Solid electrolyte battery and method for manufacturing same
The use of a foam sheet to fix the electrode body within an insulating container addresses the misalignment and reliability issues in lithium-ion batteries, enhancing the productivity and safety of solid electrolyte batteries by preventing misalignment and abnormal heat generation, resulting in high energy density and long lifespan.
Patent Information
- Application Number
- PCT/JP2024/017288
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-18
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-21
AI Technical Summary
Lithium-ion batteries face challenges with reliability and productivity due to misalignment of power generation elements during manufacturing, leading to potential short circuits and decreased battery performance, especially with the use of organic solvents which are flammable and increase the risk of abnormal heat generation.
A solid electrolyte battery design where a foam sheet is used to fix the electrode body within an insulating container, preventing misalignment and ensuring reliable contact between electrodes, and a method of manufacturing involving a foam sheet that forms between the container and electrode body to enhance adhesion and prevent positional displacement.
The solution improves the reliability and productivity of solid electrolyte batteries by preventing misalignment and short circuits, ensuring high energy density, long lifespan, and safety, while also eliminating the risk of abnormal heat generation associated with organic solvents.
Smart Images

Figure JP2024017288_21112024_PF_FP_ABST
Abstract
Description
Solid electrolyte battery and method of manufacturing the same
[0001] The present invention relates to a solid electrolyte battery with good productivity and reliability, and a method for manufacturing the same.
[0002] In recent years, with the development of portable electronic devices such as mobile phones and laptop personal computers, and the practical application of electric vehicles, there has been a growing demand for small, lightweight batteries with high capacity and high energy density.
[0003] Currently, lithium batteries, especially lithium ion batteries, that can meet this requirement use lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ), graphite or the like is used as the negative electrode active material, and an organic electrolyte solution containing an organic solvent and a lithium salt is used as the non-aqueous electrolyte.
[0004] Furthermore, with the further development of devices that use lithium-ion batteries, there is a demand for lithium-ion batteries with longer life, higher capacity, and higher energy density, as well as a high demand for the reliability of lithium-ion batteries with longer life, higher capacity, and higher energy density.
[0005] However, the organic electrolyte used in lithium-ion batteries contains flammable organic solvents, which can cause the organic electrolyte to generate excessive heat in the event of an abnormality such as a short circuit. Furthermore, with the recent trend toward higher energy density in lithium-ion batteries and an increasing amount of organic solvent in the organic electrolyte, there is a growing demand for greater reliability in lithium-ion batteries.
[0006] In light of the above, solid electrolyte batteries that use a molded body of a solid electrolyte without using an organic solvent instead of an organic solvent-based electrolyte are also being considered. Unlike organic solvent-based electrolytes, solid electrolyte batteries have high reliability because their solid electrolytes do not generate abnormal heat. Therefore, there are high expectations for them, especially in product fields that require high-capacity secondary batteries.
[0007] Furthermore, solid electrolyte batteries are not only highly safe, but also highly reliable, environmentally resistant, and have a long lifespan, making them promising maintenance-free batteries that can contribute to social development while also continuing to contribute to safety and security. Providing solid electrolyte batteries to society can contribute to achieving Goal 3 (Ensure healthy lives and promote well-being for all at all ages), Goal 7 (Ensure access to affordable, reliable, sustainable, and modern energy for all), Goal 11 (Make cities inclusive, safe, resilient, and sustainable cities and human settlements), and Goal 12 (Ensure sustainable consumption and production patterns) of the 17 Sustainable Development Goals (SDGs) established by the United Nations.
[0008] Incidentally, in batteries such as solid electrolyte batteries, a pressure member that applies pressure to a power generating element including electrodes inside an exterior body is sometimes used for the purpose of improving characteristics and productivity.
[0009] For example, Patent Document 1 proposes a sealed storage battery in which pressure spacers that deform to increase the volume occupied within the cell chamber are arranged in the stacking direction of a group of electrodes, including the electrodes, thereby improving the adhesion between the electrodes and the retainer.
[0010] Furthermore, Patent Document 2 proposes a sulfide all-solid-state battery having a pressure member made of a material that expands without generating gas when heated, between an electrode body having a sulfide solid electrolyte and an exterior body. Patent Document 2 describes that with the sulfide all-solid-state battery, the electrode body is housed in an exterior body, sealed, and then heated, thereby expanding the pressure member and obtaining a pressure force, thereby enabling efficient arrangement of the pressure member and improving productivity.
[0011] Japanese Patent Application Laid-Open No. 6-290805 Japanese Patent Application Laid-Open No. 2022-156220
[0012] However, in the case of the batteries described in Patent Documents 1 and 2, before the exterior body is sealed, the electrodes (power generating elements) that make up the electrode body are simply stacked on top of each other. Therefore, there is a risk that the power generating elements that make up the electrode body or the electrodes may become misaligned at each stage of the battery production, such as when the electrode body is housed in the exterior body, when wiring is performed after the electrode body is housed in the exterior body, and when the exterior body is sealed. This leaves room for improvement in the productivity of the battery and the reliability of the resulting battery.
[0013] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a solid electrolyte battery with good productivity and reliability, and a method for manufacturing the same.
[0014] The solid electrolyte battery of the present invention comprises an electrode body formed by stacking a plurality of pellet-shaped power generating elements, and an outer casing, each of the plurality of power generating elements having a positive electrode layer, a solid electrolyte layer, and a negative electrode layer stacked in that order, the electrode body is housed in an insulating container and enclosed in the outer casing, a foam sheet (A) is disposed at least partially between the inner surface of the container and the electrode body, and the electrode body is fixed within the container by the foam sheet (A).
[0015] Furthermore, the method for manufacturing a solid electrolyte battery of the present invention is a method for manufacturing a solid electrolyte battery having an electrode body formed by stacking a plurality of pellet-shaped power generating elements, an outer casing, and an insulating container that houses the electrode body and is enclosed within the outer casing, and is characterized by comprising the steps of: arranging a sheet that expands when heated in at least a portion between the container and the electrode body; and heating the electrode body after housing it in the container to expand the sheet and fix the side of the electrode body to the inner surface of the container.
