Layered semiconductor device having organic coating with low refractive index

The integration of a low-index layer formed by co-depositing low-index and higher-index materials with phosphazene and fluorine-containing groups in semiconductor devices addresses the challenge of achieving low refractive index coatings compatible with mass production, enhancing light extraction and stability.

WO2024236546A1PCT designated stage expired Publication Date: 2024-11-21OTI LUMIONICS INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/IB2024/054834
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-05-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Existing semiconductor devices face challenges in achieving low refractive index coatings compatible with mass production processes without compromising electrical performance or requiring specialized equipment and solvents.

Method used

A layered semiconductor device with an organic coating comprising a mixture of low-index and higher-index materials, where the low-index layer is formed by co-depositing a low-index material with a higher-index material, specifically incorporating a phosphazene moiety and fluorine-containing functional groups, to achieve a refractive index reduction without affecting charge transport properties.

Benefits of technology

The solution enables the production of semiconductor devices with reduced refractive index coatings that are compatible with existing vacuum deposition equipment and processes, maintaining electrical performance while enhancing light extraction efficiency and device stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure IB2024054834_21112024_PF_FP_ABST
    Figure IB2024054834_21112024_PF_FP_ABST
Patent Text Reader

Abstract

An opto-electronic device comprises an anode, a cathode, and at least one semiconducting layer disposed therebetween. The at least one semiconducting layer comprises a low-index layer. The low-index layer comprises a mixture of a low-index material and a higher-index material. An absorption coefficient of the low-index layer in at least a sub-range of the visible spectrum is one of no more than about: 0.1, 0.08, 0.06, 0.05,.0.03, and 0.01.
Need to check novelty before this filing date? Find Prior Art

Description

LAYERED SEMICONDUCTOR DEVICE HAVING ORGANIC COATING WITH LOWREFRACTIVE INDEXRELATED APPLICATIONS

[0001] The present application claims the benefit of priority to U.S. Provisional Patent Application No. US 63 / 503,142 filed May 18, 2023, the contents of each of which are incorporated herein by reference in their entirety.TECHNICAL FIELD

[0002] The present disclosure relates to layered semiconductor devices, and in some non-limiting examples, to a layered opto-electronic device having a plurality of sub-pixel emissive regions and a plurality of light transmissive regions, each sub-pixel comprising first and second electrodes separated by a semiconducting layer, in which the semiconducting layer may be comprised of a material that has a substantially low refractive index.BACKGROUND

[0003] In an opto-electronic device such as an organic light emitting diode (OLED), at least one semiconducting layer comprising an emissive layer may be disposed between a pair of electrodes, such as an anode and a cathode. The anode and cathode may be electrically coupled with a power source and respectively generate holes and electrons that migrate toward each other through the at least one semiconducting layer. When a pair of holes and electrons combine, light, in the form of a photon, may be emitted by the emissive layer.

[0004] OLED display panels, such as an active-matrix OLED (AMOLED) panel, may comprise a plurality of pixels, each pixel further comprising a plurality of (including without limitation, one of three, and four) sub-pixels. In some non-limiting examples, the various sub-pixels of a pixel may be characterized by one of three, and four, different colors, including without limitation, R(ed), G(reen), and B(lue). Each (sub-) pixel may have an associated emissive region, comprising a stack of an associated pair of electrodes and at least one semiconducting layer between them. In some non-limiting examples, each sub-pixel of a pixel may emit light that have an associated wavelength spectrum characterized by a given color, including without limitation, one of, R(ed), G(reen), B(lue), and W(hite). In some non-limiting examples, the (sub- ) pixels may be selectively driven by a driving circuit comprising at least one thin-film transistor(TFT) structure electrically coupled with conductive metal lines, in some non-limiting examples, within a substrate upon which the electrodes and the at least one semiconducting layer are deposited. Various coatings (layers) of such panels may, in some non-limiting examples, be formed by vacuum-based deposition processes.

[0005] In AMOLED panels, light may be emitted by a sub-pixel when a voltage is applied across an anode and a cathode of the sub-pixel. By controlling the voltage applied across the anode and the cathode, it may be possible to control the emission of light from each sub-pixel of such panel. In cases where a common cathode is provided across multiple sub-pixels, the voltage across the anode and the cathode in each sub-pixel may be controlled by modulating the voltage of the anode. In some non-limiting examples, the adjacent anodes may be spaced apart in a lateral aspect, and at least one non-emissive region may be provided therebetween.

[0006] In commonly-assigned United States Patent Application Publication No. 2022 / 018702 entitled “Opto-Electronic Device Including a Low-Index Layer”, filed 24 July 2021 by HELANDER, Michael, et al., and published on 27 January 2022 (Helander No. 1), there is disclosed a semiconductor device having a plurality of layers that extend in an interface portion and a non-interface portion of at least one lateral aspect defined by a lateral axis of the device. A low(er)-index layer, that may comprise a low-index material, that has a first refractive index at a wavelength, is disposed on a first layer surface in at least the interface portion. A higher-index layer, that may comprise a high-index material, that has a second refractive index at a wavelength, is disposed on an exposed layer surface of the device, to define an index interface with the low(er)-index layer in the interface portion. The second refractive index exceeds the first refractive index. A quantity of deposited material may be disposed on a second layer surface in the non-interface portion. The higher-index layer may cover the deposited material in the non-interface portion.

[0007] In Helander No. 1, it was noted that, in some non-limiting examples, arranging the low(er)-index layer having a first refractive index (RI) that is lower than a second RI of the higher-index layer, such that it lies between an underlying layer and the higher-index layer, may exhibit enhanced outcoupling of EM radiation relative to an equivalent device that lacks such a low(er)-index layer therebetween, and thus, may increase a fraction of EM radiation that may be extracted from such a device. Helander No. 1 discloses that the first RI may be one of no more than about: 1.7, 1.6, 1.5, 1.45, 1.35, 1.3, and 1.25.

[0008] In some non-limiting examples, the organic materials of which the at least one semiconducting layer in an opto-electronic device may be composed, including without limitation, an OLED, may comprise a polycyclic aromatic compound. Polycyclic aromatic compounds have a substantially high RI in at least the visible spectrum.

[0009] In some non-limiting examples, organic materials that may typically be employed as a hole transport layer (HTL) material, including without limitation, a-NPD, may have a RI that is at least about 1.8 in the visible spectrum.

[0010] Those having ordinary skill in the relevant art will appreciate that, in some non-limiting examples, adding at least one functional group that has a low RI to an organic material may facilitate reducing the RI thereof.

[0011] Those having ordinary skill in the relevant art will appreciate that, in some non-limiting examples, adding at least one functional group that has a low RI, to a material, may reduce a charge carrier mobility of such material, which, in some non-limiting examples, when employed as at least one semiconducting layer in an OLED device, may be associated with reduced device performance.

[0012] In Yokoyama, Daisuke, et al., “Active refractive index control using a stably evaporable perfluororesin for high-outcoupling-efficiency organic light-emitting diodes”, J. Mater. Chem. C., 2021, 9, 11115, it is disclosed that the internal quantum efficiency of organic light-emitting diodes (OLEDs) has reached nearly 100%, and thus further improvement in the external quantum efficiency can be achieved only through outcoupling enhancement. However, light propagation in OLEDs for achieving high outcoupling has mainly been controlled not by the internal organic semiconductor layers but by external optical elements, which inevitably increase process cost. Here, a method is proposed for outcoupling enhancement that actively controls the refractive index of a hole transport layer (HTL) in OLEDs using a stably evaporable perfluororesin, which has a low refractive index and high amorphousness. The co-deposition of the perfluororesin with a hole transport material lowers the refractive index of the HTL to 1.56 at 550 nm without deteriorating the electrical properties. Owing to the nano-sized pillar-like phase separation between the perfluororesin and the hole transport material, the path of charge transport is retained. Using the low-index co-deposited HTL, a 1.22-fold enhancement of the outcoupling efficiency of a phosphorescent OLED is demonstrated. The proposed method can be generally applied to OLEDs to significantly enhance their outcoupling efficiency without increasingprocess cost. The results show the potential of active refractive index control as a major strategy for achieving further high-efficiency OLEDs.

[0013] In Kohnen, Anne, et al., “Enhanced efficiency of multilayer organic light-emitting diodes with a low-refractive index hole-transport layer: An effect of improved outcoupling?”, Applied Physics, 91, 113501-1, the authors report on an internal device modification for multilayer organic light-emitting diodes (OLEDs) with enhanced efficiency that promises high compatibility with conventional manufacturing processes. By copolymerization of a hole-conducting monomer with a compound possessing a lower refractive index, a hole-transport layer with reduced optical density but slightly reduced hole-transport properties is formed. Multilayer OLEDs based on this reduced-index layer show a 25% increased efficiency compared to reference devices. The results are compared to optical simulations of the dipole emission from thin organic films. It is found that the efficiency improvement is only to some extent due to enhanced outcoupling resulting directly from the reduced refractive index but primarily due to a change of the width of the emission zone.

[0014] In Li, X., “Performance enhancement of organic light-emitting diodes with an inorganically doped hole transport layer”, PhD Thesis, West Virginia University, 2016, the author aims to improve the OLED device lifetime by doping of organic hole transport materials with inorganic transition metal oxides (TMOs), and to reduce the cost by simplifying the device layer structure and manufacturing procedure. First, stress tests under continuous wave and pulsed currents were conducted to gain a better understanding of the key factors governing the degradation process of phosphorescent OLEDs. P-type doping of hole transport materials with TMOs was then developed as an effective way to reduce the interfacial energy barrier and the operational voltage of OLED devices. Finally, selective doping of organic materials with the TMOs was developed and the concept of delta doping was applied to OLEDs for the first time.

[0015] In US Patent No. 11,469,377 entitled “Composition, organic photoelectronic element, and production methods therefor”, filed 24 June 2019 by YOKOYAMA et al., and granted 11 October 2022, there is disclosed a composition having a very low refractive index, an organic photoelectronic element using the composition, and simple methods for producing such a composition and an organic photoelectronic element. There is also disclosed a composition comprising a fluorinated polymer, an organic semiconductor material and a dopant.

[0016] In Salehi, Amin, et al., “Suppressing evanescent loss in OLEDs using low refractive index ETL”, SPIE Invited Talk, August 2017, it is disclosed that a lower refractive index (RI) electron transport layer (ETL) increases outcoupling and decreases evanescent loss by (1) shifting radiation toward the outcoupled region, and (2) requiring a larger ETL thickness. Comparative studies of a low-RI 3TPYMB device and a T2T / NBPhen device showed that a maximum external quantum efficiency (EQE) of 21% was achieved using a 3TPYMB device, nearly 75% higher than a T2T / NBPhen device.

[0017] In Smith, L.H., et al., “Using a low-index host layer to increase emission from organic light-emitting diode structures”, Org. Electron., 2006, 7, 490, it is disclosed that the out-coupling efficiency of organic light-emitting diodes (OLEDs) may be significantly increased by use of a low-index host material for the organic emitters. The authors report on modelling undertaken for substrate-emitting and top-emitting OLED structures and show that up to a 2.5 fold increase in out-coupling efficiency, over that for structures containing a standard emissive layer, may be achieved in both cases. The relationship between radiation efficiency and refractive index varies for each type of structure and this is discussed, as is the nature of the electromagnetic (EM) modes supported.

[0018] In Salehi, Amin, et al., “Highly efficient organic light-emitting diode using a low refractive index electron transport Layer”, Adv. Opt. Mater., 2017, 5, 1700197, it is disclosed that a low refractive index electron transport layer (ETL) can be very effective in enhancing the out- coupling efficiency of an organic light-emitting diode (OLED). However, most organic films show a refractive index close to 1.8. In this work, it has been discovered that tri s-[3 -(3 - pyridyl)mesityl]borane (3TPYMB) has a low refractive index of 1.65 (at 550 nm), which is the lowest refractive index ETL among the commonly used ETLs up to date. Using 3TPYMB as an ETL, a solution processed OLED is demonstrated with nearly a 76% enhancement in external quantum efficiency (EQE). Optical simulation results of this study show that 59% of the enhancement comes from the low refractive index 3TPYMB, and the remaining 17% from the change in charge balance due to the 3TPYMB ETL in the OLED devices.

[0019] In Umbach, Thorsten Erich, et al., “Low-refractive index layers in organic light-emitting diodes via electrospray deposition for enhanced outcoupling efficiencies”, Adv. Eng. Mater., 2017, 5, 1700197, a novel technology for the enhancement of the outcoupling efficiency of OLED devices is presented. By means of electrospray deposition (ESD), the active hole-transport layer (HTL) is modified to have a reduced effective refractive index due to its porosity. A green-emitting stack is tailored to demonstrate this effect, whereas additional haze effects are to be prevented. The introduction of a low-index HTL results in a more efficient light extraction by a factor of 1.05, showing excellent agreement between experiment and simulation.

[0020] In Giebink, Chris, “Low refractive index OLEDs for practical high-efficiency outcoupling”, Final Project Report, U.S. Department of Energy, 2022, the author identified a small molecule that can be co-evaporated in the hole transport layer of OLEDs at high loading to reduce the refractive index by 0.2-0.3 refractive index units without degrading charge transport. Implementing this dilution molecule in the hole transport layer of a range of single and multistack OLEDs, the author demonstrated the ability to improve their internal light extraction by up to -35% without increasing their drive voltage or reducing their operational lifetime. Importantly, these findings extend to state-of-the-art device architectures with proprietary OLED materials.

[0021] In Baek, Heume-Il, et al., “Enhancement of the OLED driving stability by introducing an LiF-mixed a-NPD hole-transport layer”, Organic Light Emitting Materials and Devices X, 2006, 6333, 6333 IB-1, it is reported that the thermal stability of OLED device can be significantly enhanced by introducing an LiF-mixed N,N’-di(l-naphthyl)-N,N’ -diphenylbenzidine (a-NPD) as a HTL in the OLED having tris(8-hydroxy quinoline) aluminum (Alq3) as a light-emitting and electron-transport layer. Compared with the reference device with the a-NPD HTL, the device having a double layer of LiF-mixed a-NPD and a-NPD as a HTL showed an increased thermal stability up to 170°C without degrading the quantum efficiency of the electroluminescence. In addition, the driving voltage variation over time (less than 3 V) was significantly suppressed while the reference device shows a variation over 6 V. The improved device stability is attributed to the enhanced thermal stability of the LiF-mixed a-NPD layer, which could be estimated from the result that the film morphology of LiF-mixed a-NPD film was nearly unchanged after heated above the glass transition temperature of a-NPD while that of a-NPD film was significantly changed.

[0022] In EP Patent Publication No. 3406752 entitled “Method for preparing an electronic device, electronic device obtainable this way and compounds for use therein”, filed 22 May 2017 by SCHOLZ et al., and published 28 November 2018, there is disclosed a method comprising the steps: a) providing, in a vaporization source, a silsesquioxane compound represented by thegeneral formula SixRxOi 5x, wherein R is a terminal hydrocarbyl group covalently bonded to Si and the terminal hydrocarbyl group may comprise at least one heteroatom selected from the group consisting of B, Si, N, P, O and S and / or which may be substituted with at least one halogen atom; and x is selected from 6, 8, 10, 12, 14 and 16; and the silsesquioxane compound is substantially free of partially condensed silsesquioxanes; b) vaporizing the silsesquioxane compound by applying thermal energy thereto; c) depositing the vaporized silsesquioxane compound on a substrate, an electronic device obtainable this way and compounds for use therein.

[0023] In US Patent No. 9,755,165 entitled “Silsesquioxane compound, organic light emitting element, display apparatus, image information processing apparatus, and image forming apparatus”, filed 25 March 2014 by NISHIDE, Yosuke et al., and granted 5 September 2017, there is disclosed an organic light emitting element having high light emitting efficiency. The organic light emitting element includes: an anode; a cathode; an emission layer placed between the anode and the cathode; and a hole transport layer formed between the anode and the emission layer, in which the hole transport layer contains a siloxane compound and a compound having a tertiary arylamine structure; and number of SP2carbon atoms in the hole transport layer is ten times or less number of silicon atoms in the hole transport layer.

[0024] In US Patent No. 8,859, 110 entitled “Cyclic phosphazene compounds and use thereof in organic light emitting diodes”, filed 17 June 2009 by FUCHS, Evelyn et al., and granted 14 October 2014, there is disclosed an organic light-emitting diode comprising at least one cyclic phosphazene compound, a light-emitting layer formed from at least one matric material and at least one emitter material, wherein the at least one matrix material comprises at least one cyclic phosphazene compound, the use of cyclic phosphazene compounds in organic light-emitting diodes and a device selected from the group consisting of stationary visual display units, mobile visual display units and illumination units comprising at least one inventive organic lightemitting diode, and selected cyclic phosphazene compounds and processes for preparing them.

[0025] In JP Patent No. 1996283416 entitled “Cyclic phosphazene compound and organic thin film EL element”, filed 14 April 1995 by SHIGEHARA, Junko et al., and granted 02 September 2004, there is disclosed a novel cyclic phosphazene compound that has high heat resistance and amorphous stability, is free of unreacted residual chlorine and impurities, and can be used as an organic compound material for elements having optical and electronic functions, such as organicthin-film EL elements, organic thin-film solar cells, and electrophotographic photoreceptors. By using this cyclic phosphazene compound, problems of heat resistance, crystallization, and degradation due to unreacted residual chlorine and impurities are improved, and an organic thin- film EL element with high brightness and long life is provided.

[0026] In US Patent No. 7,612,500 entitled “Organic electroluminescence device”, filed 17 November 2006 by SOTOYAMA, Wataru and granted 3 November 2009, an organic electroluminescence device is disclosed including a pair of electrodes and at least one organic compound layer comprising a light-emitting layer between the pair of electrodes, wherein a refractive index of at least one of the light-emitting layer or an organic compound layer on the light extraction side of the light-emitting layer is 1.6 or less. An organic EL device in which luminescence can [be] extracted with high efficiency and luminescence of high brightness can be obtained.

[0027] In US Patent Application Publication No. 2023 / 0022628 entitled “Conductive film, optoelectronic device and conductive film manufacturing method”, filed 23 September 2022 by ABE, Takefumi, et al., and published 26 January 2023, there is disclosed a novel conductive film having two regions differing in the light transmittance, an optoelectronic device having such a conductive film, and a method for producing a conductive film by which such a conductive film can readily be produced. A conductive film, which has a first region and a second region having a light transmittance higher than the first region, the conductive film having a first film formed of a conductive material as a material and a resin film formed of a fluorinated polymer as a material, the first film being disposed to overlap with at least the first region among the first region and the second region, the resin film being disposed to overlap with the second region, and the fluorinated polymer satisfying the following (1) and (2): (1) when the temperature is increased at a temperature-increasing rate of 2°C. / min under a pressure of IxlO'3Pa, the temperature at which the thermogravimetric loss rate substantially reaches 100% is 400°C. or lower; (2) when the temperature is increased at a temperature-increasing rate of 2°C. / min under a pressure of IxlO'3Pa, the temperature width from a temperature at which the thermogravimetric loss rate is 10% to a temperature at which it is 90%, is within 200°C.

[0028] In CN Patent Application Publication No. 114600264 entitled “Porous film, organic optoelectronic device, and method for producing porous film”, filed 22 October 2020 by YOKOYAMA, Daisuke et al., and published 7 June 2022, there is disclosed a porous film whichuses an organic semiconductor as a material for forming the porous film and has a lower refractive index than the organic semiconductor. Further, an organic optoelectronic device having such a porous film is provided. Further, a method for producing a porous film is provided, which enables easy production of such a porous film. A porous film having an organic semiconductor as a material for forming the porous film and having a plurality of continuous pores extending in the film thickness direction.

[0029] In US Patent No. 11,355,734 entitled “Organic photoelectronic element comprising fluorinated polymer”, filed 3 February 2020 by ABE, Takefumi, et al., and granted 7 June 2022, there is disclosed an organic photoelectronic element, of which the external quantum efficiency is improved, the power consumption is low and the service life is prolonged. The organic photoelectronic element comprises a substrate, an anode provided on the substrate, a cathode facing the anode, a light emitting layer disposed between t he anode and the cathode, and a hole transport layer provided in contact with t he light emitting layer between the light emitting layer and the anode, wherein the hole transport layer contains an organic semiconductor material and a fluorinated polymer, and at the surface of the hole transport layer in contact with the light emitting layer, the fluorinated polymer is present.

[0030] In US Patent Application Publication No. 2022 / 0372186 entitled “Fluorine-containing polymer, film, film manufacturing method, and organic opto-electronic element”, filed 3 August 2022 by ABE, Takefumi, et al., and published 24 November 2022, there is disclosed a fluorinated polymer suitable for deposition. A film containing such a fluorinated polymer as a material is provided. A method for producing a film, by which such a film can readily be produced, is provided. Further, an organic photoelectronic element having such a film in its structure is provided. A fluorinated polymer is disclosed which satisfies the following requirements (1) to (3): (1) the melting point is 200°C. or higher, (2) the thermogravimetric loss rate when the temperature is increased at a temperature-increasing rate of 2°C. / min under a pressure of IxlO'3pa, substantially reaches 100% at 400°C. or lower, (3) when the temperature is increased at a temperature-increasing rate of 2°C. / min under a pressure of IxlO'3Pa, the temperature width from a temperature at which the thermogravimetric loss rate is 10% to a temperature at which it is 90%, is within 100°C.

[0031] In US Patent No. 8,530,888 entitled “Organic light-emitting display device and method of manufacturing the same”, filed 23 February 2011 by JEONG, Hee-Seong, et al., and granted 10September 2013, there is disclosed an organic light-emitting display device that includes a substrate, a first electrode on the substrate, the first electrode including a reflection film, a hole injection layer on the first electrode, a hole transport layer on t he hole injection layer, an emission layer on the hole transport layer, an electron injection transport layer on the emission layer, a second electrode on the electron injection transport layer, the second electrode including a semi-transmissive reflective material, and a control layer positioned between a lower surface of the hole injection layer and an upper surface of the hole transport layer, the control layer including an organic material and having a refractive index lower than that of an adjacent layer.

[0032] In some non-limiting examples, there may be an aim to lower the RI of a coating comprising an organic material without altering a molecular structure of the material.

[0033] In various references, it is disclosed that in some non-limiting examples, an RI of a coating comprising an organic material may be reduced by mixing the organic material with a material having a lower RI, including without limitation, air (including without limitation porous coatings), polymers (including without limitation polytetrafluoroethylene (PTFE)), and ionic compounds (including without limitation lithium fluoride (LiF)).

[0034] However, in some non-limiting examples, such lower RI materials may have limited applicability for use in existing mass production equipment and processes. In some non-limiting examples, deposition of porous coatings may call for specialized deposition equipment that may be substantially incompatible with existing production equipment and processes. In some nonlimiting examples, polymers, including without limitation, PTFE, may be substantially incompatible with deposition using existing vacuum deposition equipment and, in some nonlimiting examples, may call for unique solvents for cleaning of shadow masks, including without limitation, fine metal masks (FMMs) typically used to pattern different layers of a semiconductor device. In some non-limiting examples, ionic compounds, including without limitation, LiF, may interact with the organic material, which may alter at least one of the charge carrier transport, and the charge carrier transport, such that electrical performance of a device constructed therewith may be reduced.

[0035] In some non-limiting examples, there may be an aim to develop an organic coating having a low RI that may be compatible with existing vacuum deposition equipment and processes used in mass production of semiconductor devices.

[0036] In some non-limiting examples, there may be an aim to develop an organic coating having a low RI that may not call for unique solvents for cleaning of shadow masks used to deposit the organic coating.

[0037] In some non-limiting examples, there may be an aim to develop an organic coating having a low RI that may not call for high temperature deposition.

[0038] In some non-limiting examples, there may be an aim to develop an organic coating having a low RI that may not reduce electrical performance of a device constructed therewith.BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Examples of the present disclosure will now be described by reference to the following figures, in which identical reference numerals in different figures indicate at least one of: identical, and in some non-limiting examples, at least one of: analogous, and corresponding elements, and in which:

[0040] FIG. l is a simplified block diagram from a longitudinal aspect, of an example device having a plurality of layers in a lateral aspect, formed by selective deposition of a patterning coating in a first portion of the lateral aspect, followed by deposition of a closed coating of deposited material in a second portion thereof, according to an example in the present disclosure;

[0041] FIG. 2 is a simplified diagram, from a longitudinal aspect, of an example version of the device of FIG. 1, in which the closed coating of deposited material in the second portion forms a second electrode of an opto-electronic device, according to an example in the present disclosure;

[0042] FIG. 3 is a schematic diagram illustrating an example cross-sectional view of an example display panel having a plurality of layers, comprising at least one aperture therewithin, through which at least one electromagnetic signal may be exchanged according to an example in the present disclosure;

[0043] FIG. 4 is a schematic diagram showing an example process for depositing a patterning coating in a pattern on an exposed layer surface of an underlying layer in an example version of the device of FIG. 1, according to an example in the present disclosure;

[0044] FIG. 5 is a schematic diagram showing an example process for depositing a deposited material in the second portion on an exposed layer surface that comprises the deposited pattern of the patterning coating of FIG. 3, where the patterning coating is a nucleation-inhibiting coating (NIC);

[0045] FIGs. 6A-6B are schematic diagrams illustrating example devices used to examine the effects of providing a low-index layer as part of an HTL on a longitudinal, and a lateral, I-V characteristic of a semi-conducting device. FIGs. 6C-6D show longitudinal, and lateral, I-V curves obtained using the devices of FIGs. 6A-6B.

[0046] FIG. 7A is a schematic diagram illustrating an example version of the device of FIG. 1 in a cross-sectional view;

[0047] FIG. 7B is a schematic diagram illustrating the device of FIG. 7A in a complementary plan view;

[0048] FIGs. 8A-8B are schematic diagrams that show various potential behaviours of a patterning coating at a deposition interface with a deposited layer in an example version of the device of FIG. 1 according to various examples in the present disclosure;

[0049] FIGs. 9A-9H are simplified block diagrams from a cross-sectional aspect, of example versions of the device of FIG. 1, showing various examples of possible interactions between the particle structure patterning coating and the particle structures according to examples in the present disclosure;

[0050] FIG. 10 is a schematic diagram illustrating an example cross-sectional view of an example version of the device of FIG. 2 with additional example deposition steps according to an example in the present disclosure;

[0051] FIG. 11 is a schematic diagram that may show example stages of an example process for manufacturing an example version of an OLED device having sub-pixel regions having a second electrode of different thickness according to an example in the present disclosure;

[0052] FIG. 12 is a schematic diagram illustrating an example cross-sectional view of an example version of an OLED device in which a second electrode is coupled with an auxiliary electrode according to an example in the present disclosure;

[0053] FIG. 13 is a schematic diagram illustrating an example cross-sectional view of an example version of an OLED device having a partition and a shaded region, such as a recess, in a non-emissive region thereof according to an example in the present disclosure;

[0054] FIGs. 14A-14B are schematic diagrams that show example cross-sectional views of an example OLED device having a partition and a shaded region, such as an aperture, in a non- emissive region, according to various examples in the present disclosure;

[0055] FIG. 15 is an example energy profile illustrating energy states of an adatom absorbed onto a surface according to an example in the present disclosure;

[0056] FIG. 16 is a schematic diagram illustrating the formation of a film nucleus according to an example in the present disclosure; and

[0057] FIG. 17 is a block diagram of an example computer device within a computing and communications environment that may be used for implementing devices and methods in accordance with representative examples of the present disclosure.

[0058] In the present disclosure, some elements / features may be identified by a reference numeral that may not be shown in any of the figures provided herein.

[0059] In the present disclosure, a reference numeral having at least one of at least one numeric value (including without limitation, in at least one of superscript, and subscript), and at least one alphabetic character (including without limitation, in lower-case) appended thereto, may be considered to refer to at least one of a particular instance, and subset thereof, of the feature (element) described by the reference numeral. Reference to the reference numeral without reference to the at least one of the appended value(s), and the character(s), may, as the context dictates, refer generally to the feature(s) described by at least one of the reference numeral, and the set of all instances described thereby. Similarly, a reference numeral may have the letter “x’ in the place of a numeric digit. Reference to such reference numeral may, as the context dictates, refer generally to feature(s) described by the reference numeral, where the character “x” is replaced by at least one of a numeric digit, and the set of all instances described thereby.

[0060] In the present disclosure, for purposes of explanation and not limitation, specific details are set forth to provide a thorough understanding of the present disclosure, including without limitation, particular architectures, interfaces and techniques. In some instances, detailed descriptions of well-known systems, technologies, components, devices, circuits, methods, and applications are omitted to not obscure the description of the present disclosure with unnecessary detail.

[0061] Further, it will be appreciated that block diagrams reproduced herein can represent conceptual views of illustrative components embodying the principles of the technology.

[0062] Accordingly, the system and method components have been represented where appropriate by conventional symbols in the drawings, showing only those specific details that arepertinent to understanding the examples of the present disclosure, to not obscure the disclosure with details that will be readily apparent to those of ordinary skill in the art having the benefit of the description herein.

[0063] Any drawings provided herein may not be drawn to scale and may not be considered to limit the present disclosure in any way.

[0064] Any feature shown in dashed outline may in some examples be considered as optional.SUMMARY

[0065] An opto-electronic device comprises an anode, a cathode, and at least one semiconducting layer disposed therebetween. The at least one semiconducting layer comprises a low-index layer. The low-index layer comprises a mixture of a low-index material and a higher-index material.

