Perovskite cell and preparation method therefor, electrode for perovskite cell, and photovoltaic module and electric device
By using a non-metallic material with a Fermi energy level of 4-5.5eV and a metal oxide electrode in the second electrode of the perovskite battery, combined with a close-contact conductive film layer structure, the stability and photoelectricity of the perovskite battery are solved. The issue of conversion efficiency achieves high stability and high efficiency photoelectric conversion.
Patent Information
- Application Number
- PCT/CN2023/095126
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-21
AI Technical Summary
While improving the photoelectric conversion efficiency, existing perovskite batteries are insufficient in stability and are susceptible to the migration and erosion of halogen ions inside perovskite materials.
The second electrode of the perovskite battery is introduced with a non-metallic material of Fermi energy level of 4-5.5 eV, and the second conductive film layer is combined with the metal or metal oxide electrode, through the first conductive film layer and the second conductive film layer. The close contact of the membrane layer improves the tolerance of perovskite batteries to halogen ions and the photoelectric conversion efficiency.
It significantly improves the stability and photoelectric conversion efficiency of perovskite batteries, enhances its resistance to halogen ions, and extends the service life of the battery.
Smart Images

Figure CN2023095126_21112024_PF_FP_ABST
Abstract
Description
Perovskite battery and preparation method thereof, electrode for perovskite battery, photovoltaic module, and electrical device Technical Field
[0001] The present application relates to a perovskite battery and a preparation method thereof, electrodes for the perovskite battery, a photovoltaic module, and an electrical device. Background Art
[0002] With the development of modern industry, global energy shortages and environmental pollution are becoming increasingly prominent. Perovskite cells, as an ideal renewable energy source, are gaining increasing attention. Perovskite cells utilize perovskite materials as a light-absorbing layer. Researchers are striving to improve both the photoelectric conversion efficiency and stability of perovskite cells. The above statements are intended only to provide background information related to this application and do not necessarily constitute prior art.
[0003] Summary of the Invention
[0004] The present application provides a perovskite cell and a preparation method thereof, an electrode for the perovskite cell, a photovoltaic module, and an electrical device, which can enable the perovskite cell to have high stability and high photoelectric conversion efficiency.
[0005] In a first aspect, the present application provides a perovskite cell, comprising a first electrode, a second electrode, a light absorbing layer, a first charge transport layer, and a second charge transport layer, wherein the light absorbing layer is located between the first electrode and the second electrode, the first charge transport layer is located between the first electrode and the light absorbing layer, and the second charge transport layer is located between the second electrode and the light absorbing layer, wherein the second electrode comprises a first conductive film layer and a second conductive film layer, and the first conductive film layer is arranged close to the second charge transport layer; the electrode material of the first conductive film layer comprises one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and the first metal, and the Fermi level of the non-metal is 4-5.5 eV; the electrode material of the second conductive film layer comprises one or more of a second metal and a second transparent conductive metal oxide.
[0006] By introducing a non-metal with a Fermi level of 4-5.5 eV into the first conductive film layer of the second electrode, the perovskite cell device's tolerance to halogen ions can be increased, thereby enhancing the stability of the perovskite cell device. Furthermore, since the second conductive film layer of the second electrode is still a metal or metal oxide electrode, the perovskite cell device can also have a higher photoelectric conversion efficiency. Therefore, the perovskite cell provided by the embodiments of the present application can have high stability and high photoelectric conversion efficiency.
[0007] In any embodiment, the non-metal includes one or more of boron, carbon, silicon, and tellurium.
[0008] In any embodiment, the work function of the first metal is 4-5.5 eV. Optionally, the first metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0009] In any embodiment, the work function of the second metal is 4-5.5 eV. Optionally, the second metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0010] In any embodiment, the first metal and the second metal are the same, thereby enabling close contact between the first conductive film layer and the second conductive film layer, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device, thereby enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0011] In any embodiment, the second transparent conductive metal oxide includes one or more of fluorine-doped tin oxide, indium tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, and indium-doped zinc oxide.
[0012] In any embodiment, the molar ratio of the non-metal to the first metal in the first conductive film layer is greater than 0 and less than or equal to 1:1, and may be 1:15-1:5. By adjusting the molar ratio of the non-metal to the first metal in the first conductive film layer within the above range, the work function of the interface between the second charge transport layer and the first conductive film layer can be adjusted within a small range, thereby improving the carrier transfer rate, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0013] In any embodiment, the thickness of the first conductive film layer is greater than 0 and less than or equal to 30 nm, and can be optionally 5-20 nm. When the thickness of the first conductive film layer is within the above range, it can effectively prevent the erosion of the second conductive film layer by the migration of halogen ions within the perovskite material, thereby further improving the stability of the perovskite battery device and enabling the perovskite battery device to have a higher photoelectric conversion efficiency.
[0014] In any embodiment, the ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is less than or equal to 1:2.6, and can be optionally 1:16-1:4. When the ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is within the above range, it can effectively prevent the corrosion of the second conductive film layer caused by the migration of halogen ions within the perovskite material, thereby further improving the stability of the perovskite cell device and enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0015] In any embodiment, the total thickness of the second electrode is 60-120 nm, and optionally 70-90 nm.
[0016] In any embodiment, the thickness of the second conductive film layer is 50-79 nm, and can be optionally 60-75 nm.
[0017] In any embodiment, the electrode material of the first electrode includes an organic conductive material, an inorganic conductive material or an organic-inorganic mixed conductive material, optionally including one or more of a first transparent conductive metal oxide, carbon, and a metal, and more optionally including one or more of fluorine-doped tin oxide, indium tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, indium-doped zinc oxide, gold, silver, aluminum, copper, and carbon.
[0018] In any embodiment, the light absorbing layer includes a perovskite material. Optionally, the perovskite material includes one or more of an inorganic halide perovskite material, an organic halide perovskite material, and an organic-inorganic hybrid halide perovskite material.
[0019] In any embodiment, the first charge transport layer is a hole transport layer, and the second charge transport layer is an electron transport layer; or, the first charge transport layer is an electron transport layer, and the second charge transport layer is a hole transport layer.
[0020] In any embodiment, the first charge transport layer is a hole transport layer, the second charge transport layer is an electron transport layer, the conduction band bottom energy level of the second charge transport layer is higher than the work function of the first conductive film layer, and the conduction band bottom energy level of the second charge transport layer is higher than the work function of the second conductive film layer. This can increase the carrier transport rate, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0021] Optionally, the work function of the first conductive film layer is higher than the work function of the second conductive film layer, thereby further improving the carrier transmission rate.
[0022] Optionally, the first metal in the first conductive film layer includes one or more of silver, copper, aluminum, and tin, and the non-metal in the first conductive film layer includes one or more of boron, carbon, silicon, and tellurium.
[0023] Optionally, the electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide, and the second metal includes one or more of silver, copper, aluminum, and tin.
[0024] In any embodiment, the first charge transport layer is an electron transport layer, the second charge transport layer is a hole transport layer, the valence band top energy level of the second charge transport layer is lower than the work function of the first conductive film layer, and the valence band top energy level of the second charge transport layer is lower than the work function of the second conductive film layer. This can increase the carrier transport rate, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0025] Optionally, the work function of the first conductive film layer is lower than the work function of the second conductive film layer, thereby further improving the carrier transmission rate.
[0026] Optionally, the first metal in the first conductive film layer includes one or more of gold, platinum, beryllium, cobalt, silver, and molybdenum, and the non-metal in the first conductive film layer includes one or more of boron, carbon, silicon, and tellurium.
[0027] Optionally, the electrode material of the second conductive film layer includes one or more second metals, and the second metal includes one or more of gold, platinum, beryllium, cobalt, silver, and molybdenum.
