Resilient ferroelectric, preparation method therefor and use thereof
By adopting a micro-crosslinking network structure with low crosslink density in ferroelectrics, the problem of unrecoverable strain in traditional ferroelectrics is solved, and the combination of high resilience and ferroelectric properties is achieved, which is suitable for wearable devices.
Patent Information
- Application Number
- PCT/CN2023/103014
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2023-06-28
- Publication Date
- 2024-11-21
AI Technical Summary
Traditional ferroelectric bodies are prone to brittle fracture or deformation during strain and cannot recover, which cannot meet the elasticity and ferroelectric requirements of wearable electronic devices. The existing elasticization methods have defects in material interface problems and uneven electric field distribution.
The linear polymer ferroelectric material with low crosslinking density is used to form a micro-crosslinking network structure with crosslinking agent, and connect the ferroelectric domains through covalent bonds to achieve high resilience and flexibility of the ferroelectric body while maintaining excellent ferroelectric properties. .
A ferroelectric body with high resilience, flexibility and ferroelectric properties is obtained, with higher residual polarization strength, thermal stability and shorter switching time, suitable for wearable devices.
Smart Images

Figure CN2023103014_21112024_PF_FP_ABST
Abstract
Description
A resilient ferroelectric and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of ferroelectric materials, and in particular to a resilient ferroelectric and a preparation method and application thereof. Background Art
[0002] Ferroelectrics are widely used due to their spontaneous polarization reversal and excellent electromechanical coupling properties. With the development of wearable and flexible electronic technologies, ferroelectrics need to be elastic in addition to being flexible to better meet the working requirements of devices.
[0003] Traditional ferroelectric materials include oxide ferroelectrics and polyvinylidene fluoride polymer ferroelectrics. Oxide ferroelectrics are prone to brittle fracture and failure when subjected to external strain; polyvinylidene fluoride polymer ferroelectrics have great plasticity and can withstand strains exceeding 500%. However, due to intermolecular slip, their deformation cannot be restored after the stress is removed, making them unable to meet working requirements.
[0004] Commonly used material elasticization methods such as structural engineering or blending will produce many incidental defects. In structural engineering, elastic structures such as islands, folds or snakes that can withstand strain will be used to connect rigid device units to achieve overall elasticization of the device. However, this will cause problems such as modulus mismatch between the elastic structure and the device unit, difficulty in miniaturization and complex preparation process. Blending refers to the physical blending of rigid materials with elastomers to obtain the ability to withstand strain. Physical blending of ferroelectrics and elastomers will not only produce problems with different material interfaces, but also polarization problems. Since the ferroelectric domains of the ferroelectric are randomly oriented after blending, the ferroelectric domains need to be oriented consistently after polarization to obtain better ferroelectric properties.
[0005] The resistivity of the elastomer is much higher than that of the ferroelectric. According to the principle of voltage division in a series circuit, the electric field is primarily distributed on the elastomer, resulting in a relatively low effective electric field for the ferroelectric. To effectively polarize the ferroelectric particles in the composite material, the electric field strength needs to be further increased, but the increased electric field is still mostly distributed on the elastomer. On the other hand, the breakdown field strength of the elastomer is not more than three orders of magnitude higher than the polarization field strength of the ferroelectric, causing the elastomer to break down before the ferroelectric particles are effectively polarized. Furthermore, during the polarization process, the charged ferroelectric particles attract or repel each other. Since the modulus of the inorganic ferroelectric is three to five orders of magnitude higher than that of the elastomer, the ferroelectric particles squeeze the elastomer, causing electromechanical breakdown.
[0006] Chemically crosslinking linear molecules can effectively prevent slippage between molecular chains. However, while the high crosslink density of typical chemical crosslinking improves the modulus, tensile strength, and electrical breakdown strength of the resulting polymer / composite, it also significantly reduces the material's tensile properties and elastic recovery. Consequently, linear ferroelectrics obtained through conventional crosslinking are difficult to use in wearable electronic devices and equipment due to their poor tensile properties, high modulus, and lack of elastic recovery. Therefore, developing a low-modulus, flexible ferroelectric material with high elastic recovery is crucial for the wearable device industry.
[0007] CN105622871A discloses a cross-linked fluoropolymer-based dielectric elastomer composite material and a preparation method thereof. The composite material comprises 60-90 parts of a fluoropolymer matrix, 8-40 parts of a functional cross-linking agent, and 1-3 parts of a catalyst to obtain a fully organic dielectric elastomer composite material with low driving voltage and large electro-deformation. The material exhibits large deformation under low electric fields, but does not possess ferroelectric properties.
[0008] Summary of the Invention
[0009] The present invention addresses the problems of insufficient resilience, irreversible deformation, and inability to rebound of ferroelectric materials, and provides a resilient ferroelectric that can have high resilience while maintaining excellent ferroelectricity and excellent comprehensive performance.
[0010] To achieve the above object, the technical solution adopted by the present invention is:
[0011] A resilient ferroelectric, comprising a ferroelectric material and a cross-linking agent; the mass ratio of the ferroelectric material to the cross-linking agent is 3-50:1;
[0012] The cross-linking density of the resilient ferroelectric is 0.01-20%. The structure of the resilient ferroelectric includes a micro-cross-linking network structure with resilient properties and ferroelectric domains. The ferroelectric domains are connected to the network structure through covalent bonds.