[0066] An opto-electronic device comprising: an anode; a cathode; and at least one semiconducting layer disposed between the anode and the cathode, the at least one semiconducting layer comprising a low-index layer; wherein: the low-index layer comprises a mixture of a low-index material and a higher-index material, wherein the low-index material comprises a phosphazene moiety and at least one fluorine (F)-containing functional group attached thereto.

[0067] In some non-limiting examples, an absorption coefficient of the low-index layer in at least a sub-range of the visible spectrum may be one of no more than about: 0.1, 0.08, 0.06, 0.05, 0.03, and 0.01.

[0068] In some non-limiting examples, a refractive index of the low-index layer may be no more than a refractive index of at least one layer arranged adjacent thereto.

[0069] In some non-limiting examples, a refractive index of the low-index layer in at least a subrange of the visible spectrum may be one of no more than about: 1.8, 1.75, 1.7, 1.65, 1.6, 1.55, 1.5, 1.45, and 1.4.

[0070] In some non-limiting examples, a characteristic refractive index of the low-index material, in at least a sub-range of the visible spectrum, may be no more than a characteristic refractive index of the higher-index material, by one of at least about: 0.1, 0.15, 0.2, 0.25, 0.3, 0.4, and 0.5.

[0071] In some non-limiting examples, a characteristic refractive index of the low-index material, in at least a sub-range of the visible spectrum, may be one of no more than about: 1.6, 1.55, 1.5, 1.45, 1.4, 1.35, and 1.3.

[0072] In some non-limiting examples, a characteristic refractive index of the higher-index material, in at least a sub-range of the visible spectrum, may be one of at least about: 1.8, 1.85, and 1.9.

[0073] In some non-limiting examples, the low-index layer may comprise, by at least one of: volume percentage, weight percentage, and mole percentage, the low-index material in a concentration of one of no more than about: 80, 75, 70, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 13, 10, 8, and 5%.

[0074] In some non-limiting examples, the low-index layer may comprise, by at least one of: volume percentage, weight percentage, and mole percentage, the low-index material in a concentration of one of at least about: 1, 3, 5, 8, 10, 15, 20, 25, 30, 35, 40, 45, and 50%.

[0075] In some non-limiting examples, the low-index material may have a band gap of one of at least about 3.4, 3.5, 4.1, 5, and 6.2, eV.

[0076] In some non-limiting examples, the low-index material may be one of: a small molecule, and an oligomer.

[0077] In some non-limiting examples, the low-index material may be an organic-inorganic hybrid material.

[0078] In some non-limiting examples, a molecular structure of the low-index material may comprise at least one of a: cyclophosphazene, fluoroalkyl, and silsesquioxane, moiety.

[0079] In some non-limiting examples, the low-index layer may comprise, by weight percentage, a low-index material comprising a cyclophosphazene moiety, in a concentration of between about 1-20%.

[0080] In some non-limiting examples, the low-index material may comprise, by weight percentage, F, in a concentration of between about 10-50%.

[0081] In some non-limiting examples, a molecular structure of the low-index material may comprise a low surface tension moiety.

[0082] In some non-limiting examples, the molecular structure of the low-index material may comprise a high surface tension moiety bonded to the low surface tension moiety.

[0083] In some non-limiting examples, the low surface tension moiety may comprise at least one of a: F, and silicon (Si), -containing moiety.

[0084] In some non-limiting examples, the F-containing moiety may be a fluoroalkyl moiety.

[0085] In some non-limiting examples, the Si-containing moiety may be a siloxyl moiety.

[0086] In some non-limiting examples, at least one of an: electron, and hole, mobility of the low- index layer may be at least about 10'5.

[0087] In some non-limiting examples, a solubility, in N-methyl-2-pyrrolidone, of at least one of the: low-index material, and higher-index layer, may be at least about 1 mg / mL.

[0088] In some non-limiting examples, the higher-index material may comprise an organic semiconducting material.

[0089] In some non-limiting examples, the organic semiconducting material may comprise a polycyclic aromatic moiety.

[0090] In some non-limiting examples, the organic semiconducting material may be a hole transport material.

[0091] In some non-limiting examples, the at least one semiconducting layer may comprise an emissive layer (EML) and the device may be configured to emit light therefrom in response to an electrical current being applied thereto.

[0092] In some non-limiting examples, the device may be a top-emission device, and the light emitted by the EML may be transmitted through the cathode.

[0093] In some non-limiting examples, the low-index layer may be arranged between the EML and the anode.

[0094] In some non-limiting examples, the low-index layer may form at least a part of a hole transport layer (HTL).

[0095] In some non-limiting examples, the at least one semiconducting layer may further comprise a hole injection layer (HIL) arranged between the EML and the anode, wherein the low-index layer is arranged between the HIL and the EML.

[0096] In some non-limiting examples, the functional group may independently comprise at least one of: F, chlorine (Cl), a hydroxyl group, a substituted alkyl group, an unsubstituted alkyl group, a substituted fluoroalkyl group, an unsubstituted fluoroalkyl group, a substituted cycloalkyl group, an unsubstituted cycloalkyl group, a substituted fluorocycloalkyl group, an unsubstituted fluorocycloalkyl group, a substituted heterocycloalkyl group, an unsubstituted heterocycloalkyl group, a substituted fluoroheterocycloalkyl group, an unsubstituted fluoroheterocycloalkyl group, a substituted alkoxy group, an unsubstituted alkoxy group, a substituted fluoroalkoxy group, an unsubstituted fluoroalkoxy group, a substituted aryloxy group, an unsubstituted aryloxy group, a substituted fluoroaryloxy group, an unsubstituted fluoroaryloxy group, a substituted heteroaryloxy group, a unsubstituted heteroaryloxy group, a substituted fluoroheteroaryl oxy group, a unsubstituted fluoroheteroaryl oxy group, a substituted aryl group, an unsubstituted aryl group, a substituted fluoroaryl group, an unsubstituted fluoroaryl group, a substituted alkyl silyl group, an unsubstituted alkylsilyl group, a substituted alkylsiloxy group, an unsubstituted alkylsiloxy group, an amino group, an amine group, an alkylamine group, an arylamine group, a cyano group, a phosphazo group, a sulfanyl group, a pentafluorosulfanyl group, a sulfide group, a sulfonyl group, a thiol group, an alkylthio group, a trifluoromethylthio group, a carbonyl group, a siloxane group, a silane group, and an organosilicon group.

[0097] In some non-limiting examples, the functional group may comprise: a linker moiety RB, a terminal moiety RT, and an intermediate moiety RDarranged between the linker moiety RBand the terminal moiety RT,' wherein: the linker moiety RBcomprises one of: O, N, sulfur (S), a substituted alkylene, an unsubstituted alkylene, a substituted fluoroalkylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted arylene, an unsubstituted arylene, a substituted heteroarylene, and an unsubstituted heteroarylene; the intermediate moiety RDcomprises: O, an ether, a substituted alkylene, an unsubstituted alkylene, a substituted fluoroalkylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted arylene, an unsubstituted arylene, a substituted phenyl, an unsubstituted phenyl, a substituted biphenyl, an unsubstituted biphenyl, a substituted binaphthalene, an unsubstituted binaphthalene, a substituted heteroarylene, and an unsubstituted heteroarylene; and the terminal moiety RTcomprises at least one of: a substituted alkyl, an unsubstituted alkyl, a branched fluoroalkyl, an unbranched fluoroalkyl, a substituted heterocycloalkyl, an unsubstituted heterocycloalkyl, a substituted alkoxy, an unsubstitutedalkoxy, a branched silyloxy, an unbranched silyloxy, a branched fluoroalkoxy, an unbranched fluoroalkoxy, a fluoroaryl, a polyfluorosulfanyl, and a fluorocycloalkyl.

[0098] In some non-limiting examples, the linker moiety RBmay be selected from: -O-, and -O- CH2-.The device of any one of claims 1 through 32, wherein the at least one F-containing functional group is represented by Chemical Formula (VII):where: p is an integer between about 1-5; q is an integer between about 6-20; and Z represents one of: H, and F.

[0099] In some non-limiting examples, / ? may be 1, and q may be an integer between about 6-20.DESCRIPTIONLayered Device

[0100] Turning now to FIG. 1, the present disclosure relates generally to layered semiconductor devices 100, and more specifically, to opto-electronic devices 200 (FIG. 2). An opto-electronic device 200 may generally encompass any device 100 that converts electrical signals into light in the form of photons and vice versa. In some non-limiting examples, an optoelectronic device 200 may comprise an organic light-emitting diode (OLED).

[0101] Those having ordinary skill in the relevant art will appreciate that, while the present disclosure is directed to opto-electronic devices 200, the principles thereof may, in some non-limiting examples, be applicable to any panel having a plurality of layers, including without limitation, at least one layer of conductive deposited material 531 (FIG. 5), including as a thin film, and in some non-limiting examples, through which electromagnetic (EM) signals may pass, including without limitation, one of partially, and entirely, at a non-zero angle relative to a plane of at least one of the layers.

[0102] In FIG. 1, there may be shown a cross-sectional view of an example layered semiconductor device 100. In some non-limiting examples, as shown in greater detail in FIG. 2, the device 100 may comprise a plurality of layers deposited upon a substrate 10.

[0103] A first lateral axis, identified as the X-axis, may be shown, together with a longitudinal axis, identified as the Z-axis. A second lateral axis, identified as the Y-axis, may beshown as being substantially transverse to both the X-axis and the Z-axis. At least one of the lateral axes may define a lateral aspect of the device 100. The longitudinal axis may define a longitudinal aspect of the device 100.

[0104] The layers of the device 100 may extend, in the lateral aspect, substantially parallel to a plane defined by the lateral axes. Those having ordinary skill in the relevant art will appreciate that the substantially planar representation shown in FIG. 1 may be, in some nonlimiting examples, an abstraction for purposes of illustration. In some non-limiting examples, there may be, across a lateral extent of the device 100, localized substantially planar strata of different thicknesses and dimension, including, in some non-limiting examples, the substantially complete absence of at least one layer separated by non-planar transition areas (including lateral gaps and even discontinuities).

[0105] Thus, while for illustrative purposes, the device 100 may be shown in its longitudinal aspect as a substantially stratified structure of substantially parallel planar layers, such device 100 may illustrate locally, a diverse topography to define features, each of which may substantially exhibit the stratified profile discussed in the longitudinal aspect.

[0106] In some non-limiting examples, a lateral aspect of an exposed layer surface 11 of the device 100 may comprise a first portion 101 and a second portion 102. In some non-limiting examples, the second portion 102 may comprise that part of the exposed layer surface 11 of the device 100 that lies beyond the first portion 101. As shown in FIG. 1, the layers of the device 100 may comprise a substrate 10, and a patterning coating 110 disposed on an exposed layer surface 11 of at least a portion of the lateral aspect thereof. In some non-limiting examples, the patterning coating 110 may be limited in its lateral extent to the first portion 101 and a deposited layer 130 may be disposed as a closed coating 140 on an exposed layer surface 11 of the device 100 in a second portion 102 of its lateral aspect.

[0107] In some non-limiting examples, at least one particle structure 150 may be disposed as a discontinuous layer 160 on the exposed layer surface 11 of the patterning coating 110. In some non-limiting examples, although not shown, at least one of: the patterning coating 110, the deposited layer 130, and at least one particle structure 150, may be deposited on a layer (underlying layer 810 (FIG. 8A)) other than the substrate 10 including without limitation, an intervening layer between the substrate 10 and at least one of: the patterning coating 110, deposited layer 130, and the at least one particle structure 150. In some non-limiting examples,the underlying layer 810 may comprise at least one of: an orientation layer, and an organic supporting layer.

[0108] In some non-limiting examples, at least one of: the patterning coating 110, the deposited layer 130, and the at least one particle structure 150, may be covered by at least one overlying layer 170.

[0109] In some non-limiting examples, such overlying layer 170 may comprise at least one of: an encapsulation layer and an optical coating. In some non-limiting examples, the encapsulation layer may comprise at least one of: a glass cap, a barrier film, a barrier adhesive, a barrier coating, an encapsulation layer, and a thin film encapsulation (TFE) layer, provided to encapsulate the device 100. In some non-limiting examples, the optical coating may comprise: at least one of: an optical, and structural, coating, and at least one component thereof, including without limitation, a polarizer, a color filter, an anti-reflection coating, an anti-glare coating, cover glass, and an optically clear adhesive (OCA).

[0110] In some non-limiting examples, at least one of: a substantially thin patterning coating 110 in the first portion 101, and a deposited layer 130 in the second portion 102, may provide a substantially planar surface on which the overlying layer 170 may be deposited. In some non-limiting examples, providing such a substantially planar surface for application of such overlying layer 170 may increase adhesion thereof to such surface.

[0111] In some non-limiting examples, the optical coating may be used to modulate optical properties of light being at least one of: transmitted, emitted, and absorbed, by the device 100, including without limitation, plasmon modes. In some non-limiting examples, the optical coating may be used as at least one of: an optical filter, index-matching coating, optical outcoupling coating, scattering layer, diffraction grating, and parts thereof.

[0112] In some non-limiting examples, the optical coating may be used to modulate at least one optical microcavity effect in the device 100 by, without limitation, tuning at least one of: the total optical path length, and the refractive index thereof. At least one optical property of the device 100 may be affected by modulating at least one optical microcavity effect including without limitation, the output light, including without limitation, at least one of: an angular dependence of an intensity thereof, and a wavelength shift thereof. In some non-limiting examples, the optical coating may be a non-electrical component, that is, the optical coating maynot be configured to at least one of: conduct, and transmit, electrical current during normal device operations.

[0113] In some non-limiting examples, the optical coating may be formed of any deposited material 531, and in some non-limiting examples, may employ any mechanism of depositing a deposited layer 130 as described herein.Opto-Electronic Device

[0114] FIG. 2 is a simplified block diagram from a longitudinal aspect, of an example opto-electronic device 200, which may be, in some non-limiting examples, an electro-luminescent device 200, according to the present disclosure. In some non-limiting examples, the device 200 may be an OLED.

[0115] The device 200 may comprise a substrate 10, upon which a frontplane 201, comprising a plurality of layers, respectively, a first electrode 220, at least one semiconducting layer 230, and a second electrode 240, may be disposed. In some non-limiting examples, the frontplane 201 may provide mechanisms for at least one of emission of EM radiation, including without limitation, photons, and manipulation of emitted EM radiation.

[0116] In some non-limiting examples, various coatings of such devices 200 may be formed by vacuum-based deposition processes.

[0117] In some non-limiting examples, the second electrode 240 may extend partially over the patterning coating 110 in a transition region 245.

[0118] In some non-limiting examples, at least one particle structure 150 of a discontinuous layer 160 of a material of which the deposited layer 130 may be comprised (deposited material 531) may extend partially over the patterning coating 110, which may act as a particle structure patterning coating 110pin the transition region 245. In some non-limiting examples, such discontinuous layer 160 may form at least a part of the second electrode 240.

[0119] In some non-limiting examples, the device 200 may be electrically coupled with a power source. When so coupled, the device 200 may emit EM radiation, including without limitation, photons, as described herein.Substrate

[0120] In some non-limiting examples, the substrate 10 may comprise a base substrate 215. In some non-limiting examples, the base substrate 215 may be formed of material suitable for use thereof, including without limitation, at least one of: an inorganic material, including without limitation, at least one of: silicon (Si), glass, metal (including without limitation, a metal foil), sapphire, and other inorganic material, and an organic material, including without limitation, a polymer, including without limitation, at least one of: a polyimide, and an Si-based polymer. In some non-limiting examples, the base substrate 215 may be one of: rigid, and flexible. In some non-limiting examples, the substrate 10 may be defined by at least one planar surface. In some non-limiting examples, the substrate 10 may have at least one exposed layer surface 11 that supports the remaining frontplane 201 components of the device 200, including without limitation, at least one of: the first electrode 220, the at least one semiconducting layer 230, and the second electrode 240.

[0121] In some non-limiting examples, such surface may be at least one of: an organic surface, and an inorganic surface.

[0122] In some non-limiting examples, the substrate 10 may comprise, in addition to the base substrate 215, at least one additional at least one of: organic, and inorganic, layer (not shown nor specifically described herein) supported on an exposed layer surface 11 of the base substrate 215.

[0123] In some non-limiting examples, such additional layers may comprise at least one organic layer, which may at least one of: comprise, replace, and supplement, at least one of the semiconducting layers 230.

[0124] In some non-limiting examples, such additional layers may comprise at least one inorganic layer, which may comprise, at least one electrode, which in some non-limiting examples, may at least one of: comprise, replace, and supplement, at least one of: the first electrode 220, and the second electrode 240.Backplane and TFT structure(s) embodied therein

[0125] In some non-limiting examples, such additional layers may comprise a backplane 202. In some non-limiting examples, the backplane 202 may comprise at least one of: power circuitry, and switching elements for driving the device 200, including without limitation, at leastone of: at least one electronic thin-film transistor (TFT) structure 206, and at least one component thereof, that may be formed by a photolithography process.

[0126] In some non-limiting examples, the backplane 202 of the substrate 10 may comprise at least one electronic, including without limitation, an opto-electronic, component, including without limitation, one of: transistors, resistors, and capacitors, such as which may support the device 200 acting as one of: an active-matrix, and a passive matrix, device 200. In some non-limiting examples, such structures may be a TFT structure 206.

[0127] In some non-limiting examples, TFT structures 206 may comprise one of: topgate, bottom-gate, n-type and p-type TFT structures 206. In some non-limiting examples, the TFT structure 206 may incorporate one of: amorphous Si (a-Si), indium gallium zinc oxide (IGZO), and low-temperature polycrystalline Si (LTPS).First Electrode

[0128] The first electrode 220 may be deposited over the substrate 10. In some nonlimiting examples, the first electrode 220 may be electrically coupled with at least one of: a terminal of the power source, and ground. In some non-limiting examples, the first electrode 220 may be so coupled through at least one driving circuit which in some non-limiting examples, may incorporate at least one TFT structure 206 in the backplane 202 of the substrate 10.

[0129] In some non-limiting examples, the first electrode 220 may comprise one of: an anode, and cathode. In some non-limiting examples, the first electrode 220 may be an anode.

[0130] In some non-limiting examples, the first electrode 220 may be formed by depositing at least one thin conductive film, over (a part of) the substrate 10. In some nonlimiting examples, there may be a plurality of first electrodes 220, disposed in a spatial arrangement over a lateral aspect of the substrate 10. In some non-limiting examples, at least one of such at least one first electrodes 220 may be deposited over (a part of) a TFT insulating layer 207 disposed in a lateral aspect in a spatial arrangement. If so, in some non-limiting examples, at least one of such at least one first electrodes 220 may extend through an opening of the corresponding TFT insulating layer 207 to be electrically coupled with an electrode of the TFT structures 206 in the backplane 202.

[0131] In some non-limiting examples, at least one of: the at least one first electrode 220, and at least one thin film thereof, may comprise various materials, including without limitation,at least one metallic material, including without limitation, at least one of: magnesium (Mg), aluminum (Al), calcium (Ca), zinc (Zn), silver (Ag), cadmium (Cd), barium (Ba), and ytterbium (Yb), including without limitation, alloys comprising any of such materials, at least one metal oxide, including without limitation, a transparent conducting oxide (TCO), including without limitation, ternary compositions such as, without limitation, at least one of: FTO, IZO, and ITO, in varying proportions, including without limitation, combinations of any plurality thereof in at least one layer, any at least one of which may be, without limitation, a thin film.Second Electrode

[0132] The second electrode 240 may be deposited over the at least one semiconducting layer 230. In some non-limiting examples, the second electrode 240 may be electrically coupled with at least one of: a terminal of the power source, and ground. In some non-limiting examples, the second electrode 240 may be so coupled through at least one driving circuit, which in some non-limiting examples, may incorporate at least one TFT structure 206 in the backplane 202 of the substrate 10.

[0133] In some non-limiting examples, the second electrode 240 may comprise one of: an anode, and a cathode. In some non-limiting examples, the second electrode 240 may be a cathode.

[0134] In some non-limiting examples, the second electrode 240 may be formed by depositing a deposited layer 130, in some non-limiting examples, as at least one thin film, over (a part of) the at least one semiconducting layer 230.

[0135] In some non-limiting examples, the deposited layer 130 may be deposited in a second portion 102, by exposing the exposed layer surface 11 of the device 200, which may, in some non-limiting examples, comprise the at least one semiconducting layer 230, to a vapor flux 412 (FIG. 4) of a patterning material 411 (FIG. 4), including without limitation, using a shadow mask 415 (FIG. 4), to form a patterning coating 110 in the first portion 101. Whether a shadow mask 415 is employed, in some non-limiting examples, as shown in FIG. 2, the patterning material 110 may be restricted, in its lateral aspect, substantially to an emissive region 210 or a non-emissive region 211, including without limitation, at least one signal -transmissive region 212 located therein.

[0136] In some non-limiting examples, there may be a plurality of second electrodes 240, disposed in a spatial arrangement over a lateral aspect of the at least one semiconducting layer 230.

[0137] In some non-limiting examples, the at least one second electrode 240 may comprise various materials, including without limitation, at least one metallic material, including without limitation, at least one of: Mg, Al, Ca, Zn, Ag, Cd, Ba, and Yb, including without limitation, alloys comprising at least one of: any of such materials, at least one metal oxide, including without limitation, a TCO, including without limitation, ternary compositions such as, without limitation, at least one of: fluorine tin oxide (FTO), indium zinc oxide (IZO), and indium tin oxide (ITO), including without limitation, in varying proportions, zinc oxide (ZnO), and other oxides comprising at least one of: indium (In), and Zn, in at least one layer, and at least one non- metallic material, any of which may be, without limitation, a thin conductive film. In some nonlimiting examples, for a Mg:Ag alloy, such alloy composition may range between about 1 :9-9: 1 by volume.

[0138] In some non-limiting examples, the deposition of the second electrode 240 may be performed using one of: an open mask, and a mask-free, deposition process.

[0139] In some non-limiting examples, the second electrode 240 may comprise a plurality of such coatings. In some non-limiting examples, such coatings may be distinct coatings disposed on top of one another.

[0140] In some non-limiting examples, the second electrode 240 may comprise a Yb / Ag bi-layer coating. In some non-limiting examples, such bi-layer coating may be formed by depositing a Yb coating, followed by an Ag coating. In some non-limiting examples, a thickness of such Ag coating may exceed a thickness of the Yb coating.

[0141] In some non-limiting examples, the second electrode 240 may be a multi-coating electrode 240 comprising a plurality of one of: a metallic coating, and an oxide coating.

[0142] In some non-limiting examples, the second electrode 240 may comprise a fullerene and Mg.

[0143] In some non-limiting examples, such coating may be formed by depositing a fullerene coating followed by an Mg coating. In some non-limiting examples, a fullerene may be dispersed within the Mg coating to form a fullerene-containing Mg alloy coating. Non-limitingexamples of such coatings are described in at least one of: United States Patent Application Publication No. 2015 / 0287846 published 8 October 2015, and in PCT International Application No. PCT / IB2017 / 054970 filed 15 August 2017 and published as W02018 / 033860 on 22 February 2018.Semiconducting layer

[0144] In some non-limiting examples, the at least one semiconducting layer 230 may comprise a plurality of layers 231, 233, 235, 237, 239, any of which may be disposed, in some non-limiting examples, in a thin film, in a stacked configuration, which may include, without limitation, at least one of: a hole injection layer (HIL) 231, a hole transport layer (HTL) 233, an emissive layer (EML) 235, an electron transport layer (ETL) 237, and an electron injection layer (EIL) 239.

[0145] In some non-limiting examples, the at least one semiconducting layer 230 may form a “tandem” structure comprising a plurality of EMLs 235. In some non-limiting examples, such tandem structure may also comprise at least one charge generation layer (CGL).

[0146] Those having ordinary skill in the relevant art will readily appreciate that the structure of the device 200 may be varied by one of: omitting, and combining, at least one of the semiconductor layers 231, 233, 235, 237, 239.

[0147] In some non-limiting examples, any of the layers 231, 233, 235, 237, 239 of the at least one semiconducting layer 230 may comprise any number of sub-layers. In some nonlimiting examples, any of such layers 231, 233, 235, 237, 239, including without limitation, sublayers) thereof may comprise various ones of: a mixture, and a composition gradient. In some non-limiting examples, although not shown, the device 200 may comprise at least one layer comprising one of: an inorganic, and an organometallic, material, and may not be necessarily limited to devices 200 comprised solely of organic materials. In some non-limiting examples, the device 200 may comprise at least one quantum dot (QD).

[0148] In some non-limiting examples, the HIL 231 may be formed using a hole injection material, which may, in some non-limiting examples, facilitate injection of holes by the anode.

[0149] In some non-limiting examples, the HTL 233 may be formed using a hole transport material, which may, in some non-limiting examples, exhibit high hole mobility.

[0150] In some non-limiting examples, the ETL 237 may be formed using an electron transport material, which may, in some non-limiting examples, exhibit high electron mobility.

[0151] In some non-limiting examples, the EIL 239 may be formed using an electron injection material, which may, in some non-limiting examples, facilitate injection of electrons by the cathode.

[0152] In some non-limiting examples, the at least one EML 235 may be formed, by way of non-limiting example, by doping a host material with at least one emitter material. In some non-limiting examples, the emitter material may be at least one of: a fluorescent emitter material, a phosphorescent emitter material, and a thermally activated delayed fluorescence (TADF) emitter material.

[0153] In some non-limiting examples, the emitter material may be one of a R(ed) emitter material, a G(reen) emitter material, and a B(lue) emitter material, that is, an emitter material that facilitates the emission of respectively, R(ed), G(reen), and B(lue) light.

[0154] In some non-limiting examples, the device 200 may be an OLED in which the at least one semiconducting layer 230 may comprise at least one EML 235 interposed between conductive thin film electrodes 220, 240, whereby, when a potential difference is applied across them, holes may be injected into the at least one semiconducting layer 230 through the anode and electrons may be injected into the at least one semiconducting layer 230 through the cathode, to migrate toward the at least one EML 235 and combine to emit light in the form of photons.

[0155] In some non-limiting examples, the device 200 may be an electro-luminescent QD device 200 in which the at least one semiconducting layer 230 may comprise an active layer comprising at least one QD. When current is provided by the power source to the first electrode 220 and second electrode 240, light, including without limitation, in the form of photons, may be emitted from the active layer comprising the at least one semiconducting layer 230 between them.

[0156] In some non-limiting examples, including where the device 200 comprises a lighting panel, an entire lateral aspect of the device 200 may correspond to a single emissive element. As such, the substantially planar cross-sectional profile shown in FIG. 2 may extend substantially along the entire lateral aspect of the device 200, such that light is emitted from the device 200 substantially along the entirety of the lateral extent thereof. In some non-limitingexamples, such single emissive element may be driven by a single driving circuit of the device 200.

[0157] In some non-limiting examples, including where the device 200 comprises a display module, the lateral aspect of the device 200 may be sub-divided into a plurality of emissive regions 210 of the device 200, in which the longitudinal aspect of the device structure 200, within each of the emissive region(s) 210, may cause light to be emitted therefrom when energized.

[0158] Those having ordinary skill in the relevant art will readily appreciate that the structure of the device 200 may be varied by the introduction of at least one additional layer (not shown) at appropriate position(s) within the at least one semiconducting layer 230 stack, including without limitation, at least one of: a hole blocking layer (HBL) (not shown), an electron blocking layer (EBL) (not shown), a charge transport layer (CTL) (not shown), and a charge injection layer (CIL) (not shown).

[0159] In some non-limiting examples, the patterning coating 110 may be formed concurrently with the at least one semiconducting layer(s) 230. In some non-limiting examples, at least one material used to form the patterning coating 110 may also be used to form the at least one semiconducting layer(s) 230. In some non-limiting examples, the ETL 237 of the at least one semiconducting layer 230 may be a patterning coating 110 that may be deposited in the first portion 101 and the second portion 102 during the deposition of the at least one semiconducting layer 230. The EIL 239 may then be selectively deposited in the emissive region 210 of the second portion 102 over the ETL 237, such that the exposed layer surface 11 of the ETL 237 in the first portion 101 may be substantially devoid of the EIL 239. The exposed layer surface 11 of the EIL 239 in the emissive region 210 and the exposed layer surface of the ETL 237, which acts as the patterning coating 110, may then be exposed to a vapor flux 532 (FIG. 5) of the deposited material 531 to form a closed coating 140 of the deposited layer 130 on the EIL 239 in the second portion 102, and a discontinuous layer 160 of the deposited material 531 on the ETL 237 in the first portion 101. In such non-limiting example, several stages for fabricating the device 200 may be reduced.Low-Index Laver

[0160] In some non-limiting examples, the at least one semiconducting layer 230 may comprise a low-index layer. In some non-limiting examples, the low-index layer may comprise amixture of a low-index material and a higher-index material. In some non-limiting examples, the low-index layer containing such mixture may be formed by co-depositing the low-index material with the higher-index material in a vacuum-based deposition process.

[0161] In some non-limiting examples, a refractive index of the low-index layer in at least a sub-range of the visible spectrum, including without limitation, at a wavelength of one of about: 460, 500, and 600, nm, may be one of no more than about: 1.7, 1.65, 1.6, 1.55, 1.5, 1.45, and 1.4.

