Near-infrared-absorbing composition, and optical member

The near-infrared absorbing composition, featuring a copper phosphonate complex, phosphate ester, and specific antioxidants, addresses solvent oxidation and coloring issues, ensuring stability and optical quality by using a titanium coupling agent to prevent solvent oxidation and maintain color stability.

WO2024237015A1PCT designated stage expired Publication Date: 2024-11-21KONICA MINOLTA INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015666
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-18
Filing Date
2024-04-22
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

Near-infrared absorbing compositions containing copper compounds and ether solvents face issues with solvent oxidation and coloring, leading to potential explosions and adverse effects on optical properties due to the use of hindered phenolic antioxidants.

Method used

Incorporating a copper phosphonate complex, phosphate ester, and specific antioxidants with structures represented by general formulas (1) to (5) into the near-infrared absorbing composition, along with a titanium coupling agent, to prevent solvent oxidation and maintain color stability.

Benefits of technology

The solution effectively suppresses solvent oxidation, reduces the risk of explosions, and prevents coloring, thereby enhancing the stability and optical properties of the cured film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015666_21112024_PF_FP_ABST
    Figure JP2024015666_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a near-infrared-absorbing composition that has the antioxidant function of a solvent but is less likely to result in discoloration; and an optical member that uses said composition. This near-infrared-absorbing composition contains a copper phosphonate complex, a phosphoric acid ester, an ether-based solvent, and an antioxidant, and contains, as the antioxidant, at least one selected from antioxidants having a structure represented by any one of general formulas (1)-(5).
Need to check novelty before this filing date? Find Prior Art

Description

Near-infrared absorbing composition and optical member

[0001] The present invention relates to a near-infrared absorbing composition and an optical component. More specifically, the present invention relates to a near-infrared absorbing composition that has a solvent oxidation inhibitory function and is resistant to coloration, and an optical component using the same.

[0002] Near-infrared cut filters are used in solid-state imaging devices. One type of near-infrared cut filter is produced by curing a liquid near-infrared absorbing composition containing a copper compound. When preparing a near-infrared absorbing composition containing a copper compound, an ether-based solvent such as tetrahydrofuran is often used for the purpose of dissolving copper acetate.

[0003] Ether-based solvents are a concern due to the generation of explosive peroxides, and therefore, an antioxidant is sometimes added to near-infrared absorbing compositions that may contain ether-based solvents.

[0004] Patent Documents 1 and 2 disclose a technique of adding a hindered phenol-based antioxidant to a near-infrared absorbing composition that may contain an ether-based solvent.

[0005] However, it has been found that when a copper compound and a hindered phenol-based antioxidant are used in combination, the cured film formed from the near-infrared absorbing composition becomes colored during the curing step or the like.

[0006] International Publication No. 2014 / 027639 Japanese Patent Application Laid-Open No. 2014-032380

[0007] The present invention has been made in consideration of the above problems and circumstances, and an object of the present invention is to provide a near-infrared absorbing composition that has a solvent oxidation inhibitory function and is resistant to coloration, and an optical component using the same.

[0008] The present inventors have investigated the causes of the above problems in order to solve them. As a result, the present inventors have found that the above problems can be solved by adding an antioxidant having a specific structure to a near-infrared absorbing composition containing a copper phosphonate complex, a phosphate ester, and an ether-based solvent, and have arrived at the present invention. That is, the above problems according to the present invention are solved by the following means.

[0009] 1. A near-infrared absorbing composition containing a phosphonic acid copper complex, further containing a phosphate ester, a solvent, and an antioxidant, wherein the solvent contains at least an ether-based solvent, and the antioxidant is at least one selected from the group consisting of a phenol-based antioxidant having a structure represented by the following general formula (1), an amine-based antioxidant having a structure represented by the following general formula (2), a phosphorus-based antioxidant having a structure represented by the following general formula (3) or (4), and a sulfur-based antioxidant having a structure represented by the following general formula (5):

[0010]

[0011] [In the general formulas (1) to (5), R 3 is an alkyl group having 1 to 4 carbon atoms. 4 ~R 9 is a substituent selected from a hydroxy group, an acyloxy group, and an alkyl group. 4 ~R 9 At least one of R is a hydroxy group and the other at least one is an acyloxy group. 10 is oxygen or an alkylene ester group having 1 to 20 carbon atoms, and may further have a substituent. 11 and R 12 is hydrogen, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. 13 ~R 21 is an alkyl group or aryl group having 1 to 20 carbon atoms, and may further have a substituent. 15 and R 16 may be bonded to each other.

[0012] 2. The near-infrared absorbing composition according to item 1, further comprising a titanium coupling agent.

[0013] 3. The near-infrared absorbing composition according to item 1, wherein the acetate ion concentration is 0.5% by mass or less.

[0014] 4. The near-infrared absorbing composition according to item 1, wherein the phosphate ester has a structure represented by the following general formula (II):

[0015]

[0016] [In the general formula (II), R 2 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may further have a substituent. 21 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structural units added, each of which is a hydrogen atom, and is in the range of 1 to 19. 21 ~R 24 represents the average number of partial structural units added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 1 to 19. m+n is the total number of m and n, and is within the range of 2 to 20. Z represents a structural unit selected from the following formulae (Z-1) and (Z-2).

[0017]

[0018] 5. The near-infrared absorbing composition according to item 1, containing, as the antioxidant, at least one selected from the phenol-based antioxidant and the amine-based antioxidant, and at least one selected from the phosphorus-based antioxidant and the sulfur-based antioxidant.

[0019] 6. The near-infrared absorbing composition according to item 1, wherein the antioxidant contains at least one selected from the phenol-based antioxidant and the amine-based antioxidant.

[0020] 7. The near-infrared absorbing composition according to item 1, wherein the content of the solvent is within a range of 61 to 98 mass %.

[0021] 8. An optical member comprising a cured product of the near-infrared absorbing composition according to any one of items 1 to 6.

[0022] According to the above-mentioned means of the present invention, it is possible to provide a near-infrared absorbing composition which has a function of preventing oxidation of a solvent and is resistant to coloration, and an optical member using the same.

[0023] The mechanism by which the effects of the present invention are manifested or the mechanism of action is not clear, but is speculated as follows.

[0024] When hydrogen is released from an ether solvent (RH), an R radical is generated. The R radical reacts with oxygen to become an ROO radical. When the ROO radical reacts with an ether solvent (RH), peroxide (ROOH) and an R radical (1) are generated. The peroxide (ROOH) is decomposed into an RO radical and an OH radical, and when these react with an ether solvent (RH), ROH, H 2 O and R radicals (2) are generated. The two generated R radicals (1) and (2) each react with oxygen to become ROO radicals, and the above cycle is repeated in a chain reaction. This chain reaction increases the amount of peroxide (ROOH). In this way, ether-based solvents are prone to generate peroxides. Since peroxides are explosive, ether-based solvents pose a risk of explosion.

[0025] In contrast, radical chain inhibitors such as phenolic antioxidants and amine antioxidants prevent ROO radicals from reacting with ether solvents (RH) to generate R radicals, thereby suppressing radical chain reactions. Peroxide decomposers such as phosphorus-based antioxidants and sulfur-based antioxidants reduce peroxides (ROOH) to ROH, thereby reducing the amount of peroxides (ROOH) and suppressing the chain reaction. Therefore, even in compositions containing ether solvents, the risk of explosion can be reduced by further adding such antioxidants.

[0026] Here, it is known that hindered phenol-based antioxidants, which are commonly used as antioxidants, are easily discolored by various factors such as heat. In near-infrared absorbing compositions containing copper compounds, dibutylhydroxytoluene (BHT) and Irganox 1010 (manufactured by BASF), which are common hindered phenol-based antioxidants, react with copper, for example, and turn yellow. Therefore, near-infrared absorbing compositions containing hindered phenol-based antioxidants have problems with the optical properties of the cured films formed, even if oxidation of the ether-based solvent is suppressed.

