Preparation method for tissue repair membrane, and tissue repair membrane prepared therefrom

By controlling the spinning current and crosslinking degree, the problem of uneven thickness and fiber diameter of the electrospinning film is solved, and an electrospinning film suitable for endometrial repair is prepared, achieving effective repair and growth promotion of the endometrium.

WO2024234497A1PCT designated stage expired Publication Date: 2024-11-21NEO MODULUS (SUZHOU) MEDICAL SCI TECH CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/115236
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2023-08-28
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In the prior art, when preparing endometrial repair membranes, the fiber diameter of the electrospun film is uneven, the thickness is uneven, and the repeatability is poor, making it difficult to ensure that the thickness and fiber diameter of each spinning film are consistent, which affects the repair effect.

Method used

By controlling the spinning current in the range of 0.01mA to 0.4mA, the current time integral value changes regularly within the range of 1C to 9C, including the constant current and linear change periods, ensuring the stability and consistency of the spinning current, and The spinning solution is formed by mixing polymer materials and crosslinking agents in real time, and the crosslinking degree is controlled between 30% and 60% to improve the elastic modulus of the film.

Benefits of technology

An electrospun film with uniform thickness and uniform fiber diameter is prepared, which has good flexibility and compliance, can effectively avoid adhesions and scar re-formation, promote the repair and growth of the endometrium, and is suitable for the natural repair of the endometrium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023115236_21112024_PF_FP_ABST
    Figure CN2023115236_21112024_PF_FP_ABST
Patent Text Reader

Abstract

A preparation method for an endometrial repair membrane. The method comprises: conveying a spinning solution to a spinning electrode of an electrostatic spinning device to perform spinning, so as to form an endometrial repair membrane, wherein within the spinning duration, a spinning current is controlled to change according to a rule, the spinning current is controlled to be within the range of 0.01-0.4 mA, and the time integral value of the spinning current is controlled to be within the range of 1-9 C. An endometrial repair membrane prepared from the method has uniform thickness, and the standard deviation (STDEV) of the thickness is less than 0.02.
Need to check novelty before this filing date? Find Prior Art

Description

Preparation method of tissue repair membrane and tissue repair membrane prepared therefrom

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit and priority of Chinese patent application No. 202310537891.3 filed on May 15, 2023, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present invention relates to the field of medical biomaterials, and in particular to a method for preparing a tissue repair membrane and the prepared tissue repair membrane. Background Art

[0004] Research data shows that uterine-related pathology is a significant factor in infertility among women of childbearing age, with the rate of infertility due to uterine cavity problems ranging from 7.8% to 34.9%. While current assisted reproductive technologies can address infertility caused by factors including fallopian tube, ovarian, and endocrine factors, they still cannot fully address infertility caused by uterine factors. For example, intrauterine adhesions (IUA) are a common cause of infertility in my country. Research indicates that the incidence of IUA after abortion can reach 15% to 40%, resulting in low post-abortion pregnancy rates.

[0005] At present, the main clinical methods used at home and abroad to solve the fibrotic scar tissue formed during the repair of the damaged uterus include the use of intrauterine devices, uterine support balloons, and biological glue (including sodium hyaluronate and chitosan, etc.) after adhesion separation surgery. The above methods mainly rely on the physical barrier effect to prevent the formation of adhesions, but are not helpful for the functional regeneration of damaged uterine tissue. There are also defects such as tissue ischemic necrosis caused by incarceration, infection, and compression, and the residence time in the uterine cavity is too short to maintain the completion of tissue repair.

[0006] In recent years, with the development of tissue engineering, implants prepared by electrospinning have also begun to be used in the field of uterine repair. Implants prepared in this way usually have good biocompatibility and can promote endometrial wound repair.

[0007] However, since high voltage is required to pull the charged solution during electrospinning, a fixed voltage is usually used to pull the charged solution. The viscosity, crosslinking degree, and voltage of the solution will affect the morphology of the final fiber, resulting in uneven fiber diameter and thickness of the electrospun membrane. For thin electrospun membranes, it is particularly difficult to obtain an electrospun membrane with uniform thickness and fiber diameter. In addition, the existing preparation methods are not reproducible. When spinning multiple times, using the same spinning solution and spinning conditions, it is difficult to ensure that the spun membranes produced each time have similar and uniform thickness.

[0008] Summary of the Invention

[0009] In view of the above-mentioned problems existing in the electrospun membrane used to repair the endometrium in the prior art, the present invention aims to provide a method for preparing a thin electrospun membrane (tissue repair membrane, i.e., endometrial repair membrane) with uniform thickness.

[0010] On the one hand, the present invention provides a method for preparing an endometrial repair membrane, comprising: transporting a spinning solution to a spinning electrode of an electrospinning device for spinning to form an endometrial repair membrane, wherein, during the spinning time, the spinning current is controlled to change regularly, and the spinning current is controlled to be in the range of 0.01 mA to 0.4 mA, and the time integral value of the spinning current is controlled to be in the range of 1C to 9C.

[0011] In some embodiments, the spinning duration includes at least one constant current period, during which the spinning current remains constant.

[0012] In some embodiments, the spinning duration includes at least one current linear variation period, and during the at least one current linear variation period, the spinning current changes linearly with time.

