Capacitor, electrical circuit, circuit board, and apparatus
The capacitor design with a nitrogen-containing cation in the APb2X5 dielectric material addresses the limitations of oxide dielectrics by enhancing solubility and uniformity, achieving high withstand voltage and cost-effective production.
Patent Information
- Application Number
- PCT/JP2024/013889
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-04-04
- Publication Date
- 2024-11-21
AI Technical Summary
Conventional capacitors using oxide dielectrics face challenges such as high manufacturing costs due to high-temperature synthesis, low elastic constants, and difficulty in increasing filling rates, as well as low solubility of inorganic halide dielectrics leading to non-uniform films and leakage currents under electric fields, which limits their withstand voltage.
A capacitor design utilizing a dielectric material APb2X5 with a cation containing a nitrogen atom, which enhances solubility and uniformity, allowing for high withstand voltage, and potentially lower manufacturing costs through low-temperature synthesis and flexible film formation.
The capacitor achieves high withstand voltage and improved performance by ensuring a uniform dielectric film, reducing leakage currents and enabling higher capacitance and flexibility, while potentially lowering production costs.
Smart Images

Figure JP2024013889_21112024_PF_FP_ABST
Abstract
Description
Capacitors, electric circuits, circuit boards, and devices
[0001] The present disclosure relates to capacitors, electric circuits, circuit boards, and devices.
[0002] Traditionally, halides have been used in devices such as perovskite solar cells.
[0003] For example, Patent Document 1 describes a ferroelectric memory element having a ferroelectric layer sandwiched between a pair of electrodes. The ferroelectric layer contains a predetermined halide-based organic-inorganic hybrid perovskite compound or an inorganic perovskite compound. Examples of halide-based organic-inorganic hybrid perovskite compounds include CH3NH3PbI3, CH5NH3PbI4, CH3NH3SnI3, and CH5NH3SnI4. Examples of inorganic perovskite compounds include CsSnI3.
[0004] JP 2016-171152 A
[0005] The present disclosure provides a capacitor that is advantageous in terms of high withstand voltage.
[0006] The capacitor of the present disclosure includes a first electrode, a second electrode, and a dielectric disposed between the first and second electrodes, the dielectric including a crystal having a composition of APb2X5, where A is a cation that is a molecular ion containing a nitrogen atom, and X is a halogen element.
[0007] According to the present disclosure, a capacitor that is advantageous from the viewpoint of high withstand voltage can be provided.
[0008] FIG. 1 is a cross-sectional view showing an example of a capacitor according to the present disclosure. FIG. 2A is a diagram showing the crystal structure of CsPbBr. FIG. 2B is a diagram showing the crystal structure of (NH)PbBr. FIG. 3A is a diagram showing the crystal structure of CsPbBr. FIG. 3B is a diagram showing the crystal structure of CsPbBr. FIG. 4A is a diagram showing the crystal structure of CsPbBr. FIG. 4B is a diagram showing the crystal structure of CsPbBr. FIG. 4C is a diagram showing the crystal structure of CsPbBr. FIG. 5A is a cross-sectional view showing another example of a capacitor according to the present disclosure. FIG. 5B is a cross-sectional view showing yet another example of a capacitor according to the present disclosure. FIG. 5C is a cross-sectional view showing yet another example of a capacitor according to the present disclosure. FIG. 6A is a diagram schematically showing an example of an electric circuit according to the present disclosure. FIG. 6B is a diagram schematically showing an example of a circuit board according to the present disclosure. FIG. 6C is a diagram schematically showing an example of a device according to the present disclosure. Fig. 7 is a graph showing an XRD pattern of a dielectric material included in a capacitor according to Example 1. Fig. 8 is a graph showing the relationship between polarization and electric field strength in a capacitor according to Example 1. Fig. 9 is a graph showing the relationship between polarization and electric field strength in a capacitor according to Comparative Example 1. Fig. 10 is a graph showing the relationship between polarization and electric field strength in a capacitor according to Comparative Example 2.
[0009] (Findings underlying the present disclosure) In recent years, electronic devices have become smaller and more highly functional, leading to advances in miniaturization, higher integration, and higher operating frequencies for electronic circuits. Similarly, miniaturization and higher performance are also required for electronic components used in electronic circuits. For example, providing a small capacitor with high capacitance would contribute to the miniaturization and higher performance of electronic components. Capacitance depends on the relative dielectric constant of the dielectric used in the capacitor; the higher the relative dielectric constant, the greater the capacitance. Capacitors using oxide dielectrics have been widely developed as dielectrics exhibiting high relative dielectric constants. However, synthesizing oxides often requires firing at high temperatures of 500°C or higher, which increases the manufacturing costs of capacitors. Furthermore, oxides often have a small elastic constant, making it difficult to increase the packing density of a powder-pressed compact. This makes it difficult to improve capacitor performance. Additionally, oxides are unlikely to have high strength against bending stress.