[0162] In some non-limiting examples, the refractive index of the low-index layer may be no more than a refractive index of at least one layer arranged adjacent thereto. In some nonlimiting examples, the low-index layer may be in direct contact with, and in some non-limiting examples, may form an interface with, such at least one adjacent layer.

[0163] In some non-limiting examples, a characteristic refractive index of the low-index material, in at least a sub-range of the visible spectrum, may be no more than a characteristic refractive index of the higher-index material, including without limitation, at a wavelength of one of about: 460, 500, and 600, nm, by one of at least about: 0.1, 0.15, 0.2, 0.25, 0.3, 0.4, and 0.5.

[0164] In some non-limiting examples, a characteristic refractive index of the low-index material, in at least a sub-range of the visible spectrum, including without limitation, at a wavelength of one of about: 460, 500, and 600, nm, may be one of no more than about: 1.6, 1.55, 1.5, 1.45, 1.4, 1.35, and 1.3.

[0165] In some non-limiting examples, a characteristic refractive index of the higher- index material, in at least a sub-range of the visible spectrum, including without limitation, at a wavelength of one of about: 460, 500, and 600, nm, may be one of at least about: 1.8, 1.85, and 1.9.

[0166] In some non-limiting examples, the low-index layer may comprise, by at least one of: volume percentage, weight percentage, and mole percentage, the low-index material in a concentration of one of no more than about: 80, 75, 70, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 13, 10, 8, and 5%.

[0167] In some non-limiting examples, the low-index layer may comprise, by at least one of: volume percentage, weight percentage, and mole percentage, the low-index material in a concentration of one of at least about: 1, 3, 5, 8, 10, 15, 20, 25, 30, 35, 40, 45, and 50%.

[0168] In some nonlimiting examples, at least one of an: electron, and hole, mobility of the low-index layer is at least about 10'5.

[0169] Without wishing to be limited by any particular theory, it may be postulated that the low-index layer formed by providing certain low-index materials in a concentration of one of between about: 25-75, 30-70, and 35-60%, may exhibit at least one opto-electronic property of the higher-index material, while also exhibiting a substantially low refractive index. In some nonlimiting examples, a CTL formed by providing a charge transport material as the higher-index material, and a low-index material in a concentration of one of between about: 25-75, 30-70, and 35-60%, may result in the low-index layer having a substantially similar charge transport property, including without limitation, electron / hole mobility, and a substantially low refractive index in comparison to a layer formed that is substantially similar but composed substantially of the charge transport material.

[0170] In some non-limiting examples, a solubility, in N-methyl-2-pyrrolidone (NMP), of at least one of the: low-index material, and higher-index layer, may be at least about 1 mg / mL.

[0171] In some non-limiting examples, the higher-index material may be an organic semiconducting material. In some non-limiting examples, the higher-index material may comprise a polycyclic aromatic moiety. In some non-limiting examples, the organic semiconducting material may be a charge transport material, including without limitation, a hole transport material.

[0172] In some non-limiting examples, the low-index layer may be provided as (a part, including without limitation, at least one sub-layer, of) the HTL 233 for a top-emitting optoelectronic device 200, including without limitation, a top-emitting OLED. In some non-limiting examples, such device 200 may be configured such that the EML 235 may be arranged between the anode and the cathode, and the low-index layer may be arranged between the EML 235 and the anode. In some non-limiting examples, an HIL 231 may be arranged between the EML 235 and the anode, and the low-index layer may be arranged between the HIL 231 and the EML 235. In some non-limiting examples, an EBL may be arranged between the HIL 231 and the EML 235, and the low-index layer may be arranged between the HIL 231 and the EBL. In some nonlimiting examples, the low-index layer may form an interface with each of the HIL 231 and the EBL.

[0173] In some non-limiting examples, the low-index material may have a band gap of one of at least about: 3.4, 3.5, 4.1, 5, and 6.2, eV. Without wishing to be limited by any particular theory, it may be postulated that the low-index material having a substantially wide band gap may reduce a likelihood of the presence of such material of at least one of: affecting the charge transport, and quenching characteristics of the low-index layer when such layer is being used as a CTL.

[0174] In some non-limiting examples, the low-index material may be one of: a small molecule, and an oligomer.

[0175] In some non-limiting examples, the low-index material may be an organic- inorganic hybrid material.

[0176] In some non-limiting examples, a molecular structure of the low-index material may comprise at least one of a: cyclophosphazene, fluoroalkyl, and silsesquioxane, moiety.

[0177] In some non-limiting examples, the low-index layer may comprise, by weight percentage, the low-index material comprising a cyclophosphazene moiety, in a concentration of between about 1-20%.

[0178] In some non-limiting examples, the low-index material may comprise, by weight percentage, F, in a concentration of between about 10-50%.

[0179] In some non-limiting examples, a molecular structure of the low-index material may comprise a low surface tension moiety, and in some non-limiting examples, may comprise a high surface tension moiety, which may be one of: bonded directly, and bonded indirectly via another moiety, to the low surface tension moiety.

[0180] In some non-limiting examples, the low surface tension moiety may comprise at least one of a: fluorine (F), and Si, -containing moiety. In some non-limiting examples, the F- containing moiety may be a fluoroalkyl moiety, and the Si-containing moiety may be a siloxyl moiety.Attributes of Semiconducting Layer / MaterialComposition

[0181] In some non-limiting examples, the at least one semiconducting layer 230, including without limitation, the HTL 233, may comprise a low-index layer. In some non-limiting examples, the low-index layer may comprise a mixture of a low-index material and a higher-index material.

[0182] In some non-limiting examples, at least one of: the low-index layer, and the low- index material, may comprise at least one of an: F, and Si, atom.

[0183] In some non-limiting examples, the low-index material may comprise a compound that comprises F. In some non-limiting examples, the low-index material may comprise a compound that comprises F and a carbon (C) atom. In some non-limiting examples, the low- index material may comprise a compound that comprises F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 0.5, 0.7, 1.0, 1.5, 2.0, and 2.5.

[0184] In some non-limiting examples, an atomic ratio of F to C may be determined by counting the F atoms present in the compound structure, and for C atoms, only counting the sp3hybridized C atoms present in the compound structure. In some non-limiting examples, the low- index material may comprise a compound that comprises, as part of its molecular sub-structure, a moiety comprising F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 1.0, 1.5, and 2.0.

[0185] In some non-limiting examples, the low-index material may comprise an organic- inorganic hybrid material.

[0186] In some non-limiting examples, the low-index material may comprise an oligomer. In some non-limiting examples, the low-index material may be an oligomer.

[0187] In some non-limiting examples, a molecular weight of the low-index material may be at least about 800 g / mol. In some non-limiting examples, a molecular weight of the compound may be one of at least about: 1,500, 1,700, 2,000, 2,200, and 2,500, g / mol.

[0188] In some non-limiting examples, a molecular weight of the low-index material may be no more than about 6,000 g / mol. In some non-limiting examples, the molar weight of the compound may be one of no more than about: 6,000, 5,500, 5,000, 4,500, 4,300, and 4,000, g / mol.

[0189] In some non-limiting examples, the low-index material may comprise a compound having a molecular structure comprising a backbone and at least one functional group bonded to the backbone. In some non-limiting examples, the backbone may be an inorganic moiety, and the at least one functional group may be an organic moiety.

[0190] In some non-limiting examples, at least a part of the molecular structure of the low-index material may be represented by Chemical Formula (I):(Mori)n (I) where:Mon represents a monomer, and n is an integer of at least 2.

[0191] In some non-limiting examples, n may be an integer of one of between about: 2- 100, 2-50, 3-20, 3-15, 3-10, and 3-7.

[0192] In some non-limiting examples, the monomer may comprise at least one of: F, and Si.

[0193] In some non-limiting examples, the monomer may comprise a functional group. In some non-limiting examples, at least one functional group may be a low surface tension moiety. In some non-limiting examples, the low surface tension moiety may comprise at least one of: F, and Si. In some non-limiting examples, the low surface tension moiety may include at least one of: a fluorocarbon group, and a siloxane group.

[0194] The surface tension attributable to a fragment of a molecular structure, including without limitation, at least one of: a monomer, a monomer backbone unit, a linker, a functional group, and a low surface tension moiety, may be determined using various known methods in the art, including without limitation, the use of a Parachor, such as may be further described, by way of non-limiting example, in “Conception and Significance of the Parachor", Nature 196: 890- 891. In some non-limiting examples, at least one functional group of the monomer may have a surface tension of one of no more than about: 25, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, and 10, dynes / cm.

[0195] In some non-limiting examples, the monomer may comprise at least one of a: CF2, and CF2H, moiety. In some non-limiting examples, the monomer may comprise at least one of a: CF2, and CF3, moiety. In some non-limiting examples, the monomer may comprise a CH2CF3 moiety. In some non-limiting examples, the monomer may comprise at least one of: C, and oxygen (O). In some non-limiting examples, the monomer may comprise a fluorocarbon moiety. In some non-limiting examples, the monomer may comprise at least one of a: vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene,and fluorinated 1,3-dioxole, moiety. In some non-limiting examples, the monomer may comprise a silsesquioxane group.

[0196] In some non-limiting examples, the molecular structure of the low-index material may comprise a plurality of different monomers. In some non-limiting examples, such molecular structure may comprise monomers that have different at least one of: molecular composition, and molecular structure. In some non-limiting examples, such molecular structures may comprise those represented by Chemical Formulae (II) and (III):(MonA)k(MonB)m(II)(MonA)k(MonB)m(Monc)o(III) where:Mon MonB, and Monceach represents a monomer, and k, m, and o each represent an integer of at least 2.

[0197] In some non-limiting examples, k, m, and o each represent an integer of one of between about: 2-100, 2-50, 3-20, 3-15, 3-10, and 3-7. Those having ordinary skill in the relevant art will appreciate that various non-limiting examples and descriptions regarding monomer, Mon, may be applicable with respect to each of Mon'', Mon8, and Monc.

[0198] In some non-limiting examples, the monomer may comprise a monomer backbone unit. In some non-limiting examples, the functional group may be bonded directly to the monomer backbone unit. In some non-limiting examples, the monomer may comprise a plurality of functional groups, which may be one of: the same, and different, from one another.

[0199] In some non-limiting examples, the monomer may be represented by Chemical Formula (IV):(M-(R)y)n (IV) where:AT represents the monomer backbone unit,R represents the functional group, y is an integer between about 1-3, and n is an integer of at least 2.

[0200] In some non-limiting examples, the monomer backbone unit M may have a high surface tension. In some non-limiting examples, the monomer backbone unit may have a surface tension that is at least that of at least one of the functional group(s) R bonded thereto. In some non-limiting examples, the monomer backbone unit may have a surface tension that is at least that of any functional group R bonded thereto.

[0201] In some non-limiting examples, the monomer backbone unit may have a surface tension of one of at least about: 25, 30, 40, 50, 75, 100; 150, 200, 250, 500, 1,000, 1,500, and 2,000, dynes / cm.

[0202] In some non-limiting examples, the low-index material may have a molecular structure that comprises a phosphazene moiety. In some non-limiting examples, the phosphazene moiety may be at least one of a: linear, branched, and cyclic, phosphazene group. In some nonlimiting examples, the backbone may comprise a phosphazene group. In some non-limiting examples, the low-index material may comprise a phosphazene moiety and at least one F- containing functional group attached thereto.

[0203] In some non-limiting examples, the monomer backbone unit may comprise phosphorus (P) and nitrogen (N). In some non-limiting examples, the monomer backbone unit may be a phosphazene monomer backbone unit.

[0204] In some non-limiting examples, at least a part of the molecular structure of the low-index layer may be represented by Chemical Formula (V):(NP-(R)y)n(V) where:NP represents the phosphazene monomer backbone unit,R represents the functional group, y is an integer between about 1-3, and n is an integer of at least 2.

[0205] In some non-limiting examples, the functional group may be an F-containing group. In some non-limiting examples, the functional group may independently comprise at least one of: F, chlorine (Cl), a hydroxyl group, a substituted alkyl group, an unsubstituted alkyl group, a substituted fluoroalkyl group, an unsubstituted fluoroalkyl group, a substituted cycloalkylgroup, an unsubstituted cycloalkyl group, a substituted fluorocycloalkyl group, an unsubstituted fluorocycloalkyl group, a substituted heterocycloalkyl group, an unsubstituted heterocycloalkyl group, a substituted fluoroheterocycloalkyl group, an unsubstituted fluoroheterocycloalkyl group, a substituted alkoxy group, an unsubstituted alkoxy group, a substituted fluoroalkoxy group, an unsubstituted fluoroalkoxy group, a substituted aryloxy group, an unsubstituted aryloxy group, a substituted fluoroaryloxy group, an unsubstituted fluoroaryloxy group, a substituted heteroaryloxy group, a unsubstituted heteroaryloxy group, a substituted fluoroheteroaryl oxy group, a unsubstituted fluoroheteroaryl oxy group, a substituted aryl group, an unsubstituted aryl group, a substituted fluoroaryl group, an unsubstituted fluoroaryl group, a substituted alkyl silyl group, an unsubstituted alkylsilyl group, a substituted alkylsiloxy group, an unsubstituted alkylsiloxy group, an amino group, an amine group, an alkylamine group, an arylamine group, a cyano group, a phosphazo group, a sulfanyl group, a pentafluorosulfanyl group, a sulfide group, a sulfonyl group, a thiol group, an alkylthio group, a trifluoromethylthio group, a carbonyl group, a siloxane group, a silane group, and an organosilicon group.

[0206] In some non-limiting examples, the low-index material may have a molecular structure comprising a siloxane group. In some non-limiting examples, the siloxane group may be one of a: linear , branched, and cyclic, siloxane group. In some non-limiting examples, the monomer backbone unit may comprise a siloxane group. In some non-limiting examples, the low-index material may comprise a siloxane group and at least one F-containing group. In some non-limiting examples, the F-containing group may be a fluoroalkyl group.

[0207] In some non-limiting examples, the low-index material may have a molecular structure comprising a silsesquioxane group. In some non-limiting examples, the silsesquioxane group may be a polyhedral oligomeric silsesquioxane (POSS). In some non-limiting examples, the monomer backbone unit may comprise a silsesquioxane group. In some non-limiting examples, the low-index material may comprise a silsesquioxane group and at least one F- containing group. In some non-limiting examples, the at least one F-containing group may be a fluoroalkyl group. In some non-limiting examples, the low-index material may comprise fluoro- silsesquioxane and fluoro-POSS.

[0208] In some non-limiting examples, at least a part of the molecular structure of the low-index material may be represented by Chemical Formula (VI):(SiOs / 2-(R)). (VI)where:R represents the functional group, and n is an integer between about 6-12.

[0209] In some non-limiting examples, n may be one of: 8, 10, and 12.

[0210] In some non-limiting examples, R may comprise a functional group with a low surface tension. In some non-limiting examples, R may comprise at least one of an: F-, and Si-, containing group. In some non-limiting examples, R may comprise at least one of a: fluorocarbon, and siloxane-containing, group. In some non-limiting examples, R may comprise at least one of a: CF2, and CF2H, group. In some non-limiting examples, R may comprise at least one of a: CF2, and CF3, group. In some non-limiting examples, R may comprise a CH2CF3 group.

[0211] In some non-limiting examples, the material represented by Chemical Formula (VI) may be a polyoctahedral silsesquioxane.Functional group, R

[0212] In some non-limiting examples, the functional group of the low-index material may independently comprise at least one of: F, Cl, a hydroxyl group, a substituted alkyl group, an unsubstituted alkyl group, a substituted fluoroalkyl group, an unsubstituted fluoroalkyl group, a substituted cycloalkyl group, an unsubstituted cycloalkyl group, a substituted fluorocycloalkyl group, an unsubstituted fluorocycloalkyl group, a substituted heterocycloalkyl group, an unsubstituted heterocycloalkyl group, a substituted fluoroheterocycloalkyl group, an unsubstituted fluoroheterocycloalkyl group, a substituted alkoxy group, an unsubstituted alkoxy group, a substituted fluoroalkoxy group, an unsubstituted fluoroalkoxy group, a substituted aryloxy group, an unsubstituted aryloxy group, a substituted fluoroaryloxy group, an unsubstituted fluoroaryloxy group, a substituted heteroaryloxy group, a unsubstituted heteroaryloxy group, a substituted fluoroheteroaryloxy group, a unsubstituted fluor oheteroaryl oxy group, a substituted aryl group, an unsubstituted aryl group, a substituted fluoroaryl group, an unsubstituted fluoroaryl group, a substituted alkyl silyl group, an unsubstituted alkylsilyl group, a substituted alkylsiloxy group, an unsubstituted alkylsiloxy group, an amino group, an amine group, an alkylamine group, an arylamine group, a cyano group, a phosphazo group, a sulfanyl group, a pentafluorosulfanyl group, a sulfide group, asulfonyl group, a thiol group, an alkylthio group, a trifluoromethylthio group, a carbonyl group, a siloxane group, a silane group, and an organosilicon group.

[0213] In some non-limiting examples, at least one functional group of the low-index material may be an F-containing moiety. In some non-limiting examples, at least one functional group may comprise: a backbone and at least one F atom attached thereto. In some non-limiting examples, the backbone may be a C-containing backbone. In some non-limiting examples, the backbone may comprise a heteroatom, including without limitation, Si.

[0214] In some non-limiting examples, the functional group may comprise: a linker moiety RB, a terminal moiety RT, and an intermediate moiety RDarranged between the linker moiety RBand the terminal moiety RT.

[0215] In some non-limiting examples, the functional group may be represented by Chemical Formula (E-l):wherein: indicates a point of attachment within the compound,RBrepresents the linker moiety,RDrepresents the intermediate moiety, andRTrepresents the terminal moiety.

[0216] In some non-limiting examples, the functional group may comprise a branching moiety RE. In some non-limiting examples, such functional group may comprise one of Chemical Formulae (E-2)-(E-4):wherein:indicates a point of attachment within the compound.

[0217] In some non-limiting examples, the functional group may comprise at least one saturated bond. In some non-limiting examples, the bonds of the functional group may be substantially saturated bonds, such that the functional group may be a saturated group. In some non-limiting examples, at least one moiety of the functional group, including without limitation, at least one of: RB, RD, RT, and RE, may be a saturated moiety. In some non-limiting examples, the functional group may comprise unsaturated bonds. In some non-limiting examples, the bonds of the functional group may be substantially unsaturated bonds, such that the functional group may be an unsaturated moiety. In some non-limiting examples, at least one moiety of the functional group, including without limitation, at least one of: RB, RD, RT, and RE, may be an unsaturated moiety.

[0218] In some non-limiting examples, the functional group may comprise one of no more than about: 4, 3, 2, and 1, ether unit(s). Without wishing to be bound by any particular theory, it may be postulated that the presence of multiple ether units within a single functional group may decrease a melting point of the compound, which may have reduced applicability in some scenarios.

[0219] In some non-limiting examples, the linker moiety RBmay correspond to a terminal part of the functional group that may be proximate to the monomer backbone unit, and may comprise the atom(s) that attach the functional group to the monomer backbone unit. In some non-limiting examples, RBmay comprise one of: O, N, sulfur (S), a substituted alkylene, an unsubstituted alkylene, a substituted fluoroal kylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted arylene, an unsubstituted arylene, a substituted heteroarylene, and an unsubstituted heteroarylene. In some non-limiting examples, RBmay comprise a phosphazene group. In some non-limiting examples, RBmay comprise at least one of: a fluoromethylene, and a difluoromethylene. In some non-limiting examples, RBmay be selected from: -O-, and -O-CH2-.

[0220] In some non-limiting examples, the intermediate moiety RDmay generally correspond to a part of the functional group arranged between the linker group, L, and the terminal moiety. In some non-limiting examples, RDmay comprise: O, an ether, a substituted alkylene, an unsubstituted alkylene, a substituted fluoroalkylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted arylene, anunsubstituted arylene, a substituted phenyl, an unsubstituted phenyl, a substituted biphenyl, an unsubstituted biphenyl, a substituted binaphthalene, an unsubstituted binaphthalene, a substituted heteroarylene, and an unsubstituted heteroarylene. In some non-limiting examples, RDmay comprise F. In some non-limiting examples, RDmay comprise a fluoroalkylene unit. In some non-limiting examples, RDmay comprise at least one of a: CF2, CFH, and CH2, unit. In some non-limiting examples, RDmay comprise a plurality of CF2 units bonded together to form a (part of a) fluoroalkylene. In some non-limiting examples, RDmay comprise at least one CH2 unit and at least one CF2 unit. In some non-limiting examples, RDmay comprise an ether unit. In some non-limiting examples, RDmay comprise saturated bonds. In some non-limiting examples, RDmay be substantially devoid of any unsaturated bonds. In some non-limiting examples, RDmay comprise unsaturated bonds. In some non-limiting examples, RDmay comprise one of no more than about: 25, 15, 13, 12, and 10, C atoms.

[0221] In some non-limiting examples, the terminal moiety RT, may correspond to a terminal part of the functional group, including without limitation, a distal part of the functional group with respect to the monomer backbone unit. In some non-limiting examples, the terminal part may correspond to a terminal part of the functional group that is opposite to the linker group, L. In some non-limiting examples where the intermediate moiety RDcomprises a cyclic intermediate moiety, RTmay comprise a moiety attached to a ring atom of the intermediate moiety. In some non-limiting examples, R may comprise F. In some non-limiting examples, R may comprise hydrogen (H). In some non-limiting examples, ^ may comprise Si. In some nonlimiting examples, ^ may comprise at least one of: a substituted alkyl, an unsubstituted alkyl, a branched fluoroalkyl, an unbranched fluoroalkyl, a substituted heterocycloalkyl, an unsubstituted heterocycloalkyl, a substituted alkoxy, an unsubstituted alkoxy, a branched silyloxy, an unbranched silyloxy, a branched fluoroalkoxy, an unbranched fluoroalkoxy, a fluoroaryl, a polyfluorosulfanyl, and a fluorocycloalkyl. In some non-limiting examples, RTmay be at least one of: F, H, CF2H, CF3, OCF3, CF2CF3, CF2CF2H, CH2CF2H, and CH2CF3. In some nonlimiting examples, A^ rnay comprise one of no more than about: 8, 6, 5, 3, 2, and 1, C atom(s).

[0222] The branching moiety R , may generally correspond to a part of the functional group from which a plurality of branches of the backbone may extend. In some non-limiting examples, REmay act as a branching point of the backbone. In some non-limiting examples, branching may occur by bonding at least three of the other moieties, forming the functional group, to RE. In some non-limiting examples, REmay be arranged in various configurations / positions of the functional group, and may be bonded to at least one of: RB, RD, and RT. In some non-limiting examples, the at least three moi eties bonded to REmay be one of: RB, RD, and RT,' RB, RB, and RB,' RD, RD,and RT, RT, and RT. In some non-limiting examples, REmay be bonded to at least one of: a plurality of RD, and a plurality of RT, where the functional group comprises a plurality of: at least one of: RD, and RT. In some non-limiting examples, REmay comprise at least one of: O, N, S, an amine, a substituted alkylene, an unsubstituted alkylene, a substituted fluoroalkylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted heterocycloalkylene, an unsubstituted heterocycloalkylene, a substituted arylene, an unsubstituted arylene, a substituted heteroarylene, and an unsubstituted heteroarylene. In some non-limiting examples, REmay comprise one of no more than about: 8, 6, 5, 3, 2, and 1, C atom(s). In some non-limiting examples, REmay be substantially devoid of C atoms.

[0223] In some non-limiting examples, RBin Chemical Formula (E-l) may be represented by one of Chemical Formulae (EA-l)-(EA-6):wherein, in Chemical Formula (EA-2), RHis one of: H, deutero (D), CF3, and a secondary functional group comprising both RDand RT.

[0224] In some non-limiting examples, the terminal moiety RTmay be bonded to the intermediate moiety RDof the secondary functional group.

[0225] In some non-limiting examples, the secondary functional group may be represented by Chemical Formula (ED-1):(ED-1)

[0226] In some non-limiting examples, RDand RTof the secondary functional group of Chemical Formula (ED-1) may be identical in molecular structure to RDand RTof the functional group of Chemical Formula (E-l). In some non-limiting examples, at least one of: RD, and RT, of the secondary functional group of Chemical Formula (ED-1) may be different from those of thefunctional group of Chemical Formula (E-l). In some non-limiting examples, descriptions regarding various non-limiting examples of RDand RTprovided herein in relation to the functional group of Chemical Formula (E-l) may apply to RDand RTof the secondary functional group of Chemical Formula (ED-1).

[0227] In some non-limiting examples, RDin Chemical Formula (E-l) may be represented by Chemical Formula (EB-1):(EB-1) wherein:X is each independently one of: H, D, F, and CF3; a is an integer between about 0-6; and b is an integer between about 0-12; and a sum of a and b is at least 1.

[0228] In some non-limiting examples, a sum of a and b may be one of no more than about 15, 12, 10, and 9.

[0229] In some non-limiting examples, RD, according to Chemical Formula (EB-1), may comprise at least one of Chemical Formulae (EB-10)-(EB-21):

[0230] In some non-limiting examples, a may be an integer between about 1-4, b may be an integer between about 4-9, and a sum of a and b may be an integer between about 6-13.

[0231] In some non-limiting examples, a may be an integer between about 2-4, b may be an integer between about 5-9, and a sum of a and b may be an integer between about 7-13.

[0232] In some non-limiting examples, RT, in Chemical Formula (E-l), may be represented by one of Chemical Formulae (EC-l)-(EC-l 1):

[0233] In some non-limiting examples, the functional group may comprise a C- containing backbone in a closed ring configuration, in some non-limiting examples, to form a cyclic structure, which may comprise at least one of: fluorocycloalkyl (including without limitation, perfluorocyclopentyl and perfluorocyclohexyl), aryl (including without limitation, phenyl and naphthyl), and biaryl (including without limitation, biphenyl, and binaphthyl).

[0234] In some non-limiting examples, the functional group may comprise a C- containing backbone in a closed cage configuration, including without limitation, adamantyl.

[0235] In some non-limiting examples, the functional group may comprise an F- containing moiety, including without limitation, a fluoroalkyl moiety, and a fluoroaryl moiety.

[0236] Those having ordinary skill in the relevant art will appreciate that, in some nonlimiting examples, various descriptions of RB, RD, RE, and RT, may have application in some nonlimiting examples of the functional group, including without limitation, those of Chemical Formulae (E-2)-(E-4). In some non-limiting examples, where the functional group comprises a plurality of a given moiety, including without limitation, at least one of: a plurality of RB, a plurality of RD, a plurality of RE, and a plurality of RT, each such moiety may be selected independently of one another.

[0237] In some non-limiting examples, the low-index material may comprise a functional group R selected from one of Chemical Formulae (F-l)-(F-314):wherein in each of Chemical Formulae (F-1)-(F-314): represents a point of attachment to the monomer backbone unit.

[0238] In some non-limiting examples, the functional group R may independently comprise an oligomer unit, and the oligomer unit may further comprise a plurality of functional group monomer units. In some non-limiting examples, a functional group monomer unit may be at least one of: CH2, and CF2. In some non-limiting examples, a functional group may comprise a CH2CF3 moiety. In some non-limiting examples, such functional group monomer units may be bonded together to form at least one of an: alkyl, and fluoroalkyl, oligomer unit. In some nonlimiting examples, the oligomer unit may further comprise a functional group terminal unit. In some non-limiting examples, the functional group terminal unit may be arranged at a terminal end of the oligomer unit and bonded to a functional group monomer unit. In some non-limiting examples, the terminal end at which the functional group terminal unit may be arranged may correspond to a fragment of the functional group that may be distal to the monomer backbone unit. In some non-limiting examples, the functional group terminal unit may comprise at least one of: CF2H, and CF3.

[0239] In some non-limiting examples, the low-index material may comprise a cyclophosphazene derivative represented by any one of Chemical Formulae (C-l)-(C-6):where:R independently represents, upon each occurrence, a substituted alkyl, an unsubstituted alkyl, a substituted fluoroalkyl, an unsubstituted fluoroalkyl, a substituted alkoxy, an unsubstituted alkoxy, a substituted fluoroalkoxy, an unsubstituted fluoroalkoxy, a substituted siloxy, an unsubstituted siloxy, a substituted fluoroalkylsiloxy, an unsubstituted fluoroalkylsiloxy, a substituted cycloalkyl, an unsubstituted cycloalkyl, a substituted fluorocycloalkyl, an unsubstituted fluorocycloalkyl, a substituted aryl, an unsubstituted aryl, a substituted fluoroaryl, an unsubstituted fluoroaryl, a substituted heteroaryl, and an unsubstituted heteroaryl.

[0240] In some non-limiting examples, at least one R in any one of Chemical Formulae (C-l)-(C-6), may be a fluoroalkyl group. In some non-limiting examples, the fluoroalkyl group may comprise at least one of a: CF2, CF2H, CH2CF3, and CF3, group. In some non-limiting examples, the fluoroalkyl group may be represented by Chemical Formula (VII):where: p is an integer between about 1-5; q is an integer between about 6-20; andZ represents one of: H, and F.

[0241] In some non-limiting examples, p may be 1 and q may be an integer between about 6-20.