[0016] According to the present invention, it is possible to provide a solid electrolyte battery with good productivity and reliability, and a method for manufacturing the same.
[0017] 1 is a perspective view showing a schematic example of a housing that can be used for the solid electrolyte battery of the present invention. It is a perspective view showing a state in which an electrode body is housed in the housing of Fig. 1. It is a cross-sectional view showing a schematic example of the solid electrolyte battery of the present invention.
[0018] The solid electrolyte battery of the present invention includes an electrode assembly including a plurality of stacked pellet-shaped power generating elements each including a positive electrode layer, a solid electrolyte layer, and a negative electrode layer stacked in that order, and an outer casing. The electrode assembly is housed in an insulating container and enclosed within the outer casing, and a foam sheet (A) is disposed at least partially between the electrode assembly and the inner surface of the container. The electrode assembly is fixed within the container, for example, by having one surface of the foam sheet (A) adhere to the inner surface of the container and the other surface of the foam sheet (A) adhere to a side surface of the electrode assembly.
[0019] FIG. 1 is a perspective view showing a schematic example of a housing that can be used for a solid electrolyte battery. The housing 10 shown in FIG. 1 has a cylindrical shape with a bottom and is capable of housing an electrode assembly therein. The housing 10 is formed of an insulating material such as resin, and has a resin sheet 20 on at least a portion of its inner surface. The resin sheet 20 can be foamed by heating to form an insulating foam sheet (A). The resin sheet 20 can be provided with an adhesive layer formed of an adhesive, and this adhesive layer can be used to adhere the resin sheet 20 to the inner surface of the housing, thereby tightly bonding the two together.
[0020] The container 10 is also provided with slits 11 , 11 for exposing the positive electrode layer connection terminal and the negative electrode layer connection terminal of the electrode assembly to the outside of the container 10 .
[0021] FIG. 2 is a perspective view schematically illustrating an electrode assembly housed inside the housing 10 of FIG. 1 . The electrode assembly 30 housed inside the housing 10 is formed by stacking a plurality of pellet-shaped power generating elements. One electrode layer (e.g., positive electrode layers) of each current collecting element constituting the electrode assembly 30 is electrically connected to another electrode layer (e.g., positive electrode layer connection terminal) via a conductive connection terminal (e.g., a positive electrode layer connection terminal) by welding the connection terminal to a lead 53, and the other electrode layer (e.g., a negative electrode layer) is electrically connected to another electrode layer (e.g., a negative electrode layer connection terminal) via a conductive connection terminal (e.g., a negative electrode layer connection terminal) by welding the connection terminal to a lead 64. The lead 53 and the electrode layer connection terminal attached to the lead 53, as well as the lead 64 and the electrode layer connection terminal attached to the lead 64, are exposed to the outside of the housing 10 through the slits 11.
[0022] A foam sheet (A) 21 is interposed between the housing 10 and the electrode assembly 30, with one side of this foam sheet (A) 21 in close contact with the inner surface of the housing 10 and the other side in close contact with the side of the electrode assembly 30. For example, by heating the housing 10 shown in FIG. 1 with the electrode assembly 30 housed therein, the resin sheet 20 foams and increases in thickness to become a foam sheet 21, and as shown in FIG. 2, the surface opposite the inner surface of the housing 10 comes into close contact with the side of the electrode assembly 30. Note that if an adhesive layer is provided on the resin sheet used to form the foam sheet (A) 21 and the resin sheet is attached to the inner surface of the housing 10 by this adhesive layer, the foam sheet (A) 21 formed by heating the resin sheet to foam it is in close contact with the inner surface of the housing 10 by being bonded to each other by the adhesive layer.
[0023] Next, an example of a solid electrolyte battery will be described with reference to the drawings. Fig. 3 is a cross-sectional view schematically showing an example of a solid electrolyte battery of the present invention. The cross-section shown in Fig. 3 corresponds to the cross-section of line II of the housing 10 housing the electrode assembly 30 shown in Fig. 2.
[0024] 3 has an electrode assembly 30 formed by stacking four pellet-shaped power generating elements 40, and an exterior body made up of a cylindrical metal exterior can 80 with a bottom and a metal lid 90. The exterior can and the lid can be made of aluminum, stainless steel, or the like.
[0025] A metal terminal 100 is attached to the lid 90 via an insulating packing 110 made of resin (such as polypropylene), glass hermetic, ceramic hermetic, or the like. When using an electrolyte that decomposes due to moisture in the air, such as a sulfide or hydride, as the solid electrolyte, it is desirable to use a glass hermetic or ceramic hermetic, which has a higher airtightness. The lid 90 is then inserted into the opening of the outer can 80, and the joint between the two is welded or the like to seal the opening of the outer can 80, thereby hermetically sealing the inside of the battery.
[0026] Each of the power generating elements 40 in the electrode assembly 30 is formed by sequentially stacking a positive electrode layer 50, a solid electrolyte layer 70, and a negative electrode layer 60. Four power generating elements 40 are stacked vertically in the drawing and connected in parallel to each other as described below to form the electrode assembly 30.
[0027] The electrode body 30 is formed by stacking each power generating element 40 so that the electrode layers of the same polarity of adjacent power generating elements 40 face each other (for example, the power generating element 40 located at the top and the power generating element 40 adjacent thereto below are stacked so that the positive electrode layers 50, 50 of each element face each other).
