Electrostatically assisted coating method using backing roll having internal electrode to which high voltage can be applied

The three-layer backing roll with high-voltage capability effectively addresses the challenges of entrained air layers in electrostatic auxiliary coating, enhancing coating speed and uniformity while ensuring safety and stability, overcoming limitations of conventional methods.

WO2024236832A1PCT designated stage expired Publication Date: 2024-11-21KOKA CHROME IND
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2023/034039
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-15
Filing Date
2023-09-20
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Conventional electrostatic auxiliary coating methods face limitations in increasing coating speed and uniformity due to entrained air layers on both sides of the web, leading to web slippage, oscillation, and coating failure, especially at higher speeds, and are restricted by voltage limitations that can cause spark discharge and short-circuit currents.

Method used

A three-layer backing roll with a highly insulating ceramic outermost layer, a conductive metal internal electrode layer, and a high-resistance ceramic middle layer allows for the application of high DC voltage up to 6 kV without spark discharge, effectively eliminating entrained air layers on both sides of the web by electrostatic forces, ensuring stable web conveyance and uniform coating.

Benefits of technology

This solution enables increased coating speed up to 400 m/min with improved uniformity and safety by preventing spark discharge and short-circuit currents, allowing for wider and longer web processing without web floating or coating failures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023034039_21112024_PF_FP_ABST
    Figure JP2023034039_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a coating method for a wide web, with which it is possible to achieve high-speed and stable coating and excellent uniformity in coating thickness. Disclosed is a method for coating a flexible plastic-based web with a coating liquid, the method comprising: a step in which the web is conveyed to a backing roll for coating and is then passed through a coating point while being supported by the backing roll in such a manner that a second surface of the web is in close contact with a part of the surface of the backing roll, which is rotating and to which a DC voltage is applied, by means of an electrostatic field of the backing roll; and a step in which a first surface of the web is coated with a coating liquid at the coating point by the coating liquid being attracted to the first surface of the web by means of an electrostatic force generated as a result of an arrangement of charges having the same polarity as the applied DC voltage. The backing roll comprises an outermost layer, an internal electrode layer, and an insulating layer, in the stated order, and is configured so that a predetermined voltage can be applied to the internal electrode layer. The outermost layer is a ceramic-based material layer that has a volume resistivity value of 107 Ωcm to 1013 Ωcm at 25°C to 100°C.
Need to check novelty before this filing date? Find Prior Art

Description

Electrostatically assisted coating method using a backing roll having an internal electrode to which a high voltage can be applied

[0001] The present invention relates to a method for applying one or more layers of a coating liquid consisting of a liquid composition, particularly an aqueous composition, to the surface of a flexible, strip-like support (hereinafter referred to as a web) that is supported by a backing roll and runs continuously, by a method such as curtain coating or bead coating, in which an electrostatic force is applied to the contact line (hereinafter referred to as a coating point) where the coating liquid comes into contact with the web, thereby preventing an air layer accompanying the front side (coating surface) of the web from being trapped between the coating liquid and the web and promoting uniform wetting of the coating liquid onto the web, thereby increasing the uniformity of the coating thickness and the coating speed.

[0002] The present invention also relates to a method for bringing the backside of a web (the side of a backing roll) into close contact with the surface of a backing roll, thereby preventing an air layer accompanying the backside of the web and the roll surface from penetrating between the web and the roll, thereby enabling the upper limit of the web speed to be increased before running problems such as fluctuations in web tension and speed, and oscillation occur.

[0003] The present invention is applicable to improving the coating method of liquid compositions, mainly aqueous compositions, in the production of photographic films, photographic printing papers, magnetic recording tapes, adhesive tapes, pressure-sensitive and heat-sensitive recording papers, coated papers, etc.

[0004] In curtain coating and bead coating, air layers are entrained on both the front and back sides of the web moving at high speed.

[0005] The thickness of the entrained air layers on the front and back sides increases in proportion to the web speed, and when a certain critical speed is reached, the coating uniformity decreases or web slippage and oscillation occur, making stable coating impossible and making it impossible to increase the coating speed beyond the critical speed. In order to increase the speed while maintaining coating uniformity, a method is needed that can simultaneously address the effects of the entrained air layers on the front and back sides of the web.

[0006] On the front surface of the web, if the web moving speed increases and the entrained air layer increases beyond a certain limit, the air layer will penetrate under the coating liquid transferred to the web at the coating point and will not be able to be pushed out by the coating liquid. If the air layer penetrates under the coating layer, the coating liquid will be prevented from wetting and spreading on the front surface of the web, or the air layer will be entrapped in the coating liquid and form bubbles, reducing the uniformity of the coating layer, making it impossible to increase the coating speed.

[0007] It has been well known that in curtain coating and bead coating, the application of an electrostatic field at the coating point increases the upper limit of the coating speed by attracting the coating liquid to the web surface through electrostatic forces acting on ions and dipolar molecules in the coating liquid. The following methods for applying an electrostatic field at the coating point have been disclosed: 1) a method in which an electrostatic charge is applied to the web from a corona discharge electrode disposed in space, and then the web is passed through the coating point while supported by a grounded coating backing roll; 2) a method in which a DC voltage is applied to a conductive coating backing roll (hereinafter referred to as "backing roll") insulated from the earth, thereby forming an electric field between the web surface and the coating liquid at the coating point; and 3) a method combining these two.

[0008] For example, Patent Documents 1 to 4 disclose a method (1) in which a dielectric web such as polyester is charged. When a dielectric web with a polar charge bound between its opposing front and back surfaces is supported on a grounded conductive backing roll and transported to a coating point, the polar charge remaining on the front side of the web attracts the coating liquid, more effectively eliminating the air layer beneath the coating liquid, thereby increasing the coating speed. Patent Documents 5 to 7 disclose a method (2) in which a DC voltage is applied to a conductive backing roll insulated from ground to charge its surface, and the web is supported on that surface and transported to a coating point, creating an electric field between the web and the coating liquid, thereby adhering the coating liquid to the web. Patent Document 7 also discloses a method combining methods (2) and (3).

