Composition for semiconductor device processing and method for producing modified substrate
The composition of a polymer with ethylenically unsaturated groups and a polymerization inhibitor ensures selective film formation on metal surfaces in semiconductor processing, addressing the challenge of maintaining surface selectivity after storage by inhibiting polymer molecular weight increase, thus enhancing semiconductor device processing.
Patent Information
- Application Number
- PCT/JP2024/015841
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2024-04-23
- Publication Date
- 2024-11-21
AI Technical Summary
Existing semiconductor processing methods struggle to selectively form films on metal-containing surfaces while maintaining selectivity after storage, as they tend to form films on non-metal surfaces due to unintended polymerization and molecular weight increases, making it difficult to preferentially modify metal surfaces.
A composition comprising a polymer with ethylenically unsaturated groups and specific functional groups that interact with metal atoms, combined with a polymerization inhibitor and a solvent, is used to form a film preferentially on metal surfaces, even after storage, by inhibiting polymer molecular weight increase and enhancing surface selectivity.
The solution allows for the effective and selective formation of films on metal surfaces, maintaining preferential modification even after storage, thereby improving semiconductor device processing by ensuring precise surface modification and film formation on intended metal-containing areas.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Composition for treating semiconductor devices, method for producing modified substrates
[0001] The present invention relates to compositions for semiconductor device processing and methods for making modified substrates.
[0002] In advanced semiconductors, there is a demand for technology capable of forming wiring widths of approximately 10 nm. Therefore, methods for selectively modifying substrates having minute regions on their surface have been investigated. This selective modification method requires materials that can modify surface regions easily and with high selectivity, and various materials are being investigated.
[0003] For example, Patent Document 1 discloses a method and composition for selectively modifying a substrate surface that can easily modify a surface region containing a metal with high selectivity and high density, and describes the composition as "a composition used in a method for selectively modifying a substrate surface having a first region containing a metal on its surface layer, the composition comprising a polymer having, at an end of its main chain or side chain, a group containing a first functional group that forms a coordinate bond with the metal, and a solvent, wherein the first functional group is a cyano group, a sulfanyl group, an ethylenic carbon-carbon double bond-containing group, an oxazoline ring-containing group, a phosphate group, an epoxy group, or a disulfide group." It also discloses that the polymer used in the composition may further have a crosslinkable group such as a polymerizable carbon-carbon double bond-containing group.
[0004] Japanese Patent Application Laid-Open No. 2022-161919
[0005] Here, the composition used for the above-mentioned selective surface modification is required to have the same performance even after a certain period of storage as before storage. The present inventors investigated the properties of a composition containing a polymer having an ethylenically unsaturated group, such as a polymerizable carbon-carbon double bond-containing group, as described in Patent Document 1, and confirmed that the composition did not exhibit the above-mentioned performance. More specifically, after storing a composition containing a polymer having a polymerizable functional group for a certain period of time, the composition was brought into contact with substrates having a surface containing metal atoms and a surface not containing metal atoms, and its properties were evaluated. In the case of the above-mentioned composition before storage, a coating was preferentially formed on the surface containing metal atoms, but in the case of the above-mentioned composition after storage, a coating was also likely to be formed on the surface not containing metal atoms, making it difficult to preferentially modify the surface containing metal atoms.
[0006] Therefore, an object of the present invention is to provide a composition for treating semiconductor devices that, when brought into contact with a substrate having a first surface containing metal atoms and a second surface not containing metal atoms, can preferentially form a coating on the first surface and can also preferentially form a coating on the first surface after storage. Another object of the present invention is to provide a method for producing a modified substrate using the composition for treating semiconductor devices.
[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.
[0008] [1] A composition for treating semiconductor devices, comprising: a polymer having an ethylenically unsaturated group and a functional group that interacts with a surface containing metal atoms in a substrate; a polymerization inhibitor; and a solvent. [2] The composition for treating semiconductor devices according to [1], wherein the functional group is a group selected from the group consisting of a nitrogen-containing group, a phosphate group or a salt thereof, a carboxy group or a salt thereof, a hydroxy group, an epoxy group, a hydrolyzable silyl group, a thiol group, and a disulfide group. [3] The composition for treating semiconductor devices according to [1] or [2], wherein the functional group is a cyano group or a phosphate group or a salt thereof. [4] The composition for treating semiconductor devices according to any one of [1] to [3], wherein the ethylenically unsaturated group is a group selected from the group consisting of a vinyl group, a vinyl ether group, a styryl group, an acryloyl group, and a methacryloyl group. [5] The composition for treating a semiconductor device according to any one of [1] to [3], wherein the ethylenically unsaturated group is a group selected from the group consisting of an alkenyl group having 2 to 4 carbon atoms and an alkenylene group having 2 to 4 carbon atoms. [6] The composition for treating a semiconductor device according to any one of [1] to [5], wherein the polymer contains a ring structure. [7] The composition for treating a semiconductor device according to any one of [1] to [6], wherein the polymer contains an aromatic ring structure. [8] The composition for treating a semiconductor device according to any one of [1] to [7], wherein the polymerization inhibitor contains a nitrogen atom. [9] The composition for treating a semiconductor device according to any one of [1] to [8], wherein the polymerization inhibitor comprises at least one compound selected from the group consisting of a phenol-based compound, a quinone-based compound, a free radical-based compound, an amine-based compound, a phosphine-based compound, and a thiol ether-based compound.
[10] The composition for treating semiconductor devices according to any one of [1] to [9], wherein the polymerization inhibitor is a phenolic compound, a quinone compound, or a free radical compound.
[11] The composition for treating semiconductor devices according to any one of [1] to
[10] , wherein the content of the polymerization inhibitor is 0.08 to 200 parts by mass per 100 parts by mass of the polymer.
[12] The composition for treating a semiconductor device according to any one of [1] to
[11] , wherein the solvent comprises at least one solvent selected from the group consisting of ester-based solvents, ketone-based solvents, and alcohol-based solvents.
[13] The composition for treating a semiconductor device according to any one of [1] to
[12] , wherein the solvent comprises at least one solvent selected from the group consisting of propylene glycol monomethyl ether acetate, ethyl lactate, γ-butyrolactone, cyclohexanone, methyl isobutyl ketone, and propylene glycol monomethyl ether.
[14] A method for producing a modified substrate, comprising the steps of contacting a substrate having a first surface containing metal atoms and a second surface not containing metal atoms with the composition for treating a semiconductor device according to any one of [1] to
[13] , and subjecting the substrate contacted with the composition to a heat treatment to form a coating on the first surface.
[15] The method for producing a modified substrate according to
[14] , wherein the second surface comprises an insulator.
[16] The method for producing a modified substrate according to
[14] or
[15] , wherein the second surface comprises silicon.
[17] The method for producing a modified substrate according to any one of
[14] to
[16] , wherein the second surface comprises silicon oxide, silicon nitride, or silicon oxycarbide.
[0009] According to the present invention, there is provided a composition for treating semiconductor devices that, when contacted with a substrate having a first surface containing metal atoms and a second surface not containing metal atoms, is capable of preferentially forming a coating on the first surface and is capable of preferentially forming a coating on the first surface even after storage. There is also provided a method for producing a modified substrate using the composition for treating semiconductor devices.
[0010] 1 is a cross-sectional view of a substrate for fabricating a striped substrate, and FIG. 2 is a cross-sectional view of a striped substrate used for evaluating selective surface modification.
[0011] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.
[0012] The meaning of each description in this specification is explained below. In this specification, a numerical range expressed using "to" means a range including the numerical values before and after "to" as the lower and upper limits. In this specification, a hydrogen atom may be a protist atom (a normal hydrogen atom) or a deuterium atom (e.g., a deuterium atom, etc.). Unless otherwise specified, the compounds described in this specification may contain structural isomers, optical isomers, and isotopes. Furthermore, structural isomers, optical isomers, and isotopes may be present alone or in combination with two or more types. In the description of groups (atomic groups) in this specification, a description that does not indicate substituted or unsubstituted includes both unsubstituted and substituted groups. For example, an "alkyl group" includes not only alkyl groups without a substituent (unsubstituted alkyl groups) but also alkyl groups with a substituent (substituted alkyl groups).
[0013] Unless otherwise specified, the "substituent" in this specification is preferably a monovalent substituent. Examples of the substituent include halogen atoms such as fluorine, chlorine, bromine, and iodine atoms; alkoxy groups such as methoxy, ethoxy, and tert-butoxy groups; aryloxy groups such as phenoxy and p-tolyloxy groups; alkoxycarbonyl groups such as methoxycarbonyl, butoxycarbonyl, and phenoxycarbonyl groups; acyloxy groups such as acetoxy, propionyloxy, and benzoyloxy groups; and acyl groups such as acetyl, benzoyl, isobutyryl, acryloyl, methacryloyl, and methoxalyl groups. alkylsulfanyl groups such as methylsulfanyl and tert-butylsulfanyl; arylsulfanyl groups such as phenylsulfanyl and p-tolylsulfanyl; alkyl groups; cycloalkyl groups; aryl groups; heteroaryl groups; hydroxyl groups; carboxy groups; formyl groups; sulfo groups; cyano groups; alkylaminocarbonyl groups; arylaminocarbonyl groups; sulfonamide groups; silyl groups; amino groups; monoalkylamino groups; dialkylamino groups; arylamino groups; alkylthio groups; and combinations thereof.