[0028] Furthermore, a positive electrode layer connection terminal 51 is disposed between the positive electrode layer 50 of the uppermost power-generating element 40 and the positive electrode layer 50 of the power-generating element 40 adjacent thereto below, for conducting electrical power to these positive electrode layers 50, 50. Also, a positive electrode layer connection terminal 52 is disposed between the positive electrode layer 50 of the lowermost power-generating element 40 and the positive electrode layer 50 of the power-generating element 40 adjacent thereto above, for conducting electrical power to these positive electrode layers 50, 50. Although not shown in FIG. 3 , the positive electrode layer connection terminals 51, 52 are each electrically connected to a lead (lead 53 in FIG. 2 ) by welding or the like, and, for example, this lead is electrically connected to the inner surface of the exterior can 80, which also serves as the positive electrode terminal, by welding or the like.
[0029] Furthermore, an anode layer connection terminal 61 is disposed above the anode layer 60 of the uppermost power-generating element 40, for conducting electrical power with the anode layer 60. Furthermore, an anode layer connection terminal 62 is disposed between the anode layer 60 of the second-highest power-generating element 40 and the anode layer 60 of the power-generating element 40 adjacent thereto below, for conducting electrical power with the anode layers 60, 60. Furthermore, an anode layer connection terminal 63 is disposed below the anode layer 60 of the lowermost power-generating element 40, for conducting electrical power with the anode layer 60. Although not shown in FIG. 3 , the anode layer connection terminals 61, 62, 63 are electrically connected to a lead (lead 64 in FIG. 2 ) by welding or the like. For example, the lead is electrically connected by welding or the like to the underside of the terminal 100, which functions as the negative terminal.
[0030] Although FIG. 3 shows a solid electrolyte battery in an embodiment in which the outer can 80 also functions as a positive electrode terminal and the terminal 100 functions as a negative electrode terminal, if necessary, the outer can 80 can also function as a negative electrode terminal and the terminal 100 functions as a positive electrode terminal.
[0031] The electrode body 30 is housed in the housing 10 and enclosed in the exterior body. A foam sheet (A) 21 is interposed between the electrode body 30 and the housing 10, and this foam sheet (A) 21 is in close contact with the side surface of the electrode body 30 on one side and with the inner surface of the housing 10 on the other side, thereby fixing the electrode body 30.
[0032] As shown in FIG. 3 , in the solid electrolyte battery of the present invention, an electrode assembly formed by stacking multiple pellet-shaped power generation elements is housed within a housing. The housing and the electrode assembly are fixed within the housing by, for example, contacting a foam sheet (A) with each other (i.e., the position of the power generation elements constituting the electrode assembly is fixed within the housing). Therefore, when the housing containing the electrode assembly is housed within an exterior body (exterior can) and wiring is performed, misalignment between the power generation elements does not occur, improving workability. This ensures high productivity for the solid electrolyte battery of the present invention. Furthermore, since misalignment between the power generation elements constituting the electrode assembly does not occur even in the battery state, high reliability can also be ensured. Furthermore, the housing prevents contact between the electrodes constituting the power generation elements of the electrode assembly and the inner surface of the exterior can, which also serves as the terminal for the counter electrode, thereby effectively preventing the occurrence of short circuits. The electrode body can be fixed in the container using the foam sheet (A) by closely adhering one surface of the foam sheet (A) to the inner surface of the container and the other surface to the side surface of the electrode body. However, as long as the position of the electrode body in the container can be fixed, for example, only a portion of one surface of the foam sheet (A) may be closely adhering to the inner surface of the container, or only a portion of the other surface of the foam sheet (A) may be closely adhering to the side surface of the electrode body.
[0033] Furthermore, since the electrode body can be accommodated in the container and then the foamed sheet (A) can be formed to fix the electrode body in the container, for example, when accommodating the electrode body, the opening diameter of the container including the sheet for forming the foamed sheet (A) can be made large to improve workability, and the electrode body can be fixed in the container by subsequently forming the foamed sheet (A) through a simple operation such as heating. Thus, in the solid electrolyte battery of the present invention, a decrease in production efficiency due to an increase in the number of manufacturing steps caused by operations such as accommodating the electrode body in the container and fixing the electrode body in the container is minimized.
[0034] Furthermore, in the solid electrolyte battery 1 shown in FIG. 3 , a foam sheet (B) 120 is interposed between the housing 10 housing the electrode assembly 30 and the outer can 80, with one side of this foam sheet (B) 120 in close contact with the outer surface of the housing 10 and the other side in close contact with the inner surface of the outer can 80. This fixes the position of the housing 10 within the outer can, thereby more effectively preventing the internal wiring from coming loose or the power-generating element from shifting position even when the battery is used in an environment subject to vibration, resulting in a more reliable battery. Note that the foam sheet (B) can fix the housing within the outer can by bringing one side of the foam sheet (B) into close contact with the outer surface of the housing and the other side into close contact with the inner surface of the outer can. However, as long as the position of the housing within the outer can is fixed, for example, only a portion of one side of the foam sheet (B) may be in close contact with the outer surface of the housing, or only a portion of the other side of the foam sheet (B) may be in close contact with the inner surface of the outer can.
[0035] A spacer 130 is disposed between the electrode assembly 30 and the terminal 100, and the electrode assembly 30 (each stacked power-generating element 40) is pressed toward the bottom of the outer can 80 by this spacer 130. As will be described later, the connection terminals that connect the electrode layers of each power-generating element 40 may or may not be fixed to adjacent electrode layers. However, even if the connection terminals are not fixed to the electrode layers, the action of the spacer 130 can ensure good connection between the connection terminals and the electrode layers, resulting in a solid electrolyte battery with superior characteristics. The spacer 130 can be made of a rubber plate, a metal spring (such as a leaf spring), or the like.
[0036] Next, the solid electrolyte battery of the present invention will be described in detail. The solid electrolyte battery of the present invention includes primary batteries and secondary batteries.
[0037] <Housing> The housing may be made of any insulating material, such as polyolefins such as polypropylene and polyethylene; polystyrene; aramid; polyamide-imide; polyimide; nylon; polyesters such as polyethylene terephthalate (PET); polyarylate, etc. The thickness of the housing (thickness of the resin (sheet) that makes up the housing) is preferably 100 to 1000 μm.