[0028] In any embodiment, the electron transport material in the electron transport layer includes one or more of an organic electron transport material, an inorganic electron transport material, and an organic-inorganic hybrid electron transport material.
[0029] In any embodiment, the hole transport material in the hole transport layer includes one or more of an organic small molecule hole transport material, an organic polymer hole transport material, and an inorganic hole transport material.
[0030] The second aspect of the present application provides a method for preparing a perovskite cell, comprising the following steps: providing a first electrode; forming a first charge transport layer on the first electrode; forming a light absorption layer on the first charge transport layer; forming a second charge transport layer on the light absorption layer; forming a first conductive film layer on the second charge transport layer; and forming a second conductive film layer on the first conductive film layer, wherein the electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and the first metal, and the Fermi level of the non-metal is 4-5.5 eV; the electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide.
[0031] In any embodiment, a method of forming the first conductive film layer on the second charge transport layer includes evaporation or sputtering.
[0032] In any embodiment, a method of forming the second conductive film layer on the first conductive film layer includes evaporation or sputtering.
[0033] In any embodiment, the non-metal and the first metal are co-evaporated to form the first conductive film layer.
[0034] In a third aspect, the present application provides an electrode for a perovskite battery, comprising a first conductive film layer and a second conductive film layer stacked together, wherein the electrode material of the first conductive film layer comprises one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and a first metal, and the Fermi level of the non-metal is 4-5.5 eV; the electrode material of the second conductive film layer comprises one or more of a second metal and a second transparent conductive metal oxide.
[0035] By introducing a non-metal with a Fermi level of 4-5.5 eV into the first conductive film layer, the perovskite cell device's tolerance to halide ions can be increased, thereby enhancing the stability of the perovskite cell device. Furthermore, since the second conductive film layer is still a metal or metal oxide electrode, the perovskite cell device can also achieve a higher photoelectric conversion efficiency. Therefore, the electrodes provided in the embodiments of the present application can enable perovskite cells to have high stability and high photoelectric conversion efficiency.
[0036] In any embodiment, the non-metal includes one or more of boron, carbon, silicon, and tellurium.
[0037] In any embodiment, the work function of the first metal is 4-5.5 eV. Optionally, the first metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0038] In any embodiment, the work function of the second metal is 4-5.5 eV. Optionally, the second metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0039] In any embodiment, the first metal and the second metal are the same, thereby enabling close contact between the first conductive film layer and the second conductive film layer, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device, thereby enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0040] In any embodiment, the second transparent conductive metal oxide includes one or more of fluorine-doped tin oxide, indium tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, and indium-doped zinc oxide.
[0041] In any embodiment, the molar ratio of the non-metal to the first metal in the first conductive film layer is greater than 0 and less than or equal to 1:1, and can be optionally 1:15-1:5. By ensuring that the molar ratio of the non-metal to the first metal in the first conductive film layer is within the above range, when applied to a perovskite cell, the work function of the interface between the charge transport layer and the second conductive film layer can be adjusted within a small range, thereby increasing the carrier transfer rate, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0042] In any embodiment, the thickness of the first conductive film layer is greater than 0 and less than or equal to 30 nm, and can be optionally 5-20 nm. When the thickness of the first conductive film layer is within the above range, when applied to a perovskite cell, it can effectively prevent the erosion of the second conductive film layer by the migration of halogen ions within the perovskite material, thereby further improving the stability of the perovskite cell device and enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0043] In any embodiment, the ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is less than or equal to 1:2.6, and can be optionally 1:16-1:4. When the ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is within the above range, when applied to a perovskite cell, it can effectively prevent the corrosion of the second conductive film layer caused by the migration of halogen ions within the perovskite material, thereby further improving the stability of the perovskite cell device and enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0044] In any embodiment, the total thickness of the electrode is 60-120 nm, optionally 70-90 nm.
[0045] In any embodiment, the thickness of the second conductive film layer is 50-79 nm, and can be optionally 60-75 nm.
[0046] A fourth aspect of the present application provides a photovoltaic module, which includes the perovskite cell according to the first aspect of the present application or the perovskite cell prepared by the method according to the second aspect of the present application.
[0047] The fifth aspect of the present application provides an electrical device, which includes one or more of the perovskite cell of the first aspect of the present application, the perovskite cell prepared by the method of the second aspect of the present application, and the photovoltaic component of the fourth aspect of the present application, and the perovskite cell and the photovoltaic component are used to supply power to the electrical device.
[0048] The electrical device of the present application includes the perovskite battery provided by the present application, and thus has at least the same advantages as the perovskite battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] To more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.
[0050] FIG1 is a schematic structural diagram of a perovskite battery provided in some embodiments of the present application.
[0051] In the accompanying drawings, which are not necessarily drawn to scale, the reference numerals are as follows: 1, first electrode; 2, first charge transport layer; 3, light absorption layer; 4, second charge transport layer; 5, second electrode; 51, first conductive film layer; 52, second conductive film layer. DETAILED DESCRIPTION
[0052] Below, with appropriate reference to the accompanying drawings, the perovskite cell and its preparation method, the electrodes for the perovskite cell, the photovoltaic module, and the embodiment of the electrical device of the present application are described in detail. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0053] " range " disclosed in the present application is limited in the form of lower limit and upper limit, and given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of special range. The scope limited in this way can be to include end value or not include end value, and can be arbitrarily combined, that is, any lower limit can form a range with any upper limit combination. For example, if the scope of 60-120 and 80-110 is listed for specific parameters, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range value 1 and 2 are listed, and if the maximum range value 3,4 and 5 are listed, then the following range can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In this application, unless otherwise specified, the numerical range " ab " represents the abbreviation of any real number combination between a and b, wherein a and b are all real numbers. For example, a numerical range of "0-5" indicates that all real numbers between "0-5" are listed herein, and "0-5" is simply an abbreviation for these numerical combinations. Furthermore, when a parameter is expressed as an integer ≥ 2, this is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0054] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present application.
[0055] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form new technical solutions, and such technical solutions should be deemed to be included in the disclosure of this application.
[0056] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), indicating that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0057] Unless otherwise specified, the terms "include" and "comprising" used in this application may be open-ended or closed-ended. For example, "include" and "comprising" may mean that other components not listed may also be included or that only the listed components are included.
[0058] Unless otherwise specified, the term "or" is used in this application to be inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition "A or B" is satisfied if any of the following conditions are met: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0059] Unless otherwise specified, in this application, the terms "first", "second", etc. are used to distinguish different objects rather than to describe a specific order or a primary-secondary relationship.
[0060] Unless otherwise specified, the terms used in this application have the common meanings that are commonly understood by those skilled in the art.
[0061] Unless otherwise specified, the values of the parameters mentioned in this application can be measured using various test methods commonly used in the art, for example, they can be measured according to the test methods provided in this application. Unless otherwise specified, the test temperature for each parameter is 25°C.
[0062] The operating principle of a perovskite cell is generally as follows: under illumination, the light-absorbing layer absorbs photon energy, generating electron-hole pairs in its valence band. The electrons are excited to the conduction band, leaving holes in the valence band. The conduction band energy level of the light-absorbing layer is typically higher than that of the electron transport layer, allowing electrons to transfer from the conduction band of the light-absorbing layer to the conduction band of the electron transport layer, and then to the conductive electrode. The valence band energy level of the light-absorbing layer is typically lower than that of the hole transport layer, allowing holes to transfer from the hole transport layer to the conductive electrode. When connected to an external circuit, this completes the circuit, generating a photocurrent.