[0027] In contrast, the antioxidant according to the present invention has a structure represented by any one of general formulas (1) to (5). The antioxidant having a structure represented by any one of general formulas (1) to (5) is less likely to discolor due to its structure being different from that of dibutylhydroxytoluene (BHT) and Irganox 1010 (manufactured by BASF), which are common hindered phenol-based antioxidants. Therefore, the near-infrared absorbing composition of the present invention containing the antioxidant having a structure represented by any one of general formulas (1) to (5) is less likely to discolor.

[0028] Schematic cross-sectional view showing an example of the configuration of a near-infrared cut filter. Schematic cross-sectional view showing an example of the configuration of an image sensor for a solid-state imaging device. Schematic cross-sectional view showing an example of the configuration of a camera module.

[0029] The near-infrared absorbing composition of the present invention is a near-infrared absorbing composition containing a phosphonate copper complex, further containing a phosphate ester, a solvent, and an antioxidant, wherein the solvent contains at least an ether-based solvent, and the antioxidant contains at least one antioxidant selected from the group consisting of antioxidants having structures represented by the above general formulas (1) to (5). This feature is a technical feature common to or corresponding to the following embodiments.

[0030] In an embodiment of the present invention, it is preferable to further contain a titanium coupling agent. This improves the dispersion stability of the phosphonate copper complex, thereby reducing the haze of the cured film formed from the near-infrared absorbing composition and improving the visible light transmittance. Furthermore, the formation of a titanium coupling agent film by the crosslinking reaction of the titanium coupling agent can suppress water penetration from the film surface, improving the moisture resistance of the cured film. Furthermore, the titanium coupling agent film also blocks oxygen, thereby suppressing the generation of peroxides derived from ether-based solvents. Furthermore, physical adsorption or crosslinking between the titanium coupling agent and the phosphonate copper complex suppresses thermal vibration of the phosphonate copper complex, improving the heat resistance of the cured film.

[0031] In an embodiment of the present invention, the acetate ion concentration is preferably 0.5% by mass or less. Near-infrared absorbing compositions containing copper complexes are generally prepared using copper acetate. Therefore, near-infrared absorbing compositions often contain acetate ions. However, acetate ions reduce the dispersion stability of the phosphonate copper complex and inhibit the function of the antioxidant. Therefore, a low acetate ion concentration is preferable. Specifically, an acetate ion concentration of 0.5% by mass or less can prevent the dispersion stability of the phosphonate copper complex from decreasing and the function of the antioxidant from being inhibited.

[0032] In an embodiment of the present invention, it is preferable that the phosphate ester has a structure represented by the above general formula (II) from the viewpoint of dispersibility and dispersion stability of the phosphonate copper complex.

[0033] In an embodiment of the present invention, it is preferable from the viewpoint of suppressing an increase in peroxides that the antioxidant contains at least one selected from the phenol-based antioxidant and the amine-based antioxidant, and at least one selected from the phosphorus-based antioxidant and the sulfur-based antioxidant.

[0034] In an embodiment of the present invention, it is preferable that the antioxidant contains at least one selected from the phenol-based antioxidant and the amine-based antioxidant, from the viewpoints of suppressing an increase in peroxides and minimizing the effect on the optical properties of the cured film.

[0035] In an embodiment of the present invention, the content of the solvent is preferably in the range of 61 to 98% by mass. By keeping the content within this range, dispersion stability is further improved and long-term storage is possible.

[0036] The optical member of the present invention is characterized by containing a cured product of the near-infrared absorbing composition of the present invention.

[0037] The present invention, its components, and embodiments and modes for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after it are included as the lower limit and upper limit.

[0038] [Outline of Near-Infrared Absorbing Composition of the Present Invention] The near-infrared absorbing composition of the present invention is a near-infrared absorbing composition containing a phosphonate copper complex, further containing a phosphate ester, a solvent, and an antioxidant, wherein the solvent contains at least an ether-based solvent, and at least one of the antioxidants has a structure represented by any one of general formulas (1) to (5) described below.

[0039] [Phosphonate Copper Complex] The near-infrared absorbing composition of the present invention is characterized by containing a phosphonate copper complex. The phosphonate copper complex is a complex in which phosphonic acid is coordinated to copper. The phosphonate copper complex absorbs near-infrared rays and contributes to adjusting the transmitted light to a desired waveform.

[0040] The phosphonic acid copper complex is preferably a phosphonic acid copper complex having a structure represented by the following general formula (I).

[0041]

[0042] [In the above general formula (I), R 1 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent.

[0043] R 1Examples of the substituent that may be substituted include alkyl groups (e.g., methyl, ethyl, trifluoromethyl, isopropyl, etc.), alkoxy groups (e.g., methoxy, ethoxy, etc.), halogen atoms (e.g., fluorine, etc.), cyano groups, nitro groups, dialkylamino groups (e.g., dimethylamino, etc.), trialkylsilyl groups (e.g., trimethylsilyl, etc.), triarylsilyl groups (e.g., triphenylsilyl, etc.), triheteroarylsilyl groups (e.g., tripyridylsilyl, etc.), benzyl groups, and heteroaryl groups (e.g., pyridyl, carbazolyl, etc.). Examples of the fused ring include 9,9'-dimethylfluorene, carbazole, and dibenzofuran.

[0044] R 1 is preferably an alkyl group having 1 to 20 carbon atoms, in terms of good resistance to humidity and heat and near-infrared absorbing properties. 1 It is more preferable that the alkyl group has 1 to 4 carbon atoms, since this can achieve both near-infrared absorption and visible light transmittance.

[0045] R 1 is an alkyl group having 1 to 20 carbon atoms, examples of which include methylphosphonic acid, ethylphosphonic acid, propylphosphonic acid, butylphosphonic acid, pentylphosphonic acid, hexylphosphonic acid, heptylphosphonic acid, octylphosphonic acid, nonylphosphonic acid, and decylphosphonic acid.

[0046] R 1 is an aryl group having 6 to 20 carbon atoms, examples of which include phenylphosphonic acid, 4-methoxyphenylphosphonic acid, 4-aminophenylphosphonic acid, 4-bromophenylphosphonic acid, 3-phosphonobenzoic acid, 4-phosphonobenzoic acid, and 4-hydroxyphenylphosphonic acid.

[0047] The following compounds (H-1) to (H-8) are examples of phosphonic acids.

[0048]

[0049] In the present invention, the phosphonic acid is preferably at least one alkylphosphonic acid selected from the following group of phosphonic acids:

[0050] Methylphosphonic acid, Ethylphosphonic acid, Propylphosphonic acid, Butylphosphonic acid, Pentylphosphonic acid, Hexylphosphonic acid, Octylphosphonic acid, 2-Ethylhexylphosphonic acid, 2-Chloroethylphosphonic acid, 3-Bromopropylphosphonic acid, 3-Methoxybutylphosphonic acid, 1,1-Dimethylpropylphosphonic acid, 1,1-Dimethylethylphosphonic acid, 1-Methylpropylphosphonic acid

[0051] The structure of the phosphonic acid copper complex is represented, for example, by the following general formula (IC).

[0052]

[0053] R in the following general formula (IC) 1 represents R in general formula (I). 1 is the same as

[0054] In general formula (IC), two reactive hydroxy groups possessed by the compound having the structure represented by general formula (I) are both formed by reacting with the same copper ion, but the form of the phosphonate copper complex is not limited to this. The "reactive hydroxy group" refers to the hydroxy group of the phosphonic acid that is directly bonded to the phosphorus atom.

[0055] In the near-infrared absorbing composition, the phosphonic acid copper complex is mainly in the form of fine particles.

[0056] As the copper ion source for the copper phosphonate complex, a copper salt capable of supplying divalent copper ions is used.

[0057] Examples of copper ion sources include copper salts of organic acids or copper salts of inorganic acids.