[0242] In some non-limiting examples, the low-index material may comprise a silsesquioxane moiety. In some non-limiting examples, the low-index material may comprise a silsesquioxane moiety represented by one of: (RSiOi.s (RSiOi.5)io, and (RSiOi.5)i2. In some non-limiting examples, the molecular structure of such compound may be represented by one of Chemical Formulae (PO-l)-(PO-3):

[0243] In some non-limiting examples, the R groups in Chemical Formulae (PO-l)-(PO- 3) may be independently selected upon occurrence of each (RSiOi.s) unit. In some non-limiting examples, R may comprise a functional group with a low surface tension. In some non-limiting examples, R may comprise at least one of a: CF2, and CF2H, moiety. In some non-limiting examples, R may comprise at least one of a: a CF2, and CF3, moiety. In some non-limiting examples, R may comprise a CH2CF3 moiety. In some non-limiting examples, a compound offormula (RSiOi.s)v comprising two different R groups may also be represented by formula (R^iOi.s l SiOi.s in which w and x sum to v. In some non-limiting examples, such compound, and other compounds containing a plurality of different R groups may be encompassed by the general formula (RSiOi.s)v.

[0244] In some non-limiting examples, at least one R in any one of Chemical Formulae (PO-l)-(PO-3) may be a fluoroalkyl group. In some non-limiting examples, the fluoroalkyl group may be represented by Chemical Formula (VII).

[0245] In some non-limiting examples, at least a part of the molecular structure of the low-index material may be represented by Chemical Formula (VIII):(SiO3 / 2-(CH2)x(CF3))n(VIII) where: x is an integer between about 1-5, and n is an integer between about 6-12.

[0246] In some non-limiting examples, n may be one of: 8, 10, and 12.

[0247] In some non-limiting examples, the compound represented by Chemical Formula (VIII) may be a polyoctahedral silsesquioxane.

[0248] In some non-limiting examples, the functional group R may be selected independently upon each occurrence of such group in any of the foregoing chemical formulae. Those having ordinary skill in the relevant art will appreciate that any of the foregoing formulae may represent a sub-structure of the compound, and at least one of additional: groups, and moieties, may be present, which are not explicitly shown in the above formulae. Those having ordinary skill in the relevant art will appreciate that various formulae provided in the present application may represent at least one of: linear, branched, cyclic, cyclo-linear, and cross-linked, structures.

[0249] In some non-limiting examples, the higher-index material may comprise an organic semiconducting material. In some non-limiting examples, the organic semiconducting material may comprise a polycyclic aromatic moiety.

[0250] In some non-limiting examples, the organic semiconducting material may comprise at least one of Chemical Formulae (AR-l)-(AR-29):

[0251] In each of Chemical Formulae (AR-l)-(AR-29):X independently represents one of: C, and a heteroatom, which, in some non-limiting examples, may act as a bonding site for the core moiety to be bonded to an R group, including without limitation, a ligand moiety; andQ independently represents one of: C, and a heteroatom, which, in some non-limiting examples, may act as a bonding site for the core moiety to be bonded to an R group, including without limitation, a ligand moiety.

[0252] In some non-limiting examples, X may be a heteroatom selected from one of: O, and N, including without limitation, one of a: substituted, and unsubstituted, heteroatom.

[0253] In some non-limiting examples, Q may be a heteroatom selected from one of: N, S, O, and Si, including without limitation, one of: substituted, and unsubstituted, heteroatom.Examples

[0254] A series of experiments were conducted in order to evaluate the effects of providing a low-index layer in a device.

[0255] The molecular structures of the low-index materials used in the experiments are set out in Table 1 below.Table 1Experiment 1

[0256] In some non-limiting examples, a series of samples was fabricated to measure their refractive indices at wavelengths of: 460, 550, and 600, nm. The results of the measurement are summarized in Table 2 below.Table 2

[0257] Based on the foregoing measurement in Table 2, it was found that EM-10 and EM-8 both exhibit characteristic refractive indices of no more than 1.40, while HTM, an example hole transport material, exhibits a substantially high refractive index of at least 1.70, across the visible spectrum. Low-index layers formed by co-depositing HTM with one of: EM-10, and EM- 8, in equal parts (1 :1 (vol:vol)), have refractive indices of no more than 1.60 across the visible spectrum.Experiment 2

[0258] In some non-limiting examples, a series of example OLED devices 200 were fabricated in which the layer composition of the HTL was varied to determine the effects of providing the low-index layer as part of the HTL 233. The general OLED device structure was as follows: Anode / HIL 231 / HTL 233 / EBL / EML 235 / HBL / ETL 237 / EIL 239 / Cathode / Capping layer (CPL). Each device 200 was fabricated as top-emitting device 200 with a reflective anode and a light-transmissive cathode. The total thickness of the HTL 233 was kept substantially the same in all devices 200. In each device 200, the current density at several different voltages were measured and the results summarized in Table 3 below.Table 3

[0259] As may be seen in Table 3, the OLED device 200 fabricated by incorporating the low-index layer in the form of HTM:EM-10 (1 : 1 (vol: vol)) as part of the HTL 233 exhibited substantially increased current densities across all three measured voltages compared to the example device in which the HTL 233 was formed only of HTM. Based on the foregoing observation, it may be concluded that the use of a low-index layer in the example device 200 may have enhanced charge mobility and avoid formation of any new trapped states. In some nonlimiting examples, while it may be widely regarded that introducing new materials into the OLED 200 stack may create trap states which would lower the current density, providing a material as described herein, including but not limited to, EM- 10, in the present example device 200 did not lead to formation of any new trap states and it enhanced the current density in the device 200.Experiment 3

[0260] A series of example devices were fabricated to examine the effects of incorporating a low-index layer as (part of) the HTL on both the longitudinal, and lateral, I-V (current-voltage) characteristics of the devices.

[0261] A cross-sectional view of an example device 600aused to examine the effects on the longitudinal I-V characteristic is shown in FIG. 6A. The example device 600acomprises a substrate 10, and a plurality of layers, deposited upon the substrate 10, comprising: a first electrode 220, a second electrode 240, an HTL 233 therebetween, a first HIL 2311 between thefirst electrode 220 and the HTL 233, and a second HIL 2312 between the HTL 233 and the second electrode 240. The first electrode 220 and the second electrode 240 are electrically coupled with a power source 204. The first and second HILs 2311, 23 h each has a layer thickness of substantially 2 nm. The HTL 233 has a layer thickness of substantially about 100 nm. The first electrode 220 comprises ITO. The second electrode 240 comprises Ag, and has a layer thickness of substantially about 40 nm. The HTL 233 comprises a layer of a mixture of HTM:EM-11 (1 : 1 (vokvol)). For comparison, a reference device was fabricated in a similar fashion except that the HTL 233 comprises a layer of substantially only HTM.

[0262] An example device 600b used to examine the effects on the lateral I-V characteristic is shown in FIG. 6B. The example device 600b has a length of substantially about 2.5 mm, and comprises a substrate 10, and two electrodes 220, disposed thereon, and separated by a gap with a width of substantially about 10 pm, such that a part of the exposed layer surface 11 of the substrate 10 is not covered by the electrodes 220. The electrodes 220 and the exposed layer surface 11 of the substrate 10 have, deposited thereon, an HTL 233 having a thickness of substantially about 100 nm. The example device 600b has a length of 2.5 mm. The electrodes 220 are electrically coupled with a power source 204. Each electrode 220 comprises ITO and has a layer thickness of substantially about 120 nm. The HTL 233 comprises a layer of a mixture of HTM:EM-11 (1 : 1 (vokvol)). For comparison, a reference device was fabricated in a similar fashion except that the HTL 233 comprises a layer of substantially only HTM.

[0263] A range of voltages was applied to the example devices 600a, 600b and their respective reference devices, and the current values corresponding to each voltage increment were recorded. The recorded current values of the reference devices (630) and the example devices 600a, 600b (640) were plotted against the corresponding voltage values in longitudinal I- V curves 610 (FIG. 6C) and lateral I-V curves 620 (FIG. 6D).

[0264] As may be seen in FIG. 6C, compared to the reference device with the HTL 233 formed of substantially only HTM, the example devices 600afabricated by incorporating the HTL 233 in the form of HTM:EM-11 (1 : 1 (vokvol)) exhibited a substantially increased longitudinal current, indicating an enhanced charge mobility. As may be seen in FIG. 6D, compared to the reference device with the HTL 233 formed of substantially only HTM, the example devices 600b fabricated by incorporating the HTL 233 in the form of HTM:EM-11 (1 : 1(vol:vol)) exhibited a substantially decreased lateral current, indicating a reduced likelihood of leak current across at least the lateral aspect of the device.SynthesisSynthesis of EM- 11

[0265] In a 2.0 L round bottom flask equipped with a stirring bar, 12.8 g of NaOH was placed in 20 mL of deionized (DI) water and suspended in 500 mL of toluene. 145.1 g of lH,lH,9H-hexadecafluoro-l -nonanol was added, and the suspension was heated at 95°C for a total of 4 hours under a continuous nitrogen gas (N2) flow. A solid crashed out during this period.

[0266] The temperature was adjusted to 85°C and a water condenser was attached to the flask under a N2 atmosphere. 13.92 g of hexachlorocyclotriphosphazene, dissolved under N2 in 100 mL of dry tetrahydrofuran (THF), was added to the reaction mixture via cannula. The reaction mixture was stirred at 85°C for 2 hours, then at room temperature for 48 hours.

[0267] The reaction was quenched by adding 200 mL of water, and filtered via vacuum filtration in a filter funnel (pore diameter: -10-20 pm). The collected solid was washed with water (3xlL), isopropyl alcohol (IL), and dichloromethane (DCM, IL). 95.2 g of white solid was collected, which was identified to be sample EM-11. Sample EM-11 was further purified by vacuum sublimation.Surface Energy

[0268] In some non-limiting examples, a characteristic surface energy may be measured from a surface formed by the material deposited (coated) in a thin film form.

[0269] Various methods and theories for determining the surface energy of a solid are known.

[0270] In some non-limiting examples, a surface energy may be calculated (derived) based on a series of contact angle measurements, in which various liquids may be brought into contact with a surface of a solid to measure the contact angle between the liquid-vapor interface and the surface. In some non-limiting examples, a surface energy of a solid surface may be equal to the surface tension of a liquid with the highest surface tension that completely wets the surface.

[0271] In some non-limiting examples, the critical surface tension of a surface may be determined according to the Zisman method, as further detailed in W. A. Zisman, Advances in Chemistry 3 (1964), pp. 1-51.

[0272] In some non-limiting examples, a characteristic surface energy of a material, including without limitation, the low-index material, may be determined by depositing the material as a substantially pure coating (e.g. a coating formed by a substantially pure material) on a substrate 10 and measuring a contact angle thereof with an applicable series of probe liquids.

[0273] In some non-limiting examples, a Zisman plot may be used to determine a maximum value of surface tension that would result in complete wetting (i.e. a contact angle 0c of 0°) of the surface.

[0274] A material which has applicability for use in providing the low-index layer may generally have a low surface energy when deposited as a thin film (coating) on a surface. In some non-limiting examples, a material with a low surface energy may exhibit low intermolecular forces.

[0275] Without wishing to be bound by any particular theory, it is now postulated that a material with a substantially high surface energy may have applicability at least in some applications that call for a high temperature reliability.

[0276] Without wishing to be bound by any particular theory, it is now postulated that a material with a surface energy of between about 13-24 dynes / cm may have applicability at least in some applications that call for a high temperature reliability.

[0277] Without wishing to be bound by any particular theory, it may be postulated that materials that form a surface having a surface energy no more than, in some non-limiting examples, about 12 dynes / cm, may have reduced applicability as a low-index material in some scenarios, as such materials may exhibit at least one of: substantially poor adhesion to layer(s) surrounding such materials, a low melting point, and a low sublimation temperature.

[0278] In some non-limiting examples, the surface values in various non-limiting examples herein may correspond to such values measured at around normal temperature and pressure (NTP), which may correspond to a temperature of 20°C, and an absolute pressure of 1 atm.

[0279] In some non-limiting examples, a series of samples was fabricated to measure the critical surface tension of the surfaces formed by the various materials. The results of the measurement are summarized in Table 4:Table 4TemperatureGlass Transition Temperature

[0280] In some non-limiting examples, at least one of: the low-index layer, and the low- index material, in some non-limiting examples, when deposited as at least one of: a film, and coating, in a form, and under circumstances similar to the deposition of the low-index layer within the device 100, may have a glass transition temperature that is one of: one of at least about: 300, 200, 170, 150, 130, 120, 110, and 100°C, and one of no more than about: 20, 0, -20, - 30, and -50°C.Sublimation Temperature

[0281] In some non-limiting examples, a material, including without limitation, a low- index material, having substantially low inter-molecular forces may tend to exhibit a substantially low sublimation temperature.

[0282] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially low sublimation temperature, may have reduced applicability for manufacturing processes that may call for substantially precise control of an average layer thickness of a closed coating 140 of a deposited film of the material.

[0283] In some non-limiting examples, a material, including without limitation, a low- index material, having a sublimation temperature that is one of no more than about: 140, 120, 110, 100 and 90°C, may tend to encounter constraints on at least one of: a deposition rate and anaverage layer thickness, of a film comprising such material that may be deposited using known deposition methods, including without limitation, vacuum thermal evaporation.

[0284] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially high sublimation temperature may have applicability in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0285] In some non-limiting examples, the low-index material may have a sublimation temperature of one of between about: 100-320, 120-300, 140-280, and 150-250°C. In some nonlimiting examples, such sublimation temperature may allow the low-index material to be substantially readily deposited as a coating using PVD.

[0286] In some non-limiting examples, a material with substantially low intermolecular forces may exhibit a substantially low sublimation temperature.

[0287] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially low sublimation temperature, may have reduced applicability for manufacturing processes that may call for substantially precise control of an average layer thickness of a closed coating 140 of the material.

[0288] In some non-limiting examples, a material, including without limitation, a low- index material, having a sublimation temperature that is one of no more than about: 140, 120, 110, 100 and 90°C, may tend to encounter constraints on at least one of: the deposition rate and the average layer thickness, of a film comprising such material that may be deposited using known deposition methods, including without limitation, vacuum thermal evaporation.

[0289] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially high sublimation temperature may have applicability in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0290] The sublimation temperature of a material, including without limitation, a low- index material, may be determined using various methods apparent to those having ordinary skill in the relevant art, including without limitation, by heating the material in an evaporation source under a substantially high vacuum environment, in some non-limiting examples, about 10'4Torr, and including without limitation, in a crucible and by determining a temperature that may be attained, to at least one of:• observe commencement of the deposition of the material onto an exposed layer surface 11 on a QCM mounted a fixed distance from the crucible;• observe a specific deposition rate, in some non-limiting examples, 0.1 A / sec, onto an exposed layer surface 11 on a QCM mounted a fixed distance from the crucible; and• reach a threshold vapor pressure of the material, in some non-limiting examples, one of about” 10'4and 10'5, Torr.

[0291] In some non-limiting examples, the QCM may be mounted about 65 cm away from the crucible for the purpose of determining the sublimation temperature.

[0292] In some non-limiting examples, the low-index material may have a sublimation temperature of one of between about: 100-320, 100-300, 120-300, 100-250, 140-280, 120-230, 130-220, 140-210, 140- 200, 150-250, and 140-190°C.Melting Point

[0293] In some non-limiting examples, a material, including without limitation, a low- index material, with substantially low inter-molecular forces may tend to exhibit a substantially low melting point.

[0294] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially low melting point may have reduced applicability in some scenarios calling for substantial temperature reliability for temperatures of one of no more than about: 60, 80, and 100°C, in some non-limiting examples, because of changes in physical properties of such material at operating temperatures that approach the melting point.

[0295] In some non-limiting examples, a material with a melting point of about 120°C may have reduced applicability in some scenarios calling for substantially high temperature reliability, including without limitation, of at least about: 100 °C.

[0296] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially high melting point may have applicability in some scenarios calling for substantially high temperature reliability.

[0297] In some non-limiting examples, the low-index material may have a melting temperature, at atmosphere pressure, that is one of at least about: 90, 100, 120, 140, 160, 180, and 200°C.Examples

[0298] In some non-limiting examples, the melting point of select example materials was measured using differential scanning calorimetry. Specifically, the melting point was determined for each sample during the second heating cycle at a heating rate of 10°C / min. The results of the measurement are summarized in Table 5:Table 5Cohesion Energy

[0299] According to Young’s equation (Equation 14) the cohesion energy (fracture toughness / cohesion strength) of a material may tend to be proportional to its surface energy (cf Young, Thomas (1805) “An essay on the cohesion of fluids”, Philosophical Transactions of the Royal Society of London, 95: 65-87).

[0300] According to Lindemann’s criterion, the cohesion energy of a material may tend to be proportional to its melting temperature (cf Nanda, K.K., Sahu, S.N, and Behera, S.N (2002), “Liquid-drop model for the size-dependent melting of low-dimensional systems” Phys. Rev. A. 66 (1): 013208).

[0301] In some non-limiting examples, a material, including without limitation, a low- index material, having substantially low inter-molecular forces may tend to exhibit a substantially low cohesion energy.

[0302] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially low cohesion energy may have reduced applicability in some scenarios that call for substantial fracture toughness, including without limitation, in a device 100 that may tend to undergo at least one of: sheer, and bending, stress during at least one of: manufacture, and use, as such material may tend to crack (fracture) in such scenarios. In some non-limiting examples, a material, including without limitation, a low-index material,having a cohesion energy of no more than about 30 dynes / cm may have reduced applicability in some scenarios in a device 100 manufactured on a flexible substrate 10.

[0303] In some non-limiting examples, a material, including without limitation, a low- index material, that has a substantially high cohesion energy, may have applicability in some scenarios calling for substantially high reliability under at least one of: sheer, and bending, stress, including without limitation, a device 100 manufactured on a flexible substrate 10.

[0304] In some non-limiting examples, a material, including without limitation, a low- index material, having a surface energy that is substantially low but is not unduly low may have applicability in some scenarios that call for substantial reliability under at least one of: sheer, and bending, stress, including without limitation, a device 100 manufactured on a flexible substrate 10.Optical / Band Gap

[0305] In the present disclosure, a semiconductor material may be described as a material that generally exhibits a band gap. In some non-limiting examples, the band gap may be formed between a highest occupied molecular orbital (HOMO) and a lowest unoccupied molecular orbital (LUMO) of the semiconductor material. Semiconductor materials may thus tend to exhibit electrical conductivity that is substantially no more than that of a conductive material (including without limitation, at least one of: a metal, and an alloy), but that is substantially at least that an insulating material (including without limitation, glass). In some non-limiting examples, the semiconductor material may comprise an organic semiconductor material. In some non-limiting examples, the semiconductor material may comprise an inorganic semiconductor material.

[0306] In some non-limiting examples, an optical gap of a material, including without limitation, a low-index material, may tend to correspond to the H0M0-LUM0 gap of the material.

[0307] In some non-limiting examples, a material, including without limitation, a low- index material, having a substantially large / wide optical (H0M0-LUM0 gap) may tend to exhibit substantially weak, including without limitation, substantially no, photoluminescence in at least one of: the deep B(lue) region of the visible spectrum, the near UV spectrum, the visible spectrum, and the NIR spectrum.

[0308] In some non-limiting examples, a material having a substantially small HOMO- LUMO gap may have applicability in some scenarios to detect a film of the material using optical techniques.

[0309] Patterning

[0310] In some non-limiting examples, with reference to FIG. 1, in some non-limiting examples, a patterning coating 110, comprising a patterning material 411, which in some nonlimiting examples, may be a nucleation inhibiting coating (NIC) material, may be disposed, in some non-limiting examples, as a closed coating 140, on an exposed layer surface 11 of an underlying layer 810, including without limitation, a substrate 10, of the device 100, in some non-limiting examples, restricted in lateral extent by selective deposition, including without limitation, using a shadow mask 415 such as, without limitation, a fine metal mask (EMM), including without limitation, to the first portion 101.

[0311] Thus, in some non-limiting examples, in the second portion 102 of the device 100, the exposed layer surface 11 of the underlying layer 810 of the device 100, may be substantially devoid of a closed coating 140 of the patterning coating 110.Patterning Coating

[0312] The patterning coating 110 may comprise a patterning material 411. In some nonlimiting examples, the patterning coating 110 may comprise a closed coating 140 of the patterning material 411.

[0313] The patterning coating 110 may provide an exposed layer surface 11 with a substantially low propensity (including without limitation, a substantially low initial sticking probability (in some non-limiting examples, under the conditions identified in the dual QCM technique described by Walker et al.) against the deposition of a deposited material 531 to be deposited thereon upon exposing such surface to a vapor flux 532 of the deposited material 531, which, in some non-limiting examples, may be substantially no more than the propensity against the deposition of the deposited material 531 to be deposited on the exposed layer surface 11 of the underlying layer 810 of the device 100, upon which the patterning coating 110 has been deposited.

[0314] Because of the attributes, including without limitation, a low initial sticking probability, of at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, against the deposition of the deposited material 531, the exposed layer surface 11 of the first portion 101 comprising the patterning coating 110 may be substantially devoid of a closed coating 140 of the deposited material 531.

[0315] However, exposure of the device 100 to a vapor flux 532 of the deposited material 531 may, in some non-limiting examples, result in the formation of a closed coating 140 of a deposited layer 130 of the deposited material 531 in the second portion 102, where the exposed layer surface 11 of the underlying layer 810 may be substantially devoid of the patterning coating 110.

[0316] Thus, in some non-limiting examples, the patterning coating 110 may be an NIC that provides high deposition (patterning) contrast against subsequent deposition of the deposited material 531, such that the deposited material 531 tends not to be deposited, in some non-limiting examples, as a closed coating 140, where the patterning coating 110 has been deposited.

[0317] In some non-limiting examples, the patterning coating 110 may comprise a patterning material 411. In some non-limiting examples, the patterning material 411 may comprise an NIC material. In some non-limiting examples, the patterning coating 110 may comprise a closed coating 140 of the patterning material 411.

[0318] In some non-limiting examples, there may be scenarios calling for providing a patterning coating 110 for causing formation of a discontinuous layer 160 of at least one particle structure 150, upon the patterning coating 110 in the first portion 101 being subjected to a vapor flux 532 of a deposited material 531. In at least some applications, the attributes of the patterning coating 110 may be such that a closed coating 140 of the deposited material 531 may be formed in the second portion 102, which may be substantially devoid of the patterning coating 110, while only a discontinuous layer 160 of at least one particle structure 150 having at least one characteristic may be formed in the first portion 101 on the patterning coating 110.

[0319] For purposes of simplicity of discussion, in the present disclosure, to the extent that a patterning coating 110 is deposited to act as a base for the deposition of at least one particle structure 150 thereon, such patterning coating 110 may be designated as a particle structurepatterning coating 110p. By contrast, to the extent that a patterning coating 110 is deposited in a first portion 101 to substantially preclude formation in such first portion 101 of a closed coating 140 of the deposited layer 130, thus restricting the deposition of a closed coating 140 of the deposited layer 130 to a second portion 102, such patterning coating 110 may be designated as a non-particle structure patterning coating 110n. Those having ordinary skill in the relevant art will appreciate that in some non-limiting examples, a patterning coating 110 may act as both a particle structure patterning coating 110pand a non-particle structure patterning coating 110n.

[0320] In some non-limiting examples, there may be scenarios calling for formation of a discontinuous layer 160 of at least one particle structure 150 of a deposited material 531, which may be, in some non-limiting examples, of one of a metal, and a metal alloy (metal / alloy), including without limitation, at least one of Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg, in the second portion 102, while depositing a closed coating 140 of the deposited material 531 having a thickness of, without limitation, one of no more than about: 100, 75, 50, 25, and 15, nm. In some non-limiting examples, an amount of the deposited material 531 deposited as a discontinuous layer 160 of at least one particle structure 150 in the first portion 101 may correspond to one of between about: 1-50, 2-25, 5-20, and 7-10% of the amount of the deposited material 531 deposited as a closed coating 140 in the second portion 102, which, by way of non-limiting example may correspond to a thickness of one of no more than about: 100, 75, 50, 25, and 15, nm.

[0321] In some non-limiting examples, the patterning coating 110 may be disposed in a pattern that may be defined by at least one region therein that may be substantially devoid of a closed coating 140 of the patterning coating 110.

[0322] In some non-limiting examples, the at least one region may separate the patterning coating 110 into a plurality of discrete fragments thereof. In some non-limiting examples, the plurality of discrete fragments of the patterning coating 110 may be physically spaced apart from one another in the lateral aspect thereof. In some non-limiting examples, the plurality of the discrete fragments of the patterning coating 110 may be arranged in a regular structure, including without limitation, an array (matrix), such that in some non-limiting examples, the discrete fragments of the patterning coating 110 may be configured in a repeating pattern.

[0323] In some non-limiting examples, at least one of the discrete fragments of the patterning coating 110 may each correspond to an emissive region 210. In some non-limitingexamples, an aperture ratio of the emissive regions 410 may be one of no more than about: 50%, 40%, 30%, and 20%.

[0324] In some non-limiting examples, the patterning coating 110 may be formed as a single monolithic coating.Attributes of Patterning Coating / MaterialComposition

[0325] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, may comprise at least one of an: F, and Si, atom. By way of nonlimiting example, the patterning material 411 for forming the patterning coating 110 may be a compound that comprises at least one of: F and Si.

[0326] In some non-limiting examples, the patterning material 411 may comprise a compound that comprises F. In some non-limiting examples, the patterning material 411 may comprise a compound that comprises F and a C atom. In some non-limiting examples, the patterning material 411 may comprise a compound that comprises F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 0.5, 0.7, 1.0, 1.5, 2.0, and 2.5.

[0327] In some non-limiting examples, an atomic ratio of F to C may be determined by counting all of the F atoms present in the compound structure, and for C atoms, only counting the sp3hybridized C atoms present in the compound structure. In some non-limiting examples, the patterning material 411 may comprise a compound that comprises, as part of its molecular substructure, a moiety comprising F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 1.0, 1.5, and 2.0.

[0328] In some non-limiting examples, the patterning material 411 may comprise an organic-inorganic hybrid material.

[0329] In some non-limiting examples, the patterning material 411 may comprise an oligomer.

[0330] In some non-limiting examples, the patterning material 411 may comprise a compound having a molecular structure comprising a backbone and at least one functional group bonded to the backbone. In some non-limiting examples, the backbone may be an inorganic moiety, and the at least one functional group may be an organic moiety.

[0331] In some non-limiting examples, such compound may have a molecular structure comprising a siloxane group. In some non-limiting examples, the siloxane group may be one ofa: linear, branched, and cyclic, siloxane group. In some non-limiting examples, the backbone may comprise a siloxane group. In some non-limiting examples, the backbone may comprise a siloxane group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group. In some non-limiting examples, such compound may comprise fluoro-siloxanes, including without limitation, Example Material 6 and Example Material 9 (discussed below).

[0332] In some non-limiting examples, the compound may have a molecular structure comprising a silsesquioxane group. In some non-limiting examples, the silsesquioxane group may be a POSS. In some non-limiting examples, the backbone may comprise a silsesquioxane group. In some non-limiting examples, the backbone may comprise a silsesquioxane group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group. In some non-limiting examples, such compound may comprise fluoro-silsesquioxane and fluoro-POSS, including without limitation, Example Material 8 (discussed below).

[0333] In some non-limiting examples, the compound may have a molecular structure comprising at least one of: a substituted aryl group, an unsubstituted aryl group, a substituted heteroaryl group, and an unsubstituted heteroaryl group. In some non-limiting examples, the aryl group may be at least one of: phenyl, and naphthyl. In some non-limiting examples, at least one C atom of an aryl group may be substituted by a heteroatom, which by way of non-limiting example may be at least one of: O, N, and S, to derive a heteroaryl group. In some non-limiting examples, the backbone may comprise at least one of: a substituted aryl group, an unsubstituted aryl group, a substituted heteroaryl group, and an unsubstituted heteroaryl group. In some nonlimiting examples, the backbone may comprise at least one of: a substituted aryl group, an unsubstituted aryl group, a substituted heteroaryl group, and an unsubstituted heteroaryl group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group.

[0334] In some non-limiting examples, the compound may have a molecular structure comprising at least one of: a substituted hydrocarbon group, an unsubstituted hydrocarbon group, a linear hydrocarbon group, a branched hydrocarbon group, and a cyclic hydrocarbon group. In some non-limiting examples, at least one C atom of the hydrocarbon group may be substituted by a heteroatom, including without limitation, at least one of: O, N, and S.

[0335] In some non-limiting examples, the compound may have a molecular structure comprising a phosphazene group. In some non-limiting examples, the phosphazene group may be at least one of a: linear, branched, and cyclic, phosphazene group. In some non-limiting examples, the backbone may comprise a phosphazene group. In some non-limiting examples, the backbone may comprise a phosphazene group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group, including without limitation, a fluoro-phosphazene, including without limitation, EM-4 (discussed below).

[0336] In some non-limiting examples, the compound may be a fluoropolymer. In some non-limiting examples, the compound may be a block copolymer comprising F. In some nonlimiting examples, the compound may be an oligomer. In some non-limiting examples, the oligomer may be a fluorooligomer. In some non-limiting examples, the compound may be a block oligomer comprising F. In some non-limiting examples, at least one of: fluoropolymers, and fluorooligomers, may comprise those having the molecular structure of at least one of: EM-3, EM-5, and EM- 7 (discussed herein).

