Optical device imprinted on surface of transparent wood and use thereof
By carefully imprinting on the transparent wood surface to build micro-nano structures, the problem of insufficient surface modification treatment of transparent wood in the prior art is solved, efficient optical performance improvement and expansion of its application potential in optical devices and other fields.
Patent Information
- Application Number
- PCT/CN2023/095229
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-21
AI Technical Summary
The existing research on functionalization of transparent wood mainly focuses on filling polymer modification and nanoparticle addition, with few surface modification treatments and lack of development of new technologies and products, resulting in the inadequate exploration of its application potential in the fields of optics and other fields.
Micro-nano structures are constructed by precision imprinting on the surface of transparent wood, and transparent wood surface imprinting optics are prepared, and ultraviolet curing glue and grating array templates are used to imprint on silicon wafers with resistivity of 1Ωcm-1-10Ωcm-1 , form grating and dot matrix structures to enhance their optical properties.
It realizes the color stripe phenomenon and efficient diffraction efficiency under laser irradiation, improves the optical performance of transparent wood, surpasses the imprinted structure with PMMA as the substrate, and broadens its application prospects in optical and optoelectronic devices.
Smart Images

Figure CN2023095229_21112024_PF_FP_ABST
Abstract
Description
A transparent wood surface imprinting optical device and its application Technical Field
[0001] The invention belongs to the technical field of optical devices, and in particular relates to a transparent wood surface imprinting optical device and application thereof. Background Art
[0002] Wood is considered a key development direction due to its abundant resources, high strength-to-weight ratio, low density, and potential for functionalization. However, over time, wood exhibits many adverse effects, including moisture absorption, cracking, warping, mildew, and photodegradation. This significantly reduces its durability and poses safety risks. To address these issues, researchers have proposed numerous cell wall modification technologies or physical and chemical modification methods at the molecular, atomic, and nanoscale. These methods utilize physical densification, filling, and high-temperature carbonization, as well as chemical methods such as extraction, grafting, polymerization, etherification, and esterification to functionalize natural wood. These methods have resulted in a range of woods with specialized functions, which are being applied to emerging fields such as bioengineering, flexible electronics, oil-water separation, seawater desalination, and energy storage.
[0003] Transparent wood, a wood-based composite material, can be prepared by in-situ depolymerization of lignin and backfilling with a refractive index-matched polymer to produce a material with excellent optical and mechanical properties. It combines the skeletal structure and anisotropy of natural wood cell walls, while boasting greater strength than wood, greater toughness than glass, and greater energy efficiency and environmental friendliness than plastic. The concept of transparent wood was first proposed in 1992. Transparent wood was prepared by bleaching, dehydrating, and impregnating with a transparent resin, primarily focusing on its preparation methods. Since 2016, two research groups, the Royal Institute of Technology in Sweden and the University of Maryland in the United States, have reported on their structural and functional research results, proposing new research directions and ideas for transparent wood, attracting widespread attention from both academia and industry. Research has shown that by modifying transparent wood based on its excellent optical and mechanical properties to impart enhanced functionalities such as thermal insulation, luminescence, and electrochromism, it holds great potential for applications in bio-based composites, optical materials, energy-saving building materials, electronic devices, solar panels, and smart sensors.
[0004] Current research on the functionalization of transparent wood focuses on modifying fillers with polymers and adding nanoparticles, or modifying the surface of transparent wood to impart different functions. Reports on functionalized transparent wood include the preparation of luminescent, magnetic, magnetically luminescent, photochromic, and thermally insulating transparent wood. Surface modification of transparent wood primarily involves coating, etching, and battery assembly. Studies have reported that coating transparent wood with poly(3,4-ethylenedioxythiophene) / poly(styrenesulfonic acid) can successfully fabricate transparent conductive electrodes. These electrochromic devices exhibit a distinct magenta-to-transparent color change at varying voltages, and have great potential for applications in energy conversion and smart windows. Constructing micro- and nanostructures on the surface of transparent wood to impart new functions is a method that is efficient, rapid, controllable, and easy to process. However, reports on this research direction remain limited, and further development of new technologies and products is needed.