[0013] In some specific embodiments, the at least one constant current period includes a first constant current period and a second constant current period, wherein the spinning current is maintained at a first constant current value during the first constant current period and maintained at a second constant current value during the second constant current period, the second constant current value being greater than the first constant current value; and the at least one linear current variation period includes a first linear current variation period, wherein the starting current of the first linear current variation period is the first constant current value and the ending current is the second constant current value. For example, the first constant current period lasts from 40 minutes to 60 minutes, the second constant current period lasts from 40 minutes to 120 minutes, and the first linear current variation period lasts from 180 minutes to 240 minutes, the first constant current value is 0.02 mA to 0.2 mA, the second constant current value is 0.02 mA to 0.4 mA, and the linear variation rate of the spinning current during the first linear current variation period is 0 to 0.1 mA / min.

[0014] In some specific embodiments, the at least one constant current period includes a first constant current period, during which the spinning current is maintained at a first constant current value; and the at least one linear current variation period includes a first linear current variation period, during which the starting current of the first linear current variation period is the first constant current value and the ending current is greater than the starting current. For example, the first constant current period lasts from 40 minutes to 60 minutes, the first linear current variation period lasts from 180 minutes to 240 minutes, the first constant current value is from 0.02 mA to 0.2 mA, the ending current is from 0.02 mA to 0.4 mA, and the linear variation rate of the spinning current during the first linear current variation period is from 0 to 0.1 mA / min.

[0015] In some embodiments, the spinning current is controlled to be in the range of 0.02 mA to 0.4 mA during the spinning time, and the time-integrated value of the spinning current during the spinning time is in the range of 2.6C to 6C.

[0016] In some embodiments, the endometrial repair membrane has a thickness of 0.01 to 10 mm, and a thickness standard deviation of less than 0.02.

[0017] In some embodiments, the spinning solution is formed as follows: a solution of a polymer material is transported through a first liquid supply pipe, a crosslinker solution is transported through a second liquid supply pipe, and the solution of the polymer material and the crosslinker solution are mixed in real time at the downstream intersection of the first liquid supply pipe and the second liquid supply pipe to form the spinning solution.

[0018] In some embodiments, the preparation method further comprises: controlling the cross-linking degree of the endometrial repair membrane to be within the range of 30% to 60%, so that the Young's modulus of a single filament of the formed endometrial repair membrane is greater than 0.5 kPa.

[0019] In some embodiments, the cross-linking degree of the endometrial repair membrane is controlled by controlling the content of the cross-linking agent.

[0020] In another aspect, the present invention provides an endometrial repair membrane prepared according to the above preparation method.

[0021] Compared with the prior art, the present invention has the following beneficial technical effects:

[0022] The method for preparing an endometrial repair membrane of the present invention controls the spinning current to change regularly, controls the spinning current to be in the range of 0.01 mA to 0.4 mA during the spinning time, and controls the time integral value of the spinning current during the spinning time to be in the range of 1C to 9C. The thickness of the endometrial repair membrane prepared by this method is uniform, and the standard deviation (STDEV) of the thickness of the prepared membrane is less than 0.02.

[0023] Furthermore, the preparation method of the present invention is reproducible. Because the current is controlled to vary regularly, and the current value and integral value remain the same for each spinning operation, when thin membranes are prepared through multiple spinning cycles, the standard deviation (STDEV) of the average thickness of multiple membranes is very small, only about 0.01. This avoids the drawback of large fluctuations in membrane thickness when spinning at a fixed spinning voltage in the prior art.

[0024] In addition, the present invention can also improve the elastic modulus of the membrane by further controlling the cross-linking degree of the membrane, so that the Young's modulus of a single fiber reaches above 0.5 kPa. The endometrial repair membrane prepared in this way has good flexibility and compliance, and is soft in texture.

[0025] Therefore, according to the method of the present invention, a thin electrospun membrane with uniform thickness, good flexibility and compliance can be prepared. When used to repair damaged endometrium, the degradation time in the body is moderate, which meets the requirements of the endometrial repair time and the female physiological cycle; it can be deformed according to the shape of the uterine cavity, and can fully meet the needs of different uterine shapes during use, and fully fit the inner wall of the uterus; it can effectively avoid the re-formation of adhesions and scars, thereby allowing the uterus to restore its normal physiological function.

[0026] In addition, due to the control of the spinning current, the fiber diameter of the membrane of the present invention ranges from 100 nm to 600 nm, and such a fiber diameter range can also be more suitable for the growth of endometrial cells.

[0027] In addition, the raw materials of the electrospinning membrane of the present invention are natural protein materials and artificial synthetic materials, including gelatin, collagen and related derivatives, artificially synthesized recombinant collagen, etc. The obtained electrospinning membrane (endometrial repair membrane) has a microscopic multi-layer structure, which is conducive to cells invading the nanofiber membrane from multiple dimensions and climbing and growing along the fiber direction, realizing 3D cell proliferation, promoting wound repair, and shortening wound repair time. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] FIG1 is a curve showing the change of spinning current over time in the method for preparing endometrial repair membrane according to Example 1, Example 2 and Example 3 of the present invention.

[0029] FIG2 is a curve showing the change of spinning current over time in the method for preparing endometrial repair membrane according to Example 4 and Example 5 of the present invention.

[0030] FIG3 is a scanning electron microscope image of the endometrial repair membrane sample 1-1 according to Example 1 of the present invention.

[0031] FIG4 is a scanning electron microscope image of the endometrial repair membrane sample 4-1 according to Example 4 of the present invention.

[0032] FIG5 is a scanning electron microscope image of the endometrial repair membrane sample 9-1 according to a comparative example of the present invention.

[0033] FIG6 is a staining diagram of a tissue section of KLE cells cultured using the endometrial repair membrane sample 1-1 of Example 1 of the present invention.