[0038] As shown in Fig. 3 , the housing may have slits for exposing the connection terminals connecting the positive electrode layers and the connection terminals connecting the negative electrode layers to the outside of the housing as needed. The slits may be omitted if not necessary, for example, when forming an electrode assembly by connecting power generating elements in series. When forming an electrode assembly by connecting power generating elements in parallel as shown in Fig. 3 , as described above, when connecting the connection terminals connecting the positive electrode layers and the negative electrode layers to leads, the slits allow the power generating elements to be housed in the housing. Therefore, the power generating elements can be housed in the housing, heated to form a foam sheet (A), and connected to each other while the power generating elements are fixed by this foam sheet (A). This prevents misalignment of the power generating elements during connection, thereby further improving the productivity of the electrode assembly and, ultimately, the productivity of solid electrolyte batteries.
[0039] The width of the slits in the container should be such that the electrode layer connection terminals and the leads to which these connection terminals are attached can be sufficiently exposed from each slit, but if the width is too wide, there is a risk that the container will not have sufficient strength, so it is preferable that the width (if there are multiple slits, the total width of all slits) be 30% or less of the outer periphery of the container when viewed in a plane.
[0040] <Foam Sheet (A) and Foam Sheet (B)> The foam sheet (A) and the foam sheet (B) can be formed by using a sheet (resin sheet) that foams when heated and foaming it. The sheet that foams when heated preferably has an adhesive layer on one side. Various foam sheets can be used as the sheet for forming the foam sheet (A) and the foam sheet (B). However, preferred are those obtained by kneading a foaming agent into various resins such as epoxy resins, urethane resins, silicone resins, polyethylene, polypropylene, polyester, polystyrene, and acrylic resins; or various rubbers such as polybutadiene and polyisoprene; and molding the resulting sheet into a sheet. The foaming agent is a compound such as N 2 , CO 2 , H 2 It is possible to use a material that generates O etc. In addition, when a sulfide-based solid electrolyte, a hydride-based solid electrolyte, or the like that has high reactivity with water is used as the solid electrolyte, H 2 Foaming agents that generate O are undesirable. There are also products in which components that generate gas upon heating are encapsulated in microcapsules. Using these products within a temperature range where the gas generated by foaming does not escape from the microcapsules (a temperature approximately 10 to 30°C lower than the maximum foaming temperature) is preferable because the foamed resin remains encapsulated in the microcapsules, eliminating the need to worry about a decrease in battery performance due to the generated gas. Examples of microcapsule-type foaming agents include Kureha Microsphere (trade name), Matsumoto Yushi Pharmaceutical's Matsumoto Microsphere (trade name), Nippon Phillite's Expancel (trade name), and Sekisui Chemical's Advancel EM (trade name). The particle diameter of the microcapsules before foaming is preferably 5 to 100 μm, and the maximum diameter is preferably less than half the layer thickness of the foam sheet. The thickness (thickness after foaming) of the foam sheet (A) or foam sheet (B) is preferably 100 to 1000 μm.
[0041] The foam sheet (A) is disposed at least partially between the inner surface of the housing and the electrode assembly, and from the viewpoint of favorably fixing the electrode assembly, it is preferable that the foam sheet (A) be present over 50% or more of the total area of the inner surface of the housing (if the housing has a slit, the total area excluding the slit). Alternatively, the foam sheet (A) may be present over the entire inner surface of the housing (100% of the total area of the inner surface).
[0042] The foam sheet (B) may be disposed at least partially between the outer surface of the housing and the inner surface of the outer can, but from the viewpoint of favorably fixing the housing containing the electrode assembly, it is preferable that the foam sheet (B) be present over 50% or more of the total area of the outer surface of the housing (if the housing has a slit, the total area excluding the slit). Alternatively, the foam sheet (B) may be present over the entire outer surface of the housing (100% of the total area of the outer surface).
[0043] <Positive Electrode Layer> The positive electrode layer of the solid electrolyte battery can be formed, for example, by molding a positive electrode mixture containing a positive electrode active material and the like.
[0044] When the solid electrolyte battery is a primary battery, the positive electrode active material can be the same as the positive electrode active material used in conventionally known non-aqueous electrolyte primary batteries. Specifically, for example, manganese dioxide, lithium-containing manganese oxide (e.g., LiMn 3 O 6 or a composite oxide having the same crystal structure as manganese dioxide (e.g., β-type, γ-type, or a mixed structure of β-type and γ-type) and containing 3.5% by mass or less, preferably 2% by mass or less, more preferably 1.5% by mass or less, particularly preferably 1% by mass or less of Li, a Ti 5/3 O 4 (4 / 3≦a<7 / 3) and other lithium-containing composite oxides; vanadium oxide; niobium oxide; titanium oxide; sulfides such as iron disulfide; graphite fluoride; Ag 2 Silver sulfides such as S; NiO 2 Nickel oxides such as:
[0045] When the solid electrolyte battery is a secondary battery, the positive electrode active material is not particularly limited as long as it is a positive electrode active material used in conventionally known non-aqueous electrolyte secondary batteries, that is, an active material capable of absorbing and releasing Li ions. Specific examples of the positive electrode active material include LiM r Mn 2-r O 4 (wherein M is at least one element selected from the group consisting of Li, Na, K, B, Mg, Ca, Sr, Ba, Ti, V, Cr, Zr, Fe, Co, Ni, Cu, Zn, Al, Sn, Sb, In, Nb, Ta, Mo, W, Y, Ru, and Rh, and 0≦r≦1), a spinel-type lithium manganese composite oxide represented by Li r Mn (1-s-r) Ni s M t O (2-u) F v (wherein M is at least one element selected from the group consisting of Co, Mg, Al, B, Ti, V, Cr, Fe, Cu, Zn, Zr, Mo, Sn, Ca, Sr, and W, and 0.8≦r≦1.2, 0<s<0.5, 0≦t≦0.5, u+v<1, −0.1≦u≦0.2, 0≦v≦0.1), a layered compound represented by 1-r M r O 2 (wherein M is at least one element selected from the group consisting of Al, Mg, Ti, V, Cr, Zr, Fe, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0≦r≦0.5), lithium cobalt composite oxide represented by LiNi 1-r M r O 2 (wherein M is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Fe, Co, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, and Ba, and 0≦r≦0.5), a lithium nickel composite oxide represented by Li 1+s M 1-r N r P.O. 4 F s(wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5, 0≦s≦1), Li 2 M 1-r N r P 2 O 7 (wherein M is at least one element selected from the group consisting of Fe, Mn, and Co, and N is at least one element selected from the group consisting of Al, Mg, Ti, Zr, Ni, Cu, Zn, Ga, Ge, Nb, Mo, Sn, Sb, V, and Ba, and 0≦r≦0.5), and the like. Among these, only one type may be used, or two or more types may be used in combination.