[0013] In some embodiments, according to the reaction formula, the definition of the crosslinking density (ρ) refers to the ratio of the number of crosslinking points (v) to the total repeating units (N0) in the polymer ferroelectric material before crosslinking, that is, ρ = v / N0. For example, in the structure of the crosslinked 1,1-difluoroethylene-trifluoroethylene copolymer P(VDF-TrFE), ρ = v / N0 = (x+y) / (m+n).
[0014] Where m and n represent the ratios of VDF and TrFE repeating units in the P(VDF-TrFE) structure, and x and y represent the ratios of repeating units crosslinked by the crosslinker. Due to the relatively low crosslink density, which is determined by the amount of polymer ferroelectric and crosslinker before crosslinking, this application assumes that the crosslinking reaction with the crosslinker has completely completed.
[0015] In some embodiments, expressed based on the amount of raw materials input, specifically, when the ferroelectric material is P(VDF-TrFE) and the crosslinking agent is an amino compound containing a diamine structure, the crosslink density ρ = 100% × 2(a / M1) / (b / M2), where M1 is the average molecular weight of a single repeating unit in P(VDF-TrFE), M2 is the molecular weight of the crosslinking agent, and a:b is the mass ratio of the crosslinking agent to P(VDF-TrFE).
[0016] The present invention uses a linear polymer ferroelectric material and a crosslinking agent to form a ferroelectric having both a network structure and reversibly reversible ferroelectric domains. The linear polymer ferroelectric material imparts high ferroelectricity to the elastic ferroelectric. The micro-crosslinking forms a network structure with a crosslinking density of 0.1%-20%, which is stable, soft, and elastic, thereby imparting elasticity to the ferroelectric while retaining ferroelectricity. The network structure is formed by the linear polymer ferroelectric material itself, has a designable chemical structure, does not produce performance mismatch problems caused by interfaces between dissimilar materials, and can meet the requirements of miniaturized device sizes. The reversibly reversible ferroelectric domains originate from polar phases in the crystalline regions of the ferroelectric polymer material, giving the resulting ferroelectric excellent resilience and flexibility, as well as higher residual polarization strength, thermal stability, and shorter switching times.
[0017] The ferroelectric material includes a polyvinylidene fluoride ferroelectric material and / or a nylon ferroelectric material. Preferably, the ferroelectric material is a polyvinylidene fluoride ferroelectric material.
[0018] In some embodiments, the polyvinylidene fluoride ferroelectric material includes a copolymer formed by any one or more monomers of vinylidene fluoride, vinyl fluoride, polyvinyl methyl ether, chlorotrifluoroethylene, trifluoroethylene, hexafluoropropylene, tetrafluoroethylene, and chlorofluoroethylene.
[0019] In some embodiments, the polyvinylidene fluoride ferroelectric material includes a self-polymer of 1,1-difluoroethylene, i.e., polyvinylidene fluoride; or, includes a binary, ternary or tetrapolymer formed by 1,1-difluoroethylene and any one of vinyl fluoride, polyvinyl methyl ether, trifluorochloroethylene, trifluoroethylene, hexafluoropropylene, tetrafluoroethylene, and chlorofluoroethylene.
[0020] Further preferably, the ferroelectric material is a copolymer of 1,1-difluoroethylene and trifluoroethylene (P(VDF-TrFE)).
[0021] The cross-linking agent includes any one or more of amino compounds, polyphenol compounds, peroxides, and polythiophenol compounds.
[0022] The amino compound includes but is not limited to any one or more of polyoxyethylene diamine, bis(aminopropyl)-terminated polydimethylsiloxane, and α-ω diamine with an intermediate carbon atom number of 6-30.
[0023] The polyphenol compound includes, but is not limited to, any one or more of hydroquinone, bisphenol A, bisphenol AF, bisphenol-terminated polyethylene glycol, and bisphenol-terminated polydimethylsiloxane.
[0024] The peroxide includes, but is not limited to, any one or more of benzoyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylhexane, 2,5-bis(butylperoxy)-2,5-dimethylhexane, and 1,4-bis-tert-butylperoxyisopropylbenzene.
[0025] In some embodiments, the crosslinking agent is any one or more of polyoxyethylene diamine, bis(3-aminopropyl)-terminated poly(dimethylsiloxane), 1,4-bis(tert-butylperoxyisopropylbenzene), and 1,2-poly(butadiene) oligomer.
[0026] Preferably, in some embodiments, the molecular weight of the polyoxyethylene diamine is 500-5000; the molecular weight of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 1000-5000. These macromolecules can act as cross-linking agents while also acting as plasticizers, thereby reducing the modulus and increasing the resilience, thereby meeting the soft and elastic requirements of wearable devices for materials.
[0027] Further preferably, in some embodiments, the molecular weight of the polyoxyethylene diamine is 1000; the molecular weight of the bis(3-aminopropyl)-terminated poly(dimethylsiloxane) is 2500.