[0014] The bonding direction of divalent groups represented in this specification is not limited unless otherwise specified. For example, when Y is -COO- in a compound represented by the formula "X-Y-Z", Y may be -CO-O- or -O-CO-. In addition, the compound may be "X-CO-O-Z" or "X-O-CO-Z".
[0015] In this specification, with respect to a compound that may have geometric isomers (cis-trans isomers), the formula representing the compound may be described in only one of the cis and trans forms for convenience. Even in such cases, unless otherwise specified, the form of the compound is not limited to either the cis or trans form, and the compound may be in either the cis or trans form.
[0016] In this specification, "(meth)acrylic" is a generic term including acrylic and methacrylic, and means "at least one of acrylic and methacrylic." Similarly, "(meth)acrylic acid" means "at least one of acrylic acid and methacrylic acid."
[0017] In this specification, "radiation" refers to, for example, the bright line spectrum of a mercury lamp, far ultraviolet light typified by excimer lasers, extreme ultraviolet light (EUV light: Extreme Ultraviolet), X-rays, electron beams (EB), etc. In this specification, "light" refers to actinic rays or radiation.
[0018] In this specification, unless otherwise specified, the weight average molecular weight (Mw), number average molecular weight (Mn), and dispersity (also referred to as molecular weight distribution) (Mw / Mn) of a polymer are defined as polystyrene-equivalent values measured by Gel Permeation Chromatography (GPC) measurement using a GPC apparatus (HLC-8120GPC manufactured by Tosoh Corporation) (solvent: tetrahydrofuran, flow rate (sample injection amount): 10 μL, column: TSK gel Multipore HXL-M manufactured by Tosoh Corporation, column temperature: 40° C., flow rate: 1.0 mL / min, detector: differential refractive index detector).
[0019] [Composition for semiconductor device treatment] The composition for semiconductor device treatment of the present invention (hereinafter also simply referred to as "composition") will be described in detail below. The composition is a composition for semiconductor device treatment that contains a polymer having an ethylenically unsaturated group and a functional group that interacts with a surface containing metal atoms in a substrate, a polymerization inhibitor, and a solvent. The mechanism by which the problem of the present invention can be solved by the composition having the above configuration is not necessarily clear, but the inventors speculate as follows. Note that the following speculation does not limit the mechanism by which the effect is obtained. In other words, even if the effect is obtained by a mechanism other than the one described below, it is still within the scope of the present invention.
[0020] The composition described in Patent Document 1 contains a polymer having a repeating unit containing an ethylenic double bond for the purpose of high-density modification of a substrate. However, depending on the storage conditions of the composition, the ethylenic double bond may undergo unintended polymerization, leading to an increase in the molecular weight of the polymer. Although the detailed mechanism is unclear, when a substrate is contacted with a composition in which the molecular weight of the polymer has increased, the polymer with increased molecular weight tends to remain on the second surface of the substrate, which does not contain metal, making it difficult to form a coating preferentially on the first surface, which contains metal. On the other hand, the composition of the present invention contains a polymerization inhibitor, which presumably suppresses the increase in the molecular weight of the polymer and allows the composition to preferentially form a coating on the first surface even after storage. Below, each component that may be contained in the composition for semiconductor device processing of the present invention is described in detail. Furthermore, the ability to preferentially form a coating on the first surface when contacted with a substrate having a first surface containing metal atoms and a second surface not containing metal atoms, and to preferentially form a coating on the first surface even after storage, is also referred to as "excellent effects of the present invention."
[0021] <Polymer> The composition contains a polymer having a functional group (hereinafter simply referred to as a "specific functional group") that interacts with a surface containing metal atoms in a substrate and an ethylenically unsaturated group. The specific functional group and the ethylenically unsaturated group will be described below.
[0022] (Functional group that interacts with a surface containing metal atoms in a substrate) The polymer has a functional group that interacts with a surface containing metal atoms in a substrate. The specific functional group can interact with a surface containing metal atoms in a substrate. Therefore, in a substrate having a first surface containing metal atoms and a second surface not containing metal atoms, as described below, the specific functional group is more likely to interact with the first surface than with the second surface. Examples of the interaction include chemical bonds, and more specifically, covalent bonds, ionic bonds, and coordinate bonds. Examples of surfaces containing metal atoms include the first surface containing metal atoms of a substrate described below. Examples of metal atoms contained in a surface containing metal atoms include metal atoms contained in the first surface described below. The specific functional group may be a group selected from the group consisting of a nitrogen-containing group, a phosphate group or a salt thereof, a carboxy group or a salt thereof, a hydroxy group, a hydroxyboron-containing group, an epoxy group, a hydrolyzable silyl group, a thiol group, and a disulfide group, and among these, a group selected from the group consisting of a nitrogen-containing group, a phosphate group or a salt thereof, a carboxy group or a salt thereof, a hydroxy group, an epoxy group, a hydrolyzable silyl group, a thiol group, and a disulfide group is preferred, and a cyano group or a phosphate group or a salt thereof is more preferred. The hydroxy group may be a phenolic hydroxy group.
[0023] Examples of the nitrogen-containing group include a cyano group (—C≡N), a primary amino group (—NH 2 ), secondary amino group (—NR T H), tertiary amino group (-NR T 2 ), and a quaternary ammonium group (—N + R T 3 ) are mentioned, and a cyano group, a primary amino group, a secondary amino group, or a tertiary amino group is preferred, and a primary amino group is more preferred. T represents an alkyl group having 1 to 3 carbon atoms, and a plurality of R T may be different from each other.
[0024] The nitrogen-containing group may have a ring structure containing a nitrogen atom as a ring member, and the ring structure may be either monocyclic or polycyclic. Examples of the nitrogen-containing group having a ring structure include a nitrogen-containing aliphatic heterocyclic group and a nitrogen-containing heteroaryl group. Examples of the nitrogen-containing aliphatic heterocyclic group include groups having a ring structure such as an oxazoline ring, a pyrrolidine ring, a piperidine ring, and a piperazine ring. Examples of the nitrogen-containing heteroaryl group include a pyridyl group, a triazine group, a pyrrole group, a pyrazole group, an imidazole group, a pyrazole group, a triazole group, a benzimidazole group, and a benztriazole group.
[0025] The salt of the phosphate group is -PO 4 2- Ct n+ 2/n It is to be noted that Ct n+ represents an n-valent cation, where n is 1 or 2. Examples of monovalent cations include Li + , Na + , K. + , and N.H. 4 + etc. n+ When represents a monovalent cation, the number is two. As a divalent cation, Mg 2+ , and Ca 2+ etc. n+ When represents a divalent cation, the number is 1. A compound having a phosphate group is also called a "phosphate compound," and the functional group name is also called "-phosphate."
[0026] The salt of a carboxy group is —COO - Ct + Ct + represents a monovalent cation, and examples thereof include the same monovalent cations as those explained above for the salts of phosphate groups.
[0027] Examples of hydrolyzable silyl groups include alkoxysilyl groups and chlorosilyl groups (groups having an -Si-Cl structure). In the alkoxysilyl group, the number of alkoxy groups bonded to the silicon atom (Si atom) is not particularly limited, but is preferably 2 or more, and more preferably 3. Of these, the alkoxysilyl group is preferably a trimethoxysilyl group or a triethoxysilyl group.
[0028] In the chlorosilyl group, the number of chlorine atoms bonded to the Si atom is preferably 1 to 3, and more preferably 1. When the number of chlorine atoms is 1 or 2, the chlorosilyl group is preferably a dialkylmonochlorosilyl group or a monoalkyldichlorosilyl group. The alkyl group may be linear, cyclic, or branched, but is preferably linear. Among these, the alkyl group is preferably a methyl group.
[0029] The polymer preferably has the specific functional group at an end of the main chain or at an end of the side chain, and in particular, it is preferable that the polymer has the specific functional group at one end of the main chain, in terms of achieving better effects of the present invention.
[0030] Examples of methods for introducing a specific functional group into the end of the main chain include a method using a compound containing a specific functional group as an initiator for radical polymerization to synthesize a polymer, and a method using a compound containing a specific functional group as an end-terminator for anionic polymerization to synthesize a polymer. Examples of initiators containing a specific functional group include cyano group-containing initiators such as azobisisobutyronitrile (AIBN). Examples of end-terminators containing a specific functional group include boroxine compounds, cyano group-containing halides, epoxy group-containing halides, and carbon-carbon triple bond-containing halides.