[0337] In some non-limiting examples, the compound may be a metal complex. In some non-limiting examples, the metal complex may be an organo-metal complex. In some nonlimiting examples, the organo-metal complex may comprise F. In some non-limiting examples, the organo-metal complex may comprise at least one ligand comprising F. In some non-limiting examples, the at least one ligand comprising F may comprise a fluoroalkyl group.

[0338] In some non-limiting examples, the patterning material 411 may comprise a plurality of different materials.Initial Sticking Probability

[0339] In some non-limiting examples, the initial sticking probability of the patterning material 411 may be determined by depositing such material as at least one of: a film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, having sufficient thickness so as to mitigate / reduce any effects on the degree of inter-molecular interaction with the underlying layer upon deposition on a surface thereof. In some non-limiting examples, the initial sticking probability may be measured on a film / coating having a thickness of one of at least about: 20, 25, 30, 50, 60, and 100, nm.

[0340] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may have an initial sticking probability against the deposition of the deposited material 531, that is one of no more than about: 0.3, 0.2, 0.15, 0.1, 0.08, 0.05, 0.03, 0.02, 0.01, 0.008, 0.005, 0.003, 0.001, 0.0008, 0.0005, 0.0003, and 0.0001.

[0341] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may have an initial sticking probability against the deposition of at least one of: Ag, and Mg that is one of no more than about: 0.3, 0.2, 0.15, 0.1, 0.08, 0.05, 0.03, 0.02, 0.01, 0.008, 0.005, 0.003, 0.001, 0.0008, 0.0005, 0.0003, and 0.0001.

[0342] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may have an initial sticking probability against the deposition of a deposited material 531 of one of between about: 0.15-0.0001, 0.1-0.0003, 0.08-0.0005, 0.08- 0.0008, 0.05-0.001, 0.03-0.0001, 0.03-0.0003, 0.03-0.0005, 0.03-0.0008, 0.03-0.001, 0.03-0.005, 0.03-0.008, 0.03-0.01, 0.02-0.0001, 0.02-0.0003, 0.02-0.0005, 0.02-0.0008, 0.02-0.001, 0.02- 0.005, 0.02-0.008, 0.02-0.01, 0.01-0.0001, 0.01-0.0003, 0.01-0.0005, 0.01-0.0008, 0.01-0.001, 0.01-0.005, 0.01-0.008, 0.008-0.0001, 0.008-0.0003, 0.008-0.0005, 0.008-0.0008, 0.008-0.001, 0.008-0.005, 0.005-0.0001, 0.005-0.0003, 0.005-0.0005, 0.005-0.0008, and 0.005-0.001.

[0343] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may have an initial sticking probability against the deposition of a plurality of deposited materials 531, including without limitation, selected from at least one of: Ag, Mg, Yb, Cd, and Zn, that is no more than a threshold value. In some non-limiting examples, such threshold value may be one of about: 0.3, 0.2, 0.18, 0.15, 0.13, 0.1, 0.08, 0.05, 0.03, 0.02, 0.01, 0.008, 0.005, 0.003, 0.001, 0.0008, 0.0005, 0.0003, and 0.0001.

[0344] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may have an initial sticking probability that is no more than such threshold value against the deposition of a plurality of deposited materials 531 selected from at least one of: Ag, Mg, Yb, Cd, and Zn. In some non-limiting examples, the patterning coating 110 may exhibit an initial sticking probability of no more than such threshold value against the deposition of a plurality of deposited materials 531 selected from at least one of: Ag, Mg, and Yb.

[0345] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may exhibit an initial sticking probability against the deposition of a first deposited material 531 of, including without limitation, below, a first threshold value, and an initial sticking probability against the deposition of a second deposited material 531 of, including without limitation, below, a second threshold value. In some nonlimiting examples, the first deposited material 531 may be Ag, and the second deposited material 531 may be Mg. In some non-limiting examples, the first deposited material 531 may be Ag, and the second deposited material may be Yb. In some non-limiting examples, the first deposited material 531 may be Yb, and the second deposited material 531 may be Mg. In some nonlimiting examples, the first threshold value may exceed the second threshold value.

[0346] In some non-limiting examples, there may be scenarios calling for providing a patterning coating 110 for causing formation of a discontinuous layer 160 of at least one particle structure 150, upon the patterning coating 110 being subjected to a vapor flux 532 of a deposited material 531. In some non-limiting examples, the patterning coating 110 may exhibit a substantially low initial sticking probability such that a closed coating 140 of the deposited material 531 may be formed in the second portion 102, which may be substantially devoid of the patterning coating 110, while the discontinuous layer 160 of at least one particle structure 150 having at least one characteristic may be formed in the first portion 101 on the patterning coating 110. In some non-limiting examples, there may be scenarios calling for formation of a discontinuous layer 160 of at least one particle structure 150 of a deposited material 531, which may be, in some non-limiting examples, of one of: a metal, and a metal alloy, in the secondportion 102, while depositing a closed coating 140 of the deposited material 531, in some nonlimiting examples, having a thickness of one of no more than about: 100, 50, 25, and 15, nm. In some non-limiting examples, an amount of the deposited material 531 deposited as a discontinuous layer 160 of at least one particle structure 150 in the first portion 101 may correspond to one of between about: 1-50, 2-25, 5-20, and 7-10% of the amount of the deposited material 531 deposited as a closed coating 140 in the second portion 102, which in some nonlimiting examples may correspond to a thickness of one of no more than about: 100, 75, 50, 25, and 15, nm.

[0347] In some non-limiting examples, there may be a positive correlation between the initial sticking probability of at least one of the: patterning coating 110, and patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, against the deposition of the deposited material 531, and an average layer thickness of the deposited material 531 thereon.Transmittance

[0348] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have a transmittance for EM radiation of at least a threshold transmittance value, after being subjected to a vapor flux 532 of the deposited material 531, including without limitation, Ag.

[0349] In some non-limiting examples, such transmittance may be measured after exposing the exposed layer surface 11 of at least one of: the patterning coating 110 and the patterning material 411, formed as a thin film, to a vapor flux 532 of the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, under typical conditions that may be used for depositing an electrode of an opto-electronic device 200, which in some non-limiting examples, may be a cathode of an organic light-emitting diode (OLED) device 200.

[0350] In some non-limiting examples, the conditions for subjecting the exposed layer surface 11 to the vapor flux 532 of the deposited material 531, including without limitation, atleast one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, may comprise: maintaining a vacuum pressure at a reference pressure, including without limitation, of one of about: 10'4Torr and 10'5Torr; the vapor flux 532 of the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, being substantially consistent with a reference deposition rate, including without limitation, of about 1 angstrom (A) / sec, which in some non-limiting examples, may be monitored using a QCM; the vapor flux 532 of the deposited material 531 being directed toward the exposed layer surface 11 at an angle that is substantially close to normal to a plane of the exposed layer surface 11; the exposed layer surface 11 being subjected to the vapor flux 532 of the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, until a reference average layer thickness, including without limitation, of about 15 nm, is reached, and upon such reference average layer thickness being attained, the exposed layer surface 11 not being further subjected to the vapor flux of the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag- containing materials, including without limitation, MgAg.

[0351] In some non-limiting examples, the exposed layer surface 11 being subjected to the vapor flux 532 of the deposited material 531, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, may be substantially at room temperature (e.g. about 25°C). In some non-limiting examples, the exposed layer surface 11 being subjected to the vapor flux 532 of the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, may be positioned about 65 cm away from an evaporation source by which the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, is evaporated.

[0352] In some non-limiting examples, the threshold transmittance value may be measured at a wavelength in the visible spectrum, which may be one of at least about: 460 nm, 500 nm, 550 nm, and 600 nm. In some non-limiting examples, the threshold transmittance value may be measured at a wavelength in at least one of: the IR, and NIR, spectrum. In some non-limiting examples, the threshold transmittance value may be measured at a wavelength of one of about: 700 nm, 900 nm, and 1,000 nm. In some non-limiting examples, the threshold transmittance value may be expressed as a percentage of incident EM power that may be transmitted through a sample. In some non-limiting examples, the threshold transmittance value may be one of at least about: 60%, 65%, 70%, 75%, 80%, 85%, and 90%.

[0353] Those having having ordinary skill in the relevant art will appreciate that high transmittance may generally indicate an absence of a closed coating 140 of the deposited material 531, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg. On the other hand, low transmittance may generally indicate presence of a closed coating 140 of the deposited material 531, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, since metallic thin films, particularly when formed as a closed coating 140, may exhibit a high degree of absorption of EM radiation.

[0354] A series of samples was fabricated to measure the transmittance of an example material, as well as to visually observe whether a closed coating 140 of Ag was formed on the exposed layer surface 11 of such example material. Each sample was prepared by depositing, on a glass substrate 10, an approximately 50 nm thick coating of an example material, then subjecting the exposed layer surface 11 of the coating to a vapor flux 532 of Ag at a rate of about 1 A / sec until a reference layer thickness of about 15 nm was reached. Each sample was then visually analyzed and the transmittance through each sample was measured.

[0355] The molecular structures of the example materials used in the samples herein are set out in Table 6 below:Table 6

[0356] Those having ordinary skill in the relevant art will appreciate that samples having little to no deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, present thereon may be substantially transparent, while samples with substantial amounts of at least one of: a metal, and an alloy, deposited thereon, including without limitation, as a closed coating 140, may in some non-limiting examples, exhibit a substantially reduced transmittance. Accordingly, the performance of various example coatings as a patterning coating 110 may be assessed by measuring transmittance through the samples, which may be inversely correlated to at least one of: an amount, and an average layer thickness, of the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, in the form of at least one of Yb, Ag, Mg, and Ag- containing materials, including without limitation, MgAg, being deposited thereon, since metallicthin films, including without limitation, when formed as a closed coating 140, may exhibit a high degree of absorption of EM radiation.

[0357] The samples in which a substantially closed coating 140 of a deposited material 531, in the form of Ag, had formed were visually identified, and the presence of such closed coating 140 in these samples was further confirmed by measurement of transmittance therethrough, which showed transmittance of no more than about 50% at a wavelength of about 460 nm.

[0358] In addition, for samples in which the absence of formation of a closed coating 140 of a deposited material 531, in the form of Ag, was identified, the absence of such closed coating 140 in these samples was further confirmed by measurement of EM transmittance therethrough, which showed transmittance (of EM radiation at a wavelength of about 460 nm) of at least about 70%.

[0359] The results are summarized in Table 7 below:Table 7

[0360] In some non-limiting examples, it was found that the materials used in the first 7 samples (HT211 to EM-2) and EM-9 in Tables 6 and 7 may have reduced applicability in some scenarios for inhibiting the deposition of the deposited material 531 thereon, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg.

[0361] On the other hand, it was found that EM-3 to EM-8 may have applicability in some scenarios, to act as a patterning coating 110 for inhibiting the deposition of the deposited material 531 including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and Ag-containing materials, including without limitation, MgAg, thereon.Deposition Contrast

[0362] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a given at least one of: a metal, and an alloy, including without limitation, at least one of: Mg, Ag, and MgAg, may have a substantially high deposition contrast when deposited on a substrate 10.

[0363] In some non-limiting examples, if a substrate 10 tends to act as a nucleationpromoting coating (NPC) 820 (FIG. 8A), and a portion 101, 102 thereof is coated with a material, including without limitation, a patterning material 411, that may tend to function as an NIC against deposition of a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag- containing material, including without limitation, MgAg, a coated portion (first portion 101) and an uncoated portion (second portion 102) may tend to have different at least one of: initial sticking probabilities, and nucleation rates, such that the deposited material 531 deposited thereon may tend to have different average film thicknesses.

[0364] As used herein, a quotient of an average film thickness of the deposited material 531 deposited in the second portion 102 divided by an average film thickness of the depositedmaterial in the first portion 101 in such scenario may be generally referred to as a deposition contrast. Thus, if the deposition contrast is substantially high, an average film thickness of the deposited material 531 in the second portion 102 may be substantially at least that of an average film thickness of the deposited material 531 in the first portion 101.

[0365] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a given deposited material 531, may have a substantially high deposition contrast when deposited on a substrate 10.

[0366] In some non-limiting examples, there may be a negative correlation between the initial sticking probability of at least one of the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, against the deposition of the deposited material 531 and a deposition contrast thereof, that is, a low initial sticking probability may be highly correlated with a high deposition contrast.

[0367] In some non-limiting examples, if the deposition contrast is substantially high, there may be little to no deposited material 531 deposited in the first portion 101, when there is sufficient deposition of the deposited material 531 to form a closed coating 140 thereof in the second portion 102.

[0368] In some non-limiting examples, if the deposition contrast is substantially low, there may be a discontinuous layer 160 of at least one particle structure 150 of the deposited material 531 deposited in the first portion 101, when there is sufficient deposition of the deposited material 531 to form a closed coating 140 in the second portion 102.

[0369] In some non-limiting examples, there may be scenarios calling for the formation of a discontinuous layer 160 of at least one particle structure 150 of the deposited material 531, in the first portion 101, when an average layer thickness of a closed coating 140 of the deposited material 531 in the second portion 102 is substantially small, including without limitation, one of no more than about: 100, 50, 25, and 15, nm, including without limitation, the formation of nanoparticles (NPs) in the first portion 101, where absorption of light by such NPs is called for, including without limitation, to protect an underlying layer 810 from light having a wavelength of no more than about 460 nm.

[0370] In some non-limiting examples, in such scenarios, there may be applicability for a deposition contrast of one of between about: 2-100, 4-50, 5-20, and 10-15.

[0371] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low deposition contrast against deposition of a deposited material 531, may have reduced applicability in some scenarios calling for substantially high deposition contrast, including without limitation, where an average layer thickness of the deposited material 531 in the first portion 101 is large, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm.

[0372] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low deposition contrast against deposition of a deposited material 531, may have reduced applicability in some scenarios calling for substantially high deposition contrast, including without limitation, scenarios calling for at least one of: the substantial absence of a closed coating 140, and a high density of, particle structures 150 in the first portion 101, including without limitation, when an average layer thickness of the deposited material 531 in the second portion 102 is large, including without limitation, one of at least about: 95, 45, 20, 10, and 8 nm, including without limitation, in some scenarios calling for the substantial absence of absorption of light in at least one of the visible spectrum and the NIR spectrum, including without limitation, scenarios calling for an increased transparency to light having a wavelength that is at least about 460 nm.

[0373] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low deposition contrast against the deposition of a deposited material 531, may have applicability in some scenarios calling for at least one of: a discontinuous layer 160 of, and a low density of, particle structures 150 of the deposited material 531 in the first portion 101, when an average layer thickness of a closed coating 140 of the deposited material 531 in the second portion 102 is substantially high, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm. In some non-limiting examples, a deposition contrast of one of between about: 2-100, 4-50, 5-20, and 10-15, may have applicability in some scenarios when an average layer thickness of the deposited material 531 in the second portion 102 is substantially high, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm.

[0374] In some non-limiting examples, a material, including without limitation, a patterning material 411, may tend to have a substantially low deposition contrast if the initial sticking probability of such material against deposition of at least one of: a metal, and an alloy, including without limitation, at least one of: Mg, Ag, and MgAg, is substantially high.Surface Energy

[0375] In some non-limiting examples, a characteristic surface energy may be measured from a surface formed by the material deposited (coated) in a thin film form.

[0376] Various methods and theories for determining the surface energy of a solid are known.

[0377] In some non-limiting examples, a surface energy may be calculated (derived) based on a series of contact angle measurements, in which various liquids may be brought into contact with a surface of a solid to measure the contact angle between the liquid-vapor interface and the surface. In some non-limiting examples, a surface energy of a solid surface may be equal to the surface tension of a liquid with the highest surface tension that completely wets the surface.

[0378] In some non-limiting examples, the critical surface tension of a surface may be determined according to the Zisman method, as further detailed in W. A. Zisman, Advances in Chemistry 3 (1964), pp. 1-51.

[0379] In some non-limiting examples, a characteristic surface energy of a material, including without limitation, a patterning material 411, in a coating, including without limitation, a patterning coating 110, may be determined by depositing the material as a substantially pure coating (e.g. a coating formed by a substantially pure material) on a substrate 10 and measuring a contact angle thereof with an applicable series of probe liquids.

[0380] In some non-limiting examples, a Zisman plot may be used to determine a maximum value of surface tension that would result in complete wetting (i.e. a contact angle 0c of 0°) of the surface.

[0381] A material which has applicability for use in providing the patterning coating may generally have a low surface energy when deposited as a thin film (coating) on a surface. In some non-limiting examples, a material with a low surface energy may exhibit low intermolecular forces.

[0382] Without wishing to be bound by any particular theory, it is now postulated that a material with a substantially high surface energy may have applicability at least in some applications that call for a high temperature reliability.

[0383] Without wishing to be bound by any particular theory, it has now been found that a patterning coating 110 comprising a material which, when deposited as a thin film, exhibits a substantially high surface energy, may, in some non-limiting examples, form a discontinuous layer 160 of at least one particle structure 150 of a deposited material 531 in the first portion 101, and a closed coating 140 of the deposited material 531 in the second portion 102, including without limitation, in cases where a thickness of the closed coating is, in some non-limiting examples, one of no more than about: 100, 75, 50, 25, and 15, nm.

[0384] In some non-limiting examples, a series of samples was fabricated to measure the critical surface tension of the surfaces formed by the various materials. The results of the measurement are summarized in Table 8:Table 8

[0385] Based on the foregoing measurement of the critical surface tension in Table 8 and the previous observation regarding one of the: presence, and absence, of a substantially closed coating 140 of a deposited material 531, in the form of Ag, it was found that materials that form substantially low surface energy surfaces when deposited as a coating, including without limitation, a patterning coating 110, which in some non-limiting examples, may be those having a critical surface tension of between about: 12-23 dynes / cm, may have applicability for forming the patterning coating 110 to inhibit deposition of a deposited material 531 thereon, including without limitation, at least one of Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg.

[0386] Without wishing to be bound by any particular theory, it may be postulated that materials that form a surface having a surface energy that is no more than, by way of nonlimiting example, about 13 dynes / cm, may have reduced applicability as a patterning material 411 in some scenarios, as such materials may exhibit at least one of: substantially poor adhesion to layer(s) surrounding such materials, a low melting point, and a low sublimation temperature.

[0387] In some non-limiting examples, a material, including without limitation, a patterning material 411 that may tend to function as an NIC for a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Mg, Ag, and a Ag-containing material, including without limitation, MgAg, may tend to exhibit a substantially low surface energy when deposited as a thin film (coating) on an exposed layer surface 11.

[0388] In some non-limiting examples, a material, including without limitation, a patterning material 411, may tend to exhibit a substantially low surface energy when deposited as a thin film (coating) on an exposed layer surface 11.

[0389] In some non-limiting examples, a material, including without limitation, a patterning material 411, with a substantially low surface energy may tend to exhibit substantially low inter-molecular forces.

[0390] In some non-limiting examples, there may be scenarios calling for a patterning material 411 that has a substantially low surface energy that is not unduly low.

[0391] In some non-limiting examples, a material, including without limitation, a patterning material 411, with a substantially high surface energy may have applicability for some scenarios to detect a film of such material using optical techniques.

[0392] Without wishing to be bound by any particular theory, it may be postulated that, in some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high surface energy may have applicability for some scenarios that call for substantially high temperature reliability.

[0393] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for at least one of: a metal, and an alloy, including without limitation, at least one of Mg, Ag, and a Ag-containing material, including without limitation, MgAg, having a substantially high surface energy may have applicability in some scenarios calling for a discontinuous layer 160 of particle structures 150 of at least one of: the metal, and the alloy, in the first portion 101, when an average layer thickness of a continuous coating 140 of at least one of: the metal, and the alloy, in the second portion 102 is substantially low, including without limitation, one of no more than about: 100, 50, 25, and 15, nm.

[0394] In some non-limiting examples, a material, including without limitation, a patterning material 411, that may function as an NIC for a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg, having a substantially low surface energy may have applicability in some scenarios calling for one of: a discontinuous layer 160 of, and a low density of, particle structures 150 of the deposited material 531 in the first portion 101, when an average layer thickness of a closed coating 140 of the deposited material 531 in the second portion 102 is substantially high, including without limitation, one of at least about: 95, 45, 20, 10, and 8, nm.

[0395] In some non-limiting examples, the surface of at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, comprising the compounds described herein,may exhibit a surface energy of one of no more than about: 24, 22, 20, 18, 16, 15, 13, 12, and 11, dynes / cm.

[0396] In some non-limiting examples, the surface values in various non-limiting examples herein may correspond to such values measured at around normal temperature and pressure (NTP), which may correspond to a temperature of 20°C, and an absolute pressure of 1 atm.

[0397] In some non-limiting examples, the surface energy may be one of at least about: 6, 7, and 8, dynes / cm.

[0398] In some non-limiting examples, the surface energy may be one of between about: 10-20, and 13-19, dynes / cm.TemperatureGlass Transition Temperature

[0399] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of: a film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have a glass transition temperature that is one of: one of at least about: 300, 200, 170, 150, 130, 120, 110, and 100°C, and one of no more than about: 20, 0, -20, -30, and -50°C.Sublimation Temperature

[0400] In some non-limiting examples, a material, including without limitation, a patterning material 411, having substantially low inter-molecular forces may tend to exhibit a substantially low sublimation temperature.

[0401] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low sublimation temperature, may have reduced applicability for manufacturing processes that may call for substantially precise control of an average layer thickness of a closed coating 140 of a deposited film of the material.

[0402] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a sublimation temperature that is one of no more than about: 140, 120, 110, 100 and 90°C, may tend to encounter constraints on at least one of: a depositionrate and an average layer thickness, of a film comprising such material that may be deposited using known deposition methods, including without limitation, vacuum thermal evaporation.

[0403] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high sublimation temperature may have applicability in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0404] In some non-limiting examples, the patterning material may have a sublimation temperature of one of between about: 100-320, 120-300, 140-280, and 150-250°C. In some nonlimiting examples, such sublimation temperature may allow the patterning material 411 to be substantially readily deposited as a coating using PVD.

[0405] In some non-limiting examples, a material with substantially low intermolecular forces may exhibit a substantially low sublimation temperature.

[0406] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low sublimation temperature, may have reduced applicability for manufacturing processes that may call for substantially precise control of an average layer thickness of a closed coating 140 of the material.

[0407] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a sublimation temperature that is one of no more than about: 140, 120, 110, 100 and 90°C, may tend to encounter constraints on at least one of: the deposition rate and the average layer thickness, of a film comprising such material that may be deposited using known deposition methods, including without limitation, vacuum thermal evaporation.

[0408] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high sublimation temperature may have applicability in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0409] The sublimation temperature of a material, including without limitation, a patterning material 411, may be determined using various methods apparent to those having ordinary skill in the relevant art, including without limitation, by heating the material in an evaporation source under a substantially high vacuum environment, in some non-limiting examples, about 10'4Torr, and including without limitation, in a crucible and by determining a temperature that may be attained, to at least one of:• observe commencement of the deposition of the material onto an exposed layer surface 11 on a QCM mounted a fixed distance from the crucible;• observe a specific deposition rate, in some non-limiting examples, 0.1 A / sec, onto an exposed layer surface 11 on a QCM mounted a fixed distance from the crucible; and• reach a threshold vapor pressure of the material, in some non-limiting examples, one of about” 10'4and 10'5, Torr.

[0410] In some non-limiting examples, the QCM may be mounted about 65 cm away from the crucible for the purpose of determining the sublimation temperature.

[0411] In some non-limiting examples, the patterning material 411 may have a sublimation temperature of one of between about: 100-320, 100-300, 120-300, 100-250, 140-280, 120-230, 130-220, 140-210, 140- 200, 150-250, and 140-190°C.Melting Point

[0412] In some non-limiting examples, a material, including without limitation, a patterning material 411, with substantially low inter-molecular forces may tend to exhibit a substantially low melting point.

[0413] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low melting point may have reduced applicability in some scenarios calling for substantial temperature reliability for temperatures of one of no more than about: 60, 80, and 100°C, in some non-limiting examples, because of changes in physical properties of such material at operating temperatures that approach the melting point.

[0414] In some non-limiting examples, a material with a melting point of about 120°C may have reduced applicability in some scenarios calling for substantially high temperature reliability, including without limitation, of at least about: 100 °C.

[0415] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially high melting point may have applicability in some scenarios calling for substantially high temperature reliability.

[0416] In some non-limiting examples, at least one of: the patterning coating 110 and the compound thereof may have a melting temperature, at atmosphere pressure, that is one of at least about: 90, 100, 120, 140, 160, 180, and 200°C.Examples

[0417] In some non-limiting examples, the melting point of select example materials was measured using differential scanning calorimetry. Specifically, the melting point was determined for each sample during the second heating cycle at a heating rate of 10°C / min. The results of the measurement are summarized in Table 9:Table 9Cohesion Energy

[0418] According to Young’s equation (Equation 14) the cohesion energy (fracture toughness / cohesion strength) of a material may tend to be proportional to its surface energy (cf Young, Thomas (1805) “An essay on the cohesion of fluids”, Philosophical Transactions of the Royal Society of London, 95: 65-87).

[0419] According to Lindemann’s criterion, the cohesion energy of a material may tend to be proportional to its melting temperature (cf Nanda, K.K., Sahu, S.N, and Behera, S.N (2002), “Liquid-drop model for the size-dependent melting of low-dimensional systems” Phys. Rev. A. 66 (1): 013208).

[0420] In some non-limiting examples, a material, including without limitation, a patterning material 411, having substantially low inter-molecular forces may tend to exhibit a substantially low cohesion energy.

[0421] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low cohesion energy may have reduced applicability in some scenarios that call for substantial fracture toughness, including without limitation, in a device 100 that may tend to undergo at least one of: sheer, and bending, stress during at least one of: manufacture, and use, as such material may tend to crack (fracture) in such scenarios. In some non-limiting examples, a material, including without limitation, a patterning material 411, having a cohesion energy of no more than about 30 dynes / cm may have reduced applicability in some scenarios in a device 100 manufactured on a flexible substrate 10.

[0422] In some non-limiting examples, a material, including without limitation, a patterning material 411, that has a substantially high cohesion energy, may have applicability in some scenarios calling for substantially high reliability under at least one of: sheer, and bending, stress, including without limitation, a device 100 manufactured on a flexible substrate 10.

[0423] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a surface energy that is substantially low but is not unduly low may have applicability in some scenarios that call for substantial reliability under at least one of: sheer, and bending, stress, including without limitation, a device 100 manufactured on a flexible substrate 10.Optical / Band Gap

[0424] In the present disclosure, a semiconductor material may be described as a material that generally exhibits a band gap. In some non-limiting examples, the band gap may be formed between a highest occupied molecular orbital (HOMO) and a lowest unoccupied molecular orbital (LUMO) of the semiconductor material. Semiconductor materials may thus tend to exhibit electrical conductivity that is substantially no more than that of a conductive material (including without limitation, at least one of: a metal, and an alloy), but that is substantially at least that an insulating material (including without limitation, glass). In some non-limiting examples, the semiconductor material may comprise an organic semiconductor material. In some non-limiting examples, the semiconductor material may comprise an inorganic semiconductor material.

[0425] In some non-limiting examples, an optical gap of a material, including without limitation, a patterning material 411, may tend to correspond to the H0M0-LUM0 gap of the material.

[0426] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially large / wide optical (H0M0-LUM0 gap) may tend to exhibit substantially weak, including without limitation, substantially no, photoluminescence in at least one of: the deep B(lue) region of the visible spectrum, the near UV spectrum, the visible spectrum, and the NIR spectrum.

[0427] In some non-limiting examples, a material having a substantially small H0M0- LUMO gap may have applicability in some scenarios to detect a film of the material using optical techniques.Refractive Index and Extinction Coefficient

[0428] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have a low refractive index.

[0429] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have a refractive index for light at a wavelength of 550 nm that may be one of no more than about: 1.55, 1.5, 1.45, 1.43, 1.4, 1.39, 1.37, 1.35, 1.32, and 1.3.

[0430] In some non-limiting examples, the refractive index, of the patterning coating 110 may be no more than about 1.7. In some non-limiting examples, the refractive index of the patterning coating 110 may be one of no more than about: 1.6, 1.5, 1.4, and 1.3. In some nonlimiting examples, the refractive index of the patterning coating 110 may be one of between about: 1.2-1.6, 1.2-1.5, and 1.25-1.45. As further described in various non-limiting examples above, the patterning coating 110 exhibiting a substantially low refractive index may have application in some scenarios, to enhance at least one of: the optical properties, and performance, of the device 100, including without limitation, by enhancing outcoupling of light emitted by the opto-electronic device 200.

[0431] Without wishing to be bound by any particular theory, it has been observed that providing the patterning coating 110 having a substantially low refractive index may, at least insome devices 100, enhance transmission of external light through the second portion 102 thereof. In some non-limiting examples, devices 100 including an air gap therein, which may be arranged near to the patterning coating 110, may exhibit a substantially high transmittance when the patterning coating 110 has a substantially low refractive index relative to a similarly configured device 100 in which such low-index patterning coating 110 was not provided.