[0009] The effect of imparting electrostatic charge to a web or assisting electrostatic charge on the surface of a conductive backing roll is to suppress the phenomenon in which an air layer accompanying the web becomes entrapped between the web surface and the coating liquid, preventing the coating liquid from wetting, thereby increasing the critical speed at which the coating transparency and thickness become non-uniform. In conventional electrostatically assisted coatings 1) to 3), the stronger the adhesion of the coating liquid to the web surface, the more effectively the entrained air layer is eliminated. Therefore, it is known that in all cases, the coating speed increases as the electrostatic charge potential on the web surface or the voltage on the backing roll surface increases. However, in electrostatically assisted coatings in which a voltage is applied to a conductive backing roll, it is known that an applied voltage exceeding 1500 V is likely to cause spark discharge from the backing roll to peripheral equipment and short-circuit currents that penetrate the web. Furthermore, even in methods of imparting electrostatic charge to a web, if the charge potential on the web surface increases, short-circuit currents that penetrate the web may occur between the coating liquid and the conductive backing roll surface at locations where the web has pinholes or low insulation resistance. For this reason, the surface potential of the web due to the electrostatic charge disclosed in Patent Document 1 is 1200 V or less. Other examples include Patent Document 4, which discloses an electrostatic auxiliary coating technique that uses the polarization effect of a coating solution containing a surfactant, and Patent Document 2, which discloses a method of charging the web with a conductive brush, thereby setting the surface potential of the web below 700 to 800 V; however, the standard recommended surface potential is even lower, at 400 to 500 V. As such, conventional electrostatic auxiliary coating using a conductive backing roll is unable to apply a sufficient potential to the coating point, and is therefore insufficient in raising the critical speed before coating problems due to an increase in entrained air occur.

[0010] Furthermore, the backside of the web and the surface of the backing roll each have their own entrained air layers. Therefore, the combined entrained air causes the web to float, and the amount of floating increases as the web speed increases. When the web floating amount exceeds a certain limit, the web transport becomes unstable, and the increase in the entrained air layer on the backside of the web also makes it difficult to increase the coating speed.

[0011] The web lift h (μm) is determined by the backing roll radius R (m) and roller speed U when the air temperature is 25°C. R (m / s), web speed U W (m / s) and web tension T (N / m) are given by the following equation (1).

[0012]

[0013] (Hashimoto Kyo, "Web Handling: Fundamental Theory and Applications," p. 73, published by the Processing Technology Research Association)

[0014] According to equation (1), the thickness of the entrained air layer entrained between the backside of the web and the roll surface decreases as the web tension T increases, and the roll radius R and web speed U W or backing roll speed U R It increases as the value of is increased (usually U W ≒U R ).

[0015] In electrostatically assisted coating, where a voltage is applied to a conductive backing roll, as the web travel speed increases and the web floats due to the air layer between the web and the backing roll, the distance from the backing roll surface to the front side of the web increases, and the air layer between the conductive backing roll and the back side of the web reduces the electrostatic capacitance, which reduces the amount of polar charge stored on the web and the electrostatic force between the web and the coating solution.

[0016] Furthermore, if the thickness of the entrained air layer on the backside of the web exceeds the sum of the surface roughness of the roll and the surface roughness of the backside of the web, contact between the web and the backing roll surface decreases, and the force pulling the web decreases. When the web pulling force decreases, the web tension and speed begin to fluctuate, causing problems such as web meandering and scratches on the backside of the web. Therefore, in order to increase the coating speed, it is absolutely necessary to take measures to prevent the web from floating by the entrained air layer sandwiched between the backside of the web and the backing roll.

[0017] The relationship between the web transport speed and the amount of lift calculated from equation (1) is shown in Figures 7 and 8. As shown in Figure 7, it is possible to suppress web lift by increasing the web tension T. However, increasing the web tension increases the load on the web transport system, increasing the amount of deflection of the backing roll and the guide rolls in the web transport path. Furthermore, if the web is thin, wrinkles are likely to occur, so there are limitations to how much the web tension can be increased.

[0018] As shown in Figure 8, reducing the diameter of the backing roll reduces the amount of web lift. However, reducing the diameter of the backing roll reduces the rigidity of the roll and increases the amount of deflection. Furthermore, as the roll diameter decreases, the roll rotation speed increases proportionally. Therefore, the faster the web moves and the wider the web becomes, the more the roll vibrates, resulting in vibration patterns on the coating film. For roller curtain coating or bead coating of wide webs 1500 mm or wider, a backing roll diameter of 100 mm or greater is preferred, considering the roll's deflection strength and the area required to install the coating head (applicator). The web tension depends on the strength and thickness of the web, but is typically around 75 to 300 N / m, taking into account web elongation and deformation. As shown in Figure 7, when using a 100 mm diameter backing roll, even with a web tension of 150 N / m, the web lift is already 6 μm at a moving speed of 100 m / min. For rolls with smooth surfaces, the traction force decreases, resulting in tension and speed fluctuations. Judging from the web floating amounts shown in Figures 7 and 8, when the diameter of the backing roll is set to 100 mm or more, in order to increase the web conveying speed to 100 m / min or more, it is necessary to prevent the web from floating by an air layer entrained on the back side of the web.

[0019] Patent Document 7 discloses a solution to the problem of web lifting caused by an entrained air layer on the backside of a web during electrostatically assisted curtain coating, in which a DC voltage is applied to a conductive backing roll with a diameter of 100 mm or more. In the examples of Patent Document 7, circumferential grooves (groove depth 0.15 mm, width 0.43 mm, pitch 1 mm) are formed on the surface of a 200 mm diameter backing roll, accounting for 10 to 30% of the roll surface area. The entrained air layer is discharged into the microgrooves, suppressing web lifting and enabling increased conveyance speed. However, the voltage applied to the conductive backing roll is 800 V or less, and the electrostatic assist effect is further reduced in the grooves, making coating unevenness more likely to occur. Therefore, the increase in coating speed when microgrooves and electrostatic assistance are used together is a maximum of 144 m / min, which is not very large.

[0020] Japanese Patent No. 2835659 Japanese Patent Publication No. 01-035702 Japanese Patent Publication No. 08-252517 Japanese Patent No. 2509316 Japanese Patent No. 06-009671 Japanese Patent Publication No. 46-027423 US Patent No. 6177141

[0021] Hashimoto Kyo, "Basic Theory and Applications of Web Handling", Published by the Processing Technology Research Association, p. 73

[0022] In curtain coating and bead coating, the front side (coating side) and back side (backing roll side) of a web moving at high speed are entrained with air layers on both sides, and their thickness increases as the web travel speed increases. However, the problems caused by entrained air layers are different on the front and back sides. On the front side, the coating liquid does not wet the web, but on the back side, the entrained air layer that penetrates between the back side of the web and the backing roll causes the web to float, resulting in unstable web running. There is a need for high-speed coating technology that can simultaneously address these different problems caused by entrained air flows on both the front and back sides of the web.

[0023] By using a backing roll that can apply a voltage of 1.5 kV or more, preferably up to about 3.5 kV, to the roll surface, the dielectric web is polarized more strongly, and the electric field between the web surface and the coating solution at the contact line between the coating solution and the web (coating point) can be made much stronger than with conventional methods, so that the coating speed can be increased as needed simply by adjusting the applied voltage.

[0024] At the same time, the backside of the web, which has been strongly polarized by the high voltage of the backing roll, is strongly attracted to the backing roll by the electric field caused by the positive charge on the backing roll surface, pushing out the accompanying air layer and adhering to the surface of the backing roll, making it possible to raise the limit speed at which web running problems occur.

[0025] In order to achieve the above object, the present invention employs the following method.