[0031] Examples of methods for introducing a specific functional group into the end of a side chain include polymerizing a monomer having a specific functional group at the end to form a repeating unit having the specific functional group at the end of the side chain (hereinafter also referred to as "repeating unit X"). Examples of monomers having a specific functional group include vinyl phosphoric acid, hydroxystyrene or its protected form, and epoxy group-containing vinyl ether.
[0032] In order to obtain a more excellent effect of the present invention, the repeating unit X is preferably present in the polymer in a block form, and more preferably present in a block form at one end of the main chain. In order to obtain a more excellent effect of the present invention, the content of the repeating unit X is preferably 0.1 mol% or more, more preferably 0.5 mol% or more, even more preferably 1 mol% or more, and particularly preferably 3 mol% or more, based on the total repeating units of the polymer. The upper limit is preferably 30 mol% or less, more preferably 10 mol% or less, and even more preferably 8 mol% or less.
[0033] (Ethylenically unsaturated group) The term "ethylenically unsaturated group" refers to a group having a double bond (C=C) between carbon atoms, and is often a monovalent group or a divalent group. The ethylenically unsaturated group does not contain an aromatic conjugated double bond between carbon atoms constituting an aromatic ring. The ethylenically unsaturated group is not particularly limited as long as it is a group having a double bond between carbon atoms, and examples thereof include groups that can form a crosslinked structure by reaction under heating conditions, active energy ray irradiation conditions, or acidic conditions.
[0034] More specifically, examples of ethylenically unsaturated groups include vinyl groups, vinyl ether groups (vinyloxy groups), allyl groups, acryloyl groups, methacryloyl groups, and styryl groups. Of these, vinyl groups, vinyl ether groups, styryl groups, acryloyl groups, and methacryloyl groups are preferred as ethylenically unsaturated groups. Furthermore, it is also preferred that the ethylenically unsaturated group be a group selected from the group consisting of alkenyl groups having 2 to 4 carbon atoms and alkenylene groups having 2 to 4 carbon atoms. In this specification, an alkenyl group refers to a group obtained by removing one hydrogen atom from an aliphatic hydrocarbon having a double bond in the molecule, and an alkenylene group refers to a group obtained by removing two hydrogen atoms from an aliphatic hydrocarbon having a double bond in the molecule. Examples of alkenyl groups having 2 to 4 carbon atoms include vinyl groups, allyl groups, isopropenyl groups, and isobutenyl groups. Examples of the alkenylene group having 2 to 4 carbon atoms include a vinylidene group and a methylvinylidene group.
[0035] The polymer may have an ethylenically unsaturated group in the main chain or in the side chain, but it is preferable that the ethylenically unsaturated group be in the main chain or in the side chain, in order to further promote crosslinking when the polymer is heated and to enable higher density modification. As a method for introducing an ethylenically unsaturated group into the polymer, there is mentioned a method for synthesizing the polymer using a monomer that gives a repeating unit containing an ethylenic double bond (hereinafter also referred to as "repeating unit A").
[0036] Repeating Unit A The repeating unit A may have one ethylenic double bond or two or more ethylenic double bonds. Examples of the structure containing an ethylenic double bond include isolated double bond structures such as an ethylene structure and a propylene structure, conjugated double bond structures such as a butadiene structure and a hexatriene structure, and carbonyl group-conjugated double bond structures such as an acrylic structure and a methacrylic structure.
[0037] Examples of the repeating unit A include repeating units represented by the following formulas (1-1) to (1-3) (hereinafter also referred to as "repeating units (A-1) to (A-3)"). The repeating unit (A-1) contains an ethylenic double bond in the main chain. The repeating unit (A-2) contains an ethylenic double bond in the main chain and in the side chain. The repeating unit (A-3) contains an ethylenic double bond in the side chain.
[0038]
[0039] In the above formula (1-1), R A1 ~R F1 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 20 carbon atoms.
[0040] In the above formula (1-2), R B2 ~R F2 R each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 20 carbon atoms. X2 represents a single bond or a divalent organic group having 1 to 20 carbon atoms. Y2 , R Z2 and R W2 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 20 carbon atoms.
[0041] In the above formula (1-3), R P represents a hydrogen atom or a methyl group. X3 represents a single bond or a divalent organic group having 1 to 20 carbon atoms. Y3 , R Z3 and R W3 each independently represents a hydrogen atom, a halogen atom, or a monovalent organic group having 1 to 20 carbon atoms.
[0042] In formula (1-1), R A1 and R B1 is preferably a monovalent organic group, and R C1 ~R F1 is preferably a hydrogen atom. An "organic group" refers to a group containing at least one carbon atom. A1 ~R F1 More specifically, the monovalent organic group having 1 to 20 carbon atoms represented by the formula (I) includes an aliphatic hydrocarbon group and an aromatic ring group. The aliphatic hydrocarbon group may be linear, branched, or cyclic, and preferably has 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms, and even more preferably 1 to 3 carbon atoms. The cyclic aliphatic hydrocarbon group may be either monocyclic or polycyclic. However, it does not have to be composed solely of an alicyclic structure, and may contain a chain structure as part of it.
[0043] Examples of linear or branched aliphatic hydrocarbon groups having 1 to 20 carbon atoms include alkyl groups such as methyl, ethyl, n-propyl, and i-propyl, alkenyl groups such as ethenyl, propenyl, and butenyl, and alkynyl groups such as ethynyl, propynyl, and butynyl. Examples of cyclic aliphatic hydrocarbon groups having 3 to 20 carbon atoms include monocyclic saturated alicyclic hydrocarbon groups such as cyclopentyl and cyclohexyl, monocyclic unsaturated alicyclic hydrocarbon groups such as cyclopentenyl and cyclohexenyl, polycyclic saturated alicyclic hydrocarbon groups such as norbornyl, adamantyl, and tricyclodecyl, and polycyclic unsaturated alicyclic hydrocarbon groups such as norbornenyl and tricyclodecenyl.
[0044] The aromatic ring group may be either an aryl group or a heteroaryl group. The number of ring members in the aromatic ring constituting the aromatic ring group is preferably 5 to 15, more preferably 5 to 10, and even more preferably 5 to 6. The aromatic ring constituting the aromatic ring group may be either a monocyclic ring or a polycyclic ring (fused ring). The fused ring may be a structure in which a plurality of aromatic rings are fused together, or a structure in which one or more aromatic rings are fused with one or more non-aromatic rings. Examples of monovalent aromatic hydrocarbon groups having 6 to 20 carbon atoms include aryl groups such as phenyl, tolyl, xylyl, naphthyl, and anthryl, and aralkyl groups such as benzyl, phenethyl, naphthylmethyl, and anthrylmethyl. The aromatic ring group may have a substituent.
[0045] The "organic group" may have at least one of a heteroatom and a halogen atom. Examples of organic groups having at least one of a heteroatom and a halogen atom include groups containing a divalent heteroatom-containing group between carbon atoms or at the terminal of the bond side of the hydrocarbon group, as well as groups in which some or all of the hydrogen atoms in the hydrocarbon group and the group containing a divalent heteroatom-containing group have been substituted with monovalent heteroatom-containing groups or halogen atoms. Examples of heteroatoms include oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, and silicon atoms. Examples of halogen atoms include fluorine atoms, chlorine atoms, bromine atoms, and iodine atoms.
[0046] Examples of the monovalent heteroatom-containing group include a hydroxy group, a carboxy group, a cyano group, an amino group, and a thiol group. Examples of the divalent heteroatom-containing group include —O—, —CO—, —S—, —CS—, —NR H -, and groups that combine two or more of these. H is a hydrogen atom or a monovalent hydrocarbon group.
[0047] In formula (1-2), R B2 ~R F2 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) is R A1 ~R F1Examples of the monovalent organic groups include those exemplified as R X2 Examples of the divalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) include R A1 ~R F1 Examples of the monovalent organic groups include those obtained by removing one hydrogen atom from the monovalent organic groups exemplified as R X2 As the alkyl group, a divalent hydrocarbon group is preferable, an alkanediyl group is more preferable, and a methanediyl group or an ethanediyl group is even more preferable.
[0048] R Y2 , R Z2 and R W2 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) is R A1 ~R F1 Examples of the monovalent organic groups include those exemplified as R Y2 is preferably a hydrogen atom. Z2 and R W2 As the alkyl group, a monovalent hydrocarbon group is preferable, an alkyl group is more preferable, and a methyl group is even more preferable.
[0049] In formula (1-3), R P is preferably a hydrogen atom. X3 Examples of the divalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) include R A1 ~R F1 Examples of the monovalent organic groups include those obtained by removing one hydrogen atom from the monovalent organic groups exemplified as R Y3 , R Z3 and R W3 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) is R A1 ~R F1 Examples of the monovalent organic groups include those exemplified as R Y3 is preferably a hydrogen atom. Z3 and R W3 As the alkyl group, a monovalent hydrocarbon group is preferable, an alkyl group is more preferable, and a methyl group is even more preferable.