[0010] Halides have the potential to overcome these disadvantages of oxides. Halides generally have high solubility in water and organic solvents, making them easy to synthesize by coating methods. Furthermore, because halides can be synthesized at low temperatures below 200°C, it is expected that capacitor manufacturing costs can be reduced. Furthermore, halides can be formed on substrates such as films that are not highly resistant to high temperatures, which is expected to lead to the realization of flexible capacitors. Meanwhile, according to the inventors' research, conventional halide dielectrics are composed of inorganic elements, and therefore have low solubility in solvents. Therefore, when a coating film containing a halide dielectric is formed by a coating method such as spin coating, the film tends to become nonuniform. Nonuniformity in the film can cause leakage current under an electric field. Thus, it has been discovered that conventional coating films containing halide dielectrics have the problem of being difficult to increase their withstand voltage.
[0011] In light of these circumstances, the present inventors have conducted extensive research into whether it is possible to increase the breakdown voltage of a film containing a halide by incorporating a molecular ion as a part of the cation in the halide. As a result, the present inventors have newly discovered that the breakdown voltage of a halide containing a specific molecular ion, a cation, and lead is likely to be increased. Based on this new finding, the present inventors have devised the capacitor of the present disclosure.
[0012] (Embodiments) Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. The present disclosure is not limited to the following embodiments.
[0013] Fig. 1 is a cross-sectional view showing an example of a capacitor according to the present disclosure. As shown in Fig. 1, a capacitor 1a includes a first electrode 11, a second electrode 12, and a dielectric 20. The dielectric 20 is disposed between the first electrode 11 and the second electrode 12. The dielectric 20 includes a crystal having a composition of APb2X5. In this composition, A is a cation that is a molecular ion containing a nitrogen atom, and X is a halogen element.
[0014] The solubility of cation A in the solvent tends to be high. As a result, dielectric 20 tends to exist uniformly between first electrode 11 and second electrode 12, and capacitor 1a tends to have a high withstand voltage.
[0015] Figure 2A shows the crystal structure of CsPb2Br5. Figure 2B shows the crystal structure of (NH4)Pb2Br5. CsPb2Br5 is Cs + , Pb 2+ , and Br - On the other hand, (NH4)Pb2Br5 is composed of inorganic ions, + is NH4 + It has a cation-substituted structure. Halide raw materials that do not contain molecular ions, such as CsPbBr, tend to have low solubility in solvents. For example, even if 0.5 millimoles (mmol) of CsBr and 1 mmol of PbBr are added to 1 ml of a mixed solvent of dimethyl sulfoxide (DMSO) and N,N-dimethylformamide (DMF) and heated at 80°C for 1 hour, the raw materials remain insoluble and do not completely dissolve, resulting in a cloudy solution. Therefore, when this solution is used to form a film using a coating method such as spin coating, an inhomogeneous film is obtained. Inhomogeneity in the film can cause leakage current under an electric field. Since CsBr has low solubility in solvents, it is thought that an inhomogeneous film will be obtained. On the other hand, for example, NHBr, which contains molecular ions containing nitrogen atoms, instantly dissolves in solvents, and even when NHBr is added to a solvent at the same molar concentration as the CsBr in the CsBr-containing solution, a colorless, transparent solution is obtained. In this way, when A in dielectric 20 of capacitor 1a is a molecular ion containing a nitrogen atom, dielectric 20 tends to exist in a uniform state, and capacitor 1a tends to have a high withstand voltage.
[0016] The cation A in the above composition may contain only nitrogen and hydrogen atoms, or may further contain carbon atoms.
[0017] The cation A in the above composition is, for example, an ammonium ion represented by the following formula (I): 1 , R 2 , R 3 , and R4 are each independently a hydrogen atom, an alkyl group, an aryl group, or NH2. In this case, the solubility of the cation A, which is a molecular ion, in the solvent tends to be high, and the capacitor 1a tends to have a high withstand voltage.
[0018]
[0019] In formula (I), R 1 and R 2 are each independently a hydrogen atom, an alkyl group, or an aryl group, and R 3 and R 4 may be a hydrogen atom. In this case, the solubility of the cation A, which is a molecular ion, in the solvent tends to be high, and the capacitor 1a tends to have a high withstand voltage.
[0020] In formula (I), R 1 , R 2 , R 3 , and R 4 may be a hydrogen atom. In this case, the solubility of the cation A, which is a molecular ion, in the solvent tends to be high, and the capacitor 1a tends to have a high withstand voltage.
[0021] In formula (I), for example, R 1 is NH2, and R 2 , R 3 , and R 4 may be a hydrogen atom. In this case, the solubility of the cation A, which is a molecular ion, in the solvent tends to be high, and the capacitor 1a tends to have a high withstand voltage.
[0022] The cation A in the above composition is an ammonium ion represented by formula (I) above, and R 1 , R 2 , R 3 , or R 4 When is an alkyl group, the alkyl group is not limited to a specific alkyl group. For example, the number of carbon atoms in the alkyl group is 1 to 20. At least one hydrogen atom in the alkyl group may be substituted or unsubstituted.
[0023] The alkyl group may be a saturated radical having a straight or branched chain. At least one hydrogen atom in the saturated radical may be substituted or unsubstituted. The alkyl group is, for example, a saturated hydrocarbon radical having a straight or branched chain and having 1 to 20 carbon atoms. At least one hydrogen atom in the saturated hydrocarbon radical may be substituted or unsubstituted. The alkyl group may be an alkyl group having 1 to 20 carbon atoms. Examples of such alkyl groups are methyl, ethyl, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, and decyl. The alkyl group may be an alkyl group having 1 to 6 carbon atoms. Examples of such alkyl groups are methyl, ethyl, propyl, butyl, pentyl, and hexyl. The alkyl group may be an alkyl group having 1 to 4 carbon atoms. Examples of such alkyl groups are methyl, ethyl, i-propyl, n-propyl, t-butyl, s-butyl, n-butyl, and pentyl.
