mL of deionized water, stir for 30 minutes, and filter; transfer 60 mL of the filtrate to a 250 mL conical flask, add 10 drops of indicator (methyl orange and phenolphthalein) and shake well. At this time, the solution turns purple; then titrate with 0.1103 mol / L hydrochloric acid as a standard solution to calculate the content of free alkaline substances (NaOH, Na2CO3) in the sample.
[0269] (2) X-ray diffraction analysis test of positive electrode active materials
[0270] The positive electrode active material prepared above was analyzed by X-ray powder diffractometer. The test can be carried out under the following conditions: CuK α The ray is the radiation source, and the wavelength of the ray is The scanning 2θ angle range is 10°-70°, and the scanning rate is 4° / min. The testing instrument can be a Brucker D8A_A25 X-ray powder diffractometer from Brucker AxS, Germany.
[0271] The peak spectrum of the X-ray diffraction pattern of the positive electrode active material is obtained by using Topas software and the Rietveld full spectrum fitting refinement method to refine the X-ray diffraction pattern of the positive electrode active material. The 2θ value of 16.0° to 16.7° corresponds to the peak position of the (003) crystal plane of the positive electrode active material.
[0272] The first peak has a 2θ value between 16.0° and 16.3°, indicating a distorted O3 phase. The second peak has a 2θ value between 16.3° and 16.7°, indicating a bulk O3 phase. The ratio of the peak intensity of the first peak to the peak intensity of the second peak is the ratio of the integrated area of the first peak to the integrated area of the second peak.
[0273] The 2θ of the (104) crystal plane diffraction peak is between 41.5° and 42.5°, and the 2θ of the (015) crystal plane diffraction peak is between 44.5° and 45.5°. The peak intensity of the (104) crystal plane diffraction peak I (104) The peak intensity of the (015) crystal plane diffraction peak I (015) The ratio I (104) :I (015) It is the ratio of the integrated area of the (104) crystal plane diffraction peak to the integrated area of the (015) crystal plane diffraction peak.
[0274] (3) Element content test of positive electrode active material
[0275] The cross-section of the positive electrode active material is prepared using a cross-section polisher (for example, the IB-09010CP argon ion cross-section polisher from JEOL, Japan). The cross-section image passes through the center of the positive electrode active material particle. The "particle center" refers to the range within a radius of 0.1 μm extending from the geometric center of the particle to the surface of the particle.
[0276] With reference to JY / T010-1996, a scanning electron microscope (e.g., a Sigma 300 scanning electron microscope from ZEISS, Germany) is used to scan a cross section of the positive electrode active material; inductively coupled plasma emission spectroscopy (ICP) is then used to detect the elemental composition of the positive electrode active material, and the molar content x of the sodium element and the molar content y of the potassium element are calculated.
[0277] The ratio of the mass of the K element in the surface area of the cross-sectional image of the positive electrode active material (the area extending 0.05L inward from the edge of the particle in the cross-sectional image, where L refers to the long axis length of the positive electrode active material particle, that is, the maximum value when the line connecting two points on the particle surface passes through the geometric center of the particle) to the mass of all K elements in the cross-sectional image of the positive electrode active material is taken as the ratio of the mass of the K element in the surface area of the positive electrode active material to the total mass of the K element in the positive electrode active material.
[0278] (4) First charge capacity and cycle performance test
[0279] The prepared positive electrode active material, conductive agent carbon black Super P, and binder polyvinylidene fluoride (PVDF) were ground and mixed uniformly in a weight ratio of 80:15:5. An appropriate amount of solvent N-methylpyrrolidone (NMP) was added and stirred to obtain a positive electrode slurry. The positive electrode slurry was evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and slit to obtain the positive electrode sheet.
[0280] Ethylene carbonate (EC) and diethyl carbonate (DEC) were mixed in equal volumes to obtain an organic solvent, and then NaClO4 was dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0281] The positive electrode sheet, separator (polypropylene film with a thickness of 12 μm), and sodium metal sheet prepared above are cut into discs of appropriate size and stacked in order, so that the separator is placed between the positive electrode sheet and the sodium metal sheet to play an isolating role. The separator is soaked with the above-mentioned electrolyte, and then compacted to obtain a button battery.