[0050] Examples of monomers that provide the repeating unit (A-1) include compounds having a conjugated double bond, such as butadiene and isoprene. Examples of monomers that provide the repeating unit (A-2) include compounds having a conjugated double bond and an isolated double bond, such as myrcene. Examples of monomers that provide the repeating unit (A-3) include compounds having a plurality of isolated double bonds, such as 4-allylstyrene and 1,5-hexadiene.
[0051] The content of the repeating unit A is preferably 0.1 mol% or more, more preferably 1 mol% or more, even more preferably 5 mol% or more, and particularly preferably 8 mol% or more, based on the total repeating units of the polymer. The upper limit is preferably 90 mol% or less, more preferably 50 mol% or less, even more preferably 30 mol% or less, and particularly preferably 20 mol% or less.
[0052] The polymer preferably contains a ring structure, more preferably an aromatic ring structure, in its structure. For example, the polymer may contain a repeating unit having an aromatic ring (hereinafter also referred to as "repeating unit B") as a repeating unit different from the repeating unit A.
[0053] Repeating Unit B Repeating unit B is a repeating unit containing an aromatic ring. Examples of aromatic rings include a benzene ring, a fused benzene ring, and a heteroaromatic ring. The number of ring members in the aromatic ring is preferably 5 to 20, and more preferably 5 to 10. More specifically, examples of the benzene ring and fused benzene ring include a naphthalene ring, an anthracene ring, a phenanthrene ring, a tetracene ring, and a pyrene ring, and examples of the heteroaromatic ring include nitrogen-containing aromatic rings such as a pyrrole ring, a pyridine ring, a pyrazine ring, and a quinoline ring, oxygen-containing aromatic rings such as a furan ring, a pyran ring, a chromene ring, and a xanthene ring, and sulfur-containing aromatic rings such as a thiophene ring and a benzothiophene ring.
[0054] Examples of the repeating unit B include a repeating unit represented by the following formula (2).
[0055]
[0056] In the above formula (2), Ar 1 represents a group obtained by removing (n+1) hydrogen atoms on the aromatic ring from an arene having 6 to 20 ring members or a heteroarene having 5 to 20 ring members. n represents an integer of 0 to 11. n is preferably 0 to 3. R 1 represents a hydrogen atom or a methyl group. 1 is preferably a hydrogen atom. 2 represents a single bond, —O—, —COO—, or —CONH—. 2 R is preferably a single bond or —COO—, and more preferably a single bond. 3 represents an amino group, a carboxy group, a hydroxy group, a nitro group, a halogen atom, or a monovalent organic group having 1 to 20 carbon atoms. When n is 2 or more, a plurality of R 3 may be the same or different from each other.
[0057] Ar 1 Examples of arenes having 6 to 20 ring members that give Ar include benzene, naphthalene, anthracene, phenanthrene, tetracene, and pyrene. 1 Examples of heteroarenes having 5 to 20 ring members that give the formula (I) include nitrogen atom-containing aromatic heterocyclic compounds such as pyrrole, pyridine, pyrazine, and quinoline, oxygen atom-containing aromatic heterocyclic compounds such as furan, pyran, chromene, and xanthene, and sulfur atom-containing aromatic heterocyclic compounds such as thiophene and benzothiophene.
[0058] R 3 The monovalent organic group having 1 to 20 carbon atoms represented by the formula (1-1) is R A1 ~R F1 Examples of the monovalent organic groups include those exemplified as R 3is preferably a monovalent organic group, more preferably a hydrocarbon group which may have a substituent, and even more preferably an aliphatic hydrocarbon group which may have a substituent. The aliphatic hydrocarbon group may be linear, branched, or cyclic. Examples of the substituent that the hydrocarbon group may have include alkoxy groups such as a hydroxy group, a methoxy group, and an ethoxy group, and halogen atoms such as a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0059] Examples of monomers that provide the repeating unit B include styrene derivatives such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, p-t-butylstyrene, 2,4,6-trimethylstyrene, p-methoxystyrene, p-t-butoxystyrene, o-vinylstyrene, m-vinylstyrene, p-vinylstyrene, o-hydroxystyrene, m-hydroxystyrene, p-hydroxystyrene, m-chloromethylstyrene, p-chloromethylstyrene, p-chlorostyrene, p-bromostyrene, p-iodostyrene, p-nitrostyrene, and p-cyanostyrene, and aromatic ring-containing (meth)acrylates such as phenyl(meth)acrylate and naphthyl(meth)acrylate.
[0060] As the repeating unit B, a repeating unit derived from styrene which may have a substituent is preferred, and a repeating unit derived from styrene is more preferred.
[0061] The polymer may have repeating units A and repeating units B in a block configuration or a random configuration, but a random configuration is preferred from the viewpoint of further increasing the insolubilization degree of the polymer when heated.
[0062] The content of the repeating unit B is preferably 10 mol% or more, more preferably 40 mol% or more, even more preferably 60 mol% or more, and particularly preferably 80 mol% or more, based on the total repeating units of the polymer. The upper limit is preferably 99 mol% or less, more preferably 95 mol% or less, and even more preferably 92 mol% or less.
[0063] Other Repeating Units The polymer may have other repeating units different from the repeating unit A and the repeating unit B. Examples of other repeating units include a repeating unit derived from a (meth)acrylic acid ester and a repeating unit derived from ethylene which may have a substituent.
[0064] Examples of (meth)acrylic acid esters include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, t-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate; (meth)acrylic acid cycloalkyl esters such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 1-methylcyclopentyl (meth)acrylate, 2-ethyladamantyl (meth)acrylate, and 2-(adamantan-1-yl)propyl (meth)acrylate; and (meth)acrylic acid substituted alkyl esters such as 2-hydroxyethyl (meth)acrylate, 3-hydroxyadamantyl (meth)acrylate, 3-glycidylpropyl (meth)acrylate, and 3-trimethylsilylpropyl (meth)acrylate.
[0065] Examples of ethylene which may have a substituent include alkenes such as propene, butene, and pentene; vinylcycloalkanes such as vinylcyclopentane and vinylcyclohexane; cycloalkenes such as cyclopentene and cyclohexene; vinyl phosphoric acid, 4-hydroxy-1-butene, vinyl glycidyl ether, and vinyl trimethylsilyl ether.
[0066] When the polymer has other repeating units, the content of the other repeating units is preferably 30 mol % or less, more preferably 20 mol % or less, still more preferably 10 mol % or less, and particularly preferably 6 mol % or less, based on the total repeating units of the polymer. The lower limit is, for example, preferably 0.1 mol % or more.
[0067] When the polymer has other repeating units, the other repeating units may be present in the polymer in the form of blocks, or may be present randomly relative to the repeating unit A or the repeating unit B.
[0068] The weight average molecular weight (Mw) of the polymer is preferably 1,000 or more, more preferably 2,000 or more, even more preferably 3,000 or more, and particularly preferably 4,000 or more. The upper limit is preferably 50,000 or less, more preferably 30,000 or less, even more preferably 10,000 or less, and particularly preferably 7,000 or less. The dispersity (Mw / Mn, molecular weight distribution) of the polymer is preferably 5 or less, more preferably 2 or less, even more preferably 1.5 or less, and particularly preferably 1.3 or less. The lower limit is preferably 1.1 or more.
[0069] The polymer content is preferably 15% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 95% by mass or more, based on the total solid content of the composition. The upper limit is preferably 99.9% by mass or less, more preferably 99% by mass or less, and even more preferably 98% by mass or less. The "total solid content" refers to the sum of the components contained in the composition other than the solvent described below.
[0070] <Polymerization inhibitor> The composition contains a polymerization inhibitor. The polymerization inhibitor is not particularly limited, but is preferably a radical polymerization inhibitor. It is also preferable that the polymerization inhibitor contains a nitrogen atom. Nitrogen atoms are easily adsorbed to metals such as copper, but not to non-metals such as silicon oxide. Therefore, when the polymerization inhibitor contains a nitrogen atom, the polymerization inhibitor is more likely to be adsorbed to a surface containing metal atoms such as copper. Furthermore, since specific functional groups such as phosphate groups in a polymer are easily adsorbed to nitrogen atoms, as a result, polymers are more likely to be deposited on surfaces containing metal atoms such as copper, starting from the polymerization inhibitor adsorbed to the surface containing metal atoms, and the selectivity of the polymer on surfaces containing metal atoms relative to surfaces not containing metal atoms is improved.
[0071] The polymerization inhibitor preferably contains at least one compound selected from the group consisting of a phenolic compound, a quinone compound, a free radical compound, an amine compound, a phosphine compound, and a thiol ether compound, and is more preferably a phenolic compound, a quinone compound, or a free radical compound in terms of achieving better effects of the present invention.