[0063] The light-absorbing layer includes perovskite materials. Perovskite materials generally use halide perovskite materials (for example, inorganic halide perovskite materials, organic halide perovskite materials, organic-inorganic hybrid halide perovskite materials, etc.), which have the advantages of large carrier diffusion length, easily adjustable band gap, high defect tolerance and low manufacturing cost, and therefore have received widespread attention.
[0064] Metal electrodes are currently commonly used conductive electrodes. However, metal electrodes are easily corroded by the migration of halogen ions inside the perovskite material. That is, the metal electrode material easily reacts with halogen ions to form metal halides, thereby reducing the stability of the perovskite battery device and affecting the photoelectric conversion efficiency of the perovskite battery device.
[0065] In view of this, the inventors improved the structure of perovskite batteries.
[0066] The present application provides a perovskite cell. Figure 1 is a schematic diagram of the structure of a perovskite cell provided in some embodiments of the present application. As shown in Figure 1, the perovskite cell includes a first electrode 1, a second electrode 5, a light absorbing layer 3, a first charge transport layer 2, and a second charge transport layer 4. The light absorbing layer 3 is located between the first electrode 1 and the second electrode 5, the first charge transport layer 2 is located between the first electrode 1 and the light absorbing layer 3, and the second charge transport layer 4 is located between the second electrode 5 and the light absorbing layer 3. The second electrode 5 includes a first conductive film layer 51 and a second conductive film layer 52, with the first conductive film layer 51 being disposed adjacent to the second charge transport layer 4.
[0067] The electrode material of the first conductive film layer 51 includes one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and a first metal, and the Fermi level of the non-metal is 4-5.5 eV; the electrode material of the second conductive film layer 52 includes one or more of a second metal, a second transparent conductive metal oxide.
[0068] The second electrode of the perovskite battery provided in an embodiment of the present application includes a first conductive film layer and a second conductive film layer, the first conductive film layer is located between the second charge transfer layer and the second conductive film layer, and the electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, and an alloy formed by a non-metal and the first metal.
[0069] By introducing a non-metal with a Fermi level of 4-5.5 eV into the first conductive film layer of the second electrode, the perovskite cell device's tolerance to halogen ions can be increased, thereby enhancing the stability of the perovskite cell device. Furthermore, since the second conductive film layer of the second electrode is still a metal or metal oxide electrode, the perovskite cell device can also have a higher photoelectric conversion efficiency. Therefore, the perovskite cell provided by the embodiments of the present application can have high stability and high photoelectric conversion efficiency.
[0070] The Fermi level of non-metals is 4-5.5 eV. Therefore, the Fermi level of non-metals is close to the work function of currently used metal or metal oxide electrodes, which does not affect carrier transport. This can improve the stability of perovskite solar cell devices while also enabling them to achieve higher photoelectric conversion efficiency. In some embodiments, the non-metals may include one or more of boron, carbon, silicon, and tellurium.
[0071] In some embodiments, the molar ratio of the non-metal to the first metal in the first conductive film layer 51 may be greater than 0 and less than or equal to 1:1.
[0072] By making the molar ratio of the non-metal in the first conductive film layer less than or equal to that of the first metal, carrier transport is facilitated, thereby improving the stability of the perovskite battery device while making the perovskite battery device have a higher photoelectric conversion efficiency.
[0073] Optionally, the molar ratio of the non-metal to the first metal in the first conductive film layer 51 may be 1:15-1:5.
[0074] By making the molar ratio of the non-metal to the first metal in the first conductive film layer within the above range, the work function of the contact surface between the second charge transport layer and the first conductive film layer can also be adjusted within a small range, thereby improving the carrier transfer rate, thereby improving the stability of the perovskite battery device while making the perovskite battery device have a higher photoelectric conversion efficiency.
[0075] In some embodiments, the thickness of the first conductive film layer 51 may be greater than 0 and less than or equal to 30 nm, and may be 5-20 nm.
[0076] The thickness of the first conductive film layer is within the above range, which can effectively prevent the erosion of the second conductive film layer by the migration of halogen ions inside the perovskite material, thereby further improving the stability of the perovskite battery device and also enabling the perovskite battery device to have a higher photoelectric conversion efficiency.
[0077] In some embodiments, the ratio of the thickness of the first conductive film layer 51 to the total thickness of the second electrode 5 may be less than or equal to 1:2.6, and may be 1:16-1:4.
[0078] The ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is within the above range, which can effectively prevent the erosion of the second conductive film layer by the migration of halogen ions inside the perovskite material, thereby further improving the stability of the perovskite battery device and also enabling the perovskite battery device to have a higher photoelectric conversion efficiency.
[0079] In some embodiments, the total thickness of the second electrode 5 (ie, the sum of the thicknesses of the first conductive film layer and the second conductive film layer) may be 60-120 nm, optionally 65-100 nm, or 70-90 nm.
[0080] In some embodiments, the thickness of the second conductive film layer 52 may be 50-115 nm, optionally 50-79 nm, or 60-75 nm.
[0081] In some embodiments, the work function of the first metal may be 4-5.5 eV. Optionally, the first metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0082] In some embodiments, the work function of the second metal may be 4-5.5 eV. Optionally, the second metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0083] In some embodiments, the first metal and the second metal may be the same, thereby enabling close contact between the first conductive film layer and the second conductive film layer, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device, thereby enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0084] In some embodiments, the second transparent conductive metal oxide may include one or more of fluorine-doped tin oxide (FTO), indium tin oxide (ITO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), and indium-doped zinc oxide (IZO).
[0085] The first electrode 1 is close to the light incident side. In some embodiments, the electrode material of the first electrode 1 may include an organic conductive material, an inorganic conductive material, or an organic-inorganic mixed conductive material. As an example, the electrode material of the first electrode 1 may include one or more of a first transparent conductive metal oxide, carbon, and a metal, and may optionally include one or more of fluorine-doped tin oxide (FTO), indium tin oxide (ITO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), indium-doped zinc oxide (IZO), gold, silver, aluminum, copper, and carbon, and more optionally include one or more of fluorine-doped tin oxide (FTO), indium tin oxide (ITO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), and indium-doped zinc oxide (IZO).
[0086] The thickness of the first electrode is not particularly limited and can be selected according to actual needs. For example, in some embodiments, the thickness of the first electrode 1 can be 10-700 nm.
[0087] The perovskite cell provided in the embodiments of the present application may be a regular structure cell or a reverse structure cell.
[0088] In some embodiments, the first charge transport layer 2 is a hole transport layer, and the second charge transport layer 4 is an electron transport layer, thereby forming an inverted structure battery.
[0089] In some embodiments, the first charge transport layer 2 is an electron transport layer, and the second charge transport layer 4 is a hole transport layer, thereby forming a formal structure battery.
[0090] In some embodiments, the first charge transport layer 2 is a hole transport layer, the second charge transport layer 4 is an electron transport layer, the conduction band bottom energy level (CBM) of the second charge transport layer 4 is higher than the work function of the first conductive film layer 51, and the conduction band bottom energy level (CBM) of the second charge transport layer 4 is higher than the work function of the second conductive film layer 52. This can increase the carrier transport rate, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0091] Optionally, the work function of the first conductive film layer 51 is higher than the work function of the second conductive film layer 52 , thereby further improving the carrier transmission rate.
[0092] Optionally, the first metal in the first conductive film layer 51 includes one or more of silver, copper, aluminum, and tin, and the non-metal in the first conductive film layer 51 includes one or more of boron, carbon, silicon, and tellurium.
[0093] Optionally, the electrode material of the second conductive film layer 52 includes one or more of a second metal and a second transparent conductive metal oxide, and the second metal includes one or more of silver, copper, aluminum, and tin.