[0028] More preferably, polyoxyethylene diamine with a molecular weight of 1000 is used. The resilient ferroelectric prepared by combining the cross-linking agent with polyvinylidene fluoride has more excellent comprehensive properties of ferroelectric material and resilience.
[0029] In some embodiments, the resilient ferroelectric has a crosslink density of 0.1-20%. Crosslink density refers to the ratio of the number of crosslink points to the number of linear polymer repeating units. Excessively high crosslink density can affect the material's resilience. The inventors discovered that achieving micro-crosslinking within the system is necessary to achieve both resilience and ferroelectricity.
[0030] Preferably, in some embodiments, the crosslink density of the resilient ferroelectric is 0.2-10%, such as 0.4%, 0.5%, 0.6%, 0.8%, 1%, 1.5%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or any value therebetween.
[0031] Further preferably, the cross-linking density of the resilient ferroelectric is 0.3-5%.
[0032] Further preferably, the crosslinking density of the resilient ferroelectric is 0.43-2.16%.
[0033] In some embodiments, the mass ratio of the ferroelectric material to the crosslinking agent is 3-50:1, preferably 8-20:1, such as 5:1, 10:1, 15:1, 20:1, 25:1, 30:1, 35:1, 40:1, 45:1, or any value therebetween.
[0034] Preferably, the mass ratio of the ferroelectric material to the cross-linking agent is 5-35:1, preferably 8-35:1.
[0035] In the present invention, a low dose of cross-linking agent is mixed with the ferroelectric material to achieve micro-cross-linking within the ferroelectric material while maintaining ferroelectricity. However, excessive cross-linking leads to a decrease in the elasticity of the finished product, and a reduction in crystallinity leads to a decrease in remanent polarization and even the disappearance of ferroelectricity.
[0036] Preferably, for a system using polyethylene oxide diamine as a crosslinking agent, the crosslinking density is 0.1-5%. When the crosslinking density exceeds 5%, the elasticity of the material will decrease, and even the ferroelectricity will also decrease.
[0037] The elastic recovery rate of the resilient ferroelectric is 10-400%, the resilience is above 60%, and the residual polarization intensity is 3uC / cm 2 above.
[0038] The elastic recovery rate is defined as the ratio of the length of the sample recovered after the tensile stress is removed to the original length, that is, elastic recovery rate = 100% × (L1-L2) / (L1-L0), where L o L is the original straightened length of the sample when no external force is applied; L1 is the length of the sample after the external force is applied; L2 is the straightened length of the sample after the external force is removed for a certain period of time.
[0039] The present invention also provides a method for preparing the resilient ferroelectric, comprising the steps of: mixing a ferroelectric material and a crosslinking agent and then covalently crosslinking to obtain the resilient ferroelectric; or, mixing a ferroelectric material, a crosslinking agent and an inorganic ferroelectric material and then covalently crosslinking to obtain the resilient ferroelectric.
[0040] The mixing includes any of various methods such as dissolution mixing, melt blending, extrusion, injection molding, etc.;
[0041] In some embodiments, the solvent used in the dissolving and mixing process includes any one or more of N,N-dimethylformamide, cyclohexane, trifluoroacetic acid, cyclohexanone, diethyl carbonate, isophorone, etc. After the dissolving and mixing, the solvent is removed by volatilization or drying.
[0042] In some embodiments, specifically, after dissolving and mixing, the solution is cast into a film, and after most of the solvent is volatilized at room temperature, it is placed in a vacuum oven at 60-80° C. and dried for 4-24 hours.
[0043] The covalent crosslinking includes chemical crosslinking and / or radiation crosslinking.
[0044] The chemical crosslinking includes the steps of: thermally crosslinking the mixture at 100-350°C for more than 1 minute; in some embodiments, the mixture is thermally crosslinked at 200-350°C for more than 30 minutes, such as at 220°C, 240°C, 260°C, 280°C, 300°C, 320°C, and 340°C, and the thermal crosslinking time is more than 40 minutes, more than 1 hour, more than 1.5 hours, more than 2 hours, or more than 2.5 hours.
[0045] The radiation crosslinking comprises the steps of placing the mixture under any one of ultraviolet light, visible light, near infrared light, electrons, neutrons, α particles, β particles, X rays or γ rays for electromagnetic radiation crosslinking.
[0046] In some embodiments, the preparation method further comprises mixing with a co-crosslinking agent.
[0047] In some embodiments, the co-crosslinking agent includes any one or more of 1,2-poly(butadiene) oligomer, di(meth)acrylate-terminated polyethylene glycol, glycerol acrylate, pentaerythritol acrylate, acrylic acid triester, acrylic acid isocyanate, and propyleneoxy triazine.
[0048] The present invention also provides the use of the resilient ferroelectric in wearable devices. The material has excellent softness and high resilience, and is suitable for the preparation of wearable devices with high flexibility and elasticity requirements.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] (1) The present invention mixes a trace amount of cross-linking agent with a ferroelectric material to obtain a ferroelectric having both a resilient network structure and reversible ferroelectric domains. The resulting ferroelectric has excellent resilience and flexibility while having higher residual polarization strength, thermal stability, shorter switching time, and excellent overall performance.
[0051] (2) The ferroelectric of the present invention has excellent resilience, flexibility and ferroelectric properties, and can be used to prepare wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] FIG1 is a schematic diagram of the network structure of the resilient ferroelectric prepared in Example 1 of the present invention.