[0072] Examples of phenolic compounds include 4-methoxyphenol, hydroquinone, 2-tert-butylhydroquinone, 4-tert-butylcatechol, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 2,5-di-tert-butyl-4-methylphenol, 2,6-di-tert-butyl-4-methylphenol, 4,4'-thiobis(3-methyl-6-t-butylphenol), 2,2'-methylenebis(4-methyl-6-t-butylphenol), 4-methoxynaphthol, 2,4-bis(octylthiomethyl)-6-methylphenol, p-nitrosophenol, and α-nitroso-β-naphthol.
[0073] The quinone compounds include 1,4-benzoquinone, 1,2-benzoquinone, and 1,4-naphthoquinone.
[0074] Examples of free radical compounds include poly(4-methacryloyloxy-2,2,6,6-tetramethylpiperidine-N-oxyl), 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl, 2,2,6,6-tetramethylpiperidine 1-oxyl, 2,2-diphenyl-1-picrylhydrazyl, and triphenylpherdazyl. Of the free radical compounds, nitroxyl radical compounds are preferred, and nitroxyl radical compounds having a piperidine skeleton are more preferred. Examples of nitroxyl radical compounds having a piperidine skeleton include poly(4-methacryloyloxy-2,2,6,6-tetramethylpiperidine-N-oxyl), 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl, and 2,2,6,6-tetramethylpiperidine 1-oxyl.
[0075] Examples of amine compounds include p-phenylenediamine, 4-aminodiphenylamine, N,N-diethylhydroxylamine, N,N'-diphenyl-p-phenylenediamine, N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, N,N'-di-2-naphthyl-p-phenylenediamine, diphenylamine, N-phenyl-β-naphthylamine, 4,4'-dicumyl-diphenylamine, 4,4'-dioctyl-diphenylamine, phenothiazine, 2-methoxyphenothiazine, phenoxazine, N-nitrosodiphenylamine, N-nitrosophenylnaphthylamine, N-nitrosodinaphthylamine, p-nitrosodiphenylamine, N-nitroso-N-phenylhydroxylamine, N-nitroso-N-phenylhydroxylamine aluminum, and cupferron. Each of the compounds exemplified as the amine compound may form a metal salt or a metal complex. Among the amine compounds, salts of N-nitroso compounds are preferred. Examples of salts of N-nitroso compounds include N-nitroso-N-phenylhydroxylamine aluminum.
[0076] An example of the phosphine compound is tris(2,4-di-tert-butylphenyl)phosphite.
[0077] Other examples of the polymerization inhibitor include nitrobenzene-based compounds such as nitrobenzene and 4-nitrotoluene, and thiol ether-based compounds such as dioctadecyl 3,3'-thiodipropionate, dilauryl thiodipropionate, dimyristyl thiodipropionate, and distearyl thiodipropionate.
[0078] The molecular weight of the polymerization inhibitor is preferably 1,000 or less, more preferably 800 or less, and even more preferably 500 or less. There is no particular restriction on the lower limit of the molecular weight, but it is preferably 80 or more.
[0079] The content of the polymerization inhibitor is preferably 0.0001% by mass or more, more preferably 0.001% by mass or more, even more preferably 0.005% by mass or more, and particularly preferably 0.010% by mass or more, relative to the total solids content of the composition. The upper limit is preferably 70% by mass or less, more preferably 10% by mass or less, and even more preferably 2% by mass or less. Furthermore, in order to achieve better effects of the present invention, the content of the polymerization inhibitor is preferably 0.001 parts by mass or more, more preferably 0.08 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 1.0 parts by mass or more, relative to 100 parts by mass of the polymer. The upper limit is preferably 200 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the polymer. The composition may contain one type of polymerization inhibitor alone, or two or more types. When two or more types of polymerization inhibitors are contained, it is preferable that the total amount thereof is within the above range.
[0080] <Solvent> The composition contains a solvent. The solvent is not particularly limited as long as it can dissolve or disperse at least the polymer, the polymerization inhibitor, and any optional components added as needed. Examples of the solvent include water and organic solvents. Examples of the organic solvent include ester-based solvents, ketone-based solvents, alcohol-based solvents, ether-based solvents, hydrocarbon-based solvents, amide-based solvents, and sulfur-containing solvents.
[0081] Examples of ester solvents include n-butyl acetate, ethyl lactate, propylene glycol acetate, propylene glycol monomethyl ether acetate, γ-butyrolactone, and δ-valerolactone.
[0082] Examples of ketone solvents include acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone.
[0083] Examples of alcohol-based solvents include aliphatic alcohol-based solvents having 1 to 18 carbon atoms, such as methanol, ethanol, 1-propanol, 2-propanol (also referred to as isopropyl alcohol (IPA)), 2-butanol, isobutyl alcohol, tert-butyl alcohol, isopentyl alcohol, and 4-methyl-2-pentanol (also referred to as methyl isobutyl carbinol (MIBC)); alicyclic alcohol-based solvents having 3 to 18 carbon atoms, such as cyclohexanol; aromatic alcohol-based solvents, such as benzyl alcohol; and ketone alcohol-based solvents, such as diacetone alcohol. The number of carbon atoms in the alcohol-based solvent is preferably 1 to 8, more preferably 2 to 7, and even more preferably 3 to 6.
[0084] The alcohol-based solvent may be a polyol-based solvent or a glycol ether-based solvent.
[0085] Examples of polyol-based solvents include glycol-based solvents having a carbon number of 2 to 18. Examples of glycol-based solvents include ethylene glycol, propylene glycol (1,2-propanediol), 1,3-propanediol, diethylene glycol, and dipropylene glycol.
[0086] Examples of glycol ether solvents include glycol monoether solvents having 3 to 19 carbon atoms. Examples of glycol monoether solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol mono-n-propyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, triethylene glycol monomethyl ether, triethylene glycol monoethyl ether, triethylene glycol monobutyl ether, 1-methoxy-2-propanol, 2-methoxy-1-propanol, 1-ethoxy-2-propanol, 2-ethoxy-1-propanol, propylene glycol monomethyl ether, propylene glycol mono-n-propyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol mono-n-propyl ether, tripropylene glycol monoethyl ether, tripropylene glycol monomethyl ether, ethylene glycol monobenzyl ether, and diethylene glycol monobenzyl ether. The glycol ether solvent preferably has 1 to 8 carbon atoms, more preferably 2 to 7 carbon atoms, and even more preferably 3 to 6 carbon atoms.
[0087] Examples of ether solvents include diethyl ether, diisopropyl ether, dibutyl ether, t-butyl methyl ether, cyclohexyl methyl ether, and tetrahydrofuran.
[0088] Examples of hydrocarbon solvents include aliphatic hydrocarbon solvents such as n-pentane and n-hexane; alicyclic hydrocarbon solvents such as cyclohexane and methylcyclohexane; and aromatic hydrocarbon solvents such as toluene and xylene.
[0089] Examples of amide solvents include formamide, monomethylformamide, dimethylformamide, acetamide, monomethylacetamide, dimethylacetamide, monoethylacetamide, diethylacetamide, and N-methylpyrrolidone.
[0090] Examples of sulfur-containing solvents include dimethyl sulfone, dimethyl sulfoxide, and sulfolane.
[0091] Among these, the solvent preferably contains at least one solvent selected from the group consisting of ester-based solvents, ketone-based solvents, and alcohol-based solvents, and more preferably contains at least one solvent selected from the group consisting of propylene glycol monomethyl ether acetate, ethyl lactate, γ-butyrolactone, cyclohexanone, methyl isobutyl ketone, and propylene glycol monomethyl ether.
[0092] The content of the solvent is preferably 90 to 99.999% by mass, more preferably 95 to 99.9% by mass, and even more preferably 97 to 99.9% by mass, relative to the total mass of the composition. The solids concentration of the composition is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more. The upper limit is preferably 30% by mass or less, more preferably 10% by mass or less, and even more preferably 3% by mass or less. Two or more solvents may be used in combination. When two or more solvents are used in combination, the total content thereof is preferably within the above range.
[0093] <Thermal Acid Generator> The composition may contain a thermal acid generator. A thermal acid generator is a compound that generates an acid upon heating. The thermal acid generator may be either ionic or nonionic. When the polymer contains an aromatic ring and an ethylenic double bond, the aromatic ring and the ethylenic double bond in the polymer may be crosslinked by a Friedel-Crafts reaction due to the action of the acid generated from the thermal acid generator.