[0094] In some embodiments, the first charge transport layer 2 is an electron transport layer, the second charge transport layer 4 is a hole transport layer, the valence band top energy level (VBM) of the second charge transport layer 4 is lower than the work function of the first conductive film layer 51, and the valence band top energy level (VBM) of the second charge transport layer 4 is lower than the work function of the second conductive film layer 52. This can increase the carrier transport rate, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0095] Optionally, the work function of the first conductive film layer 51 is lower than the work function of the second conductive film layer 52 , thereby further improving the carrier transmission rate.
[0096] Optionally, the first metal in the first conductive film layer 51 includes one or more of gold, platinum, beryllium, cobalt, silver, and molybdenum, and the non-metal in the first conductive film layer 51 includes one or more of boron, carbon, silicon, and tellurium.
[0097] Optionally, the electrode material of the second conductive film layer 52 includes one or more second metals, and the second metal includes one or more of gold, platinum, beryllium, cobalt, silver, and molybdenum, thereby improving the carrier transmission rate.
[0098] The type of electron transport material in the electron transport layer is not particularly limited and can be selected according to actual needs. For example, the electron transport material can include one or more of an organic electron transport material, an inorganic electron transport material, and an organic-inorganic hybrid electron transport material.
[0099] In some embodiments, the electron transport material may include one or more of the following materials and their derivatives and materials obtained by doping or passivation: [6,6]-phenyl C 61 Methyl butyrate (abbreviated as PC 61 BM), [6,6]-phenyl C 71 Methyl butyrate (abbreviated as PC 71 BM), fullerene C60, fullerene C70, SnO2, TiO2, ZnO. When the electron transport material is within the above range, the bottom energy level of its conduction band can better match the bottom energy level of the conduction band of the light absorbing layer, thereby facilitating the transmission of electrons.
[0100] The thickness of the electron transport layer is not particularly limited and can be selected according to actual needs. For example, in some embodiments, the thickness of the electron transport layer can be 1-300 nm.
[0101] The type of hole transport material in the hole transport layer is not particularly limited and can be selected according to actual needs. For example, the hole transport material can include one or more of organic small molecule hole transport materials, organic polymer hole transport materials, and inorganic hole transport materials.
[0102] In some embodiments, the hole transport material may include one or more of the following materials and their derivatives and materials obtained by doping or passivation: poly [bis (4-phenyl) (2,4,6-trimethylphenyl) amine] (abbreviated as PTAA), poly 3-hexylthiophene (abbreviated as P3HT), triphenylamine with triptycene as the core (abbreviated as H101), 3,4-ethylenedioxythiophene-methoxytriphenylamine (abbreviated as EDOT-OMeTPA), N- (4-anilino) carbazole-spirobifluorene (abbreviated as CzPAF-SBF), poly (3,4-ethylenedioxythiophene): polystyrenesulfonic acid (abbreviated as PEDOT:PSS), 2,2',7,7'-tetrakis (N,N-p-methoxyanilino) -9,9'-spirobifluorene (abbreviated as Spiro-OMeTAD), methoxytriphenylamine-fluoroformamidine (abbreviated as OMeTPA-FA), polythiophene, nickel oxide (NiO x , 0<x<1), molybdenum oxide (MoO3), cuprous iodide (CuI), cuprous oxide (Cu2O), cuprous thiocyanate (CuSCN).
[0103] The thickness of the hole transport layer is not particularly limited and can be selected according to actual needs. For example, in some embodiments, the thickness of the hole transport layer can be 5-1000 nm.
[0104] In some embodiments, the light absorbing layer may include a perovskite material. The type of perovskite material is not specifically limited and can be selected according to actual needs. In some embodiments, the perovskite material in the light absorbing layer may include one or more of an inorganic halide perovskite material, an organic halide perovskite material, and an organic-inorganic hybrid halide perovskite material.
[0105] The perovskite material may include one or more of the materials shown as ABX3, A2CDX6.
[0106] A represents an inorganic cation, an organic cation, or an organic-inorganic mixed cation. As an example, A may include CH3NH3 + (abbreviated as MA + )、CH(NH2)2 + (abbreviated as FA + )、Li + 、Na + , K + , Rb + 、Cs +Alternatively, A may include CH3NH3 + 、CH(NH2)2 + 、Cs + One or more of .
[0107] B represents an inorganic cation, an organic cation, or an organic-inorganic mixed cation. Alternatively, B may represent a divalent metal cation. As an example, B may include Pb 2+ 、Sn 2+ 、Be 2+ Mg 2+ , Ca 2+ 、Sr 2+ 、Ba 2+ 、Zn 2+ 、Ge 2+ 、Fe 2+ 、Co 2+ 、Ni 2+ Optionally, B may include Pb 2+ 、Sn 2+ One or both of them.
[0108] C represents an inorganic cation, an organic cation, or an organic-inorganic mixed cation. Alternatively, C may represent a monovalent metal cation. As an example, C may include Li + 、Na + , K + , Rb + 、Cs + 、Ag + One or more of .
[0109] D represents an inorganic cation, an organic cation, or an organic-inorganic mixed cation. Alternatively, D may represent a trivalent metal cation. As an example, D may include In 3+ 、Bi 3+ One or more of .
[0110] X represents an inorganic anion, an organic anion, or an organic-inorganic mixed anion. Alternatively, X may represent a halogen ion. As an example, X may include F - 、Cl - Br - , I - Optionally, X may include Cl - Br - , I - One or more of .
[0111] In some embodiments, the perovskite material in the light absorbing layer may include but is not limited to CH3NH3PbI3 (abbreviated as MAPbI3), CH(NH2)2PbI3 (abbreviated as FAPbI3), Cs 0.05 (FA 0.83 MA 0.17 ) 0.95 Pb(I 0.83 Br 0.17 )3 (abbreviated as CsFAMA), one or more of CsPbI3, CsPbI2Br, CsPbIBr2, Cs2NaInCl6, Cs2KBiCl6, and Cs2AgInCl6.
[0112] In some embodiments, the band gap of the light absorbing layer may be 1.20 eV to 2.30 eV. The band gap of the light absorbing layer can be obtained by obtaining an ultraviolet absorption curve through ultraviolet absorption spectrum absorption and then calculated using the Tauc equation.
[0113] The thickness of the light absorbing layer is not particularly limited and can be selected according to actual needs. In some embodiments, the thickness of the light absorbing layer can be 400-1000 nm.
[0114] In some embodiments, the perovskite cell further includes a substrate, such as a glass substrate, and a transparent metal conductive oxide may be disposed on the surface of the substrate.
[0115] The perovskite cell provided in the embodiments of the present application is not limited to the above structure, and may also include other functional layers, for example, it may also include a passivation layer arranged between the first charge transport layer and / or the second charge transport layer and the light absorption layer.
[0116] In some embodiments, a perovskite cell may include a substrate, a first electrode 1, a first charge transport layer 2, a light absorption layer 3, a second charge transport layer 4, a first conductive film layer 51, and a second conductive film layer 52, which are stacked in sequence. The electrode material of the first conductive film layer 51 includes one or more of a mixture of a non-metal and a first metal, an alloy of a non-metal and the first metal, and the non-metal includes one or more of boron, carbon, silicon, and tellurium. The electrode material of the second conductive film layer 52 includes one or more of a second metal and a second transparent conductive metal oxide. Optionally, a passivation layer is further provided between the first charge transport layer 2 and the light absorption layer 3, and / or between the second charge transport layer 4 and the light absorption layer 3.