[0058] Specific examples of copper ion sources include copper salts of organic acids such as anhydrous copper acetate, anhydrous copper formate, anhydrous copper stearate, anhydrous copper benzoate, anhydrous copper acetoacetate, anhydrous copper ethylacetoacetate, anhydrous copper methacrylate, anhydrous copper pyrophosphate, anhydrous copper naphthenate, and anhydrous copper citrate, and hydrates or hydrates of the copper salts of these organic acids; copper salts of inorganic acids such as copper oxide, copper chloride, copper sulfate, copper nitrate, copper phosphate, basic copper sulfate, and basic copper carbonate, and hydrates or hydrates of the copper salts of these inorganic acids; and copper hydroxide.

[0059] The content of the phosphonate copper complex in the near-infrared absorbing composition is preferably within a range of 1 to 50 mass %, more preferably within a range of 1 to 30 mass %. By keeping the content within this range, dispersion becomes more stable.

[0060] [Phosphate Ester] The near-infrared absorbing composition of the present invention is characterized by containing a phosphate ester. The phosphate ester may be a copper complex.

[0061] The phosphate ester disperses the phosphonate copper complex in the near-infrared absorbing composition and prevents the particle size of the particles formed by the phosphonate copper complex from increasing. This improves the visible light transmittance of the cured film of the near-infrared absorbing composition. Furthermore, the inclusion of the phosphate ester in the near-infrared absorbing composition improves the solubility of the antioxidant in ether-based solvents.

[0062] Phosphate esters are also available as commercially available products, such as the following:

[0063] 1) Manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd. Plysurf A212C: polyoxyethylene tridecyl ether phosphate Plysurf A215C: polyoxyethylene tridecyl ether phosphate Plysurf A208F: polyoxyethylene alkyl (C8) ether phosphate Plysurf M208F: polyoxyethylene alkyl (C8) ether phosphate-monoethanolamine salt Plysurf A208N: polyoxyethylene alkyl (C12,13) ​​ether phosphate Plysurf A208B: polyoxyethylene lauryl ether phosphate (oil-based dispersant) Plysurf A210B: polyoxyethylene lauryl ether phosphate Plysurf A219B: polyoxyethylene lauryl ether phosphate (aqueous dispersant) Plysurf DB-01: polyoxyethylene lauryl ether phosphate-monoethanolamine salt Plysurf AL: polyoxyethylene styrenated phenyl ether phosphate, etc.

[0064] 2) Nikko Chemicals Co., Ltd. NIKKOL DDP-2: Polyoxyethylene alkyl (C12-C15) ether phosphate (2 E.O. di(C12-15) pareth-2 phosphate) NIKKOL DDP-4: Polyoxyethylene alkyl (C12-C15) ether phosphate (4 E.O. di(C12-15) pareth-4 phosphate) NIKKOL DDP-6: Polyoxyethylene alkyl (C12-C15) ether phosphate (6 E.O. di(C12-15) pareth-6 phosphate) NIKKOL DDP-8: Polyoxyethylene alkyl (C12-C15) ether phosphate (8 E.O. di(C12-15) pareth-8 phosphate) NIKKOL DDP-10: polyoxyethylene alkyl (C12-C15) ether phosphate (10E.O. di(C12-15)paleth-10 phosphate), NIKKOL DLP-10: polyoxyethylene lauryl ether sodium phosphate (sodium dilaureth-10 phosphate), NIKKOL DOP-8NV: polyoxyethylene oleyl ether sodium phosphate (sodium dioleth-8 phosphate), etc.

[0065] 3) ADEKA COLE TS-230E (aromatic phosphate ester), ADEKA COLE CS-141E (aromatic phosphate ester), ADEKA COLE CS1361E (aromatic phosphate ester), ADEKA COLE CS-279 (aromatic phosphate ester), ADEKA COLE PS-440E (aliphatic phosphate ester), ADEKA COLE PS-810E (aliphatic phosphate ester), ADEKA COLE PS-807 (aliphatic phosphate ester), ADEKA COLE PS-984 (aliphatic phosphate ester), etc., manufactured by ADEKA COLE Corporation

[0066] From the viewpoint of dispersibility and dispersion stability of the copper phosphonate complex, the phosphate ester preferably has a structure represented by the following general formula (II):

[0067]

[0068] [In the general formula (II), R 2 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, and may further have a substituent. 21 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structural units added, each of which is a hydrogen atom, and is in the range of 1 to 19. 21 ~R 24 represents the average number of partial structural units added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 1 to 19. m+n is the total number of m and n, and is within the range of 2 to 20. Z represents a structural unit selected from the following formulae (Z-1) and (Z-2).

[0069]

[0070] R 21 ~R 24 When all of are hydrogen atoms, the partial structure in the parentheses in the formula is called an "ethylene oxide structure." In the formula, m is the average number of ethylene oxide structures added.

[0071] R 21 ~R 24The partial structure in the parentheses in the formula, in which at least one of the above is an alkyl group having 1 to 4 carbon atoms and the others are hydrogen atoms, is called an "alkyl-substituted ethylene oxide structure." In the formula, n is the average number of alkyl-substituted ethylene oxide structures added.

[0072] The compound having the structure represented by general formula (II), in which m and n are both within the range of 1 to 19, has a high ability to form a complex with copper and is highly effective as a dispersant.

[0073] The compound having the structure represented by general formula (II) has a combination of an ethylene oxide structure and an alkyl-substituted ethylene oxide structure, and therefore has many types of isomers, which increases the entropy of the compound, making it highly effective as a dispersant.

[0074] The compound having the structure represented by the general formula (II) is 21 ~R 24 Therefore, the effects of the ethylene oxide structure and the alkyl-substituted ethylene oxide structure are exerted in a well-balanced manner, and the near-infrared absorbing composition can have good dispersibility and dispersion stability.

[0075] In general formula (II), R 2 is preferably an alkyl group having 6 to 16 carbon atoms from the viewpoint of dispersibility of the copper complex and resistance to humidity and heat.

[0076] The compound having the structure represented by general formula (II) is a diester when Z is formula (Z-1), and a monoester when Z is formula (Z-2).

[0077] The mixing ratio of the diester and the monoester is preferably such that the molar ratio of the monoester to the total amount of the diester and the monoester is within the range of 20 to 95%.

[0078] Specific examples of compounds having a structure represented by general formula (II) are shown in the following Tables IV to V. The compounds having a structure represented by general formula (II) according to the present invention are not limited to these.

[0079] In Tables IV, the exemplary compounds having both (Z-1) and (Z-2) in the "Structure" column for "Z" are mixtures of compounds in which Z is represented by formula (Z-1) and compounds in which Z is represented by formula (Z-2).

[0080]

[0081]

[0082]

[0083]

[0084]

[0085] A specific description will be given of Exemplary Compound 1. Exemplary Compound 1 is a mixture of a compound (diester) in which Z is represented by formula (Z-1) and a compound (monoester) in which Z is represented by formula (Z-2).

[0086] A compound (monoester) in which Z is formula (Z-2) is represented, for example, by the structure of Exemplary Compound 1-1 below. A compound (diester) in which Z is formula (Z-1) is represented, for example, by the structure of Exemplary Compound 1-2 below.

[0087]

[0088] In Exemplified Compound 1, the molar ratio of the compound (monoester) in which Z is formula (Z-2) is 50%, and Exemplified Compound 1-1 and Exemplified Compound 1-2 are contained in the same molar amount.

[0089] m and n are the average addition numbers. Therefore, even in the case of Exemplified Compound 1 in which m is 5 and n is 5, the number of ethylene oxide structures in one molecule is not necessarily 5, and the number of alkyl-substituted ethylene oxide structures is not necessarily 5.

[0090] Compounds having a structure represented by general formula (II) can be synthesized with reference to the methods described in, for example, JP-A-2005-255608, JP-A-2015-000396, JP-A-2015-000970, JP-A-2015-178072, JP-A-2015-178073, and Japanese Patent No. 4422866.