[0026] The present invention provides an electrostatically assisted coating method using a highly safe backing roll in a process for applying a liquid composition (especially an aqueous composition) to a continuously running web supported by the roll. This method prevents spark discharge to peripheral equipment, short-circuit current in the web, and electric shock even when a high DC voltage of up to 6 kV is applied. The backing roll has a three-layer structure on the roll surface, consisting of an outermost layer / internal electrode layer / bottom layer, with a highly insulating ceramic bottom layer, a conductive metal internal electrode layer, and a high-resistance ceramic material layer. The internal electrode layer is completely electrically shielded from the backing roll core and peripheral equipment by the outermost and bottom layers. Because the dielectric strength of the outermost and bottom layers is 6 kV or higher, spark discharge to peripheral equipment and short-circuit current in the web are completely prevented even when a high DC voltage of up to 6 kV is applied to the internal electrode layer.

[0027] That is, the method of the present invention is as follows: (1) A method for applying a coating liquid comprising a liquid composition by discharging it from a grounded applicator onto a first surface of a continuously moving flexible plastic web having first and second opposing surfaces, the method comprising the steps of: conveying the web along a path to a backing roll for coating; passing the web through a coating point while supporting the second surface of the web in close contact with a part of the surface of the rotating backing roll to which a DC voltage is applied by an electrostatic field of the backing roll; and attracting the coating liquid at the coating point and applying it to the first surface of the web by an electrostatic force generated by coordinating, on the first surface of the web, charges of the same polarity as the DC voltage applied to the backing roll; the backing roll comprising an outermost layer to which the web is in close contact, a conductive monopolar internal electrode layer adjacent to the inner side of the outermost layer, and an insulating layer adjacent to the inner side of the internal electrode layer; the backing roll being configured to be able to apply a predetermined voltage to the internal electrode layer; and the outermost layer having a volume resistivity of 10 7 ~10 13a ceramic material layer of Ωcm, and the surface of the backing roll is, in a state where the predetermined voltage is applied to the internal electrode layer, charged with a charge of the same sign as the voltage applied to the internal electrode, and the second surface of the web, which has come into contact with the outermost layer by the electrostatic force of the charge, is brought into close contact with the outermost layer and rotated and transported, and the coating liquid is attracted to and brought into contact with the first surface of the web during rotation and transport, and deposited on the first surface of the web.

[0028] In the coating method, (2) a charge having a polarity opposite to that of the DC voltage applied to the internal electrode layer is applied to a first surface of the web opposite to the second surface before the coating liquid comes into contact with the web during rotational transport; (3) the DC voltage applied to the internal electrode layer is 0.3 to 6.0 KV; (4) the diameter of the backing roll is 100 mm or more; (5) at least one of the insulating layer, the internal electrode layer, and the outermost layer is a material formed by a thermal spraying method or a material using either an inorganic or organic binder, and at least one of the insulating layer, the internal electrode layer, and the outermost layer of the backing roll is subjected to a sealing treatment; (6) The outermost layer is made of a ceramic material, and the ceramic material is an alumina-based, zirconium oxide-based, or magnesium oxide-based ceramic containing a compound selected from titanium oxide, chromium oxide, silicon oxide, manganese oxide, nickel oxide, and iron oxide, or an aluminum oxide-based ceramic containing 5 to 17% by weight of titanium oxide; (7) The ceramic material contains at least one selected from aluminum nitride-based, silicon carbide-based, and silicon nitride-based materials, and an organic or inorganic binder; (8) The thickness of the outermost layer is 50 to 500 μm; (9) The center line average surface roughness Ra of the outermost layer is 0.01 to 5 μm; (10) The internal electrode layer is made of a conductive material containing tungsten or molybdenum; (11) The thickness of the internal electrode layer is 5 to 50 μm; (12) The insulating layer contains at least one highly insulating material selected from aluminum oxide, aluminum oxide containing 2 to 4% by weight of titanium oxide, magnesium oxide, beryllium oxide, aluminum nitride, or ceramic material containing silicon nitride, porcelain, and enamel; (13) The volume resistivity of the insulating layer is 10 13 (14) The insulating layer has a thickness of 50 to 500 μm.

[0029] The present invention provides an electrostatically assisted coating method using a highly safe backing roll that, in a process for applying a liquid composition (especially an aqueous composition) to a continuously running web supported by the roll, does not generate spark discharge to peripheral equipment, does not generate short-circuit current in the web, and does not cause electric shock even if a high DC voltage of up to 6 kV is applied to the roll surface. This backing roll has a tightly closed three-layer structure consisting of an outermost layer / internal electrode layer / insulating layer, with a highly insulating ceramic as the bottom layer, a conductive metal as the internal electrode layer, and a high-resistance ceramic material as the outermost layer. The internal electrode layer is completely electrically shielded from the backing roll core and peripheral equipment by the outermost and bottom layers. Because the dielectric strength of the outermost and bottom layers is 6 kV or higher, spark discharge to peripheral equipment is completely prevented even when a high DC voltage of up to 6 kV is applied to the internal electrode layer.

[0030] The volume resistivity of the outermost layer of high-resistivity semiconductor ceramic is 10 7 ~10 13 Because the internal electrode has a resistivity of Ωcm, when a DC voltage is applied to the internal electrode, charges migrate from the internal electrode to the outermost surface, charging the surface of the outermost layer with the same polarity as the internal electrode. At the same time, the web in contact with the outermost surface of the backing roll is dielectrically polarized by the electric field of the internal electrode, and the internal electric dipoles are oriented so that the backside is charged with a charge of the opposite polarity to the internal electrode potential and the frontside is charged with a charge of the same polarity. The coating liquid is then attracted to the web surface by the electrostatic charge of the same polarity as the internal electrode oriented on the web surface, thereby adhering to the web and eliminating the air layer entrained on the front side of the web, promoting wetting of the coating liquid onto the web. At the same time, the charge of the opposite polarity to that of the internal electrode oriented on the backside of the web is attracted to the free charge of the same polarity as the internal electrode that is charged on the surface of the high-resistivity semiconductor ceramic, the outermost layer of the backing roll, so the web adheres to the backing roll surface. In this way, in the present invention, the influence of the entrained air layer on both the front and back sides of the web is eliminated, making it possible to significantly increase the coating speed onto the web.

[0031] The present invention can achieve the following effects. 1. By applying a high DC voltage of up to 6 kV to an internal electrode installed on the outer surface of a backing roll, it becomes possible to coat a liquid composition (especially an aqueous composition) with electrostatic assistance without generating spark discharge to surrounding equipment or damaging the web due to short-circuit current. 2. While applying a high DC voltage to the internal electrode of the backing roll, an external auxiliary electrode is installed in the space above the front surface of the web, and a DC voltage of 1.5 to 6 kV of opposite polarity to that of the internal electrode is simultaneously applied, thereby enabling electrostatically assisted coating, in which a charge of opposite polarity to that of the internal electrode is applied to the front surface of the web. 3. Even if the diameter of the backing roll is 100 mm or more, the electrostatic force generated by the electrostatic charge on the surface of the high-resistivity semiconductor ceramic on the outermost surface allows the web to be completely adhered to the backing roll, enabling effective electrostatically assisted coating of the web surface. Furthermore, by preventing rocking or slippage due to web lift, it becomes possible to increase the web conveyance speed to 400 m / min or more. 4. Since the diameter of the backing roll can be increased in accordance with the length of the roll, it is possible to increase the rigidity of the roll, making it easier to make the web wider.