[0053] FIG2 is an X-ray near-edge absorption spectrum of the resilient ferroelectric prepared in Example 1-2, A is Example 1, and B is Example 2.
[0054] FIG3 is an X-ray photoelectron spectrum of the resilient ferroelectric prepared in Example 1, wherein FIG3 is the full spectrum and FIG3 is the detailed spectrum of nitrogen.
[0055] FIG4 shows stress-strain curves of the resilient ferroelectric prepared in Example 1 and pure P(VDF-TrFE).
[0056] FIG5 is a cyclic stress-strain curve of the resilient ferroelectric prepared in Example 1, and the inset is a cyclic stress-strain curve of a pure P(VDF-TrFE) sample.
[0057] FIG6 shows the fatigue test results of the resilient ferroelectric prepared in Example 1 and commercial fluororubber.
[0058] FIG7 shows the ferroelectric fatigue test results of the resilient ferroelectric prepared in Example 1.
[0059] FIG8 is a dielectric constant-temperature curve of the resilient ferroelectric prepared in Example 1 and pure P(VDF-TrFE).
[0060] FIG9 is a DSC curve of the resilient ferroelectric prepared in Example 1.
[0061] FIG10 is a stress-strain curve of the resilient ferroelectrics with different crosslinking densities prepared in Example 1-2.
[0062] FIG11 shows the crystallinity of the resilient ferroelectrics with different crosslinking densities prepared in Example 1-2.
[0063] FIG12 is a stress-strain curve of the resilient ferroelectric prepared in Example 3.
[0064] FIG13 is a cyclic stress-strain curve of the resilient ferroelectric prepared in Example 3 under 120% tension.
[0065] FIG14 is a PE hysteresis curve of the resilient ferroelectric prepared in Example 3 under 100% tensile strain.
[0066] FIG15 is a cyclic stress-strain curve of the resilient ferroelectric prepared in Example 4 under 100% tensile strain.
[0067] FIG16 is a PE hysteresis curve of the resilient ferroelectric prepared in Example 4 under 80% tensile strain.
[0068] FIG17 is a cyclic stress-strain curve of the resilient ferroelectric prepared in Example 5 under 190% tensile strain.
[0069] FIG18 is a PE hysteresis curve of the resilient ferroelectric prepared in Example 5 under 150% tensile strain.
[0070] FIG19 is a cyclic stress-strain curve of the resilient ferroelectric prepared in Example 6 under 150% tensile strain.
[0071] FIG20 is a PE hysteresis curve of the resilient ferroelectric prepared in Example 6 under 120% tensile strain.
[0072] FIG21 is a schematic diagram of the preparation process of the fully elastic device of Application Example 1.
[0073] FIG22 shows the tensile fatigue test results of the fully elastic device of Application Example 1 under a cyclic strain of 70%.
[0074] FIG23 shows the PE hysteresis curves of the fully elastic device of Application Example 1 under different electric field intensities when the strain is 0.
[0075] FIG24 shows the PE hysteresis curves of the fully elastic device in Application Example 1 at different frequencies.
[0076] FIG25 shows the PE hysteresis curve, saturation polarization intensity curve, remnant polarization intensity curve and coercive field curve of the fully elastic device of Application Example 1 under different tensile strains. DETAILED DESCRIPTION
[0077] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art will make modifications or equivalent substitutions based on understanding the technical solution of the present invention, without departing from the spirit and scope of the technical solution of the present invention, and all should be encompassed within the protection scope of the present invention.
[0078] The raw materials used in the following specific embodiments were purchased from the market, among which the copolymer of 1,1-difluoroethylene and trifluoroethylene P (VDF-TrFE) was purchased from Arkema Piezotech. FC45, in which the molar ratio of VDF and TrFE is 55 / 45 mol%. The crosslink density is calculated as follows:
[0079] The average molecular weight of a single repeating unit in P(VDF-TrFE) is M1, the molecular weight of the crosslinker is M2, the mass ratio of the crosslinker and P(VDF-TrFE) is a:b, and the crosslinking density ρ = 100% × 2(a / M1) / (b / M2).
[0080] The mechanical properties of the materials were tested in accordance with GBT528-2009.
[0081] Example 1
[0082] 0.2 g of P(VDF-TrFE) and 0.02 g of polyoxyethylene diamine (PEG-diamine) with a molecular weight of 1000 Da were dissolved in 1 mL of N,N-dimethylformamide, and the dissolved solution was then cast in a mold to prepare a mixed film.
[0083] After the mixed film evaporated most of the solvent at room temperature, it was placed in a vacuum oven and dried overnight at room temperature. It was then dried at 60°C for 6 hours, then heated to 250°C for crosslinking for 0.5 hours. The resulting film was a 60μm thick elastic ferroelectric, hereinafter referred to as crosslinked P(VDF-TrFE). The mass ratio of ferroelectric material to crosslinker was 10:1, corresponding to a crosslink density of 1.44%. The reaction equation for the crosslinking system is as follows:
[0084] In this cross-linked P(VDF-TrFE), it is assumed that all amino groups are fully cross-linked to form imine bonds, resulting in twice as many cross-linking points as the starting PEG. The ratio n / m of VDF and TrFE in P(VDF-TrFE) is 55 / 45 mol%, and the average molecular weight of the repeating unit is M1 = 0.55 × 64.034 + 0.45 × 82.024 = 72.1295 (VDF molecular weight is 64.034, TrFE molecular weight is 82.024).