[0091] Hereinafter, several methods for synthesizing the exemplary compounds shown in the table will be specifically explained. Note that the method for synthesizing the compound having the structure represented by general formula (II) is not limited to the following synthesis methods.

[0092] (Method for synthesizing exemplary compound 53) 130 g (1.0 mol) of n-octanol is placed in an autoclave. 116 g (2.0 mol) of propylene oxide is added to this using potassium hydroxide as a catalyst under conditions of a pressure of 147 kPa and a temperature of 130°C. Subsequently, 88 g (2.0 mol) of ethylene oxide is further added to this. Next, after confirming that no n-octanol remains, the adduct is placed in a reactor. This is reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80°C for 5 hours. The reaction product is washed with distilled water, and the solvent is removed by distillation under reduced pressure. This affords exemplary compound 53 shown below.

[0093]

[0094] (Method for synthesizing exemplary compound 54) 130 g (1.0 mol) of n-octanol is placed in an autoclave. 116 g (2.0 mol) of propylene oxide is added to this using potassium hydroxide as a catalyst at a pressure of 147 kPa and a temperature of 130°C. 44 g (1.0 mol) of ethylene oxide is then added to this. After confirming that no n-octanol remains, the adduct is placed in a reactor. 47 g (0.33 mol) of phosphoric anhydride is reacted with this in a toluene solution at 80°C for 5 hours. The reaction product is washed with distilled water, and the solvent is removed by distillation under reduced pressure. This affords exemplary compound 54 shown below.

[0095]

[0096] (Method of Synthesizing Exemplary Compound 60) 130 g (1.0 mol) of 2-ethylhexanol is placed in an autoclave. 145 g (2.5 mol) of propylene oxide is added to this using potassium hydroxide as a catalyst under conditions of a pressure of 147 kPa and a temperature of 130°C. Subsequently, 110 g (2.5 mol) of ethylene oxide is further added to this. Next, after confirming that no 2-ethylhexanol remains, the adduct is placed in a reactor. This is reacted with 47 g (0.33 mol) of phosphoric anhydride using a toluene solution at 80°C for 5 hours. The reaction product is washed with distilled water, and the solvent is removed by distillation under reduced pressure. This allows the following exemplary compound 60 to be obtained.

[0097]

[0098] (Method of Synthesizing Exemplary Compound 61) 130 g (1.0 mol) of 2-ethylhexanol is placed in an autoclave. 87 g (1.5 mol) of propylene oxide is added to this using potassium hydroxide as a catalyst under conditions of a pressure of 147 kPa and a temperature of 130°C. 66 g (1.5 mol) of ethylene oxide is then added to this. After confirming that no 2-ethylhexanol remains, the adduct is placed in a reactor. 47 g (0.33 mol) of phosphoric anhydride is reacted with this in a toluene solution at 80°C for 5 hours. The reaction product is washed with distilled water, and the solvent is removed by distillation under reduced pressure. This allows the following exemplary compound 61 to be obtained.

[0099]

[0100] The content of the phosphate ester in the near-infrared absorbing composition is preferably in the range of 0.5 to 20 mass%, more preferably in the range of 1 to 10 mass%. By having the content in this range, both dispersion stability and moist heat resistance can be more satisfactorily achieved.

[0101] [Solvent] The near-infrared absorbing composition of the present invention contains a solvent, and is characterized in that the solvent contains at least an ether-based solvent.

[0102] The inclusion of an ether-based solvent improves the dispersibility of other components, which in turn makes it easier to form a copper complex and improves the visible light transmittance of the cured film of the near-infrared absorbing composition.

[0103] Examples of ether solvents include anisole, diethyl ether, dibutyl ether, diisopropyl ether, tetrahydrofuran, 1,4-dioxane, 2,3-dimethyl-1,4-dioxane, ethylene glycol monomethyl ether, 2-propylene glycol monomethyl ether cyclopentyl methyl ether, 4-methyltetrahydropyran, and 2-methyltetrahydrofuran.

[0104] From the viewpoint of dispersibility of other components, the ether solvent preferably has a cycloalkyl group or a cycloether group. Preferred cycloalkyl groups are cyclopentyl and cyclohexyl groups. Preferred cycloether groups are tetrahydrofuran and tetrapyran groups.

[0105] The structures of ether solvents suitable for the present invention are shown below.

[0106]

[0107] The near-infrared absorbing composition of the present invention may contain a solvent other than the ether-based solvent, as long as the effect of the present invention is not impaired.

[0108] Examples of solvents other than ether solvents include hexane, heptane, cyclohexane, methylcyclohexane, methanol, ethanol, n-propanol, ethylene glycol, acetone, methyl ethyl ketone, toluene, xylene, mesitylene, cyclohexylbenzene, isopropyl biphenyl, methylene chloride, 1,1,2-trichloroethane, chloroform, 2-ethylhexane, 2-pentanol, sec-butylbenzene, and 2-methylcyclohexylbenzene.

[0109] The content of the solvent in the near-infrared absorbing composition is preferably in the range of 61 to 98 mass %, more preferably in the range of 70 to 95 mass %. When the content is in this range, dispersion stability can be maintained and better long-term storage is possible.

[0110] [Antioxidant] The near-infrared absorbing composition of the present invention is characterized by containing at least one antioxidant selected from a phenol-based antioxidant having a structure represented by the following general formula (1), an amine-based antioxidant having a structure represented by the following general formula (2), a phosphorus-based antioxidant having a structure represented by the following general formula (3) or (4), and a sulfur-based antioxidant having a structure represented by the following general formula (5).

[0111]

[0112] [In the general formulas (1) to (5), R 3 is an alkyl group having 1 to 4 carbon atoms. 4 ~R 9 is a substituent selected from a hydroxy group, an acyloxy group, and an alkyl group. 4 ~R 9 At least one of R is a hydroxy group and the other at least one is an acyloxy group. 10 is oxygen or an alkylene ester group having 1 to 20 carbon atoms, and may further have a substituent. 11 and R 12 is hydrogen, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. 13 ~R 21 is an alkyl group or aryl group having 1 to 20 carbon atoms, and may further have a substituent. 15 and R 16 may be bonded to each other.

[0113] The alkylene ester group is a divalent linking group represented by the following structural formula: In the structural formula, * represents a bonding site. *—(CH 2 ) n -COO-*

[0114] The antioxidant prevents oxidation of the ether-based solvent and contributes to reducing the risk of explosion. Furthermore, when used in combination with the ether-based solvent, the antioxidant also contributes to improving the dispersibility and dispersion stability of the phosphonate copper complex.

[0115] The near-infrared absorbing composition of the present invention preferably contains at least one selected from the phenolic antioxidant and the amine antioxidant. The phenolic antioxidant or the amine antioxidant functions as a radical chain inhibitor. Furthermore, if the antioxidant forms a copper complex, it may precipitate and adversely affect the optical properties, etc., of the cured film. However, the phenolic antioxidant and the amine antioxidant are less likely to form a copper complex, and therefore are less likely to adversely affect the optical properties, etc., of the cured film, and are therefore also preferred in this respect.

[0116] From the viewpoint of suppressing an increase in peroxides, the near-infrared absorbing composition of the present invention more preferably contains at least one selected from the phenol-based antioxidant and the amine-based antioxidant, and at least one selected from the phosphorus-based antioxidant and the sulfur-based antioxidant. The phenol-based antioxidant or the amine-based antioxidant functions as a radical chain inhibitor. The phosphorus-based antioxidant or the sulfur-based antioxidant functions as a peroxide decomposer. By using these antioxidants in combination, an increase in peroxides can be effectively suppressed.

[0117] Examples of antioxidants having structures represented by general formulas (1) to (5) are shown below.