[0094] Examples of ionic thermal acid generators include cations such as triphenylsulfonium, 1-dimethylthionaphthalene, 1-dimethylthio-4-hydroxynaphthalene, 1-dimethylthio-4,7-dihydroxynaphthalene, 4-hydroxyphenyldimethylsulfonium, benzyl-4-hydroxyphenylmethylsulfonium, 2-methylbenzyl-4-hydroxyphenylmethylsulfonium, 2-methylbenzyl-4-acetylphenylmethylsulfonium, 2-methylbenzyl-4-benzoyloxyphenylmethylsulfonium, 1-(4-n-butoxynaphthalen-1-yl)tetrahydrothiophenium, 1-(4,7-dibutoxy-1-naphthalenyl)tetrahydrothiophenium, diphenyliodonium, and di(t-butylphenyl)iodonium; Examples of the salt include salts with anions such as fluorinated alkylsulfonates, such as methanesulfonate, trifluoromethanesulfonate, and nonafluorobutane-1-sulfonate; sulfonate ions, such as camphorsulfonate and p-toluenesulfonate ion; phosphate ions, such as hexafluorophosphate ion; borate ions, such as tetrafluoroborate ion; and antimonate ions, such as hexafluoroantimonate ion.
[0095] Examples of nonionic thermal acid generators include halogen-containing compounds, diazomethane compounds, sulfone compounds, sulfonate compounds, carboxylate compounds, phosphate compounds, N-sulfonyloxyimide compounds, and sulfonebenzotriazole compounds. Specific examples of N-sulfonyloxyimide compounds include N-(trifluoromethylsulfonyloxy)succinimide and N-(2-trifluoromethylphenylsulfonyloxy)phthalimide.
[0096] The acid generation temperature of the thermal acid generator is preferably 80° C. or higher, more preferably 100° C. or higher, even more preferably 120° C. or higher, and particularly preferably 150° C. or higher. The upper limit is preferably 250° C. or lower, more preferably 230° C. or lower, even more preferably 210° C. or lower, and particularly preferably 190° C. or lower. The "acid generation temperature" of the thermal acid generator can be measured, for example, as the peak temperature at the maximum endothermic peak or maximum exothermic peak in the DSC curve obtained when the temperature is raised from 30° C. to 300° C. at a heating rate of 10° C. / min.
[0097] The content of the thermal acid generator is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, relative to 100 parts by mass of the polymer. The upper limit is preferably 400 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 30 parts by mass or less, particularly preferably 10 parts by mass or less, and most preferably 6 parts by mass or less.
[0098] <Optional Components> The composition may contain optional components in addition to the components described above. Examples of optional components include surfactants.
[0099] <Method for Producing Composition> The method for producing the composition is not particularly limited, and the composition can be produced, for example, by mixing the above-mentioned components. The order or timing for mixing the components in the composition is not particularly limited. For example, the composition can be produced by adding a polymer and a polymerization inhibitor to a stirrer such as a mixer containing a purified solvent, and then thoroughly stirring the mixture. When the composition contains components other than the polymer and the polymerization inhibitor, the other components may be added simultaneously with the polymer and the polymerization inhibitor, or may be added at different times. In the production process for producing the composition, the steps described below may be carried out.
[0100] (Metal Removal Step) The above production method may include a metal removal step of removing metal components from the above components and / or composition (hereinafter also referred to as "material to be purified").
[0101] (Filtration step) The above production method preferably includes a filtration step of filtering the liquid to remove foreign matter, coarse particles, etc. from the liquid. The filtration method is not particularly limited, and known filtration methods can be used. Among them, filtering using a filter is preferred. Examples of the filter include a high-density polyethylene filter having pores of about 0.45 μm.
[0102] (Static Elimination Step) The method for producing the composition may further include a static elimination step of eliminating static electricity from the composition.
[0103] [Method for Producing Modified Substrate] The method for producing a modified substrate of the present invention (hereinafter also referred to as "the present production method") includes a step of contacting a substrate having a first surface containing metal atoms and a second surface not containing metal atoms with the composition for treating semiconductor devices (hereinafter also referred to as "composition layer forming step"), and a step of forming a coating on the first surface by subjecting the substrate that has been contacted with the composition (hereinafter also referred to as "heating step").
[0104] Preferably, the manufacturing method further includes, after the heating step, a step of removing portions other than the coating formed on the first surface with a rinse liquid (hereinafter also referred to as a "removing step"). The manufacturing method may also include, for example, a step of contacting the surface of the substrate after the removing step with alcohol, dilute acid, ozone, or plasma (hereinafter also referred to as a "contacting step"), a step of depositing a pattern on the surface of the substrate after the removing step by a CVD method or an ALD method (hereinafter also referred to as a "depositing step"), and a step of removing the polymer on the surface of the substrate after the removing step by etching (hereinafter also referred to as an "etching step"). Each step will be described below.
[0105] <Composition Layer Forming Step> In this step, a substrate is contacted with the composition for semiconductor device treatment to form a composition layer on the surface of the substrate. Methods for forming a composition layer on a substrate include various coating methods such as slit coating, inkjet coating, rotary coating (spin coating), casting coating, roll coating, and screen printing.
[0106] The substrate has a first surface containing metal atoms and a second surface not containing metal atoms. Examples of metal atoms include copper, iron, zinc, cobalt, aluminum, tin, tungsten, zirconium, titanium, tantalum, germanium, molybdenum, ruthenium, gold, silver, platinum, palladium, and nickel. Among these, copper, tantalum, cobalt, and tungsten are preferred. Examples of the form in which the metal atoms are contained in the first surface include simple metals, alloys, metal nitrides, metal oxides, and silicides.
[0107] Examples of elemental metals include elemental metals such as copper, iron, cobalt, tungsten, and tantalum. Examples of alloys include nickel-copper alloys, cobalt-nickel alloys, and gold-silver alloys. Examples of metal nitrides include tantalum nitride, titanium nitride, iron nitride, and aluminum nitride. Examples of metal oxides include tantalum oxide, aluminum oxide, iron oxide, and copper oxide. Examples of silicides include iron silicide and molybdenum silicide. The first surface preferably contains an elemental metal, alloy, metal nitride, or silicide, more preferably an elemental metal or metal nitride, and even more preferably an elemental copper, cobalt, or tungsten.
[0108] The second surface is a surface that does not contain metal atoms, i.e., a surface that is composed only of nonmetal atoms. The second surface often contains an insulator. Examples of the form in which the nonmetal atoms are contained in the second surface include a nonmetal element, a nonmetal oxide, a nonmetal nitride, and a nonmetal oxynitride.
[0109] Examples of non-metallic elements include silicon and carbon. Examples of non-metallic oxides include silicon oxide and silicon oxycarbide. Examples of non-metallic nitrides include SiN. x and Si 3 N 4Examples of non-metallic oxynitrides include SiON, etc. Among these, the second surface preferably contains a non-metallic oxide, more preferably contains silicon, and further preferably contains silicon oxide, silicon nitride, or silicon oxycarbide.
[0110] The shape of the first and second surfaces of the substrate is not particularly limited, and examples thereof include a planar shape, a dotted shape, and a striped shape in a planar view. The size of the first and second surfaces is not particularly limited, and regions of a desired size can be used. The shape of the substrate is not particularly limited, and can be a plate-like shape or any other desired shape.
[0111] <Heating Step> In this step, the composition layer formed in the composition layer forming step is heated. This step promotes bond formation between the first surface and specific functional groups in the composition, and also promotes crosslinking between ethylenically unsaturated groups. Furthermore, as described above, when the polymer contains an aromatic ring and an ethylenic double bond and the composition contains a thermal acid generator, the aromatic ring and the ethylenic double bond in the polymer may be crosslinked by a Friedel-Crafts reaction due to the action of the acid generated from the thermal acid generator. As a result, a coating containing a cured product of the polymer (a crosslinked product of the polymer) is laminated on the first surface. Heating may be performed in one step, or in multiple steps of two or more steps. When the heating is performed in two steps, bond formation between the surface containing metal atoms and specific functional groups is further promoted in the first step, and crosslinking of the polymer is further promoted in the second step, thereby enabling modification at a higher density.
[0112] Examples of heating means include an oven and a hot plate. The heating temperature is preferably 80°C or higher, more preferably 100°C or higher, even more preferably 130°C or higher, and particularly preferably 150°C or higher. The upper limit is preferably 400°C or lower, more preferably 300°C or lower, even more preferably 200°C or lower, and particularly preferably 180°C or lower. The heating time is preferably 10 seconds or longer, more preferably 60 seconds or longer, even more preferably 120 seconds or longer, and particularly preferably 300 seconds or longer. The upper limit is preferably 120 minutes or shorter, more preferably 60 minutes or shorter, even more preferably 1,200 seconds or shorter, and particularly preferably 600 seconds or shorter.
[0113] <Removal Step> In this step, excess components on the substrate after the heating step are removed with a rinse solution. This removes the excess components from the substrate, resulting in a substrate with a selectively modified first surface. As the rinse solution, an organic solvent is typically used, and examples include polyhydric alcohol partial ether carboxylate solvents such as propylene glycol monomethyl ether acetate and monoalcohol solvents such as isopropanol.