[0085] Therefore, when the mass ratio of the crosslinking agent raw materials PEG diamine (molecular weight M1 = 1000) and P(VDF-TrFE) is a:b (1:10 in this embodiment), in the crosslinking system, the crosslinking density ρ = 100% × 2(a / M2 / (b / M1) = 100% × 2 × (1 / 1000) / (10 / 72.1295) = 1.44%.
[0086] The schematic diagram of the network structure of the prepared resilient ferroelectric is shown in Figure 1, where 1 is the ferroelectric domain and 2 is the cross-linking point. The material has excellent resilience, can retract after stretching, and has stable performance.
[0087] The cross-linked P(VDF-TrFE) and PEG-diamine starting materials prepared in Example 1 were subjected to X-ray absorption near-edge spectroscopy (XANES). The results, shown in Figure 2A, show the absence of PEG-diamine peaks in the cross-linked P(VDF-TrFE), indicating that the cross-linking agent, PEG-diamine, was essentially completely reacted. X-ray photoelectron spectroscopy (XPS) scans of both materials are shown in Figure 3. Figure A shows the full spectrum, while Figure B shows the nitrogen element fine spectrum. These results also demonstrate the complete disappearance of the starting diamine peak, indicating complete cross-linking.
[0088] Figure 4 shows the stress-strain curves of cross-linked P(VDF-TrFE)a with a cross-linking density of 1.44% and pure P(VDF-TrFE)b. It can be seen that the elongation at break and modulus of the cross-linked P(VDF-TrFE) are significantly lower than those of pure P(VDF-TrFE), the necking phenomenon disappears, and the stress-strain curve of the cross-linked P(VDF-TrFE) exhibits the mechanical properties characteristics of an elastomer.
[0089] Figure 5 shows the cyclic stress-strain curve of cross-linked P(VDF-TrFE) with a cross-linking density of 1.44%, and the inset is the cyclic stress-strain curve of a pure sample of P(VDF-TrFE). It can be clearly seen that the resilient ferroelectric obtained in this embodiment is an elastic material with obvious resilience. Compared with the cyclic stress-strain curve of P(VDF-TrFE), after ten stretching-unloading cycles and a maximum strain of 125%, the elastic recovery rate can still reach more than 90%, showing good elastic properties.
[0090] The elastic ferroelectric prepared in Example 1 was mixed with commercial fluororubber (Japan Daikin, brand: DAI-EL) TM G-801, whose main component is P(VDF-HFP) elastomer) was subjected to fatigue test comparison, and the results are shown in Figure 6. It can be seen that the resilience of the cross-linked P(VDF-TrFE) in Example 1 is basically comparable to that of commercial elastomers. From the test results, it can be seen that the elastic recovery rate of the cross-linked P(VDF-TrFE) film and the commercial fluoroelastomer film will decrease with the increase in the number of cycles, but tend to be stable after 200 cycles. Compared with the elastic recovery rate of fluororubber after 200 cycles (>80%), the elastic recovery rate of the cross-linked P(VDF-TrFE) is slightly lower (>70%), and the elastic recovery effect is slightly different.
[0091] FIG7 shows the ferroelectric fatigue test results of the resilient ferroelectric prepared in Example 1, indicating that the polarization direction of the ferroelectric domain in the resilient ferroelectric can be flipped more than 5 million times without significant decrease in the remanent polarization intensity.
[0092] Figure 8 shows the comparison results of the dielectric constant changes of cross-linked P(VDF-TrFE) and pure P(VDF-TrFE) with temperature. It can be seen that at 63°C, both of them have a dielectric constant mutation phenomenon, that is, the cross-linked P(VDF-TrFE) film still has the same Curie transition as pure P(VDF-TrFE) and is still a ferroelectric material.
[0093] Figure 9 shows the DSC curve of the prepared cross-linked P(VDF-TrFE), showing obvious glass transition (-20°C), Curie transition (63°C), and crystalline melting peak (153°C), proving that the cross-linked film still has thermal properties similar to those of pure P(VDF-TrFE), and its ferroelectric properties will remain good.
[0094] Example 2
[0095] According to the preparation process parameters of Example 1, the usage of P(VDF-TrFE) and polyoxyethylene diamine with a molecular weight of 1000Da was changed to 100:3, 100:5, 100:8, 100:12, and 100:15, respectively, to obtain crosslinking densities of 0.43%, 0.72%, 1.15%, 1.73%, and 2.16%, respectively. The calculation method of the crosslinking density was the same as in Example 1.
[0096] FIG2B shows the X-ray near-edge absorption spectra (XANES) of cross-linked P(VDF-TrFE) and PEG-diamine raw materials with different cross-linking densities. It can also be seen that in the resilient ferroelectric materials with different cross-linking densities, the cross-linking agent raw materials are basically completely reacted and cross-linking is complete.