[0118] (Examples of phenolic antioxidants having a structure represented by general formula (1))

[0119] (Examples of amine-based antioxidants having a structure represented by general formula (2))

[0120] (Examples of phosphorus-based antioxidants having a structure represented by general formula (3) or (4))

[0121] (Examples of sulfur-based antioxidants having a structure represented by general formula (5))

[0122] For reference, antioxidants not having the structures represented by general formulas (1) to (5) are exemplified below. When these antioxidants are used, the cured product of the near-infrared absorbing composition is likely to become discolored.

[0123] (Examples of phenolic antioxidants not having the structure represented by general formula (1))

[0124] (Examples of phosphorus-based antioxidants not having a structure represented by general formula (3) or (4))

[0125] The antioxidants mentioned above are manufactured by the following manufacturers: Sumilizer series: Sumitomo Chemical Co., Ltd. Adeka Stab series: ADEKA Corporation Sanol series: Sankyo Co., Ltd. Tinuvin series: BASF Corporation Irganox series: BASF Corporation

[0126] The total content of the antioxidant in the near-infrared absorbing composition is preferably in the range of 0.001 to 6 mass %, more preferably in the range of 0.005 to 3 mass %. When the content is in this range, the antioxidant function of the ether-based solvent can be appropriately exhibited.

[0127] [Titanium Coupling Agent] The near-infrared absorbing composition of the present invention preferably contains a titanium coupling agent. This improves the dispersion stability of the phosphonate copper complex, thereby reducing the haze of the cured film formed from the near-infrared absorbing composition and improving the visible light transmittance. Furthermore, the formation of a titanium coupling agent film by the crosslinking reaction of the titanium coupling agent can inhibit water penetration from the film surface, improving the moisture resistance of the cured film. Furthermore, the titanium coupling agent film also blocks oxygen, thereby suppressing the generation of peroxides derived from ether-based solvents. Furthermore, physical adsorption or crosslinking between the titanium coupling agent and the phosphonate copper complex suppresses the thermal vibration of the phosphonate copper complex, improving the heat resistance of the cured film.

[0128] The titanium coupling agent is preferably a compound having a structure represented by the following general formula (III) or (IV).

[0129] General formula (III) (R 3 O) 4-m Ti(O-R 4 -OH) m General formula (IV) (R 3 O) 4-m Ti(OCOR 5 ) m

[0130] [In general formulas (III) and (IV), m is an integer of 1 to 4. 3 and R 5 are each independently an alkyl group having 1 to 30 carbon atoms, and may further have a substituent. 4 is an alkylene group having 1 to 30 carbon atoms, which may further have a substituent.

[0131] R 3 and R 5 The alkyl group having 1 to 30 carbon atoms represented by the formula (I) may be linear or branched. Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, a tert-butyl group, an n-hexyl group, a 2-ethylhexyl group, an n-octyl group, a 2-butyloctyl group, a 2-hexyloctyl group, an n-decyl group, a 2-hexyldecyl group, an n-dodecyl group, and an n-stearyl group. Each alkyl group may further have a substituent. The number of carbon atoms in the alkyl group is preferably 6 to 20.

[0132] R 4 The alkylene group having 1 to 30 carbon atoms, represented by the formula (I), may be linear or branched. Examples of the alkylene group include a methylene group, an ethylene group, an n-propylene group, an isopropylene group, an n-butylene group, a tert-butylene group, an n-hexylene group, a 2-ethylhexylene group, an n-octylene group, a 2-butyloctylene group, a 2-hexyloctylene group, an n-decylene group, a 2-hexyldecylene group, an n-dodecylene group, an n-stearylene group, and a 1-propyl-2-ethyl-propylene group. Each alkylene group may further have a substituent. The alkylene group preferably has 6 to 20 carbon atoms.

[0133] R 3 ~R 5Examples of the substituents that each of the groups may have include alkoxy groups (e.g., methoxy groups, ethoxy groups, etc.), halogen atoms (e.g., fluorine atoms, etc.), cyano groups, nitro groups, dialkylamino groups (e.g., dimethylamino groups, etc.), trialkylsilyl groups (e.g., trimethylsilyl groups, etc.), triarylsilyl groups (e.g., triphenylsilyl groups, etc.), triheteroarylsilyl groups (e.g., tripyridylsilyl groups, etc.), benzyl groups, aryl groups (e.g., phenyl groups, etc.), heteroaryl groups (e.g., pyridyl groups, carbazolyl groups, etc.), trifluoromethyl groups, etc., and examples of fused rings include 9,9'-dimethylfluorene, carbazole, dibenzofuran, etc.

[0134] Examples of compounds having a structure represented by general formula (III) include titanium alkylene glycolates.

[0135] Specific examples of the compound having the structure represented by general formula (III) are shown below: The compound having the structure represented by general formula (III) according to the present invention is not limited to these.

[0136]

[0137]

[0138] Compounds having the structure represented by general formula (III) are also available as commercially available products, such as Orgatix TC-245 (manufactured by Matsumoto Fine Chemical Co., Ltd.).

[0139] Examples of compounds having a structure represented by general formula (IV) include titanium isostearate and polyhydroxytitanium stearate.

[0140] Specific examples of the compound having the structure represented by general formula (IV) are shown below: The compound having the structure represented by general formula (IV) according to the present invention is not limited to these.

[0141]

[0142] Compounds having a structure represented by general formula (IV) are also available as commercially available products, such as Orgatix TC-800, Orgatix ZC-200, and Orgatix ZC-320 (all manufactured by Matsumoto Fine Chemical Co., Ltd.), TBSTA, DPSTA-25, S-151, S-152, S-181, and TBP (all manufactured by Nippon Soda Co., Ltd.), and Plainact TTS (manufactured by Ajinomoto Fine-Techno Co., Inc.).

[0143] The compound having the structure represented by the above general formula (III) or (IV) can also be obtained by referring to the synthesis method described in, for example, JP-A-2011-219704.

[0144] The content of the titanium coupling agent in the near-infrared absorbing composition is preferably in the range of 0.05 to 10 mass%, more preferably in the range of 0.1 to 1 mass%. When the content is in this range, the dispersion stability of the dispersion, the moist heat resistance of the cured film, and the heat resistance of the cured film can be well balanced.

[0145] [Acetate Ion Concentration] The near-infrared absorbing composition of the present invention preferably has an acetate ion concentration of 0.5% by mass or less. Near-infrared absorbing compositions containing a copper complex are generally prepared using copper acetate. Therefore, near-infrared absorbing compositions often contain acetate ions. However, acetate ions reduce the dispersion stability of the phosphonate copper complex and inhibit the function of the antioxidant. Therefore, a low acetate ion concentration is preferable. Specifically, an acetate ion concentration of 0.5% by mass or less can prevent the dispersion stability of the phosphonate copper complex from decreasing and the function of the antioxidant from being inhibited.

[0146] The acetate ion concentration can be measured by the following procedure. Approximately 2 g of the near-infrared absorbing composition is mixed with 2.5 mL of ultrapure water and shaken for 10 minutes. This mixture is centrifuged, and the aqueous phase is removed. The acetate ion concentration of the removed aqueous phase is measured using an organic acid running buffer and a capillary electrophoresis device.

[0147] The acetate ion concentration in the near-infrared absorbing composition can be reduced by azeotropic treatment. Specifically, the acetate ion concentration in the near-infrared absorbing composition can be reduced by azeotropically treating the near-infrared absorbing composition using, for example, methylcyclohexane, toluene, or the like as an azeotropic solvent.

[0148] [Other Components] The near-infrared absorbing composition of the present invention may contain other components within a range that does not impair the effects of the present invention. Examples of other components include a sensitizer, a crosslinking agent, a curing accelerator, a filler, a thermal curing accelerator, a thermal polymerization inhibitor, a plasticizer, a conductive particle, a bulking agent, an antifoaming agent, a flame retardant, a leveling agent, a release accelerator, a fragrance, a surface tension adjuster, a chain transfer agent, etc.