[0034] FIG. 7 is a staining diagram of a tissue section of KLE cells cultured using the endometrial repair membrane sample 6 of Example 6 of the present invention.

[0035] FIG8 is a staining diagram of a tissue section of KLE cells cultured using the endometrial repair membrane sample 7 of Example 6 of the present invention.

[0036] FIG9 is a stained image of a tissue section of the endometrial repair membrane sample 1-1 according to Example 1 of the present invention 30 days after implantation into the uterus of a rabbit.

[0037] Figure 10 is a photograph of the endometrial status before surgery in a patient with intrauterine adhesions.

[0038] FIG11 is a photograph of the endometrium status 30 days after the endometrial repair membrane sample 1-1 according to Example 1 of the present invention was implanted into the patient's body.

[0039] FIG12 is a stained photograph of an electrospun membrane section 3 days after the endometrial repair membrane sample 1-1 according to Example 1 of the present invention was implanted into a patient's body. DETAILED DESCRIPTION

[0040] The various aspects of the present invention are described in detail below with reference to the accompanying drawings and specific embodiments. It should be understood by those skilled in the art that the various exemplary embodiments described below are only for illustration and do not constitute any limitation on the scope of protection of the present invention.

[0041] In an exemplary embodiment of the present invention, the spinning solution is spun into a fiber membrane material by an electrospinning device. In order to obtain an electrospinning membrane with uniform thickness, the spinning current is controlled to change regularly during the spinning time, and the time integral value of the spinning current during the spinning time is adjusted in real time to be maintained in the range of 1C to 9C, for example, in the range of 2.6C to 6C, and the spinning current is controlled in real time to always be in the range of 0.01 to 0.4 mA.

[0042] In some specific embodiments, the control of the spinning current can be achieved by adjusting the spinning voltage. The spinning voltage range is 45 to 60 kV, and the total spinning time is 250 min to 380 min. The spinning current is controlled to change with time by adjusting the spinning voltage to achieve the required spinning current time integral value of 1 to 9 C (for example, 2.6 to 6 C), and to ensure that the current is always in the range of 0.01 to 0.4 mA, for example, in the range of 0.02 to 0.4 mA.

[0043] In some specific embodiments, the spinning time can be divided into several time periods, and each time period is controlled so that the current changes regularly.

[0044] For example, the spinning time may include at least one constant current period, during which the spinning current remains constant. The spinning time may also include at least one linear current variation period, during which the spinning current varies linearly with time.

[0045] In some specific embodiments, the at least one constant current period includes a first constant current period and a second constant current period, wherein the spinning current is maintained at a first constant current value during the first constant current period and maintained at a second constant current value during the second constant current period; and the at least one linear current variation period includes a first linear current variation period, wherein the starting current of the first linear current variation period is the first constant current value and the ending current is the second constant current value, wherein the second constant current value is greater than the first constant current value. For example, the spinning duration is sequentially composed of the first constant current period, the first linear current variation period, and the second constant current period, wherein the first constant current value is in the range of 0.02-0.2 mA, the second constant current value is in the range of 0.02-0.4 mA, and the spinning current increases from the first constant current value to the second constant current value at an increasing rate of 0.001 mA / min (the increasing rate may be 0.001 mA / min or any value in the range of 0-0.1 mA / min). The first constant current period lasts 40 minutes to 60 minutes; the first current linear change period lasts 180 minutes to 240 minutes; and the second constant current period lasts 40 minutes to 120 minutes.

[0046] In an optional embodiment, the spinning time may only include the first constant current period and the first current linear change period. For example, the spinning time is composed of the first constant current period and the first current linear change period in sequence. Among them, the initial first constant current value is in the range of 0.02 to 0.2 mA, the second constant current value is in the range of 0.02 to 0.4 mA, and the spinning current increases from the first constant current value to the termination current at a growth rate of 0.001 mA / min (the growth rate can be 0.001 mA / min or any value in the range of 0 to 0.1 mA / min). The first constant current period takes 40 minutes to 60 minutes; the first linear current change period takes 180 minutes to 240 minutes.

[0047] In an alternative embodiment, the spinning time may consist of a plurality of constant current periods and a plurality of linear current variation periods, or may include only constant current periods or only linear current variation periods. Within the linear current variation periods, the spinning current may increase or decrease at different rates.

[0048] The endometrial repair membrane (electrospinning membrane) prepared according to embodiments of the present invention can be prepared to a thickness of 0.01 to 10 mm, for example, 0.20 to 0.25 mm, with a thickness standard deviation (STDEV) of less than 0.02. Furthermore, when repeated preparations were performed using the same current variation pattern, the same current-time integral value, and the same current value, the average thickness standard deviation (STDEV) of the resulting multiple membranes was only 0.01.

[0049] The fiber diameter of the endometrial repair membrane thus prepared ranges from 100 nm to 500 nm, for example, from 200 nm to 400 nm, and is a thin electrospun membrane with uniform thickness.

[0050] In order to improve the elastic modulus, the present invention can further control the cross-linking degree of the membrane to be in the range of 10% to 90% (eg, 30% to 60%), so that the Young's modulus of a single filament of the formed endometrial repair membrane is greater than 0.5 kPa.