[0432] In some non-limiting examples, a series of samples was fabricated to measure the refractive index at a wavelength of 550 nm for the coatings formed by some of the various example materials. The results of the measurement are summarized in Table 10 below:Table 10

[0433] Based on the foregoing measurement of refractive index in Table 10, and the observation regarding one of: the presence, and absence, of a substantially closed coating 140 of Ag in these samples, it was found that materials that form a low refractive index coating, which in some non-limiting examples, may be those having a refractive index of one of no more than about: 1.4 and 1.38, may have applicability in some scenarios for forming the patterning coating 110 to substantially inhibit deposition of a deposited material 531 thereon, including withoutlimitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg.

[0434] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have a low refractive index.

[0435] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have a refractive index for light at a wavelength of 550 nm that may be one of no more than about: 1.55, 1.5, 1.45, 1.43, 1.4, 1.39, 1.37, 1.35, 1.32, and 1.3.

[0436] In some non-limiting examples, the patterning coating 110 may be at least one of: substantially transparent, and light-transmissive.

[0437] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under similar circumstances to the deposition of the patterning coating 110 within the device 100, may have an extinction coefficient that may be no more than about 0.01 for light at a wavelength that is one of at least about: 600, 500, 460, 420, and 410, nm.

[0438] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may have an extinction coefficient that may be one of at least about: 0.05, 0.1, 0.2, and 0.5 for light at a wavelength that is one of no more than about: 400, 390, 380, and 370, nm.

[0439] In this way, at least one of: the patterning coating 110, and the patterning material 411, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may absorb light in the UVA spectrum incident upon the device 100, thereby reducing a likelihood that light in the UVA spectrum may impart constraints in terms of at least one of: device performance, device stability, device reliability, and device lifetime.

[0440] In some non-limiting examples, the patterning coating 110 may exhibit an extinction coefficient of one of no more than about: 0.1, 0.08, 0.05, 0.03, and 0.01, in the visible light spectrum.Photoluminescence, Absorption and Other Optical Effects

[0441] In some non-limiting examples, photoluminescence of at least one of: a coating, and a material may be observed through a photoexcitation process. In a photoexcitation process, at least one of: the coating, and the material, may be subjected to light emitted by a source, including without limitation, a UV lamp.

[0442] When the emitted light is absorbed by at least one of: the coating, and the material, the electrons thereof may be temporarily excited. Following excitation, at least one relaxation process may occur, including without limitation, at least one of: fluorescence and phosphorescence, in which light may be emitted from at least one of: the coating, and the material.

[0443] The light emitted from at least one of: the coating, and the material, during such process may be detected, for example, by a photodetector, to characterize the photoluminescence properties of at least one of: the coating, and the material.

[0444] In some non-limiting examples, the optical gap of the various coatings / materials may correspond to an energy gap of the coating / material from which light is one of: absorbed, and emitted, during the photoexcitation process.

[0445] In some non-limiting examples, photoluminescence may be detected by subjecting the coating / material to light having a wavelength corresponding to the UV spectrum, such as in some non-limiting examples, one of: UVA, and UVB. In some non-limiting examples, light for causing photoexcitation may have a wavelength of about 365 nm.

[0446] In some non-limiting examples, the patterning material 411 may not substantially exhibit photoluminescence at any wavelength corresponding to the visible spectrum.

[0447] In some non-limiting examples, the patterning material 411 may not exhibit photoluminescence upon being subjected to light having a wavelength of one of at least about: 300, 320, 350 m, and 365, nm.

[0448] As used herein, at least one of: the coating, and the material, that is photolumine scent, may be one that exhibits photoluminescence at a wavelength when irradiatedwith an excitation radiation at a certain wavelength. In some non-limiting examples, at least one of: the coating, and the material, that is photoluminescent, may exhibit photoluminescence at a wavelength that exceeds about 365 nm, which is a wavelength of the radiation source frequently used in fluorescence microscopy, upon being irradiated with an excitation radiation having a wavelength of 365 nm.

[0449] At least one of: the coating, and the material, that is photoluminescent, may be detected on a substrate 10 using standard optical techniques including without limitation, fluorescence microscopy, which may establish the presence of such at least one of: the coating, and the material.

[0450] In some non-limiting examples, a coating, including without limitation, a patterning coating 110, may exhibit photoluminescence, including without limitation, by comprising a material that exhibits photoluminescence.

[0451] In some non-limiting examples, the presence of such patterning coating 110 may be detected (observed) using routine characterization techniques such as fluorescence microscopy upon deposition of the patterning coating 110.

[0452] In some non-limiting examples, a coating, including without limitation, a patterning coating 110, may exhibit photoluminescence at a wavelength corresponding to at least one of: the UV spectrum, and visible spectrum, including without limitation, by comprising a material that exhibits photoluminescence. In some non-limiting examples, photoluminescence may occur at a wavelength (range) corresponding to the UV spectrum, including, without limitation, one of: the UVA spectrum, and UVB spectrum. In some non-limiting examples, photoluminescence may occur at a wavelength (range) corresponding to the visible spectrum. In some non-limiting examples, photoluminescence may occur at a wavelength (range) corresponding to one of: deep B(lue) and near UV.

[0453] In some non-limiting examples, at least one of the materials of the patterning coating 110 that may exhibit photoluminescence may comprise at least one of: a conjugated bond, an aryl moiety, a donor-acceptor group, and a heavy metal complex.

[0454] In some non-limiting examples, a coating, including without limitation, a patterning coating 110, comprised of a material, including without limitation, a patterning material 411, having substantially weak to no photoluminescence (absorption) in a wavelengthIllrange of one of at least about: 365, and 460, nm, may tend to not act as one of: a photoluminescent, and an absorbing, coating and may have applicability in some scenarios calling for substantially high transparency in at least one of: the visible spectrum, and the NIR spectrum.

[0455] In some non-limiting examples, such material may tend to exhibit substantially low photoluminescence upon being subjected to light having a wavelength of about 365 nm, which is a wavelength of the radiation source frequently used in fluorescence microscopy. The presence of such materials, including without limitation, a patterning material 411, especially when deposited, in some non-limiting examples, as a thin film, may have reduced applicability in some scenarios calling for typical optical detection techniques, including without limitation, fluorescence microscopy. This may impose constraints in some scenarios in which such material may be selectively deposited, for example through an FMM, over part(s) of a substrate 10, as there may be some scenarios for determining, following the deposition of the material, the part(s) in which such materials are present.

[0456] In some non-limiting examples, a material with substantially low to no absorption at a wavelength that is one of at least about: 365 nm, and 460 nm, may have applicability in some scenarios calling for substantially high transparency in at least one of: the visible spectrum, and the NIR spectrum.

[0457] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, in some non-limiting examples, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may not substantially attenuate light passing therethrough, in at least the visible spectrum.

[0458] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may not substantially attenuate light passing therethrough, in at least one of: the IR spectrum, and the NIR spectrum.

[0459] In this way, at least one of: the patterning coating 110, and the patterning material 411, when deposited as at least one of a: film, and coating, in a form, and under circumstances similar to the deposition of the patterning coating 110 within the device 100, may absorb light in the UVA spectrum incident upon the device 100, thereby reducing a likelihood that light in theUVA spectrum may impart constraints in terms of at least one of: device performance, device stability, device reliability, and device lifetime.

[0460] In some non-limiting examples, the patterning coating 110 may act as an optical coating.

[0461] In some non-limiting examples, the patterning coating 110 may modify at least one of: at least one property, and at least one characteristic, of light (including without limitation, in the form of photons) emitted by the device 100. In some non-limiting examples, the patterning coating 110 may exhibit a degree of haze, causing emitted light to be scattered. In some nonlimiting examples, the patterning coating 110 may comprise a crystalline material for causing light transmitted therethrough to be scattered. Such scattering of light may facilitate enhancement of the outcoupling of light from the device 100 in some non-limiting examples. In some non-limiting examples, the patterning coating 110 may initially be deposited as a substantially non-crystalline, including without limitation, substantially amorphous, coating, whereupon, after deposition thereof, the patterning coating 110 may become crystallized and thereafter serve as an optical coupling.

[0462] In some non-limiting examples, the patterning material 411 may exhibit insignificant, including without limitation, no detectable, absorption when subjected to light having a wavelength of one of at least about: 300 nm, 320 nm, 350 nm, and 365 nm.

[0463] In some non-limiting examples, the patterning coating 110 may not exhibit any substantial light absorption at any wavelength corresponding to the visible spectrum.Average Laver Thickness

[0464] In some non-limiting examples, an average layer thickness of the patterning coating 110 may be one of no more than about: 10, 8, 7, 6, and 5 nm.Weight

[0465] Without wishing to be bound by any particular theory, it may be postulated that, for compounds that are adapted to form surfaces with substantially low surface energy, there may be scenarios calling for, in at least some applications, the molar weight of such compounds to be one of between about: 800-3,000, 900-2,000, 900-1,800, and 900-1,600, g / mol.

[0466] In some non-limiting examples, the molar weight of the compound of the at least one patterning material 411 may be no more than about 6,000 g / mol. In some non-limitingexamples, the molar weight of the compound may be one of no more than about: 6,000, 5,500, 5,000, 4,500, 4,300, and 4,000, g / mol.

[0467] In some non-limiting examples, the molar weight of the compound may be one of at least about: 500, 550, 580, 650, 750, 1,000, 1,200, 1,300, 1,500, 1,700, 2,000, 2,200, and 2,500, g / mol.

[0468] In some non-limiting examples, the molar weight of the compound may be one of between about: 800-4,000, 900-2,000, 900-1,800, and 900-1,600, g / mol.

[0469] In some non-limiting examples, a percentage of the molar weight of such compound that may be attributable to the presence of F atoms, may be one of between about: 40-90, 45-85, 50- 80, 55-75, and 60-75%. In some non-limiting examples, F atoms may constitute a majority of the molar weight of such compound.Inter-Relationships Between Patterning Coating Attributes

[0470] Without wishing to be bound by any particular theory, it may be postulated that exposed layer surfaces 11 exhibiting low initial sticking probability with respect to the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg, may exhibit high transmittance. Without wishing to be bound by any particular theory, it may be postulated that exposed layer surfaces 11 exhibiting high sticking probability with respect to the deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg, may exhibit low transmittance.

[0471] In some non-limiting examples, a material, including without limitation, a patterning material 411, may tend to have a substantially high initial sticking probability against deposition of a deposited material, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg, if the material has a substantially high surface energy.

[0472] In some non-limiting examples, a patterning coating 110 having a substantially low surface energy and a substantially high melting point may have applicability in some scenarios calling for high temperature reliability. In some non-limiting examples, there may be challenges in achieving such a combination from a single material given that in some non-limiting examples, a single material having a low surface energy may tend to exhibit a low melting point.

[0473] In some non-limiting examples, a patterning material 411 that has a substantially low surface tension that is not unduly low, may have applicability in some scenarios calling for a substantially high melting point, including without limitation, between about 15-22 dynes / cm.

[0474] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a surface tension that is substantially low, but not unduly low, may have applicability in some scenarios that call for a substantially high sublimation temperature.

[0475] In some non-limiting examples, a coating, including without limitation, a patterning coating 110, comprised of a material, including without limitation, a patterning material 411, having a substantially low surface energy and a substantially high sublimation temperature may have application in some scenarios calling for substantially high precision in the control of the average layer thickness of a film comprising such material.

[0476] Without wishing to be bound by any particular theory, it may be postulated that materials that form an exposed layer surface 11 having a surface energy, in some non-limiting examples, of one of no more than about: 13, 14, and 15, dynes / cm, may have reduced applicability as a patterning material 411 in some scenarios, as such materials may exhibit at least one of substantially low adhesion to layer(s) surrounding such materials, a substantially low melting point, and a substantially low sublimation temperature.

[0477] Without wishing to be bound by any particular theory, it may be postulated that materials that form an exposed layer surface 11 having a surface energy, in some non-limiting examples, of one of no more than about: 13, 15, and 17, dynes / cm, may have reduced applicability as a patterning material 411 in some scenarios, as such materials may exhibit at least one of: substantially poor cohesion strength, a substantially low melting point, and a substantially low sublimation temperature.

[0478] Without wishing to be bound by any particular theory, it may be postulated that such compounds, including without limitation, of at least one patterning material 411, may exhibit at least one property that may have applicability in some scenarios for forming at least one of: a coating, and layer, having at least one of: a substantially high melting point, in some non-limiting examples, of at least 100°C, a substantially low surface energy, and a substantiallyamorphous structure, when deposited, in some non-limiting examples, using vacuum-based thermal evaporation processes.

[0479] In some non-limiting examples, a coating, including without limitation, a patterning coating 110, having a substantially low surface energy, a substantially high cohesion energy, and a substantially high melting point may have applicability in some scenarios that call for substantially high reliability under various conditions. In some non-limiting examples, there may be challenges in achieving such a combination from a single material, given that, in some non-limiting examples, a unitary material having a substantially low surface energy may tend to exhibit a substantially low cohesion energy and a substantially low melting point.

[0480] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low surface energy and a substantially high cohesion energy may have applicability in some scenarios that call for substantially high reliability under at least one of: sheer, and bending, stress. In some non-limiting examples, there may be challenges in achieving such a combination from a single material, given that, in some non-limiting examples, a thin film formed substantially of a single material having a substantially low surface energy may tend to exhibit a substantially low cohesion energy.

[0481] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low surface energy may tend to exhibit at least one of: a substantially large, and substantially wide, optical gap.

[0482] In general, a material with a low surface energy may exhibit at least one of: a large, and wide, optical gap which, by way of non-limiting example, may correspond to the H0M0-LUM0 gap of the material.

[0483] It has also now been found that a patterning coating 110 formed by a compound exhibiting a substantially low surface energy may also exhibit a substantially low refractive index.

[0484] In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 411, may exhibit a surface energy of no more than about 25 dynes / cm and a refractive index of no more than about 1.45. In some non-limiting examples, at least one of: the patterning coating 110, and the patterning material 711, may comprise a material exhibiting a surface energy of no more than about 20 dynes / cm and a refractive index of no more than about 1.4.

[0485] In some non-limiting examples, a material, including without limitation, a patterning material 411, having a substantially low surface energy may have applicability in some scenarios calling for substantially weak to no, at least one of photoluminescence, and absorption, in a wavelength range that is one of at least about: 365 nm and 460 nm.

[0486] In some non-limiting examples, a material, including without limitation, a patterning material 411, having at least one of a substantially large, and substantially wide optical gap (and H0M0-LUM0 gap) may tend to exhibit a substantially weak to no photoluminescence in at least one of the deep B(lue) region of the visible spectrum, the near UV spectrum, the visible spectrum, and the NIR spectrum.

[0487] Without wishing to be bound by any particular theory, it has been observed that compounds with substantially low surface energies that also have a molar weight of no more than about 1,000 g / mol, may exhibit at least one of a substantially low sublimation temperature of, without limitation, no more than about 100°C, and a substantially low melting point of, without limitation, one of no more than about: 100°C, and 80°C, such that compounds may have reduced applicability in certain scenarios.

[0488] Without wishing to be bound by any particular theory, it may be postulated that, for compounds that are adapted to form surfaces with substantially low surface energy, there may be scenarios calling for, in some non-limiting examples, the molar weight of such compounds to be one of between about: 500-6,000, 550-5,500, 580-4500, 580-4,000, 650-3,800, 750-3,500, and 1,000-3,000, g / mol.

[0489] At least some materials with at least one of: one of: a large, and wide, optical gap, and H0M0-LUM0 gap, may exhibit substantially weak to no photoluminescence in at least one of: the visible spectrum, the deep B(lue) region thereof, and the near UV spectrum. In some nonlimiting examples, a material with a substantially small H0M0-LUM0 gap may have applicability in applications to detect a film of the material using optical techniques. In some non-limiting examples, a material with higher surface energy may have applicability for applications to detect of a film of the material using optical techniques.

[0490] In some non-limiting examples, a material having a substantially large H0M0- LUMO gap may have applicability in some scenarios calling for weak to no at least one of: photoluminescence, and absorption, in a wavelength range of one of at least about: 365, and 460, nm.Doping

[0491] In some non-limiting examples, the patterning coating 110 may exhibit, including without limitation, because of at least one of: the patterning material 411 used, and the deposition environment, at least one nucleation site for the deposited material 531.

[0492] In some non-limiting examples, the patterning coating 110 may be doped, including without limitation, by at least one of: covering, and supplementing, with another material that may act as at least one of: a seed, and heterogeneity, to act as such a nucleation site for the deposited material 531. In some non-limiting examples, such other material may comprise an NPC 820 material. In some non-limiting examples, such other material may comprise an organic material, in some non-limiting examples, at least one of: a polycyclic aromatic compound, and a material comprising a non-metallic element, including without limitation, at least one of: O, S, N, and C, whose presence might otherwise be a contaminant in at least one of: the source material, equipment used for deposition, and the vacuum chamber environment. In some non-limiting examples, such other material may be deposited in a layer thickness that is a fraction of a monolayer, to avoid forming a closed coating 140 thereof.Rather, the monomers of such other material may tend to be spaced apart in the lateral aspect so as form discrete nucleation sites for the deposited material.Plurality of Materials Forming a Patterning Coating

[0493] In some non-limiting examples, forming a patterning coating 110 of a single patterning material 411 against the deposition of a deposited material 531, including without limitation, at least one of: a given metal, and a given alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg, that satisfies constraints of at least one material property selected from at least one of: initial sticking probability, transmittance, deposition contrast, surface energy, glass transition temperature, melting point, sublimation temperature, evaporation temperature, cohesion energy, optical gap, photoluminescence, refractive index, extinction coefficient, absorption, other optical effect, average layer thickness, molar weight, and composition, for a given scenario, may impose challenges, given the substantially complex inter-relationships between the various material properties.

[0494] In some non-limiting examples, the patterning coating 110 may comprise a plurality of materials. In some non-limiting examples, the patterning coating 110 may comprise a first material and a second material. In some non-limiting examples, the patterning coating 110 may comprise additional materials, including without limitation, at least one of: a third material, and a fourth material.

[0495] In some non-limiting examples, at least one of the plurality of materials of the patterning coating 110 may serve as an NIC when deposited as a thin film.

[0496] In some non-limiting examples, at least one of the plurality of patterning materials 411 may serve as an NIC when deposited as a thin film. In some non-limiting examples, at least one of the patterning materials 411 may not serve as an NIC. In some non-limiting examples, such at least one of the patterning materials 411 that do not serve as an NIC may form an NPC 820 when deposited as a thin film. In some non-limiting examples, the presence of the first material in the patterning coating 110 may result in an increased initial sticking probability thereof compared to cases in which the patterning coating 110 is formed of the second material and is substantially devoid of the first material.

[0497] In some non-limiting examples, at least one of the: first, and second, material, may comprise a molecule that comprises at least one of: a cage structure, a cyclic structure, and an organic-inorganic hybrid structure.

[0498] In some non-limiting examples, the host may comprise a fully condensed oligomer. In some non-limiting examples, the molecular structure of the host may be substantially devoid of any partially condensed, including without limitation, uncondensed, moieties.

[0499] In some non-limiting examples, the first material may form an NPC 820 when deposited as a thin film, and the second material may form an NIC when deposited as a thin film.

[0500] In some non-limiting examples, employing a plurality of patterning materials 411 that each satisfy a different combination of constraints of the at least one material property, may have applicability in some scenarios to achieve a combination of characteristics of the patterning coating 110, including without limitation, at least one of: high patterning contrast, low propensity to crystallize in a thin film form,low risk of cohesion failure and / or delamination in a thin film form,• the patterning coating 110 exhibiting a photoluminescent response, and• formation of at least one particle structure 150 on an exposed layer surface 11 of the patterning coating 110.

[0501] In some non-limiting examples, at least one of the materials of the patterning coating 110 may be adapted to form a surface having a low surface energy when deposited as a thin film. In some non-limiting examples, the first material, when deposited as a thin film, may be adapted to form a surface having a lower surface energy than a surface provided by a thin film comprising the second material.

[0502] In some non-limiting examples, the patterning coating 110 may exhibit photoluminescence, including without limitation, by comprising a material which exhibits photoluminescence.

[0503] In some non-limiting examples, the first material may exhibit photoluminescence at a wavelength corresponding to the visible spectrum, and the second material may not exhibit substantial photoluminescence at any wavelength corresponding to the visible spectrum.

[0504] In some non-limiting examples, the second material may not substantially exhibit photoluminescence at any wavelength corresponding to the visible spectrum. In some nonlimiting examples, the second material may not exhibit photoluminescence upon being subjected to light having a wavelength of one of at least about: 300, 320, 350, and 365 nm. In some nonlimiting examples, the second material may exhibit insignificant to no detectable absorption when subjected to such light.

[0505] In some non-limiting examples, the second optical gap of the second material may be wider than the photon energy of the light emitted by the source, such that the second material does not undergo photoexcitation when subjected to such light. However, in some non-limiting examples, the patterning coating 110 comprising such second material may nevertheless exhibit photoluminescence upon being subjected to light due to the first material exhibiting photoluminescence. In some non-limiting examples, the presence of the patterning coating 110 may be detected using routine characterization techniques such as fluorescence microscopy upon deposition of the patterning coating 110.

[0506] In some non-limiting examples, the first material may have a first optical gap, and the second material may have a second optical gap. In some non-limiting examples, the second optical gap may exceed the first optical gap. In some non-limiting examples, a difference between the first optical gap and the second optical gap may exceed one of about: 0.3, 0.5, 0.7, 1, 1.3, 1.5, 1.7, 2, 2.5, and 3, eV.

[0507] In some non-limiting examples, the first optical gap may be one of no more than about: 4.1, 3.5, and 3.4, eV. In some non-limiting examples, the second optical gap may exceed one of about: 3.4, 3.5, 4.1, 5, and 6.2, eV.

[0508] In some non-limiting examples, at least one of: the first optical gap, and the second optical gap, may correspond to the H0M0-LUM0 gap.

[0509] In some non-limiting examples, an optical gap of at least one of: the various coatings, and materials, including without limitation, at least one of: the first optical gap, and the second optical gap, may correspond to an energy gap of at least one of: the coating, and the material, from which light is at least one of: absorbed, and emitted, during the photoexcitation process.

[0510] In some non-limiting examples, a concentration, including without limitation by weight, of the first material in the patterning coating 110 may be no more than that of the second material in the patterning coating 110. In some non-limiting examples, the patterning coating 110 may comprise one of at least about: 0.1, 0.2, 0.5, 0.8, 1, 3, 5, 8, 10, 15, and 20, wt.%, of the first material. In some non-limiting examples, the patterning coating 110 may comprise one of no more than about: 50, 40, 30, 25, 20, 15, 10, 8, 5, 3, and 1, wt.%, of the first material. In some non-limiting examples, a remainder of the patterning coating 110 may be comprised substantially of the second material.

[0511] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: F, and Si. In some non-limiting examples, at least one of the: first, and second, material, may comprise at least one of: F, and Si. In some non-limiting examples, the first material may comprise at least one of: F, and Si, and the second material may comprise at least one of: F, and Si. In some non-limiting examples, the first material and the second material both may comprise F. In some non-limiting examples, the first material and the second materialboth may comprise Si. In some non-limiting examples, each of the first material and the second material may comprise at least one: F, and Si.

[0512] In some non-limiting examples, at least one material of the first material and the second material may comprise both F and Si. In some non-limiting examples, one of the first material and the second material may not comprise at least one of: F, and Si. In some nonlimiting examples, the second material may comprise at least one of: F, and Si, and the first material may not comprise at least one of: F, and Si.

[0513] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise a compound that comprises F. In some non-limiting examples, at least one of the: first, and second, material, may comprise a compound that comprises F and C. In some non-limiting examples, at least one of the: first, and second, material, may comprise a compound that comprises F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 0.5, 0.7, 1, 1.5, 2, and 2.5.

[0514] In some non-limiting examples, an atomic ratio of F to C may be determined by counting the F atoms present in the compound structure, and for C atoms, only counting the sp3hybridized C atoms present in the compound structure. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise a compound that comprises, as part of its molecular sub-structure, a moiety comprising F and C in an atomic ratio corresponding to a quotient of F / C of one of at least about: 1, 1.5, and 2.

[0515] In some non-limiting examples, at least one of the materials of the patterning coating 110, which in some non-limiting examples, may be at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 110 may comprise an sp2C atom. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 110 may comprise an sp3C atom. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and an sp3C atom, and at least one of the other materials of the patterning coating 110 may comprise an sp2C atom. In some non-limiting examples, at least oneof the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and an sp3C atom, wherein all F bonded to a C atom may be bonded to an sp3C atom, and at least one of the other materials of the patterning coating 110 may comprise an sp2C atom. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and an sp3C atom wherein all F bonded to a C atom may be bonded to an sp3C atom, and at least one of the other materials of the patterning coating 110 may comprise an sp2C atom and may not comprise F. In some non-limiting examples, in any of the foregoing non-limiting examples, “at least one of the materials of the patterning coating 110” may correspond to the second material, and the “at least one of the other materials of the patterning coating 110” may correspond to the first material.

[0516] Those having ordinary skill in the relevant art will appreciate that the presence of materials in a coating which comprises at least one of: F, an sp2C atom, an sp3C atom, an aromatic hydrocarbon moiety, other functional groups, and other moieties, may be detected using various methods known in the art, including by way of non-limiting example, X-ray Photoelectron Spectroscopy (XPS).

[0517] In some non-limiting examples, at least one of the materials of the patterning coating 110, which by way of non-limiting example may be at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 110 may comprise an aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the materials of the patterning coating 110 may not comprise an aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise an aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 110 may comprise an aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise an aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 110 may comprise an aromatic hydrocarbon moiety and may not comprise F. In some non-limiting examples, the aromatic hydrocarbon moiety may comprise at least one of: a substituted polycyclic aromatic hydrocarbon moiety, anunsubstituted polycyclic aromatic hydrocarbon moiety, a substituted phenyl moiety, and an unsubstituted phenyl moiety.

[0518] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 110 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the materials of the patterning coating 110 may be devoid of a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and may be devoid of a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 110 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and may be devoid of a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 110 may comprise a polycyclic aromatic hydrocarbon moiety and may be devoid of F.

[0519] Without wishing to be bound by any particular theory, it may be postulated that, in some non-limiting examples, the presence of a high surface tension moiety in a compound, including without limitation, a moiety comprising at least one sp2C atom, including without limitation, a polycyclic aromatic hydrocarbon moiety, may decrease an ability of a patterning coating 110 comprising such a compound to function as an NIC against deposition of a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg. In some non-limiting examples, the patterning coating 110 comprising such a compound may have a substantially high initial sticking probability, due to the presence of the high surface tension moiety.

[0520] In some non-limiting examples, it may be postulated that the presence of a high surface tension moiety in a compound, including without limitation, a moiety comprising at least one sp2C atom, including without limitation, a polycyclic aromatic hydrocarbon moiety, may increase the reliability of a patterning coating 110 comprising such compound by, includingwithout limitation, increasing at least one of the: cohesion energy, and stability, of the patterning coating 110.

[0521] Without wishing to be bound by any particular theory, it may be postulated that, in some non-limiting examples, the presence of a low surface tension moiety in a compound, including without limitation, a moiety comprising at least one F atom, including without limitation, a fluoroalkyl moiety, may increase an ability of a patterning coating 110 comprising such a compound to function as an NIC against deposition of a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg. In some nonlimiting examples, the patterning coating 110 comprising such a compound may have a substantially low initial sticking probability, due to the presence of the low surface tension moiety.

[0522] In some non-limiting examples, it may be postulated that the presence of a low surface tension moiety in a compound, including without limitation, a moiety comprising at least one F atom, including without limitation, a fluoroalkyl moiety, may decrease the reliability of a patterning coating 110 comprising such compound by, including without limitation, decreasing the cohesion energy of the patterning coating 110.

[0523] In some non-limiting examples, a mixed ligand compound comprising: a high surface tension moiety, and a low surface tension moiety, may have applicability in some scenarios. In some non-limiting examples, such mixed ligand compound may have applicability in providing a substantially homogeneous patterning coating 110. Without wishing to be bound by any particular theory, it may be postulated that a patterning coating 110 comprising a compound having a high surface tension moiety and a low surface tension moiety, including without limitation, the mixed ligand compound, may exhibit an: increased reliability, and ability to inhibit the deposition of a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag- containing material, including without limitation, MgAg.

[0524] In some non-limiting examples, a composition comprising a plurality of compounds, including without limitation, at least one compound comprising a high surface tension moiety, and at least one compound comprising a low surface tension moiety, may have applicability in some scenarios. Without wishing to be bound by any particular theory, it may bepostulated that a patterning coating 110 comprising such a composition may exhibit an: increased reliability, and ability to inhibit the deposition of a deposited material 531, including without limitation, at least one of: a metal, and an alloy, including without limitation, at least one of: Yb, Ag, Mg, and a Ag-containing material, including without limitation, MgAg.

[0525] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise an organic-inorganic hybrid material.

[0526] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise an oligomer.

[0527] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise a compound having a molecular structure comprising a backbone and at least one functional group bonded to the backbone. In some non-limiting examples, the backbone may be an inorganic moiety, and the at least one functional group may be an organic moiety.

[0528] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may have a molecular structure comprising a siloxane group. In some non-limiting examples, the siloxane group may be one of: a linear siloxane group, a branched siloxane group, and a cyclic siloxane group. In some non-limiting examples, the backbone may comprise a siloxane group. In some non-limiting examples, the backbone may comprise a siloxane group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group. In some non-limiting examples, such compound may comprise fluoro-siloxanes.

