Method for producing a nozzle unit for wafer manufacture, and nozzle unit

The glass nozzle unit, formed through a hot molding process, addresses the challenges of material pairing and thermal stress in existing nozzle units by providing a strong, precise, and long-lasting solution for microtin drop generation, enhancing the reliability and precision of wafer production.

WO2024235771A1PCT designated stage expired Publication Date: 2024-11-21FRAUNHOFER GESELLSCHAFT ZUR FORDERUNG DER ANGEWANDTEN FORSCHUNG EV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/EP2024/062660
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2024-05-07
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Current nozzle units for producing microtin drops used in wafer manufacturing are plagued by inconsistent quality, limited strength, and short service life due to material pairing issues, thermal stress, and contamination, which affect the reproducibility and precision of microtin drop generation.

Method used

A method for producing a nozzle unit exclusively from glass material using a hot molding process, where the glass forming blank is tempered to a forming temperature and then cooled to a lower temperature, enabling precise formation of a nozzle body that withstands high pressures and oscillatory excitation, thus eliminating material pairing disadvantages and enhancing strength and surface quality.

Benefits of technology

The glass nozzle unit achieves high strength, precise dimensions, and extended service life, ensuring consistent and reproducible generation of microtin drops for generating UV or EUV light, improving the reliability and precision of wafer production processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure EP2024062660_21112024_PF_FP_ABST
    Figure EP2024062660_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a nozzle unit (150) for generating tin microdroplets (14) which are used for generating plasma for emitting light within a device for wafer manufacture, comprising the steps of: providing a preform (130), wherein the preform (130) consists of a glass material, first temperature adjustment of the preform (130) to a forming temperature, forming the preform (130) in such a way that a nozzle body (152) suitable for generating tin microdroplets (14) is formed, and second temperature adjustment of the nozzle body (152) to a cool-down temperature which is lower than the forming temperature.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Method for producing a nozzle unit for wafer production and nozzle unit

[0002] The invention relates to a method for producing a nozzle unit for generating micro-tin droplets used for generating plasma for emitting light within a wafer manufacturing apparatus, a method for generating plasma for emitting light within a wafer manufacturing apparatus, a nozzle unit for generating micro-tin droplets, a microchip, a manufacturing system for producing a nozzle unit and a device for generating plasma.

[0003] Photolithography is one of the central processes in semiconductor and microsystem technology for the production of integrated circuits and other products. Photolithography is based on an exposure process in which the image of a photomask is transferred to a wafer coated with a light-sensitive photoresist. Subsequently, the exposed or unexposed areas of the photoresist are dissolved, forming a lithographic mask that allows for further processing using chemical and / or physical processes, such as the introduction of material into the open windows or the etching of recesses beneath the open windows.

[0004] In more modern processes, the photomask can be created using a Bragg mirror, which carries an image of the structures to be created on its surface. The state of the art is the use of UV light to expose the wafer. In particular, the use of DUV (deep ultraviolet) or EUV (extreme ultraviolet) is state of the art.

[0005] To generate this UV light, tiny tin droplets are dispensed into a vacuum chamber and exposed to a laser in such a way that the tin droplets are converted into plasma. This plasma emits the UV light, which can then be directed onto the wafer using a generally complex mirror system. Tin is used, among other things, because it can generate UV light with a particularly short wavelength.

[0006] An important aspect is the production of tin droplets with a size in the low micrometer range. Nozzles made of metal and glass are typically used for this purpose, both to ensure the purity of the tin and to ensure high nozzle strength, allowing for reproducible dispensing of the tin droplets. However, these nozzles cannot currently be manufactured with reproducible quality due to their variable component quality, and their service life and strength are unpredictable or only predictable to a limited extent.

[0007] The nozzle requires high dimensional accuracy and a high surface quality while maintaining a defined inner diameter to ensure, among other things, a long service life. Furthermore, the nozzle must withstand high pressures ranging from 700 bar to 3,000 bar to ensure consistently uniform dispensing of the tin droplets.

[0008] Processes for manufacturing nozzle units for generating micro tin droplets are therefore generally known, but they have various disadvantages. Such nozzles are manufactured in the state of the art by combining different materials with differing geometries and properties. This can be achieved, for example, with glass-to-metal sealing (GTMS) or by using additional and intermediate materials such as glass frits. However, this leads to unintended stress concentrations due to the heating and / or cooling processes as well as due to inconsistent thermal expansion coefficients of the materials. Furthermore, the strength of the composite depends on a variety of influencing factors, such as the temperature-time curve, the force-time curve, the atmosphere, the surface, the thermal expansion coefficients (GTE), and their respective homogeneity during the process.Furthermore, oxidation, contamination or soiling in the bonding layer between the different materials can result in insufficient strength of the bond.