[0024] When at least one hydrogen atom in the alkyl group is replaced by a substituent, the substituent may include, for example, one or more substituents selected from the group consisting of an alkyl group, an aryl group, a cyano group, and an amino group. The alkyl group may have 1 to 20 carbon atoms. At least one hydrogen atom in the alkyl group may be substituted or unsubstituted. At least one hydrogen atom in the aryl group may be substituted or unsubstituted. Examples of the substituent include alkylamino groups, dialkylamino groups, arylamino groups, diarylamino groups, arylalkylamino groups, amido groups, acylamide groups, hydroxy groups, oxo groups, halo groups, carboxy groups, ester groups, acyl groups, acyloxy groups, alkoxy groups, aryloxy groups, haloalkyl groups, sulfonic acid groups, sulfhydryl groups, alkylthio groups, arylthio groups, sulfonyl groups, phosphate groups, phosphate ester groups, phosphonic acid groups, and phosphonate ester groups. Examples of the substituted alkyl group include haloalkyl groups, hydroxyalkyl groups, aminoalkyl groups, alkoxyalkyl groups, and alkaryl groups. An alkaryl group is, for example, an alkyl group having 1 to 20 carbon atoms in which at least one hydrogen atom is replaced by an aryl group. The alkaryl group is not limited to a specific alkaryl group. Examples of alkaryl groups include benzyl, benzhydryl, trityl, phenethyl, styryl, and cinnamyl groups.
[0025] The cation A in the above composition is an ammonium ion represented by formula (I) above, and R 1 , R 2 , R 3 , or R 4When is an aryl group, the aryl group is not limited to a specific aryl group. The aryl group may be, for example, a monocyclic or bicyclic aromatic group. The aryl group may have a ring structure containing, for example, 6 to 14 carbon atoms, and preferably a ring structure containing 6 to 10 carbon atoms. At least one hydrogen atom in the aryl group may be substituted or unsubstituted. Examples of aryl groups include a phenyl group, a naphthyl group, an indenyl group, and an indanyl group. When the aryl group is substituted, the aryl group may have one or more substituents selected from the group consisting of an unsubstituted alkyl group having 1 to 6 carbon atoms, an unsubstituted aryl group, a cyano group, an amino group, an alkylamino group, a dialkylamino group having 1 to 10 carbon atoms, an arylamino group, a diarylamino group, an arylalkylamino group, an amido group, an acylamide group, a hydroxy group, a halo group, a carboxy group, an ester group, an acyl group, an acyloxy group, an alkoxy group having 1 to 20 carbon atoms, an aryloxy group, a haloalkyl group, a sulfhydryl group, an alkylthio group having 1 to 10 carbon atoms, an arylthio group, a sulfonic acid group, a phosphoric acid group, a phosphoric acid ester group, a phosphonic acid group, a phosphonic acid ester group, and a sulfonyl group. The aryl group may have no substituent, one substituent, two substituents, or three substituents. A substituted aryl group may be a single alkylene group having 1 to 6 carbon atoms, or a group represented by the formula -X-R 9 -or-X-R 9 It may be substituted at the 2-position with a bidentate group represented by -X-. 9 is an alkylene group having 1 to 6 carbon atoms; X is O, S, and NR 10 R is selected from the group consisting of 10is a hydrogen atom, an aryl group, or an alkyl group having 1 to 6 carbon atoms. A substituted aryl group may be an aryl group fused with a cycloalkyl group or an aryl group fused with a heterocyclyl group. The ring atoms of the aryl group may contain one or more heteroatoms, as in a heteroaryl group. Such heteroaryl groups are substituted or unsubstituted monocyclic or bicyclic heteroaromatic groups containing 6 to 10 atoms in the ring portion including one or more heteroatoms. The heteroaryl group may, for example, be a five- or six-membered ring and contain at least one heteroatom selected from O, S, N, P, Se, and Si. The heteroaryl group may, for example, contain one, two, or three heteroatoms. Examples of heteroaryl groups include pyridyl, pyrazinyl, pyrimidinyl, pyridazinyl, furanyl, thienyl, pyrazolidinyl, pyrrolyl, oxazolyl, oxadiazolyl, isoxazolyl, thiadiazolyl, thiazolyl, isothiazolyl, imidazolyl, pyrazolyl, quinolyl, and isoquinolyl groups. Heteroaryl groups can be unsubstituted or substituted, for example, as described above for aryl groups. Heteroaryl groups can have zero, one, two, or three substituents.
[0026] In formula (I), R 1 , R 2 , R 3 , and R 4 Each of R is independently, for example, a hydrogen atom, NH, a methyl group, or an ethyl group. 1 , R 2 , R 3 , and R 4 may independently be a hydrogen atom, NH2, or a methyl group.