[0117] In some embodiments, a perovskite cell may include a substrate, a first electrode 1, a first charge transport layer 2, a light absorption layer 3, a second charge transport layer 4, a first conductive film layer 51, and a second conductive film layer 52, stacked in sequence. The electrode material of the first conductive film layer 51 includes one or more of a mixture of a non-metal and a first metal, an alloy of a non-metal and the first metal, and the non-metal includes one or more of boron, carbon, silicon, and tellurium. The electrode material of the second conductive film layer 52 includes a second metal, and the first and second metals are the same. Optionally, a passivation layer is further provided between the first charge transport layer 2 and the light absorption layer 3, and / or between the second charge transport layer 4 and the light absorption layer 3.
[0118] This allows the first conductive film layer and the second conductive film layer to be in close contact, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0119] [Preparation method]
[0120] The embodiments of the present application also provide a method for preparing the above-mentioned perovskite battery.
[0121] The method includes the following steps: providing a first electrode 1; forming a first charge transport layer 2 on the first electrode 1; forming a light absorption layer 3 on the first charge transport layer 2; forming a second charge transport layer 4 on the light absorption layer 3; forming a first conductive film layer 51 on the second charge transport layer 4; and forming a second conductive film layer 52 on the first conductive film layer 51. The electrode material of the first conductive film layer 51 includes one or more of a mixture of a non-metal and a first metal, an alloy of a non-metal and the first metal, and the Fermi level of the non-metal is 4-5.5 eV. The electrode material of the second conductive film layer 52 includes one or more of a second metal and a second transparent conductive metal oxide.
[0122] In some embodiments, the method of forming the first conductive film layer 51 on the second charge transport layer 4 may include evaporation or sputtering. In some embodiments, the evaporation may be vacuum evaporation. Optionally, the vacuum degree of the evaporation may be 10 -4 to 10 - 6 Pa, the evaporation rate can be 0.1-5A / s. In some embodiments, sputtering can be magnetron sputtering. Optionally, the operating pressure can be 10 -3 to 10 -7 Pa, sputtering power density can be 800-1200W / cm 2 .
[0123] In some embodiments, the non-metal and the first metal can be co-evaporated to form a first conductive film layer. By adjusting the evaporation rates of the non-metal and the first metal, the molar ratio of the non-metal and the first metal can be adjusted, and the thickness of the first conductive film layer can also be adjusted.
[0124] In some embodiments, the method of forming the second conductive film layer 52 on the first conductive film layer 51 may include evaporation or sputtering. In some embodiments, the evaporation may be vacuum evaporation. Optionally, the vacuum degree of the evaporation may be 10 -4 to 10 -6 Pa, the evaporation rate can be 0.1-5A / s. In some embodiments, sputtering can be magnetron sputtering. Optionally, the operating pressure can be 10 -3 to 10 -7 Pa, sputtering power density can be 800-1200W / cm 2 .
[0125] In some embodiments, the method includes the following steps: providing a first electrode 1; forming a first charge transport layer 2 on the first electrode 1; forming a light absorption layer 3 on the first charge transport layer 2; forming a second charge transport layer 4 on the light absorption layer 3; co-evaporating a non-metal and a first metal on the second charge transport layer 4 to form a first conductive film layer 51; and further evaporating the first metal on the first conductive film layer 51 to form a second conductive film layer 52. The electrode material of the first conductive film layer 51 includes one or more of a mixture of a non-metal and the first metal, an alloy of a non-metal and the first metal, and the non-metal has a Fermi level of 4-5.5 eV; the electrode material of the second conductive film layer 52 includes the first metal. This allows the first conductive film layer and the second conductive film layer to be in close contact, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device. This can improve the stability of the perovskite cell device while also enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0126] The film forming methods of the first charge transport layer 2, the light absorbing layer 3, and the second charge transport layer 4 are not subject to specific restrictions, and film forming methods known in the art may be used, for example, chemical bath deposition, chemical vapor deposition, electrochemical deposition, physical epitaxial growth, thermal evaporation, atomic layer deposition, magnetron sputtering, precursor liquid spin coating, precursor liquid slit coating, precursor liquid scraping, mechanical pressing, sol-gel method, pulsed laser deposition, etc.
[0127] The perovskite cell provided in the embodiments of the present application can be used alone as a single-junction perovskite cell, or can be made into a stacked cell with perovskite-type or other types of perovskite cells, such as a perovskite-perovskite stacked cell or a perovskite-crystalline silicon stacked cell.
[0128] The embodiments of the present application also provide an electrode for a perovskite battery.
[0129] The electrode provided in the embodiment of the present application includes a first conductive film layer and a second conductive film layer that are stacked together. The electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and the first metal, and the Fermi level of the non-metal is 4-5.5eV; the electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide.
[0130] The electrode provided in the embodiment of the present application includes a first conductive film layer and a second conductive film layer stacked together, and the electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, and an alloy formed by a non-metal and the first metal.
[0131] By introducing a non-metal with a Fermi level of 4-5.5 eV into the first conductive film layer, the perovskite cell device's tolerance to halide ions can be increased, thereby enhancing the stability of the perovskite cell device. Furthermore, since the second conductive film layer is still a metal or metal oxide electrode, the perovskite cell device can also achieve a higher photoelectric conversion efficiency. Therefore, the electrodes provided in the embodiments of the present application can enable perovskite cells to have high stability and high photoelectric conversion efficiency.
[0132] The Fermi level of non-metals is 4-5.5 eV. Therefore, the Fermi level of non-metals is close to the work function of currently used metal or metal oxide electrodes, which does not affect carrier transport. This can improve the stability of perovskite solar cell devices while also enabling them to achieve higher photoelectric conversion efficiency. In some embodiments, the non-metals may include one or more of boron, carbon, silicon, and tellurium.
[0133] In some embodiments, a molar ratio of the non-metal to the first metal in the first conductive film layer may be greater than 0 and less than or equal to 1:1.
[0134] By making the molar ratio of non-metal in the first conductive film layer less than or equal to that of the first metal, it is beneficial to carrier transport when applied to perovskite cells, thereby improving the stability of the perovskite cell device while making the perovskite cell device have a higher photoelectric conversion efficiency.
[0135] Optionally, the molar ratio of the non-metal to the first metal in the first conductive film layer may be 1:15-1:5.
[0136] By making the molar ratio of the non-metal to the first metal in the first conductive film layer within the above range, when applied to perovskite cells, the work function of the contact surface between the charge transfer layer and the second conductive film layer can also be adjusted within a small range, thereby improving the carrier transfer rate, and further improving the stability of the perovskite cell device while making the perovskite cell device have a higher photoelectric conversion efficiency.
[0137] In some embodiments, the thickness of the first conductive film layer may be greater than 0 and less than or equal to 30 nm, and may be 5-20 nm.
[0138] When the thickness of the first conductive film layer is within the above range and is applied to a perovskite cell, it can effectively prevent the erosion of the second conductive film layer by the migration of halogen ions inside the perovskite material, thereby further improving the stability of the perovskite cell device and enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0139] In some embodiments, the ratio of the thickness of the first conductive film layer to the total thickness of the second electrode 5 may be less than or equal to 1:2.6, and may be optionally 1:16-1:4.
[0140] The ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is within the above range. When applied to a perovskite cell, it can effectively prevent the erosion of the second conductive film layer by the migration of halogen ions inside the perovskite material, thereby further improving the stability of the perovskite cell device and also enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0141] In some embodiments, the total thickness of the electrode (ie, the sum of the thicknesses of the first conductive film layer and the second conductive film layer) may be 60-120 nm, optionally 65-100 nm, or 70-90 nm.
[0142] In some embodiments, the thickness of the second conductive film layer may be 50-115 nm, optionally 50-79 nm, or 60-75 nm.
[0143] In some embodiments, the work function of the first metal may be 4-5.5 eV. Optionally, the first metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0144] In some embodiments, the work function of the second metal may be 4-5.5 eV. Optionally, the second metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt.