[0032] 1 is a cross-sectional view showing an example of the method of the present invention in which electrostatic assisted coating is performed using only a backing roll to which a high voltage is applied to the internal electrode. It is a diagram schematically showing the charge distribution state in part A of FIG. 1. It is an external view of the method of the present invention, viewed from an oblique direction. It is a cross-sectional view of a modified method of the present invention in which electrostatic assisted coating is performed using a backing roll to which a high voltage is applied to the internal electrode and a method of applying an electrostatic charge to the web in combination. It is a diagram schematically showing the charge distribution state in part B of FIG. 4. It is an external view of a modified method of the present invention, viewed from an oblique direction. It is a graph showing the change in web lift amount with respect to tension and web speed for a backing roll with a diameter of φ200 mm. It is a graph showing the change in web lift amount with respect to backing roll diameter and web speed at a web tension of 150 N / m.

[0033] The method of the present invention is shown in Figures 1 to 3. Figure 2 shows a schematic diagram of the charge distribution state in part A shown in Figure 1.

[0034] (1) In order to improve coating capacity, in addition to increasing the web transport speed, it is important to lengthen the backing roll to widen the web. However, when the web tension is constant, lengthening the backing roll rapidly increases the amount of roll deflection. Therefore, to prevent backing roll deflection, it is necessary to simultaneously increase the backing roll diameter to increase the roll rigidity. (The amount of roll deflection is proportional to the cube of the roll length and inversely proportional to the fourth power of the moment of inertia (which is approximately proportional to the roll diameter).) However, as shown in Equation (1) above, increasing the roll diameter also proportionally increases the entrained air layer on the backside of the web. An increase in the entrained air layer lowers the upper limit of the web transport speed, making it impossible to increase the diameter of the backing roll and therefore the roll length. On the other hand, the present invention can eliminate the influence of the entrained air layer on the backside of the web, making it possible to widen the web by increasing the backing roll diameter and roll length as necessary. Judging from FIG. 8, the influence of the entrained air layer becomes significant when the diameter of the web-transporting roll is 100 mm or more, so the present invention is more effective when applied to a backing roll having a diameter of 100 mm or more.

[0035] The internal electrode layer 3 of the backing roll 1 of the present invention is a conductive layer adjacent to the outermost layer 4 on the inside with no gap therebetween and in contact with the outermost layer 4. The internal electrode layer 3 is of a unipolar type and is wired for connection to a high-voltage DC power supply 5 so that a DC voltage can be applied thereto, but the internal electrode layer 3 is completely insulated from the earth and the core metal 16 of the backing roll 1 by the insulating layer 2 adjacent thereto on the inside.

[0036] Generally, there are two types of internal electrode layers 3: monopolar and bipolar, depending on the voltage application method. A monopolar type has only a single internal electrode, either positive (+) or negative (-), and voltage is applied only between this single electrode and the ground. A bipolar type has two or more internal electrodes of different polarities. However, when the web, which is the object to be attracted, is grounded, charge (current) leaks to the ground, making the electrostatic attraction force unstable. In the present invention, a monopolar type is used for the internal electrode layer 3. The internal electrode layer 3 is formed continuously and uniformly over an area wider than the width of the web 7 in the axial direction of the backing roll 1, and over the entire circumference of the backing roll 1 in the rotational direction of the backing roll 1. If the internal electrode 3 is comb-shaped, strip-shaped, or spiral-shaped, shape unevenness will occur in the coating layer. Note that the internal electrode layer 3 does not need to be formed on both ends of the cylindrical surface of the backing roll 1, which are outside the support area of ​​the web 7.

[0037] The outermost layer 4 is made of a high-resistivity ceramic material, and the volume resistivity is 10 7 ~10 13 Ωcm, and more preferably 10 8 ~10 12 In the field of static electricity, the volume resistivity is 10 13 Materials with a volume resistivity of 10 Ωcm or more are classified as insulators because static electricity does not easily move. 6 Materials with a volume resistivity of less than Ωcm are called electrostatic conductors, and static electricity moves easily, resulting in an equipotential when a voltage is applied. 7 ~10 13 These materials are classified as intermediate between conductors and insulators, and are classified as "electrostatic semiconductors." When a voltage is applied, a minute current flows, and it is known that free charges move to the surface and become charged, just like a conductor. The amount of charge on these free charges depends on the applied voltage. Unlike conductive metal surfaces, the surface of these highly resistive semiconducting ceramic materials only experiences a localized charge of 0.001 to 10 μA / cm2, even when a high voltage of 3.5 to 6 kV is applied. 2Therefore, the discharge caused by the free charges on the surface becomes a minute corona and does not develop into an arc discharge, and no spark discharge occurs toward surrounding equipment.

[0038] In the present invention, as shown in Fig. 2, when a DC voltage is applied to the internal electrode layer 3, free charges 17 of the same polarity as the internal electrode 3 migrate to and become charged on the surface of the outermost layer 4. When the second surface 13 (back side) of the web 7 comes into contact with the surface of the outermost layer 4, dipoles 18 inside the web 7 are oriented with the polarity opposite to that of the free charges 17 toward the surface of the outermost layer 4 due to dielectric polarization caused by the electric field of the internal electrode. The web 7 then adheres to the surface of the outermost layer 4 due to the electrostatic force between the charges 17 on the surface of the outermost layer 4 and the opposite charges of the dipoles oriented on the second surface 13 of the web 7. At this time, the first surface 12 (front side) of the web, which is the coating surface, is polarized and charged to the same polarity as the internal electrode 3 due to the electrostatic field of the internal electrode 3. This "polar charge" attracts the coating liquid toward the first surface 12 of the web 7 during rotational transport, making it possible to form a uniform coating layer 11 on the first surface 12 of the web 7 without creating an air layer between the coating liquid 9 and the first surface 12 of the web 7. The higher the voltage applied to the internal electrode 3, the greater the amount of polar charge accumulated on the first surface 12 due to dielectric polarization of the web 7, and the stronger the electric field, making it possible to significantly increase the coating speed.

[0039] (2) Figures 4 and 5 are side views showing an example of a modified method of the present invention. Figure 5 shows a schematic diagram of the distribution of charges in part B of Figure 4.