[0027] The lead ions in the dielectric 20 have, for example, lone pairs of electrons. A lone pair is an electron pair formed by two electrons belonging to a specific atom, and is not shared with other atoms. For example, Pb 2+ The ion has a lone pair of electrons. 2+In the ions, two electrons have been taken from Pb, and the two electrons filling the s orbital of the outermost shell form a lone pair. Electrons forming a lone pair are less likely to bond with surrounding ions, and may cause an unstable electronic state or a special crystal structure. Therefore, if the lead ions in the dielectric 20 have lone pairs, the dielectric constant of the dielectric 20 tends to be high. On the other hand, as lead ions, Pb 2+ In addition to ions, Pb 4+ ions may also be present. 4+ In the Pb ion, four electrons are removed from the Pb, and the outermost s orbital is empty. 4+ The ions do not have lone pairs of electrons. In this case, a crystal structure with a low coordination number is easily formed, and the relative dielectric constant of the material is unlikely to increase.
[0028] For example, all of the lead ions in the dielectric 20 may have lone pairs of electrons, or only some of the lead ions in the dielectric 20 may have lone pairs of electrons.
[0029] X in the dielectric 20 includes, for example, at least one selected from the group consisting of F, Cl, Br, and I. In this case, the dielectric 20 is more likely to have a high relative dielectric constant.
[0030] The dielectric 20 has, for example, an inverse perovskite structure. With such a structure, the dielectric 20 is more likely to have a high relative dielectric constant.
[0031] The reversed perovskite structure is a structure in which the arrangement of cations and anions in a normal perovskite compound is reversed. In other words, the positive and negative charges of ions occupying specific sites in the perovskite compound are reversed to the positive and negative charges of ions occupying those specific sites in the reversed perovskite compound.
[0032] 3A and 3B are diagrams showing the crystal structure of CsPbBr3. FIG. 3B is a diagram showing the crystal structure shown in FIG. 3A viewed along the negative c-axis direction. CsPbBr3 has a perovskite structure. FIGS. 4A, 4B, and 4C are diagrams showing the crystal structure of CsPb2Br5. FIG. 4B is a diagram showing the crystal structure of CsPb2Br5 represented by a coordination polyhedron centered on an anion. FIG. 4C is a diagram showing the crystal structure shown in FIG. 4B viewed along the negative c-axis direction. CsPb2Br5 has an inverse perovskite structure. As shown in FIG. 3A, in CsPbBr3, Cs is located at the A site of the perovskite structure, Pb is located at the B site, and Br is located at the X site. 4B, in CsPbBr, Br is located at the site corresponding to the A site of the perovskite structure, Br is located at the site corresponding to the B site, and Cs or Pb is located at the site corresponding to the X site. In other words, CsPbBr is expressed as (Br)Br(CsPb) in the notation ABX.
[0033] When the dielectric 20 containing a crystal having a composition of APbX has an inverse perovskite structure, for example, Cs is substituted with a cation A, which is a molecular ion, in the crystal structure shown in FIG. 4B. In the inverse perovskite structure shown in FIG. 4B, cations are arranged at the vertices of multiple octahedra that share vertices, and there is a site where an anion is arranged at the center of the octahedron. This makes it easier for ions to align along a straight line in the inverse perovskite structure, and polarization is likely to increase. This makes it easier for the dielectric 20 to have a high relative dielectric constant.
[0034] The anti-perovskite structure of halides having the composition APb2X5 includes NH4Pb2Br5 type structure, Cs3CoCl5 type structure, La2CuSbS5 type structure, La4FeSb2S 10 The structure may be a Ba4In2Te2S5 type structure, a Y2HfS5 type structure, or a TlPb2Cl5 type structure.
[0035] The dielectric constant of the dielectric 20 is not limited to a specific value. The dielectric constant of the dielectric 20 at room temperature is, for example, 30 or more at 1 MHz, and may be 35 or more, 40 or more, 45 or more, 50 or more, 60 or more, 70 or more, 80 or more, 90 or more, or 100 or more. The room temperature is, for example, a specific temperature in the range of 20° C. to 25° C. The dielectric constant of the dielectric 20 at room temperature is, for example, 10,000 or less at 1 MHz. In other words, the dielectric constant of the dielectric 20 at room temperature is, for example, 30 or more and 10,000 or less at 1 MHz.
[0036] As shown in FIG. 1 , in the capacitor 1 a, the dielectric 20 is formed as, for example, a film. The method for disposing the dielectric 20 on the capacitor 1 a is not limited to a specific method. The dielectric 20 may be formed by, for example, spin coating, inkjet, die coating, roll coating, bar coating, Langmuir-Blodgett, dip coating, or spray coating. This makes it easier for the dielectric 20 to exist uniformly between the first electrode 11 and the second electrode 12, and makes it easier for the capacitor 1 a to have a high withstand voltage. The dielectric 20 may be formed by sputtering, anodization, vacuum evaporation, pulsed laser deposition (PLD), atomic layer deposition (ALD), or chemical vapor deposition (CVD).
[0037] 1 , the dielectric 20 is disposed, for example, between the first electrode 11 and the second electrode 12 in the thickness direction of the dielectric 20. The second electrode 12 covers, for example, at least a portion of the dielectric 20.