[0145] In some embodiments, the first metal and the second metal may be the same, thereby enabling close contact between the first conductive film layer and the second conductive film layer, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device, thereby enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0146] In some embodiments, the second transparent conductive metal oxide may include one or more of fluorine-doped tin oxide (FTO), indium tin oxide (ITO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), and indium-doped zinc oxide (IZO).
[0147] In some embodiments, the electrode includes a first conductive film layer and a second conductive film layer stacked together, the electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and the first metal, and the non-metal includes one or more of boron, carbon, silicon, and tellurium; the electrode material of the second conductive film layer includes a second metal, and the first metal and the second metal are the same.
[0148] This allows the first conductive film layer and the second conductive film layer to be in close contact, thereby helping to reduce contact resistance and increase the fill factor of the perovskite cell device, thereby improving the stability of the perovskite cell device while enabling the perovskite cell device to have a higher photoelectric conversion efficiency.
[0149] An embodiment of the present application also provides a photovoltaic module, which includes the perovskite cell provided in the embodiment of the present application or the perovskite cell prepared by the preparation method provided in the embodiment of the present application. The perovskite cell can be used as a power source for the photovoltaic module after processes such as series and parallel connection and packaging.
[0150] In some embodiments, the photovoltaic module includes the single-junction perovskite cell, the perovskite-perovskite tandem cell, or the perovskite-crystalline silicon tandem cell provided in the embodiments of the present application.
[0151] An embodiment of the present application also provides an electrical device, which includes one or more of the perovskite cell provided in the embodiment of the present application, the perovskite cell prepared by the method provided in the embodiment of the present application, and the photovoltaic module provided in the embodiment of the present application. The above-mentioned perovskite cell and photovoltaic module can be used to supply power to the electrical device.
[0152] In some embodiments, the power-consuming device may be a common device including the perovskite cell or photovoltaic module provided in the embodiments of the present application, such as equipment used in the fields of communications, transportation, industry and agriculture, lighting, etc. As examples, the power-consuming device may include satellites, communications equipment, traffic lights, lighthouses, wireless telephone booths, monitoring equipment for oil drilling, power systems, camping lanterns, electric vehicles, and electronic device chargers.
[0153] Example
[0154] The following examples describe the present disclosure in more detail and are intended to be illustrative only, as various modifications and variations within the scope of the present disclosure will be apparent to those skilled in the art. Unless otherwise indicated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and used directly without further processing, and all instruments used in the examples are commercially available.
[0155] Example 1-1
[0156] Preparation of the first electrode
[0157] Twenty pieces of 2.0 cm × 2.0 cm ITO-coated conductive glass were taken, and 0.35 cm of the ITO layer was removed from each end by laser etching to expose the glass substrate. After that, they were ultrasonically cleaned with water, acetone, and isopropyl alcohol in sequence, the solvents were blown off with a nitrogen gun, and then further cleaned in a UV ozone machine to obtain the first electrode.
[0158] Preparation of hole transport layer
[0159] A 2 mg / mL PTAA-chlorobenzene solution was spin-coated on the first electrode at a rate of 5000 rpm, and then annealed on a hot plate at 100° C. for 10 min to obtain a hole transport layer with a thickness of about 20 nm.
[0160] Preparation of light-absorbing layer
[0161] A perovskite precursor solution was spin-coated onto the hole transport layer at a rate of 1000-5000 rpm, followed by annealing at 100°C for 30 minutes and cooling to room temperature to form a light-absorbing layer with a thickness of approximately 680 nm. The perovskite material was CsFAMA, the solvent was N,N-dimethylformamide, and the precursor solution concentration was 1.5 mol / L.
[0162] Preparation of electron transport layer
[0163] Spin coat [6,6]-phenyl C on the light absorbing layer at a rate of 1000-1500 rpm 61 Methyl butyrate (PC 61 The substrate was prepared by spin coating a bathocuproin (BCP) passivation layer at a speed of 5000 rpm. The thickness of the PCBM layer was about 60 nm, and the thickness of the BCP passivation layer was about 6 nm.
[0164] Preparation of the second electrode
[0165] The above-mentioned sample was placed in an evaporation machine, and copper and silicon were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then the copper electrode was evaporated at a rate of 2A / s to obtain the second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0166] The perovskite cell structure finally obtained in Example 1-1 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / Cu+Si / Cu.
[0167] Example 1-2
[0168] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1.
[0169] Preparation of the second electrode
[0170] The above-mentioned sample was placed in an evaporation machine, and copper and boron were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then the copper electrode was evaporated at a rate of 2A / s to obtain the second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0171] The perovskite cell structure finally obtained in Example 1-2 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / Cu+B / Cu.
[0172] Examples 1-3
[0173] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1.
[0174] Preparation of the second electrode
[0175] The above-mentioned sample was placed in an evaporation machine, and copper and tellurium were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then the copper electrode was evaporated at a rate of 2A / s to obtain the second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0176] The perovskite cell structure finally obtained in Example 1-3 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / Cu+Te / Cu.
[0177] Examples 1-4
[0178] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1.
[0179] Preparation of the second electrode
[0180] The above-mentioned sample was placed in an evaporation machine, and copper and carbon were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then the copper electrode was evaporated at a rate of 2A / s to obtain the second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0181] The perovskite cell structure finally obtained in Example 1-4 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / Cu+C / Cu.
[0182] Examples 1-5 to 1-9
[0183] The preparation of the perovskite cell was the same as that of Example 1-1, except that the molar ratio of the non-metal to the first metal in the first conductive film layer of the second electrode was different. Specific parameters are shown in Table 1. The molar ratio of the non-metal to the first metal can be adjusted by adjusting the evaporation rates of copper and silicon.
[0184] Examples 1-10 to 1-16
[0185] Except for the different thickness of the first conductive film layer of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1. The specific parameters are shown in Table 1.
[0186] Examples 1-17 to 1-18
[0187] Except for the different type of the second conductive film layer of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1. The specific parameters are shown in Table 1.
[0188] Comparative Example 1-1
[0189] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1.
[0190] Preparation of the second electrode
[0191] The above-mentioned sample was placed in an evaporation machine, and a copper electrode was evaporated to 80 nm at a rate of 1 A / s to complete the preparation of the perovskite battery device.
[0192] The perovskite cell structure finally obtained in Comparative Example 1-1 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / Cu.
[0193] Comparative Example 1-2
[0194] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1.
[0195] Preparation of the second electrode
[0196] The above sample was placed in an evaporation machine and 5.5nm ITO was evaporated to complete the preparation of the first conductive film layer; then a copper electrode was evaporated at a rate of 2A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0197] The perovskite cell structure finally obtained in Comparative Example 1-2 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / ITO / Cu.
[0198] Comparative Examples 1-3
[0199] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 1-1.
[0200] Preparation of the second electrode
[0201] The above-mentioned sample was placed in an evaporation machine, and a Bi electrode was evaporated to 5.5 nm at a rate of 1 A / s to complete the preparation of the first conductive film layer; then a copper electrode was evaporated at a rate of 2 A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80 nm, completing the preparation of the perovskite battery device.
[0202] The perovskite cell structure finally obtained in Comparative Examples 1-3 is ITO / PTAA / CsFAMA / PC 61 BM / BCP / Bi / Cu.
[0203] The performance of the perovskite cells provided in Examples 1-1 to 1-18 and Comparative Examples 1-1 to 1-3 was tested. The results are shown in Table 1.