[0051] The spinning solution in the present invention can be formed by real-time mixing of a polymer solution and a crosslinking agent solution, wherein the polymer material can be one or more of collagen, elastin, proteoglycan, gelatin and its derivatives. Specifically, the polymer solution is transported by a first liquid supply pipe, and the preparation method of the polymer solution is as follows: one or more of purified water, acetic acid, ethyl acetate, PBS buffer, and ethanol are mixed to form a lysate, one or more of collagen, elastin, proteoglycan, gelatin and its derivatives are mixed and added to the configured lysate, structural protein and its derivatives are mixed and dissolved with a mixed solvent in a mass ratio of 1:3 to 1:12, and stirred until the polymer material is completely dissolved. The crosslinking agent solution is transported by a second liquid supply pipe, and the crosslinking agent solution is mixed and configured by one or more of glutaraldehyde aqueous solution, glyoxal aqueous solution, EDC (1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride), and NHS (N-hydroxysuccinimide). The liquid flow rate ratio in the first liquid supply pipe and the second liquid supply pipe can be adjusted according to the crosslinking agent addition ratio. The first liquid supply pipe and the second liquid supply pipe merge at the tail end, so that the polymer material solution and the cross-linking agent solution are evenly mixed to form a spinning solution, and then the spinning solution is transported to the spinning electrode of the electrospinning device for spinning.

[0052] Because the polymer solution and crosslinker solution are mixed in real time, the degree of crosslinking in the membrane can be controlled by adjusting the crosslinker content. For example, the polymer solution is a gelatin solution with a concentration of 16.7%, and the crosslinker solution is a glyoxal solution with a concentration of 10%, so that the crosslinker accounts for 15% by weight of the spinning solution.

[0053] During the electrospinning process, spinning may include needleless spinning, single-needle spinning, and multi-needle spinning. The receiving device includes a rotating collecting core shaft, a flat collecting plate, and a reel. The distance between the spinning nozzle and the receiving device ranges from 50 to 600 mm. The flow rate of the spinning solution ranges from 1 to 20 ml / hr, and the spinning current is controlled as described above.

[0054] In order to further increase the degree of cross-linking, the membrane obtained by spinning can also be subjected to high-temperature treatment to remove residual solvent. The temperature range of high-temperature treatment in the oven is 50 to 160°C and the time range is 2 to 10 hours.

[0055] The prepared electrospun membrane (endometrial repair membrane) can be sterilized by dry heat sterilization, high-pressure steam sterilization, hydrogen peroxide plasma sterilization, ethylene oxide sterilization or irradiation sterilization, or sterilized by gradient ethanol immersion and washing before use.

[0056] The following will describe in detail various aspects of the present invention with reference to specific embodiments:

[0057] [Example 1]

[0058] Example 1 provides a method for preparing an endometrial repair membrane, comprising the following steps:

[0059] (i) A solution was prepared by mixing 200 ml of glacial acetic acid, 200 ml of ethyl acetate, and 100 ml of water. 100 g of gelatin was added to the solution and stirred for 10 hours to completely dissolve the gelatin, thereby obtaining a first solution.

[0060] (ii) 50 ml of a glyoxal aqueous solution was prepared, wherein the concentration of glyoxal was 10%, to obtain a second solution.

[0061] (iii) adding the first solution into the first liquid supply tube of the electrospinning device and the second solution into the second liquid supply tube, setting the liquid supply rate of the first liquid supply tube to 2 ml / h and the liquid supply rate of the second liquid supply tube to 0.5 ml / h, and starting the liquid supply at the same time. At the confluence of the first liquid supply tube and the second liquid supply tube, the first solution and the second solution are evenly mixed to form a spinning solution.

[0062] (iv) delivering the spinning solution to the spinning electrode of the electrospinning apparatus for spinning, wherein the spinning temperature is 25° C., the humidity of the spinning space is 40% RH, the spinning working distance is 150 mm, the receiving drum speed is 80 rpm, and the receiving area is 30 cm x 300 cm.

[0063] During the spinning time, the spinning voltage is adjusted so that the spinning current is controlled according to the curve A2 shown in FIG1 , as follows:

[0064] The total spinning time is 330 minutes, which consists of a first constant current period, a first current linear change period, and a second constant current period. The initial current (i.e., the first constant current value) is set to 0.1 mA. During the first constant current period, the current is controlled to remain constant at 0.1 mA for 40 minutes. Then, during the first linear current change period, the current is controlled to increase uniformly over time at a rate of 0.001 mA / min to 0.32 mA (the termination current, i.e., the second constant current value). This period lasts for 220 minutes. Thereafter, during the second constant current period, the current is controlled to remain constant at 0.32 mA for approximately 70 minutes. In this embodiment, the time integral value Q of the spinning current is controlled to be 4C.

[0065] (v) After the spinning is completed, the nanofiber membrane is obtained, and the nanofiber membrane is placed in an oven and treated at 150° C. for 6 h to obtain a treated nanofiber membrane (i.e., an electrospun membrane for endometrial repair, also known as an endometrial repair membrane).

[0066] The spinning was repeated 9 times, and each time the first solution and the second solution were prepared using the same formula and preparation method, and the same current control and the same spinning conditions were used, thereby obtaining 10 membrane samples, which were numbered as sample 1-1 to sample 1-10.

[0067] The size of the membrane samples prepared by the method of this embodiment is 30 cm*300 cm, and the thickness is shown in the thickness measurement below.

[0068] [Example 2]

[0069] This embodiment adopts a preparation method similar to that of Example 1, except that the current range and current-time integral value are controlled differently under the same spinning time. Specifically, in the spinning step (iv):

[0070] During the spinning time, the spinning voltage is adjusted so that the spinning current is controlled according to the curve A1 shown in FIG1 , as follows:

[0071] The total spinning time is 330 minutes, which consists of a first constant current period, a first linear current change period, and a second constant current period. The initial current (i.e., the first constant current value) is set to 0.18 mA. During the first constant current period, the current is controlled to remain constant at 0.18 mA for 40 minutes. Then, during the first linear current change period, the current is controlled to increase uniformly over time at a rate of 0.001 mA / min to 0.4 mA (the termination current, i.e., the second constant current value). This period lasts for 220 minutes. Thereafter, during the second constant current period, the current is controlled to remain constant at 0.4 mA. This period lasts for approximately 70 minutes. In this embodiment, the time integral value Q of the spinning current is controlled to be 6C.