[0046] When the solid electrolyte battery is a secondary battery, the average particle size of the positive electrode active material is preferably 0.1 μm or more, more preferably 0.5 μm or more, and preferably 25 μm or less, more preferably 10 μm or less, from the viewpoint of reducing side reactions that cause battery capacity degradation and increasing the density of the positive electrode. The positive electrode active material may be primary particles or secondary particles formed by aggregation of primary particles. When the positive electrode layer contains a solid electrolyte, using a positive electrode active material with an average particle size in the above range allows for a large interface with the solid electrolyte, thereby further improving the load characteristics of the battery.
[0047] The average particle diameter of the positive electrode active material and the average particle diameter of other particles (such as solid electrolytes) referred to in this specification are determined by a particle size distribution measuring device (such as a Microtrac particle size distribution measuring device "HRA9320" manufactured by Nikkiso Co., Ltd.) and are the 50% diameter value (D) in the volume-based integrated fraction when determining the integrated volume from particles with small particle sizes. 50 ) means
[0048] When the positive electrode layer contains a solid electrolyte, the positive electrode active material preferably has a reaction suppression layer on its surface to suppress reaction with the solid electrolyte contained in the positive electrode layer.
[0049] If the positive electrode active material and the solid electrolyte come into direct contact in the positive electrode layer, the solid electrolyte may oxidize to form a resistance layer, which may reduce ionic conductivity in the layer. By providing a reaction suppression layer on the surface of the positive electrode active material that suppresses reaction with the solid electrolyte and preventing direct contact between the positive electrode active material and the solid electrolyte, it is possible to suppress the reduction in ionic conductivity in the positive electrode layer due to oxidation of the solid electrolyte.
[0050] The reaction suppression layer may be made of a material that has ion conductivity and can suppress the reaction between the positive electrode active material and the solid electrolyte. Examples of materials that can form the reaction suppression layer include oxides containing Li and at least one element selected from the group consisting of Nb, P, B, Si, Ge, Ti, Zr, Ta, and W, more specifically, LiNbO 3 Nb-containing oxides such as Li 3 P.O. 4 , Li 3 BO 3 , Li 4 SiO 4 , Li 4 GeO 4 , LiTiO 3 , LiZrO 3 , Li 2 WO 4 The reaction suppression layer may contain only one of these oxides, or may contain two or more of them, or may contain a composite compound of two or more of these oxides. Among these oxides, it is preferable to use an Nb-containing oxide, such as LiNbO 3 It is more preferable to use
[0051] The reaction suppression layer is preferably present on the surface in an amount of 0.1 to 2.0 parts by mass per 100 parts by mass of the positive electrode active material, which allows for effective suppression of the reaction between the positive electrode active material and the solid electrolyte.
[0052] Examples of methods for forming a reaction suppression layer on the surface of a positive electrode active material include the sol-gel method, mechanofusion method, CVD method, PVD method, and ALD method.
[0053] The content of the positive electrode active material in the positive electrode layer is preferably 20 to 95 mass %.
[0054] Examples of conductive additives for the positive electrode include carbon materials such as carbon black (thermal black, furnace black, channel black, ketjen black, acetylene black, etc.), graphite (natural graphite, artificial graphite), graphene, vapor-grown carbon fiber, carbon nanofiber, and carbon nanotube; powders of Cu, Ni, Al, Au, and Pd alone or alloys thereof, or porous bodies thereof; and these may be used alone or in combination of two or more. The content of the conductive additive in the positive electrode layer is preferably 0.1 to 15% by mass.
[0055] The positive electrode layer may contain a solid electrolyte. The solid electrolyte used in the positive electrode layer is not particularly limited as long as it has Li ion conductivity, and examples thereof include sulfide-based solid electrolytes, hydride-based solid electrolytes, halide-based solid electrolytes, and oxide-based solid electrolytes.
[0056] The sulfide-based solid electrolyte is Li 2 S-P 2 S 5 , Li 2 S-SiS 2 , Li 2 S-P 2 S 5 -GeS 2 , Li 2 S-B 2 S 3 In addition to particles of glass, thio-LISICON type particles [Li 10 GeP 2 S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 Li12-12a-b+c+6d-eM, etc. 1 3+a-b-c-d M 2 b M 3 c M 4 d M 5 12-e X e (However, M1 is Si, Ge or Sn, M 2 is P or V, M 3 is Al, Ga, Y or Sb, M 4 is Zn, Ca, or Ba, M 5 is either S or S and O, and X is F, Cl, Br or I, 0≦a<3, 0≦b+c+d≦3, 0≦e≦3], or argyrodite type [Li 6 P.S. 5 Li, such as Cl 7-k P.S. 6-k X k (wherein X represents one or more halogen elements, and 0.2<k<2.0), Li 7-f+g P.S. 6-f Cl f+g (wherein 0.05≦g≦0.9, −3.0f+1.8≦g≦−3.0f+5.7), Li 7-h P.S. 6-h Cl i Br j (where h=i+j, 0<h≦1.8, 0.1≦i / j≦10.0) can also be used.