[0038] The materials forming the first electrode 11 and the second electrode 12 are not limited to a specific material. Each of the first electrode 11 and the second electrode 12 includes, for example, a metal. The first electrode 11 includes, for example, a valve metal. Examples of the valve metal are Al, Ta, Nb, Pb, Sn, and Bi. The first electrode 11 includes, for example, at least one valve metal selected from the group consisting of Al, Ta, Nb, Pb, Sn, and Bi. The first electrode 11 may include a noble metal such as gold or platinum, nickel, or a metal element of Group 13, Group 14, or Group 15.
[0039] The second electrode 12 may contain, for example, a valve metal such as Al, Ta, Nb, Pb, Sn, or Bi, or may contain a noble metal such as gold, silver, or platinum, or may contain nickel, or may contain a metal element of Group 13, Group 14, or Group 15. The second electrode 12 contains, for example, at least one selected from the group consisting of Al, Ta, Nb, Bi, gold, silver, platinum, and nickel.
[0040] 1 , the first electrode 11 has a principal surface 11p. One principal surface of the dielectric 20 is in contact with the principal surface 11p, for example. The second electrode 12 has a principal surface 12p parallel to the principal surface 11p. The other principal surface of the dielectric 20 is in contact with the principal surface 12p, for example.
[0041] 5A is a cross-sectional view showing another example of a capacitor according to the present disclosure. Capacitor 1b shown in FIG. 5A is configured similarly to capacitor 1a, except for portions that will be particularly described. Components of capacitor 1b that are identical to or correspond to components of capacitor 1a are given the same reference numerals, and detailed descriptions are omitted. The description of capacitor 1a also applies to capacitor 1b, unless technically inconsistent. The same also applies to capacitors 1c and 1d, which will be described later.
[0042] The capacitor 1b shown in Fig. 5A is an electrolytic capacitor. As shown in Fig. 5A, in the capacitor 1b, at least a portion of the first electrode 11 is porous. With this configuration, the surface area of the first electrode 11 tends to be large, and the capacitor 1b tends to have a higher capacitance. Such a porous structure can be formed by, for example, etching a metal foil and sintering a powder.
[0043] 5A , for example, a film of a dielectric 20 is formed on the surface of the porous portion of the first electrode 11. The dielectric 20 can be formed by, for example, spin coating, inkjet, die coating, roll coating, bar coating, Langmuir-Blodgett, dip coating, or spray coating. The dielectric 20 may also be formed by, for example, sputtering, anodization, vacuum deposition, PLD, ALD, or CVD.
[0044] The first electrode 11 contains a valve metal such as Al, Ta, Nb, Zr, Hf, Pb, Sn, or Bi. The second electrode 12 may contain, for example, a solidified silver-containing paste, a carbon material such as graphite, or both the solidified silver-containing paste and a carbon material.
[0045] In capacitor 1b, for example, electrolyte 13 is disposed between first electrode 11 and second electrode 12. More specifically, electrolyte 13 is disposed between dielectric 20 and second electrode 12. In capacitor 1b, for example, second electrode 12 and electrolyte 13 form cathode 15. In capacitor 1b, electrolyte 13 is disposed so as to fill voids around the porous portion of first electrode 11, for example.
[0046] The electrolyte 13 includes, for example, at least one selected from the group consisting of an electrolytic solution and a conductive polymer. Examples of the conductive polymer include polypyrrole, polythiophene, polyaniline, and derivatives thereof. The electrolyte 13 may be a manganese compound such as manganese oxide. The electrolyte 13 may also include a solid electrolyte.
[0047] The electrolyte 13 containing a conductive polymer can be formed by chemically polymerizing, electrolytically polymerizing, or both chemically and electrolytically polymerizing a raw material monomer on the dielectric 20. The electrolyte 13 containing a conductive polymer may also be formed by depositing a solution or dispersion of the conductive polymer on the dielectric 20.
[0048] 5B is a cross-sectional view showing yet another example of a capacitor according to the present disclosure. In the capacitor 1c shown in FIG. 5B, at least a portion of the first electrode 11 is porous. This configuration tends to increase the surface area of the first electrode 11, and the capacitor 1c tends to have a higher capacitance. Such a porous structure can be formed by, for example, etching a metal foil and sintering a powder.
[0049] 5B , for example, a film containing the dielectric 20 is formed on the porous portion of the first electrode 11. Examples of methods that can be used to form the film containing the dielectric 20 include spin coating, inkjet coating, die coating, roll coating, bar coating, Langmuir-Blodgett coating, dip coating, and spray coating. In the capacitor 1c, the dielectric 20 is disposed so as to fill the voids around the porous portion of the first electrode 11, for example.
[0050] FIG. 5C is a cross-sectional view showing yet another example of a capacitor according to the present disclosure. In the capacitor 1d shown in FIG. 5C, the dielectric 20 is formed, for example, as a film. A different dielectric 22, which is different from the dielectric 20, is dispersed and disposed in this film. Methods for forming this film include spin coating, inkjet printing, die coating, roll coating, bar coating, Langmuir-Blodgett coating, dip coating, and spray coating. For example, a film including the dielectric 20 and the different dielectric 22 can be obtained by forming a coating of a precursor liquid containing the raw material of the dielectric 20 and particles of the different dielectric 22 by the above-described method. This film may be formed by sputtering, anodization, vacuum deposition, PLD, ALD, or CVD.