[0005] Summary of the Invention
[0006] To address the above issues, one of the objectives of the present invention is to provide a transparent wood surface-embossed optical device. This device uses transparent wood as a substrate and utilizes precise embossing to create micro- and nanostructures on the surface. This device has broad application prospects in optical devices, optical imaging, optoelectronic devices, and other fields.
[0007] In order to achieve the above object, the present invention can adopt the following technical solutions:
[0008] On one hand, the present invention provides a transparent wood surface imprinted optical device, the preparation method of which comprises: cleaning and drying the transparent wood surface, spin-coating PMMA on the substrate surface, and then spin-coating UV curing glue on the PMMA layer; then placing the transparent wood on a surface with a resistivity of 1Ωcm -1 -10Ωcm -1 On a P-doped (100) n-type silicon wafer, a transparent grating array template imprint template is attached to the spin-coated UV adhesive layer and exposed. After the exposure is completed, the soft template is peeled off to obtain a grating structure transparent wood in the UV adhesive layer; repeat the above operation, replace the lattice structure imprint template to prepare a lattice structure transparent wood.
[0009] Another aspect of the present invention provides a use of the transparent wood surface imprinted optical device in the preparation of optical devices or optoelectronic devices.
[0010] Another aspect of the present invention provides an application of a transparent wood surface embossed optical device in optical imaging.
[0011] The present invention provides advantageous effects, including: an optical device imprinted on a transparent wood surface, prepared by impregnation with PMMA, offering advantages over optical devices fabricated by UV-imprinting grating and lattice structures on transparent wood surfaces. Furthermore, under laser irradiation, both structures on the transparent wood substrate produce colored fringes (a phenomenon known as iridescence), also known as structural color. The grating structures on the transparent wood substrate also diffract, with both exhibiting greater diffraction efficiencies than those obtained by imprinting grating and lattice structures on PMMA substrates. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] FIG1 is a schematic diagram of the preparation process of an optical device imprinted on a transparent wood surface according to an embodiment of the present invention; wherein (a) is a flow chart for preparing the transparent wood surface, and (b) is a flow chart for nanoimprinting a grating structure on the transparent wood surface;
[0013] Figure 2 is a characterization diagram of the grating structure on the surface of transparent wood; (a) is a SEM image, and (b) is an AFM image;
[0014] Figure 3 is a characterization diagram of the lattice structure of the transparent wood surface; (a) is a SEM image; (b) is an AFM image;
[0015] Figure 4 shows the light transmittance of the grating and lattice structures on the PMMA surface and the grating and lattice structures on the transparent wood surface;
[0016] Figure 5 shows the reflectivity of the grating and lattice structures on the PMMA surface and the grating and lattice structures on the transparent wood surface;
[0017] FIG6 is a simplified schematic diagram of the diffraction pattern and efficiency device;
[0018] Figure 7 shows the surface structural colors and diffraction patterns of grating structures on PMMA and transparent wood surfaces; (a) is PMMA, and (b) is transparent wood;
[0019] Figure 8 shows the surface structural colors and diffraction patterns of the lattice structures on the surfaces of PMMA (a) and transparent wood (b); (a) is PMMA and (b) is transparent wood;
[0020] Figure 9 shows the diffraction effects of the PMMA surface lattice structure and grating structure, and the transparent wood surface lattice structure and grating structure. DETAILED DESCRIPTION
[0021] The examples are provided to better illustrate the present invention, but are not intended to limit the present invention to the examples. Therefore, non-essential improvements and adjustments to the embodiments made by those skilled in the art based on the above-mentioned invention still fall within the scope of protection of the present invention.