[0149] For these components, reference can be made to the contents described in, for example, paragraphs

[0183] to

[0260] of JP-A No. 2012-003225, paragraphs

[0101] to

[0102] of JP-A No. 2008-250074, paragraphs

[0103] to

[0104] of JP-A No. 2008-250074, paragraphs

[0107] to

[0109] of JP-A No. 2008-250074, and the like.

[0150] [Near-infrared absorbing cured film] The near-infrared absorbing composition of the present invention can be used to form a near-infrared absorbing cured film.

[0151] The near-infrared absorbing cured film can be formed, for example, by the following procedure: A coating liquid is prepared by mixing a near-infrared absorbing composition and a curable resin. The coating liquid is applied to a substrate by a wet coating method such as spin coating or using a dispenser to form a coating film. The coating film is cured by a predetermined heat treatment. This allows the near-infrared absorbing cured film to be formed.

[0152] The thickness of the near-infrared absorbing cured film is preferably in the range of 10 to 500 μm, more preferably in the range of 10 to 300 μm.

[0153] The film thickness of the near-infrared absorbing cured film can be measured using, for example, a film thickness meter combining the following devices: Terminal: DIGIMICRO MH-15M (manufactured by NIKON Corporation) Stand: DIGIMICRO STAND MS-5C (manufactured by NIKON Corporation) Reader: DIGITAL READ OUT TC-101A (manufactured by NIKON Corporation)

[0154] The curable resin used to form the near-infrared absorbing cured film preferably has optical transparency to visible light and near-infrared light, and is capable of dispersing the fine particles in the near-infrared absorbing composition.

[0155] The copper phosphonate complex is a substance with relatively low polarity and disperses well in hydrophobic materials, so the curable resin is preferably a resin having a polysiloxane structure (silicone) or a resin having an acrylic group, an epoxy group, or a phenyl group.

[0156] Among these, resins having a polysiloxane structure are particularly preferred because they are resistant to thermal decomposition, have high optical transparency for visible light and near-infrared light, and are highly heat-resistant.

[0157] Specific examples of resins having a polysiloxane structure include KR-255, KR-300, KR-2621-1, KR-211, KR-311, KR-216, KR-212, and KR-251 manufactured by Shin-Etsu Chemical Co., Ltd., and SS-6203, SS-6309, VS-9301, and VS-9506 manufactured by Sanyu Rec Co., Ltd.

[0158] From the viewpoint of low gas permeability and moisture resistance, it is also preferable to use a matrix resin having an epoxy group as the curable resin.

[0159] Specific examples of resins having an epoxy group include KJC-X5 (manufactured by Shin-Etsu Chemical Co., Ltd.), NLD-L-672 (manufactured by Sanyu Rec Co., Ltd.), LE-1421 (manufactured by Sanyu Rec Co., Ltd.), and EpiFine series (manufactured by KISCO Corporation).

[0160] It is also preferable to use a resin having both a polysiloxane structure and an epoxy group as the curable resin. Such a resin exhibits high heat resistance and moisture resistance, and therefore has properties suitable for use as a material for an image sensor for a solid-state imaging device.

[0161] Specific examples of resins having both a polysiloxane structure and an epoxy group include the EpiFine series (manufactured by KISCO Corporation) and the ILLUMIKA series (manufactured by Kaneka Corporation).

[0162] [Optical Member] The optical member of the present invention is characterized by containing a cured product of the near-infrared absorbing composition. The cured product of the near-infrared absorbing composition is, for example, the above-mentioned near-infrared absorbing cured film.

[0163] Examples of optical components include visibility correction components for CCDs, visibility correction components for CMOSs, visibility correction components for other light receiving elements, photometric components, heat ray absorbing components, optical filters, fiber components (optical fibers), noise cutting components, display covers or display filters such as plasma display front panels, projector front panels, light source heat ray cutting components, color tone correction components, illumination brightness adjustment components, components for light amplification elements, components for wavelength conversion elements, components for Faraday elements, components for isolators, components for optical disks, and the like.

[0164] Examples of uses of optical members containing a cured product of the near-infrared absorbing composition are given below.

[0165] (Near-infrared cut filter) The optical member of the present invention is, for example, a near-infrared cut filter. The near-infrared cut filter includes, for example, a transparent dielectric substrate and a near-infrared absorbing layer on at least one surface thereof. The near-infrared absorbing layer is a cured product of the near-infrared absorbing composition of the present invention.

[0166] It is preferable to further provide a dielectric multilayer film on at least one surface of the transparent dielectric substrate, since this allows more flexible adjustment of the spectral characteristics of the near-infrared cut filter.

[0167] The near-infrared absorbing layer and the dielectric multilayer film may be provided in contact with the transparent dielectric substrate, or may be provided via an intermediate layer.

[0168] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a near-infrared cut filter.

[0169] The near-infrared cut filter 9 shown in FIG. 1 comprises a near-infrared absorbing layer 22 on one surface of a transparent dielectric substrate 21, and further comprises a dielectric multilayer film 23 on the other surface.

[0170] The material of the transparent dielectric substrate is not particularly limited, and may be made of, for example, glass or an optical resin such as polycarbonate (PC), polymethyl methacrylate (PMMA), cycloolefin polymer (COP), or silicone.

[0171] The thickness of the transparent dielectric substrate is preferably within the range of 0.01 to 1 mm.

[0172] The transparent dielectric substrate is required to transmit visible light, and therefore preferably has an average spectral transmittance of 80% or more in the wavelength range of 450 to 600 nm.

[0173] A dielectric multilayer film is a film formed by laminating multiple layers made of materials with different refractive indices, and is used to control the transmittance of each wavelength of light. By providing a dielectric multilayer film together with a near-infrared absorbing layer, the spectral characteristics of the near-infrared cut filter can be adjusted more freely.

[0174] The spectral characteristics of the dielectric multilayer film can be adjusted by the thickness and material of each layer of the dielectric multilayer film, and the material of each layer can be, for example, titanium oxide, silicon oxide, aluminum oxide, zirconium oxide, tantalum pentoxide, niobium pentoxide, lanthanum oxide, yttrium oxide, zinc oxide, zinc sulfide, indium oxide, silica, alumina, lanthanum fluoride, magnesium fluoride, sodium aluminum hexafluoride, or other dielectric materials.

[0175] A near-infrared cut filter having a dielectric multilayer film can be produced by laminating each dielectric layer on a transparent dielectric substrate by a method such as vacuum deposition, chemical vapor deposition, sputtering, etc. A near-infrared cut filter having a dielectric multilayer film can also be produced by bonding a separately prepared dielectric multilayer film to a transparent dielectric substrate with an adhesive.

[0176] (Image Sensor for Solid-State Imaging Device) The near-infrared cut filter can be provided in an image sensor for a solid-state imaging device. The image sensor for a solid-state imaging device is a component mainly composed of a solid-state imaging device substrate equipped with a light receiving element. In addition to the near-infrared cut filter, the image sensor for a solid-state imaging device may also include a planarizing layer, a glass substrate, etc.

[0177] FIG. 2 is a schematic cross-sectional view showing an example of the configuration of an image sensor for a solid-state imaging device.

[0178] 2 is composed of a solid-state imaging element substrate 10 having a light-receiving element on the light-receiving surface of a silicone substrate, a planarization layer 8 provided on the solid-state imaging element substrate 10, a near-infrared cut filter 9 provided on the planarization layer 8, and a glass substrate 3 (light-transmitting substrate) arranged above the near-infrared cut filter 9. Each member is bonded with an adhesive 2.

[0179] (Camera Module) The image sensor for a solid-state imaging device can be provided in a camera module. The camera module may be composed of an imaging lens, a lens holder, a light-shielding and electromagnetic shield, etc. in addition to the image sensor for a solid-state imaging device.

[0180] FIG. 3 is a schematic cross-sectional view showing an example of the configuration of a camera module.