[0282] At 25°C, the button battery was charged to 4.2V at a current density of 10 mA / g to obtain the initial charge capacity of the button battery; and then discharged to 1.5V at a current density of 10 mA / g to obtain the initial discharge capacity of the button battery.
[0283] The first charge gram capacity of the positive electrode active material (mAh / g) = the first charge capacity of the button cell / the mass of the positive electrode active material.
[0284] At 25°C, the button cell was charged at a constant current density of 100 mA / g to 4.2 V, and then discharged at a constant current density of 100 mA / g to 1.5 V to obtain the first-cycle discharge capacity of the button cell. The button cell was subjected to cyclic charge and discharge testing according to the above method, and the discharge capacity after each cycle was recorded. The capacity retention rate of the button cell after 200 cycles = the discharge capacity of the button cell after 200 cycles / the first-cycle discharge capacity of the button cell.
[0285] (5)Na + Diffusion coefficient test
[0286] At 25°C, charge the button cell at a constant current of 0.1C to 4.2V, then discharge it at a constant current of 0.1C to 1.5V. Then charge the button cell at a constant current of 1C to 4.2V, then charge it at a constant voltage until the current is less than or equal to 0.05C. After standing for 6 hours, perform an electrochemical impedance spectroscopy (EIS) test using an electrochemical workstation. Then, use fitting software (such as Zview) to fit the impedance of the high-frequency, medium-frequency, and low-frequency regions of the electrochemical impedance spectrum according to the equivalent circuit curve fitting method. The test frequency can be 100kHz-0.01Hz, the voltage amplitude can be set to 10mV, and the electrochemical workstation can be a German Zahner electrochemical workstation.
[0287] According to the fitted electrochemical impedance spectrum and formula Z ′ =R s +R ct +σw -1 / 2 The Warburg coefficient σ (corresponding to the slope of the low-frequency region) can be obtained. ct represents the charge transfer resistance, R s Represents resistance in ohms.
[0288] Na + Diffusion coefficient D Na+ =(R 2 T 2 ) / (2A 2 n 4 F 4 C 2 σ 2 R is the gas constant, which is 8.314 J / (mol·K); T is 298 K; A is the area of the electrode, in cm 2 ; n is the number of electrons transferred during the reaction; F is the Faraday constant, which is 96500C / mol; C is the bulk concentration of sodium ions, in mol / cm3 , C=ρ / M, ρ is the density of the positive electrode film layer, unit is g / cm 3 , M is the molar mass of the positive electrode active material, the unit is g / mol.
[0289] Na + The higher the diffusion coefficient, the faster the solid-phase diffusion rate of sodium ions in the positive electrode active material and the better the rate performance.
[0290] The test results are shown in Table 2.
[0291] Comparative Example 1 is a positive electrode active material without any surface modification. From the test results in Table 2, it can be seen that the surface of the positive electrode active material contains a large amount of free alkaline substances, and the capacity of the positive electrode active material is low, the solid phase diffusion rate of sodium ions is slow, and the cycle stability is poor, thereby affecting the energy density, cycle performance and rate performance of the battery.
[0292] The positive electrode active material prepared in Comparative Example 2 is a positive electrode active material uniformly doped with K ions. From the test results in Table 2, it can be seen that after the K ions are uniformly doped in the bulk phase, there are still a large number of free alkaline substances on the surface of the positive electrode active material, and the capacity of the positive electrode active material is low, the solid phase diffusion rate of sodium ions is slow, and the cycle stability is poor, which will affect the energy density, cycle performance and rate performance of the battery.
[0293] The positive electrode active material of Comparative Example 3 was obtained by washing the positive electrode active material of Comparative Example 1 with water. From the test results in Table 2, it can be seen that although the content of free alkaline substances on the surface of the positive electrode active material is reduced, the sodium content of the positive electrode active material itself is also significantly reduced (x decreases significantly), and the capacity of the positive electrode active material is low, the solid phase diffusion rate of sodium ions is slow, and the cycle stability is poor, thereby affecting the energy density, cycle performance and rate performance of the battery.