[0009] Furthermore, nozzles for generating micro-tin droplets can be manufactured by direct manufacturing, for example, by grinding and / or polishing a raw material. In this case, the raw material is machined purely by machining, which has a negative impact on the service life under the required dynamic load spectrum. Furthermore, direct manufacturing leads to edge zone damage, fractures due to stress concentration, and chemical degradation of the glass due to the polishing suspension. Direct manufacturing of nozzles thus leads to an inadequate service life.

[0010] Another option for manufacturing nozzles for micro-tin droplets is primary forming. In primary forming, the nozzle is created from the melt. The disadvantage of primary forming is the introduction of higher stresses and significant shrinkage during the cooling phase. This results in poor dimensional stability and mold accuracy of the component, making it impossible to meet the high demands placed on nozzles for micro-tin droplets.

[0011] WO22268413A1 discloses a composite nozzle made of metal and glass, which, however, has the disadvantages described above of a nozzle consisting of a combination of different materials.

[0012] WO22002662A1 discloses a nozzle for dispensing a fluid, comprising an inner tube made of glass and an electrically controllable element made of a conductive metal surrounding the tube. It is an object of the invention to provide a method for producing a nozzle unit for generating micro-tin droplets used to generate plasma for emitting light within a wafer production apparatus, a method for generating plasma for emitting light within a wafer production apparatus, a nozzle unit for generating micro-tin droplets, a microchip, a manufacturing system for producing a nozzle unit, and a device for generating plasma, which reduce or eliminate one or more of the aforementioned disadvantages. In particular, it is an object of the invention to provide a solution that enables precise and reproducible generation of micro-tin droplets.

[0013] This object is achieved by the method, the nozzle unit, the microchip, the manufacturing system, and the device according to the features of the independent patent claims. Further advantageous embodiments of these aspects are specified in the respective dependent patent claims. The features disclosed in the patent claims, the description, and the drawings can be combined individually in any technologically expedient manner, with further embodiments of the invention being shown.

[0014] According to a first aspect, the object mentioned at the outset is achieved by a method for producing a nozzle unit for generating micro-tin droplets, which are used to generate plasma for emitting light, in particular UV light, preferably DUV light and / or EUV light, within a device for wafer production, comprising the steps of: providing a forming blank, wherein the forming blank consists of a glass material, first tempering of the forming blank to a forming temperature, forming the forming blank in such a way that a nozzle body suitable for generating micro-tin droplets is formed, and second tempering of the nozzle body to a cooling temperature which is lower than the forming temperature.

[0015] The invention is based on the finding that a nozzle unit for generating micro-tin droplets within a wafer production device can consist exclusively of a glass material. A nozzle unit consisting exclusively of a glass material overcomes, in particular, the disadvantages described above. In particular, the disadvantages of material pairings are overcome. Furthermore, such a nozzle unit made of glass material can enable particularly high strength while simultaneously providing the properties for generating high-purity micro-tin droplets.

[0016] The invention is further based on the finding that the advantages of a nozzle unit made exclusively from glass material are realized when the nozzle unit is manufactured using a hot-forming process. Only the forming process enables the precise manufacture of the nozzle unit while simultaneously achieving high surface qualities, tight tolerances, and advantageous material properties. Thus, the nozzle unit produced using the hot-forming process differs from a conventionally manufactured nozzle made from glass material and from nozzles consisting of material pairs.

[0017] The method is designed for producing the nozzle unit. The nozzle unit is intended for generating micro-tin droplets, which are used to generate plasma for emitting light within a wafer production device. As an alternative to the tin material, other materials can also be used that can be used to generate plasma for emitting light within a wafer production device. A wafer production device is to be understood, in particular, as a device for producing semiconductors.

[0018] In particular, the plasma can be generated with the microtin droplets in such a way that it emits EUV light with a wavelength of 13.5 nm. The corresponding requirements for such a nozzle unit have been described in detail above. In particular, such a nozzle unit should withstand the various load spectrums during the generation of the microtin droplets, especially with regard to high temperatures, temperature fluctuations, pressures, and pressure fluctuations.

[0019] The generation of micro-tin droplets can occur directly or indirectly with the nozzle unit during its intended use. On the one hand, the generation of micro-tin droplets can mean the direct generation of tin droplets, in particular through oscillatory excitation of the nozzle unit, for example, at a frequency between 50 and 60 kHz. On the other hand, it can mean the generation of a tin material jet, which subsequently breaks down into droplets or is divided into droplets. The wafer production device can be a device for the complete production of a wafer or for the production of a semi-finished product for wafer production.

[0020] The method comprises the step of providing the forming blank, wherein the forming blank consists of the glass material. The forming blank can have conventional geometries. Preferably, the forming blank is spherical, gob-shaped, tubular, and / or bar-shaped. Alternatively, the forming blank can have the embodiments described below.