[0072] The spinning was repeated 9 times, and each time the first solution and the second solution were prepared using the same formula and preparation method, and the same current control and the same spinning conditions were used, thereby obtaining 10 membrane samples, which were numbered as sample 2-1 to sample 2-10.

[0073] The size of the membrane samples prepared by the method of this embodiment is 30 cm*300 cm, and the thickness is shown in the thickness measurement below.

[0074] [Example 3]

[0075] This embodiment adopts a preparation method similar to that of Example 1, except that the current range and current-time integral value are controlled differently under the same spinning time. Specifically, in the spinning step (iv):

[0076] During the spinning time, the spinning voltage is adjusted so that the spinning current is controlled according to the curve A3 shown in FIG1 , as follows:

[0077] The total spinning time is 330 minutes, consisting of a first constant current period, a first linear current change period, and a second constant current period. The initial current (i.e., the first constant current value) is 0.02 mA. During the first constant current period, the current is controlled to remain constant at 0.02 mA for 40 minutes. The current is then increased uniformly over time at a rate of 0.001 mA / min to 0.24 mA (the final current, i.e., the second constant current value) during the first linear current change period, which lasts for 220 minutes. Thereafter, the current is controlled to remain constant at 0.24 mA during the second constant current period, which lasts for approximately 70 minutes. In this embodiment, the time integral value Q of the spinning current is controlled to be 2.6C.

[0078] The spinning was repeated 9 times, and each time the first solution and the second solution were prepared using the same formula and preparation method, and the same current control and the same spinning conditions were used, thereby obtaining 10 membrane samples, which were numbered as sample 3-1 to sample 3-10.

[0079] The size of the membrane samples prepared by the method of this embodiment is 30 cm*300 cm, and the thickness is shown in the thickness measurement below.

[0080] [Example 4]

[0081] This embodiment adopts a preparation method similar to that of Example 1, except that different spinning currents and spinning times are used, but the current-time integral value is 4 C. Specifically, in the spinning step (iv):

[0082] During the spinning time, the spinning voltage is adjusted so that the spinning current is controlled according to the curve B1 shown in FIG2 , as follows:

[0083] The total spinning time was 250 minutes, consisting of a first constant current period and a first linear current variation period. The initial current was 0.18 mA (i.e., the first constant current value). During the first constant current period, the current was maintained constant at 0.18 mA for 40 minutes. During the first linear current variation period, the current was then increased uniformly over time at a rate of 0.001 mA / min to 0.39 mA (the final current), which lasted for 210 minutes. In this embodiment, the time integral of the spinning current, Q, was controlled to be 4C.

[0084] The spinning was repeated 9 times, and each time the first solution and the second solution were prepared using the same formula and preparation method, and the same current control and the same spinning conditions were used, thereby obtaining 10 membrane samples, which were numbered as sample 4-1 to sample 4-10.

[0085] The size of the membrane samples prepared by the method of this embodiment is 30 cm*300 cm, and the thickness is shown in the thickness measurement below.

[0086] [Example 5]

[0087] This embodiment adopts a preparation method similar to that of Example 1, except that different spinning currents and spinning times are used, but the current-time integral value is 4 C. Specifically, in the spinning step (iv):

[0088] During the spinning time, the spinning voltage is adjusted so that the spinning current is controlled according to the curve B3 shown in FIG2 , as follows:

[0089] The total spinning time is 380 minutes, consisting of a first constant current period, a first linear current change period, and a second constant current period. The initial current (i.e., the first constant current value) is 0.05 mA. During the first constant current period, the current is controlled to remain constant at 0.05 mA for 40 minutes. The current is then increased uniformly over time at a rate of 0.001 mA / min to 0.27 mA (the final current, i.e., the second constant current value) during the first linear current change period, which lasts for 220 minutes. Thereafter, the current is controlled to remain constant at 0.27 mA during the second constant current period, which lasts for approximately 120 minutes. In this embodiment, the time integral value Q of the spinning current is controlled to be 4C.

[0090] The spinning was repeated 9 times, and each time the first solution and the second solution were prepared using the same formula and preparation method, and the same current control and the same spinning conditions were used, thereby obtaining 10 membrane samples, which were numbered as sample 5-1 to sample 5-10.

[0091] The size of the membrane samples prepared by the method of this embodiment is 30 cm*300 cm, and the thickness is shown in the thickness measurement below.

[0092] [Example 6]

[0093] In this embodiment, a preparation method similar to that of Example 1 is used, except that the concentrations of the glyoxal solutions are different. Glyoxal solutions with concentrations of 5% and 20% are selected as the second solution (cross-linking agent solution), respectively.

[0094] In this embodiment, the membrane obtained by electrospinning using a 5% aqueous solution of glyoxal as the crosslinking agent solution is numbered as Sample 6, and the membrane obtained by electrospinning using a 20% aqueous solution of glyoxal as the crosslinking agent solution is numbered as Sample 7.

[0095] The size of the membrane sample prepared by the method of this embodiment is 30 cm*300 cm, and the thickness and other properties are described below.