[0294] From the test results of Examples 1-25 and Comparative Examples 1 and 3, it can be seen that the use of + By washing with an alkaline detergent and sintering, a positive electrode active material with a decreasing K content from the particle surface to the particle interior can be obtained. The test results in Table 2 show that the positive electrode active materials prepared in Examples 1-25 have a low free alkaline substance content, a high capacity, a high sodium ion solid-phase diffusion rate, and high cycling stability, thereby enabling batteries with high energy density and good cycling and rate performance.
[0295] Figure 7 is an X-ray diffraction pattern of the positive electrode active materials prepared in Example 1, Comparative Example 1 and Comparative Example 3. Figure 8 is a cycle curve diagram of the button batteries prepared in Example 1, Comparative Example 1 and Comparative Example 3.
[0296] As shown in Figure 7, compared with the positive electrode active material prepared in Comparative Example 1, the (003) crystal plane diffraction peak of the positive electrode active material obtained by water washing in Comparative Example 3 has a significant shift to a lower angle, and the 2θ of the (003) crystal plane diffraction peak of the positive electrode active material after water washing is less than 16.3°, indicating that the water washing process will destroy the layered structure of the positive electrode active material. Further combined with the test results in Table 2, it can be seen that after water washing, the O3 phase of the positive electrode active material is almost completely transformed into an O3 phase with lattice distortion. Example 1 uses a K-containing + The positive electrode active material prepared in Comparative Example 1 was washed and sintered with an alkaline washing solution. Compared to the positive electrode active material in Comparative Example 1, the resulting positive electrode active material exhibited a smaller shift in the (003) crystal plane diffraction peak toward lower angles. Furthermore, the 2θ value of the (003) crystal plane diffraction peak after washing was greater than 16.3°, indicating that the O3 phase structure of the positive electrode active material remained well-maintained after washing. Further, in conjunction with the test results in Table 2, it can be seen that the positive electrode active material prepared in Example 1 contained a small amount of lattice-distorted O3 phase.
[0297] It can also be seen from Figure 7 and Table 2 that compared with the positive electrode active material prepared in Comparative Example 1, the positive electrode active material obtained by water washing in Comparative Example 3 has an enhanced (015) crystal plane diffraction peak and a weakened (104) crystal plane diffraction peak. (104) / I (015) Example 1 uses a K + The positive electrode active material prepared in Comparative Example 1 was washed and sintered with an alkaline washing solution. The positive electrode active material thus obtained had almost no change in the intensity and position of each characteristic peak in the X-ray diffraction pattern compared with the positive electrode active material of Comparative Example 1.
[0298] As shown in FIG8 , the positive electrode active material prepared in Example 1 has high cycle stability and can improve the cycle performance of the battery.
[0299] The positive electrode active material of Comparative Example 4 was obtained by washing the positive electrode active material of Comparative Example 1 with an aqueous NaOH solution. From the test results in Table 2, it can be seen that although the content of free alkaline substances on the surface of the positive electrode active material is reduced, the crystal structure stability of the positive electrode active material is poor, and it is easy to undergo irreversible transformation from a layered structure to a rock salt phase structure, thereby resulting in poor cycle stability of the positive electrode active material during long-term charge and discharge of the battery. At the same time, the solid phase diffusion rate of sodium ions in the positive electrode active material is slow, which in turn leads to poor cycle performance and rate performance of the battery.
[0300] The test results of Examples 1-4 also show that the particle morphology and / or particle size of the positive electrode active materials are different, and the performance of the positive electrode active materials obtained after the same washing process and sintering process are slightly different, and the obtained positive electrode active materials all have good performance.
[0301] It can also be seen from the test results of Examples 1 and 5-9 that when the alkaline detergent contains Na + and K + When the cathode active material and the battery performance are further improved.
[0302] It can also be seen from the test results of Examples 1 and 10-12 that the performance of the positive electrode active material and the battery can be further improved by further adjusting the pH of the alkaline detergent.
[0303] It can also be seen from the test results of Examples 1 and 13-25 that the performance of the positive electrode active material and the battery can be further improved by further adjusting parameters such as washing temperature, washing time, sintering temperature, and sintering time.