[0057] Examples of hydride-based solid electrolytes include LiBH 4 , LiBH 4 and a solid solution of the following alkali metal compound (e.g., LiBH 4 and the alkali metal compound in a molar ratio of 1:1 to 20:1. The alkali metal compound in the solid solution may be at least one selected from the group consisting of lithium halides (LiI, LiBr, LiF, LiCl, etc.), rubidium halides (RbI, RbBr, RbF, RbCl, etc.), cesium halides (CsI, CsBr, CsF, CsCl, etc.), lithium amide, rubidium amide, and cesium amide.
[0058] Examples of halide-based solid electrolytes include monoclinic LiAlCl 4 , defect spinel type or layer structure LiInBr 4 , monoclinic Li 6-3m Y m X 6(wherein 0 < m < 2 and X = Cl or Br), and other known compounds described in, for example, WO 2020 / 070958 and WO 2020 / 070955 can also be used.
[0059] Examples of oxide-based solid electrolytes include Li 2 O-Al 2 O 3 -SiO 2 -P 2 O 5 -TiO 2 Li-based glass ceramics 2 O-Al 2 O 3 -SiO 2 -P 2 O 5 -GeO 2 Lithium-ion-based glass ceramics, garnet-type 7 La 3 Zr 2 O 12 , NASICON type Li 1+O Al 1+O Ti 2-O (P.O. 4 ) 3 , Li 1+p Al 1+p Ge 2-p (P.O. 4 ) 3 , perovskite-type Li 3q La 2/3-q TiO 3 Examples include:
[0060] Among these solid electrolytes, sulfide-based solid electrolytes are preferred because of their high Li ion conductivity, sulfide-based solid electrolytes containing Li and P are more preferred, and argyrodite-type sulfide-based solid electrolytes are even more preferred because of their particularly high Li ion conductivity and high chemical stability.
[0061] The content of the solid electrolyte in the positive electrode layer is preferably 4 to 80 mass %.
[0062] The positive electrode layer may contain a binder, or may not contain a binder if good moldability can be ensured without using a binder, such as in the case of a positive electrode in which a sulfide-based solid electrolyte is contained and powder of the positive electrode mixture is charged into a molding die and compacted.
[0063] Examples of the binder contained in the positive electrode layer include fluororesins such as PVDF.
[0064] When a binder is required in the positive electrode layer, the content is preferably 15% by mass or less, and preferably 0.5% by mass or more. On the other hand, when a binder is not required in the positive electrode layer from the viewpoint of formability, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).
[0065] The positive electrode layer may have a current collector. Examples of the current collector for the positive electrode layer include metal foils such as aluminum and stainless steel; sheet-like conductive porous substrates such as punched metal, mesh, expanded metal, and foamed metal; and carbon sheets. As the sheet-like conductive porous substrate, it is preferable to use a foamed metal porous body. A specific example of a foamed metal porous body is "Celmet (registered trademark)" from Sumitomo Electric Industries, Ltd.
[0066] The positive electrode layer can be formed, for example, by compressing a positive electrode mixture prepared by mixing a positive electrode active material, a conductive additive, a solid electrolyte, and, if necessary, a binder, by pressure molding or the like.
[0067] In the case of a positive electrode layer having a current collector, it can be formed by, for example, pressing the current collector onto a pressed molded body of the positive electrode mixture obtained as described above.
[0068] The thickness of the positive electrode layer is usually 50 μm or more, but from the viewpoint of increasing the capacity of the battery, it is preferably 200 μm or more, and is usually 2000 μm or less.
[0069] The thickness of the current collector for the positive electrode layer is preferably 0.01 to 0.1 mm.
[0070] <Negative Electrode Layer> The negative electrode layer of the solid electrolyte battery can be formed, for example, by molding a negative electrode mixture containing a negative electrode active material and the like.
[0071] When the solid electrolyte battery is a primary battery, examples of the negative electrode active material include metallic lithium and lithium alloys (lithium-aluminum alloys, lithium-indium alloys, etc.).
[0072] When the solid electrolyte battery is a secondary battery, the negative electrode active material may be, for example, one or a mixture of two or more carbonaceous materials capable of absorbing and releasing lithium, such as graphite, pyrolytic carbons, cokes, glassy carbons, fired bodies of organic polymer compounds, mesocarbon microbeads (MCMB), and carbon fibers. Furthermore, simple substances, compounds, and alloys thereof containing elements such as Si, Sn, Ge, Bi, Sb, and In; compounds capable of charging and discharging at low voltages close to those of lithium metal, such as lithium-containing nitrides or lithium-containing oxides; lithium metal; and lithium / aluminum alloys. For example, Li 4 Ti 5 O 12 and TiO 2 , NbO 2.5-δ (0≦δ≦0.5), MoO 3-δ (0≦δ≦1), WO 3-δ (0≦δ≦1), TiNb 2 O 7 Metal oxides such as WS 2 , MoS 2 or a mixture of two or more of these metal sulfides can also be used as the negative electrode active material.
[0073] The content of the negative electrode active material in the negative electrode layer is preferably 50 to 95 mass %.
[0074] The negative electrode layer can contain a solid electrolyte. The solid electrolyte contained in the negative electrode layer can be one or more of the sulfide-based solid electrolytes, hydride-based solid electrolytes, and oxide-based solid electrolytes previously exemplified as the solid electrolytes that can be contained in the positive electrode layer. Among the solid electrolytes exemplified above, sulfide-based solid electrolytes are more preferably used because they have high Li ion conductivity and also have the function of enhancing the negative electrode layer, and argyrodite-type sulfide-based solid electrolytes are even more preferably used.
[0075] The content of the solid electrolyte in the negative electrode layer is preferably 4 to 70 mass %.