[0097] Figure 10 shows the stress-strain curves of P(VDF-TrFE) resilient ferroelectrics with different cross-linking densities. It can be seen that with the increase of cross-linking density, the material modulus continues to decrease. The decrease in modulus is conducive to the realization of elasticity, the yield point disappears, and the material gradually transitions from plastic deformation to elastic deformation.
[0098] Figure 11 shows the crystallinity of P(VDF-TrFE) resilient ferroelectrics with different crosslink densities, as measured by DSC. It can be seen that the crystallinity of crosslinked films decreases with increasing crosslink density. The crystallinity of a ferroelectric film significantly determines its polarization strength. Increasing crosslink density strengthens the crosslinking network's effect on crystal refinement and disrupts the ordered arrangement of molecular chains, resulting in a decrease in crystallinity. Therefore, an appropriate crosslink density is required to achieve a balance between elasticity and ferroelectricity.
[0099] Example 3
[0100] 1 g of P(VDF-TrFE) and 0.3 g of bis(3-aminopropyl)-terminated poly(dimethylsiloxane) with a molecular weight of 2500 Da were dissolved in 3 mL of cyclohexane. The mass ratio of ferroelectric material to crosslinker was 10:3, corresponding to a crosslinking density of 3%. The dissolved solution was then spin-coated on a conductive substrate to prepare a hybrid film.
[0101] After most of the solvent in the mixed film evaporated at room temperature, it was placed in a vacuum oven and dried at room temperature overnight. It was then dried at 60°C for 6 hours, then heated to 250°C for cross-linking for 0.5 hours, and then cooled to room temperature to obtain an elastic ferroelectric with a thickness of 1 μm.
[0102] Figures 12-14 are the test curves of the resilient ferroelectric obtained in Example 3, Figure 12 is the stress-strain curve; Figure 13 is the cyclic stress-strain curve under 120% tensile strain, and Figure 14 is the PE hysteresis curve under 100% tensile strain. It can be seen that the elastic ferroelectric material still has good ferroelectric properties under large strain.
[0103] Example 4
[0104] 15 g of 1,1-difluoroethylene-trifluoroethylene copolymer and 0.3 g of 1,4-di-tert-butylperoxyisopropylbenzene were mixed and added into an injection molding extruder, and then passed through different molds and fixtures to obtain a block mixture.
[0105] The mixture was placed in a vacuum oven and cross-linked at 320° C. for 1 hour, and then cooled to room temperature. The mass ratio of the ferroelectric material to the cross-linking agent was 50:1, and an elastic ferroelectric with a cross-linking density of 2% was obtained.
[0106] Figures 15-16 are the test curves of the resilient ferroelectric obtained in Example 4. Figure 15 is the cyclic stress-strain curve of the resilient ferroelectric under 100% tensile strain; Figure 16 is the PE hysteresis curve under 80% tensile strain. It can be seen that the elastic ferroelectric material still has good ferroelectric properties under large strain.
[0107] Example 5
[0108] 2 g of a copolymer of 1,1-difluoroethylene-trifluoroethylene-chlorotrifluoroethylene and 0.3 g of 1,4-bis-tert-butylperoxyisopropylbenzene were dissolved in 4 mL of cyclohexanone, and the dissolved solution was cast in a mold to prepare a mixed film.
[0109] After most of the solvent in the mixed film evaporated at room temperature, it was placed in a vacuum oven and dried at room temperature overnight. It was then dried at 60°C for 6 hours, then heated to 250°C for cross-linking for 0.5 hours, and then cooled to room temperature. The mass ratio of ferroelectric material to cross-linking agent was 20:3, and an elastic ferroelectric with a cross-linking density of 10% and a thickness of 32 μm was obtained.
[0110] Figures 17-18 are the test curves of the resilient ferroelectric obtained in Example 5, Figure 17 is the cyclic stress-strain curve under 190% tensile strain, and Figure 18 is the PE hysteresis curve under 150% tensile strain. It can be seen that the elastic ferroelectric material still has good ferroelectric properties under large strain and is a relaxor ferroelectric material.
[0111] Example 6
[0112] 3 g of nylon-5 copolymer and 0.3 g of 1,4-bis-tert-butylperoxyisopropylbenzene were dissolved in 6 mL of a mixed solvent of trifluoroacetic acid and acetone (molar ratio of 6:4), and then the dissolved solution was cast in a mold to prepare a mixed film.
[0113] After most of the solvent in the mixed film evaporated at room temperature, it was placed in a vacuum oven and dried at room temperature overnight. It was then dried at 60°C for 6 hours, then heated to 220°C for cross-linking for 0.5 hours, and then cooled to room temperature. The mass ratio of ferroelectric material to cross-linking agent was 7.5:1, and an elastic ferroelectric with a cross-linking density of 3% and a thickness of 80 μm was obtained.
[0114] Figures 19-20 are test curves of the elastic ferroelectric obtained in Example 6. Figure 19 is a cyclic stress-strain curve under 150% tensile strain, and Figure 20 is a PE hysteresis curve under 120% tensile strain. It can be seen that the elastic ferroelectric material obtained from cross-linked nylon also has good ferroelectric properties under large strain.