[0181] The camera module 1 shown in Fig. 3 is configured to include a solid-state imaging element image sensor similar to that shown in Fig. 2, a lens holder 5, an imaging lens 4, and a light-shielding and electromagnetic shield 6. As in Fig. 2, the solid-state imaging element image sensor is configured to include a solid-state imaging element substrate 10, a planarizing layer 8, a near-infrared cut filter 9, and a glass substrate 3. The light-shielding and electromagnetic shield 6 is disposed so as to surround the periphery of the solid-state imaging element image sensor. Each component is bonded with an adhesive 7.

[0182] Furthermore, the camera module 1 is connected to a circuit board 12, which is a mounting board, via solder balls 11 (connecting material), which are connecting members.

[0183] In the camera module 1 , incident light L from the outside passes through the imaging lens 4 , the glass substrate 3 , the near-infrared cut filter 9 and the planarization layer 8 in this order, before reaching the light receiving element of the solid-state imaging element substrate 10 .

[0184] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, operations were carried out at room temperature (25°C). In the following examples, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0185] <Synthesis of Phosphate Ester> Exemplary Compounds 63, 75, and 79, which are phosphate esters, were synthesized according to the following procedure.

[0186] (Synthesis Procedure for Exemplary Compound 63) 130 g (1.0 mol) of 2-ethylhexanol was placed in an autoclave. 116 g (2.0 mol) of propylene oxide was added to this using potassium hydroxide as a catalyst under conditions of a pressure of 147 kPa and a temperature of 130°C. Subsequently, 88 g (2.0 mol) of ethylene oxide was further added to this. Next, after confirming that no 2-ethylhexanol remained, the adduct was placed in a reactor. This was reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80°C for 5 hours. The reaction product was washed with distilled water, and the solvent was distilled off under reduced pressure. Thus, Exemplary Compound 63 was obtained.

[0187] (Synthesis Procedure for Exemplary Compound 75) 186 g (1.0 mol) of n-dodecanol was placed in an autoclave. 87 g (1.5 mol) of propylene oxide was added to the autoclave using potassium hydroxide as a catalyst under conditions of a pressure of 147 kPa and a temperature of 130°C. 66 g (1.5 mol) of ethylene oxide was then added to the autoclave. After confirming that no n-dodecanol remained, the adduct was placed in a reactor. 47 g (0.33 mol) of phosphoric anhydride was reacted with the adduct in toluene at 80°C for 5 hours. The reaction product was washed with distilled water, and the solvent was removed by distillation under reduced pressure. Exemplary Compound 75 was thus obtained.

[0188] (Synthesis Procedure for Exemplary Compound 79) 186 g (1.0 mol) of n-dodecanol was placed in an autoclave. 116 g (2.0 mol) of propylene oxide was added to the autoclave using potassium hydroxide as a catalyst at a pressure of 147 kPa and a temperature of 130°C. Subsequently, 88 g (2.0 mol) of ethylene oxide was further added to the autoclave. After confirming that no n-dodecanol remained, the adduct was placed in a reactor. This was reacted with 47 g (0.33 mol) of phosphoric anhydride in toluene at 80°C for 5 hours. The reaction product was washed with distilled water, and the solvent was removed by distillation under reduced pressure. Exemplary Compound 79 was thus obtained.

[0189] <Preparation of Antioxidant-Containing Solvents> The solvents and antioxidants listed in Table VI were mixed to prepare antioxidant-containing solvents 1 to 21. Details of the antioxidants used are as described above.

[0190]

[0191] <Preparation of near-infrared absorbing composition 1> Copper (II) acetate monohydrate [1.82 g, 10 mmol] and antioxidant-containing solvent 1 [82 g] were mixed and stirred for 3 hours. This liquid was filtered to remove insoluble matter. The resulting solution was designated solution A.

[0192] Plysurf A208N (1.6 mmol) as a phosphate ester was dissolved in antioxidant-containing solvent 1 (7 g). Solution A was added to the solution and stirred at room temperature for 30 minutes. The resulting solution was designated as solution B.

[0193] Propylphosphonic acid (8.8 mmol) as phosphonic acid was dissolved in antioxidant-containing solvent 1 (7 g). The resulting solution was designated solution C.

[0194] Solution C was added to Solution B while stirring. The mixture was stirred at room temperature for 16 hours. The resulting solution was designated Solution D.

[0195] The entire amount of Solution D and 30 g of methylcyclohexane were placed in a flask. While heating this in an oil bath (Tokyo Rikakikai Co., Ltd., model: OSB-2100) at 50 to 100°C, a solvent removal and acetic acid removal treatment was carried out for 40 minutes using a rotary evaporator (Tokyo Rikakikai Co., Ltd., model: N-1000). As a result, the concentration of the near-infrared absorber (phosphonic acid copper complex and phosphate ester) in this system was adjusted to 20 mass%. This treatment of Solution D is called azeotropic treatment.

[0196] Thereafter, the antioxidant-containing solvent 1 was added to this system to adjust the concentration of the near-infrared absorber (phosphonic acid copper complex and phosphate ester) to 10 mass %, thereby obtaining a near-infrared absorbing composition 1.

[0197] <Preparation of Near-Infrared Absorbing Compositions 2 to 25 and 31 to 36> Near-infrared absorbing compositions 2 to 25 and 31 to 36 were prepared in the same manner as in the preparation of near-infrared absorbing composition 1, except that the types of the antioxidant-containing solvent, phosphonic acid, and phosphoric acid ester used were changed as shown in Table VII, respectively.

[0198] The amount of phosphate ester added in Solution B was 1.6 mmol, regardless of the type of phosphate ester, and the amount of phosphonic acid added in Solution C was 8.8 mmol, regardless of the type of phosphonic acid.

[0199] Near infrared absorbing compositions with "none" in the "azeotropic treatment" column in Table VII were prepared without azeotropic treatment.

[0200] <Preparation of Near-Infrared Absorbing Composition 26> A near-infrared absorbing composition 26′ having a concentration of the near-infrared absorbent (phosphonic acid copper complex and phosphate ester) of 10 mass% was prepared in the same manner as in the preparation of the near-infrared absorbing composition 1, except that the types of the antioxidant-containing solvent, phosphonic acid, and phosphate ester to be used were changed as shown in Table VII, respectively.

[0201] Orgatix TC-245 (organic titanium compound, manufactured by Matsumoto Fine Chemical Co., Ltd.) as a titanium coupling agent was dissolved in the antioxidant-containing solvent 2 to prepare a titanium coupling agent solution with a titanium coupling agent concentration of 10% by mass.

[0202] The titanium coupling agent solution (0.5 parts by mass) was added to the near-infrared absorbing composition 26′ (10 parts by mass), and the mixture was stirred at room temperature for 10 minutes to prepare a near-infrared absorbing composition 26. In the near-infrared absorbing composition 26, the content of the titanium coupling agent was 5% by mass when the content of the near-infrared absorbent (phosphonic acid copper complex and phosphate ester) was taken as 100% by mass.

[0203] <Preparation of near-infrared absorbing compositions 27 to 30>

[0204] Near infrared absorbing compositions 27 to 30 were prepared in the same manner as in the preparation of near infrared absorbing composition 26, except that the types of the antioxidant-containing solvent, phosphonic acid, phosphate ester, and titanium coupling agent to be used were changed as shown in Table VII, respectively.

[0205] Orgatix TC-800 used as a titanium coupling agent in the preparation of near-infrared absorbing compositions 27 to 30 is an organic titanium compound manufactured by Matsumoto Fine Chemical Co., Ltd.

[0206] <Measurement of Acetate Ion Concentration> Approximately 2 g of the near-infrared absorbing composition was mixed with 2.5 mL of ultrapure water and shaken for 10 minutes. This mixture was centrifuged, and the aqueous phase was removed. The acetate ion concentration of the removed aqueous phase was measured using an organic acid running buffer and a capillary electrophoresis device. The measured acetate ion concentrations were as shown in Table VII.