[0076] The negative electrode layer may contain a conductive additive. Specific examples include carbon materials such as graphite (natural graphite, artificial graphite), graphene, carbon black, vapor-grown carbon fiber, carbon nanofiber, and carbon nanotube. The content of the conductive additive in the negative electrode layer is preferably 1 to 10 mass %.
[0077] The negative electrode layer may or may not contain a binder. Specific examples thereof include the same binders as those exemplified above as binders that can be contained in the positive electrode layer. For example, when the negative electrode layer contains a sulfide-based solid electrolyte, if good formability can be ensured in forming the negative electrode layer without using a binder, the negative electrode layer may not contain a binder.
[0078] When a binder is required in the negative electrode layer, the content is preferably 15% by mass or less, and preferably 0.5% by mass or more. On the other hand, when good formability can be obtained without the binder in the negative electrode layer, the content is preferably 0.5% by mass or less, more preferably 0.3% by mass or less, and even more preferably 0% by mass (i.e., no binder is contained).
[0079] The negative electrode layer may have a current collector. Examples of the current collector for the negative electrode layer include sheet-like conductive porous substrates such as copper or nickel foil, punched metal, mesh, expanded metal, and foamed metal; carbon sheets; and the like. As the sheet-like conductive porous substrate, it is preferable to use a foamed metal porous body. A specific example of a foamed metal porous body is "Celmet (registered trademark)" by Sumitomo Electric Industries, Ltd.
[0080] The negative electrode layer can be formed, for example, by compressing a negative electrode mixture prepared by mixing a negative electrode active material, a conductive additive, a solid electrolyte, and, if necessary, a binder, by pressure molding or the like.
[0081] In the case of a negative electrode layer having a current collector, it can be formed by, for example, pressing a current collector onto a pressed molded product of the negative electrode mixture obtained as described above.
[0082] The thickness of the negative electrode layer is usually 100 μm or more, but is preferably 200 μm or more from the viewpoint of increasing the capacity of the battery, and is usually 3000 μm or less.
[0083] The thickness of the current collector for the negative electrode layer is preferably 0.01 to 0.1 mm.
[0084] <Solid Electrolyte Layer> For the solid electrolyte layer in a solid electrolyte battery, one or more of the sulfide-based solid electrolytes, hydride-based solid electrolytes, and oxide-based solid electrolytes exemplified above as solid electrolytes that can be contained in the positive electrode layer can be used. Among the above-exemplified solid electrolytes, it is more preferable to use a sulfide-based solid electrolyte, and it is even more preferable to use an argyrodite-type sulfide-based solid electrolyte, in order to improve battery characteristics.
[0085] The solid electrolyte layer can be formed by a method of compressing a solid electrolyte by pressure molding or the like; a method of applying a solid electrolyte layer-forming composition prepared by dispersing a solid electrolyte in a solvent onto a substrate, a positive electrode, or a negative electrode, drying the composition, and, if necessary, performing pressure molding such as pressing.
[0086] The solid electrolyte layer may also have a porous body such as a resin nonwoven fabric as a support.
[0087] It is preferable to select a solvent for the solid electrolyte layer-forming composition that is less likely to deteriorate the solid electrolyte. In particular, sulfide-based solid electrolytes and hydride-based solid electrolytes undergo chemical reactions with trace amounts of water, so it is preferable to use a nonpolar aprotic solvent, such as hydrocarbon solvents such as hexane, heptane, octane, nonane, decane, decalin, toluene, and xylene. It is particularly preferable to use an ultra-dehydrated solvent with a water content of 0.001% by mass (10 ppm) or less. Fluorine-based solvents such as "Vertrel (registered trademark)" manufactured by DuPont-Mitsui Fluorochemicals, "Zeorolla (registered trademark)" manufactured by Nippon Zeon Co., Ltd., and "Novec (registered trademark)" manufactured by Sumitomo 3M Co., Ltd., as well as nonaqueous organic solvents such as dichloromethane and diethyl ether can also be used.
[0088] The thickness of the solid electrolyte layer is preferably 10 to 500 μm.
[0089] <Power-generating element and electrode body> The power-generating element is in the form of a pellet, and is formed by sequentially laminating a positive electrode layer, a solid electrolyte layer, and a negative electrode layer. To obtain the power-generating element, for example, a positive electrode layer (or a negative electrode layer) may be formed in advance by pressure molding, and the solid electrolyte layer and the negative electrode layer (or a positive electrode layer) may be sequentially pressure molded using this as a base material, or a positive electrode layer may be formed in advance by pressure molding on one side of a solid electrolyte layer formed in advance by pressure molding, and the negative electrode layer may be formed in advance by pressure molding on the other side of the solid electrolyte layer.
[0090] The shape of the power generating element in plan view is not particularly limited, and may be a circle, an ellipse, a polygon such as a square, or the like.
[0091] The electrode assembly is formed by stacking a plurality of power generating elements and connecting adjacent power generating elements in parallel or in series. When connecting power generating elements in parallel, for example, a method of stacking adjacent power generating elements so that electrode layers of the same polarity face each other can be used, as shown in FIG.
[0092] When the power generating elements are connected in series, for example, a method can be employed in which adjacent power generating elements are stacked so that their electrode layers with opposite polarities face each other.
[0093] In both cases where the power generation elements are connected in parallel and in series, the opposing electrode layers may be electrically connected by interposing a conductive connection terminal between them. The connection terminal that electrically connects the electrode layers may be fixed to either one of the opposing electrode layers, or may not be fixed to either electrode layer. When fixing the connection terminal to the electrode layer, for example, the connection terminal may be welded to the metal current collector of an electrode layer having the metal current collector.
[0094] The number of power generating elements in the electrode body is not particularly limited as long as it is plural (two or more), and it is possible to have 10, 20 or more depending on the characteristics required of the solid electrolyte battery.