[0021] The forming blank consists of the glass material. The glass material can, in principle, be any glass material suitable for forming nozzle bodies for producing micro tin droplets. In particular, the glass material can be borosilicate glass or aluminosilicate glass.

[0022] It is preferred that the blank volume of the forming blank substantially corresponds to the glass volume of the nozzle body. Alternatively, the forming blank may have a blank volume that is greater than the volume of the nozzle body. It is particularly preferred that the volume of the nozzle unit and / or the nozzle body be less than or equal to the blank volume.

[0023] The method further comprises the step of first tempering the forming blank to a forming temperature. The forming temperature of the forming blank is to be understood in particular as the temperature at which the forming blank is formable, so that the external shape of the forming blank can be changed by external influences, but without melting or destroying the forming blank.

[0024] The forming temperature can be, for example, between 600 °C and 1100 °C, in particular between 700 °C and 950 °C. The first tempering step is preferably divided into sub-steps. It is preferred that a first sub-step of the first tempering step provides a first heating rate up to a first temperature T1. Rapid heating is possible at the beginning because the viscoelastic structural changes of the glass material in this first sub-step are uncritical and have no negative impact on the risk of sticking or breakage.

[0025] It is preferred that, in a second sub-step of the first tempering, heating takes place at a second heating rate to a temperature T2 > T1, wherein the second heating rate is lower than the first heating rate. By adjusting the heating rates accordingly, an overshoot of the maximum achievable temperature T3, in particular the forming temperature, can be prevented. Furthermore, it may be preferred that the first tempering include a third sub-step in which a defined holding time t1 takes place at a temperature T3 that is preferred for the temperature homogeneity of the glass.

[0026] After the first tempering of the forming blank to the forming temperature, in particular temperature T3, the next step takes place: forming the forming blank such that a nozzle body suitable for producing micro tin droplets is formed. The forming can be carried out by pressing and drawing and / or be media-assisted, for example by applying negative and / or positive pressure. In particular, the forming can be carried out using upper and / or lower forming tools. Furthermore, a combination of these forming means can be preferred. It is preferred that the forming of the forming blank is carried out using a forming force, wherein the forming force is adjusted depending on the glass viscosity of the forming blank.

[0027] The design of a nozzle body suitable for generating micro-tin droplets means, in particular, that a nozzle body is designed suitable for generating micro-tin droplets for generating plasma for emitting light within a wafer production device. This means, in particular, that the nozzle body is a solid body that can withstand the high loads encountered during the generation of micro-tin droplets. Furthermore, it is preferred that the nozzle body be formed in such a way that it requires no post-processing, in particular, no grinding or polishing is required, in order to also withstand the high demands of generating micro-tin droplets.

[0028] Furthermore, nozzle units for producing micro-tin droplets are typically excited at 50-60 kHz oscillations during normal operation, so the nozzle body must also withstand this vibrational excitation. The nozzle body is specifically understood as the formed blank. The forming temperature of the blank is, in particular, lower than the melting temperature of the blank or the glass material of the blank.

[0029] The method further comprises the step of: second tempering of the nozzle body to a cooling temperature that is lower than the forming temperature. It is preferred that the second tempering comprises two or more sub-steps. In particular, it is preferred that in a first sub-step of the second tempering, the nozzle body is cooled to a temperature T4 < T3 at a first cooling rate. It is further preferred that the temperature T4 is selected such that deformation of the nozzle body under its own weight is no longer possible.

[0030] In a second sub-step of the second tempering step, it is preferred that temperature T4 be maintained for a holding time t2. This holding time serves to reduce any remaining stresses in the nozzle body.

[0031] Furthermore, in a third sub-step of the second tempering, it is preferred that a fifth temperature T5 <T4 eingestellt wird. Die zweite Kühlrate ist vorzugsweise gering gewählt, sodass ein langsames Kühlen der Vermeidung des Einfrierens von Spannungen aufgrund von zu schnellem Kühlen der viskoelastischen Struktur des Glasmaterials dient. In einem vierten Teilschritt der zweiten Temperierung ist es bevorzugt, dass mit einer dritten Kühlrate größer der zweiten Kühlrate auf eine Raumtemperatur gekühlt wird.

[0032] It is preferred that the method performs the steps in the following order: provision, first tempering, forming, second tempering. In a preferred embodiment of the method, the forming blank is provided in two parts with an inner element and a corresponding outer element, and the inner element is arranged within the outer element, so that a material connection is formed between the inner element and the outer element during the forming process.

[0033] The outer element, in particular, has a recess within which the inner element can be arranged. In particular, the recess of the outer element and the inner element are dimensioned such that the inner element is arranged within the outer element with essentially no play. Essentially free of play means, in particular, that a fit between the inner element and the outer element can be designed as a slight clearance fit or as a slight interference fit.