[0040] In a modified method of the present invention, a spatial auxiliary electrode 14 is additionally installed at a position upstream of the coating point using the same apparatus configuration as the method of the present invention, and a high voltage of opposite polarity to that of the internal electrode 4 is applied to generate corona discharge, thereby charging the first surface 12 of the web 7 with free charges 19 of opposite polarity to that of the internal electrode layer 3.

[0041] The outermost layer 4 of the backing roll 1 has a maximum withstand voltage of 6 kV and a volume resistivity of 10 7 ~10 13Since the electrical resistance is Ωcm, even if the web to which the electric charge 19 is applied has pinholes or areas with weak insulation resistance, the occurrence of a short-circuit current from the coating liquid at these defective locations to the backing roll 1 is prevented. Therefore, by raising the corona discharge potential of the external auxiliary electrode 14 installed in the space upstream of the coating point as needed, it is possible to increase the amount of free charge 19 on the first surface 12 of the web 7, thereby further significantly increasing the electrostatically assisted coating speed. A DC (-) voltage of 3.5 to 6 kV is sufficiently effective for the external auxiliary electrode, and if it is installed at an appropriate distance from peripheral equipment, spark discharge will not occur.

[0042] Furthermore, the electrostatic force between the charges 17 on the surface of the outermost layer 4 and the charges 19 on the first surface of the web causes the web 7 to adhere more strongly to the surface of the outermost layer 4, completely preventing the intrusion of the entrained air flow to the back side of the web 7. Therefore, in accordance with an increase in the coating speed, the web transport speed can also be increased significantly as needed.

[0043] (3) Because the web 7, which is the adherend of the present invention, is flexible, a uniform and strong adhesive force is required on all contact surfaces between the web 7 and the backing roll 1, without any loose parts. To obtain the electrostatic force required for electrostatic adhesion of the web 7, a voltage of DC (+) 0.3 to 3.5 kV is usually sufficient to apply to the internal electrode layer 3. The higher the applied voltage, the stronger the electrostatic auxiliary effect, and if the applied voltage is 0.3 kV or less, the electrostatic force will be insufficient. Since the withstand voltage of the outermost layer 4 is a maximum of 6 kV or more, no spark discharge will occur even if DC +3.5 kV is applied.

[0044] (4) At least one of the insulating layer 4, the internal electrode layer 3, and the outermost layer 2 of the backing roll 1 is made of a material formed by a thermal spraying method or a material using either an inorganic or organic binder, and at least one of them has been subjected to a sealing treatment.

[0045] Thermal spraying as used in this invention is a coating technology in which a coating material is melted or softened by heating, turned into fine particles, accelerated, and collided with the surface of the object to be coated, whereby the flattened particles are solidified and deposited to form a coating. There are various thermal spraying methods, which are classified according to the type of material and heat source used, but in the case of this invention, atmospheric plasma spraying is particularly suitable.

[0046] Furthermore, when a thermal spray ceramic material is used for the outermost layer 4 and the outermost layer 2, it is preferable that at least one of the insulating layer 2, the internal electrode layer 3, and the outermost layer 4 be subjected to a sealing treatment. A thermal spray ceramic coating is a collection of flattened spray particles, with minute gaps between these particles, forming interconnected pores that account for 3 to 10 vol% of the total volume of the thermal spray coating. In a normal atmospheric environment, humid air or liquid penetrates these pores, resulting in water molecules adsorbing to the pore walls, resulting in extremely low insulation resistance and voltage resistance of the thermal spray coating. By infiltrating the thermal spray ceramic with an insulating sealant, the interconnected pores disappear, resulting in a ceramic material with stable volume resistivity, high voltage resistance, and excellent corrosion resistance. Sealing after coating with a ceramic material is a practical technique that can be performed even on large backing rolls with diameters of 200 mm or more used in actual machines. Materials used for sealing include low-viscosity silicone oligomers (e.g., 8-40 mPas, 25°C), low-viscosity epoxy resins (e.g., 80-400 mPas, 25°C), polyester resins, lithium silicate aqueous solutions for forming inorganic coatings, and metal alkoxides for forming inorganic sols. These liquid sealing agents can be diluted with a solvent to reduce their viscosity. In the present invention, low-viscosity silicone oligomers and low-viscosity epoxy resins are preferred because they exhibit excellent impregnation properties, insulating performance, and voltage resistance. Furthermore, the thickness of the sealing layer is preferably such that the entire sprayed layer is sealed. It is important to penetrate the pores of the sprayed coating with the sealing agent, seal the pores, and then heat-cure the coating to stabilize the volume resistivity and voltage resistance of the sealing agent. Unless the pores within the sprayed coating are properly sealed, it is impossible to adjust the volume resistivity and voltage resistance of the insulating layer 2 and the outermost layer 4 to their original values.

[0047] The volume resistivity of the outermost layer 4 after the sealing treatment at 25 to 100°C is 10 7 ~10 13 Ωcm, preferably 10 8 ~10 12 Ωcm, more preferably 10 9 ~10 12 The volume resistivity is 10 7 If the volume resistivity is less than Ωcm, it will be impossible to prevent the occurrence of short circuit current or spark discharge to peripheral devices from the coating solution connected to the earth through the web 7 in contact with the surface of the backing roll 1. 7 Below this level, it is not preferable because it becomes impossible to carry out electrostatic auxiliary coating by applying a high voltage of 1.5 kV or more to the surface of the back roll and the web.

[0048] On the other hand, the volume resistivity of the outermost layer 4 is 10 13 If the electrical resistance exceeds Ωcm, the outermost layer 4 becomes an insulating dielectric, and substantially no free charges 17 flow from the internal electrode layer 3. As a result, the surface of the outermost layer 4 cannot be charged with free charges 17 of the same polarity as the internal electrode 3, which is undesirable. If the electrical properties of the outermost layer 4 are insulating dielectric, the dipoles 18 are oriented so that the surface direction of the outermost layer 4 becomes charged with the same polarity as the internal electrode 3 due to dielectric polarization caused by the voltage of the internal electrode 3. Here, the charge on the surface of the outermost layer 4 is due to charges fixed to the dipoles and cannot be neutralized and eliminated by free charges. When the web 7 separates from the backing roll, a reverse charge remains on the surface of the outermost layer 4 due to peeling charging. While a voltage is applied to the backing roll, this reverse charge is trapped by the fixed charges at the dipole ends of the outermost layer 4, and although the apparent charge potential decreases, it remains as it is without being eliminated. When the surface of the outermost layer 4 becomes like this, the web 7 is repelled from the surface of the outermost layer 4. That is, the outermost layer 4 has a volume resistivity of 10 13 If the resistivity is higher than Ωcm, the web becomes an insulating dielectric, and the peeling charge of the web remains on the surface without being neutralized, so that the web cannot adhere to the surface of the outermost layer 4, causing problems with the running of the web.

[0049] (5) The outermost layer 4 is made of a ceramic material, and the ceramic material is an alumina-based, zirconium oxide-based, or magnesium oxide-based ceramic containing a compound selected from titanium oxide, chromium oxide, silicon oxide, manganese oxide, nickel oxide, and iron oxide, or an aluminum oxide-based ceramic containing 5 to 17 wt % titanium oxide.