[0095] <Connection terminals and leads> For connection terminals for extracting power from the electrode layers of the power generating element (connection terminals that connect the electrode layers of adjacent power generating elements) and leads for connecting the connection terminals, metal foils (plates) such as stainless steel, nickel, aluminum, iron, copper, clad materials combining these materials, and materials obtained by plating these materials with nickel, chromium, nickel chromium, etc. can be used.
[0096] The thickness of the connection terminals and leads made of metal foil (plate) is preferably 10 to 100 μm. There are no particular restrictions on the size of the connection terminals and leads, but when they are exposed to the outside of the housing through a slit in the housing, their width is set to be shorter than the width of the slit.
[0097] <Exterior Body> The exterior body of a solid electrolyte battery is not particularly limited, but because the electrode body contained therein is formed by stacking a plurality of power generating elements, an exterior body having a bottomed tubular exterior can (a rectangular tubular can or a cylindrical can) and a lid as shown in Fig. 3 is preferably used. The exterior can and the lid can be connected by welding or by crimping with a gasket.
[0098] <Method for manufacturing a solid electrolyte battery> When manufacturing a solid electrolyte battery, a sheet for forming the foam sheet (A) (resin sheet 20 in FIG. 1 ) is placed on the inner surface of a housing, and an electrode assembly having a power generation element laminated thereon is housed in this housing, or an electrode assembly having a sheet for forming the foam sheet (A) placed on its side is housed in a housing and heated to foam the sheet into a foam sheet (A), and one side of the foam sheet (A) is brought into close contact with the inner surface of the housing and the other side is brought into close contact with the side of the electrode assembly, thereby fixing the electrode assembly in the housing. For example, in the case of an electrode assembly in which power generation elements are connected in parallel, connection of the power generation elements in the electrode assembly can be carried out after fixing the power generation elements in the housing with the foam sheet (A) by using a housing having slits as described above.
[0099] The housing with the electrode assembly fixed therein by the foam sheet (A) is housed in an outer can, and necessary wiring is provided thereto, and if necessary, the housing is fixed inside the outer can by the foam sheet (B), and then the opening of the outer can is sealed with a lid to form an outer housing, thereby completing a solid electrolyte battery. Furthermore, the formation of the foam sheet (B) [formation of the foam sheet (B) by heating a sheet for the foam sheet (B)] can also be performed after the formation of the outer housing (after sealing).
[0100] The present invention can be implemented in other forms without departing from the spirit of the present invention. The embodiments disclosed in this application are merely examples, and the present invention is not limited to these embodiments. The scope of the present invention shall be interpreted in accordance with the appended claims rather than the description in the above specification, and all modifications within the scope of the claims are included in the scope of the claims.
[0101] The solid electrolyte battery of the present invention can be used in the same applications as conventionally known primary batteries and secondary batteries, but as described above, because of its excellent heat resistance, it can be preferably used in applications where it is exposed to high temperatures.
[0102] REFERENCE SIGNS LIST 1 solid electrolyte battery 10 container 20 resin sheet 21 foam sheet (A) 30 electrode body 40 power generating element 50 positive electrode layer 51, 52 positive electrode layer connection terminal 53 lead 60 negative electrode layer 61, 62, 63 negative electrode layer connection terminal 64 lead 70 solid electrolyte layer 80 outer can 90 lid 100 terminal 110 insulating packing 120 foam sheet (B) 130 spacer
Claims
1. A solid electrolyte battery comprising: an electrode body formed by stacking a plurality of pellet-shaped power generating elements; and an exterior body; each of the plurality of power generating elements has a positive electrode layer, a solid electrolyte layer, and a negative electrode layer stacked in that order; the electrode body is contained within an insulating container and enclosed within the exterior body; a foam sheet (A) is disposed at least partially between the inner surface of the container and the electrode body, and the electrode body is fixed within the container by the foam sheet (A).
2. The solid electrolyte battery according to claim 1, wherein the foamed sheet (A) is a sheet foamed by heating.
3. The solid electrolyte battery according to claim 1, wherein the foam sheet (A) has an adhesive layer and is adhered to the inner surface of the container by the adhesive layer.
4. The solid electrolyte battery according to claim 1, wherein the exterior body has a cylindrical or rectangular exterior can, a foam sheet (B) is disposed at least partially between the container and the exterior can, and the container is fixed within the exterior can by the foam sheet (B).
5. The solid electrolyte battery according to claim 4, wherein the foamed sheet (B) is a sheet foamed by heating.
6. The solid electrolyte battery according to claim 4, wherein the foam sheet (B) has an adhesive layer and is bonded to the outer surface of the container or the inner surface of the exterior can by the adhesive layer.
7. The solid electrolyte battery according to claim 1, wherein adjacent power generating elements are connected in series.
8. The solid electrolyte battery according to claim 1, further comprising a conductive positive electrode layer connection terminal that is electrically connected to the positive electrode layer to allow electrical power to be drawn from the positive electrode layer, and a conductive negative electrode layer connection terminal that is electrically connected to the negative electrode layer to allow electrical power to be drawn from the negative electrode layer, and adjacent power generating elements are connected in parallel via the positive electrode layer connection terminal and the negative electrode layer connection terminal.
9. The solid electrolyte battery according to claim 8, wherein a side surface of the container has slits for exposing the positive electrode layer connection terminal and the negative electrode layer connection terminal to the outside of the container.
10. A method for producing a solid electrolyte battery having an electrode body formed by stacking a plurality of pellet-shaped power generating elements, an outer casing, and an insulating container that houses the electrode body and is enclosed within the outer casing, the method comprising the steps of: placing a sheet that foams when heated in at least a portion between the container and the electrode body; and heating the electrode body after housing it in the container to foam the sheet and fix the side of the electrode body to the inner surface of the container.
Citation Information
Patent Citations
Secondary cell
JP2020181743A
battery
JP2021174578A
Sulfide all-solid-state battery
JP2022156220A
Battery
JP2023013065A
Battery
JP2023046619A