[0034] In a further preferred embodiment of the method, it is provided that the forming temperature of the inner element is higher than that of the outer element, and the forming blank is tempered to the forming temperature of the outer element, which is below the forming temperature, preferably below the transformation temperature, of the inner element, so that the outer element is formed and connected to the inner element.

[0035] Because the selected forming temperature is lower than the forming temperature of the inner element, it is ensured that the inner element is essentially undeformed. Thus, only the outer element is formed and molded to the inner element. As a result, the inner element is essentially unaffected by the forming process, so the properties of the inner element are essentially retained.

[0036] It is particularly preferred that the inner element has a mold passage designed to form a material channel of the nozzle body, and that the mold passage is retained during the forming process. The mold passage preferably extends through the inner element. The mold passage is preferably designed as a through-opening. Furthermore, the mold passage preferably extends from a proximal end to a distal end of the inner element. This is achieved in particular by the selected forming temperature being below the forming temperature of the inner element, so that the mold passage is not affected by the forming process.

[0037] It is further preferred that the mold passage of the inner element be subjected to an overpressure at least during the forming process. This overpressure further ensures that the mold passage is maintained during the forming process.

[0038] It may further be preferred for the forming blank to have the forming passage. In particular, a one-piece forming blank may have the forming passage.

[0039] In a further preferred embodiment of the method, the outer element is formed with at least two different outer parts, and the two different outer parts approximate a contour of the nozzle unit. The at least two different outer parts can, for example, be arranged one above the other or next to one another in a nozzle passage direction. It is preferred that the at least two different outer parts have different outer diameters. The outer parts can, for example, be disc-shaped and / or sleeve-shaped. The at least two different outer parts are, in particular, dimensioned such that they abut one another.

[0040] In a further preferred embodiment of the method, forming means are used in such a way that a material channel is formed in the nozzle body, at least during the forming process. The material channel in the nozzle body preferably extends from a proximal open end to a distal open end, so that a tin material can be guided through the material channel.

[0041] It is preferred that the material channel has a diameter of less than 50 pm, less than 40 pm, less than 30 pm, and in particular less than 20 pm. The forming means can be arranged and configured to form the material channel in a solid forming blank or by means of the forming passage described above. The forming means can, for example, penetrate into the forming passage.

[0042] In a further preferred embodiment, the forming means comprise or are a forming wire and / or a forming mandrel, which is / are arranged such that it / they form the material channel. The forming wire preferably has a stop at a lower end, which has a larger diameter than the forming passage, so that the glass blank can be held by means of the stop. It is further preferred that the forming wire has a forming spring and / or a forming weight at a lower end, so that the forming wire can be tensioned.

[0043] A preferred development of the method provides that the forming wire is moved relative to the forming blank, in particular during forming, so that adhesion of the forming wire to the forming blank is avoided or reduced. It may be preferred that the forming wire is moved in one direction and / or back and forth. Furthermore, it may be preferred that the forming wire is excited to oscillate. Furthermore, it may be preferred that the forming wire is rotated about a longitudinal axis of the forming wire. Furthermore, it is preferred that an electrical voltage is applied to the wire in such a way that adhesion is prevented or reduced.

[0044] In a further preferred development of the method, the material channel is introduced after forming, preferably after the second tempering. It is preferred that the material channel is introduced using a laser drilling process and / or selective laser etching.

[0045] In a further preferred development of the method, it is provided that the nozzle body with the material channel is designed in such a way that the micro-tin drops can be produced during normal operation at a pressure of more than 700 bar, preferably more than 1,000 bar, in particular more than 1,500 bar.

[0046] According to a further aspect, the object mentioned above is achieved by a method for generating plasma for emitting light within a wafer production device, comprising the steps of generating micro-tin droplets, exposing the micro-tin droplets to a laser beam so that the micro-tin droplets are converted in the plasma to provide light, in particular EUV light, for exposing a wafer, wherein the micro-tin droplets are generated using a nozzle unit consisting of formed glass. The nozzle unit consisting of formed glass is produced in particular using a method according to one of the embodiments described above.

[0047] According to a further aspect, the object mentioned at the outset is achieved by a nozzle unit for generating micro-tin drops which are used to generate plasma for emitting light, in particular EUV light, within a device for wafer production, in particular produced by a method according to one of the embodiments described above, comprising a nozzle body with a material channel, wherein the nozzle unit consists of formed glass.

[0048] The nozzle body extends, in particular, from a proximal end to a distal end. The material channel is open, in particular, at the proximal end and at the distal end, so that a tin material can be guided through the material channel from the proximal end to the distal end.