[0051] The different dielectric 22 is not limited to a specific dielectric as long as it is a dielectric of a different type from the dielectric 20. The different dielectric 22 has, for example, a higher dielectric constant than that of the dielectric 20. The different dielectric 22 may be, for example, a perovskite compound such as BaTiO3, PbTiO3, or SrTiO3, or may be a layered perovskite compound. The different dielectric 22 may contain at least one selected from the group consisting of a Ruddlesden-Popper compound, a Dion-Jacobson compound, a tungsten bronze compound, and a pyrochlore compound.
[0052] The size of the particles of the different dielectric material 22 is not limited to a specific value, and the particles of the different dielectric material 22 have a size of, for example, 1 nm or more and 100 nm or less.
[0053] 6A is a diagram schematically illustrating an example of an electric circuit according to the present disclosure. The electric circuit 3 includes a capacitor 1a. The electric circuit 3 may be an active circuit or a passive circuit. The electric circuit 3 may be a discharge circuit, a smoothing circuit, a decoupling circuit, or a coupling circuit. Since the electric circuit 3 includes the capacitor 1a, the electric circuit 3 is likely to exhibit the desired performance. For example, the capacitor 1a in the electric circuit 3 is likely to reduce noise. The electric circuit 3 may include a capacitor 1b, 1c, or 1d instead of the capacitor 1a.
[0054] 6B is a diagram schematically illustrating an example of a circuit board according to the present disclosure. As shown in FIG. 6B, the circuit board 5 includes a capacitor 1a. For example, an electric circuit 3 including the capacitor 1a is formed on the circuit board 5. The circuit board 5 may be an embedded board or a motherboard. The circuit board 5 may include a capacitor 1b, 1c, or 1d instead of the capacitor 1a.
[0055] FIG. 6C is a diagram schematically illustrating an example of a device according to the present disclosure. As shown in FIG. 6C , the device 7 includes, for example, a capacitor 1a. The device 7 includes, for example, a circuit board 5 including the capacitor 1a. Because the device 7 includes the capacitor 1a, the device 7 is likely to exhibit desired performance. The device 7 may be an electronic device, a communication device, a signal processing device, or a power supply device. The device 7 may be a server, an AC adapter, an accelerator, or a flat panel display such as a liquid crystal display (LCD). The device 7 may be a USB charger, a solid-state drive (SSD), an information terminal such as a PC, a smartphone, or a tablet PC, or an Ethernet switch.
[0056] (Additional Note) From the above description, the following techniques are disclosed.
[0057] (Technology 1) A capacitor comprising: a first electrode; a second electrode; and a dielectric disposed between the first electrode and the second electrode, wherein the dielectric contains a crystal having a composition of APb2X5, wherein in the composition, A is a cation that is a molecular ion containing a nitrogen atom, and X is a halogen element.
[0058] (Technology 2) The capacitor according to Technology 1, wherein the cation further contains a carbon atom.
[0059] (Technology 3) The cation is an ammonium ion represented by the following formula (I): 1 , R 2 , R 3 , and R 4 Each of the groups independently represents a hydrogen atom, an alkyl group, an aryl group, or NH2.
[0060] (Technology 4) In the formula (I), R 1 and R 2 are each independently a hydrogen atom, an alkyl group, or an aryl group, and R 3 and R4 Each of the groups is a hydrogen atom.
[0061] (Technology 5) In the formula (I), R 1 , R 2 , R 3 , and R 4 Each of the groups is a hydrogen atom.
[0062] (Technology 6) In the formula (I), R 1 is NH2, and R 2 , R 3 , and R 4 Each of the groups is a hydrogen atom.
[0063] (Technology 7) The capacitor according to any one of Technologies 1 to 6, wherein the dielectric has an inverse perovskite structure.
[0064] (Technology 8) An electric circuit comprising the capacitor according to any one of Technologies 1 to 7.
[0065] (Technology 9) A circuit board comprising the capacitor according to any one of Technologies 1 to 7.
[0066] (Technology 10) A device comprising the capacitor according to any one of technologies 1 to 7.
[0067] The present disclosure will be described in more detail below with reference to examples. Note that the following examples are illustrative and the present disclosure is not limited to the following examples.
[0068] Example 1 A glass substrate manufactured by Nippon Sheet Glass Co., Ltd. was prepared, having an indium-doped SnO2 layer on its surface. The indium-doped SnO2 layer served as an electrode. The glass substrate was subjected to ultrasonic cleaning for 10 minutes in a container filled with ethanol to clean the surface. The surface was then subjected to UV ozone treatment for 30 minutes to remove adsorbed materials from the surface of the glass substrate.
[0069] Next, 0.5 mmol of NH4Br and 1 mmol of PbBr2 were added to 1 ml of a mixed solvent of DMSO and DMF to obtain a mixed solution. The volume ratio of DMSO to DMF in the mixed solvent was 1:4. When the solution was heated to 80°C, the NH4Br and PbBr2 readily dissolved, and impurities were removed using a filter to obtain the coating solution of Example 1. In a glove box, 80 μl of the coating solution of Example 1 was dropped onto the indium-doped SnO2 layer of the glass substrate, and a coating film was obtained by spin coating. The inside of the glove box was filled with N2, and the oxygen concentration was below 0.1 ppm (parts per million) by volume. The coating film was then baked on a hot plate maintained at 80°C for 30 minutes. In this way, a dielectric layer was formed. This dielectric layer mainly contained an antiperovskite compound having the composition NH4Pb2Br5. Finally, gold was evaporated onto the dielectric layer to form electrodes, thus obtaining the capacitor according to Example 1.