[0115] Comparative Example 1: No crosslinking agent was added and no crosslinking step was performed
[0116] 0.2 g of polyvinylidene fluoride was dissolved in 1 mL of N,N-dimethylformamide, and then the dissolved solution was cast in a mold to prepare an organic film.
[0117] After most of the solvent in the organic film was evaporated at room temperature, it was placed in a vacuum oven and dried at room temperature overnight. It was then dried at 60° C. for 6 hours and then cooled to room temperature to obtain a ferroelectric with a thickness of 60 μm.
[0118] Comparative Example 2
[0119] 0.2 g of 1,1-difluoroethylene-trifluoroethylene and 0.003 g of polyoxyethylene diamine with a molecular weight of 1000 Da were dissolved in 1 mL of N,N-dimethylformamide, and then the dissolved solution was cast in a mold to prepare a mixed film.
[0120] After most of the solvent in the mixed film was evaporated at room temperature, it was placed in a vacuum oven and dried at room temperature overnight. It was then dried at 60°C for 6 hours, then heated to 250°C for cross-linking for 0.5 hours, and then cooled to room temperature. The mass ratio of ferroelectric material to cross-linker was 66.7:1, and an elastic ferroelectric with a cross-linking density of 0.1% and a thickness of 60 μm was obtained. Its stress-strain curve still had a yield point, indicating that due to the low cross-linking density, it still exhibited soft plastic deformation rather than elastic deformation.
[0121] Comparative Example 3
[0122] 0.2 g of polyvinylidene fluoride and 0.4 g of polyoxyethylene diamine with a molecular weight of 1000 Da were dissolved in 1 mL of N,N-dimethylformamide, and then the dissolved solution was cast in a mold to prepare a mixed film.
[0123] After most of the solvent in the mixed film evaporated at room temperature, it was placed in a vacuum oven and dried at room temperature overnight. It was then dried at 60°C for 6 hours, then heated to 250°C for cross-linking for 0.5 hours, and then cooled to room temperature. The mass ratio of ferroelectric material to cross-linking agent was 0.5:1, and an elastic ferroelectric with a cross-linking density of 40% and a thickness of 60 μm was obtained. Its stress modulus increased to 300 MPa and the yield strain was 3%, showing typical hard plastic deformation characteristics.
[0124] The ferroelectrics prepared in Examples 1, 3-6, and Comparative Examples 1-3 were cut into rectangular strips and subjected to mechanical property testing. The test results are shown in Table 1. For tensile strain, the ferroelectric films were tested according to GBT528-2009, cut to standard size, and then tested on a universal material testing machine. The saturation polarization, remnant polarization, and coercive electric field data were obtained using a Premiere II instrument manufactured by Radiant (USA). Test conditions were: At room temperature, force was applied to the polymer film in increments of 20 and 40 MV / m, over a frequency range of 0.05 to 10 kHz.
[0125] Table 1 Performance data of Examples 1, 3-6 and Comparative Examples 1-3
[0126] Application Examples
[0127] Hysteresis loop: Electrodes are plated on both sides of the ferroelectric film, and then a Sawyer-Tower circuit is used to test the hysteresis loop. As shown in Figure 21, the preparation process of the fully elastic device specifically includes: spin-coating a 5% dextran solution on a silicon wafer. After the solvent evaporates, a mixed solution of 1,1-difluoroethylene-trifluoroethylene copolymer (number average molecular weight 240,000, purchased from Piezotech, France) and polyoxyethylene diamine (molecular weight 1000) (mass ratio 10:1) is spin-coated on the dextran. After the solvent evaporates completely in a vacuum, the mixture is cross-linked at 240°C for 1 hour under vacuum to obtain a cross-linked polymer layer. A layer of liquid gallium is then applied to the cross-linked polymer layer using a mask. A layer of polydimethylsiloxane is then solidified on the liquid gallium. The dextran is then dissolved and removed with water. Finally, another layer of liquid gallium is applied to the other side of the cross-linked polymer layer, perpendicular to the upper layer of liquid gallium, to obtain the fully elastic device.
[0128] The fully elastic device was subjected to a tensile fatigue test under a cyclic strain of 70%. As shown in FIG22 , the fully elastic device still had a recovery rate of more than 70% after more than eight million stretching cycles.
[0129] Figure 23 shows the PE hysteresis curves of the fully elastic device at different electric field intensities when the strain is 0, where s is the PE hysteresis curve when the electric field intensity is 40 MV / m, t is the PE hysteresis curve when the electric field intensity is 80 MV / m, u is the PE hysteresis curve when the electric field intensity is 119 MV / m, v is the PE hysteresis curve when the electric field intensity is 160 MV / m, w is the PE hysteresis curve when the electric field intensity is 178 MV / m, x is the PE hysteresis curve when the electric field intensity is 198 MV / m, y is the PE hysteresis curve when the electric field intensity is 218 MV / m, and z is the PE hysteresis curve when the field intensity is 240 MV / m;
[0130] FIG24 shows the PE hysteresis curves of the fully elastic device at different frequencies, where j is the PE hysteresis curve at 100 Hz, k is the PE hysteresis curve at 200 Hz, m is the PE hysteresis curve at 500 Hz, n is the PE hysteresis curve at 1000 Hz, p is the PE hysteresis curve at 2000 Hz, q is the PE hysteresis curve at 5000 Hz, and r is the PE hysteresis curve at 10000 Hz.