[0049] Orthogonal to the material channel and / or to a passage axis of the nozzle, the nozzle preferably has a round cross-section. The nozzle body preferably has, adjacent to the proximal end, a proximal section which has a substantially rectangular cross-section. Adjacent to the distal end, the nozzle preferably has a distal section which has a smaller diameter than the proximal section. Between the proximal section and the distal section, a central section is preferably provided which has a larger diameter than the distal section and a smaller diameter than the proximal section. It is preferred that the transitions from the proximal section to the central section and / or from the central section to the distal section are round, so that notch effects are reduced.It is preferred that the nozzle body is designed such that the micro-tin drops can be generated, in particular dispensed, at a pressure of more than 700 bar, preferably more than 1,000 bar, in particular more than 1,500 bar, during intended operation of the nozzle unit. In particular, the nozzle body is designed to withstand a pressure in the material channel of more than 700 bar, preferably more than 1,000 bar, in particular more than 1,500 bar. Furthermore, the nozzle body is designed to withstand a pressure in the material channel of more than 700 bar, preferably more than 1,000 bar, in particular more than 1,500 bar, when subjected to an oscillation frequency between 50 and 60 kHz.

[0050] In a preferred embodiment of the nozzle unit, the nozzle body can be arranged with the material channel and is designed to withstand a process temperature of more than 250°C, in particular between 250°C and 300°C, during normal operation. Furthermore, the nozzle body preferably has a coupling surface with which the nozzle body can be coupled to a droplet generation unit in a fluid-tight manner.

[0051] Furthermore, it is preferred that the nozzle body has a high surface quality and surface integrity. Furthermore, it is preferred that the surface quality and surface integrity are verifiable.

[0052] According to a further aspect, the object mentioned at the outset is achieved by a microchip produced by a method for generating plasma according to the embodiment variant described above.

[0053] The microchip was created, in particular, by dividing a wafer produced using the method. The method is merely a partial process, with the further steps of lithography and wafer production being known to those skilled in the art.

[0054] According to a further aspect, the object mentioned at the outset is achieved by a manufacturing system for producing a nozzle unit for generating micro-tin droplets, which are used to generate plasma for emitting light within a wafer production device, comprising a tempering device arranged and designed to temper a forming blank consisting of a glass material to a forming temperature and / or a nozzle body consisting of a glass material to a cooling temperature, and a forming device arranged and designed to reshape the forming blank such that the nozzle body is configured to be suitable for generating micro-tin droplets. The fact that the nozzle body is configured to be suitable for generating micro-tin droplets means, in particular, that it is used to generate plasma for emitting light within a wafer production device.

[0055] It is preferred that the forming device has an upper forming unit and / or a lower forming unit. It is preferred that the upper forming unit has an annular gap and a gap connection, wherein the annular gap can be evacuated via the gap connection, thereby creating a vacuum, allowing the forming blank to be sucked onto the upper forming unit.

[0056] Furthermore, it is preferred that the upper forming unit has a forming passage through which a negative pressure and / or positive pressure can be generated in a cavity of the forming device. Furthermore, a forming wire can be passed through the forming passage, with which a material channel can be formed in the nozzle body. Furthermore, it is preferred that the cavity has a venting channel.

[0057] It is preferred that the upper forming unit has a forming mandrel with which a material channel can be formed in the nozzle body.

[0058] It is preferred that the lower mold unit is formed in two parts, wherein an end of the lower mold unit facing away from the upper mold unit has an end piece so that the cavity can be formed with sharp edges.

[0059] Furthermore, it is preferred that the forming wire has a wire stop, which can be used to hold a tubular forming blank. Furthermore, a forming spring and / or a forming weight can be arranged on the forming wire to guide the wire straight.

[0060] According to a further aspect, the object mentioned at the outset is achieved by a device for generating plasma for emitting light, in particular EUV light, for wafer production, comprising a drop generation unit which is arranged and designed to generate micro-tin drops with a nozzle unit and to provide the micro-tin drops to an application unit, wherein the application unit is arranged and designed to apply a laser beam to the micro-tin drops so that the micro-tin drops are converted into plasma in order to provide light, in particular EUV light, for application to a wafer, wherein the nozzle unit consists of formed glass.

[0061] For further advantages, design variants and details of the individual aspects and their possible further training, please refer to the description of the other aspects, the corresponding features and further training.

[0062] Preferred embodiments are explained using the accompanying figures. They show:

[0063] Fig. 1: a schematic, two-dimensional view of an exemplary

[0064] Variant of a device for generating plasma;

[0065] Fig. 2: a schematic, two-dimensional view of an exemplary

[0066] Embodiment of a manufacturing system for producing a nozzle unit;

[0067] Figs. 3 - 8: schematic, two-dimensional detailed views of a manufacturing system for producing a nozzle unit;

[0068] Fig. 9: schematic, two-dimensional views of exemplary

[0069] Embodiments of a forming blank and a nozzle unit;

[0070] Figs. 10 - 12: schematic, two-dimensional views of exemplary embodiments of forming blanks;

[0071] Fig. 13: schematic, two-dimensional views of a forming blank and a formed forming blank within a lower forming unit; Fig. 14: a schematic view of an exemplary method for

[0072] Manufacturing a nozzle unit;

[0073] Fig. 15: a schematic view of an exemplary method for

[0074] Generation of plasma.