[0022] The terms used herein are only used to describe specific embodiments and are not intended to limit the present disclosure. Unless the context has a significantly different meaning, expressions in the singular include expressions in the plural. As used herein, it should be understood that terms such as "include", "have", "comprise" and the like are intended to indicate the presence of features, numbers, operations, components, parts, elements, materials or combinations. The terms of the present invention are disclosed in the specification and are not intended to exclude the possibility that one or more other features, numbers, operations, components, parts, elements, materials or combinations thereof may exist or may be added. As used herein, " / " may be interpreted as "and" or "or", depending on the circumstances.
[0023] The embodiment of the present invention provides a transparent wood surface imprinted optical device, the preparation method of which includes: cleaning and drying the transparent wood surface, spin-coating PMMA on the substrate surface, and then spin-coating UV curing glue on the PMMA layer; then placing the transparent wood on a surface with a resistivity of 1Ωcm -1 -10Ωcm -1 On a P-doped (100) n-type silicon wafer, a transparent grating array template imprint template is attached to the spin-coated UV adhesive layer and exposed. After the exposure is completed, the soft template is peeled off to obtain a grating structure transparent wood in the UV adhesive layer; repeat the above operation, replace the lattice structure imprint template to prepare a lattice structure transparent wood.
[0024] It should be noted that related studies have reported that micro-nanostructures are constructed on solid wood to achieve thermal stability of light transmission through microstructure construction on the wood surface. The study exposed the cellulose fibril aggregates from the skeleton of the cell wall through the delignification process, and then performed mold replication under wet conditions, and fixed the designed configuration in a dry state, thereby achieving precise replication of fine patterns with sizes ranging from 40nm to 50μm, and a multi-scale structure with nano-sized lines on the surface of a micron hemisphere can be obtained. The study also demonstrated the use of surface-embossed wood as a microlens array (MLA), which showed excellent imaging capabilities and thermal stability even at high temperatures of up to 150°C. However, this material is sensitive to moisture in a humid environment, and the solution causes shrinkage and swelling, resulting in instability of optical properties.
[0025] The present invention uses transparent wood as a substrate and precisely imprints micro-nanostructures onto its surface, thereby producing a transparent wood surface-imprinted optical device. Furthermore, under laser irradiation, the transparent wood surface-imprinted optical device in the embodiments of the present invention produces colored stripes (a phenomenon known as iridescence), also known as structural color, on both structures on the transparent wood substrate. The grating structures on the transparent wood also diffract, and the diffraction efficiency of both is greater than that of grating and lattice structures imprinted on PMMA.
[0026] In some specific embodiments, in the method for preparing the transparent wood surface imprinted optical device, in step (1), the method for removing lignin includes: preparing sodium chlorite into a bleaching solution with a mass fraction of 0.5%-1.5%, adjusting the pH to 4.5-4.7 with glacial acetic acid / acetic acid buffer solution, immersing balsa wood chips in the bleaching solution and cooking at 75°C-85°C to obtain a delignified porous template.
[0027] It should be noted that removing lignin, the component of wood that absorbs visible light, increases the porosity and permeability of the wood cell wall, providing more fluid channels for subsequent resin impregnation. At the same time, the natural wood honeycomb cell wall structure and its original directional arrangement and multi-level assembly structure can still be maintained during the lignin removal process.
[0028] In some specific embodiments, in the method for preparing the transparent wood surface imprinted optical device, in step (2), the vacuum-cyclic impregnation includes: prepolymerizing MMA at 70°C-80°C for 15 minutes using 2,2-azobisisobutyronitrile as an initiator; placing the prepolymerized MMA in an ice-water bath, rapidly cooling it to ambient temperature, and then placing the delignified porous wood; impregnating with the solution under a vacuum pressure range of -0.09 MPa to -0.08 MPa; wrapping the delignified porous wood between two layers of glass slides with aluminum foil, drying, and curing; and peeling the delignified porous wood from the glass to obtain the transparent wood.
[0029] Another embodiment of the present invention provides a use of the above-mentioned transparent wood surface imprinted optical device in the preparation of optoelectronic devices.
[0030] Yet another embodiment of the present invention provides an application of the above-mentioned transparent wood surface imprinting optical device in optical imaging.