[0096] [Comparative Example]

[0097] This comparative example adopts a preparation method similar to that of Example 1, except that a fixed spinning voltage is used and the spinning current and the current-time integral value are not specifically controlled. Specifically, in the spinning step (iv):

[0098] The total spinning time was 330 min. The spinning voltage was set to a fixed voltage of 55 kV. The spinning voltage was observed every ten minutes to keep the voltage constant, and the current at that time was recorded.

[0099] The spinning was repeated 9 times, and each time the first solution and the second solution were prepared using the same formula and preparation method, and the same voltage control (i.e., the voltage was maintained at a constant voltage of 55 kV) and the same spinning conditions were used, thereby obtaining 10 membrane samples in this comparative example, which were numbered as sample 8-1 to sample 8-10.

[0100] Observation of the current values ​​revealed no regular pattern across the 10 spinning runs. Furthermore, the time-integrated current values ​​varied from experiment to experiment, fluctuating irregularly within the range of 2C to 6C. The time-integrated current values ​​for samples 8-1 to 8-10 were: Q1 = 5C, Q2 = 3C, Q3 = 5C, Q4 = 5C, Q5 = 4C, Q6 = 2C, Q7 = 4C, Q8 = 3C, Q9 = 6C, and Q10 = 2C. The current range and integral values ​​for each sample are shown in Table 1.

[0101] The size of the film samples prepared by the method of this comparative example is 30 cm*300 cm, and the thickness is shown in the thickness measurement below.

[0102] The thickness of the electrospun membrane samples prepared in the exemplary embodiments and comparative examples of the present invention were measured and observed using a scanning electron microscope.

[0103] 1. Thickness measurement

[0104] Measure the thickness of the sample and calculate the average thickness (Avg) and thickness standard deviation (STDEV) of the sample. Specifically, the measurement and calculation are performed as follows:

[0105] Take sample 1-1 as an example. Sample 1-1 is a 30cm*300cm electrospun membrane (endometrial repair membrane). The thickness of sample 1-1 was measured at 10 points in the middle of its length and every 3cm along its width. The thickness measurements at these 10 points were: 0.200mm, 0.215mm, 0.227mm, 0.224mm, 0.217mm, 0.208mm, 0.203mm, 0.208mm, 0.222mm, and 0.229mm. The average thickness of sample 1-1 was calculated to be 0.215mm.

[0106] Calculate the thickness standard deviation (STDEV) of sample 1-1 according to formula (1):

[0107] Where σ is the thickness standard deviation (STDEV), x i is the thickness measurement value of each point of the sample, μ is the average thickness of the sample, and N is the number of samples.

[0108] From this calculation, it was found that the standard deviation (STDEV) of the thickness of a single film of Sample 1-1 was 0.010.

[0109] The thickness of samples 1-2 to 1-10 was measured according to the above method, and the thickness standard deviation (STDEV) of each film was calculated, as shown in Table 1 below.

[0110] According to the above calculations, the average thickness Avg of samples 1-1 to 1-10 are 0.215 mm, 0.204 mm, 0.232 mm, 0.225 mm, 0.229 mm, 0.207 mm, 0.220 mm, 0.221 mm, 0.225 mm, and 0.220 mm, respectively.

[0111] The thickness standard deviation (STDEV) of the 10 films of samples 1-1 to 1-10 was calculated according to the above formula (1), where σ is the thickness standard deviation (STDEV) of the 10 films, and x is i is the average thickness Avg of each film, μ is the average thickness of ten films, and N is the number of samples. Calculation shows that the standard deviation (STDEV) of the thickness of the ten films is 0.010.

[0112] The remaining samples were measured and calculated in the same manner as samples 1-1 to 1-10. The specific results are shown in Table 1.

[0113] Table 1. Current integral value, spinning time, thickness, and thickness standard deviation data for samples 1-10

[0114] In Table 1, the thickness dispersion is represented by the thickness standard deviation STDEV. The smaller the STDEV, the more concentrated the data distribution and the more uniform the thickness.

[0115] According to Table 1, by controlling the current change during the spinning process, making the current in the range of 0.01 to 0.4 mA, the current time integral value in the range of 1C to 9C, and making the current change according to a regular pattern (for example, including at least one current constant period and at least one current linear change period), a thin electrospun membrane with uniform thickness can be prepared. Moreover, the membrane thickness increases with the increase of the current time integral value, and the membrane thickness with equal integral values ​​is similar. Specifically, the STDEV values ​​of the single membranes of samples 1 to 5 are all in the range of 0.006 to 0.013, all less than 0.02. It can be seen that the preparation method according to the present invention can produce a thin electrospun membrane (endometrial repair membrane) with uniform thickness.

[0116] The method is also reproducible, capable of producing thin, uniformly thick electrospun membranes over multiple spinning cycles. For samples 1-1 to 1-10, when the current was controlled to vary regularly during multiple spinning cycles (e.g., including two periods of constant current and one period of linear current variation), the STDEV of multiple membranes with the same current-time integral and current values ​​was very low. The average STDEV of the thickness of the ten membranes from samples 1-1 to 1-10 was only 0.010.

[0117] In contrast, when the fixed voltage method is used to prepare electrospinning membranes, the current changes irregularly, the current-time integral value also changes irregularly, and the STDEV value of a single membrane will be greater than 0.02.

[0118] Furthermore, when using a fixed voltage method to prepare electrospun membranes, the current and current-time integral values ​​vary with each spinning cycle, leading to even greater variations in membrane thickness during multiple spinning cycles. As shown in Table 1, the average thickness of samples 8-1 to 8-10 (10 membranes) is 0.263 mm, and the STDEV of the 10 membranes is 0.163. This means that the thickness of the 10 membranes is irregularly distributed within the range of 0.071 to 0.533 mm. This thickness deviation is nearly 20 times greater than the STDEV of multiple membranes from the current-controlled sample of the present invention.