[0075] In the figures, identical or essentially functionally identical or similar elements are designated by the same reference numerals. The following exemplary embodiments are preferred embodiments of the invention.

[0076] In the exemplary embodiments, the described components of the embodiments each represent individual features of the invention that are to be considered independently of one another. These also further develop the invention independently of one another and are therefore to be considered as components of the invention, either individually or in a combination other than that shown. Furthermore, the described embodiments can also be supplemented by further features of the invention already described.

[0077] Figure 1 shows a schematic, two-dimensional view of an exemplary embodiment of a device 1 for generating plasma. The device 1 for generating plasma comprises a droplet generation unit 2. The droplet generation unit 2 has a first nozzle unit 4 and a second nozzle unit 8 for generating microtin drops 14.

[0078] The micro-tin droplets 14 are used to generate plasma for emitting light within a wafer production device. The device 1 can, in particular, be part of a wafer production device. The nozzle units 4, 8 are each coupled to a feed line 6, 10 with a tin bath of the droplet generation unit 2. The micro-tin droplets 14 are provided with the nozzle units 4, 8 of the application unit 12. In the application unit 12, in particular, a vacuum can be formed in which the micro-tin droplets 14 can be subjected to a laser and thus converted into plasma. Figure 2 shows a schematic, two-dimensional view of an exemplary embodiment of a manufacturing system 100 for manufacturing a nozzle unit. The manufacturing system 100 is designed to manufacture a nozzle unit for generating micro-tin droplets.In particular, the manufacturing system 100 is configured to perform a method for manufacturing the nozzle unit 150 for generating micro tin drops 14 used to generate plasma for emitting light within a wafer manufacturing apparatus.

[0079] The manufacturing system 100 is particularly designed to carry out the following steps: first tempering of a forming blank 130 consisting of a glass material to a forming temperature, forming the forming blank 130 such that a nozzle body 152 suitable for producing micro tin drops 14 is formed, and second tempering of the nozzle body 152 to a cooling temperature which is lower than the forming temperature.

[0080] For this purpose, the manufacturing system 100 comprises the tempering device 102, which is arranged and designed to temper the forming blank 130, consisting of a glass material, to a forming temperature and / or a nozzle body 152, consisting of a glass material, to a cooling temperature.

[0081] Furthermore, the manufacturing system 100 comprises the forming device 104, which is arranged and configured to form the forming blank 130 such that the nozzle body 152 is configured to be suitable for producing micro-tin droplets 14. The forming device 104 comprises, in particular, the upper forming unit 108 and the lower forming unit 110. The forming units 108, 110 can be moved toward one another so that the forming blank 106, which is only schematically illustrated, is formed into the cavity of the lower forming unit 110.

[0082] Figures 3-8 show schematic, two-dimensional detailed views of a manufacturing system for producing a nozzle unit. Figure 3 shows an upper forming unit 108 with an annular gap 114 and a gap connection 116. The annular gap 114 is designed to provide a forming blank 106, 130 by creating a vacuum in the annular gap 114 using the gap connection 116. The vacuum draws the forming blank 106, 130 toward the upper forming unit 108 so that it can be handled by the upper forming unit.

[0083] The lower forming unit 110 forms the cavity 120, wherein a venting channel 122 is provided at the lower end of the cavity 120 in order to enable optimal forming of the forming blank 106, 130.

[0084] Furthermore, a forming wire 118 is shown, which can be passed through the forming passage 112 in the upper forming unit 108, so that the forming wire 118 can be moved through the forming blank 106, 130. Thus, a material channel 154 can be formed.

[0085] Figure 4 shows a two-part lower forming unit 110. The forming unit 110 has an end piece 124 on a side facing away from the upper forming units 108, which end piece includes the venting channel 122. The cavity is open within the lower forming unit 110, making it easy to manufacture. After production, the end piece 124 can be attached to the lower forming unit, for example, by screwing, thus creating a sharp edge in the lower area.

[0086] Figure 5 shows that the upper forming unit 108 may include a forming mandrel 126. When the forming blank 130 is placed in the cavity 120 and is at the forming temperature, the upper forming unit 108 with the forming mandrel 126 may be moved vertically downward, so that a material channel 154 is formed in the nozzle body 152 by means of the forming mandrel 126.

[0087] Figure 6 shows the use of the forming wire 118 in a specific application. The forming wire 118 extends through the forming passage 112 and through the forming passage 132 of the forming blank 130. On the side of the forming wire 118 facing the lower forming unit 110, the forming wire 118 has a wire stop 128. The wire stop 128 is designed to form a stop for the forming blank 130, so that the forming blank 130 can be handled with the forming wire 118. Figure 7 shows that the forming wire can have a forming spring 136 and a forming weight 138 in order to use the wire in an optimal manner.