[0114] <Contacting Step> In this step, the surface of the substrate after the removing step is brought into contact with alcohol, dilute acid, hydrogen peroxide solution, ozone, or plasma. This allows the air-oxidized film layer formed on the second surface to be removed. Examples of dilute acids include dilute hydrochloric acid, dilute sulfuric acid, dilute nitric acid, dilute citric acid, dilute oxalic acid, dilute maleic acid, dilute acetic acid, dilute isobutyric acid, and dilute 2-ethylhexanoic acid.
[0115] <Deposition Step> In this step, a pattern is deposited on the surface of the substrate after the removal step by CVD (chemical vapor deposition) or ALD (atomic layer deposition). This allows a pattern to be selectively formed on the second surface that is not covered with the coating. In particular, a coating is less likely to be formed by ALD in the region where the coating is formed, and a coating is more likely to be selectively formed by ALD on the second surface. In other words, the coating formed by the composition has excellent inhibitory properties against ALD coating formation.
[0116] <Etching Step> In this step, the polymer on the surface of the substrate after the removing step is removed by etching. 4 or O 2 Examples of known etching methods include chemical dry etching, which uses a gas or the like and utilizes the difference in etching rate between layers, reactive ion etching (RIE), such as chemical wet etching (wet development), which uses a liquid etching solution such as an organic solvent or hydrofluoric acid, and physical etching, such as sputter etching and ion beam etching. Of these, reactive ion etching is preferred as the etching method, and chemical dry etching or chemical wet etching is more preferred.
[0117] Before chemical dry etching, radiation may be applied as needed. When the portion to be removed by etching is a polymer containing polymethyl methacrylate blocks, UV irradiation or the like can be used as the radiation. Oxygen plasma treatment can also be used. The UV irradiation or oxygen plasma treatment decomposes the polymethyl methacrylate blocks, making them more susceptible to etching.
[0118] Examples of organic solvents used in chemical wet etching include alkanes such as n-pentane, n-hexane, and n-heptane, cycloalkanes such as cyclohexane, cycloheptane, and cyclooctane, saturated carboxylic acid esters such as ethyl acetate, n-butyl acetate, i-butyl acetate, and methyl propionate, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and methyl n-pentyl ketone, and alcohols such as methanol, ethanol, 1-propanol, 2-propanol, and 4-methyl-2-pentanol. These solvents may be used alone or in combination of two or more.
[0119] The present invention will be described in more detail below with reference to examples. The materials, amounts used, ratios, treatment details, treatment procedures, etc. shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the examples shown below.
[0120] [Materials used in preparing compositions] The structure or name of each component used in preparing the compositions of each example and comparative example is shown below.
[0121] <Polymer> P-1: Polymer synthesized according to the following procedure: 0.098 g (0.6 mmol) of azobisisobutyronitrile, 11.25 g (0.108 mol) of styrene, 0.83 g (0.002 mol) of 2-cyano-2-propyldodecyl trithiocarbonate, 1.63 g (0.012 mol) of myrcene, and 20 g of anisole were added to a three-necked flask reaction vessel, and the mixture was heated and stirred at 80°C for 8 hours under a nitrogen atmosphere. The polymerization solution was purified by precipitation into 300 g of methanol, and the resulting yellow viscous material was recovered and dissolved in 20 g of propylene glycol monomethyl ether acetate. 0.49 g (0.003 mol) of azobisisobutyronitrile and 2.03 g (0.010 mol) of tert-dodecanethiol were added, and the mixture was refluxed at 80°C for 2 hours to carry out a cleavage reaction of the trithiocarbonate terminal. The resulting polymerization solution was concentrated under reduced pressure and purified by precipitation in 1,000 g of methanol, yielding a pale yellow viscous product. This viscous product was then dried under reduced pressure at 60°C to yield 6.5 g of polymer (P-1) as a pale yellow solid. This polymer (P-1) had an Mw of 4,500, an Mn of 4,000, and an Mw / Mn of 1.13. The specific functional group in polymer (P-1) was a cyano group, and the ethylenically unsaturated group (a group selected from the group consisting of alkenyl groups having 2 to 4 carbon atoms and alkenylene groups having 2 to 4 carbon atoms) was contained in a unit derived from myrcene.
[0122] P-2: Polymer synthesized by the following procedure: 0.098 g (0.6 mmol) of azobisisobutyronitrile, 10.63 g (0.102 mol) of styrene, 0.58 g (0.002 mol) of dibenzyl trithiocarbonate, 1.63 g (0.012 mol) of myrcene, and 20 g of anisole were added to a three-necked flask reaction vessel, and the mixture was heated and stirred at 80°C for 5 hours under a nitrogen atmosphere. Next, 0.64 g (0.006 mol) of vinyl phosphoric acid was added, and the mixture was heated and stirred at 80°C for 3 hours. This polymerization solution was purified by precipitation into 300 g of methanol, and the resulting yellow viscous material was recovered and dissolved in 20 g of propylene glycol monomethyl ether acetate. 0.49 g (0.003 mol) of azobisisobutyronitrile and 2.03 g (0.010 mol) of tert-dodecanethiol were added, and the mixture was refluxed at 80°C for 2 hours to carry out a cleavage reaction of the trithiocarbonate terminal. The resulting polymerization solution was concentrated under reduced pressure and purified by precipitation into 1,000 g of methanol to obtain a pale yellow viscous material. This viscous material was then dried under reduced pressure at 60°C to obtain 6.5 g of polymer (P-2) as a pale yellow solid. This polymer (P-2) had an Mw of 4,600, an Mn of 3,800, and an Mw / Mn of 1.21. The specific functional group in the polymer (P-2) is a phosphate group, and the ethylenically unsaturated group (a group selected from the group consisting of an alkenyl group having 2 to 4 carbon atoms and an alkenylene group having 2 to 4 carbon atoms) is contained in a unit derived from myrcene.
[0123] P-3: Polymer synthesized according to the following procedure. A three-necked flask reaction vessel was dried under reduced pressure, and then 120 g of THF that had been subjected to distillation and dehydration treatment under a nitrogen atmosphere was poured into the vessel and cooled to -78°C. 2.09 mL (2.03 mmol) of a 1N cyclohexane solution of sec-butyllithium (sec-BuLi) was poured into the THF. Furthermore, 11.1 mL (0.062 mol) of styrene that had been subjected to adsorption filtration with silica gel and distillation and dehydration treatment to remove the polymerization inhibitor, and 0.78 mL (5.38 mmol) of 4-allylstyrene were poured dropwise over 30 minutes, and it was confirmed that the polymerization system was orange. During this dropwise pouring, care was taken to ensure that the internal temperature of the reaction solution did not exceed -60°C. 0.34 mL (2.03 mmol) of bromopropionitrile as a terminal terminator and 4.1 mL (2.03 mmol) of a 0.5N tetrahydrofuran solution of lithium chloride were added, and a termination reaction of the polymerization terminals was carried out. The reaction solution was warmed to room temperature, and the resulting reaction solution was concentrated and the solvent was replaced with MIBK. Thereafter, 1,000 g of a 2% by mass aqueous solution of oxalic acid was poured in and stirred, and after standing, the lower aqueous phase was removed. This operation was repeated three times to remove the Li salt. Thereafter, 1,000 g of ultrapure water was poured in and stirred, and the lower aqueous phase was removed. This operation was repeated three times to remove the oxalic acid, and then the solution was concentrated and added dropwise to 500 g of methanol to precipitate a polymer, and the solid was recovered using a Buchner funnel. This solid was dried under reduced pressure at 60 ° C. to obtain 10.5 g of a white polymer (P-3). This polymer (P-3) had an Mw of 5,300, an Mn of 5,100, and an Mw / Mn of 1.04. The specific functional group in the polymer (P-3) is a cyano group, and the ethylenically unsaturated group (a group selected from the group consisting of an alkenyl group having 2 to 4 carbon atoms and an alkenylene group having 2 to 4 carbon atoms) is contained in a unit derived from 4-allylstyrene.