[0050] The material of the outermost layer 4 of the present invention is preferably a material having a volume resistivity of 10 7 ~10 13 It is a material that can be adjusted to Ωcm and has excellent handling properties. In terms of adhesion and density with the internal electrode layer 2, stability of the volume resistivity value, ease of handling, etc., an aluminum oxide ceramic material layer containing 5 to 17 wt %, preferably 7 to 15 wt %, of titanium oxide by thermal spraying is the best.

[0051] (6) In a similar sense, in the present invention, the outermost layer 4 and the insulating layer 2 are also preferably non-oxide ceramic material layers using organic or inorganic binders applied by a coating method. As long as the volume resistivity and withstand voltage can be ensured, the outermost layer 4 and the insulating layer 2 may be coating layers formed by applying a coating material made of a ceramic material containing an organic or inorganic binder and at least one selected from an aluminum nitride, silicon carbide, and silicon nitride binder blended to have a volume resistivity suitable for the present invention.

[0052] (7) The thickness of the outermost layer 4 is preferably 50 μm or more, and more preferably 80 to 500 μm. The lower limit of this thickness is the minimum film thickness necessary to ensure that the outermost layer 4 does not have pinholes or the like penetrating to the internal electrode layer 3, and is the film thickness that can ensure a withstand voltage for the minimum applied voltage necessary for stable adhesion of the web 7. The upper limit of this thickness is set taking into account the maximum applied voltage. To obtain a stronger electrostatic assist effect, a higher applied voltage is required, and it is necessary to increase the thickness of the outermost layer 4 to increase the withstand voltage. However, since a sufficient effect can be obtained with a voltage applied to the internal electrode layer of 3.5 kV, a maximum withstand voltage of 6 kV is sufficient, taking a safety factor into consideration. Increasing the thickness of the outermost layer 4 beyond 500 μm, at which the withstand voltage is obtained, is not preferable because it simply increases the spraying time.

[0053] (8) The surface roughness of the outermost layer 4 of the backing roll 1 of the present invention is a centerline average surface roughness Ra of 0.01 to 5 μm. A smooth surface of less than 0.01 μm is difficult to obtain using current ceramic layer polishing techniques. The greater the surface roughness of the outermost layer 4, the more stable the web travel at high speeds. However, a surface roughness exceeding 5 μm is undesirable because the surface roughness of the outermost layer 4 is transferred to the back surface of the web.

[0054] (9) As the material for the internal electrode layer 3, a sintered conductive paste such as tungsten, molybdenum, high-performance activated carbon, copper, or silver can be used. However, a thermal spray coating of tungsten or molybdenum applied by a plasma spraying method has high thermal conductivity and is also preferable in terms of handling.

[0055] (10) The volume resistivity of the outermost layer 4 is 10 7 ~10 13 Since the internal electrode resistance is as high as Ωcm, even when a high voltage of 6 kV is applied to the internal electrode, the total current flowing from the internal electrode to the web surface is very small, at several mA or less, so that the thickness of the internal electrode layer 3 is sufficient for 5 to 50 μm, and it is preferable that the thickness is as thin as possible in order to smooth the boundaries of the internal electrode 3 at both ends of the roll.

[0056] (11) As the highly insulating material for the insulating layer 2, preferred are ceramic spray coatings made of high-purity alumina of 99.6% or higher or alumina containing 2 to 4 wt% titanium oxide, or coating materials made of ceramic materials selected from magnesium oxide, beryllium oxide (BeO), aluminum nitride (AlN), silicon nitride (Si3N4), etc. Polymer resins selected from polyimide, polyphenylene oxide, polyethylene tetrafluoride (Teflon®), polytrifluorochloroethylene, polyethylene, polypropylene, polystyrene, etc., or SiO2-based glass films such as porcelain and enamel are also acceptable. However, in the present invention, ceramic spray coatings made of high-purity alumina of 99.6% or higher or alumina containing 2 to 4 wt% titanium oxide are most preferred in terms of insulating performance, thermal conductivity, ease of handling, cost, etc.

[0057] (12) The volume resistivity of the insulating layer 2, which is the innermost layer in contact with the core metal 16 of the backing roll 1 of the present invention, is 10 13 It is preferable that the resistance is Ωcm or more in order to reduce the leakage current from the internal electrode layer 3 to the core metal 16 via the insulating layer 2 to an ineffective level.

[0058] (13) The thickness of the insulating layer 2 is preferably 50 to 500 μm, and if it is less than 50 μm, the withstand voltage is insufficient to apply the minimum voltage of 0.3 kV to the internal electrode layer 3 to obtain the necessary adhesion. In order to enable application of a voltage of up to 6 kV to the internal electrode layer, it is desirable that the withstand voltage of the insulating layer 3 be 6 kV or more, and a thickness of 500 μm is sufficient for this withstand voltage.

[0059] (14) Webs used in the present invention include paper, plastic films, resin-coated paper, synthetic paper, etc. Examples of materials for plastic films include polyolefins such as polyethylene and polypropylene, vinyl polymers such as polyvinyl acetate, polyvinyl chloride, and polystyrene, polyamides such as 6,6-nylon and 6-nylon, polyesters such as polyethylene terephthalate and polyethylene-2,6-naphthalate, polycarbonates, and cellulose acetates such as cellulose triacetate and cellulose diacetate. Resins used in resin-coated paper are typically polyolefins such as polyethylene, but are not necessarily limited to these. The web can have one or several pre-coated layers.

[0060] (15) The term "coating liquid" includes various liquid compositions depending on the application, and can be used to form, for example, a photosensitive emulsion layer, undercoat layer, protective layer, backing layer, antistatic layer, or antihalation layer of a photographic material, or an ink-absorbing layer in the case of an inkjet receiving medium. It can also be used to form a magnetic layer, undercoat layer, lubricating layer, protective layer, backing layer, adhesive layer, colored layer, or anticorrosive layer of a magnetic recording medium. These coating liquids can contain a water-soluble binder or an organic binder.

[0061] (16) The surface tension and coatability of the coating solution can be modified using surfactants, such as nonionic surfactants such as polyalkylene oxides and water-soluble adducts of glycidol and alkylphenols, anionic surfactants such as alkylaryl polyether sulfates and sulfonates, amphoteric surfactants such as arylalkyltaurines, N-alkyl and N-acyl β-aminopropionates, saponins, and alkylammonium sulfonate betaines.

[0062] (17) A thickener can be used in the coating liquid to adjust the viscosity.

[0063] (17) Coating applicators to which the present invention can be applied include bead coating applicators, curtain coating applicators, extrusion coating applicators, and slide extrusion coating applicators.

[0064] [Measurement Methods] The methods for measuring physical property values ​​used in the present invention are as follows.