[0088] Figure 8 shows that the upper forming unit 108 can have a second cavity 140 and a recess 142 for arranging the lower forming unit 110. A specific geometry of the nozzle unit 150 can be produced using the second cavity 140.

[0089] Figure 9 shows on the left side a specific design of a blank 130 with a forming passage 132. By appropriately pressing and drawing the forming blank 130, which has been tempered to a forming temperature, the nozzle unit 150 shown on the right in the figure is formed.

[0090] The nozzle unit 150 has a nozzle body 152 through which the material channel 154 extends. The nozzle body 152 extends from the proximal end 156 to the distal end 158. The material channel 154 extends through the nozzle body 158 between the proximal end 156 and the distal end 158.

[0091] A tin material can pass through the material channel from the proximal end to the distal end and be dispensed at the distal end. Adjacent to the proximal end 156, the nozzle body 152 has a proximal section 160 and adjacent to the distal end 158, a distal section 164. A central section 162 is provided between the proximal section 160 and the distal section 164.

[0092] Figure 10 shows a particular embodiment of a forming blank 130 having a forming passage 132. In particular, the forming blank 130 is preformed and closely approximates the contour of the nozzle body 152. Such a geometry of the forming blank 130 can be determined, for example, by means of simulations. Such a forming blank 130 has the advantage that only a small degree of deformation is required for forming, thus simplifying the forming process. Furthermore, the production of a high surface quality and dimensional accuracy is possible in a particularly advantageous manner. The near-net-shape forming blank 130 also makes it possible to introduce fewer stresses during the actual forming process, thereby reducing the risk of damage.

[0093] Figure 11 shows a two-part forming blank 130 with an inner element 146 and a corresponding outer element 144. The inner element 146 is arranged within the outer element 144. The inner element 146 further comprises the forming passage 132. The two-part forming blank 130 can also be formed in multiple parts, as shown in Figure 12. On the left, it is shown that the outer element 144 can have three outer parts 148, 166, 168. The outer parts 148, 166, 168 are arranged in a sleeve-like manner around the inner element 146. On the right in the image, a comparable structure is shown, wherein the outer element 144 is formed from a total of four round-shaped outer parts 148, 166, 168, 170.

[0094] Figure 13 shows how the individual parts of a two-part forming blank 130 with a plurality of outer parts are joined together using the method for producing a nozzle unit 150. The formed nozzle unit 150 with the nozzle body 152 is shown on the right side of the image.

[0095] Figure 14 shows a schematic view of an exemplary method for manufacturing a nozzle unit. In step 200, a forming blank 130 is provided, wherein the forming blank 130 is made of a glass material. In step 202, the forming blank 130 is tempered to a forming temperature.

[0096] In step 204, the forming blank 130 is formed to form a nozzle body 152 suitable for generating micro-tin droplets. In step 206, the nozzle body 152 is tempered to a cooling temperature that is lower than the forming temperature.

[0097] Figure 15 shows a schematic view of an exemplary method for generating plasma. The method comprises step 300: generating micro-tin droplets 14. The method further comprises step 302: exposing the micro-tin droplets 14 to a laser beam, such that the micro-tin droplets 14 are converted into plasma to provide EUV light for impinging on a wafer. The micro-tin droplets 14 are generated using a nozzle unit 150 made of formed glass. The method described above for producing a nozzle unit 150 for generating micro-tin droplets, which are used to generate plasma for emitting light within a wafer production device, has the particular advantage that a nozzle unit 150 can be produced that has superior properties compared to the nozzle units known in the prior art. In particular, this nozzle unit has a longer service life.Furthermore, the nozzle unit 150 has a better surface quality and a better shape accuracy, so that the generated micro tin drops can be dispensed more precisely.

[0098] Overall, the wafer manufacturing process can be optimized by several percent, resulting in annual cost savings of several million euros for a single wafer production run. Furthermore, wafer quality is further improved, allowing individual structures to be produced with greater reliability and precision. This results in generally more powerful microchips that can be used in a wide variety of applications.

[0099] REFERENCE SYMBOL

[0100] Device for generating plasma

[0101] Drop generation unit first nozzle unit first feed second nozzle unit second feed

[0102] loading unit

[0103] Microtin drops

[0104] manufacturing system

[0105] Tempering device

[0106] Forming device

[0107] Forming blank upper forming unit lower forming unit

[0108] Forming pass

[0109] Annular gap

[0110] Gap connection

[0111] Form wire

[0112] cavity

[0113] ventilation duct

[0114] End piece

[0115] Form mandrel

[0116] Wire stop forming blank mold passage wire fastening forming spring forming weight second cavity recess outer element inner element outer part nozzle unit nozzle body material channel proximal end distal end proximal section middle section distal section outer part

[0117] outer part

[0118] outer part

Claims

CLAIMS 1. A method for producing a nozzle unit (150) for generating micro-tin drops (14) used to generate plasma for emitting light within a wafer manufacturing apparatus, comprising the steps of: Providing a forming blank (130), wherein the forming blank (130) consists of a glass material, first tempering the forming blank (130) to a forming temperature, Forming the forming blank (130) in such a way that a nozzle body (152) suitable for producing micro tin drops (14) is formed, and second tempering of the nozzle body (152) to a cooling temperature which is lower than the forming temperature.