[0124] <Thermal Acid Generator> A-1: diphenyliodonium nonafluorobutane-1-sulfonate (acid generation temperature = 170°C)
[0125] <Polymerization inhibitors> I-1: 4-methoxyphenol (phenolic compound) I-2: N-nitroso-N-phenylhydroxylamine aluminum (amine compound) I-3: poly(4-methacryloyloxy-2,2,6,6-tetramethylpiperidine-N-oxyl) (free radical compound) I-4: 4-tert-butylcatechol (phenolic compound) I-5: 1,4-benzoquinone (quinone compound) I-6: phenothiazine (amine compound) I-7: N,N-diethylhydroxylamine (amine compound) I-8: 4-hydroxy-2,2,6,6-tetramethylpiperidine 1-oxyl (free radical compound) I-9: cupferron (amine compound) I-10: 2,2-diphenyl-1-picrylhydrazyl (free radical compound) I-11: triphenylpherdazyl (free radical compound) I-12: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (phenolic compound) I-13: 2,2,6,6-tetramethylpiperidine 1-oxyl (free radical compound) I-14: Tris(2,4-di-tert-butylphenyl)phosphite (phosphine compound) I-15: Dioctadecyl 3,3'-thiodipropionate (thiol ether compound) I-16: 2,4-bis(octylthiomethyl)-6-methylphenol (phenolic compound)
[0126] <Solvent> S-1: Propylene glycol monomethyl ether acetate (PGMEA) S-2: Ethyl lactate
[0127] [Method of Preparing Composition] The method of preparing the composition of Example 1 is described below. 0.05 g of thermal acid generator (A-1), 0.02 g of polymerization inhibitor (I-1), 74.03 g of solvent (S-1), and 24.67 g of solvent (S-2) were added to 1.25 g of polymer (P-1), stirred, and then filtered through a high-density polyethylene filter having 0.45 μm pores to prepare a composition. Furthermore, the compositions of each example and comparative example were prepared in the same manner as in Example 1, except that the types and amounts of each component shown in the table below were used.
[0128] [Substrate Surface Modification] Using the compositions of each Example and Comparative Example, the substrate surface was modified according to the following procedure. A copper (Cu) substrate was immersed in a 1% by mass aqueous solution of citric acid, and then dried under a nitrogen flow to remove the oxide film on the surface. Silicon oxide (SiO 2 The Cu substrate and SiO 2 The composition prepared above was spin-coated onto a substrate at 1,500 rpm and heated for 180 seconds at 150° C. The substrate was then washed with PGMEA.
[0129] [Evaluation Method] The substrates prepared by the above procedure were used to evaluate the storage stability of the compositions and the selectivity of surface modification.
[0130] <Contact Angle> The water contact angle of the substrate surface prepared by the above procedure was measured using a contact angle meter (Drop Master DM-503, manufactured by Kyowa Interface Science Co., Ltd.) This evaluation was carried out within 24 hours after the preparation of the composition.
[0131] <Evaluation of Storage Stability> Substrates were modified in the same manner as described above in [Modification of Substrate Surface] using the compositions of each Example and Comparative Example that had been stored at 45° C. for one month. The water contact angle of this substrate surface was measured according to the procedure described above in <Contact Angle>, and the obtained values were used to evaluate storage stability in accordance with the following criteria.
[0132] (Evaluation Criteria) A: Water contact angle is 50° or less B: Water contact angle is more than 50° and less than 60° C: Water contact angle is 60° or more
[0133] <Evaluation of selective surface modification on a striped substrate made of copper-silicon oxide> An 8-inch substrate (Cu-EPC: 10,000 Å / Cu-Seed: 1,000 Å / TaN Barrier Layer: 250 Å / silicon oxide (silicon oxide): 5,000 Å / silicon wafer, 0.18 μm trench) shown in FIG. 1 was polished with CMP slurry, and copper (Cu) and silicon oxide (SiO 2A substrate with Cu-EPC and Cu-Seed arranged in stripes was fabricated. The substrate was then immersed in a 5% by mass aqueous solution of oxalic acid and dried under nitrogen flow to remove the surface oxide film. The substrate shown in Figure 1 includes a silicon wafer 1, Cu-EPC 2, Cu-seed 3, TaN (tantalum nitride) 4, and silicon oxide 5. The composition stored at 45°C for one month in the above-mentioned <Evaluation of Storage Stability> was spin-coated onto this substrate at 1,500 rpm using a track (ACT8, manufactured by Tokyo Electron Ltd.), and then heated at 150°C for 180 seconds. The substrate was then washed with PGMEA. The surface was then observed with a scanning probe microscope (Dimension iCON, manufactured by Bruker), and the film thickness of the coated portion was calculated based on the unevenness. The average thickness (Å) of the coating formed on the copper and silicon oxide regions of the copper-silicon oxide stripe substrate is shown in the table. In the table, "ND" indicates that the thickness was too small to be detected. Note that the copper and tantalum nitride regions on the copper-silicon oxide stripe substrate are surfaces containing the above-mentioned metal atoms, while the silicon oxide region corresponds to a surface not containing metal atoms.
[0134] [Results] The above evaluation results are shown in Table 1. In the table, Comparative Example 2 shows the results for a blank substrate whose surface was not treated with the composition.
[0135]
[0136]
[0137]
[0138] As shown in the table, it was confirmed that the compositions of the present invention in each Example exhibited the desired effects. On the other hand, in the Comparative Examples, since the compositions did not contain a polymerization inhibitor, the storage stability of the compositions was poor, and the silicon oxide was also modified with the polymer, making it impossible to selectively modify the substrate surface.
[0139] Furthermore, comparisons between Examples 1 to 16 and the like confirmed that the effects of the present invention are even better when the polymerization inhibitor contained in the composition is a phenolic compound, a quinone compound, or a free radical compound. Comparisons between Examples 8 and 19, and between Examples 13 and 20 and the like confirmed that when the polymerization inhibitor contained in the composition contains a nitrogen atom and the polymer has a specific functional group such as a phosphate group or a salt thereof, the contact angle value of the copper substrate after modification is relatively large, which confirms that the polymer is more likely to deposit on a surface containing metal atoms such as copper, and the selectivity of the polymer on a surface containing metal atoms relative to a surface not containing metal atoms is improved.
[0140] 1 Silicon wafer 2 Cu-EPC 3 Cu-seed 4 TaN 5 Silicon oxide
Claims
1. A composition for semiconductor device processing comprising: a polymer having an ethylenically unsaturated group and a functional group that interacts with a surface containing metal atoms in a substrate; a polymerization inhibitor; and a solvent.
2. The composition for treating a semiconductor device according to claim 1, wherein the functional group is a group selected from the group consisting of a nitrogen-containing group, a phosphate group or a salt thereof, a carboxy group or a salt thereof, a hydroxy group, an epoxy group, a hydrolyzable silyl group, a thiol group and a disulfide group.
3. The composition for treating a semiconductor device according to claim 1 or 2, wherein the functional group is a cyano group or a phosphate group or a salt thereof.
4. The composition for treating a semiconductor device according to claim 1 or 2, wherein the ethylenically unsaturated group is a group selected from the group consisting of a vinyl group, a vinyl ether group, a styryl group, an acryloyl group and a methacryloyl group.
5. The composition for treating a semiconductor device according to claim 1 or 2, wherein the ethylenically unsaturated group is a group selected from the group consisting of an alkenyl group having 2 to 4 carbon atoms and an alkenylene group having 2 to 4 carbon atoms.
6. The composition for processing a semiconductor device according to claim 1 or 2, wherein the polymer comprises a ring structure.
7. The composition for treating a semiconductor device according to claim 6, wherein said polymer comprises an aromatic ring structure.
8. The composition for treating a semiconductor device according to claim 1 or 2, wherein the polymerization inhibitor comprises a nitrogen atom.
9. The composition for treating semiconductor devices according to claim 1 or 2, wherein the polymerization inhibitor comprises at least one compound selected from the group consisting of phenolic compounds, quinone compounds, free radical compounds, amine compounds, phosphine compounds and thiol ether compounds.
10. The composition for processing a semiconductor device according to claim 9, wherein the polymerization inhibitor is a phenolic compound, a quinone compound or a free radical compound.
11. The composition for treating semiconductor devices according to claim 1 or 2, wherein the content of the polymerization inhibitor is 0.08 to 200 parts by mass based on 100 parts by mass of the polymer.
12. The composition for treating a semiconductor device according to claim 1 or 2, wherein the solvent comprises at least one solvent selected from the group consisting of ester-based solvents, ketone-based solvents and alcohol-based solvents.
13. The composition for processing a semiconductor device of claim 12, wherein the solvent comprises at least one solvent selected from the group consisting of propylene glycol monomethyl ether acetate, ethyl lactate, gamma-butyrolactone, cyclohexanone, methyl isobutyl ketone, and propylene glycol monomethyl ether.
14. A method for producing a modified substrate, comprising the steps of: contacting a substrate having a first surface containing metal atoms and a second surface not containing metal atoms with a composition for treating a semiconductor device according to claim 1 or 2; and forming a coating on the first surface by subjecting the substrate contacted with the composition to a heat treatment.
15. The method of producing a modified substrate according to claim 14, wherein the second surface comprises an insulator.
16. The method of claim 14, wherein the second surface comprises silicon.
17. The method of claim 14, wherein the second surface comprises silicon oxide, silicon nitride, or silicon oxycarbide.
Citation Information
Patent Citations
Substrate processing method and substrate processing system
JP2020107855A
Maleimide resin, curable resin composition, and cured product of the same
JP2022176111A
Substrate with film formed thereon
WO2023033146A1