[0529] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety and a siloxane moiety, and at least one of the other materials of the patterning coating 110 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety, and a siloxane moiety, and at least one of the materials of thepatterning coating 110 may not comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety, and a siloxane moiety, and may not comprise a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 110 may comprise a polycyclic aromatic hydrocarbon moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety, and a siloxane moiety, and may not comprise a polycyclic aromatic hydrocarbon moiety, and at least one of the other materials of the patterning coating 110 may comprise a polycyclic aromatic hydrocarbon moiety and may not comprise at least one of: a fluorocarbon moiety, and a siloxane moiety.

[0530] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may have a molecular structure comprising a silsesqui oxane group. In some non-limiting examples, the silsesquioxane group may be a polyoctahedral silsesquioxane (POSS). In some non-limiting examples, the backbone may comprise a silsesquioxane group. In some non-limiting examples, the backbone may comprise a silsesquioxane group and at least one functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group.

[0531] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may have a molecular structure comprising at least one of: a substituted aryl group, an unsubstituted aryl group, a substituted heteroaryl group, and an unsubstituted heteroaryl group. In some nonlimiting examples, the aryl group may be at least one of: phenyl, and naphthyl. In some nonlimiting examples, at least one C atom of an aryl group may be substituted by a heteroatom, which by way of non-limiting example may be at least one of: O, N, and S, to derive a heteroaryl group. In some non-limiting examples, the backbone may comprise at least one of: a substituted aryl group, an unsubstituted aryl group, a substituted heteroaryl group, and an unsubstituted heteroaryl group. In some non-limiting examples, the molecular structure of the compound may include: (i) the backbone comprising at least one of: a substituted aryl group, an unsubstituted aryl group, a substituted heteroaryl group, and an unsubstituted heteroaryl group; and (ii) at leastone functional group comprising F. In some non-limiting examples, the at least one functional group comprising F may be a fluoroalkyl group.

[0532] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the other materials of the patterning coating 110 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F, and at least one of the materials of the patterning coating 110 may not comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 110 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise F and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 110 may comprise a phenyl moiety and may not comprise F.

[0533] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety and a siloxane moiety, and at least one of the other materials of the patterning coating 110 may comprise a phenyl moiety. In some nonlimiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety, and a siloxane moiety, and at least one of the materials of the patterning coating 110 may not comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety, and a siloxane moiety and may not comprise a phenyl moiety, and at least one of the other materials of the patterning coating 110 may comprise a phenyl moiety. In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may comprise at least one of: a fluorocarbon moiety, and a siloxane moiety and may not comprise a phenyl moiety, and at least one of the other materials of the patterningcoating 110 may comprise a phenyl moiety and may not comprise either of: a fluorocarbon moiety, and a siloxane moiety.

[0534] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may have a molecular structure comprising at least one of: a substituted hydrocarbon group, and an unsubstituted hydrocarbon group. In some non-limiting examples, the compound may have a molecular structure comprising at least one of: a linear hydrocarbon group, a branched hydrocarbon group, and a cyclic hydrocarbon group. In some non-limiting examples, at least one C atom of the hydrocarbon group may be substituted by a heteroatom, including without limitation, at least one of: O, N, and S.

[0535] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may be a fluoropolymer. In some non-limiting examples, the compound may be a block copolymer comprising F. In some non-limiting examples, the compound may be an oligomer. In some nonlimiting examples, the oligomer may be a fluorooligomer. In some non-limiting examples, the compound may be a block oligomer comprising F.

[0536] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may be a metal complex. In some non-limiting examples, the metal complex may be an organo-metal complex. In some non-limiting examples, the organo-metal complex may comprise F. In some non-limiting examples, the organo-metal complex may comprise at least one ligand comprising F. In some non-limiting examples, the at least one ligand comprising F may comprise a fluoroalkyl group.

[0537] In general, at least one of: the molecular structures, and molecular compositions, of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may be different. In some non-limiting examples, the materials may be selected such that they possess at least one property which is one of: substantially similar to, and substantially different from, one another, including without limitation, at least one of: at least one of: a molecular structure of a monomer, a monomer backbone, and a functional group; a presence of a element in common; a similarity in molecular structure; a characteristic surface energy; a refractive index; a molar weight; and a thermal property, including without limitation,at least one of: a melting temperature, a sublimation temperature, a glass transition temperature, and a thermal decomposition temperature.

[0538] In some non-limiting examples, at least one of the: first, and second, material, of the patterning coating 110 may be an oligomer.

[0539] In some non-limiting examples, the first material may comprise a first oligomer, and the second material may comprise a second oligomer. Each of the first oligomer and the second oligomer may comprise a plurality of monomers.

[0540] In some non-limiting examples, the monomer may comprise at least one of a: CF2, and CF2H, moiety. In some non-limiting examples, the monomer may comprise at least one of a: CF2, and CF3, moiety. In some non-limiting examples, the monomer may comprise a CH2CF3 moiety. In some non-limiting examples, the monomer may comprise at least one of: C, and O. In some non-limiting examples, the monomer may comprise a fluorocarbon monomer. In some non-limiting examples, the monomer may comprise at least one of a: vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, hexafluoropropylene, and fluorinated 1,3- di oxole, moiety.

[0541] In some non-limiting examples, the monomer may comprise a monomer backbone and a functional group. In some non-limiting examples, the functional group may be bonded, one of: directly, and via a linkage group, to the monomer backbone. In some non-limiting examples, the monomer may comprise the linkage group, and the linkage group may be bonded to the monomer backbone and to the functional group. In some non-limiting examples, the monomer may comprise a plurality of functional groups, which may be one of: the same, and different, from one another. In such examples, each functional group may be bonded, one of: directly, and via a linkage group, to the monomer backbone. In some non-limiting examples, where a plurality of functional groups is present, a plurality of linkage groups may also be present.

[0542] In some non-limiting examples, the molecular structure of the second material, may comprise a plurality of different monomers. In some non-limiting examples, such molecular structure may comprise monomer species that have different at least one of: molecular composition, and molecular structure.

[0543] While some non-limiting examples have been described herein with reference to a first material and a second material, it will be appreciated that the patterning coating may further include at least one additional material, including, without limitation, at least one of a: third, and fourth, material, and descriptions regarding at least one of: the molecular structures, and properties, of at least one of: the first material, the second material, the first oligomer, and the second oligomer, may be applicable with respect to additional materials which may be contained in the patterning coating 110.

[0544] In some non-limiting examples, a difference in the sublimation temperature of the plurality of materials of the patterning coating 110, including, without limitation, a difference between the first material and the second material, may be one of no more than about: 5, 10, 15, 20, 30, 40, and 50°C.

[0545] In some non-limiting examples, a difference in a melting temperature of the plurality of materials of the patterning coating 110, including, without limitation, a difference between the first material and the second material, may be one of no more than about: 5, 10, 15, 20, 30, 40, and 50°C.

[0546] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may have a low characteristic surface energy.

[0547] In some non-limiting examples, at least one of the materials of the patterning coating 110, including without limitation, at least one of the first material and the second material, may have a low characteristic surface energy of no more than about 20 dynes / cm.

[0548] In some non-limiting examples, the surface energy of each of the at least two materials of the patterning coating 110, including, without limitation, those of the first material and the second material, is one of no more about: 25, 21, 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, and 10, dynes / cm.

[0549] In some non-limiting examples, a refractive index at a wavelength at least one of: 500, and 460, nm, of at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may be one of no more than about: 1.5, 1.45, 1.44, 1.43, 1.42, and 1.41.

[0550] In some non-limiting examples, a molar weight of at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may be one of at least about: 750, 1,000, 1,250, 1,500, 1,750, and 2,000, g / mol.

[0551] In some non-limiting examples, a molar weight of at least one of the materials of the patterning coating 110, including without limitation, at least one of the: first, and second, material, may be one of no more than about: 10,000, 8,000, 7,000, and 5,000, g / mol.

[0552] In some non-limiting examples, the patterning coating 110 may comprise a plurality of materials exhibiting similar thermal properties. In some non-limiting examples, the patterning coating 110 may comprise a plurality of materials with similar thermal properties, including without limitation, at least one of a: melting, and sublimation, temperature.

[0553] In some non-limiting examples, a method for manufacturing a layered semiconductor device 100, including without limitation, an opto-electronic device 200 may comprise actions of: depositing a patterning coating on a first exposed layer surface 11 of the device 100 in a first portion 101 of a lateral aspect thereof; and depositing a deposited material 531 on a second exposed layer surface 11 of the device 100 in a second portion 102 of the lateral aspect thereof. An initial sticking probability against deposition of the deposited material 531 onto an exposed layer surface 11 of the patterning coating 110 in the first portion 101, may be substantially no more than the initial sticking probability against deposition of the deposited material 531 onto an exposed layer surface 11 in the second portion 102, such that the exposed layer surface 11 of the patterning coating 110 in the first portion 101 may be substantially devoid of a closed coating 140 of the deposited material 531. In some non-limiting examples, the patterning coating 110 deposited on the first exposed layer surface 11 of the device 100 may comprise a first material and a second material.

[0554] In some non-limiting examples, depositing the patterning coating 110 on the first exposed layer surface 11 of the device 100 may comprise providing a mixture comprising a plurality of materials, and causing the mixture to be deposited onto the first exposed layer surface 11 of the device 100 to form the patterning coating 110 thereon. In some non-limiting examples, the mixture may comprise the first material and the second material. In some non-limiting examples, the first material and the second material may both be deposited onto the first exposed layer surface 11 to form the patterning coating 110 thereon.

[0555] In some non-limiting examples, the mixture comprising the plurality of materials may be deposited onto the first exposed layer surface 11 of the device 100 by a PVD process, including without limitation, thermal evaporation. In some non-limiting examples, the patterning coating 110 may be formed by evaporating the mixture from a single evaporation source and causing the mixture to be deposited on the first exposed layer surface 11 of the device 100. In some non-limiting examples, the mixture comprising, by way of non-limiting example, the first material and the second material, may be placed in a single evaporation source (crucible) to be heated under vacuum. Once the evaporation temperature of the materials is reached, a vapor flux generated therefrom may be directed towards the first exposed layer surface 11 of the device 100 to cause the deposition of the patterning coating 110 thereon.

[0556] Without wishing to be bound by any particular theory, it may be postulated that a composition comprising a plurality of materials, including without limitation, a first material and a second material, with at least one of a substantially similar: sublimation temperature, and molar weight, may have applicability in some scenarios calling for the formation of a substantially homogenous patterning coating 110, even over a prolonged deposition period, during which the patterning coating 110 may be deposited from a crucible containing such composition.

[0557] For the purpose of the present disclosure, the terms “composition” and “mixture” may be interchangeably used to refer to the same concept.

[0558] In some non-limiting examples, the patterning coating 110 may be deposited by co-evaporation of the first material and the second material. In some non-limiting examples, the first material may be evaporated from a first evaporation source, and the second material may be concurrently evaporated from a second evaporation source such that the mixture may be formed in the vapor phase and may be co-deposited onto the first exposed layer surface 11 to provide the patterning coating 110 thereon.Display Panel and User Device

[0559] Turning now to FIG. 3, there is shown a cross-sectional view of an example layered opto-electronic device 200, such as a display panel 300. In some non-limiting examples, the display panel 300 may comprise a plurality of layers deposited on a substrate 10, culminating with an outermost layer that forms a face 301 thereof. In some non-limiting examples, the display panel 300 may be a version of the device 200.

[0560] The face 301 of the display panel 300 may extend across a lateral aspect thereof, substantially along a plane defined by the lateral axes.

[0561] In some non-limiting examples, the face 301, and indeed, the entire display panel 300, may act as a face of a user device 310 through which at least one EM signal 331 may be exchanged therethrough at a non-zero angle relative to the plane of the face 301. In some nonlimiting examples, the user device 310 may be a computing device 310, such as, without limitation, a smartphone, a tablet, a laptop, an e-reader, and some other electronic device 310, such as a monitor, a television set, and a smart device 310, including without limitation, an automotive display, windshield, a household appliance, and a medical, commercial, and industrial device 310.

[0562] In some non-limiting examples, the face 301 may correspond to, and in some nonlimiting examples, mate with, at least one of: a body 320, and an opening 321 therewithin, within which at least one under-display component 330 may be housed.

[0563] In some non-limiting examples, the at least one under-display component 330 may be formed, including without limitation, at least one of: integrally, and as an assembled module, with the display panel 300 on a surface thereof opposite to the face 301.

[0564] In some non-limiting examples, at least one aperture 322 may be formed in the display panel 300 to allow for the exchange of at least one EM signal 331 through the face 301 of the display panel 300, at a non-zero angle to the plane defined by the lateral axes, including without limitation, concomitantly, the layers of the display panel 300, including without limitation, the face 301 of the display panel 300.

[0565] In some non-limiting examples, the at least one aperture 322 may be understood to comprise one of: the absence, and reduction in at least one of: thickness, and capacity, of a substantially opaque coating otherwise disposed across the display panel 300. In some nonlimiting examples, the at least one aperture 322 may be embodied as a signal-transmissive region 212 as described herein.

[0566] However the at least one aperture 322 is embodied, the at least one EM signal 331 may pass therethrough such that it passes through the face 301. As a result, the at least one EM signal 331 may be considered to exclude any light that may extend along the plane defined by thelateral axes, including without limitation, any electric current that may be conducted across at least one particle structure 150 laterally across the display panel 300.

[0567] Further, those having ordinary skill in the relevant art will appreciate that the at least one EM signal 331 may be differentiated from light per se, including without limitation, one of: electric current, and an electric field generated thereby, in that the at least one EM signal 331 may convey, either one of: alone, and in conjunction with other EM signals 331, some information content, including without limitation, an identifier by which the at least one EM signal 331 may be distinguished from other EM signals 331. In some non-limiting examples, the information content may be conveyed by at least one of: specifying, altering, and modulating, at least one of: the wavelength, frequency, phase, timing, bandwidth, intensity, time of flight, resistance, capacitance, impedance, conductance, and other characteristic of the at least one EM signal 331.

[0568] In some non-limiting examples, the at least one EM signal 331 passing through the at least one aperture 322 of the display panel 300 may comprise at least one photon and, in some non-limiting examples, may have a wavelength spectrum that lies, without limitation, within at least one of: the visible spectrum, the IR spectrum, and the NIR spectrum. In some non-limiting examples, the at least one EM signal 331 passing through the at least one aperture 322 of the display panel 300 may have a wavelength that lies, without limitation, within at least one of: the IR, and NIR spectrum.

[0569] In some non-limiting examples, the at least one EM signal 331 passing through the at least one aperture 322 of the display panel 300 may comprise ambient light incident thereon.

[0570] In some non-limiting examples, the at least one EM signal 331 exchanged through the at least one aperture 322 of the display panel 300 may be at least one of: transmitted, and received, by the at least one under-display component 330.

[0571] In some non-limiting examples, the at least one under-display component 330 may have a size that is at least a single signal-transmissive region 212, but may underlie not only a plurality thereof, but also at least one emissive region 210 extending therebetween. Similarly, in some non-limiting examples, the at least one under-display component 330 may have a size that is at least a single one of the apertures 322.

[0572] In some non-limiting examples, the at least one under-display component 330 may comprise a receiver 330r, adapted to receive and process at least one received EM signal 33 lr, passing through the at least one aperture 322 from beyond the user device 310. Non-limiting examples of such receiver 330r include an under-display camera (UDC), and a sensor, including without limitation, IR sensor / detector, an NIR sensor / detector, a LIDAR sensing module, a fingerprint sensing module, an optical sensing module, an IR (proximity) sensing module, an iris recognition sensing module, and a facial recognition sensing module, including without limitation, a part thereof.

[0573] In some non-limiting examples, the at least one under-display component 330 may comprise a transmitter 330t adapted to emit at least one transmitted EM signal 33 It passing through the at least one aperture 322 beyond the user device 310. Non-limiting examples, of such transmitter 330t include a source of light, including without limitation, a built-in flash, a flashlight, an IR emitter, a NIR emitter, a LIDAR sensing module, a fingerprint sensing module, an optical sensing module, an IR (proximity sensing module, an iris recognition sensing module, and a facial recognition sensing module, including without limitation, a part thereof.

[0574] In some non-limiting examples, the at least one received EM signal 33 lr may include at least a fragment of the at least one transmitted EM signal 33 It which is one of: reflected off, and otherwise returned by, an external surface to the user device 310, including without limitation, a user 30.

[0575] In some non-limiting examples, the at least one EM signal 331 passing through the at least one aperture 322 of the display panel 300 beyond the user device 310, including without limitation, those transmitted EM signals 33 It emitted by the at least one under-display component 330 that may comprise a transmitter 330t, may emanate from the display panel 300, and pass back as received EM signals 33 lr through the at least aperture 322 of the display panel 300 to at least one under-display component 330 that may comprise a receiver 330r.

[0576] In some non-limiting examples, the under-display component 330 may comprise an IR emitter and an IR sensor. In some non-limiting examples, such under-display component 330 may comprise, as one of: a part, component, and module, thereof: at least one of: a dotmatrix projector, a time-of-flight (ToF) sensor module, which may operate as one of: a direct ToF, and an indirect ToF, sensor, a vertical cavity surface-emitting laser (VCSEL), flood illuminator, NIR imager, folded optics, and a diffractive grating.

[0577] In some non-limiting examples, there may be a plurality of under-display components 330 within the user device 310, a first one of which may comprise a transmitter 330t for emitting at least one transmitted EM signal 33 It to pass through the at least one aperture 322, beyond the user device 310, and a second one of which may comprise a receiver 330r, for receiving at least one received EM signal 33 lr. In some non-limiting examples, such transmitter 330t and receiver 330r may be embodied in a single under-display component 330.

[0578] In some non-limiting examples, the display panel 300 may comprise at least one signal-exchanging part 303 and at least one display part 307.

[0579] In some non-limiting examples, the at least one display part 307 may comprise a plurality of emissive regions 210, in some non-limiting examples, laid out in a lateral pattern. In some non-limiting examples, the emissive regions 210 in the at least one display part 307 may correspond to (sub-) pixels 1115 / 216 of the display panel 300.

[0580] In some non-limiting examples, the at least one signal-exchanging part 303 may comprise at least one emissive region 210 and at least one signal-transmissive region 212. In some non-limiting examples, the at least one emissive region 210 in the at least one signalexchanging part 303 may correspond to (sub-) pixel(s) 1115 / 216 of the display panel 300, and in some non-limiting examples, may be substantially laid out in a similar, including without limitation, identical, lateral pattern as in the at least one display part 307.

[0581] In some non-limiting examples, the at least one display part 307 may be adjacent to, and in some non-limiting examples, separated by, at least one signal-exchanging part 303.

[0582] In some non-limiting examples, the at least one signal-exchanging part 303 may be positioned proximate to an extremity of the display panel 300, including without limitation, at least one of: an edge, and a corner, thereof. In some non-limiting examples, the at least one signal-exchanging part 303 may be positioned substantially centrally within the lateral aspect of the display panel 300.

[0583] In some non-limiting examples, the at least one display part 307 may substantially surround, including without limitation, in conjunction with at least one other display part 307, the at least one signal-exchanging part 303.

[0584] In some non-limiting examples, the at least one signal-exchanging part 303 may be positioned proximate to an extremity and configured such that the at least one display part(s) 307 do(es) not completely surround the at least one signal-exchanging part 303.

[0585] In some non-limiting examples, a pixel density of the at least one emissive region 210 of the at least one signal-exchanging part 303 may be substantially the same as a pixel density of the at least one emissive region 210 of the at least one display part 307 proximate thereto, at least in an area thereof that is substantially proximate to the at least one signalexchanging part 303. In some non-limiting examples, the pixel density of the display panel 300 may be substantially uniform thereacross. In at least some applications, there may be scenarios calling for the at least one signal-exchanging part 303 and the at least one display part 307 to have substantially the same pixel density, including without limitation, so that a resolution of the display panel 300 may be substantially the same across both the at least one signal-exchanging part 303 and the at least one display part 307 thereof.

[0586] Those having ordinary skill in the relevant art will appreciate that there may be scenarios calling for the layout of (sub-) pixels 1115 / 216 in the signal-exchanging part 303 of the display panel 300 to resemble, to some extent, the layout thereof in the display part 307 of the display panel 300, including without limitation, a size, shape, (colour) order, and configuration of (sub-) pixels 1115 / 216, and wherein a spacing between adjacent (sub-) pixels 1115 / 216 (“pitch”) in the signal-exchanging part 303 is one of the same, and an integer multiple thereof, of a pitch thereof in the display part 307.

[0587] Having said this, examples in the present disclosure may have applicability in scenarios in which the layout of (sub-) pixels 1115 / 216 in the signal-exchanging part 303 may be substantially different than the layout thereof in the display part 307 of the display panel 300.

[0588] In some non-limiting examples, a pixel density of the signal-exchanging part 303 of the display panel 300 may be no more than a pixel density of the display part 307 of the display panel 300.

[0589] In some non-limiting examples, at least one of a: size, shape, configuration, and pitch, of the (sub-) pixels 1115 / 216 in the signal-exchanging part 303 of the display panel 300 may be substantially identical to that of the (sub-) pixels 1115 / 216 in the display part 307 of the display panel 300, however a number of such (sub-) pixels 1115 / 216 may be reduced in the signal-exchanging part 303 of the display panel 300. In such scenarios, in some non-limitingexamples, a common FMM may be used for patterning at least the (sub-) pixels 1115 / 216 in both the signal-exchanging part 303 and the display part 307, with an attendant reduction of manufacturing cost and complexity. In such scenarios, in some non-limiting examples, those apertures in the FMM corresponding to those (sub-) pixel(s) 1115 / 216 that are not present (omitted) in the signal-exchanging part 303 may be covered (blocked) when in use with the signal-exchanging part 303, so as to substantially preclude the formation of such at least one (sub-) pixel(s) 1115 / 216.

[0590] In some non-limiting examples, at least one signal-transmissive region 212 may be formed in region(s) where the formation of such at least one (sub-) pixel(s) 1115 / 216 have been substantially precluded in the signal-exchanging part 303.

[0591] In some non-limiting examples, the display panel 300 may further comprise at least one transition region (not shown) between the at least one signal-exchanging part 303 and the at least one display part 307, wherein the configuration of at least one of: the emissive regions 210, and the signal-transmissive regions 212 therein, may differ from those of at least one of: the at least one signal-exchanging part 303, and the at least one display part 307. In some nonlimiting examples, such transition region may be omitted such that the emissive regions 210 may be provided in a substantially continuous repeating pattern across both the at least one signalexchanging part 303 and the at least one display part 307.

[0592] In some non-limiting examples, the at least one signal-exchanging part 303 may have a polygonal contour, including without limitation, at least one of a substantially square, and rectangular, configuration.

[0593] In some non-limiting examples, the at least one signal-exchanging part 303 may have a curved contour, including without limitation, at least one of a substantially circular, oval, and elliptical, configuration.

[0594] In some non-limiting examples, the signal-transmissive regions 212 in the at least one signal-exchanging part 303 may be configured to allow EM signals having a wavelength (range) corresponding to the IR spectrum to pass through the entirety of a cross-sectional aspect thereof.

[0595] In some non-limiting examples, the at least one signal-exchanging part 303 may have a reduced number of, including without limitation, be substantially devoid of, backplanecomponents, including without limitation, TFT structures 206, including without limitation, metal trace lines, capacitors, and other light-absorbing element, including without limitation, opaque elements, the presence of which may otherwise interfere with the capture of the EM signals by the at least one under-display component 330, including without limitation, the capture of an image by a camera.

[0596] In some non-limiting examples, the user device 310 may house at least one transmitter 330t for transmitting at least one transmitted EM signal 33 It through at least one first signal-transmissive region 212 in, and in some non-limiting examples, substantially corresponding to, a first signal-exchanging part 303, beyond the face 301. In some non-limiting examples, the user device 310 may house at least one receiver 33 Or for receiving at least one received EM signal 33 lr through at least one second signal-transmissive region 212 in, and in some non-limiting examples, substantially corresponding to, a second signal-exchanging part 303, from beyond the face 301. In some non-limiting examples, the at least one received EM signal 33 lr may be the same as the at least one transmitted EM signal 33 It, reflected off an external surface, including without limitation, a user 30, including without limitation, for biometric authentication thereof.

[0597] In some non-limiting examples, at least one of: the at least one transmitter 330t, and the at least one receiver 330t, may be arranged behind the corresponding at least one signalexchanging part 303, such that EM signals, including without limitation, IR signals may be at least one of: emitted, and received, respectively, by passing through the at least one signalexchanging part 303 of the display panel 300. In some non-limiting examples, the at least one transmitter 330t and the at least one receiver 33 Or may both be arranged behind a single signalexchanging part 303, which in some non-limiting examples, may be elongated along at least one configuration axis, such that it extends across both the at least one transmitter 330t and the at least one receiver 33 Or.

[0598] In some non-limiting examples, the display panel 300 may further comprise a non-display part (not shown), which in some non-limiting examples, may be substantially devoid of any emissive regions 210. In some non-limiting examples, the user device 310 may house at least one of: an under-display component 330, including without limitation, a camera, and a non under-display component, including without limitation, a punch-hole camera, which in somenon-limiting examples, may be provided in at least one of: a cut-out in the panel 300, and a bezel thereof, arranged within the non-display part.

[0599] In some non-limiting examples, the non-display part may be arranged adjacent to, and in some non-limiting examples, between a plurality of signal-exchanging parts 303 corresponding to a plurality of under-display components 330, including without limitation, a transmitter 330t and a receiver 33 Or.

[0600] In some non-limiting examples, the non-display part may comprise a through-hole part (not shown), which in some non-limiting examples, may be arranged to overlap at least one of: the under-display, and the non under-display, component. In some non-limiting examples, the display panel 300 may, in the through-hole part, be substantially devoid of any of at least one of: a layer, coating, and component, that may otherwise be present in at least one of: the at least one signal-exchanging part 303, and the at least one display part 307, including without limitation, a component of at least one of: the backplane 202, and the frontplane 201, the presence of which may otherwise interfere with at least one of: the transmission of EM signals through the panel 300, and the capture of the EM signals by such at least one of: the underdisplay, and non under-display, component, including without limitation, the capture of an image by the camera. In some non-limiting examples, an overlying layer 170, including without limitation, at least one of: a polarizer, and one of: a cover glass, and a glass cap, of the display panel 300, may extend substantially across the at least one signal-exchanging part 303, the at least one display part 307, and the non-display part, such that it may extend substantially across the display panel 300. In some non-limiting examples, the through-hole part may be substantially devoid of a polarizer in order to enhance the transmission of light therethrough.

[0601] In some non-limiting examples, the non-display part may comprise a non through- hole part, which in some non-limiting examples, may be arranged between the through-hole part and an adjacent signal-exchanging part 303 in a lateral aspect. In some non-limiting examples, the non through-hole part may surround at least a part of a perimeter of the through-hole part. In some non-limiting examples, the user device 310 may comprise additional ones of at least one of: a module, component, and sensor, in a part of the user device 310 corresponding to the non through-hole part of the display panel 300.

[0602] In some non-limiting examples, the emissive regions 210 in the at least one signalexchanging part 303 may be electrically coupled with at least one TFT structure located in thenon-through-hole part of the non-display part. That is, in some non-limiting examples, the TFT structures 206 for actuating the (sub-) pixels 1115 / 216 in the at least one signal-exchanging part 303 may be relocated outside the at least one signal-exchanging part 303 and within the non through-hole part of the display panel 300, such that a substantially high transmission of light, in at least one of: the IR spectrum, and the NIR spectrum, may be directed through the non-emissive regions 211 within the at least one signal-exchanging part 303. In some non-limiting examples, the TFT structures 206 in the non through-hole part may be electrically coupled with (sub-) pixels 1115 / 216 in the at least one signal-exchanging part 303 via conductive trace(s). In some non-limiting examples, at least one of the transmitter 330t and the receiver 33 Or may be arranged to be proximate to the non through-hole part in the lateral aspect, such that a distance over which electrical current travels between the TFT structures 206 and the (sub-) pixels 1115 / 216 associated therewith, may be reduced.Emissive Region(s)

[0603] In some non-limiting examples, including where the OLED device 200 may comprise a display module, the lateral aspect of the device 200 may be sub-divided into a plurality of emissive regions 210 of the device 200, in which the longitudinal aspect of the device 200 structure, within each of the emissive region(s) 210, may cause light to be emitted therefrom when energized.

[0604] In some non-limiting examples, an individual emissive region 210 may have an associated pair of electrodes 220, 240, one of which may act as an anode and the other of which may act as a cathode, and at least one semiconducting layer 230 between them. Such an emissive region 210 may emit light at a given wavelength spectrum and may correspond to one of: a pixel 1115, and a sub-pixel 216 thereof. In some non-limiting examples, a plurality of sub-pixels 216, each corresponding to and emitting light of a different wavelength (range) may collectively form a pixel 1115.

[0605] In some non-limiting examples, the wavelength spectrum may correspond to a colour in, without limitation, the visible spectrum. The light at a first wavelength (range) emitted by a first sub-pixel 216 of a pixel 1115 may perform differently than the light at a second wavelength (range) emitted by a second sub-pixel 216 thereof because of the different wavelength (range) involved.