[0304] It can also be seen from the test results of Examples 1-25 that by further adjusting the mass ratio of the K element in the surface region of the positive electrode active material, the performance of the positive electrode active material and the battery can be further improved.
[0305] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and any embodiments having substantially the same structure and effect as the technical concept within the scope of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the present application, any other embodiments that can be conceived by those skilled in the art and that combine some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A positive electrode active material comprising a layered transition metal oxide represented by formula (I), Na x K y M a A b B c O m Q n Formula (I) x>0.5, 0<y<0.5, 0<a≤1, 0≤b≤1 / 3, 0≤c≤1 / 3, 1.9≤m≤2, 0≤n≤0.1, M includes one or more of Mn, Fe, Co, Ni, Cu, A includes one or more metal elements of Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, Group VIB, B includes one or more non-metal elements of Group IIIA, Group IVA, Group VA, Group VIA, Q includes one or more non-metal elements of Group VA and Group VIIA, The positive electrode active material includes K element, and the content of K element decreases from the particle surface of the positive electrode active material to the particle interior.
2. The positive electrode active material according to claim 1, wherein The area formed by extending a distance of 0.05L from the particle surface of the positive electrode active material to the interior of the particle is recorded as the surface area of the positive electrode active material, L refers to the major axis length of the positive electrode active material particle, and the mass of the K element in the surface area of the positive electrode active material is 50% to 95% of the total mass of the K element in the positive electrode active material, and can be optionally 70% to 90%.
3. The positive electrode active material according to claim 1 or 2, wherein The positive electrode active material includes one or more of an O3 phase, a P2 phase, and a P3 phase.
4. The positive electrode active material according to any one of claims 1 to 3, wherein The positive electrode active material includes an O3 phase, and in the peak spectrum of the X-ray diffraction spectrum of the positive electrode active material, there are two diffraction peaks in the range of 2θ of 16.0° to 16.7°, the diffraction peak with 2θ between 16.0° and 16.3° is recorded as the first peak, and the diffraction peak with 2θ between 16.3° and 16.7° is recorded as the second peak, and the ratio of the peak intensity of the first peak to the peak intensity of the second peak is less than or equal to 0.1:1, and can be optionally less than or equal to 0.076:
1.
5. The positive electrode active material according to any one of claims 1 to 4, wherein The positive electrode active material includes an O3 phase, and the X-ray diffraction spectrum of the positive electrode active material includes a (104) crystal plane diffraction peak with 2θ located between 41.5° and 42.5° and a (015) crystal plane diffraction peak with 2θ located between 44.5° and 45.5°, and the ratio of the peak intensity of the (104) crystal plane diffraction peak to the peak intensity of the (015) crystal plane diffraction peak is greater than 10:
1.
6. The positive electrode active material according to any one of claims 1 to 5, wherein A includes one or more elements selected from the group consisting of Li, Ti, Zr, Sb, Nb, Mg, Ca, Mo, Zn, Cr, W, Bi, Sn, Ge, Al, Ba, Sr, and V; and / or B includes one or more elements selected from Si, P, B, S, and Se; and / or, Q includes one or more elements of F, Cl, and N; and / or, x ≥ 2 / 3; and / or, 0.012≤y≤0.05; and / or, 0≤b≤1 / 3, 0≤c≤1 / 3, and 0<b+c≤1 / 3.
7. The positive electrode active material according to claim 6, wherein The positive electrode active material includes a layered transition metal oxide represented by formula (I-1), Na x K y Mn p Fe q M′ a-p-q A b B c O m Q n Formula (I-1) 0<p<1, 0<q<1, apq≥0, M includes one or more elements of Co, Ni, and Cu; Optionally, 0<p≤2 / 3; Optionally, 0<q≤1 / 3; Optionally, 0<apq≤1 / 3.
8. The positive electrode active material according to any one of claims 1 to 7, wherein The content of free alkaline substances on the surface of the positive electrode active material is 0.2-20wt%, and can be 0.5-1.4wt%; and / or, The pH of the positive electrode active material is 11.5-13.5, and can be 11.8-12.