[0070] (Crystal Structure Analysis) X-ray diffraction (XRD) measurements were performed to identify the crystal structure of the dielectric material contained in the dielectric layer of the capacitor according to Example 1. In this measurement, Cu-Kα radiation was used as the X-ray, and the measurement was performed in a dry argon atmosphere. FIG. 7 is a graph showing the XRD pattern of the dielectric material contained in the dielectric layer of the capacitor according to Example 1. In FIG. 7, the horizontal axis represents the diffraction angle 2θ [degrees], and the vertical axis represents the relative intensity of the X-ray diffraction intensity. The lower part of FIG. 7 shows the results of a simulation of the XRD pattern of KSnCl of a (NH)PbBr type having an antiperovskite structure. This suggests that the dielectric material contained in the dielectric layer of the capacitor according to Example 1 has an antiperovskite structure.
[0071] (Composition Analysis) Using an X-ray photoelectron spectroscopy (XPS) device PHI VersaProbe 2 manufactured by ULVAC-PHI, Inc., the contents of N, Pb, and Br per unit weight of the dielectric material contained in the dielectric layer of the capacitor according to Example 1 were measured by XPS measurement. Taking into account the composition estimated from the results of XRD measurement, the N:Pb:Br molar ratio was calculated based on the contents of N, Pb, and Br obtained from the results of XPS measurement. As a result, it was found that the dielectric material contained in the dielectric layer of the capacitor according to Example 1 had a relationship of N:Pb:Br = 1:2:5, similar to the molar ratio of the raw materials.
[0072] (Evaluation of Withstand Voltage and Polarization) Polarization-Electric field (PE) measurements were performed on the capacitor of Example 1 using a ferroelectric tester Premier II manufactured by Radiant Technology, and a P-E curve for the capacitor of Example 1 was obtained. The dielectric properties of the capacitor of Example 1 were evaluated based on this P-E curve. FIG. 8 is a graph (P-E curve) showing the relationship between polarization and electric field strength of the capacitor of Example 1. In FIG. 8, the vertical axis represents polarization, and the horizontal axis represents electric field strength. The maximum value of the electric field strength in the P-E curve was determined to be the withstand voltage of the capacitor of Example 1. The withstand voltage of Example 1 was 418 kV / cm, and the maximum polarization was 1.39 μC / cm 2 The results are shown in Table 1.
[0073] Example 2 A coating solution according to Example 2 was obtained in the same manner as in Example 1, except that 0.375 mmol of NHBr, 0.75 mmol of PbBr, 0.125 mmol of NHCl, and 0.25 mmol of PbCl were added to 1 ml of a mixed solvent of DMSO and DMF. A capacitor according to Example 2 was fabricated in the same manner as in Example 1, except that the coating solution according to Example 2 was used instead of the coating solution according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Example 2 was determined based on XRD and XPS measurements in the same manner as in Example 1. The crystal structure of the dielectric material contained in the dielectric layer of the capacitor according to Example 2 was determined based on XRD measurements in the same manner as in Example 1. A P-E curve of the capacitor according to Example 2 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1.
[0074] Example 3 A coating solution according to Example 3 was obtained in the same manner as in Example 1, except that 0.25 mmol of NHBr, 0.5 mmol of PbBr, 0.25 mmol of NHCl, and 0.5 mmol of PbCl were added to 1 ml of a mixed solvent of DMSO and DMF. A capacitor according to Example 3 was fabricated in the same manner as in Example 1, except that the coating solution according to Example 3 was used instead of the coating solution according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Example 3 was determined based on XPS measurement in the same manner as in Example 1. The crystal structure of the dielectric material contained in the dielectric layer of the capacitor according to Example 3 was determined based on XRD measurement and XRD measurement in the same manner as in Example 1. A P-E curve of the capacitor according to Example 3 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1.
[0075] Example 4 A coating solution according to Example 4 was obtained in the same manner as in Example 1, except that 0.5 mmol of NH4Cl and 1 mmol of PbCl2 were added to 1 ml of a mixed solvent of DMSO and DMF. A capacitor according to Example 4 was fabricated in the same manner as in Example 1, except that the coating solution according to Example 4 was used instead of the coating solution according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Example 4 was determined based on XRD measurement and XPS measurement in the same manner as in Example 1. The crystal structure of the dielectric material contained in the dielectric layer of the capacitor according to Example 4 was determined based on XRD measurement in the same manner as in Example 1. A P-E curve of the capacitor according to Example 4 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1.
[0076] Example 5 A coating solution according to Example 5 was obtained in the same manner as in Example 1, except that 0.45 mmol of NHBr, 0.05 mmol of CHNHBr, and 1 mmol of PbBr were added to 1 ml of a mixed solvent of DMSO and DMF. A capacitor according to Example 5 was fabricated in the same manner as in Example 1, except that the coating solution according to Example 5 was used instead of the coating solution according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Example 5 was determined based on XRD and XPS measurements in the same manner as in Example 1. The crystal structure of the dielectric material contained in the dielectric layer of the capacitor according to Example 5 was determined based on XRD measurements in the same manner as in Example 1. A P-E curve of the capacitor according to Example 5 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1.