[0031] It should be noted that research on functionalizing transparent wood surfaces through nanoimprinting of micro- and nanostructures is currently lacking. This precision-imprinted transparent wood could broaden its application areas, including in optical devices, optical imaging, and optoelectronics. Furthermore, by combining the microstructure and optical advantages of transparent wood, nanoimprinting grating and lattice structures onto its surface could open up new applications for transparent wood in fields such as optics, biology, and electronics.
[0032] In addition, since the grating structure and lattice structure are arranged perpendicular to the direction of the wood fibers, based on the anisotropic fiber-based porous wood structure, if light propagates parallel to the longitudinal and tubular wood cell directions, the resin-filled pores can be regarded as multimode waveguides with relatively high loss; when light is incident from a direction perpendicular to the wood fibers, the incident light diffracts under the obstacle of the nanofibrils, and combined with the micro-nanostructure embossed on the transparent wood surface, the diffraction efficiency is enhanced.
[0033] In order to better understand the present invention, the content of the present invention is further explained below with reference to specific examples, but the content of the present invention is not limited to the following examples.
[0034] 1. Preparation of optical devices embossed on transparent wood surfaces
[0035] Example 1
[0036] According to the process diagram shown in FIG1 , a transparent wood surface imprinted optical device is prepared as follows:
[0037] (1) Sodium chlorite was prepared into a bleaching solution with a mass fraction of 1% (adjusted to pH 4.6 using glacial acetic acid / acetic acid buffer solution); 1 mm thick balsa wood was cut into 30 mm × 20 mm (radial) specifications; the balsa wood chips were immersed in the bleaching solution and steamed at 80°C for 6 h to remove lignin from the wood to obtain delignified wood;
[0038] (2) Methyl methacrylate (MMA) was prepolymerized at 75°C for 15 min using 2,2-azobisisobutyronitrile (0.3 wt%) as an initiator. The prepolymerized MMA was placed in an ice-water bath, rapidly cooled to ambient temperature, and then placed in delignified wood. The delignified balsa wood sample was impregnated with the solution under a vacuum pressure range of -0.09 MPa to -0.08 MPa for 30 min. This was repeated three times to ensure complete impregnation of the polymer. The delignified balsa wood was wrapped with aluminum foil between two glass slides and cured in an oven at 75°C for 4 h. The wood was peeled off from the glass to obtain transparent wood.
[0039] (3) Ultrasonic cleaning of the transparent wood surface with acetone or ethanol, followed by drying with nitrogen; setting the speed of the glue spreader to 3000 rpm, first spin-coating PMMA on the substrate surface, and then spin-coating UV-curable glue (made in the laboratory) on the PMMA layer; placing the transparent wood on a surface with a resistivity of 1-10 Ωcm -1On a P-doped (100) n-type silicon wafer, a transparent imprint template (a regular array template with a diameter of 400 nm and a period of 600 nm) is attached to the spin-coated UV adhesive layer, and the two are placed together in a UV exposure device and exposed in a nitrogen atmosphere for 10 minutes to solidify the UV adhesive. After the exposure is completed, the soft template is peeled off, and a grating structure matching the soft template structure is obtained in the UV adhesive layer; the above operation is repeated, and the imprint template is replaced with a lattice structure to prepare a transparent wood with a lattice structure.
[0040] 2. Characterization of optical devices imprinted on transparent wood surfaces
[0041] Example 2
[0042] The components of the balsa wood, delignified balsa wood, and clear wood in Example 1 were analyzed, and the results are shown in Table 1.
[0043] Table 1 Composition analysis of balsa, delignified balsa and clear wood
[0044] Example 3
[0045] The transparent wood surface grating structure prepared in Example 1 was observed using a scanning electron microscope and an atomic force microscope, respectively. The results are shown in FIG2 , where (a) is a scanning electron microscope image (SEM) and (b) is an atomic force microscope image (AFM).
[0046] The surface lattice structure of the transparent wood prepared in Example 1 was observed using a scanning electron microscope and an atomic force microscope, respectively. The results are shown in FIG3 , where (a) is a scanning electron microscope image (SEM) and (b) is an atomic force microscope image (AFM).