[0119] It can be seen from this that the present invention can avoid the defects of large fluctuations in membrane thickness and poor repeatability when using a fixed spinning voltage for spinning by controlling the current and the current time integral value and making the current change regularly to perform electrospinning. In addition, the spinning method used in the present invention is repeatable and can still ensure the preparation of a thin electrospinning membrane with uniform thickness after multiple spinning cycles.

[0120] 2. Scanning electron microscopy observation

[0121] Scanning electron microscopy was performed on the membrane samples of Examples 1 to 5 to observe the fiber diameter. It was found that the fiber diameter distribution was uniform and narrow, ranging from 200 to 400 nm. The electron microscope image of sample 1-1 is shown in Figure 3, and the electron microscope image of sample 4-1 is shown in Figure 4.

[0122] Scanning electron microscopy observation was performed on the comparative membrane samples, and it was observed that the fiber diameter distribution of the comparative membrane samples was wide, ranging from 100 to 900 nm. Among them, the electron microscope image of sample 9-1 is shown in Figure 5, and it can be seen that there is still adhesion and stranding between the fibers (as shown in the circle marks in Figure 5).

[0123] It can be seen from this that by controlling the spinning current and the integral value within a specific range and controlling the current to change regularly, the fiber diameter range of the electrospun membrane can be made narrower, between 100nm and 500nm (for example, 200nm to 400nm). Such a fiber diameter range can be more suitable for the growth of endometrial cells.

[0124] The following is a cross-linking test, a mechanical property test, and a KLE cell culture experiment performed on the membrane samples prepared in exemplary embodiments 1 and 6 of the present invention:

[0125] 1. Cross-linking degree test

[0126] The cross-linking degree of samples 1-1, 6 and 7 was tested by using an ultraviolet spectrophotometer (UV1600) to measure the absorbance of the samples at 346 nm, and the cross-linking degree was calculated according to formulas (2) and (3).

[0127] Where: N is the amount of ε-amino group in the lysine side chain (mol / g), A is the absorbance value, 1.46×10 4 is the molar absorption coefficient of trinitrobenzene derivatives, b is the optical path length (cm), and X is the sample weight (g).

[0128] Through testing and calculation, it can be seen that the cross-linking degrees of sample 1-1, sample 6 and sample 7 are 45%, 20% and 78% respectively.

[0129] It can be seen that due to the real-time mixing of gelatin solution and cross-linking agent solution, the cross-linking degree of the electrospun membrane is affected by the cross-linking agent content. The greater the cross-linking agent content, the higher the cross-linking degree of the electrospun membrane.

[0130] 2. Mechanical properties test

[0131] The mechanical properties of single nanofibers of samples 1-1, 6, and 7 were tested using a nanoindenter (stiffness: 5.15 N / m; tip radius: 28.5 μm).

[0132] The test showed that the Young's modulus of the single fiber of sample 1-1 was about 1.02 kPa, the Young's modulus of the single fiber of sample 6 was about 0.56 kPa, and the Young's modulus of the single fiber of sample 7 was about 2.05 kPa. This shows that the higher the degree of crosslinking, the greater the Young's modulus of the single fiber, and appropriate crosslinking can enhance the mechanical properties of the fiber.

[0133] 3. KLE cell culture experiment

[0134] Samples 1-1, 6, and 7 were subjected to KLE cell culture experiments.

[0135] Specifically, the samples were sterilized using ethylene oxide, cut into 1 cm*1 cm squares, inoculated with KLE cells, cultured for 7 days, fixed, and stained with HE sections to observe the growth of cells on samples 1-1, sample 6, and sample 7.

[0136] FIG6 is a stained image of a tissue section of membrane sample 1-1, FIG7 is a stained image of a tissue section of membrane sample 6, and FIG8 is a stained image of a tissue section of membrane sample 7.

[0137] As shown in Figures 6 to 8, sample 1-1 has a significant effect on promoting the proliferation of KLE cells. This shows that the electrospun membrane with a cross-linking degree of 45% (sample 1-1) has the best effect on promoting cell proliferation.

[0138] According to the above tests, it can be seen that by further controlling the cross-linking degree of the electrospun membrane, the Young's modulus of a single filament of the electrospun membrane can be improved, and when the cross-linking degree is controlled within a certain range, it is conducive to cell proliferation. The electrospun membrane prepared in this way has good flexibility and compliance, a soft texture, and is conducive to repairing the endometrium.

[0139] The following in vivo degradation experiments and clinical experiments were conducted on the electrospun membrane samples prepared in the exemplary embodiments of the present invention:

[0140] 1. In vivo degradation experiment in rabbits

[0141] Sample 1-1 was implanted into rabbits to observe the degradation of the spinning membrane and the repair of the endometrium.

[0142] Specifically, sample 1-1 was implanted into the uterus of a rabbit. Thirty days later, the rabbit uterine tissue was sliced ​​and stained with HE to observe the degradation of the spinning membrane in the rabbit uterus. The repair status was confirmed by observing the integrity of the endometrium.

[0143] The experimental results showed that sample 1-1 was completely degraded (as shown in FIG9 ), the endometrial contour was intact, and the repair effect was good.

[0144] It can be seen that considering the duration of endometrial repair and the requirements of the female physiological cycle, sample 1-1 (thickness of 0.215±0.010mm) is suitable for endometrial repair.