6.
9. The positive electrode active material according to any one of claims 1 to 8, wherein The morphology of the positive electrode active material includes one or more of spherical single crystals, flaky single crystals, and spherical polycrystals; and / or, The volume distribution particle size Dv50 of the positive electrode active material is 3-15 μm, and can be 4-9 μm.
10. A method for preparing a positive electrode active material, comprising the following steps: Providing an initial positive electrode active material, the initial positive electrode active material comprising a sodium-containing layered transition metal oxide; The initial positive electrode active material is washed with an alkaline washing solution, wherein: The alkaline washing solution includes K + ; After washing, the positive electrode active material is obtained by drying, wherein the positive electrode active material comprises a layered transition metal oxide represented by formula (I), Na x K y M a A b B c O m Q n Formula (I) x>0.5, 0<y<0.5, 0<a≤1, 0≤b≤1 / 3, 0≤c≤1 / 3, 1.9≤m≤2, 0≤n≤0.1, M includes one or more of Mn, Fe, Co, Ni, and Cu, A includes one or more metal elements from Group IA, Group IIA, Group IIIA, Group IVA, Group VA, Group IIB, Group IVB, Group VB, and Group VIB, B includes one or more non-metal elements from Group IIIA, Group IVA, Group VA, and Group VIA, Q includes one or more non-metal elements from Group VA and Group VIIA, and the positive electrode active material includes K element, and the content of K element decreases from the particle surface of the positive electrode active material to the particle interior.
11. The preparation method according to claim 10, wherein: In the step of washing the initial positive electrode active material with an alkaline washing solution, The washing temperature is less than or equal to 35°C, and can be 20°C-30°C; and / or, The washing time is less than or equal to 60 minutes, and can be 5-20 minutes; and / or, The pH of the alkaline washing solution is greater than or equal to 12, and can be optionally 13-14.
12. The preparation method according to claim 10 or 11, wherein: The solute in the alkaline washing solution includes one or more of potassium hydroxide, potassium carbonate and potassium bicarbonate; and / or, The solvent in the alkaline washing solution includes one or more of water, alcohol solvents, and ester solvents, and may optionally include water.
13. The preparation method according to any one of claims 10 to 12, wherein: The alkaline washing solution also includes Na + , Optionally, Na + With K + The molar ratio is 1:(0.1-10), and can be optionally 1:(0.2-2).
14. The preparation method according to any one of claims 10 to 13, wherein: The preparation method further comprises the steps of: sintering the initial positive electrode active material after washing to obtain the positive electrode active material; Optionally, the sintering temperature is 300° C.-600° C., optionally 450° C.-550° C.; and / or, Optionally, the sintering time is less than or equal to 10 hours, and may be 3 hours to 8 hours; and / or, Optionally, the sintering atmosphere is an oxygen-containing atmosphere. More preferably, the volume fraction of oxygen in the sintering atmosphere is 15%-40%.
15. A positive electrode sheet, comprising a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein: The positive electrode film layer comprises the positive electrode active material according to any one of claims 1 to 9 or the positive electrode active material prepared by the preparation method according to any one of claims 10 to 14, Optionally, the content of the positive electrode active material in the positive electrode film layer is 50 wt % to 99 wt %, more preferably 85 wt % to 99 wt %, based on the total weight of the positive electrode film layer.
16. A battery comprising the positive electrode sheet according to claim 15.
17. An electrical device comprising the battery according to claim 16.
Citation Information
Patent Citations
Composite cathode active material, cathode and lithium battery each including the same, and method of preparing composite cathode active material
CN111106328A
Positive electrode active material, preparation method thereof and sodium ion battery
CN111554919A
Positive pole piece for secondary battery, secondary battery, battery module, battery pack and device
CN114256443A
Positive electrode active material, positive electrode plate and sodium ion battery
CN115472819A
Positive electrode active material for nonaqueous electrolyte secondary battery, manufacturing method of the positive electrode active material, positive electrode including the positive electrode active material, and battery including the positive electrode
JP2012033463A
Cited By
Method for detecting residual alkali in sodium ion layered oxide positive electrode material
CN119827700A