[0047] The PMMA-coated surface grating structure and lattice structure in Example 1 and the transparent wood surface grating structure and lattice structure were tested for light transmittance, and the results are shown in FIG4 .
[0048] The reflectivity test was conducted on the PMMA-coated surface grating structure and lattice structure and the transparent wood surface grating structure and lattice structure in Example 1. The results are shown in FIG5 .
[0049] The surface grating structures coated with PMMA and transparent wood in Example 1 were tested for surface structural color and diffraction pattern with reference to the diffraction pattern and simplified schematic diagram of the efficiency device shown in FIG6 , respectively. The results are shown in FIG7 , where (a) is PMMA and (b) is transparent wood.
[0050] The surface lattice structures of the PMMA-coated and transparent wood in Example 1 were tested for surface structural color and diffraction pattern with reference to the diffraction pattern and the simplified schematic diagram of the efficiency device shown in FIG6 , respectively. The results are shown in FIG8 , where (a) is PMMA and (b) is transparent wood.
[0051] The diffraction effect of the PMMA-coated surface grating structure and lattice structure and the transparent wood surface grating structure and lattice structure in Example 1 was tested, and the results are shown in FIG9 .
[0052] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not limiting. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the purpose and scope of the technical solutions of the present invention, which should all be covered by the scope of the claims of the present invention.
Claims
1. A transparent wood surface embossed optical device, It is characterized in that The preparation method comprises: cleaning and drying the surface of the transparent wood, spin coating PMMA on the substrate surface, and then spin coating UV curing glue on the PMMA layer; and then placing the transparent wood on a surface with a resistivity of 1 cm -1 -10Ωcm -1 On a P-doped (100) n-type silicon wafer, a transparent grating array template imprint template is attached to the spin-coated UV adhesive layer and exposed. After the exposure, the soft template is peeled off to obtain a grating structure transparent wood in the UV adhesive layer; repeat the above operation, replace the lattice structure imprint template to prepare a lattice structure transparent wood.
2. The transparent wood surface embossed optical device according to claim 1, It is characterized in that The preparation method of transparent wood comprises: (1) using balsa wood as raw material and removing lignin to prepare delignified porous wood; (2) preparing transparent wood by vacuum-circulation impregnation of the delignified porous wood.
3. The transparent wood surface embossed optical device according to claim 2, It is characterized in that In step (1), the method for removing lignin comprises: preparing sodium chlorite into a bleaching solution with a mass fraction of 0.5%-1.5%, adjusting the pH to 4.5-4.7 with glacial acetic acid / acetic acid buffer solution, immersing the balsa wood chips in the bleaching solution and cooking at 75°C-85°C to obtain a delignified porous template.
4. The transparent wood surface embossed optical device according to claim 2 or 3, It is characterized in that In step (2), the vacuum-circulation impregnation comprises: prepolymerizing MMA at 70°C-80°C for 15 minutes using 2,2-azobisisobutyronitrile as an initiator; placing the prepolymerized MMA in an ice water bath, rapidly cooling it to ambient temperature, and then placing the delignified porous wood; impregnating the wood with a solution under a vacuum pressure range of -0.09 MPa to -0.08 MPa; wrapping the delignified porous wood between two layers of glass slides with aluminum foil, drying, and curing; and peeling the delignified porous wood from the glass to obtain transparent wood.
5. Use of the transparent wood surface imprinted optical device according to claims 1 to 4 in the preparation of optoelectronic devices.
6. Use of the transparent wood surface imprinting optical device according to claims 1 to 4 in optical imaging.
Citation Information
Patent Citations
Method for preparing orderly gallium nitride nano pillar array with ultraviolet soft imprinting
CN103383980A
Production method of transparent timber
CN106243391A
Preparation method for light-emitting transparent wood
CN108297219A
Manufacturing method for high-flexibility high-elasticity and high-transparency wood film
CN108312281A
Transparent wood composite, systems and method of fabrication
CN108699420A