[0065] 1. Centerline Average Roughness Ra When measuring the surface roughness of a backing roll, if measurement was possible while the roll was in its original state, the average roughness Ra of the surface was measured using a portable surface roughness meter. The measuring instrument conformed to JIS B0651, and a stylus with a conical shape with an apex angle of 60 degrees and a spherical tip with a radius of curvature of 2 μm was used. The measuring method conformed to JIS B0601-2013, with a cutoff value of 0.8 mm, to determine the centerline average roughness Ra. The measuring instrument used was a Surfcoder SE1700α from Kosaka Laboratory Co., Ltd.

[0066] 2. Volume Resistivity The volume resistivity of the outermost layer 4 on the surface of the backing roll 1 is measured in accordance with JIS C2141-1992, a test method for ceramic materials for electrical insulation. A main electrode with an outer diameter of 26 mm and a guard electrode with an outer diameter of 48 mm and an inner diameter of 38 mm are cut out from a conductive adhesive sheet and attached to the curved surface of the outermost layer 4 so that the guard electrode and main electrode are concentric, conforming to the three-terminal method of JIS C2141. A conductor with terminals attached with conductive adhesive tape is used at the contact points on the surfaces of the main electrode and guard electrode. The internal electrode layer 3 of the backing roll is used as the counter electrode. The value measured one minute after the start of measurement is adopted. The measuring instrument used was a Super Insulation Meter R-503 manufactured by Kawaguchi Electric Works. A DC voltage of 500 V is applied between the main electrode and the internal electrode layer 3 and the guard electrode, and the volume resistance R is calculated from the current value I (A) flowing between the main electrode and the counter electrode (internal electrode layer 3). V (= V / I) was calculated, and the volume resistivity ρ was calculated using the following formula: V Calculate.

[0067] ρ V (Ω cm) = R V × A / d A = π × D 2 / 4 where, V: applied voltage (V) R V : Volume resistance (Ω) ρ V : volume resistivity (Ωcm) A: area of ​​main electrode (cm 2 ) D: outer diameter of main electrode (cm) d: thickness of outermost layer (cm) The thickness d was measured using a magnetic or eddy current thickness meter. The measuring instrument used was a magnetic / eddy current dual thickness meter FMP20 manufactured by Fischer Instruments.

[0068] Example 1 In the method of FIG. 1, a web 7 was continuously transported to a backing roll 1, and a DC voltage was applied only to the internal electrode 3 of the backing roll, thereby carrying out electrostatically assisted curtain coating according to the method of the present invention.

[0069] The backing roll 1 used here was produced as follows.

[0070] The entire surface of the center of the cylindrical core 16 made of steel and having a diameter of 200 mm was sandblasted, and then a 50 μm thick 80 wt % Ni / 20 wt % Cr alloy was deposited by plasma spraying as a bonding layer to improve the adhesion of the ceramic layer. Subsequently, aluminum oxide (alumina) (99.6 wt % Al) was deposited as a highly insulating material on the surface of the bonding layer. 2 O 3 ) was laminated to a thickness of 250 μm by plasma spraying, and then the sprayed alumina layer was sealed with a low viscosity epoxy resin to obtain a volume resistivity of 10 14 An insulating layer 2 having a resistance of Ωcm or more was formed. Tungsten (W) having a thickness of 30 μm was laminated on the insulating layer 2 by plasma spraying to form the internal electrode layer 3. At this time, a 20 mm wide area was masked from both ends in the width direction of the backing roll 1 so that the internal electrode layer 3 would not be formed in this area. After removing the masks on both ends, titanium oxide (TiO 2 ) 10 wt %, and the remaining 90 wt % is alumina (Al 2 O 3An alumina-based ceramic material consisting of tungsten) was laminated by plasma spraying to a thickness of 400 μm as the outermost layer 4. Similarly, the alumina-based ceramic material layer was sealed together with the tungsten layer of the internal electrode layer 3 with a low viscosity epoxy resin, resulting in a volume resistivity of 5.6×10 10 An outermost layer 4 having a resistance of Ωcm was obtained.

[0071] The outermost layer 4 after the sealing treatment was polished with a diamond grinding wheel to a residual thickness of 300 μm and a surface roughness Ra of 0.05 μm after polishing. To enable electrical connection to the internal electrode layer 3, a rectangular mask of 20 mm x 30 mm was applied to one end of the roll during thermal spraying of the outermost layer 4, and after thermal spraying of the outermost layer 4, the internal electrode layer 3 was exposed at the end of the roll in a width of 20 mm x 10 mm. A slip ring 6 was connected to the exposed internal electrode layer 3. A DC high-voltage power supply 5 was connected to the slip ring 6, and a DC voltage of (+) 3.5 kV was applied to the internal electrode 3. When a voltage was applied to the internal electrode, no current was felt by the human body even when the surface of the outermost layer 4 was touched with a finger.

[0072] The web 7 was a 100 μm thick polyethylene terephthalate film with a 0.3 μm thick gelatin undercoat layer formed thereon. The web 7 was placed in a heating furnace at a temperature of 90 to 100° C., and its front and back surfaces were alternately brought into contact with grounded rolls to remove charge until the surface potential reached ±50 V or less. The web was then cooled to 25° C.

[0073] The gelatin composition was applied so that the thickness of the wet coating layer 11 would be 60 μm, with a curtain height of the coating solution 9 of 10 cm, a coating angle of 30° forward from the top of the roll, a tension of 150 N / m on the web 7, and a conveying speed of 400 m / min for the web 7. The coating solution used was a 15% aqueous gelatin solution containing 0.1% sodium dodecyl benzene sulfonate, and the low shear viscosity was adjusted to 100 mPa s with a thickener. The flow rate of the coating solution was set to 4 cc / sec per cm of coating width.

[0074] The back surface 12 of the web 7 was in close contact with the surface of the backing roll 1, and the web ran stably. Coating continued without any coating problems due to the air layer accompanying the surface of the web 7 being drawn under the coating liquid, and the wet coating layer 11 had good thickness uniformity and a smooth surface. No spark discharge occurred from the backing roll to the surroundings, and no short-circuit current was generated that penetrated the web 7 from the coating liquid 9 toward the roll surface.

[0075] Comparative Example 1 When coating was performed under the same configuration and conditions as in Example 1, with the voltage to the internal electrode 3 set to 0 (zero), the entrained air layer could not be eliminated by the curtain of coating liquid 9 alone, and the coating liquid did not wet the surface 12 of the web 7, making uniform coating impossible. In addition, the web 7 floated up from the backing roll, and the traction force of the backing roll 1 on the web 7 decreased, causing fluctuations in the tension and speed of the web 7 and making the running unstable, making it impossible to continue coating.