[0606] In some non-limiting examples, an active region 208 of an individual emissive region 210 may be defined to be bounded, in the longitudinal aspect, by the first electrode 220 and the second electrode 240, and to be confined, in the lateral aspect, to an emissive region 210, defined by presence of each of the first electrode 220, the second electrode 240, and the at least one semiconducting layer 230 therebetween (“emissive region layers”), that is, the first electrode 220, the second electrode 240, and the at least one semiconducting layer 230 therebetween, overlap laterally.

[0607] Those having ordinary skill in the relevant art will appreciate that the lateral aspect of the emissive region 210, and thus the lateral boundaries of the active region 208, may not correspond to the entire lateral aspect of at least one of: the first electrode 220, and the second electrode 240. Rather, the lateral aspect of the emissive region 210 may be substantially no more than the lateral extent of either of: the first electrode 220, and the second electrode 240. In some non-limiting examples, at least one of: parts of the first electrode 220 may be covered by the PDL(s) 209, and parts of the second electrode 240 may not be disposed on the at least one semiconducting layer 230, with the result, in at least one scenario, that the emissive region 210 may be laterally constrained thereby.

[0608] In some non-limiting examples, at least one of the various emissive region layers may be deposited by deposition of a corresponding constituent emissive region layer material.

[0609] In some non-limiting examples, some of the at least one semiconducting layers 230 may be laid out in a desired pattern by vapor deposition of the corresponding emissive region layer material through a fine metal mask (FMM) having apertures corresponding to the desired locations where the emissive region layer material is to be deposited. In some non-limiting examples, a plurality of the emissive region layers may be laid out in a similar pattern, including without limitation, by depositing the respective emissive region layer material thereof in their respective deposition stages using an FMM.

[0610] In some non-limiting examples, as discussed herein, the emissive region layer material corresponding to at least one of the first electrode 220 and the second electrode 240, including without limitation, the second electrode 240, may be deposited by prior deposition of a patterning coating 110 by vapor deposition of a patterning material through an FMM having apertures corresponding to the desired locations where the patterning coating 110 is to bedeposited and thereafter depositing the emissive region layer material using one of: an open mask, and mask-free, deposition process.

[0611] In some non-limiting examples, the patterning coating 110 may be adapted to impact a propensity of a vapor flux 532 of a deposited material 531 of which the emissive region layer material may be comprised, to be deposited thereon, including without limitation, an initial sticking probability against the deposition of the deposited material 531 that is no more than an initial sticking probability against the deposition of the deposited material 531 of the exposed layer surface 11 of the at least one semiconducting layer 230.

[0612] In some non-limiting examples, the first electrode 220 may be disposed over an exposed layer surface 11 of the device 200, in some non-limiting examples, within at least a part of the lateral aspect of the emissive region 210. In some non-limiting examples, at least within the lateral aspect of the emissive region 210 of the (sub-) pixel(s) 1115 / 216, the exposed layer surface 11, may, at the time of deposition of the first electrode 220, comprise the TFT insulating layer 207 of the various TFT structures 206 that make up the driving circuit for the emissive region 210 corresponding to a single display (sub-) pixel 1115 / 216.

[0613] In some non-limiting examples, the TFT insulating layer 207 may be formed with an opening extending therethrough to permit the first electrode 220 to be electrically coupled with a TFT electrode including, without limitation, a TFT drain electrode.

[0614] Those having ordinary skill in the relevant art will appreciate that the driving circuit may comprise a plurality of TFT structures 206. In FIG. 2, for purposes of simplicity of illustration, only one TFT structure 206 may be shown, but it will be appreciated by those having ordinary skill in the relevant art, that such TFT structure 206 may be representative of at least one of: such plurality thereof, and at least one component thereof, that comprise the driving circuit.

[0615] In some non-limiting examples, an extremity of the first electrode 220 may be covered by at least one PDL 209 such that a part of the at least one PDL 209 may be interposed between the first electrode 220 and the at least one semiconducting layer 230, such that such extremity of the first electrode 220 may lie beyond the active region 208 of the associated emissive region 210.

[0616] In some non-limiting examples, the at least one semiconducting layer 230 (including without limitation, at least one of: layers 231, 233, 235, 237, 239 thereof) may bedeposited over the exposed layer surface 11 of the device 200, including at least a part of the lateral aspect of such emissive region 210 of the (sub-) pixel(s) 1115 / 216. In some non-limiting examples, at least within the lateral aspect of the emissive region 210 of the (sub-) pixel(s) 1115 / 216, such exposed layer surface 11, may, at the time of deposition of such at least one semiconducting layer 230 comprise the first electrode 220.

[0617] In some non-limiting examples, the at least one semiconducting layer 230 may also extend beyond the lateral aspect of the emissive region 210 of the (sub-) pixel(s) 1115 / 216 and at least partially within the lateral aspects of the surrounding non-emissive region(s) 211. In some non-limiting examples, such exposed layer surface 11 of such surrounding non-emissive region(s) 211 may, at the time of deposition of the at least one semiconducting layer 230, comprise the PDL(s) 209.

[0618] In some non-limiting examples, the second electrode 240 may be disposed over an exposed layer surface 11 of the device 200, including at least a part of the lateral aspect of the emissive region 210 of the (sub-) pixel(s) 1115 / 216. In some non-limiting examples, at least within the lateral aspect of the emissive region 210 of the (sub-) pixel(s) 1115 / 216, such exposed layer surface 11, may, at the time of deposition of the second electrode 220, comprise the at least one semiconducting layer 230.

[0619] In some non-limiting examples, the second electrode 240 may also extend beyond the lateral aspect of the emissive region 210 of the (sub-) pixel(s) 1115 / 216 and at least partially within the lateral aspects of the surrounding non-emissive region(s) 211. In some non-limiting examples, an exposed layer surface 11 of such surrounding non-emissive region(s) 211 may, at the time of deposition of the second electrode 240, comprise the PDL(s) 209.

[0620] In some non-limiting examples, the second electrode 240 may extend throughout a substantial part, including without limitation, substantially all, of the lateral aspects of the surrounding non-emissive region(s) 211.

[0621] In some non-limiting examples, individual emissive regions 210 of the device 200 may be laid out in a lateral pattern. In some non-limiting examples, the pattern may extend along a first lateral direction. In some non-limiting examples, the pattern may also extend along a second lateral direction, which in some non-limiting examples, may extend at an angle relative to the first lateral direction. In some non-limiting examples, the second lateral direction may be substantially normal to the first lateral direction. In some non-limiting examples, the pattern mayhave a number of elements in such pattern, each element being characterized by at least one feature thereof, including without limitation, at least one of: a wavelength of light emitted by the emissive region 210 thereof, a shape of such emissive region 210, a dimension (along at least one of: the first, and second, lateral directi on(s)), an orientation (relative to at least one of: the first, and second, lateral directi on(s)), and a spacing (relative to at least one of: the first, and second, lateral direction(s)) from a previous element in the pattern. In some non-limiting examples, the pattern may repeat in at least one of: the first, and second, lateral direction(s).

[0622] In some non-limiting examples, each individual emissive region 210 of the device 200 may be associated with, and driven by, a corresponding driving circuit within the backplane 202 of the device 200, for driving an OLED structure for the associated emissive region 210. In some non-limiting examples, including without limitation, where the emissive regions 210 may be laid out in a regular pattern extending in both the first (row) lateral direction and the second (column) lateral direction, there may be a signal line in the backplane 202, corresponding to each row of emissive regions 210 extending in the first lateral direction and a signal line, corresponding to each column of emissive regions 210 extending in the second lateral direction. In such a non-limiting configuration, a signal on a row selection line may energize the respective gates of the switching TFT structure(s) 206 electrically coupled therewith and a signal on a data line may energize the respective sources of the switching TFT structure(s) 206 electrically coupled therewith, such that a signal on a row selection line / data line pair may electrically couple and energise, by the positive terminal of the power source, the anode of the OLED structure of the emissive region 210 associated with such pair, causing the emission of a photon therefrom, the cathode thereof being electrically coupled with the negative terminal of the power source 204.

[0623] In some non-limiting examples, a single display pixel 1115 may comprise three sub-pixels 216, which in some non-limiting examples, may correspond respectively to a single sub-pixel 216 of each of three colours, including without limitation, at least one of: a R(ed) subpixel 216R, a G(reen) sub-pixel 216G, and a B(lue) sub-pixel 216B. In some non-limiting examples, a single display pixel 1115 may comprise four sub-pixels 216, each corresponding respectively to a single sub-pixel 216 of each of two colours, including without limitation, a R(ed) sub-pixel 216R, and a B(lue) sub-pixel 216B, and two sub-pixels 216 of a third colour, including without limitation, a G(reen) sub-pixel 216G. In some non-limiting examples, a single display pixel 1115 may comprise four sub-pixels 216, which in some non-limiting examples,may correspond respectively to a single sub-pixel 216 of each of three colours, including without limitation, at least one of: a R(ed) sub-pixel 216R, a G(reen) sub-pixel 216G, and a B(lue) subpixel 216B, and a fourth W(hite) sub-pixel 216w.

[0624] In some non-limiting examples, the emission spectrum of the light emitted by a given (sub-) pixel 1115 / 216 may correspond to the colour by which the (sub-) pixel 1115 / 216 may be denoted. In some non-limiting examples, the wavelength of the light may not correspond to such colour, but further processing may be performed, in a manner apparent to those having ordinary skill in the relevant art, to transform the wavelength to one that does so correspond.

[0625] In some non-limiting examples, the emission spectrum of the light emitted by a given (sub-) pixel 1115 / 216, corresponding to the colour by which the (sub-) pixel 1115 / 216 may be denoted, may be related to at least one of: the structure and composition of the at least one semiconducting layer 230 extending between the first electrode 220 and the second electrode 240 thereof, including without limitation, the at least one EML 235. In some non-limiting examples, the at least one EML 235 of the at least one semiconducting layer 230 may be tuned to facilitate the emission of light having an emission spectrum corresponding to the colour by which the (sub- ) pixel 1115 / 216 may be denoted. In some non-limiting examples, the EML 235 of a R(ed) subpixel 216R may comprise a R(ed) EML material, including without limitation, a host material doped with a R(ed) emitter material. In some non-limiting examples, the EML 235 of a G(reen) sub-pixel 216G may comprise a G(reen) EML material, including without limitation, a host material doped with a G(reen) emitter material. In some non-limiting examples, the EML 235 of a B(lue) sub-pixel 216B may comprise B(lue) EML material, including without limitation, a host material doped with a B(lue) emitter material.

[0626] In some non-limiting examples, at least one characteristic of at least one of the at least one semiconducting layer 230, including without limitation, the HIL 231, the HTL 233, the EML 235, the ETL 237, and the EIL 239, including without limitation, a presence thereof, an absence thereof, a thickness thereof, a composition thereof, and an order thereof, in the longitudinal aspect, may be selected to facilitate emission therefrom of light having a wavelength spectrum corresponding to the colour by which a given sub-pixel 216 may be denoted, including without limitation, at least one of: R(ed), G(reen), and B(lue).

[0627] In some non-limiting examples, emission of light having a wavelength spectrum corresponding to a plurality of colours selected from: R(ed), G(reen), and B(lue) may facilitateemission of light having a wavelength spectrum corresponding to a different colour, including without limitation W(hite) (R+G+B), Y(ellow) (R+G), C(yan) (G+B), and M(agenta) (B+R), according to the additive colour model.

[0628] In some non-limiting examples, the exposed layer surface 11 of the device 100 may be exposed to a vapor flux 532 of a deposited material 531, including without limitation, in one of: an open mask, and mask-free, deposition process.

[0629] In some non-limiting examples, in at least a part of the emissive region 210, the at least one semiconducting layer 230 may be deposited over the exposed layer surface 11 of the device 200, which in some non-limiting examples, comprise the first electrode 220.

[0630] In some non-limiting examples, the exposed layer surface 11 of the device 200, which may, in some non-limiting examples, comprise the at least one semiconducting layer 230, may be exposed to a vapor flux 412 of the patterning material 411, including without limitation, using a shadow mask 415, to form a patterning coating 110 in the first portion 101. Whether a shadow mask 415 is employed, the patterning coating 110 may be restricted, in its lateral aspect, substantially to a signal-transmissive region 212.

[0631] In some non-limiting examples, a lateral aspect of at least one emissive region 210 may extend across and include at least one TFT structure 206 associated therewith for driving the emissive region 210 along data and scan lines (not shown), which, in some non-limiting examples, may be formed of at least one of: Cu, and a TCO.

[0632] In some non-limiting examples, the (sub-) pixels 1115 / 216 may be disposed in a side-by-side arrangement. In some non-limiting examples, a (colour) order of the sub-pixels 216 of a first pixel 1115 may be the same as a (colour) order of the sub-pixels 216 of a second pixel 1115. In some non-limiting examples, a (colour) order of the sub-pixels 216 of a first pixel 1115 may be different from a (colour) order of the sub-pixels 216 of a second pixel 1115.

[0633] In some non-limiting examples, the sub-pixels 216 of adjacent pixels 1115 may be aligned in at least one of: a row, column, and array, arrangement.

[0634] In some non-limiting examples, a first at least one of: a row, and a column, of aligned sub-pixels 216 of adjacent pixels 1115 may comprise sub-pixels 216 of one of: a same, and a different, colour.

[0635] In some non-limiting examples, a first at least one of: a row, and a column, of aligned sub-pixels 216 of adjacent pixels 1115 may be aligned with at least one of a second, and a third, at least one of a row, and a column, of aligned sub-pixels 216 of adjacent pixels 1115.

[0636] In some non-limiting examples, a first at least one of a row, and a column, of aligned sub-pixels 216 of adjacent pixels 1115 may be one of offset from, and mis-aligned with, at least one of a second, and a third, at least one of a row, and a column, of aligned sub-pixels 216 of adj acent pixels 1115.

[0637] In some non-limiting examples, the sub-pixels 216 of adjacent pixels 1115 of such at least one of first, second, and third, at least one of a row, and a column, may be arranged such that corresponding sub-pixels 216 of each of the at least one of first, second, and third, at least one of a row, and a column, may be of a same colour.

[0638] In some non-limiting examples, the sub-pixels 216 of adjacent pixels 1115 of such at least one of first, second, and third, at least one of a row, and a column, may be arranged such that corresponding sub-pixels 216 of each of the at least one of first, second and third, at least one of a row, and a column, may be of different colours.

[0639] In some non-limiting examples, in the at least one signal-exchanging part 303 of a display panel 300, the at least one signal-transmissive region 212 may be disposed between a plurality of emissive regions 210. In some non-limiting examples, the at least one signal- transmissive region 212 may be disposed between adjacent (sub-) pixels 1115 / 216. In some nonlimiting examples, the adjacent sub-pixels 216 surrounding the at least one signal -transmissive region 212 may form part of a same pixel 1115. In some non-limiting examples, the adjacent sub-pixels 216 surrounding the at least one signal-transmissive region 212 may be associated with different pixels 1115.

[0640] In some non-limiting examples, a region that may be substantially devoid of a closed coating 140 of a second electrode material (“cathode-free region”), including without limitation, the at least one signal-transmissive region 212, in some non-limiting examples, may exhibit different opto-electronic characteristics from other regions, including without limitation, the at least one emissive region 210. In some non-limiting examples, such cathode-free regions may nevertheless comprise some second electrode material, including without limitation, in the form of a discontinuous layer 160 of one of at least one particle structure 150, and at least one instance of such particle structures 150.

[0641] In some non-limiting examples, this may be achieved by laser ablation of the second electrode material. However, in some non-limiting examples, laser ablation may create a debris cloud, which may impact the vapour deposition process.

[0642] In some non-limiting examples, this may be achieved by disposing a patterning coating 110, which may, in some non-limiting examples, be a nucleation inhibiting coating (NIC), using an FMM, in a pattern on an exposed layer surface 11 of the at least one semiconducting layer 230 prior to depositing a deposited material 531 for forming the second electrode 240 thereon.

[0643] In some non-limiting examples, the patterning coating 110 may be adapted to impact a propensity of a vapor flux 532 of the deposited material 531 to be deposited thereon, including without limitation, an initial sticking probability against the deposition of the deposited material 531 that is no more than an initial sticking probability against the deposition of the deposited material 531 of the exposed layer surface 11 of the at least one semiconducting layer 230.

[0644] In some non-limiting examples, the patterning coating 110 may be deposited in a pattern that may correspond to the first portion 101 of a lateral aspect, including without limitation, of at least some of the signal-transmissive regions 212.

[0645] In some non-limiting examples, the patterning coating 110 may be deposited in a plurality of stages, each using a different FMM defining a different pattern within the first portion 101, that respectively correspond to a different subset of the signal -transmissive regions 212.

[0646] In some non-limiting examples, the display panel 300 may, subsequent to (all of the stages of) the deposition of the patterning coating 110, be subjected to a vapor flux 532 of the deposited material 531, in one of: an open mask, and mask-free, deposition process, to form the second electrode 240 for each of the emissive regions 210 corresponding to a (sub-) pixel 1115 / 216 in at least the second portion 102 of the lateral aspect, but not in the first portion 101 of the lateral aspect.

[0647] In some non-limiting examples, although not shown, the overlying layer 170 may be arranged above at least one of: the second electrode 240, and the patterning coating 110. In some non-limiting examples, although not shown, the overlying layer 170 may be deposited atleast partially across the lateral extent of the opto-electronic device 200, in some non-limiting examples, covering the second electrode 240 in the second portion 102, and, in some nonlimiting examples, at least partially covering the at least one particle structure 150 and forming an interface with the patterning coating 110 at the exposed layer surface 11 thereof in the first portion 101.Non-Emissive Regions

[0648] In some non-limiting examples, the various emissive regions 210 of the device 200 may be substantially surrounded and separated by, in at least one lateral direction, at least one non-emissive region 211, in which at least one of: the structure, and configuration, along the longitudinal aspect, of the device 200 shown, without limitation, may be varied, to substantially inhibit light to be emitted therefrom.

[0649] In some non-limiting examples, the non-emissive regions 211 may comprise those regions in the lateral aspect, that are substantially devoid of an emissive region 210.

[0650] In some non-limiting examples, the longitudinal topology of the various layers of the at least one semiconducting layer 230 may be varied to define at least one emissive region 210, surrounded (at least in one lateral direction) by at least one non-emissive region 211.

[0651] A non-limiting example of an implementation of the longitudinal aspect of the device 200 as applied to an emissive region 210 corresponding to a single display (sub-) pixel 1115 / 216 of the display 200 will now be described. While features of such implementation are shown to be specific to the emissive region 210, those having ordinary skill in the relevant art will appreciate that in some non-limiting examples, more than one emissive region 210 may encompass features in common.

[0652] In some non-limiting examples, the lateral aspects of the surrounding non- emissive region(s) 211 may be characterized by the presence of a corresponding PDL 209.

[0653] In some non-limiting examples, a thickness of the PDL 209 may increase from a minimum, where it covers the extremity of the first electrode 220, to a maximum beyond the lateral extent of the first electrode 220. In some non-limiting examples, the change in thickness of the at least one PDL 209 may define a valley shape centered about the emissive region 210. In some non-limiting examples, the valley shape may constrain the field of view (FOV) of the light emitted by the emissive region 210.

[0654] While the PDL(s) 209 have been generally illustrated herein as having a linearly- sloped surface to form a valley-shaped configuration that define the emissive region(s) 210 surrounded thereby, those having ordinary skill in the relevant art will appreciate that in some non-limiting examples, at least one of: the shape, aspect ratio, thickness, width, and configuration of such PDL(s) 209 may be varied. In some non-limiting examples, a PDL 209 may be formed with one of: a substantially steep part and a more gradually sloped part. In some non-limiting examples, such PDL(s) 209 may be configured to extend substantially normally away from a surface on which it is deposited, that may cover at least one edge of the first electrode 220. In some non-limiting examples, such PDL(s) 209 may be configured to have deposited thereon at least one semiconducting layer 230 by a solution-processing technology, including without limitation, by printing, including without limitation, ink-jet printing.

[0655] In some non-limiting examples, the PDLs 209 may be deposited substantially over the TFT insulating layer 207, although, as shown, in some non-limiting examples, the PDLs 209 may also extend over at least a part of the deposited first electrode 220, including without limitation, its outer edges.

[0656] In some non-limiting examples, the lateral extent of at least one of the non- emissive regions 211 may be at least, and in some non-limiting examples, exceed, including without limitation, be a multiple of, the lateral extent of the emissive region 210 interposed therebetween.

[0657] In some non-limiting examples, a thickness of at least one PDL 209 in at least one signal-transmissive region 212, in some non-limiting examples, of at least one non-emissive region 211, in...

Claims

WHAT IS CLAIMED IS:

1. An opto-electronic device comprising: an anode; a cathode; and at least one semiconducting layer disposed between the anode and the cathode, the at least one semiconducting layer comprising a low-index layer; wherein: the low-index layer comprises a mixture of a low-index material and a higher-index material, wherein the low-index material comprises a phosphazene moiety and at least one fluorine (F)-containing functional group attached thereto.

2. The opto-electronic device of claim 1, wherein an absorption coefficient of the low-index layer in at least a sub-range of the visible spectrum is one of no more than about: 0.1, 0.08, 0.06, 0.05, 0.03, and 0.01.

3. The device of claim 1, wherein a refractive index of the low-index layer is no more than a refractive index of at least one layer arranged adjacent thereto.

4. The device of any one of claims 1 through 3, wherein a refractive index of the low-index layer in at least a sub-range of the visible spectrum is one of no more than about: 1.8, 1.75, 1.7, 1.65, 1.6, 1.55, 1.5, 1.45, and 1.4.

5. The device of any one of claims 1 through 4, wherein a characteristic refractive index of the low-index material, in at least a sub-range of the visible spectrum, is no more than a characteristic refractive index of the higher-index material, by one of at least about: 0.1, 0.15, 0.2, 0.25, 0.3, 0.4, and 0.5.

6. The device of any one of claims 1 through 5, wherein a characteristic refractive index of the low-index material, in at least a sub-range of the visible spectrum, is one of no more than about: 1.6, 1.55, 1.5, 1.45, 1.4, 1.35, and 1.3.

7. The device of any one of claims 1 through 6, wherein a characteristic refractive index of the higher-index material, in at least a sub-range of the visible spectrum, is one of at least about: 1.8, 1.85, and 1.9.

8. The device of any one of claims 1 through 7, wherein the low-index layer comprises, by at least one of: volume percentage, weight percentage, and mole percentage, the low-index material in a concentration of one of no more than about: 80, 75, 70, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 13, 10, 8, and 5%.

9. The device of any one of claims 1 through 8, wherein the low-index layer comprises, by at least one of: volume percentage, weight percentage, and mole percentage, the low-index material in a concentration of one of at least about: 1, 3, 5, 8, 10, 15, 20, 25, 30, 35, 40, 45, and 50%.

10. The device of any one of claims 1 through 9, wherein the low-index material has a band gap of one of at least about 3.4, 3.5, 4.1, 5, and 6.2, eV.

11. The device of any one of claims 1 through 10, wherein the low-index material is one of: a small molecule, and an oligomer.

12. The device of any one of claims 1 through 11, wherein the low-index material is an organic-inorganic hybrid material.

13. The device of any one of claims 1 through 12, wherein a molecular structure of the low- index material comprises at least one of a: cyclophosphazene, fluoroalkyl, and silsesquioxane, moiety.

14. The device of claim 13, wherein the low-index layer comprises, by weight percentage, a low-index material comprising a cyclophosphazene moiety, in a concentration of between about 1-20%.

15. The device of any one of claims 13 and 14, wherein the low-index material comprises, by weight percentage, F, in a concentration of between about 10-50%.

16. The device of any one of claims 1 through 15, wherein a molecular structure of the low- index material comprises a low surface tension moiety.

17. The device of claim 16, wherein the molecular structure of the low-index material comprises a high surface tension moiety bonded to the low surface tension moiety.

18. The device of any one of claims 16 and 17, wherein the low surface tension moiety comprises at least one of a: F, and silicon (Si), -containing moiety.

19. The device of claim 18, wherein the F-containing moiety is a fluoroalkyl moiety.

20. The device of any one of claims 18 and 19, wherein the Si-containing moiety is a siloxyl moiety.

21. The device of any one of claims 1 through 20, wherein at least one of an: electron, and hole, mobility of the low-index layer is at least about 10'5.

22. The device of any one of claims 1 through 21, wherein a solubility, in N-methyl-2- pyrrolidone, of at least one of the: low-index material, and higher-index layer, is at least about 1 mg / mL.

23. The device of any one of claims 1 through 22, wherein the higher-index material comprises an organic semiconducting material.

24. The device of claim 23, wherein the organic semiconducting material comprises a polycyclic aromatic moiety.

25. The device of any one of claims 23 and 24, wherein the organic semiconducting material is a hole transport material.

26. The device of any one of claims 1 through 25, wherein the at least one semiconducting layer comprises an emissive layer (EML) and the device is configured to emit light therefrom in response to an electrical current being applied thereto.

27. The device of claim 26, wherein the device is a top-emission device, and the light emitted by the EML is transmitted through the cathode.

28. The device of any one of claims 26 and 27, wherein the low-index layer is arranged between the EML and the anode.

29. The device of any one of claims 26 through 28, wherein the low-index layer forms at least a part of a hole transport layer (HTL).

30. The device of any one of claims 28 and 29, wherein the at least one semiconducting layer further comprises a hole injection layer (HIL) arranged between the EML and the anode, wherein the low-index layer is arranged between the HIL and the EML.

31. The device of any one of claims 1 through 30, wherein the functional group independently comprises at least one of: F, chlorine (Cl), a hydroxyl group, a substituted alkyl group, an unsubstituted alkyl group, a substituted fluoroalkyl group, an unsubstituted fluoroalkyl group, a substituted cycloalkyl group, an unsubstituted cycloalkyl group, a substituted fluorocycloalkyl group, an unsubstituted fluorocycloalkyl group, a substituted heterocycloalkyl group, an unsubstituted heterocycloalkyl group, a substituted fluoroheterocycloalkyl group, an unsubstituted fluoroheterocycloalkyl group, a substituted alkoxy group, an unsubstituted alkoxy group, a substituted fluoroalkoxy group, an unsubstituted fluoroalkoxy group, a substituted aryloxy group, an unsubstituted aryloxy group, a substituted fluoroaryloxy group, an unsubstituted fluoroaryloxy group, a substituted heteroaryloxy group, a unsubstituted heteroaryloxy group, a substituted fluoroheteroaryl oxy group, a unsubstituted fluoroheteroaryl oxy group, a substituted aryl group, an unsubstituted aryl group, a substituted fluoroaryl group, an unsubstituted fluoroaryl group, a substituted alkyl silyl group, an unsubstituted alkylsilyl group, a substituted alkylsiloxy group, an unsubstituted alkylsiloxygroup, an amino group, an amine group, an alkylamine group, an arylamine group, a cyano group, a phosphazo group, a sulfanyl group, a pentafluorosulfanyl group, a sulfide group, a sulfonyl group, a thiol group, an alkylthio group, a trifluoromethylthio group, a carbonyl group, a siloxane group, a silane group, and an organosilicon group.

32. The device of any one of claims 1 through 31, wherein the functional group comprises: a linker moiety RB, a terminal moiety RT, and an intermediate moiety RDarranged between the linker moiety RBand the terminal moiety RBwherein: the linker moiety RBcomprises one of: O, N, sulfur (S), a substituted alkylene, an unsubstituted alkylene, a substituted fluoroalkylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted arylene, an unsubstituted arylene, a substituted heteroarylene, and an unsubstituted heteroarylene; the intermediate moiety RDcomprises: O, an ether, a substituted alkylene, an unsubstituted alkylene, a substituted fluoroalkylene, an unsubstituted fluoroalkylene, a substituted cycloalkylene, an unsubstituted cycloalkylene, a substituted arylene, an unsubstituted arylene, a substituted phenyl, an unsubstituted phenyl, a substituted biphenyl, an unsubstituted biphenyl, a substituted binaphthalene, an unsubstituted binaphthalene, a substituted heteroarylene, and an unsubstituted heteroarylene; and the terminal moiety RTcomprises at least one of: a substituted alkyl, an unsubstituted alkyl, a branched fluoroalkyl, an unbranched fluoroalkyl, a substituted heterocycloalkyl, an unsubstituted heterocycloalkyl, a substituted alkoxy, an unsubstituted alkoxy, a branched silyloxy, an unbranched silyloxy, a branched fluoroalkoxy, an unbranched fluoroalkoxy, a fluoroaryl, a polyfluorosulfanyl, and a fluorocycloalkyl.

33. The device of claim 32, wherein the linker moiety RBis selected from: -O-, and -O-CH2-.

34. The device of any one of claims 1 through 33, wherein the at least one F-containing functional group is represented by Chemical Formula (VII):where: p is an integer between about 1-5; q is an integer between about 6-20; andZ represents one of: H, and F.

35. The device of claim 34, wherein p is 1, and q is an integer between about 6-20.

Citation Information

Patent Citations

  • Organic electroluminescence device

    US7612500B2

  • Silsesquioxane compound, organic light emitting element, display apparatus, image information processing apparatus, and image forming apparatus

    US9755165B2

  • Porous film, organic optoelectronic element, and porous film manufacturing method

    WO2021079927A1

  • Opto-electronic device including a low-index layer

    WO2022018702A1

  • Device including a low=index coating and a radiation-modifying layer

    WO2022074637A1