2. The method according to claim 1, wherein the forming blank (130) is provided in two parts with an inner element (146) and a corresponding outer element (144), and the inner element (146) is arranged within the outer element (144) so ​​that a material connection is formed between the inner element (146) and the outer element (144) during the forming process.

3. Method according to one of the preceding claims, wherein the forming temperature of the inner element (146) is higher than that of the outer element (144), and the forming blank (130) is tempered to the forming temperature of the outer element (144), which is below the forming temperature of the inner element (146), so that the outer element (144) is formed and connected to the inner element (146).

4. Method according to the preceding claim 3, wherein the inner element (146) has a forming passage (132) which is designed to form a material channel of the nozzle body (152), and the forming passage (132) is retained during the forming.

5. Method according to one of the preceding claims, wherein the outer element (144) is formed with two different outer parts (148, 166, 168, 170) and the at least two different outer parts (148, 166, 168, 170) approximate a contour of the nozzle unit (150).

6. Method according to one of the preceding claims, wherein Forming means are used in such a way that a material channel (154) is formed in the nozzle body (152) at least during the forming process.

7. Method according to one of the preceding claims, wherein the forming means comprise or are a forming wire (118) and / or a forming mandrel (128) which is arranged such that it forms the material channel (154).

8. Method according to one of the preceding claims, wherein the forming wire (118) is moved relative to the forming blank (130) so that adhesion of the forming wire (118) to the forming blank (130) is avoided.

9. Method according to one of the preceding claims, wherein the forming wire (118) is moved in one direction and / or back and forth.

10. Method according to one of the preceding claims, wherein the forming wire (118) is excited in an oscillating manner.

11. Method according to one of the preceding claims, wherein the forming wire (118) is rotated about a longitudinal axis of the forming wire.

12. Method according to one of the preceding claims, wherein the nozzle body (152) with the material channel (154) is formed in such a way that the micro-tin drops (14), in particular during normal operation, can be produced at a pressure of more than 700 bar, preferably more than 1000 bar, in particular more than 1500 bar.

13. A method for generating plasma for emitting light within a wafer manufacturing apparatus, comprising the steps of: Production of micro-tin drops (14), exposure of the micro-tin drops (14) to a laser beam so that the micro-tin drops (14) are converted into plasma in order to provide light, in particular EUV light, for exposure to a wafer, wherein the micro-tin drops (14) are produced with a nozzle unit (150) consisting of formed glass.

14. Nozzle unit (150) for generating micro-tin drops (14) used to generate plasma for emitting light within a wafer manufacturing device, in particular manufactured by a method according to one of claims 1-12, comprising a nozzle body (152) with a material channel, wherein the nozzle unit (150) consists of formed glass.

15. A microchip manufactured by a method according to claim 13.

16. Manufacturing system (100) for producing a nozzle unit (150) for generating micro tin drops (14) used to generate plasma for emitting light within a wafer manufacturing device, comprising a tempering device (102) arranged and designed to heat a forming blank (130) consisting of a glass material on a forming temperature and / or to temper a nozzle body (152) consisting of a glass material to a cooling temperature, and a forming device (104) which is arranged and designed to form the forming blank (130) in such a way that the nozzle body (152) is designed to be suitable for producing micro-tin drops (14).

17. Device (1) for generating plasma for emitting light, in particular EUV light, for wafer production, comprising a drop generation unit (2) which is arranged and designed to generate micro-tin drops (14) with a nozzle unit (150) and to provide the micro-tin drops (14) to an application unit (12), - wherein the application unit (12) is arranged and designed to apply a laser beam to the micro-tin drops (14) so ​​that the micro-tin drops (14) are converted into plasma in order to provide light, in particular EUV light, for applying to a wafer, - wherein the nozzle unit (150) consists of formed glass.

Citation Information

Patent Citations

  • Apparatus for and method of accelerating droplets in a droplet generator for an EUV source

    WO2022002662A1

  • Pressure-energized ferrule for high pressure droplet generator nozzle

    WO2022268413A1

  • Systems and methods for protecting an EUV light source chamber from high pressure source material leaks

    US20100258747A1

  • Droplet generator nozzle

    US20220363596A1

  • Hybrid droplet generator for extreme ultraviolet light sources in lithographic radiation systems

    WO2021233645A1