[0204] (1) Initial photoelectric conversion efficiency (PCE0) test of perovskite cells
[0205] Under standard simulated sunlight (AM 1.5G, 100mW / cm 2 ) irradiation, the performance of the perovskite battery was tested to obtain the IV curve. According to the IV curve and the data fed back by the test equipment, the short-circuit current Jsc (unit: mA / cm 2 ), open-circuit voltage Voc (V), maximum light output current Jmpp (mA), and maximum light output voltage Vmpp (V). The fill factor (FF) of the perovskite cell (in %) was calculated using the formula FF = Jsc × Voc / (Jmpp × Vmpp). The photoelectric conversion efficiency (PCE) of the perovskite cell (in %) was calculated using the formula PCE = (Jsc × Voc × FF) / Pw, where Pw represents the input power (in mW).
[0206] (2) Stability test of perovskite cells
[0207] The perovskite cell was placed in a dry room at 65°C on a hot plate for accelerated testing with a humidity of about 5%. After 10 days, the photoelectric conversion efficiency was retested and recorded as PCE. 10 . Take PCE 10 / PCE0 represents the stability of the perovskite cell.
[0208] Table 1
[0209] It can be seen from the test results in Table 1 that by making the second electrode include a first conductive film layer and a second conductive film layer, the first conductive film layer is located between the electron transport layer and the second conductive film layer, and the electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and the first metal, and the electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide, the stability of the perovskite cell can be greatly improved, and the photoelectric conversion efficiency of the perovskite cell can also be improved.
[0210] Example 2-1
[0211] Preparation of the first electrode
[0212] Twenty pieces of 2.0 cm × 2.0 cm ITO-coated conductive glass were taken, and 0.35 cm of the ITO layer was removed from each end by laser etching to expose the glass substrate. After that, they were ultrasonically cleaned with water, acetone, and isopropyl alcohol in sequence, the solvents were blown off with a nitrogen gun, and then further cleaned in a UV ozone machine to obtain the first electrode.
[0213] Preparation of electron transport layer
[0214] A tin dioxide nanoparticle solution (commercially available, can be diluted before use) was spin-coated on the first electrode at a speed of 1000-3000 rpm, and then annealed at 150° C. for 30 min. After cooling to room temperature, an electron transport layer with a thickness of about 20 nm was obtained.
[0215] Preparation of light-absorbing layer
[0216] A perovskite precursor solution was spin-coated onto the hole transport layer at a rate of 1000-5000 rpm, followed by annealing at 100°C for 30 minutes and cooling to room temperature to form a light-absorbing layer with a thickness of approximately 680 nm. The perovskite material was CsFAMA, the solvent was N,N-dimethylformamide, and the precursor solution concentration was 1.5 mol / L.
[0217] Preparation of hole transport layer
[0218] Spiro solution (commercially available, with a concentration of 72.3 mg / ml, using chlorobenzene as the solvent and containing additives such as lithium salt) was dynamically spin-coated on the light-absorbing layer at a speed of 4000-4000 rpm without annealing to directly obtain a hole transport layer with a thickness of about 180 nm.
[0219] Preparation of the second electrode
[0220] The above-mentioned sample was placed in an evaporation machine, and gold and silicon were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then a gold electrode was evaporated at a rate of 2A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0221] The perovskite cell structure finally obtained in Example 2-1 is ITO / SnO2 / CsFAMA / Spiro / Au+Si / Au.
[0222] Example 2-2
[0223] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1.
[0224] Preparation of the second electrode
[0225] The above-mentioned sample was placed in an evaporation machine, and gold and boron were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then a gold electrode was evaporated at a rate of 2A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0226] The perovskite cell structure finally obtained in Example 2-2 is ITO / SnO2 / CsFAMA / Spiro / Au+B / Au.
[0227] Example 2-3
[0228] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1.
[0229] Preparation of the second electrode
[0230] The above-mentioned sample was placed in an evaporation machine, and gold and tellurium were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then a gold electrode was evaporated at a rate of 2A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0231] The perovskite cell structure finally prepared in Example 2-3 is ITO / SnO2 / CsFAMA / Spiro / Au+Te / Au.
[0232] Examples 2-4
[0233] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1.
[0234] Preparation of the second electrode
[0235] The above-mentioned sample was placed in an evaporation machine, and gold and carbon were co-evaporated at rates of 1A / s and 0.1A / s respectively to complete the preparation of the first conductive film layer with a thickness of 5.5nm; then a gold electrode was evaporated at a rate of 2A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0236] The perovskite cell structure finally obtained in Example 2-4 is ITO / SnO2 / CsFAMA / Spiro / Au+C / Au.
[0237] Examples 2-5 to 2-6
[0238] Except for the different type of the second conductive film layer of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1. The specific parameters are shown in Table 2.
[0239] Comparative Example 2-1
[0240] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1.
[0241] Preparation of the second electrode
[0242] The above-mentioned sample was placed in an evaporation machine, and a gold electrode was evaporated to 80 nm at a rate of 1 A / s to complete the preparation of the perovskite battery device.
[0243] The perovskite cell structure finally obtained in Comparative Example 2-1 is ITO / SnO2 / CsFAMA / Spiro / Au.
[0244] Comparative Example 2-2
[0245] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1.
[0246] Preparation of the second electrode
[0247] The above-mentioned sample was placed in an evaporation machine, and ITO 5.5nm was evaporated to complete the preparation of the first conductive film layer; then a gold electrode was evaporated at a rate of 2A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80nm, completing the preparation of the perovskite battery device.
[0248] The perovskite cell structure finally obtained in Comparative Example 2-2 is ITO / SnO2 / CsFAMA / Spiro / ITO / Au.
[0249] Comparative Examples 2-3
[0250] Except for the different preparation process of the second electrode, the preparation of the perovskite cell is the same as that of Example 2-1.
[0251] Preparation of the second electrode
[0252] The above-mentioned sample was placed in an evaporation machine, and a Bi electrode was evaporated to 5.5 nm at a rate of 1 A / s to complete the preparation of the first conductive film layer; then a gold electrode was evaporated at a rate of 2 A / s to obtain a second conductive film layer. The total thickness of the second electrode was 80 nm, completing the preparation of the perovskite battery device.
[0253] The perovskite cell structure finally obtained in Comparative Example 2-3 is ITO / SnO2 / CsFAMA / Spiro / Bi / Au.
[0254] The performance test methods of the perovskite cells of Examples 2-1 to 2-6 and Comparative Examples 2-1 to 2-3 were the same as those of Examples 1-1 to 1-18 and Comparative Examples 1-1 to 1-3. The results are shown in Table 2.
[0255] Table 2
[0256] It can be seen from the test results in Table 2 that by making the second electrode include a first conductive film layer and a second conductive film layer, the first conductive film layer is located between the hole transport layer and the second conductive film layer, and the electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, an alloy formed by a non-metal and the first metal, and the electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide, the stability of the perovskite cell can be greatly improved, and the photoelectric conversion efficiency of the perovskite cell can also be improved.
[0257] It can also be seen from the test results in Table 2 that, in a regular structure battery, when the second conductive film layer includes a second metal, the photoelectric conversion efficiency can be further improved.
[0258] The above description is merely a specific embodiment of the present application, but the scope of protection of the present application is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present application, and such modifications or substitutions should be included in the scope of protection of the present application. Therefore, the scope of protection of the present application should be based on the scope of protection of the claims.
Claims
1. A perovskite battery, comprising: a first electrode; a second electrode; a light absorbing layer, located between the first electrode and the second electrode; A first charge transport layer, located between the first electrode and the light absorbing layer; as well as A second charge transport layer is located between the second electrode and the light absorbing layer, in, The second electrode comprises a first conductive film layer and a second conductive film layer, wherein the first conductive film layer is arranged close to the second charge transport layer; The electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, and an alloy formed by a non-metal and the first metal, and the Fermi level of the non-metal is 4-5.5 eV; The electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide.