[0076] Example 2 In the same coating apparatus as in Example 1, a web 7 was transported around a backing roll 1 having a diameter of 200 mm, a voltage of +3.5 kV was applied to the internal electrode 3, and a tungsten wire electrode 14 having a diameter of 0.5 mm was additionally installed at a distance of 10 mm from the web as shown in FIG. 2, and a voltage of −3 kV was applied to the internal electrode 3, so that a negative charge (−) was deposited from the electrode 14 onto the first surface of the web 7, thereby performing electrostatically assisted curtain coating according to a modified method of the present invention.

[0077] The web 7 is a polyethylene-coated paper having a thickness of 100 μm, and is coated with a gelatin undercoat layer having a thickness of 0.6 μm. The web 7 has been placed in a heating furnace at a temperature of 90 to 100° C., where the back and front surfaces are alternately brought into contact with grounded rolls to remove charge until the surface potential is reduced to ±50 V or less, and then cooled to 25° C.

[0078] The gelatin composition was applied to a wet thickness of 35 μm at a curtain height of 10 cm, a coating angle of 30° forward from the roll apex, a web 7 tension of 150 N / m, and a web conveying speed of 400 m / min. The coating solution 9 was a 12% aqueous gelatin solution containing 0.1% sodium dodecyl benzene sulfonate. The low-shear viscosity was adjusted to 21 mPa·s using a thickener, and the flow rate of the coating solution was set to 2.3 cc / sec per cm of coating width. The second surface 13 of the web 7 was in close contact with the surface of the backing roll 1, and running was stable. The first surface 12 of the web 7 was able to continue coating stably without causing coating problems due to entrainment of the accompanying air layer into the coating solution, and the thickness uniformity of the wet coating layer 11 and surface smoothness were both good. No spark discharge or glow discharge occurred from the backing roll to the surroundings, and no short-circuit current was generated from the coating solution 9 through the web 7 toward the roll surface.

[0079] (Comparative Example 2) When coating was performed under the same configuration conditions as in Example 2 with the voltage to the internal electrode 3 set to 0 (zero), the coating liquid 9 was able to form a wet coating layer 11 that adhered closely to the entire first surface 12 of the web. However, an entrained air layer entered between the back surface 13 of the web and the backing roll, causing the web 7 to float, which resulted in unstable tension and speed of the web 7, causing it to vibrate and run unstably, making it impossible to continuously form a wet coating layer 11 with a smooth surface.

[0080] REFERENCE SIGNS LIST 1 Backing roll 2 Insulating layer 3 Internal electrode (+) 4 Outermost layer 5 DC high-voltage power supply (for internal electrode) 6 Slip ring 7 Strip-shaped support (web) 8 Applicator (coating head) 9 Curtain of coating liquid 10 Coating liquid contact line (coating point) 11 Wet coating layer 12 Web first surface (front surface) 13 Web second surface (back surface) 14 Spacing auxiliary electrode (-) 15 DC high-voltage power supply (for spacing auxiliary electrode) 16 Roll core metal 17 Free charge (+) 18 Dipole inside web 19 Surface charge (-)

Claims

1. A method for applying a coating liquid comprising a liquid composition to a first surface of a continuously moving flexible plastic web having first and second opposing surfaces by flowing the coating liquid from a grounded applicator onto the first surface of the web, the method comprising the steps of: conveying the web along a path to a backing roll for coating, and passing the web through a coating point while supporting the second surface of the web by the electrostatic field of the backing roll, which is rotating and to which a DC voltage is applied; and attracting the coating liquid at the coating point and applying it to the first surface of the web by electrostatic force generated by the coordination of charges of the same polarity as the DC voltage applied to the backing roll on the first surface of the web, the backing roll comprising an outermost layer to which the web is in close contact, a conductive monopolar internal electrode layer adjacent to the inner side of the outermost layer, and an insulating layer adjacent to the inner side of the internal electrode layer, the backing roll being configured to be able to apply a predetermined voltage to the internal electrode layer, the outermost layer having a volume resistivity of 10 7 ~10 13 a ceramic material layer of Ωcm, the surface of the backing roll being charged with a charge of the same sign as the voltage applied to the internal electrode layer in a state in which the predetermined voltage is applied to the internal electrode layer, the second surface of the web in contact with the outermost layer by the electrostatic force of the charge is brought into close contact with the outermost layer and rotated and transported, and the coating liquid is attracted to and brought into contact with a first surface of the web during rotation and transport, and deposited on the first surface of the web.

2. The coating method according to claim 1, wherein a charge having a polarity opposite to that of the DC voltage applied to the internal electrode layer is applied to a first surface of the web opposite to the second surface before the coating liquid comes into contact with the web during rotational transport.

3. The coating method according to claim 1, wherein the DC voltage applied to the internal electrode layer is 0.3 to 6.0 KV.

4. The coating method according to claim 1, wherein the diameter of the backing roll is 100 mm or more.

5. The coating method according to claim 1, wherein at least one of the insulating layer, the internal electrode layer, and the outermost layer is made of a material formed by a thermal spraying method or a material using either an inorganic or organic binder, and at least one of the insulating layer, the internal electrode layer, and the outermost layer of the backing roll is subjected to a sealing treatment.

6. The coating method according to claim 1, wherein the outermost layer is made of a ceramic material, and the ceramic material is an alumina-based, zirconium oxide-based, or magnesium oxide-based ceramic containing a compound selected from titanium oxide, chromium oxide, silicon oxide, manganese oxide, nickel oxide, and iron oxide, or an aluminum oxide-based ceramic containing 5 to 17% by weight of titanium oxide.

7. The coating method according to claim 1, wherein the outermost layer is made of a ceramic material, the ceramic material containing at least one selected from aluminum nitride, silicon carbide, and silicon nitride, and an organic or inorganic binder.

8. The coating method according to claim 1, wherein the outermost layer has a thickness of 50 to 500 μm.

9. The coating method according to claim 1, wherein the center line average surface roughness Ra of the outermost layer of the backing roll is 0.01 μm to 5 μm.

10. The coating method according to claim 1, wherein the internal electrode layer is made of a conductive material containing tungsten or molybdenum.

11. The coating method according to claim 1, wherein the internal electrode layer has a thickness of 5 to 50 μm.

12. The coating method according to claim 1, wherein the insulating layer comprises at least one highly insulating material selected from the group consisting of aluminum oxide, aluminum oxide-based materials containing 2 to 4 weight percent titanium oxide, magnesium oxide-based materials, beryllium oxide-based materials, aluminum nitride-based materials, and ceramic materials containing silicon nitride, porcelain, and enamel.

13. The volume resistivity of the insulating layer is 10 13 The coating method according to claim 1 , wherein the resistivity is Ωcm or more.

14. The coating method according to claim 1, wherein the insulating layer has a thickness of 50 to 500 μm.

Citation Information

Patent Citations

  • Digital recorder

    JP1989035702A

  • Production of alkylarsine compound

    JP1994009671A

  • Method for curtain-coating support with composition

    JP1996252517A

  • High speed coating method and equipment

    JP2509316B2

  • Application method

    JP2835659B2