[0207] <Evaluation of Dispersibility> The near-infrared absorbing composition immediately after preparation was diluted with toluene to a solids concentration of 0.5% by mass. The average particle size of the fine particles in the diluted dispersion was measured by dynamic light scattering using a zeta potential / particle size measurement system (ELSZ-1000ZS, manufactured by Otsuka Electronics Co., Ltd.). Based on the measured average particle size, the dispersibility was evaluated according to the following evaluation criteria. The evaluation results are shown in Table VIII.

[0208] AA: The average particle size is 100 nm or less. A: The average particle size is more than 100 nm and not more than 500 nm. B: The average particle size is more than 500 nm and not more than 1000 nm. C: The average particle size is more than 1000 nm.

[0209] <Evaluation of Liquid Storage Stability> After leaving the near-infrared absorbing composition at room temperature for one month, it was diluted with toluene so that the solid content concentration was 0.5 mass %. The average particle size of the fine particles in the diluted dispersion was measured by a dynamic light scattering method using a zeta potential / particle size measurement system (ELSZ-1000ZS, manufactured by Otsuka Electronics Co., Ltd.).

[0210] Based on the measured average particle size, the storage stability was evaluated according to the following evaluation criteria, and the evaluation results are shown in Table VIII.

[0211] AA: The average particle size is 100 nm or less. A: The average particle size is more than 100 nm and not more than 500 nm. B: The average particle size is more than 500 nm and not more than 1000 nm. C: The average particle size is more than 1000 nm.

[0212] <Evaluation of Heat Discoloration Resistance> Three drops of the near-infrared absorbing composition were placed on a glass slide and heated on a hot plate at 70°C. A glass slide was placed on the droplets, and the two glass slides were bonded together. This was heated at 150°C for 15 minutes, and further heated at 175°C for 15 minutes. The tristimulus values ​​X, Y, and Z of the light source color defined in JIS Z8701 of this sample were measured using a spectrophotometer (Spectrophotometer V-780, manufactured by JASCO Corporation).

[0213] The yellow index (yellowness index) YI was calculated from the following formula: YI=100(1.2985X-1.1335Z) / Y

[0214] Furthermore, ΔYI was calculated from the following formula: ΔYI=YI-YI 0 YI 0 : YI when a near-infrared absorbing composition containing no antioxidant was evaluated in the same manner

[0215] Based on the calculated ΔYI, the resistance to heat discoloration was evaluated according to the following evaluation criteria, and the evaluation results are shown in Table VIII.

[0216] A: ΔYI is 1 or less. B: ΔYI is more than 1 and 3 or less. C: ΔYI is more than 3.

[0217] <Evaluation of Peroxide Increase Resistance> Samples were prepared by adding 0.35% by mass of each antioxidant to antioxidant-free tetrahydrofuran. This sample was dissolved in a titration solvent, a mixed solvent of acetic acid and chloroform (3:2). A saturated potassium iodide solution was added to the sample in a nitrogen atmosphere, and the container was sealed. The container was left in the dark for approximately 10 minutes to liberate iodine. After leaving the sample, it was titrated with a sodium thiosulfate standard solution to determine the amount of peroxide [meq / kg]. The titration was performed by potentiometric titration using an automatic titrator and a platinum electrode. The automatic titrator used was a GT-200 manufactured by Mitsubishi Chemical Analytech Co., Ltd. After leaving the sample at room temperature for one month, it was titrated again to determine the amount of peroxide [meq / kg]. The amount of peroxide increase [meq / kg] was calculated from the amount of peroxide before and after leaving it for one month.

[0218] Based on the calculated peroxide increase amount [meq / kg], the resistance to peroxide increase was evaluated according to the following evaluation criteria. The evaluation results are shown in Table VIII.

[0219] AA: The amount of peroxide increase is 5 meq / kg or less. A: The amount of peroxide increase is more than 5 meq / kg and 10 meq / kg or less. B: The amount of peroxide increase is more than 10 meq / kg and 15 meq / kg or less. C: The amount of peroxide increase is more than 15 meq / kg.

[0220]

[0221]

[0222] From the above results, it can be confirmed that the near-infrared absorbing composition of the present invention has the function of preventing oxidation of the solvent, and is resistant to coloration by heating.

[0223] The present invention can be used in near-infrared absorbing compositions and optical components.

[0224] REFERENCE SIGNS LIST 1 camera module 2 adhesive 3 glass substrate 4 imaging lens 5 lens holder 6 light-shielding and electromagnetic shield 7 adhesive 8 planarizing layer 9 near-infrared cut filter 10 solid-state imaging element substrate 11 solder ball 12 circuit board 14 image sensor for solid-state imaging element 21 transparent dielectric substrate 22 near-infrared absorbing layer 23 dielectric multilayer film

Claims

1. A near-infrared absorbing composition containing a phosphonic acid copper complex, further containing a phosphoric acid ester, a solvent, and an antioxidant, wherein the solvent contains at least an ether-based solvent, and the antioxidant contains at least one selected from a phenol-based antioxidant having a structure represented by the following general formula (1), an amine-based antioxidant having a structure represented by the following general formula (2), a phosphorus-based antioxidant having a structure represented by the following general formula (3) or (4), and a sulfur-based antioxidant having a structure represented by the following general formula (5). [In the general formulas (1) to (5), R 3 is an alkyl group having 1 to 4 carbon atoms. 4 ~R 9 is a substituent selected from a hydroxy group, an acyloxy group, and an alkyl group. 4 ~R 9 At least one of R is a hydroxy group and the other at least one is an acyloxy group. 10 is oxygen or an alkylene ester group having 1 to 20 carbon atoms, which may further have a substituent. 11 and R 12 is hydrogen, an alkyl group having 1 to 20 carbon atoms, or an alkoxy group having 1 to 20 carbon atoms. 13 ~R 21 R is an alkyl group or an aryl group having 1 to 20 carbon atoms, which may further have a substituent. 15 and R 16 may be bonded to each other.

2. The near infrared absorbing composition according to claim 1, further comprising a titanium coupling agent.

3. The near infrared absorbing composition according to claim 1, wherein the acetate ion concentration is 0.5 mass % or less.

4. The near infrared absorbing composition according to claim 1, wherein the phosphoric acid ester has a structure represented by the following general formula (II): [In the general formula (II), R 2 represents an alkyl group having 1 to 20 carbon atoms or an aryl group having 6 to 20 carbon atoms, which may further have a substituent. 21 ~R 24 each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 21 ~R 24 represents the average number of partial structural units added that are all hydrogen atoms, and is in the range of 1 to 19. 21 ~R 24 represents the average number of partial structural units added, at least one of which is an alkyl group having 1 to 4 carbon atoms, and is within the range of 1 to 19. m+n is the total number of m and n, and is within the range of 2 to 20. Z represents a structural unit selected from the following formulae (Z-1) and (Z-2).

5. The near infrared absorbing composition according to claim 1, comprising, as the antioxidant, at least one selected from the group consisting of the phenol-based antioxidant and the amine-based antioxidant, and at least one selected from the group consisting of the phosphorus-based antioxidant and the sulfur-based antioxidant.

6. The near infrared absorbing composition according to claim 1, wherein the antioxidant is at least one selected from the group consisting of the phenol-based antioxidant and the amine-based antioxidant.

7. The near infrared absorbing composition according to claim 1, wherein the content of the solvent is within the range of 61 to 98 mass %.

8. An optical component comprising a cured product of the near infrared absorbing composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Near-infrared absorbing composition, near-infrared absorbing film, and image sensor for solid-state imaging element

    JP2019081896A

  • Housing member

    JP2022116998A

  • Resin composition and application therefor

    WO2014027639A1

  • Method for producing near-infrared absorbent, near-infrared absorbent and use of same

    WO2014119618A1

  • Resin composition and use thereof

    WO2014175231A1