[0077] Example 6 A coating liquid according to Example 6 was obtained in the same manner as in Example 1, except that 0.45 mmol of NHBr, 0.05 mmol of HC(NH)Br, and 1 mmol of PbBr were added to 1 ml of a mixed solvent of DMSO and DMF. +is a salt having a cation. A capacitor according to Example 6 was produced in the same manner as in Example 1, except that the coating liquid according to Example 6 was used instead of the coating liquid according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Example 6 was determined based on XRD measurement and XPS measurement in the same manner as in Example 1. The crystal structure of the dielectric material contained in the dielectric layer of the capacitor according to Example 6 was determined based on XRD measurement in the same manner as in Example 1. A P-E curve of the capacitor according to Example 6 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1.
[0078] Comparative Example 1 A coating solution according to Comparative Example 1 was obtained in the same manner as in Example 1, except that 0.5 mmol of KBr and 1 mmol of PbBr2 were added to 1 ml of a mixed solvent of DMSO and DMF. A capacitor according to Comparative Example 1 was fabricated in the same manner as in Example 1, except that the coating solution according to Comparative Example 1 was used instead of the coating solution according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Comparative Example 1 was determined based on XRD and XPS measurements in the same manner as in Example 1. The crystalline structure of the dielectric material contained in the dielectric layer of the capacitor according to Comparative Example 1 was determined based on XRD measurements in the same manner as in Example 1. A P-E curve for the capacitor according to Comparative Example 1 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1. FIG. 9 is a graph (P-E curve) showing the relationship between polarization and electric field strength for the capacitor according to Comparative Example 1. In FIG. 9, the vertical axis represents polarization, and the horizontal axis represents electric field strength.
[0079] Comparative Example 2 A coating solution according to Comparative Example 2 was prepared in the same manner as in Example 1, except that 0.5 mmol of CsBr and 1 mmol of PbBr2 were added to 1 ml of a mixed solvent of DMSO and DMF. A capacitor according to Comparative Example 2 was fabricated in the same manner as in Example 1, except that the coating solution according to Comparative Example 2 was used instead of the coating solution according to Example 1. The composition of the dielectric material contained in the dielectric layer of the capacitor according to Comparative Example 2 was determined based on XRD and XPS measurements in the same manner as in Example 1. The crystalline structure of the dielectric material contained in the dielectric layer of the capacitor according to Comparative Example 2 was determined based on XRD measurements in the same manner as in Example 1. A P-E curve for the capacitor according to Comparative Example 2 was obtained, and the withstand voltage and maximum polarization were determined in the same manner as in Example 1. The results are shown in Table 1. FIG. 10 is a graph (P-E curve) showing the relationship between polarization and electric field strength for the capacitor according to Comparative Example 2. In FIG. 10, the vertical axis represents polarization, and the horizontal axis represents electric field strength.
[0080] As shown in Table 1, the dielectric material contained in the dielectric layers of the capacitors according to Examples 1 to 6 contains lead ions as metal cations and cations that are molecular ions containing nitrogen atoms. Comparing each Example with Comparative Examples 1 and 2, it can be seen that the inclusion of molecular ions containing nitrogen atoms tends to increase the withstand voltage of the capacitor. Furthermore, the high withstand voltage also increases the maximum polarization.
[0081]
[0082] The capacitor according to the present disclosure is useful because it tends to have a high withstand voltage.
[0083] 1a, 1b, 1c, 1d Capacitor 3 Electric circuit 5 Circuit board 7 Device 11 First electrode 11p, 12p Main surface 12 Second electrode 13 Electrolyte 15 Cathode 20 Dielectric 22 Different dielectric
Claims
1. A capacitor comprising: a first electrode; a second electrode; and a dielectric disposed between the first electrode and the second electrode, the dielectric comprising a crystal having a composition of APb2X5, wherein A is a cation that is a molecular ion containing a nitrogen atom, and X is a halogen element.
2. The capacitor of claim 1, wherein the cation further comprises a carbon atom.
3. The cation is an ammonium ion represented by the following formula (I): 1 , R 2 , R 3 , and R 4 The capacitor of claim 1 , wherein each of is independently a hydrogen atom, an alkyl group, an aryl group, or NH 2 .
4. In the formula (I), R 1 and R 2 are each independently a hydrogen atom, an alkyl group, or an aryl group, and R 3 and R 4 The capacitor of claim 3 , wherein each of is a hydrogen atom.
5. In the formula (I), R 1 , R 2 , R 3 , and R 4 The capacitor of claim 4 , wherein each of is a hydrogen atom.
6. In the formula (I), R 1 is NH2, and R 2 , R 3 , and R 4 The capacitor of claim 3 , wherein each of is a hydrogen atom.
7. The capacitor of claim 1, wherein the dielectric has an inverse perovskite structure.
8. An electric circuit comprising the capacitor according to claim 1.
9. A circuit board comprising the capacitor according to claim 1.
10. A device comprising the capacitor according to claim 1.
Citation Information
Patent Citations
Liquid electrolyte-free, solid-state solar cells with inorganic hole transport materials
US20130233377A1
Switchable photovoltaic devices
US20210043854A1
Capacitor, electric circuit, circuit board, and apparatus
WO2023233918A1