[0131] Figure 25 shows the PE hysteresis curve, saturation polarization intensity curve, residual polarization intensity curve and coercive field curve of the fully elastic device under different tensile strains, where A is the PE hysteresis curve at 0% tensile strain, B is the PE hysteresis curve at 5% tensile strain, C is the PE hysteresis curve at 10% tensile strain, D is the PE hysteresis curve at 20% tensile strain, E is the PE hysteresis curve at 30% tensile strain, F is the PE hysteresis curve at 40% tensile strain, G is the PE hysteresis curve at 50% tensile strain, H is the PE hysteresis curve at 60% tensile strain, J is the PE hysteresis curve at 70% tensile strain, K is the curve of coercive field changing with strain, L is the curve of saturation polarization intensity changing with strain, and M is the curve of residual polarization intensity changing with strain.
[0132] It can be seen from the above that the fully elastic device obtained in this test example can still maintain good elasticity at a cyclic tensile strain of 125%. As the frequency increases, the saturation polarization intensity and remnant polarization intensity of the fully elastic device decrease.
[0133] In summary, it can be seen that the elastic ferroelectric with a network structure prepared by the present invention can have high elasticity while having good ferroelectric properties. Specifically, the increase in the amount of cross-linking agent leads to an increase in the cross-linking density, which gradually changes from plastic deformation to elastic deformation, and at the same time, the ferroelectricity is slightly reduced. In Comparative Example 1, since no cross-linking agent was added, there are no cross-linking points in the product, and the product is still plastic deformation with a clear yield point; the cross-linking density in Comparative Example 2 is still relatively low, which is plastic deformation; the cross-linking density in Comparative Example 3 is too high, resulting in a significant increase in modulus and strength, a clear yield point, a decrease in elongation at break, and a drastic decrease in ferroelectricity due to too low crystallinity.
Claims
1. A resilient ferroelectric, It is characterized in that The resilient ferroelectric comprises a ferroelectric material and a cross-linking agent, and its structure comprises a micro-cross-linked network structure having resilient properties; The mass ratio of the ferroelectric material to the cross-linking agent is 3-50:1; and the cross-linking density of the resilient ferroelectric is 0.01-20%.
2. The resilient ferroelectric according to claim 1, It is characterized in that The ferroelectric material includes polyvinylidene fluoride ferroelectric material and / or nylon ferroelectric material; And / or, the cross-linking agent includes any one or more of amino compounds, polyphenol compounds, peroxides, and polythiophenol compounds.
3. The resilient ferroelectric according to claim 2, It is characterized in that The polyvinylidene fluoride ferroelectric material includes a copolymer formed by any one or more monomers of vinylidene fluoride, vinyl fluoride, polyvinyl methyl ether, chlorotrifluoroethylene, trifluoroethylene, hexafluoropropylene, tetrafluoroethylene, and chlorofluoroethylene.
4. The resilient ferroelectric according to claim 1, It is characterized in that The elastic strain of the resilient ferroelectric is 5-400%, and the number of tensile strain cycles is 10 6 above.
5. A method for preparing a resilient ferroelectric according to any one of claims 1 to 4, It is characterized in that The method comprises the following steps: dissolving and mixing a ferroelectric material and a cross-linking agent, and then covalently cross-linking the mixture to obtain the resilient ferroelectric.
6. The method for preparing the resilient ferroelectric according to claim 5, It is characterized in that The covalent crosslinking includes chemical crosslinking and / or radiation crosslinking.
7. The method for preparing a resilient ferroelectric according to claim 6, wherein the chemical crosslinking comprises the steps of: thermally crosslinking the mixture at 100-350°C for more than 1 minute; The radiation crosslinking comprises the steps of placing the mixture under any environment of ultraviolet light, visible light, near infrared light, electrons, neutrons, α particles, β particles, X-rays or γ rays for electromagnetic radiation crosslinking.
8. The method for preparing the resilient ferroelectric according to claim 5, It is characterized in that A co-crosslinking agent is also included in the mixture.
9. The method for preparing the resilient ferroelectric according to claim 8, It is characterized in that The co-crosslinking agent includes any one or more of 1,2-poly (butadiene) oligomer, di (meth) acrylate-terminated polyethylene glycol, glyceryl acrylate, pentaerythritol acrylate, triester phosphate acrylate, acrylate isocyanate, propyleneoxy triazine, polyamino compounds, polyphenol compounds, and polythiol compounds.
10. Use of the resilient ferroelectric according to any one of claims 1 to 4 in a wearable device.
Citation Information
Patent Citations
Crosslinked fluorine polymer based dielectric elastomer compound material and preparation method therefor
CN105622871A
Method for preparing cross-linked fluorinated polymer film
CN111094368A
Crosslinkable electroactive fluorinated polymers comprising photoactive groups
CN113423740A
Method for patterning a ferroelectric polymer layer
US20070166838A1
Polymer and polymer actuator comprising the same
US20100201227A1
Cited By
Polyvinylidene fluoride film based on cross-linking reaction, preparation method and application
CN120082086A