[0145] 2. Clinical trials

[0146] Patients with intrauterine adhesions and fertility requirements were screened for clinical trials. The preoperative endometrial status of the patient was shown in FIG10 . The intrauterine adhesions were separated by hysteroscopic surgery.

[0147] Sample 1-1 (electrospun membrane with a thickness of 0.215±0.010 mm) was selected for clinical trials on patients:

[0148] Sample 1-1 was sterilized using ethylene oxide, and two 4cm×4cm membranes were taken and delivered into the separated uterine cavity through a delivery device; 3 days later, one of the membrane sections was taken out for MASSON staining and observed under a microscope. The microscopic slice photograph is shown in Figure 12. In Figure 12, area A is gelatin fiber and area B is cell-enriched gelatin fiber. It can be seen that the gelatin fiber membrane is enriched with a large number of cells in the uterine cavity blood; 30 days later, the hysteroscopy was repeated, and the status of the patient's endometrium is shown in Figure 11. It can be seen that the patient's uterine cavity is intact, adhesions have disappeared, and the endometrial gland openings (as indicated by the arrows in Figure 11) are dense and obvious.

[0149] It can be seen that the electrospun membrane prepared according to the method of the present invention can effectively treat and repair the damaged endometrium, avoid the re-formation of adhesions and scars, and restore the normal physiological function of the uterus.

[0150] The present invention has been described above in detail with reference to specific embodiments. These embodiments are merely illustrative and are not intended to limit the scope of protection of the present invention. Those skilled in the art may make various modifications, variations, or substitutions to the present invention without departing from the spirit and scope of the present invention. Therefore, various equivalent variations made in accordance with the present invention are still within the scope of the present invention.

Claims

1. A method for preparing a tissue repair membrane, comprising: A spinning solution is delivered to the spinning electrode of an electrospinning device for spinning to form a tissue repair membrane, characterized in that the preparation method includes: during the spinning time, the spinning current is controlled to change regularly, and the spinning current is controlled to be in the range of 0.01mA to 0.4mA, and the time integral value of the spinning current is controlled to be in the range of 1C to 9C.

2. The preparation method according to claim 1, characterized in that The spinning time includes at least one constant current period, during which the spinning current is kept constant.

3. The preparation method according to claim 2, characterized in that: The spinning time includes at least one current linear variation period, and in the at least one current linear variation period, the spinning current changes linearly with time.

4. The preparation method according to claim 3, characterized in that: The at least one constant current period includes a first constant current period and a second constant current period, in which the spinning current is maintained at a first constant current value during the first constant current period, and in which the spinning current is maintained at a second constant current value during the second constant current period, and the second constant current value is greater than the first constant current value; The at least one current linear change period includes a first current linear change period, a starting current of the first current linear change period is a first current constant value, and a termination current is a second current constant value.

5. The preparation method according to claim 4, characterized in that: The first constant current period lasts for 40 minutes to 60 minutes, the second constant current period lasts for 40 minutes to 120 minutes, the first current linear change period lasts for 180 minutes to 240 minutes, the first current constant value is 0.02 mA to 0.2 mA, the second current constant value is greater than 0.02 mA and not greater than 0.4 mA, and the linear change rate of the spinning current in the first current linear change period is 0 to 0.1 mA / min.

6. The preparation method according to claim 3, characterized in that: The at least one constant current period includes a first constant current period, during which the spinning current is maintained at a first constant current value; The at least one current linear change period includes a first current linear change period, a starting current of the first current linear change period is a first current constant value, and a termination current is greater than the starting current.

7. The preparation method according to claim 6, characterized in that: The first current constant period lasts for 40 minutes to 60 minutes, the first current linear change period lasts for 180 minutes to 240 minutes, the first current constant value is 0.02 mA to 0.2 mA, the termination current is greater than 0.02 mA and not greater than 0.4 mA, and the linear change rate of the spinning current in the first current linear change period is 0 to 0.1 mA / min.

8. The preparation method according to claim 1, characterized in that: The spinning current is controlled to be in the range of 0.02 mA to 0.4 mA during the spinning time, and the time integral value of the spinning current during the spinning time is in the range of 2.6C to 6C.

9. The preparation method according to claim 1, characterized in that: The thickness of the tissue repair membrane is 0.01-10 mm, and the thickness standard deviation is less than 0.

02.

10. The preparation method according to claim 1, characterized in that: The spinning solution is formed by the following method: a solution of a polymer material is transported through a first liquid supply pipe, a solution of a crosslinking agent is transported through a second liquid supply pipe, and the solution of the polymer material and the solution of the crosslinking agent are mixed in real time at the downstream intersection of the first liquid supply pipe and the second liquid supply pipe to form the spinning solution.

11. The preparation method according to claim 10, characterized in that: The preparation method further comprises: controlling the cross-linking degree of the tissue repair membrane to be within the range of 30% to 60%, so that the Young's modulus of a single filament of the formed tissue repair membrane is greater than 0.5 kPa.

12. The preparation method according to claim 11, characterized in that: The cross-linking degree of the tissue repair membrane can be controlled by controlling the content of the cross-linking agent.

13. The tissue repair membrane obtained by the preparation method according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Preparation method of collagen membrane

    CN103046225A

  • Biomimetic structure type polymer actuator and preparation method thereof

    CN104389173A

  • Conductive parallel fiber membrane capable of promoting rapid repair of peripheral nervous tissues and preparation method of conductive parallel fiber membrane

    CN105920672A

  • Electroactive double-layer periosteal-like material and preparation method thereof