2. The perovskite cell according to claim 1, wherein: The non-metal includes one or more of boron, carbon, silicon, and tellurium; and / or, The work function of the first metal is 4-5.5 eV. Optionally, the first metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt; and / or, The work function of the second metal is 4-5.5 eV. Optionally, the second metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt; and / or, The second transparent conductive metal oxide includes one or more of fluorine-doped tin oxide, indium tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, and indium-doped zinc oxide.
3. The perovskite cell according to claim 1 or 2, wherein: The first metal is the same as the second metal.
4. The perovskite battery according to any one of claims 1 to 3, wherein: The molar ratio of the non-metal to the first metal in the first conductive film layer is greater than 0 and less than or equal to 1:1, and may be 1:15-1:
5.
5. The perovskite cell according to any one of claims 1 to 4, wherein: The thickness of the first conductive film layer is greater than 0 and less than or equal to 30 nm, and may be 5-20 nm; and / or, The ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is less than or equal to 1:2.6, and can be optionally 1:16-1:
4.
6. The perovskite cell according to claim 5, wherein: The total thickness of the second electrode is 60-120 nm, and optionally 70-90 nm; and / or, The thickness of the second conductive film layer is 50-79 nm, and can be 60-75 nm.
7. The perovskite cell according to any one of claims 1 to 6, wherein: The electrode material of the first electrode includes an organic conductive material, an inorganic conductive material or an organic-inorganic mixed conductive material, optionally including one or more of a first transparent conductive metal oxide, carbon, and a metal, and more optionally including one or more of fluorine-doped tin oxide, indium tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, indium-doped zinc oxide, gold, silver, aluminum, copper, and carbon; and / or, The light absorbing layer includes a perovskite material. Optionally, the perovskite material includes one or more of an inorganic halide perovskite material, an organic halide perovskite material, and an organic-inorganic hybrid halide perovskite material.
8. The perovskite cell according to any one of claims 1 to 7, wherein: The first charge transport layer is a hole transport layer, and the second charge transport layer is an electron transport layer; or, the first charge transport layer is an electron transport layer, and the second charge transport layer is a hole transport layer.
9. The perovskite cell according to any one of claims 1 to 8, wherein: The first charge transport layer is a hole transport layer, the second charge transport layer is an electron transport layer, the conduction band bottom energy level of the second charge transport layer is higher than the work function of the first conductive film layer, and the conduction band bottom energy level of the second charge transport layer is higher than the work function of the second conductive film layer; Optionally, a work function of the first conductive film layer is higher than a work function of the second conductive film layer.
10. The perovskite cell according to claim 9, wherein: The first metal in the first conductive film layer includes one or more of silver, copper, aluminum, and tin, and the non-metal in the first conductive film layer includes one or more of boron, carbon, silicon, and tellurium; and / or, The electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide, and the second metal includes one or more of silver, copper, aluminum, and tin.
11. The perovskite cell according to any one of claims 1 to 8, wherein: The first charge transport layer is an electron transport layer, the second charge transport layer is a hole transport layer, the valence band top energy level of the second charge transport layer is lower than the work function of the first conductive film layer, and the valence band top energy level of the second charge transport layer is lower than the work function of the second conductive film layer; Optionally, a work function of the first conductive film layer is lower than a work function of the second conductive film layer.
12. The perovskite cell according to claim 11, wherein: The first metal in the first conductive film layer includes one or more of gold, platinum, beryllium, cobalt, silver, and molybdenum, and the non-metal in the first conductive film layer includes one or more of boron, carbon, silicon, and tellurium; and / or, The electrode material of the second conductive film layer includes one or more second metals, and the second metal includes one or more of gold, platinum, beryllium, cobalt, silver, and molybdenum.
13. The perovskite cell according to any one of claims 8 to 12, wherein: The electron transport material in the electron transport layer includes one or more of an organic electron transport material, an inorganic electron transport material, and an organic-inorganic hybrid electron transport material; and / or, The hole transport material in the hole transport layer includes one or more of an organic small molecule hole transport material, an organic polymer hole transport material, and an inorganic hole transport material.
14. A method for preparing the perovskite battery according to any one of claims 1 to 13, comprising the following steps: providing a first electrode; forming a first charge transport layer on the first electrode; forming a light absorbing layer on the first charge transport layer; forming a second charge transport layer on the light absorbing layer; forming a first conductive film layer on the second charge transport layer; as well as forming a second conductive film layer on the first conductive film layer, The electrode material of the first conductive film layer includes one or more of a mixture of a non-metal and a first metal, and an alloy formed by a non-metal and a first metal, and the Fermi level of the non-metal is 4-5.5eV; the electrode material of the second conductive film layer includes one or more of a second metal and a second transparent conductive metal oxide.
15. The method according to claim 14, wherein: The method of forming the first conductive film layer on the second charge transport layer comprises evaporation or sputtering; and / or, The method of forming the second conductive film layer on the first conductive film layer comprises evaporation or sputtering; and / or, The non-metal and the first metal are co-evaporated to form the first conductive film layer.
16. An electrode for a perovskite battery, comprising a first conductive film layer and a second conductive film layer stacked in layers, wherein the electrode material of the first conductive film layer comprises one or more of a mixture of a non-metal and a first metal, and an alloy formed by a non-metal and a first metal, and the Fermi level of the non-metal is 4-5.5 eV; the electrode material of the second conductive film layer comprises one or more of a second metal and a second transparent conductive metal oxide.
17. The electrode according to claim 16, wherein The non-metal includes one or more of boron, carbon, silicon, and tellurium; and / or, The work function of the first metal is 4-5.5 eV. Optionally, the first metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt; and / or, The work function of the second metal is 4-5.5 eV. Optionally, the second metal includes one or more of gold, silver, copper, aluminum, tin, molybdenum, platinum, beryllium, and cobalt; and / or, The second transparent conductive metal oxide includes one or more of fluorine-doped tin oxide, indium tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, boron-doped zinc oxide, and indium-doped zinc oxide.
18. The electrode according to claim 16 or 17, wherein The first metal is the same as the second metal.
19. The electrode according to any one of claims 16 to 18, wherein: The molar ratio of the non-metal to the first metal in the first conductive film layer is greater than 0 and less than or equal to 1:1, and may be 1:15-1:
5.
20. The electrode according to any one of claims 16 to 19, wherein: The thickness of the first conductive film layer is greater than 0 and less than or equal to 30 nm, and may be 5-20 nm; and / or, The ratio of the thickness of the first conductive film layer to the total thickness of the second electrode is less than or equal to 1:2.6, and can be optionally 1:16-1:
4.
21. The electrode according to claim 20, wherein The total thickness of the electrode is 60-120 nm, optionally 70-90 nm; and / or, The thickness of the second conductive film layer is 50-79 nm, and can be 60-75 nm.
22. A photovoltaic module, comprising the perovskite cell according to any one of claims 1 to 13, or a perovskite cell prepared by the method according to any one of claims 14 to 15.
23. An electrical device, comprising one or more of the perovskite cell according to any one of claims 1 to 13, the perovskite cell prepared by the method according to any one of claims 14 to 15, and the photovoltaic module according to claim 22, wherein the perovskite cell and the photovoltaic module are used to supply power to the electrical device.
Citation Information
Patent Citations
Novel planar heterojunction perovskite solar cell with high efficiency and long life manufactured by adopting low-temperature solution method
CN105024013A
Metal halide perovskite materials, preparation method thereof as well as solar cell device and preparation method of solar cell device
CN109912458A
Perovskite solar cell and preparation method thereof
CN111668373A
Perovskite solar cell, preparation method thereof and photovoltaic system
CN114695671A
Solar cell, preparation method thereof and photovoltaic module
CN115274885A